Method for manufacturing recycled plastic
The method addresses the inefficiencies in recycling plastic packaging by heating and kneading printed materials without desorbing layers, ensuring high polyolefin content and controlled pressure, resulting in strong and burn-resistant recycled plastic.
Patent Information
- Application Number
- JP2023086349
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-05-25
- Publication Date
- 2024-12-05
AI Technical Summary
Existing methods for recycling plastic packaging materials with printed layers face challenges such as reduced production efficiency due to the need for a desorption process, presence of foreign matter, and issues with compatibility of colorants and binder resins, leading to reduced tensile strength and increased burns during extrusion.
A method for producing recycled plastic using an extrusion device with a screw and discharge section, where the printed material is heated and kneaded without desorbing the base material and printing layer, maintaining a high polyolefin resin content, and controlling chlorine content, pressure, and using additives like antioxidants and compatibilizers to improve compatibility and suppress burns.
The method results in recycled plastic with excellent tensile strength and reduced foreign matter, burning immediately after the start of extrusion and during continuous extrusion, enhancing production efficiency and product quality.
Smart Images

Figure 2024169132000001 
Figure 2024169132000002 
Figure 2024169132000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for producing recycled plastics. [Background technology]
[0002] In recent years, plastic film packaging, plastic bottles, and other plastic products have been discarded and dumped as garbage in the ocean, causing environmental pollution problems. Plastic products are crushed in seawater and become submicron-sized fragments (microplastics), which float in the seawater. Microplastics are ingested by marine organisms such as fish and become concentrated in their bodies. As a result, there are concerns about the impact on the health of seabirds and humans who consume marine organisms as food.
[0003] In food packaging materials, polyolefin substrates such as polypropylene substrates (PP) and polyethylene substrates (PE) are often used as film substrates. Examples of food packaging materials include laminated laminates in which a film substrate is printed with printing ink and a sealant film is laminated on the printed layer, optionally via an adhesive layer, and printed matter in which one side of a film substrate is printed with printing ink and a heat sealant is printed on the other side. The printed matter can reduce the amount of plastic because no sealant film is required to be laminated, and is expected to contribute to environmental protection. In addition, there is a demand for material recycling from the viewpoint of further environmental protection. However, printed matter is difficult to material recycle due to problems such as compatibility between colorants and binder resins contained in film substrates and printed layers.
[0004] As a material recycling method for packaging materials, an invention has been disclosed in which a printed matter and laminated packaging material with a removable printed layer on a plastic substrate is separated from the printed layer in a release liquid containing a surfactant (Patent Document 1). However, the presence of a printing layer release step increases the time required to complete processing and increases the amount of manual setup work, resulting in a problem of reduced production volume. Note that the invention described in Patent Document 1 does not at all anticipate a method for material recycling packaging materials without separating the printed layer. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] International Publication No. 2021 / 230032 Summary of the Invention [Problem to be solved by the invention]
[0006] An object of the present invention is to provide a method for producing recycled plastics which have excellent tensile strength and which produce little foreign matter and little discoloration immediately after the start of extrusion and after continuous extrusion. [Means for solving the problem]
[0007] As a result of extensive research into the above problems, the present inventors have found that the above problems can be solved by using the packaging material described below, and have thus completed the present invention.
[0008] That is, the present invention relates to the following [1] to
[13] .
[0009] [1] A method for producing recycled plastic, comprising the steps of: obtaining recycled plastic from a printed matter using an extrusion device equipped with a first screw and a discharge portion; The printed matter includes a heat seal layer, a substrate, and a printing layer, The printed matter has not been subjected to a detachment step in which the substrate and the printing layer are detached, The chlorine content of the printed matter is 0.4% by mass or less based on the total mass, The printed matter contains a polyolefin resin (A) in an amount of 80 mass% or more based on the total mass of the printed matter, a heating, melting and kneading step of heating, melting and kneading the printed matter in the extrusion device to obtain a resin composition (D); and A method for producing recycled plastic, comprising an extrusion step of extruding the resin composition (D) from a discharge part of an extrusion device at a pressure of 18 MPa or less.
[0010] [2] The method for producing recycled plastics described in [1], wherein the heat seal layer contains a polyolefin resin (B) and / or an acrylic resin.
[0011] [3] The method for producing recycled plastics according to [2], wherein the polyolefin resin (B) contains an ethylene-vinyl acetate copolymer resin and / or a polyethylene resin (except for the case where the polyolefin resin (B) is an ethylene-vinyl acetate copolymer resin).
[0012] [4] A method for producing recycled plastics according to any one of claims [1] to [3], wherein the polyolefin resin (A) comprises a polyethylene resin and / or a polypropylene resin.
[0013] [5] The method for producing recycled plastics described in any one of [1] to [4], wherein the printed matter further includes a barrier layer.
[0014] [6] The method for producing recycled plastics described in [5], wherein the barrier layer is a vapor deposition layer including a vapor deposition film, or a barrier coat layer.
[0015] [7] The method for producing recycled plastics described in any one of [1] to [6], wherein the printed matter further has a surface protective layer on the printed layer.
[0016] [8] The method for producing recycled plastics according to any one of [1] to [7], wherein the printed layer contains a pigment and a binder resin, and the chlorine content of the binder resin is 5 mass% or less.
[0017] [9] The method for producing recycled plastics according to any one of [1] to [8], wherein the heating, melting and kneading step is carried out in the presence of an antioxidant.
[0018]
[10] The method for producing recycled plastics according to any one of [1] to [9], wherein the heating, melting and kneading step is carried out in the presence of a compatibilizer.
[0019]
[11] The method for producing recycled plastics according to any one of [1] to
[10] , wherein the heating and melting temperature in the heating, melting and kneading step is 120 to 280°C.
[0020]
[12] The method for producing recycled plastics according to any one of [1] to
[12] , wherein the rotation speed of the first screw of the extrusion device is 50 to 1000 rpm.
[0021]
[13] A method for producing a molded product made of recycled plastic, the molded product being produced by the method for producing recycled plastic described in any one of [1] to
[12] . Effect of the Invention
[0022] According to the present invention, it is possible to provide a method for producing recycled plastics which have excellent tensile strength and which have little foreign matter and little discoloration immediately after the start of extrusion and after continuous extrusion. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0023] The following describes in detail the embodiments of the present invention. However, the embodiments or explanations of the requirements described are merely examples of the embodiments of the present invention, and the present invention is not limited to these contents as long as they do not depart from the gist of the present invention.
[0024] [Manufacturing methods for recycled plastics] The present invention is a method for producing recycled plastic, which uses an extrusion device equipped with a screw and a discharge section to obtain recycled plastic from a printed matter that has not undergone a detachment process of detaching the substrate and the printed layer, wherein the printed matter includes a heat seal layer, a substrate layer, and a printed layer, and the printed matter has not undergone a detachment process of detaching the substrate and the printed layer, has a chlorine content of 0.4 mass% or less based on the total mass of the printed matter, and contains 80 mass% or more of polyolefin resin (A) based on the total mass of the printed matter, and includes a heating, melting, and kneading process of heating, melting, and kneading the printed matter in the extrusion device to obtain a resin composition (D), and an extrusion process in which the resin composition (D) is extruded from the discharge section of the extrusion device at a pressure of 18 MPa or less.
[0025] The polyolefin resin (A) contained in the printed matter refers to all polyolefin resins contained in each layer of the printed matter. Examples of the polyolefin resin contained in each layer of the printed matter include the polyolefin resin (B) contained in the heat seal layer described below and the polyolefin resin (C) contained in the substrate described below, but are not limited thereto, and the polyolefin resin contained in any layer such as a barrier layer or a surface protection layer is also included in the polyolefin resin (A).
[0026] The detachment process in the phrase "the printed matter has not undergone a detachment process in which the substrate and the printed layer are detached" refers to a detachment and removal process in which most of the printed layer is detached and removed from the printed matter, for example, using an alkali, and if the printed layer is unintentionally removed for some reason, it cannot be said to have "undergone a detachment process."
[0027] In the manufacturing method of the present invention, a printed matter including a heat seal layer, a base layer, and a printing layer is heated, melted, and kneaded, so that (1) the heat seal layer in a molten state suppresses aggregation of the colorant that may be contained in the printing layer and is compatible with the binder resin that may be contained in the printing layer, thereby improving the compatibility between the components of the printed matter during melt kneading, (2) the chlorine content in the printed matter is 0.4 mass% or less based on the total mass of the printed matter, so that foaming of the recycled plastic and damage to equipment due to chlorine gas generation in the heating, melting, and kneading process can be suppressed, (3) the polyolefin resin (A) content in the printed matter is 80 mass% or more based on 100 mass% of the printed matter, so that the heat seal layer, base layer, and printing layer are kneaded without layer separation in the heating, melting, and kneading process, and (4) the pressure of the discharge part of the extrusion device is set to 18 MPa or less, so that foreign matter can be prevented from passing through the filter, and therefore foreign matter and discoloration can be suppressed immediately after the start of extrusion and after continuous extrusion, and it is thought that the tensile strength can be improved. The mechanism of the above-mentioned effect is merely a guess and does not limit the invention in any way.
[0028] The foreign matter and discoloration immediately after the start of extrusion, which is the subject of the present invention, refers to the foreign matter and discoloration of the recycled plastic that is initially discharged from the discharge part of the extrusion device after the printed material is fed into the extrusion device in the heating, melting and kneading process. Also, the foreign matter and discoloration after continuous extrusion refers to the foreign matter and discoloration of the recycled plastic that is discharged from the discharge part of the extrusion device after the production of recycled plastic has been continued for 5 hours in the extrusion device. The above-mentioned foreign matter and discoloration were evaluated visually by heating and melting the recycled plastic again and forming it into a film.
[0029] The production method of the present invention essentially includes a heating, melting and kneading step of heating, melting and kneading the printed matter to obtain a resin composition (D) and an extrusion step of extruding the obtained resin composition (D), but preferably further includes a cooling step of cooling the extruded resin composition (D) to obtain a recycled plastic. The shape of the obtained recycled plastic is not particularly limited, and examples thereof include a rod-like, granular, cubic, rectangular, and amorphous shape.
[0030] From the viewpoint of handling of the printed matter, the manufacturing method of the present invention preferably further includes a crushing step of crushing the packaging material before the heat melt kneading step. From the viewpoint of removing foreign matter such as dust and dirt, it is preferable to include a cleaning step of washing the printed matter before the heat melt kneading step. From the viewpoint of removing moisture, it is preferable to include a dehydration drying step of dehydrating and / or drying the printed matter before the heat melt kneading step. In addition, it is preferable to carry out the heat melt kneading step in the presence of additives such as antioxidants and compatibilizers. From the viewpoint of removing foreign matter, it is preferable that the extrusion device is equipped with a foreign matter separator at its discharge section. From the viewpoint of handling of the recycled plastic, it is preferable to include a pelletizing step of shredding the extruded resin composition (D) after the cooling step or simultaneously with the cooling step.
[0031] <Crushing process> The crushing step is preferably carried out before the heating melt kneading step. The crushing step is preferably carried out before or simultaneously with the washing step described below, and more preferably before the washing step described below. The crushing method in the crushing step is not particularly limited, and examples thereof include a method using a jaw crusher, an impact crusher, a cutter mill, a stamp mill, a ring mill, a roller mill, a jet mill, or a hammer mill. The size of the fragments of the printed matter after crushing is preferably 1 mm to 50 mm in side length, more preferably 3 mm to 40 mm, and even more preferably 5 mm to 30 mm. When the size of the fragments of the printed matter after crushing is within the above range, the efficiency of the washing step and the dehydration drying step due to the expansion of the surface area and the homogenization of the resin composition are promoted, and the generation of foreign matter immediately after the start of extrusion and after continuous extrusion can be suppressed.
[0032] <Cleaning process> The washing step is preferably carried out on the printed matter before the heating, melting and kneading step, and is preferably carried out on the crushed printed matter after the above-mentioned crushing step. Examples of the washing method include a batch method and a continuous method, and a washing liquid such as water, a detergent, a neutralizing agent, an alkaline aqueous solution, etc. may be used.
[0033] <Dehydration drying process> The dehydration and drying process is preferably carried out on the printed matter before the heating, melting and kneading process, and the dehydration method is preferably a centrifugal dehydration method, and the drying method is preferably a hot air drying method. In the dehydration and drying process, either dehydration or drying alone may be carried out, but it is preferable to carry out both dehydration and drying. The moisture content in the printed matter after the dehydration and drying process is preferably 3% by mass or less, more preferably 2% by mass or less, even more preferably 1% by mass or less, and particularly preferably 0.6% by mass or less, based on the total mass of the printed matter. When the moisture content in the printed matter after the dehydration and drying process is within the above range, foaming due to evaporation of water during heating and melting can be suppressed.
[0034] <Heat melt kneading process> The heating, melting and kneading process is a process in which the printed matter is heated, melted and kneaded using an extrusion device equipped with a first screw, and in this process, the printed matter is heated and melted, and is further kneaded by the first screw, thereby changing the printed matter into a continuous phase resin composition. The higher the uniformity of the resin composition, the more the generation of foreign matter can be suppressed immediately after the start of extrusion of the recycled plastic and after continuous extrusion.
[0035] In the heat-melt-kneading step, the heat-melt temperature is preferably 120° C. to 280° C., more preferably 170° C. to 250° C., and even more preferably 180° C. to 240° C. When the heat-melt temperature is within the above range, both uniformity and low thermal history of the recycled plastic can be achieved, and therefore generation of foreign matter can be suppressed immediately after the start of extrusion of the recycled plastic and after continuous extrusion.
[0036] The rotation speed of the first screw is preferably 50 to 1000 rpm, more preferably 80 rpm to 850 rpm, and even more preferably 100 rpm to 600 rpm. When the rotation speed of the first screw is within the above range, the balance between the uniformity of the recycled plastic, the short residence time in the extrusion device, and the suppression of shear heat generation is good, so that the occurrence of foreign matter and burns immediately after the start of extrusion and after continuous extrusion can be suppressed. Note that the screw rotation speed of 50 to 900 rpm is equivalent to a shear rate of 222 to 4004 sec-1 The shear rate was calculated using the following formula under the conditions of the examples described later. Formula: (pi) x (screw diameter) x (screw rotation speed) / {(60 x (minimum gap distance between the cylinder inner wall and the screw)} Screw diameter: 34mm Minimum clearance between the cylinder inner wall and the screw: 0.4mm
[0037] The residence time of the resin composition in the extrusion device is preferably 10 to 120 seconds, more preferably 15 to 80 seconds, and particularly preferably 20 to 40 seconds. When the residence time of the resin composition in the extrusion device is within the above range, the heating time and kneading efficiency are good, so that the generation of foreign matter immediately after the start of extrusion of the recycled plastic and after continuous extrusion can be suppressed.
[0038] <Extrusion device> The extrusion device used in the manufacturing method of the present invention is equipped with a first screw and a discharge part. The extrusion device is a commonly used device capable of melting and molding a thermoplastic resin, etc., and for example, a known extrusion device described in JP 2017-148997 A can be used. Specifically, the extrusion device preferably has a first supply port for supplying material, a heating and melting kneading section for heating, melting and kneading the material such as a thermoplastic resin supplied from the first supply port, and a discharge section for discharging the thermoplastic resin heated, melted and kneaded in the heating and melting kneading section.
[0039] In the extrusion device, the material is melted by shear heat caused by the rotation of the first screw and heating by an electric heater, etc., and the molten material is kneaded by the rotation of the first screw. Examples of the extrusion device include a twin-screw extruder, a single-screw extruder, and a rotor-type twin-screw kneader, but from the viewpoint of kneading efficiency, a twin-screw extruder or a rotor-type twin-screw kneader is preferred.
[0040] <How to add additives> In the manufacturing method of the present invention, the heating and melting kneading step is preferably carried out in the presence of an antioxidant and / or a compatibilizer. The antioxidant and / or the compatibilizer are different from those contained in the printed matter beforehand. In addition, known additives other than the antioxidant and the compatibilizer may be added within a range that does not impair the effects of the present invention. As a method for adding the additive, a method in which the printed matter to which the additive has been added is supplied from the first supply port in the heating and melting kneading step, or a method in which the additive is added using an extrusion device equipped with a second supply port and a second screw are preferred examples. The extrusion device can be created by connecting barrels together, so that one or more of the barrels can be equipped with a second supply port and a second screw, and the positions of the second supply port and the second screw may be anywhere in the extrusion device. It is preferable that the additive added from the second supply port is mixed into the resin composition that has been introduced and heated and melted from the first supply port while being kneaded by the second screw.
[0041] Additives Examples of the additives include antioxidants, compatibilizers, lubricants, weather stabilizers, plasticizers, and antistatic agents, with antioxidants and compatibilizers being preferred.
[0042] Antioxidants By using an antioxidant, the occurrence of scorching can be suppressed, and recycled plastics with less scorching immediately after the start of extrusion and after continuous extrusion can be obtained. As the antioxidant, known antioxidants such as phenol-based, phosphoric acid-based, sulfur-based, and amine-based antioxidants can be used, with phenol-based and phosphoric acid-based antioxidants being preferred. The antioxidant addition rate relative to 100% by mass of the printed matter is preferably 0.01 to 3% by mass, more preferably 0.05 to 1% by mass, and even more preferably 0.1 to 0.5% by mass. When the antioxidant addition rate is within the above range, the occurrence of scorching immediately after the start of extrusion and after continuous extrusion can be suppressed.
[0043] (Phenol-based antioxidant) Examples of the phenol-based antioxidant include monophenol-based, bisphenol-based, trisphenol-based, tetraphenol-based, polyphenol-based, and thiobisphenol-based antioxidants. The bisphenol-based, trisphenol-based, and tetraphenol-based antioxidants, which have a large tanning suppression effect, are preferred, and the tetraphenol-based antioxidants are more preferred.
[0044] As commercially available phenolic antioxidants, Irganox 1010, Irganox 1076, Irganox 245 (manufactured by BASF), etc. can be used.
[0045] (Phosphate-based antioxidant) Examples of the phosphoric acid-based antioxidant include monononyl-based, dinonyl-based, trinonyl-based, allyl-based, alkylaryl-based, monoalkyl-based, dialkyl-based, trialkyl-based, and dioxa-based antioxidants. Of these, the trinonyl-based, allyl-based, alkylaryl-based, trialkyl-based, and dioxa-based antioxidants are preferred, as they have a greater tanning suppression effect, and the dioxa-based antioxidants are more preferred.
[0046] Commercially available phosphoric acid-based antioxidants that can be used include Irgafos168 (manufactured by BASF) and ADK STAB PEP-36 (manufactured by ADEKA).
[0047] (Compatibilizer) By using a compatibilizer, the colorant and binder resin derived from the printed layer can be more easily mixed with other components, making it possible to obtain recycled plastic with less foreign matter immediately after the start of extrusion and after continuous extrusion. The compatibilizer preferably contains a polyolefin copolymer, and suitable examples of the polyolefin copolymer include polyolefin-styrene copolymer, polyolefin-acrylic copolymer, polyolefin-acrylonitrile copolymer, (maleic anhydride) modified polyolefin, etc. However, the polyolefin copolymer is not limited to these. The "copolymer" may be a block copolymer, a random copolymer, or a graft copolymer. (Hereinafter, in the case of a graft copolymer, it will be expressed as "main chain = g = side chain".) Preferred forms of the compatibilizer include polyethylene=g=polystyrene, polyethylene=g=styrene-acrylonitrile copolymer, polypropylene=g=styrene-acrylonitrile copolymer, ethylene-ethyl acrylate copolymer=g=styrene-acrylonitrile copolymer, oxazoline group-containing polystyrene, polycarbonate=g=glycidyl methacrylate-styrene-acrylonitrile copolymer, maleic anhydride-modified polyolefin, and the like, with maleic anhydride-modified polyolefin being preferred.
[0048] Examples of maleic anhydride-modified polyolefins include maleic anhydride-modified polyethylene, maleic anhydride-modified polypropylene, maleic anhydride-modified ethylene-butene copolymer, ethylene-glycidyl methacrylate copolymer, and maleic anhydride-modified styrene-butadiene copolymer, and among these, maleic anhydride-modified polyethylene and maleic anhydride-modified polypropylene are preferred.
[0049] The addition rate of the compatibilizer relative to 100% by mass of the printed matter is preferably 0.01 to 1% by mass, more preferably 0.05 to 0.5% by mass, and even more preferably 0.1 to 0.2% by mass. When the addition rate of the compatibilizer is within the above range, the compatibility between the binder resin derived from the printed layer and the polyolefin resin is improved, so that the generation of foreign matter immediately after the start of extrusion and after continuous extrusion can be suppressed.
[0050] As the compatibilizer, commercially available products such as Admer Q series (manufactured by Mitsui Chemicals, Inc.) and Eumex series (manufactured by Sanyo Chemical Industries, Ltd.) can be used.
[0051] (lubricant) The lubricant serves to reduce friction between resin compositions in an extrusion device and between the resin composition and the extrusion device. Examples of the lubricant include hydrocarbon-based lubricants such as paraffin wax and synthetic polyethylene, fatty acid-based lubricants such as stearic acid and behenin, higher alcohol-based lubricants such as stearyl alcohol, fatty acid amide-based lubricants such as stearic acid amide, oleic acid amide, and erucic acid amide, metal soap-based lubricants such as calcium, zinc, and magnesium stearate, and ester-based lubricants such as glycerin monostearate and glycerin monooleate, with fatty acid amide-based lubricants being preferred.
[0052] The addition rate of the lubricant relative to 100% by mass of the printed matter is preferably 0.01 to 5% by mass, more preferably 0.03 to 3% by mass, and even more preferably 0.05 to 1% by mass.
[0053] As the lubricant, commercially available products such as Fatty Acid Amide S (manufactured by Kao Corporation) and Fatty Acid Amide ON can be used.
[0054] (Weather resistance stabilizer) Weathering stabilizers absorb ultraviolet rays and extend the weathering life of plastics. Examples of weathering stabilizers include benzotriazoles, triazines, benzophenones, benzoates, and hindered amines.
[0055] The addition rate of the weather resistance stabilizer relative to 100% by mass of the printed matter is preferably 0.05 to 5% by mass, and more preferably 0.1 to 2% by mass.
[0056] As the weather resistance stabilizer, commercially available products such as Adeka STAB ALA series (manufactured by ADEKA CORPORATION) can be used.
[0057] (Plasticizer) Plasticizers have the role of imparting flexibility to plastics. Examples of plasticizers include epoxidized vegetable oils such as epoxidized soybean oil and epoxidized linseed oil, phthalate esters such as dioctyl phthalate and dibutyl phthalate, and polyesters such as polyesters made of dibasic acids and glycols.
[0058] The addition rate of the plasticizer relative to 100% by mass of the printed matter is preferably 0.1 to 50% by mass, more preferably 0.5 to 30% by mass, and even more preferably 1 to 15% by mass.
[0059] As the plasticizer, commercially available products such as Adesizer PN series (manufactured by ADEKA Corporation) can be used.
[0060] (Antistatic agent) The antistatic agent has a role of suppressing static electricity buildup in plastics. Examples of the antistatic agent include fatty acid sulfonates and fatty acid esters.
[0061] As the antistatic agent, commercially available products such as Electromaster series (manufactured by Kao Corporation) and Electrostripper (manufactured by Kao Corporation) can be used.
[0062] The addition rate of the antistatic agent relative to 100% by mass of the printed matter is preferably 0.05 to 3% by mass, and more preferably 0.1 to 2% by mass.
[0063] <Extrusion process> In the extrusion step, the resin composition (D) is discharged from a discharge part of the extrusion device. In one embodiment, it is preferable that the discharge part includes a foreign matter separator, and the resin composition (D) is discharged through the foreign matter separator. In discharging the heated, melted and kneaded resin composition (D), the extrusion pressure of the extruder is 18 MPa or less, more preferably 0.1 to 18 MPa, further preferably 1 to 12 MPa, and particularly preferably 3 to 7 MPa, from the viewpoint of durability of the extruder. The extrusion pressure of the extruder does not need to be constant all the time, but the extrusion pressure referred to here is the maximum extrusion pressure during the extrusion process. When the extrusion pressure is within the above range, the foreign matter separation efficiency by the foreign matter separation device is good, so that the generation of foreign matter immediately after the start of extrusion and after continuous extrusion can be suppressed. The extrusion pressure is affected by the processing temperature, screw rotation speed, discharge amount, resin viscosity, and the foreign matter separation device (screen mesh, etc.) used to remove foreign matter from the recycled plastic. In addition, clogging of the mesh with insoluble matter, foreign matter, etc., and foaming due to moisture, chlorine-containing substances, etc. are also factors that cause pressure changes.
[0064] The discharge rate of the extrusion device is preferably 5 to 60 kg per hour, more preferably 10 to 50 kg, and particularly preferably 15 to 40 kg per hour. When it is within the above range, the extrusion pressure and kneading efficiency are good, so that the generation of foreign matter and scorching can be suppressed immediately after the start of extrusion of the recycled plastic and after continuous extrusion.
[0065] 《Foreign matter separation device》 The discharge part of the extrusion device is preferably equipped with a foreign matter separation device to remove foreign matter in the resin composition (D). For example, a screen mesh (metal mesh) can be used as the foreign matter separation device. For example, the screen mesh can be woven, such as plain weave, twill weave, plain tatami weave, and twill tatami weave, or punched metal type, and from the viewpoint of removing foreign matter, the plain weave is preferred. Taking into consideration the removal of foreign matter, discharge pressure, and clogging, the size of the screen mesh is preferably 20 to 200 mesh, more preferably 60 to 150 mesh, and even more preferably 80 to 140 mesh.
[0066] <Cooling process> The resin composition (D) extruded in the extrusion step is preferably cooled in the cooling step to form a recycled plastic. Examples of the cooling method in the cooling step include air cooling, wind cooling, and water cooling. In the present invention, it is preferable to include a water cooling step. The cooling temperature in the cooling step is preferably 20°C to 80°C, and more preferably 30°C to 60°C. The cooling step may be carried out simultaneously with the pelletizing step described below, or may be carried out after the pelletizing step. Specifically, for example, the extruded resin composition (D) may be pelletized while being air-cooled immediately after extrusion, and then water-cooled.
[0067] <Pelletizing process> The recycled plastic may be processed into pellets by a pelletizing process, or may be pelletized during the cooling process. Examples of the pelletizing method include a hot cut method and a strand cut method, and are not particularly limited. However, in consideration of continuous productivity, the hot cut method is preferred.
[0068] [Printed material] In the method for producing recycled plastics of the present invention, a printed matter is used as a raw material. The printed matter includes a heat seal layer, a base layer, and a printed layer. At least one of the layers includes a polyolefin resin, and the polyolefin resin is contained in an amount of 80 mass% or more of the total mass of the printed matter. Note that when multiple layers are actually laminated in contact with each other, such as the first printed layer and the second printed layer, the layers are collectively referred to simply as the printed layer. Specific examples of the configuration of the printed matter include, but are not limited to, the following configurations. In the configuration descriptions (1) to (4) below, " / " indicates the boundary between layers. (1) Heat seal layer / substrate / printing layer (2) Heat seal layer / substrate / printing layer / surface protection layer (3) Heat seal layer / substrate / barrier layer / printing layer (4) Heat seal layer / substrate / barrier layer / printing layer / surface protection layer However, the form of the printed matter used in the present invention is not limited to these.
[0069] Since the present invention is mainly focused on the production of recycled polyolefin resin, the printed matter used contains polyolefin resin in an amount of 80% by mass or more based on the total mass of the printed matter. The polyolefin resin content is more preferably 85% by mass or more, even more preferably 90% by mass or more, and even more preferably 95% by mass or more. When it is within the above range, the homogeneity of the resin composition is improved, so that the generation of foreign matter immediately after the start of extrusion of the recycled plastic and after continuous extrusion can be suppressed. The polyolefin is preferably polypropylene and / or polyethylene. The polypropylene is more preferably a copolymer with ethylene and / or butene.
[0070] [Heat seal layer] The heat seal layer preferably contains a polyolefin resin (B) and / or an acrylic resin, and more preferably contains a polyolefin resin (B). The heat seal layer is preferably located on the opposite side of the substrate layer to the side having the printed layer. The unit area mass of the heat seal layer is 1 to 18 g / m 2 and 3 to 12 g / m 2 When the content is within the above range, the generation of foreign matter and scorch marks immediately after the start of extrusion of the recycled plastic and after continuous extrusion can be suppressed.
[0071] The heat seal layer may contain, in addition to the polyolefin resin (B) and / or the acrylic resin, a known thermoplastic resin such as a urethane resin, a polylactic acid resin, etc. These may be used alone or in combination of two or more kinds.
[0072] The resin content of the heat seal layer is preferably 70 to 100% by mass, more preferably 90 to 100% by mass, based on 100% by mass of the heat seal layer. When the resin content is within the above range, the generation of foreign matter and burns immediately after the start of extrusion of the recycled plastic and after continuous extrusion can be suppressed.
[0073] <Polyolefin resin (B)> Examples of the polyolefin resin (B) include ethylene-vinyl acetate copolymer resin, polyethylene resin, polypropylene resin, polybutene resin, etc., with ethylene-vinyl acetate copolymer resin and polyethylene resin being preferred.
[0074] <Ethylene-vinyl acetate copolymer resin> The ethylene-vinyl acetate copolymer resin is a copolymer made of ethylene and vinyl acetate. The vinyl acetate content in the ethylene-vinyl acetate copolymer resin is preferably 5 to 50 mass%, more preferably 10 to 40 mass%, and particularly preferably 20 to 30 mass%, based on 100 mass% of the ethylene-vinyl acetate copolymer resin. The minimum film-forming temperature of the ethylene-vinyl acetate copolymer resin is preferably 40 to 120°C, more preferably 60 to 100°C. When the vinyl acetate content and the minimum film-forming temperature are within the above ranges, the heat sealability of the printed matter is good. The glass transition temperature of the ethylene-vinyl acetate copolymer resin is preferably -60 to 20°C, more preferably -25 to 5°C.
[0075] Examples of the ethylene-vinyl acetate copolymer resin that can be used include Aquatex EC series manufactured by Japan Coating Resins Co., Ltd., and Sumikaflex S-201HQ, S-305, S-305HQ, S-400HQ, S-401HQ, S-408HQE, S-450HQ, S-455HQ, S-456HQ, S-460HQ, S-467HQ, S-470HQ, S-480HQ, S-510HQ, S-520HQ, S-752, and S-755 manufactured by Sumitomo Chemical Co., Ltd. <Polyethylene resin (excluding ethylene-vinyl acetate copolymer resin)> As the polyethylene resin, low density polyethylene, linear low density polyethylene, and high density polyethylene can be used, and also ionic polyethylene resin can be used.
[0076] <Polyethylene resin having ionic groups> The polyethylene resin having an ionic group is not particularly limited, but may be a copolymer of ethylene and an unsaturated carboxylic acid neutralized with a metal ion, specifically an ethylene-(meth)acrylic acid copolymer neutralized with a metal ion. The metal ion may be either a monovalent metal ion or a polyvalent metal ion, such as a zinc ion or a sodium ion, and the degree of neutralization of the polyethylene resin having an ionic group is preferably 5 to 90%.
[0077] As the polyethylene resin, for example, commercially available products such as "S-500", "S420" and "S200" from the Chemipearl series manufactured by Mitsui Chemicals, Inc. can be used.
[0078] <Acrylic resin> The acrylic resin refers to a structure obtained by vinyl polymerization of an ethylenically unsaturated monomer including a monomer having an acrylic group or a methacrylic group. The acid value of the acrylic resin is preferably 20 to 120 mgKOH / g, more preferably 30 to 100 mgKOH / g, and particularly preferably 40 to 80 mgKOH / g. When the acid value of the acrylic resin is within the above range, the compatibility with the colorant is improved, and thus the generation of foreign matter immediately after the start of extrusion of the recycled plastic and after continuous extrusion can be suppressed. The glass transition temperature of the acrylic resin is preferably -40 to 90°C, more preferably -30 to 70°C, and particularly preferably -20 to 50°C. When the glass transition temperature of the acrylic resin is within the above range, the compatibility with the colorant is improved, and thus the generation of foreign matter immediately after the start of extrusion of the recycled plastic and after continuous extrusion can be suppressed. In addition, preferred examples of the acrylic resin include a homopolymer of an acrylic monomer, a copolymer of an acrylic monomer and an acidic monomer, and a copolymer of ethylene and an acrylic monomer.
[0079] Examples of the monomer having an unsaturated double bond including the (meth)acrylic monomer include alkyl ester compounds of (meth)acrylic acid such as methyl (meth)acrylate, ethyl (meth)acrylate, n-propyl (meth)acrylate, n-butyl (meth)acrylate, n-hexyl (meth)acrylate, n-octyl (meth)acrylate, decyl (meth)acrylate, and lauryl (meth)acrylate; (meth)acrylic acid amide derivatives containing at least one N-substituted methylol group, such as N-methylol (meth)acrylamide; Aminoalkyl esters of (meth)acrylic acid such as dimethylaminoethyl (meth)acrylate, diethylaminoethyl (meth)acrylate, dipropylaminoethyl (meth)acrylate, dimethylaminopropyl (meth)acrylate, diethylaminopropyl (meth)acrylate, and dipropylaminopropyl (meth)acrylate; Mono- or diesters of (meth)acrylic acid of glycols such as diethylene glycol and dipropylene glycol, Styrene, α-methylstyrene and other styrene derivatives, Hydroxyalkyl ester compounds of (meth)acrylic acid, such as 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, and 3-hydroxypropyl (meth)acrylate; Acrylic acid, methacrylic acid, Examples of suitable vinyl compounds include those having an acid group such as maleic acid and itaconic acid. From the viewpoint of the heat sealability of the printed matter, the acrylic resin preferably has a carboxyl group and / or a hydroxyl group, and when the acrylic resin has a hydroxyl group, it preferably contains a hydroxyalkyl ester compound of (meth)acrylic acid as a monomer constituting the acrylic resin.
[0080] As the acrylic resin, commercially available products may be used, such as JONCRYL PDX7356, PDX-7326, and PDX-7430 manufactured by BASF, and PE-1126, JE-1113, and KE1148 manufactured by Seiko PMC Corporation.
[0081] <Additives> The heat seal layer may further contain optional additives such as an antifoaming agent, an emulsifier, a preservative, a plasticizer, an amide wax, a hydrocarbon wax, and a chelating crosslinking agent, and preferably contains an antifoaming agent and / or an emulsifier.
[0082] Defoaming Agent The heat seal layer preferably contains an antifoaming agent from the viewpoint of improving the smoothness of the heat seal layer. When the heat seal layer contains an antifoaming agent, the heat seal strength is improved. Examples of the antifoaming agent include silicon-based antifoaming agents and non-silicon-based antifoaming agents, and from the viewpoint of antifoaming properties, silicon-based antifoaming agents are preferred. The content of the antifoaming agent in the heat seal layer is preferably 0.01 to 1 mass%, more preferably 0.05 to 0.5 mass%, and particularly preferably 0.1 to 0.3 mass%, based on 100 mass% of the heat seal layer.
[0083] "emulsifier" From the viewpoint of solubility in water, the heat seal layer preferably contains an emulsifier. Examples of the emulsifier include vinyl alcohol resin, ethylene-vinyl alcohol copolymer resin, nonionic surfactant, cationic surfactant, anionic surfactant, etc., and from the viewpoint of recyclability, vinyl alcohol resin and cationic surfactant are preferred. The content of the emulsifier in the heat seal layer is preferably 0.01 to 1 mass%, more preferably 0.05 to 0.5 mass%, and particularly preferably 0.1 to 0.3 mass%, based on 100 mass% of the heat seal layer.
[0084] As the defoaming agent, a commercially available product may be used, for example, BYK-024, BYK-025, or BYK-028 manufactured by BYK.
[0085] <Formation of heat seal layer> The heat seal layer can be formed, for example, by (1) applying a thermoplastic resin by heating and melting it on the substrate surface opposite to the surface protective layer, or (2) printing using a heat seal agent and then drying and removing the volatile components. The preferred method of formation is the method of (2) using a heat seal agent. The preferred printing method of the heat seal agent is the gravure printing method or the flexographic printing method. For example, in gravure printing, the heat seal agent is diluted with a diluting solvent to an appropriate viscosity and concentration as necessary, and is supplied to each printing unit alone or in a mixture, and then applied, and the coating is fixed by drying in an oven to obtain a heat seal layer.
[0086] <Heat sealant> The heat-sealing agent preferably contains a polyolefin resin (B) and / or an acrylic resin, and further preferably contains a solvent. The heat-sealing agent may also contain the above-mentioned additives. From the viewpoint of environmental load, the heat-sealing agent is preferably water-based.
[0087] (gravure printing) << Gravure version >> In gravure printing, the gravure plate is a cylindrical metal plate on which recesses for each color are formed by engraving, etching, or laser. There are no restrictions on the use of engraving and laser, and they can be set arbitrarily according to the pattern. Lines of 80 to 250 are used appropriately, and the higher the line count, the finer the printing.
[0088] Gravure printing machine In a gravure printing press, one printing unit is equipped with the gravure plate and doctor blade. There are many printing units, and each unit has an oven drying unit. Printing is performed by rotary printing, and a roll-to-roll printing method is used. The type of plate and the type of doctor blade are appropriately selected according to the specifications.
[0089] [Base material] The substrate is preferably a plastic substrate mainly containing polyolefin resin (C) as a raw material. The substrate is preferably in the form of a film or sheet, since the uniformity of the recycled plastic is improved, resulting in a reduction in foreign matter and an improvement in tensile strength. Substrates mainly containing polyolefin resin (C) have higher heat resistance than ester-based substrates, and are less susceptible to thermal decomposition and hydrolysis during the heating, melting and kneading process and the recycled plastic molding process, making it possible to maintain a high molecular weight. Further, examples of plastic substrates mainly containing polyolefin resin (C) include biaxially oriented polypropylene (OPP), non-oriented polypropylene (CPP), polyethylene such as low density polyethylene (LDPE), linear low density polyethylene (LLDPE), medium density polyethylene (MDPE), high density polyethylene (HDPE), acid-modified polyethylene, acid-modified polypropylene, copolymer polypropylene, and films laminated with these. The thickness of the substrate is not particularly limited, and is preferably 5 μm or more and 150 μm or less, more preferably 10 μm or more and 70 μm or less, from the viewpoint of reducing foreign matter and improving the tensile strength of recycled plastics. In addition, films having heat sealability are preferably used, and CPP, heat sealable OPP, etc. are included.
[0090] The substrate mainly containing polyolefin resin (C) may be a simple laminate of polyolefin substrates, or a substrate different from the polyolefin substrate may be laminated. The "substrate different from the polyolefin substrate" may be a film having properties different from the polyolefin substrate, and may be of any type. In addition, in the case of a laminated substrate, it may be in a form including an adhesive layer. The method of laminating plastics is not particularly limited, and may be a conventionally known method such as coextrusion, heat fusion, and pressure bonding via an adhesive layer.
[0091] The substrate is preferably in a form containing additives such as antistatic agents, antifogging agents, and ultraviolet protection agents by coating or kneading, in a form having an easily adhesive coating layer (e.g., a layer containing polyvinyl alcohol and its derivatives), in a form in which the surface of the substrate is corona-treated or low-temperature plasma-treated, in a form in which the substrate is a barrier substrate having a vapor deposition layer or a barrier coating layer, etc. The above-mentioned additions and processing are also carried out for the purpose of improving the wettability of printing inks and other coating agents, or for the purpose of imparting specific functionality to the film, and are suitably used, for example, to provide a packaging material with excellent visibility of the contents by preventing fogging of the packaging material due to moisture.
[0092] [Print layer] The printed layer can be a layer that displays any design, pattern, letter, symbol, etc. for the purpose of providing decoration or aesthetics; displaying the contents, expiration date, and manufacturer or seller. The printed layer may be a solid printed layer that does not have a design, pattern, letter, symbol, etc. The method for forming the printed layer is not particularly limited, and it can be formed, for example, using a printing ink containing a colorant and a binder resin. The printed layer may be a single layer or a multi-layer structure, and may be provided on the surface layer. The thickness of the printed layer is 0.1 to 12 g / m 2 It is preferable that the thickness is 0.5 to 6 g / m 2 More preferably, it is 1 to 3 g / m 2 It is more preferable that:
[0093] <Binder resin contained in the printing layer> The printing layer preferably contains a binder resin. The binder resin contained in the printing layer refers to the binding resin in the printing layer. Examples of the binder resin contained in the printing layer include, but are not limited to, urethane resin, cellulose resin, polyamide resin, rosin resin, ethylene-vinyl acetate copolymer resin, vinyl chloride-vinyl acetate copolymer resin, vinyl acetate resin, acrylic resin, styrene resin, dammar resin, styrene-acrylic copolymer resin, styrene-maleic acid copolymer resin, polyester resin, alkyd resin, terpene resin, phenol-modified terpene resin, ketone resin, cyclized rubber, butyral, polyacetal resin, petroleum resin, and modified resins thereof. These resins can be used alone or in a mixture of two or more. Among the above, it is preferable to contain one or more selected from the group consisting of resins other than vinyl chloride-vinyl acetate copolymer resin, and it is more preferable to contain urethane resin and styrene-acrylic resin.
[0094] (Chlorine content of binder resin in print layer) The chlorine content of the binder resin is the content (mass%) of chlorine atoms based on the mass of the binder resin. The binder resin contained in the printed layer preferably has a chlorine content of 0 to 5 mass%, more preferably 0 to 3 mass%, and even more preferably 0 to 2 mass%. When the chlorine content of the binder resin contained in the printed layer is within the above range, chlorine generation during the heating, melting, and kneading process can be suppressed, so that the tensile strength of the recycled plastic is good. The chlorine contained in the binder resin may come from the ethylenically unsaturated monomer itself used, which may contain chlorine atoms, or from a compound containing chlorine atoms that is mixed in during the manufacturing process.
[0095] In the present invention, the chlorine content of the resin is measured in accordance with JIS K0127 (2013). In this measurement method, a sample pretreated by a combustion method is quantified by ion chromatography. The chlorine content of the printed layer can be simply calculated from the chlorine content of each of the raw materials constituting the printed layer using the following formula: The same applies to each of the other layers. Formula: Chlorine content (%) in total mass of binder resin solids = mass of chlorine in total mass of binder resin solids / total mass of binder resin solids (%) Formula: Chlorine content (%) in total mass of solids in printed layer = mass of chlorine in total mass of solids in printed layer / total mass of solids in printed layer (%)
[0096] Coloring Agent The printed layer preferably contains a colorant. The colorant is preferably a pigment, and either an organic pigment or an inorganic pigment can be used. The colorant may be used alone or in combination of two or more kinds. In consideration of quality deterioration due to coloring of recycled plastics, the content of the colorant in the total mass of the printed layer is preferably 30% by mass or less, more preferably 25% by mass or less, and even more preferably 23% by mass or less.
[0097] (Organic pigments) Examples of the organic pigment include, but are not limited to, soluble azo pigments, insoluble azo pigments, azo pigments, phthalocyanine pigments, halogenated phthalocyanine pigments, anthraquinone pigments, anthanthrone pigments, dianthraquinonyl pigments, anthrapyrimidine pigments, perylene pigments, perinone pigments, quinacridone pigments, thioindigo pigments, dioxazine pigments, isoindolinone pigments, quinophthalone pigments, azomethine azo pigments, flavanthrone pigments, diketopyrrolopyrrole pigments, isoindoline pigments, indanthrone pigments, and carbon black pigments. Further examples include carmine 6B, lake red C, permanent red 2B, disazo yellow, pyrazolone orange, carmine FB, chromophthalic yellow, chromophthalic red, phthalocyanine blue, phthalocyanine green, dioxazine violet, quinacridone magenta, quinacridone red, indanthrone blue, pyrimidine yellow, thioindigo bordeaux, thioindigo magenta, perylene red, perinone orange, isoindolinone yellow, aniline black, diketopyrrolopyrrole red, and daylight fluorescent pigments.
[0098] (Inorganic pigments) Examples of inorganic pigments include titanium oxide, zinc oxide, zinc sulfide chromium oxide, aluminum particles, mica, bronze powder, chrome vermilion, yellow lead, cadmium yellow, cadmium red, ultramarine, Prussian blue, red iron oxide, yellow iron oxide, iron black, titanium oxide, zinc oxide, silica, barium sulfate, kaolin, clay, calcium carbonate, and magnesium carbonate. Aluminum can be either leafing or non-leafing type, with the non-leafing type being preferred.
[0099] Additives The printed layer or the printing ink used to form the printed layer may contain known additives such as defoamers, fragrances, flame retardants, hydrocarbon waxes, thickeners, leveling agents, dispersants, curing agents, silane coupling agents, plasticizers, infrared absorbers, and ultraviolet absorbers, as necessary, and preferably contains at least one selected from the group consisting of hydrocarbon waxes and dispersants.
[0100] <Formation of printing layer> The printing layer can be formed, for example, by printing on a substrate using a printing ink and then removing the volatile components. The printing method is preferably a gravure printing method or a flexographic printing method. For example, the ink is diluted with a diluting solvent to a viscosity and concentration suitable for gravure printing, and is supplied to each printing unit alone or in a mixture and printed. The printing layer can then be obtained by fixing the coating by drying in an oven or the like.
[0101] <Printing ink manufacturing method> The printing ink used to form the printing layer can be produced, for example, by dispersing a pigment in an organic solvent with a resin or the like using a dispersing machine, and then mixing the resulting pigment dispersion with a resin, various additives, an organic solvent, and the like. As the dispersing machine, a commonly used machine, for example, a roller mill, a ball mill, a pebble mill, an attritor, or a sand mill, can be used. The particle size distribution of the pigment in the pigment dispersion can be adjusted by appropriately changing the size of the grinding media of the dispersing machine, the packing rate of the grinding media, the dispersion processing time, the discharge speed of the pigment dispersion, the viscosity of the pigment dispersion, and the like. The viscosity of the printing ink at 25°C is preferably in the range of 10 to 1000 mPa·s or less from the viewpoint of preventing the pigment from settling and dispersing appropriately. The above viscosity is measured at 25°C using a Tokimec Co., Ltd. B-type viscometer.
[0102] <Layers other than the heat seal layer, the substrate, and the printing layer> [Surface protection layer] The printed matter may further have a surface protective layer. The surface protective layer is preferably located on the side of the substrate opposite to the side having the heat seal layer. The mass per unit area of the surface protection layer is 1.5 to 12 g / m 2 and more preferably 3 to 8.4 g / m 2 The surface protective layer can be formed by an overcoat agent, and the formation method can be appropriately selected from known printing methods such as gravure printing and flexographic printing, and is preferably gravure printing. From the viewpoint of printability, the viscosity of the overcoat agent is preferably 20 to 200 mPa·s. In the present invention, the "overcoat agent" refers to an agent that does not contain a colorant such as a pigment, but does not exclude an agent that contains a small amount of a colorant that has been unintentionally mixed in.
[0103] (Binder resin contained in surface protective layer) The surface protective layer preferably contains a binder resin. Examples of the binder resin contained in the surface protective layer include cellulose resin, polyamide resin, urethane resin, rosin resin, ethylene-vinyl acetate copolymer resin, vinyl chloride-vinyl acetate copolymer resin, vinyl acetate resin, styrene resin, acrylic resin, styrene-acrylic copolymer resin, styrene-maleic acid copolymer resin, polyester resin, dammar resin, alkyd resin, terpene resin, phenol-modified terpene resin, ketone resin, cyclized rubber, butyral, polyacetal resin, petroleum resin, and modified resins thereof. These resins can be used alone or in a mixture of two or more. Among the above, it is more preferable to contain a cellulose resin or a styrene-acrylic resin.
[0104] Additives The surface protective layer or the overcoat agent used to form the surface protective layer may contain any additives, such as a plasticizer, an amide wax, a hydrocarbon wax, a chelating crosslinking agent, etc., as necessary.
[0105] <Formation of surface protective layer> The surface protective layer can be formed, for example, by printing an overcoat agent on a printed layer of a printed material having a printed layer provided on a substrate, and then removing the volatile components. Examples of printing methods include gravure printing and flexographic printing. For example, the overcoat agent is diluted with a diluting solvent to a viscosity and concentration suitable for gravure printing, and is supplied to each printing unit alone or in a mixture and applied. Thereafter, the coating is fixed by drying in an oven or the like to obtain a surface protective layer.
[0106] <Method of manufacturing the overcoat agent> The overcoat agent can be obtained by feeding a resin solution, in which a resin is dissolved or dispersed in a solvent, and a solvent into an agitator equipped with an agitating blade, a rotor, etc., and mixing and stirring the solvent. There is no particular restriction on the stirring speed, and stirring can be performed at 50 to 2000 rpm. In order to improve the handling and coating properties of the overcoat agent, a solvent can also be appropriately added. From the viewpoint of printability and the like, the viscosity of the overcoat agent is preferably 50 to 300 mPa·s.
[0107] [Barrier layer] The printed matter may further include a barrier layer. The barrier layer exists for the purpose of imparting barrier properties to the printed matter, and the barrier layer exists to control the permeation of objects to be blocked, such as light, magnetism, and various gases, through the packaging material, and contains a barrier component. The barrier layer may be a vapor deposition layer or a barrier coat layer.
[0108] (deposited layer) When the printed matter has a vapor deposition layer as a barrier layer, the vapor deposition layer preferably includes a vapor deposition film, and it is preferable to use, as the vapor deposition layer, one or more selected from the group consisting of a substrate having a vapor deposition film, an intermediate substrate having a vapor deposition film, and a sealant having a vapor deposition film. By having a vapor deposition layer including a vapor deposition film, the printed matter has high gas barrier properties, specifically oxygen barrier properties and water vapor barrier properties, and a packaging container produced using the printed matter can suppress a decrease in the mass of the contents filled therein.
[0109] The vapor-deposited film may be a vapor-deposited film of one or more inorganic substances or inorganic oxides such as silicon (Si), aluminum (Al), magnesium (Mg), calcium (Ca), potassium (K), tin (Sn), sodium (Na), boron (B), titanium (Ti), lead (Pb), zirconium (Zr), yttrium (Y), etc. The vapor-deposited film may be composed of two or more layers, and may be composed of the same material or different materials. Among the above, from the viewpoints of adhesion and gas barrier properties, the vapor-deposited film is preferably made of aluminum, aluminum oxide (alumina) or silicon oxide (silica).
[0110] The thickness of the vapor-deposited film is preferably 1 nm or more and 150 nm or less, more preferably 5 nm or more and 60 nm or less, and even more preferably 10 nm or more and 40 nm or less. By making the thickness of the vapor-deposited film 1 nm or more, the oxygen barrier property and water vapor barrier property of the vapor-deposited layer can be further improved. Furthermore, by making the thickness of the vapor-deposited film 150 nm or less, the generation of foreign matter immediately after the start of extrusion of the recycled plastic and after continuous extrusion can be suppressed.
[0111] The method for forming the vapor-deposited film may be a conventional method, for example, a physical vapor deposition method (PVD method) such as a vacuum deposition method, a sputtering method, or an ion plating method, or a chemical vapor deposition method (CVD method) such as a plasma chemical vapor deposition method, a thermal chemical vapor deposition method, or a photochemical vapor deposition method.
[0112] (Barrier coat layer) When the printed matter has a barrier coat layer as a barrier layer, the barrier coat layer is formed by a barrier coating agent. The barrier coat layer is preferably adjacent to the substrate, intermediate substrate, sealant and / or printed layer. This can improve the oxygen barrier property and water vapor barrier property of the printed matter.
[0113] The barrier coating agent may be, for example, a barrier coating agent made of a resin alone, including gas barrier resins such as vinyl chloride-vinylidene chloride copolymer, vinyl acetate-vinylidene chloride copolymer, acrylate-vinylidene chloride copolymer, ethylene-vinyl alcohol copolymer (EVOH), polyvinyl alcohol, polyacrylonitrile, polyamide resin, polyester resin, urethane resin, and (meth)acrylic resin, as well as a barrier coating agent made of an inorganic layered compound and a resin, such as those described below.
[0114] The inorganic layered compound is, for example, a clay mineral such as a kaolinite group, a smectite group, or a mica group, and is a crystalline inorganic compound having a layered structure. The type, particle size, aspect ratio, etc. of these inorganic layered compounds are appropriately selected and are not particularly limited. Among them, the smectite group such as montmorillonite, hectorite, and saponite are suitable, and resin is easily incorporated between the layers of the inorganic layered compound to form a composite. In particular, among this group, montmorillonite has the best stability in a molten state and coatability.
[0115] In addition, the resin used in the barrier coating agent made of inorganic layered compound and resin is not particularly limited as long as it is easily incorporated between the layers of the inorganic layered compound, but it is preferable to use a water-soluble polymer. Examples of water-soluble polymers include polyvinyl alcohol (PVA), polyvinylpyrrolidone, starch, methyl cellulose, carboxymethyl cellulose, acrylic resin, and sodium alginate. In particular, the gas barrier property is most excellent when polyvinyl alcohol (PVA) is used.
[0116] The barrier coat layer may further comprise a composition containing a hydrolysis / polycondensation product of a metal alkoxide. This metal alkoxide is a compound represented by the following general formula, M(OR)n, where M is a metal, R is an alkyl group, and n is the coordination number of the alkoxy group. It is preferable that M is selected from the group consisting of Si, Ti, Ar, and Zr, and R is selected from a methyl group and an ethyl group. In particular, tetraethoxysilane [Si(OC 2 H 5 ) 4 〕, triisopropoxyaluminum [Al(O-2'-C 3 H 7 ) 3 ] is preferably used, since the hydrolysis product of the alkoxide is relatively stable in an aqueous solvent.
[0117] The above-mentioned components can be added to the barrier coating agent either alone or in combination. Furthermore, known additives such as an isocyanate compound, a silane coupling agent, a dispersant, a stabilizer, a viscosity adjuster, a colorant, etc. can be added within a range that does not impair the barrier properties of the barrier coating agent.
[0118] The barrier coat layer can be formed by dissolving or dispersing the above-mentioned material in water or a suitable solvent, applying the solution, and drying the solution. Alternatively, the barrier coat layer can be formed by applying a commercially available barrier coat agent and drying the solution.
[0119] The barrier coating agent can be applied by any of the commonly used conventional methods such as dipping, roll coating, screen printing, spraying, etc.
[0120] The thickness of the barrier coat layer is preferably 0.01 μm to 10 μm, more preferably 0.1 μm to 5 μm, and even more preferably 0.3 μm to 3 μm. By making the thickness of the barrier coat layer 0.01 μm or more, the oxygen barrier property and water vapor barrier property of the printed matter can be improved. By making the thickness of the barrier coat layer 10 μm or less, the foreign matter immediately after the start of extrusion of the recycled plastic and after continuous extrusion can be reduced, and further, the tensile strength is excellent.
[0121] <Chlorine content in printed matter> Due to halogen elements that may be contained in the printed matter, halogen gas or acidic gas, hydrogen chloride, may be generated during the production of recycled plastics, which may damage equipment or endanger human health. In addition, the generated gas may change the pressure in the cylinder, causing the extrusion amount and / or extrusion pressure to be unstable, resulting in irregular shapes and dimensions of the recycled plastics. If bubbles are generated during the production of recycled plastics, when the recycled plastics are used to produce molded products, the surface is likely to become uneven, which may deteriorate the surface condition of the molded products. Therefore, in the printed matter, the chlorine content is preferably 0.4% by mass or less, more preferably 0.2% by mass or less, and even more preferably 0.1% by mass or less, based on the total mass of the printed matter.
[0122] <Method for measuring chlorine content in printed matter> In the present invention, the chlorine content of the printed matter is measured in accordance with JIS K0127 (2013). In this measurement method, a sample pretreated by a combustion method is quantified by ion chromatography.
[0123] <Melt mass flow rate (MFR) of printed matter> The melt mass flow rate (MFR) of the printed matter is measured by crushing the printed matter into pieces with a side length of 5 mm to 10 mm. The MFR in the present invention is a value measured in accordance with JIS K7210 under conditions of a temperature of 190°C and a pressure of 2.6 kgf. The MFR of the printed matter is preferably 0.5 to 15 g / 10 min, more preferably 1.0 to 14 g / 10 min, and even more preferably 3 to 13 g / 10 min. When the MFR of the printed matter is within the above range, the fluidity in the heating, melting and kneading step is improved, and therefore the occurrence of scorching immediately after the start of extrusion and after continuous extrusion can be suppressed.
[0124] <Pigment content in printed matter> The content of the pigment in the printed matter is preferably 5% by mass or less, more preferably 3% by mass or less, and even more preferably 1.5% by mass or less, based on 100% by mass of the printed matter. When the content of the pigment in the printed matter is within the above range, the generation of foreign matter immediately after the start of extrusion of the recycled plastic and after continuous extrusion can be suppressed.
[0125] <Binder resin content in printed matter> The content of the binder resin in the printed matter is preferably 10% by mass or less, more preferably 7% by mass or less, and particularly preferably 5% by mass or less, based on 100% by mass of the printed matter. When the content of the binder resin in the printed matter is within the above range, the generation of foreign matter immediately after the start of extrusion of the recycled plastic and after continuous extrusion can be suppressed.
[0126] [Recycled plastics] Using the above-mentioned method for producing recycled plastic, recycled plastic can be obtained from printed matter. The recycled plastic may contain pigments and binder resins derived from the printed layer. It may also contain additives added in the heat-melt-kneading process.
[0127] <Pigment content in recycled plastics> The content of the pigment in the recycled plastic is preferably 5% by mass or less, more preferably 3% by mass or less, and even more preferably 1.5% by mass or less, based on 100% by mass of the recycled plastic. When the content of the pigment in the recycled plastic is within the above range, the generation of foreign matter immediately after the start of extrusion of the recycled plastic and after continuous extrusion can be suppressed.
[0128] <Binder resin content in recycled plastics> The content of the binder resin in the recycled plastic is preferably 10% by mass or less, more preferably 7% by mass or less, and particularly preferably 5% by mass or less, based on 100% by mass of the recycled plastic. When the content of the binder resin in the recycled plastic is within the above range, the generation of foreign matter immediately after the start of extrusion of the recycled plastic and after continuous extrusion can be suppressed.
[0129] <Content of antioxidants in recycled plastics> The content of the antioxidant in the recycled plastic is preferably 0.01 to 5 mass%, more preferably 0.01 to 3 mass%, further preferably 0.05 to 1 mass%, and particularly preferably 0.1 to 0.5 mass%, based on 100 mass% of the recycled plastic. When the content of the antioxidant in the recycled plastic is within the above range, the occurrence of scorching immediately after the start of extrusion of the recycled plastic and after continuous extrusion can be suppressed.
[0130] <Compatibilizer content in recycled plastics> The content of the compatibilizer in the recycled plastic is preferably 0.01 to 3 mass%, and more preferably 0.05 to 0.5 mass%, based on 100 mass% of the recycled plastic. When the content of the compatibilizer in the recycled plastic is within the above range, the occurrence of burns immediately after the start of extrusion of the recycled plastic and after continuous extrusion can be suppressed.
[0131] <Melt mass flow rate (MFR) of recycled plastics> The melt mass flow rate (MFR) of the recycled plastic is greatly affected by the thermal history such as the temperature during molding and the cooling speed. The melt mass flow rate (MFR) of the recycled plastic is preferably 0.5 to 20 g / 10 min, more preferably 3 to 15 g / 10 min, depending on the composition of the printed matter and the recycling method. When the melt mass flow rate (MFR) of the recycled plastic is within the above range, the occurrence of burns immediately after the start of extrusion and after continuous extrusion can be suppressed, and the method is further suitable for various moldings. The manufacturing method of the present invention preferably includes a step of adjusting the melt mass flow rate (MFR) of the recycled plastic by changing the thermal history. The measurement of the melt mass flow rate (MFR) of the recycled plastic is performed in the same manner as the measurement of the melt mass flow rate (MFR) of the printed matter described above.
[0132] <Molded products> Molded products can be obtained by molding the recycled plastic obtained by the present invention. The molding method is not particularly limited, and examples thereof include injection molding, extrusion molding, blow molding, and compression molding. Molded products can be used for various purposes such as home appliances, stationery, automobile parts, toys, sporting goods, medical supplies, and building and construction materials.
[0133] <Film molding> The obtained recycled plastic can be, for example, heated and melted, extruded using a slit-shaped device called a T-die, molded into a film, and then cooled and solidified with a cooling roll to obtain a film molded product. The heat-melting temperature is preferably 100 to 210° C. The thickness of the film molded product is preferably 10 to 300 μm. EXAMPLES
[0134] The present invention will be described in detail below with reference to examples, but the present invention is not limited to these examples. In the present invention, parts and % represent parts by mass and % by mass unless otherwise noted.
[0135] (Hydroxyl value) The hydroxyl value is the number of milligrams of potassium hydroxide required to neutralize acetic acid bonded to hydroxyl groups when 1 g of a sample is acetylated, and was measured by the method described in JIS K 0070.
[0136] (Acid value) The acid value is the number of milligrams of potassium hydroxide required to neutralize the free fatty acids, resin acids, etc. contained in 1 g of a sample, and was measured by the method described in JIS K 0070.
[0137] (amine value) The amine value is the amount of potassium hydroxide in mg equivalent to the amount of hydrochloric acid required to neutralize the amino groups contained in 1 g of sample, and was measured in accordance with JIS K 0070. 0.5 to 2 g of sample was precisely weighed out (sample solid content: Sg), and 50 mL of a mixed solution of methanol / methyl ethyl ketone = 60 / 40 (mass ratio) was added to the precisely weighed sample to dissolve it. Bromophenol blue was added as an indicator to the resulting solution, and the resulting solution was titrated with a 0.2 mol / L ethanolic hydrochloric acid solution (titer: f). The point at which the color of the solution changed from green to yellow was set as the end point, and the titration amount (AmL) at this point was used to calculate the amine value according to the following formula. (Formula) Amine value = (A x f x 0.2 x 56.108) / S [mgKOH / g]
[0138] (mass average molecular weight) The weight average molecular weight was determined by measuring the molecular weight distribution using a gel permeation chromatography (GPC) device (HLC-8220 manufactured by Tosoh Corporation) and calculating the molecular weight converted using polystyrene as a standard substance. The measurement conditions are shown below. Columns: The following columns were used in series connection: Tosoh Corporation TSKgel Super AW2500 Tosoh Corporation TSKgel Super AW3000 Tosoh Corporation TSKgel Super AW4000 Tosoh Corporation's TSK gelguard column Super AWH Detector: RI (differential refractometer) Measurement conditions: Column temperature 40℃ Eluent: Tetrahydrofuran Flow rate: 1.0mL / min
[0139] (Glass transition temperature (Tg)) The glass transition temperature was determined by differential scanning calorimetry (DSC). The measurement was performed using a Rigaku Corporation DSC8231 with a measurement temperature range of -70 to 250°C and a heating rate of 10°C / min. The midpoint (inflection point) of the baseline shift due to the glass transition in the DSC curve was taken as the glass transition point.
[0140] (Chlorine content) The chlorine content was measured in accordance with JIS K0127 (2013). On a transparent substrate, the ink or binder resin was applied to a thickness of 2.0 μm to form a coating film, which was then dried at 80°C and 0.5 g of the coating film was scraped off. The scraped off coating film was pretreated by the combustion method, and the chlorine content of the obtained sample was quantified by ion chromatography (Shimadzu Corporation LC-20ADsp) to determine the chlorine content. The chlorine content of the printed matter was determined in the same manner as above, except that 0.5 g of the printed matter was cut out and pretreated by the combustion method and used as the sample.
[0141] (Melt Mass Flow Rate (MFR) Measurement) The MFR was measured at a temperature of 190°C and a pressure of 2.6 kgf according to the method described in JIS K 7210-1: 2014. The MFR of the printed matter was measured by crushing it so that the side length was 5 mm to 10 mm.
[0142] (Moisture content measurement method) The moisture content was measured in accordance with JIS K 0068 (2001). The measuring equipment and reagents are shown below. Measuring equipment: Karl Fischer moisture meter MKC-710D (Kyoto Electronics Manufacturing Co., Ltd.) : Moisture vaporizer ADP-611 (Kyoto Electronics Manufacturing Co., Ltd.) Karl Fischer reagent: ChemAqua Water Standard 1 (Kyoto Electronics Manufacturing Co., Ltd.)
[0143] (Calculation of polyolefin resin (A) content) The content of polyolefin resin (A) in the printed matter was calculated using the following formula. Formula: (Mass of polyolefin resin (A) in printed matter) / (Mass of printed matter) x 100 More specifically, the following formula was applied: Formula: 1m of print 2 Resin mass per [g] = (substrate thickness) x (substrate density) + (coating weight of barrier layer) + (coating weight of printing layer) + (coating weight of heat seal layer) Formula: Mass [g] of polyolefin resin (A) in printed matter = (substrate thickness) x (substrate density) + (coating amount of heat seal layer) x (polyolefin ratio in heat seal layer) Formula: Polyolefin resin (A) content in printed matter [%] = (mass of polyolefin resin in printed matter) / (1 m 2 (mass per unit) x 100 In addition, if the printed matter has a layer not described above, such as a barrier layer, the coating amount and polyolefin ratio of the corresponding layer can be added to the calculation formula.
[0144] The substrate thickness and substrate density used in the examples are as follows. Corona-treated biaxially oriented polypropylene (OPP) film (thickness 40 μm) Density: 0.91 g / cm 3 Corona-treated biaxially oriented polypropylene (OPP) film (thickness 60 μm) Density: 0.91 g / cm 3 High density polyethylene film (HDPE) film (thickness 40μm) Density: 0.94g / cm 3 Linear low density polyethylene (LLDPE) film (thickness 150μm) Density: 0.91g / cm 3 Nylon (NY) film (thickness 15 μm) Density: 1.15 g / cm 3
[0145] (Resin synthesis) <Synthesis Example 1> Urethane resin PU1 A condensation product of 3-methyl-1,5-pentanediol (MPD) and sebacic acid (SA), a polyester polyol having a number average molecular weight of 2,000 (hereinafter referred to as "MPD / SA"), 100 parts of 1,4-butanediol (hereinafter referred to as "1,4-BD"), 28.5 parts of isophorone diisocyanate (hereinafter referred to as "IPDI"), and 32.1 parts of ethyl acetate were mixed and reacted at 90°C for 5 hours under a nitrogen atmosphere to obtain a urethane prepolymer with a terminal isocyanate. Next, 11.0 parts of isophoronediamine (hereinafter referred to as "IPDA"), 1.0 part of N-(2-aminoethyl)ethanolamine (hereinafter referred to as "AEA"), 1.0 part of dibutylamine (hereinafter referred to as "DBA"), and 298.1 parts of mixed solvent 1 (ethyl acetate / isopropanol = 70 / 30 (mass ratio)) were stirred and mixed, and the obtained urethane prepolymer with terminal isocyanate was gradually added at 40°C. The reaction was carried out at 80° C. for 1 hour to obtain a solution of urethane resin PU1 having a solid content of 30 mass %, an amine value of 6.5 mg KOH / g, a hydroxyl value of 3.8 mg KOH / g, and a mass average molecular weight of 50,000. The chlorine content of urethane resin PU1 was 0 mass %.
[0146] <Preparation Example 1> Preparation of heat sealant HS1 91.7 parts of acrylic resin emulsion AC1 (JONCRYL PDX7356 manufactured by BASF, acid value: 78 mgKOH / g, glass transition temperature: 25°C, solid content: 50%), 8.2 parts of a water / isopropyl alcohol mixed solvent (mass ratio 1:1), and 0.1 part of BYK-024 (antifoaming agent manufactured by BYK) were added and mixed with stirring to obtain a heat sealing agent HS1. <Preparation Examples 2-4> Preparation of heat sealant HS2-4 Heat sealing agents HS2 to HS4 were obtained in the same manner as in Preparation Example 1, except that the raw materials and compounding ratios shown in Table 1 were used. The properties of the raw materials used are as follows. Polyethylene resin emulsion PE1 (Mitsui Chemicals, Chemipearl S500, ionomer resin, solid content: 50%) Ethylene-vinyl acetate copolymer resin emulsion EVA1 (Sumitomo Chemical Co., Ltd., Sumikaflex S-400HQ, minimum film-forming temperature: 0°C, glass transition temperature: 0°C, vinyl alcohol resin emulsifier, solid content: 50%) Polylactic acid resin emulsion PL1 (Miyoshi Oil Co., Ltd., PL-3000, solid content 50%)
[0147] [Table 1]
[0148] <Preparation Example 5> Printing ink Y1 40 parts of urethane resin PU1 solution, 15 parts of polyvinyl butyral resin (PVB) solution, 5 parts of CI pigment blue 15:3 (manufactured by Toyo Color Co., Ltd., product name: LIONOL BLUE FG-7330, chlorine content 0% by mass, nitrification degree 0% by mass), silica particles (hydrophilic silica, average particle diameter 3.0 μm, specific surface area 300 m 2 A pigment dispersion was obtained by mixing 0.8 parts of ethyl acetate / g) and 33.4 parts of a mixed solvent of n-propyl acetate / isopropanol = 70 / 30 (mass ratio) and dispersing for 20 minutes with a bead mill. The resulting pigment dispersion was mixed with 0.8 parts of chlorinated polypropylene solution, 3.5 parts of propylene glycol monomethyl ether, and 1.5 parts of water and stirred to obtain printing ink Y1.
[0149] <Preparation Examples 6 and 7, Comparative Preparation Example 1> Printing inks Y2 to 4 Printing inks Y2 to Y4 were obtained in the same manner as in Preparation Example 5, except that the raw materials and blending ratios shown in Table 2 were used. The properties of the raw materials used are as follows. PVB solution: A 30% solids solution of polyvinyl butyral resin (glass transition point 70°C, mass average molecular weight 50,000, chlorine content 0 mass%, nitration degree 0 mass%) having vinyl alcohol units, vinyl acetate units, and vinyl butyral units and containing 73 mass% butyral ring groups in a 1 / 1 ethyl acetate / isopropanol mixed solvent. Vinyl chloride-vinyl acetate solution: Vinyl chloride-vinyl acetate copolymer resin (manufactured by Nissin Chemical Co., Ltd.) Rubain TA3, chlorine content 47.1% by mass, nitrification degree 0% by mass, 30% solids in ethyl acetate solution Chlorinated polypropylene solution: solids 30%, chlorine content in solids 30%, solvent: ethyl acetate
[0150] [Table 2]
[0151] <Preparation Example 8> Preparation of nitrocellulose resin solution NC1 59.6 parts of nitrocellulose nc1 (NV.70% (solvent: isopropyl alcohol), mass average molecular weight: 10,000, viscosity at 25% solution concentration: 2 seconds, glass transition temperature: 155°C) was mixed and dissolved in 33.6 parts of ethyl acetate and 33.6 parts of isopropyl alcohol to obtain a nitrocellulose resin solution (NC1) with a solid content of 30%.
[0152] <Preparation Example 9> Preparation of polyamide resin solution PA1 30 parts of polyamide resin pa1 (manufactured by Tsuno Foods Co., Ltd., product name Vegichem Green 725, NV. 100%, glass transition temperature 50°C, mass average molecular weight 8,000) and 70 parts of isopropyl alcohol were charged and dissolved at 50°C for 2 hours under a nitrogen stream to obtain a polyamide resin solution (PA1) with a solid content of 30%.
[0153] Preparation Example 10: Preparation of overcoat agent Z1 13.5 parts of nitrocellulose resin solution NC1, 52.1 parts of polyamide resin solution PA1, 1.9 parts of diethylene glycol monobutyl ether, 3 parts of hexamethylenbisoleic acid amide, 8.3 parts of polyethylene wax, 14 parts of ethyl acetate / propyl acetate / isopropanol mixed solvent (mass ratio=1 / 1 / 1), 6.3 parts of methylcyclohexane / methylpropylene glycol mixed solvent (mass ratio=1 / 1), and 0.9 parts of water were stirred and mixed to obtain overcoat agent Z1.
[0154] <Preparation Example 11> Preparation of Barrier Coating Agent V1 6 parts of polyvinyl alcohol resin PVA1 (manufactured by Kuraray, Exeval AQ-4104, ethylene vinyl alcohol resin, ethylene content: 6 mol%, solid mass %=100%) and 92 parts of mixed solvent (water / IPA=8 / 2) were heated with stirring, and the heating and stirring were continued at 95°C for 1 hour, after which the heating was stopped and the stirring was continued until the temperature returned to normal, to obtain an aqueous solution of polyvinyl alcohol resin PVA1. Montmorillonite (swelling, average particle size: 2 μm, aspect ratio: 500, specific surface area: 13.1 m) was added to the aqueous solution of polyvinyl alcohol resin PVA1. 2 / g, particle thickness: 1 nm, particle spread: 500 nm, solids mass %=100%) were added and mixed and stirred to obtain barrier coating agent V1.
[0155] (Example of printed matter production) <Manufacturing example 1> Printed matter A1 A heat seal layer was formed by printing the heat sealant HS1 twice over the entire surface of the corona-treated surface of the substrate, a corona-treated biaxially oriented polypropylene (OPP) film (thickness 40 μm), using a gravure printing machine equipped with a gravure plate with a plate depth of 50 μm, at a printing speed of 50 m / min and an in-line oven temperature of 70°C, to obtain an intermediate printed matter a1 having a heat seal layer / substrate structure. Next, the printing ink Y1 and the overcoat agent Z1 were diluted with a mixed solvent of ethyl acetate:isopropyl alcohol = 7:3 (mass ratio) and the viscosity was adjusted to 15 seconds in Zahn cup #3 (Rigo Co., Ltd.) at 25 ° C. In addition, the barrier coat agent V1 was diluted with a mixed solvent of water:isopropyl alcohol = 1:1 (mass ratio) and the viscosity was adjusted to 16 seconds in Zahn cup #3 (Rigo Co., Ltd.) at 25 ° C. A barrier layer was formed by printing diluted barrier coating agent V1 twice on the surface of the intermediate printed matter a1 opposite to the heat seal layer of the substrate using a gravure printing machine equipped with a gravure plate having a plate depth of 30 μm under conditions of a printing speed of 50 m / min and an in-line oven temperature of 60° C., and then a printed layer was formed by printing diluted printing ink Y1 on the barrier layer under conditions of a printing speed of 50 m / min and an in-line oven temperature of 60° C. Next, an overcoat agent Z1 was printed on the printed layer using a gravure printing machine equipped with a gravure plate having a plate depth of 30 μm under conditions of a printing speed of 50 m / min and an in-line oven temperature of 60° C., to obtain a printed matter A1 having a configuration of heat seal layer / barrier layer / substrate / printed layer / surface protective layer.
[0156] <Production Examples 2-11, Comparative Production Examples 1-3> Printed matter A2-14 Printed matters A2 to A15 were obtained in the same manner as in Production Example 1, except that the raw materials and layer structures were changed as shown in Table 3.
[0157] [Table 3]
[0158] (Manufacturing of recycled plastics) <Example 1> {Production of recycled plastics B1 and BB1} 100 kg of A1-sized printed matter was crushed into pieces of 2 cm x 2 cm using a cutter mill (U-210, manufactured by Nishimura Machinery Works), washed with water, and then dehydrated in a centrifugal dehydrator (YDK-FS, manufactured by Iwatsuki Machinery Works) and further dried with hot air until the moisture content was 0.5%. The printed matter A1 obtained through the above process, Irganox 1010 (phenolic antioxidant), and Umex 1010 (maleic anhydride modified polypropylene compatibilizer) were fed into a twin-screw extruder (manufactured by Japan Steel Works, Ltd., screw diameter: 34 mm, minimum gap distance between the cylinder inner wall and the screw: 0.4 mm) and melted and kneaded for 30 seconds at a screw rotation speed of 200 rpm, 230°C, and an extrusion flow rate of 20 kg / h. The amount of Irganox 1010 added to the printed matter A1, which was 100% by mass, was adjusted to 0.2% by mass. The amount of Eumex 1010 added to the printed matter A1, which was 100% by mass, was adjusted to 0.15% by mass.
[0159] Then, the resin composition was extruded from the discharge part of the extrusion device using a 120 mesh screen. The pressure of the discharge part immediately after the start of extrusion was 2 MPa. The extruded resin composition was immediately cut with a pelletizer and cooled by immersing it in cold water. In this way, a pellet-shaped recycled plastic B1 was obtained, which was recycled from the printed matter A1. After obtaining the recycled plastic B1, the operation was continued for 5 hours (long run) under the manufacturing conditions of the recycled plastic B1, and the extruded resin composition after 5 hours was immediately cut with a pelletizer and cooled by immersing it in cold water. The pressure at the discharge part after 5 hours of continuous extrusion was 4 MPa. In this way, the recycled plastic BB1 in the form of pellets, which was recycled in a long run from the printed matter A1, was obtained.
[0160] <Examples 2 to 24, Comparative Examples 1 to 4> Recycled plastics B2 to B28, BB2 to 28 Recycled plastics B2 to B27 and BB2 to BB27 were obtained in the same manufacturing process as recycled plastics B1 and BB1, respectively, according to the raw materials and conditions shown in Table 5. The raw materials used are as follows. Irganox1010: Phenolic antioxidant (manufactured by BASF) Irgafos168: Phosphate-based antioxidant (manufactured by BASF) · Irganox PS 800FL: Sulfur-based antioxidant (manufactured by BASF) Nolac CD: Amine-based antioxidant (manufactured by Ouchi Shinko Chemical Industry Co., Ltd.) UMEX 1001: Maleic anhydride modified polypropylene compatibilizer (manufactured by Sanyo Chemical Industries, melting point: 142°C) Bondfast E: Ethylene-glycidyl methacrylate copolymer compatibilizer (Sumitomo Chemical Co., Ltd., melting point: 103°C) Bondfast-7L: Ethylene-glycidyl methacrylate copolymer compatibilizer (Sumitomo Chemical Co., Ltd., melting point: 60°C) Bondfast-7M: Ethylene-glycidyl methacrylate copolymer compatibilizer (Sumitomo Chemical Co., Ltd., melting point: 52°C) In addition, the rotation speed of 1100 rpm is equivalent to a shear rate of 4900 sec -1 It is.
[0161] [Evaluation of recycled plastics] The pellet-shaped recycled plastics obtained in the above Examples and Comparative Examples were extrusion-molded at 230° C. using a T-die extruder to produce a film-shaped molded product having a thickness of 50 μm. The following evaluations were performed using the film-shaped molded product. <Foreign matter evaluation> The obtained film-like molded product was cut into 0.5 m 2 The number of foreign particles (approximately 100 μm or larger) that could be detected by visual inspection was counted and evaluated according to the following criteria. The evaluation results are shown in Table 4. Note that A, B, and C are ranges that are acceptable for practical use. A (Good): The number of foreign objects is less than 50. B (Acceptable): The number of foreign objects is between 50 and 100. C (Acceptable): The number of foreign objects is between 100 and 200. D (defective): 200 or more foreign objects
[0162] <Burst rating> The film-like molded product thus obtained was evaluated for visually discernible fading according to the following criteria. The evaluation results are shown in Table 4. Note that A, B, and C are within the ranges where no practical problems occur. A (Good): No marks (no color change) B (Fair): Slightly scorched (some areas have turned light brown) C (Fair): Burns are visible (light brown discoloration is visible in multiple areas or overall) D (Poor): Many burns are observed (black or brown foreign objects or discolored areas are observed)
[0163] <Tensile strength evaluation> The obtained film-like molded product was cut into a width of 10 mm and a length of 160 mm, and measured using a tensile tester (manufactured by Toyo Seiki Seisakusho) in accordance with a method conforming to JIS K7127:1999, and evaluated according to the following criteria. The evaluation results are shown in Table 4. Note that A, B, and C are ranges that are acceptable for practical use. Tensile strength test conditions Tensile speed: 300 mm / min, Tensile direction: Length direction Tensile strength evaluation criteria A: Tensile strength is 5MPa or more B: Tensile strength is 3MPa or more and less than 5MPa C: Tensile strength is 1MPa or more and less than 3MPa D: Tensile strength is less than 1 MPa
[0164] [Table 4]
[0165] From the above results, in Comparative Example 1, the pressure from the discharge part of the extrusion device exceeded 18 MPa, so the evaluation of the burn after continuous extrusion was poor. In Comparative Example 2, since it did not include a heat seal layer, the evaluation of the foreign matter and the evaluation of the burn after continuous extrusion were poor. In Comparative Example 3, the chlorine content in the printed matter exceeded 0.4 mass% of the total mass of the printed matter, so the tensile strength was poor. In Comparative Example 4, the olefin content in the printed matter was less than 80 mass% of the total mass of the printed matter, so the evaluation of the foreign matter immediately after the start of extrusion and the tensile strength, as well as the evaluation of the foreign matter after continuous extrusion were poor. On the other hand, in the examples, the printed matter includes a heat seal layer, a substrate and a printing layer, the chlorine content in the printed matter is 0.4 mass% or less of the total mass of the printed matter, the olefin content in the printed matter is 80 mass% or more of the total mass of the printed matter, and the pressure from the discharge part of the extrusion device is 18 MPa or less, so that a recycled plastic having excellent tensile strength and little foreign matter and discoloration immediately after the start of extrusion and after continuous extrusion could be obtained.
Claims
1. A method for producing recycled plastic, comprising the steps of: obtaining recycled plastic from a printed matter using an extrusion device having a first screw and a discharge portion; The printed matter includes a heat seal layer, a substrate, and a printing layer, The printed matter has not been subjected to a detachment step in which the substrate and the printing layer are detached, The chlorine content of the printed matter is 0.4% by mass or less based on the total mass, The printed matter contains a polyolefin resin (A) in an amount of 80 mass% or more based on the total mass of the printed matter, A heating, melting and kneading step of heating, melting and kneading the printed matter in the extrusion device to obtain a resin composition (D); and A method for producing recycled plastic, comprising an extrusion step of extruding the resin composition (D) from a discharge portion of an extrusion device at a pressure of 18 MPa or less.
2. The method for producing recycled plastics according to claim 1 , wherein the heat seal layer contains a polyolefin resin (B) and / or an acrylic resin.
3. The method for producing recycled plastic according to claim 2, wherein the polyolefin resin (B) contains an ethylene-vinyl acetate copolymer resin and / or a polyethylene resin (except for the ethylene-vinyl acetate copolymer resin).
4. The method for producing recycled plastics according to claim 1 or 2, wherein the polyolefin resin (A) contains a polyethylene resin and / or a polypropylene resin.
5. The method for producing recycled plastic according to claim 1 or 2, wherein the printed matter further comprises a barrier layer.
6. The method for producing recycled plastic according to claim 5, wherein the barrier layer is a vapor deposition layer including a vapor deposition film, or a barrier coat layer.
7. The method for producing recycled plastics according to claim 1 or 2, wherein the printed matter further has a surface protective layer on the printed layer.
8. The method for producing recycled plastic according to claim 1 or 2, wherein the printed layer contains a pigment and a binder resin, and the chlorine content of the binder resin is 5% by mass or less.
9. The method for producing recycled plastics according to claim 1 or 2, wherein the heating, melting and kneading step is carried out in the presence of an antioxidant.
10. The method for producing recycled plastic according to claim 1 or 2, wherein the heating, melting and kneading step is carried out in the presence of a compatibilizer.
11. The method for producing recycled plastic according to claim 1 or 2, wherein the heating and melting temperature in the heating and melting kneading step is 120 to 280°C.
12. The method for producing recycled plastic according to claim 1 or 2, wherein the rotation speed of the first screw of the extrusion device is 50 to 1000 rpm.
13. A method for producing a molded product of recycled plastic, produced by the method for producing recycled plastic according to claim 1 or 2.
Citation Information
Patent Citations
Ink remover for recycling plastic laminate into recycled materials, ink film separation / removal method, and method of isolating and recovering separated or removed ink film
WO2021230032A1