SUBSTRATE FOR SiC SEMICONDUCTOR DEVICE, SiC JOINT SUBSTRATE, SiC POLYCRYSTALLINE SUBSTRATE, AND MANUFACTURING METHOD OF SiC POLYCRYSTALLINE SUBSTRATE
By laminating SiC polycrystalline and single-crystal substrates and applying a heat treatment with a straightening jig to correct warpage, the method addresses warpage issues in SiC semiconductor devices, improving manufacturing efficiency and reducing costs.
Patent Information
- Application Number
- JP2023086412
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-05-25
- Publication Date
- 2024-12-05
- Estimated Expiration
- 2043-05-25
AI Technical Summary
SiC semiconductor devices face challenges due to warpage issues during back grinding, which can lead to transportation errors and processing difficulties, particularly in bonded substrates combining polycrystalline and single-crystal SiC substrates, affecting manufacturing efficiency and cost.
A method involving the lamination of a SiC polycrystalline substrate and a SiC single crystal substrate, with a heat treatment process to correct warpage, followed by back grinding to achieve a warpage of 0.17 mm/inch or less, using a combination of a straightening jig, ring-shaped jig, and weight to apply opposing force during heat treatment.
The method effectively reduces warpage to manageable levels, preventing transportation and processing errors, enhancing manufacturing efficiency and reducing costs by maintaining substrate flatness during back grinding.
Smart Images

Figure 2024169169000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a silicon carbide (hereinafter sometimes referred to as "SiC") polycrystalline substrate and a manufacturing method thereof, a SiC bonded substrate obtained by bonding a SiC single crystal substrate to a SiC polycrystalline substrate, and a substrate for a SiC semiconductor device in which a SiC single crystal epitaxial layer and a semiconductor circuit are formed on the SiC bonded substrate. [Background technology]
[0002] SiC is a wide band gap semiconductor with a wide band gap of 2.2 to 3.3 eV, and due to its excellent physical and chemical properties, it has been researched and developed as an environmentally resistant semiconductor material. In recent years, SiC has attracted attention as a material for power devices such as high-voltage, high-output electronic devices and high-frequency electronic devices, and short-wavelength optical devices from blue to ultraviolet, and research and development into it has become more active. However, it is difficult to manufacture high-quality large-diameter single crystals of SiC, which has hindered the practical use of SiC devices.
[0003] To solve this problem, an improved Lely process has been developed, which uses a SiC single crystal substrate as a seed crystal and performs sublimation recrystallization. Using this improved Lely process, it is possible to grow SiC single crystals while controlling the crystal polytype (4H-SiC, 6H-SiC, 15R-SiC, etc.), carrier type, and impurity concentration of the SiC single crystal. This technology has significantly reduced the crystal defect density, and has led to the practical application of Schottky barrier diodes (SBDs) and field effect transistors (MOSFETs) on the substrate.
[0004] However, in the improved Lely process, which uses a SiC single crystal substrate as a seed crystal, the manufacturing cost of single crystal SiC substrates is high due to the slow crystal growth rate and the high processing costs involved in processing the SiC single crystal ingot into wafers through processes that mainly consist of cutting and polishing. This high manufacturing cost has also been a factor that has hindered the practical application of SiC devices, and there has been a strong demand for the development of technology that can provide inexpensive SiC substrates for semiconductor device applications, especially for high-voltage, high-power electronic elements.
[0005] Therefore, a technology has been provided for manufacturing a semiconductor substrate (hereinafter, sometimes referred to as a "SiC bonded substrate") that combines a low-cost support substrate portion and high-quality single-crystal SiC by using high-quality single-crystal SiC only for the device formation layer portion and fixing it to a support substrate (a material having strength, heat resistance, and cleanliness that can withstand the device manufacturing process: for example, polycrystalline SiC) using a bonding method that does not involve the formation of an oxide film at the bonding interface (see, for example, Patent Document 1). In particular, a SiC bonded substrate using polycrystalline SiC as a support substrate is advantageous over a single-crystal SiC substrate in that it is possible to reduce manufacturing costs while taking advantage of the characteristics of single-crystal SiC when applied to power devices. As single-crystal SiC substrates become more widespread, attention is being paid to SiC bonded substrates that can be manufactured more inexpensively.
[0006] On the other hand, problems related to the "warping" of the substrate in the manufacturing process of devices using single crystal SiC substrates have also become apparent. In general, the "warping" of the substrate is considered very important in the manufacturing process of devices. This is because a substrate with a large warp may cause errors in automatic transport in the manufacturing process of devices or problems in which the substrate cannot be held on the processing table. In addition, even if the substrate can be held on the processing table due to a large warp of the substrate, sufficient flatness cannot be ensured, and for example, in the exposure process (lithography process), a part of the substrate surface is out of focus and a clear mask image cannot be formed. The effect of this defocus phenomenon is greater the finer the circuit. It is also a cause for concern about a decrease in yield in the dicing and package assembly processes. In response to this, for example, according to Patent Document 2, a single crystal SiC substrate is provided that has a surface in which processing damage has been removed from the front and back of the substrate by CMP or diamond polishing, and that has small warping of the substrate, which is explained by the distortion and residual stress obtained by Raman spectroscopy and X-ray method. Moreover, Patent Document 3 provides a polycrystalline SiC molded body with small warpage, which is explained by the residual stress value measured by the X-ray method. [Prior art documents] [Patent documents]
[0007] [Patent Document 1] JP 2015-15401 A [Patent Document 2] JP 2015-59073 A [Patent Document 3] Patent Publication No. 2021-54666 Summary of the Invention [Problem to be solved by the invention]
[0008] The warpage of the substrate also occurs during thinning processing after mounting a surface circuit pattern in the manufacturing process of a vertical power device in which the current flow direction is the thickness direction of the substrate, for example, back grinding (BG) processing. In this thinning processing process, it is necessary to remove about 40 to 60% of the original substrate thickness. For example, in a 6-inch diameter SiC single crystal substrate, the thickness after thinning processing by grinding is about 150 μm to 200 μm compared to the plate thickness of 350 μm, so the amount of grinding is large, and grinding processing with high processing efficiency is generally adopted. In a substrate for a semiconductor device using a SiC single crystal substrate that is not bonded, the warpage of the substrate is suppressed to about 1 mm or less, and no problems due to the above-mentioned warpage occur. In contrast, in the case of a SiC bonded substrate in which a SiC polycrystalline substrate and a SiC single crystal substrate are bonded, the warpage after back grinding exceeds 1 mm, and there is a risk of problems due to the warpage occurring in the subsequent process, such as a transport error or a problem in which the substrate cannot be held on the processing table. In particular, when the amount of back grinding exceeds the thickness of the substrate, the amount of warping becomes extremely large. This is thought to be because the substrate becomes thinner, the rigidity of the substrate itself becomes smaller, and the balance of internal stresses becomes lost.
[0009] This warping during back grinding occurs when a processing damage layer is generated on the back of the substrate by the grinding process, and the difference in the state of the processed surfaces on the front and back of the substrate causes the Twyman effect, resulting in large warping of the substrate. On the other hand, chemical mechanical polishing (CMP), which does not involve a processing damage layer, is less likely to cause large warping of the substrate, but the polishing speed is extremely slow, about 1 / 100, compared to grinding, and it is expensive. For this reason, back grinding is essential to thin the substrate, rather than polishing.
[0010] Therefore, from the standpoint of cost and manufacturing efficiency, if it were possible to provide a substrate that is less likely to warp during backgrinding, assuming that only backgrinding would be used for thinning, the process window for grinding that can achieve the desired processed state would be widened, making it easier to optimize the backgrinding design in the device manufacturing process.
[0011] The present invention has been made in view of these problems, and has an object to provide a SiC substrate for a semiconductor device, a SiC bonded substrate, a SiC polycrystalline substrate, and a method for manufacturing a SiC polycrystalline substrate, which are capable of sufficiently suppressing the amount of warping of the substrate after backside grinding in a substrate for a SiC semiconductor device having a structure in which a SiC polycrystalline substrate and a SiC single crystal substrate are bonded together. [Means for solving the problem]
[0012] In order to solve the above problems, the substrate for a SiC semiconductor device of the present invention is a substrate for a SiC semiconductor device which is formed by stacking, in this order, a support substrate made of SiC polycrystal, a SiC single crystal substrate bonded to a surface of the support substrate, a SiC single crystal epitaxial layer formed on the surface of the SiC single crystal substrate, and components of a semiconductor element formed on the SiC single crystal epitaxial layer, wherein a surface of the support substrate which is not bonded to the SiC single crystal substrate is a ground surface, and the amount of warping of the ground surface relative to the diameter of the ground surface is 0.17 mm / inch or less.
[0013] In order to solve the above problems, the SiC bonded substrate of the present invention is a SiC bonded substrate comprising a support substrate made of SiC polycrystal and a SiC single crystal substrate bonded to a surface of the support substrate, the surface of the support substrate not bonded to the SiC single crystal substrate is back-ground to remove 40 to 60% of the thickness of the support substrate to form a ground surface, and the amount of warping of the ground surface relative to the diameter of the ground surface is 0.17 mm / inch or less.
[0014] In order to solve the above problems, the SiC polycrystalline substrate of the present invention is a SiC bonded substrate having a stack of a support substrate made of SiC polycrystal and a SiC single crystal substrate bonded to a surface of the support substrate, the support substrate being used as the SiC polycrystalline substrate, wherein a surface of the support substrate that is not bonded to the SiC single crystal substrate is back-ground to grind the thickness of the support substrate by 40 to 60% to form a ground surface, and the amount of warping of the ground surface relative to the diameter of the ground surface is 0.17 mm / inch or less.
[0015] In order to solve the above problems, the present invention provides a method for manufacturing a SiC polycrystalline substrate, in which a support substrate made of SiC polycrystal and a SiC single crystal substrate bonded to a surface of the support substrate are stacked together to form a SiC bonded substrate, the method comprising the steps of: forming a SiC polycrystalline film on a seed substrate; separating the seed substrate and the SiC polycrystalline film after the film forming step; heat treating the SiC polycrystalline film by holding the film at a temperature of 1600°C or higher but lower than 2000°C after the separation step; and grinding and polishing the SiC polycrystalline film to process it into the support substrate after the heat treatment step, wherein the heat treatment step involves maintaining the SiC polycrystalline film in a warped state opposite to the warp of the SiC polycrystalline film. Effect of the Invention
[0016] According to the present invention, it is possible to provide a SiC substrate for a semiconductor device, a SiC bonded substrate, a SiC polycrystalline substrate, and a method for manufacturing a SiC polycrystalline substrate, which are capable of sufficiently suppressing the amount of warping of the substrate after backside grinding in a SiC substrate for a semiconductor device having a structure in which a SiC polycrystalline substrate and a SiC single crystal substrate are bonded together. [Brief description of the drawings]
[0017] [Figure 1] FIG. 1 is a schematic perspective view of a SiC polycrystalline substrate. [Diagram 2] FIG. 1 is a schematic perspective view of a SiC bonded substrate. [Diagram 3] FIG. 1 is a schematic cross-sectional view of a substrate for a SiC semiconductor device. [Figure 4] 1 is a schematic cross-sectional view of a MOSFET, which is an example of a SiC semiconductor device. [Diagram 5] 1 is a flowchart showing an example of a method for manufacturing a support substrate and a SiC bonded substrate. [Figure 6] 1 is a flowchart showing an example of a method for manufacturing a SiC semiconductor device. [Figure 7] 1 is a schematic side view showing a method for correcting warpage of a SiC polycrystalline film 100. FIG. [Figure 8] 8 is a schematic side view showing a method for correcting warpage of a SiC polycrystalline film 100, which is different from that shown in FIG. 7. [Figure 9] 9 is a schematic diagram showing a method for correcting warpage of a SiC polycrystalline film 100, which is different from that shown in FIGS. [Figure 10] 10 is a schematic diagram showing a method for correcting warpage of a SiC polycrystalline film 100, which is different from that shown in FIGS. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0018] Hereinafter, an example of an embodiment of the present invention will be described in detail with reference to the drawings, but the present invention is not limited to this embodiment.
[0019] [SiC polycrystalline substrate] The SiC polycrystalline substrate is used as a support substrate for a SiC bonded substrate in which a support substrate made of SiC polycrystal and a SiC single crystal substrate bonded to the surface of the support substrate are laminated. For example, as shown in FIG. 1, the SiC polycrystalline substrate 1 is formed of polycrystalline SiC formed by a CVD method. The SiC polycrystalline substrate 1 is disc-shaped with a thickness of 200 μm to 500 μm and a size of 4 inches to 8 inches in diameter. For example, it is formed into a 6-inch disc-shaped with a thickness of about 350 μm. The polycrystalline SiC of the SiC polycrystalline substrate 1 is composed of any one of 4H-SiC crystal, 6H-SiC crystal, and 3C-SiC crystal, or a mixture thereof.
[0020] For example, if surface 11 of SiC polycrystalline substrate 1 is a surface that bonds with a SiC single crystal substrate, surface 12 opposite surface 11 is a surface that does not bond with a SiC single crystal substrate, and in the process of manufacturing a SiC semiconductor device, surface 12 is back-ground to thin the SiC polycrystalline substrate 1. Note that surface 12 may be a surface that bonds with a SiC single crystal substrate, in which case surface 11 is a surface that does not bond with a SiC single crystal substrate, and surface 11 is back-ground.
[0021] By performing back grinding on the SiC polycrystalline substrate 1, the thickness of the SiC polycrystalline substrate 1 is ground by 40 to 60% to form the ground surface 13, and the warp amount of the ground surface 13 relative to the diameter of the ground surface 13 is 0.17 mm / inch or less.
[0022] By keeping the amount of warpage at 0.17 mm / inch or less, problems caused by warpage, such as transport errors in subsequent processes and the inability to hold the substrate on the processing table, can be prevented.
[0023] For example, if the size of the SiC polycrystalline substrate 1 is a disk shape with a diameter of 4 inches, 6 inches, or 8 inches, the diameters of the ground surface 13 are also 4 inches, 6 inches, and 8 inches, respectively. The amount of warping of 0.17 mm / inch or less means that the amount of warping per inch is 0.17 mm or less, and is a value rounded off to one decimal place. When the diameter of the ground surface 13 is 4 inches, the amount of warping of the ground surface 13 is 0.7 mm or less, when the diameter of the ground surface 13 is 6 inches, the amount of warping of the ground surface 13 is 1.0 mm or less, and when the diameter of the ground surface 13 is 8 inches, the amount of warping of the ground surface 13 is 1.4 mm or less.
[0024] In order to more reliably prevent problems caused by warping, such as transport errors in later processes and the inability to hold the substrate on the processing table, it is preferable that the amount of warping of the ground surface 13 is 1.0 mm or less when the SiC polycrystalline substrate 1 is disk-shaped with a diameter of 6 to 8 inches, for example. That is, by having the amount of warping be 0.17 mm / inch or less, problems caused by warping, such as transport errors in later processes and the inability to hold the substrate on the processing table, can be more reliably prevented for currently mainstream disk-shaped SiC polycrystalline substrates 1 with a diameter of 6 inches or less.
[0025] When the SiC polycrystalline substrate 1 is subjected to back-grinding to grind 40 to 50% of the thickness of the SiC polycrystalline substrate 1 to form the ground surface 13, it is preferable that the amount of warping of the ground surface 13 relative to the diameter of the ground surface 13 is 0.085 mm / inch or less.
[0026] By keeping the amount of warpage at 0.085 mm / inch or less, problems caused by warpage, such as transport errors in subsequent processes and the inability to hold the substrate on the processing table, can be more reliably prevented.
[0027] For example, if the size of the SiC polycrystalline substrate 1 is a disk shape with a diameter of 4 inches, 6 inches, or 8 inches, the diameter of the ground surface 13 is also 4 inches, 6 inches, or 8 inches, respectively. The amount of warping of 0.085 mm / inch or less means, rounded off to one decimal place, that the amount of warping of the ground surface 13 is 0.3 mm or less when the diameter of the ground surface 13 is 4 inches, that the amount of warping of the ground surface 13 is 0.5 mm or less when the diameter of the ground surface 13 is 6 inches, and that the amount of warping of the ground surface 13 is 0.7 mm or less when the diameter of the ground surface 13 is 8 inches. Furthermore, even if the diameter of the ground surface 15 is 12 inches, the amount of warping of the ground surface 15 is 1.0 mm or less, which is a level that can prevent problems caused by warping, such as transport errors and failure to hold the substrate on the processing table in the subsequent process.
[0028] In order to more reliably prevent problems caused by warping, such as transport errors in subsequent processes and the inability to hold the substrate on the processing table, it is more preferable that the amount of warping of the ground surface 13 be 0.5 mm or less, for example, when the SiC polycrystalline substrate 1 is disk-shaped and has a diameter of 6 to 8 inches.
[0029] In the process of thinning the SiC polycrystalline substrate 1, approximately 40 to 60% of the original thickness of the SiC polycrystalline substrate 1 is removed by back-grinding, but the extent to which the SiC polycrystalline substrate 1 is thinned depends on the tolerance for thickness unevenness of the SiC semiconductor device and how densely the device is mounted.
[0030] Here, the SiC polycrystalline substrate 1 can be ground using a grinder with a grindstone of No. 5000 to No. 8000. The ground surface after grinding has a surface roughness Ra of 1 nm to 5 nm.
[0031] The amount of warping of the ground surface 13 can be measured using a shape measuring device such as a three-dimensional measuring device.
[0032] [SiC bonded substrate] 2, the SiC bonded substrate 3 includes a SiC polycrystalline substrate 1 and a SiC single crystal substrate 2 bonded to the surface of the SiC polycrystalline substrate 1. The SiC single crystal substrate 2 is made of single crystal SiC and has a diameter of 4 to 8 inches, which is the same as that of the SiC polycrystalline substrate 1. The thickness is not particularly limited, but may be, for example, about 0.5 μm to 2.0 μm. The SiC bonded substrate 3 is made by using a high-quality SiC single crystal substrate 2 for a portion forming a component of a semiconductor device and bonding it to the SiC polycrystalline substrate 1, which is a support substrate, to thereby provide a substrate that combines a low-cost support substrate portion with high-quality single crystal SiC.
[0033] Back surface 14 of SiC polycrystalline substrate 1, which is the surface not bonded to SiC single crystal substrate 2, is back-ground in the process of manufacturing a SiC semiconductor device, and SiC polycrystalline substrate 1 is thinned. By back-grinding SiC polycrystalline substrate 1, the thickness of SiC polycrystalline substrate 1 is ground by 40 to 60% to form ground surface 15, and the amount of warping of ground surface 15 with respect to the diameter of ground surface 15 is 0.17 mm / inch or less. Note that the opposite surface 12 corresponds to back surface 14, and ground surface 13 corresponds to ground surface 15.
[0034] By keeping the amount of warpage at 0.17 mm / inch or less, problems caused by warpage, such as transport errors in subsequent processes and the inability to hold the substrate on the processing table, can be prevented.
[0035] For example, if the size of the SiC polycrystalline substrate 1 is a disk shape with a diameter of 4 inches, 6 inches, or 8 inches, the diameter of the ground surface 15 is also 4 inches, 6 inches, or 8 inches, respectively. The amount of warping of 0.17 mm / inch or less means, rounded off to one decimal place, that the amount of warping of the ground surface 15 is 0.7 mm or less when the diameter of the ground surface 15 is 4 inches, that the amount of warping of the ground surface 15 is 1.0 mm or less when the diameter of the ground surface 15 is 6 inches, and that the amount of warping of the ground surface 15 is 1.4 mm or less when the diameter of the ground surface 15 is 8 inches.
[0036] In order to more reliably prevent problems caused by warping, such as transport errors in later processes and the inability to hold the substrate on the processing table, it is preferable that the amount of warping of the ground surface 15 is 1.0 mm or less when the SiC polycrystalline substrate 1 is disk-shaped with a diameter of 6 to 8 inches. That is, by having the amount of warping be 0.17 mm / inch or less, problems caused by warping, such as transport errors in later processes and the inability to hold the substrate on the processing table, can be more reliably prevented for currently mainstream disk-shaped SiC polycrystalline substrates 1 with a diameter of 6 inches or less.
[0037] By performing back grinding on the SiC polycrystalline substrate 1, the thickness of the SiC polycrystalline substrate 1 is ground by 40 to 50% to form the ground surface 15, and in this state, it is preferable that the amount of warping of the ground surface 15 with respect to the diameter of the ground surface 15 is 0.085 mm / inch or less.
[0038] By keeping the amount of warpage at 0.085 mm / inch or less, problems caused by warpage, such as transport errors in subsequent processes and the inability to hold the substrate on the processing table, can be more reliably prevented.
[0039] For example, if the size of the SiC polycrystalline substrate 1 is a disk shape with a diameter of 4 inches, 6 inches, or 8 inches, the diameter of the ground surface 15 is also 4 inches, 6 inches, or 8 inches, respectively. The amount of warping of 0.085 mm / inch or less means, rounded off to one decimal place, that the amount of warping of the ground surface 15 is 0.3 mm or less when the diameter of the ground surface 15 is 4 inches, that the amount of warping of the ground surface 15 is 0.5 mm or less when the diameter of the ground surface 15 is 6 inches, and that the amount of warping of the ground surface 15 is 0.7 mm or less when the diameter of the ground surface 15 is 8 inches. Furthermore, even if the diameter of the ground surface 15 is 12 inches, the amount of warping of the ground surface 15 is 1.0 mm or less, which is a level that can prevent problems caused by warping, such as transport errors and failure to hold the substrate on the processing table in the subsequent process.
[0040] In order to more reliably prevent problems caused by warping, such as transport errors in subsequent processes and the inability to hold the substrate on the processing table, it is more preferable that the amount of warping of ground surface 15 be 0.5 mm or less, for example, when SiC polycrystalline substrate 1 is disk-shaped and has a diameter of 6 to 8 inches.
[0041] [SiC semiconductor device substrates] 3, the substrate 6 for a SiC semiconductor device is a substrate in which a SiC polycrystalline substrate 1, a SiC single crystal substrate 2 bonded to the surface of the SiC polycrystalline substrate 1, a SiC single crystal epitaxial layer 4 formed on the surface of the SiC single crystal substrate 2, and a semiconductor element component 5 formed on the SiC single crystal epitaxial layer 4 are laminated in this order. Here, the semiconductor element component 5 is not particularly limited, but may be, for example, a source electrode 51, a gate electrode 52, a gate insulating film 53, and a N + It is composed of a source 54 and a P-well 55. The substrate for semiconductor device is a substrate in a state before being divided into individual devices.
[0042] In the process of manufacturing a SiC semiconductor device, ground surface 16, which is the surface of SiC polycrystalline substrate 1 that is not bonded to SiC single crystal substrate 2, is back-ground to thin SiC polycrystalline substrate 1. By back-grinding SiC polycrystalline substrate 1, SiC polycrystalline substrate 1 is ground by 40% to 60% to reduce its thickness, forming ground surface 16, and the amount of warping of ground surface 16 with respect to the diameter of ground surface 16 is 0.17 mm / inch or less. Ground surface 16 corresponds to ground surface 13 and ground surface 15.
[0043] By keeping the amount of warpage at 0.17 mm / inch or less, problems caused by warpage, such as transport errors in subsequent processes and the inability to hold the substrate on the processing table, can be prevented.
[0044] For example, if the size of the SiC polycrystalline substrate 1 is a disk shape with a diameter of 4 inches, 6 inches, or 8 inches, the diameters of the ground surface 16 are also 4 inches, 6 inches, and 8 inches, respectively. The amount of warping of 0.17 mm / inch or less means, rounded off to one decimal place, that the amount of warping of the ground surface 16 is 0.7 mm or less when the diameter of the ground surface 16 is 4 inches, that the amount of warping of the ground surface 16 is 1.0 mm or less when the diameter of the ground surface 16 is 6 inches, and that the amount of warping of the ground surface 16 is 1.4 mm or less when the diameter of the ground surface 16 is 8 inches.
[0045] In order to more reliably prevent problems caused by warping, such as transport errors in later processes and the inability to hold the substrate on the processing table, it is preferable that the amount of warping of the ground surface 16 is 1.0 mm or less when the SiC polycrystalline substrate 1 is disk-shaped with a diameter of 6 to 8 inches. That is, by having the amount of warping be 0.17 mm / inch or less, problems caused by warping, such as transport errors in later processes and the inability to hold the substrate on the processing table, can be more reliably prevented for currently mainstream disk-shaped SiC polycrystalline substrates 1 with a diameter of 6 inches or less.
[0046] [SiC semiconductor device] The SiC semiconductor device 7 of this embodiment is obtained by dividing the substrate for the SiC semiconductor device into individual pieces. As shown in Fig. 4, a semiconductor device for a vertical power device in which the current flows in the thickness direction of the substrate has a structure in which a drain electrode 8 is formed as a back electrode on the ground surface 16 of the substrate 6 for the SiC semiconductor device.
[0047] [Manufacturing method for SiC polycrystalline substrate] Next, a method for manufacturing a SiC polycrystalline substrate will be described. This manufacturing method is a method for manufacturing a SiC polycrystalline substrate 1 used as a support substrate in a SiC bonded substrate 3 in which a SiC polycrystalline substrate 1 serving as a support substrate and a SiC single crystal substrate 2 bonded to the surface of the SiC polycrystalline substrate 1 are laminated, and includes a film forming step, a separation step, a heat treatment step, and a grinding / polishing step, which will be described below. Fig. 5 is a flow chart of an example of a method for manufacturing the SiC polycrystalline substrate 1 and the SiC bonded substrate 3 serving as a support substrate, and shows steps S10 to S80.
[0048] <Step S10 (film formation process)> In the manufacturing method of the SiC polycrystalline substrate 1, a SiC polycrystalline film is formed on a seed substrate in step S10. The seed substrate made of carbon, silicon, or the like is used as a base substrate, and a SiC polycrystalline film is formed on the base substrate by a CVD method or the like.
[0049] <Step S20 (separation process)> Next, in step S20, the seed substrate and the SiC polycrystalline film are separated from each other. For example, the base material on which the SiC polycrystalline film is formed can be removed by burning or dissolving it with acid.
[0050] <Step S30 (Heat Treatment Process)> In this embodiment, the objective is to suppress warping of the SiC semiconductor device substrate 6 that occurs when the SiC polycrystalline substrate 1 is thinned by the back grinding process (step S110) described later, and for this purpose, a heat treatment process is performed.
[0051] When the SiC polycrystalline film is separated from the seed substrate after the separation process, it will have a warp of about several tens of μm even before the back grinding process. The direction of the warp of the SiC polycrystalline film after the separation process can be determined using a shape measuring device such as the above-mentioned three-dimensional measuring device, as well as various simple measurements and visual inspection. In the heat treatment process, the SiC polycrystalline film is heat treated in a state where the warp has been corrected. The warp is corrected by maintaining a state in which a force is applied to the SiC polycrystalline film in the direction opposite to the direction of the warp of the SiC polycrystalline film.
[0052] For example, the SiC polycrystalline film may be placed on a straightening tool capable of straightening the warpage of the SiC polycrystalline film, and a weight may be applied from above to straighten the shape so that a force acts in the opposite direction to the warpage of the SiC polycrystalline film (for example, so that the SiC polycrystalline film warps in the opposite direction to the warpage of the SiC polycrystalline film), and heat treatment may be performed while maintaining this state. By performing heat treatment while applying stress to the SiC polycrystalline film with the straightening tool, it is possible to relieve the internal stress of the SiC polycrystalline film so as to suppress the warpage of the SiC polycrystalline film after the grinding process described below.
[0053] The correction tool is not particularly limited as long as it has a shape capable of correcting the warpage of the SiC polycrystalline film. The correction tool may be made of, for example, graphite or alumina. As an example, FIG. 7 shows a schematic side view illustrating a method for correcting the warpage of the SiC polycrystalline film 100. In FIG. 7(a), the disk-shaped SiC polycrystalline film 100 is warped with a concave center and a raised periphery, and has a convex spherical surface 110 protruding downward at the center and a concave spherical surface 120 opposite to the spherical surface 110 and concave at the center. The SiC polycrystalline film 100 is placed on the correction tool 200 so that the spherical surface 110 of the SiC polycrystalline film 100 is in contact with the correction surface 210 of the correction tool 200, and the weight 300 is placed on the SiC polycrystalline film 100 so that the spherical surface 120 of the SiC polycrystalline film 100 is in contact with the spherical surface 310 of the weight 300 (FIG. 7(b)). Heat treatment is performed while maintaining this state.
[0054] The correction surface 210 of the correction tool 200 is a convex spherical surface protruding upward, and if the diameter of the SiC polycrystalline film 100 is 6 inches, the radius of curvature of the correction surface 210 may be 5.0 m or less, and is preferably 4.5 m to 3.0 m from the viewpoint of effectively correcting the warpage of the SiC polycrystalline film 100. Furthermore, the center 220 of the correction surface 210 protrudes the most on the correction surface 210, and from the viewpoint of effectively correcting the warpage of the SiC polycrystalline film 100, it is preferable that the center 220 protrudes 0.6 mm to 0.8 mm from the outer periphery 230 of the correction surface 210.
[0055] The weight is not limited in shape or weight as long as it can be placed so that the entire surface of the spherical surface 110 of the SiC polycrystalline film 100 is in close contact with the entire surface of the correction surface 210 of the correction tool 200. In addition, the weight may be made of a material such as graphite or alumina. For example, the spherical surface 310 of the weight 300 may be a concave spherical surface that is concave upward, and may have a concave spherical shape that matches the convex spherical shape of the correction surface 210. By making the shape match the spherical shape, it is possible to prevent scratches and the like from occurring on the SiC polycrystalline film 100. In order to make the shape match the spherical shape, the radius of curvature of the spherical surface 310 may be 5.0 m or less, and from the viewpoint of effectively correcting the warpage of the SiC polycrystalline film 100, it is preferably 4.5 m to 3.0 m. Moreover, center 320 of spherical surface 310 is the deepest recess on spherical surface 310, and from the viewpoint of effectively correcting the warpage of SiC polycrystalline film 100, center 320 is preferably recessed from outer periphery 330 of spherical surface 310 by 0.6 mm to 0.8 mm.
[0056] The weight of the weight 300 is not particularly limited as long as it can be placed so that the entire surface of the spherical surface 110 of the SiC polycrystalline film 100 is in close contact with the entire surface of the correction surface 210 of the correction tool 200. For example, if the thickness of the SiC polycrystalline film 100 is 1.0 mm or less, the weight of the weight 300 may be 3 kg or more and 8 kg or less, and preferably 4 kg or more and 6 kg or less. If the weight of the weight 300 is less than 3 kg, the warp of the SiC polycrystalline film 100 may not be sufficiently corrected. Also, if the weight of the weight 300 exceeds 8 kg, a defect such as cracking of the SiC polycrystalline film 100 may occur.
[0057] Fig. 8 is a schematic side view showing a method for correcting warpage of a SiC polycrystalline film 100, which is different from that shown in Fig. 7. Unlike the case of Fig. 7, the SiC polycrystalline film 100 is placed on the correcting jig 200a with the spherical surface 120 facing down so as to contact the correcting surface 210a of the correcting jig 200a, and further, the weight 300a is placed on the SiC polycrystalline film 100 so that the spherical surface 110 of the SiC polycrystalline film 100 and the spherical surface 310a of the weight 300a are in contact with each other (Fig. 8(b)). Heat treatment may be performed while maintaining this state.
[0058] The correction surface 210a of the correction tool 200a is a downwardly concave spherical surface, and if the diameter of the SiC polycrystalline film 100 is 6 inches, the radius of curvature of the correction surface 210a may be 5.0 m or less, and is preferably 4.5 m to 3.0 m from the viewpoint of effectively correcting the warpage of the SiC polycrystalline film 100. Furthermore, the center 220a of the correction surface 210a is the most concave on the correction surface 210a, and from the viewpoint of effectively correcting the warpage of the SiC polycrystalline film 100, it is preferable that the center 220a is concave by 0.6 mm to 0.8 mm from the outer periphery 230a of the correction surface 210a.
[0059] Moreover, the spherical surface 310a of the weight 300a is a convex spherical surface protruding downward, and may be a convex spherical shape that matches the concave spherical shape of the correcting surface 210a. By making the shape match the spherical shape, it is possible to prevent scratches and the like from occurring on the SiC polycrystalline film 100. In order to make the shape match the spherical shape, the radius of curvature of the spherical surface 310a may be 5.0 m or less, and from the viewpoint of effectively correcting the warpage of the SiC polycrystalline film 100, it is preferably 4.5 m to 3.0 m. Moreover, the center 320a of the spherical surface 310a is the most protruding part on the spherical surface 310a, and from the viewpoint of effectively correcting the warpage of the SiC polycrystalline film 100, it is preferable that the center 320a protrudes 0.6 mm to 0.8 mm from the outer periphery 330a of the spherical surface 310a.
[0060] For example, if the thickness of the SiC polycrystalline film 100 is 1.0 mm or less, the weight of the weight 300a should be 3 kg or more and 8 kg or less, and preferably 4 kg or more and 6 kg or less. If the weight of the weight 300a is less than 3 kg, the warpage of the SiC polycrystalline film 100 may not be sufficiently corrected. Also, if the weight of the weight exceeds 8 kg, the SiC polycrystalline film 100 may crack.
[0061] The warpage of the SiC polycrystalline film 100 can be effectively corrected by applying a force in the opposite direction to the warpage of the SiC polycrystalline film 100, for example by pressing the peripheral portion of the SiC polycrystalline film 100 with a weight to warp the SiC polycrystalline film 100 in the opposite direction. For this reason, a weight 300b may be placed on the peripheral portion of the SiC polycrystalline film 100 via a ring-shaped jig 400 shown in FIG. 9(a) so as to press the peripheral portion of the SiC polycrystalline film 100 (FIG. 9(b)). In addition, by using the ring-shaped jig 400, it is not necessary to process the lower surface of the weight into a spherical shape, so that a weight 300b having a flat lower surface 310b that can be easily manufactured can be used. The ring jig 400 can be made of a material such as graphite or alumina. In addition, a weight with a ring-shaped lower surface may be used so as to contact only the peripheral portion of the SiC polycrystalline film 100.
[0062] Moreover, the warpage of the SiC polycrystalline film 100 can be corrected simultaneously for a plurality of SiC polycrystalline films 100. For example, as shown in Fig. 10, a plurality of sheet-like carbon sheets 500 may be inserted between and stacked on a plurality of SiC polycrystalline films 100, and the warpage may be corrected using a correction jig 200 and a weight 300. By interposing the carbon sheets 500 between the SiC polycrystalline films 100, adhesion between the SiC polycrystalline films 100 caused by sublimation and recrystallization of the surfaces of the SiC polycrystalline films 100 when the SiC polycrystalline films 100 are heat-treated can be suppressed or prevented.
[0063] As shown by dotted line L in Figures 7 to 10, in either case, the warping of SiC polycrystalline film 100 can be reliably corrected by stacking correcting tool 200, SiC polycrystalline film 100, and weight 300 so that the center of spherical surface 110 of SiC polycrystalline film 100, the center of correction surface 210 of correcting tool 200, and the center of spherical surface 310 of weight 300 are on the same straight line, and this straight line (dotted line L in Figures 7 to 10) is parallel to the vertical direction.
[0064] The heat treatment process is performed after the separation process of step S20 and before the back grinding process (step S110). The heat treatment of the SiC polycrystalline substrate 1 is possible, for example, before the back grinding process in the manufacturing process of the SiC polycrystalline substrate, the manufacturing process of the SiC bonded substrate 3, or the manufacturing process of the substrate 6 for the SiC semiconductor device. However, as described below, if the heat treatment temperature of the SiC polycrystalline film exceeds 1700°C, sublimation and recrystallization of SiC on the surface of the SiC polycrystalline substrate begins, causing the surface to deteriorate. For this reason, it is preferable to perform the heat treatment in the manufacturing process of the SiC polycrystalline substrate, and in particular, by performing the heat treatment before the grinding process (step S40) of the SiC polycrystalline substrate, defects such as surface deterioration caused by the heat treatment can be eliminated in the grinding process (step S40). In addition, the heat treatment process can reduce warpage after back grinding.
[0065] In step S30, the SiC polycrystalline film after the separation step is heat-treated by holding it at a temperature of 1600° C. or higher and lower than 2000° C. This step may be a step of holding the SiC polycrystalline film at a temperature between 1700° C. and 1800° C. for 3 hours or longer.
[0066] The higher the heat treatment temperature of the SiC polycrystalline film, the smaller the warpage of the substrate after the back grinding process tends to be. Heat treatment can alleviate the internal stress during the formation of the SiC polycrystalline substrate, thereby reducing the warpage of the substrate. If the heat treatment temperature is less than 1600°C, the effect of improving the warpage of the substrate after the back grinding process is small. If the heat treatment temperature is 1700°C or higher, sublimation and recrystallization of SiC begins from the surface layer of the SiC polycrystalline film, and if it exceeds 1800°C, the sublimation and recrystallization of SiC tends to proceed excessively. If the heat treatment temperature exceeds 2000°C, crater-like pores or depressions of several μm to several tens of μm may be formed on the surface layer of the SiC polycrystalline film, which is not preferable because it may cause problems in the formation of the back electrode. It is preferable to perform the heat treatment while holding the polycrystalline film at 1700°C or higher and 1800°C or lower.
[0067] The holding time for holding the SiC polycrystalline film at 1600°C or more and less than 2000°C is preferably 3 hours or more. If the holding time is less than 3 hours, the effect of improving the warpage of the substrate after backside polishing may be small. There is no particular upper limit to the holding time, but it is preferably 30 hours or less. If the holding time exceeds 30 hours, the effect will not increase any more, and the longer the holding time, the greater the disadvantage in terms of manufacturing costs. The holding time is preferably 20 hours or more and 30 hours or less.
[0068] The atmosphere of the SiC polycrystalline film during the heat treatment is preferably at least one of an inert gas atmosphere such as argon (Ar) or nitrogen (N) or a vacuum atmosphere to prevent unnecessary reactions such as oxidation. For example, it is preferable that the inside of a heat treatment furnace used for the heat treatment is in a state where an inert gas is flowing, and the flow rate is not limited as long as the furnace is sufficiently filled with the inert gas. The heat treatment may be performed using an atmosphere-controlled heating furnace or the like.
[0069] <Steps S40 (grinding process) and S50 (polishing process)> In step 40, the SiC polycrystalline film is ground to a predetermined thickness, and in step 50, the surface of the SiC polycrystalline film is polished. After these grinding and polishing steps, the SiC polycrystalline substrate that is ready to be bonded to a SiC single crystal substrate is the SiC polycrystalline substrate 1 according to this embodiment that can be used as a support substrate.
[0070] [Manufacturing method for SiC bonded substrate] <Steps S60 to S80> Steps S60 to S80 are a method for manufacturing a SiC bonded substrate. In step S60, the above-mentioned SiC polycrystalline substrate 1 and a separately prepared SiC single crystal substrate 2 are bonded (bonding step). As described in Patent Document 1, the single crystal SiC substrate 2 may be manufactured by bonding a thick SiC single crystal substrate to a support substrate (step 60) using a peeling technique (also called Smart Cut (registered trademark)) using ablation of hydrogen atoms, and then separating the substrate to manufacture a thin SiC single crystal substrate on the support substrate (step 70). After that, in step S80, a polishing step is performed to polish the surface of the SiC single crystal substrate, resulting in a SiC bonded substrate 3 including the SiC polycrystalline substrate 1 and the SiC single crystal substrate 2.
[0071] The SiC single crystal substrate to be bonded may be a SiC single crystal produced by the improved Rayleigh process, or a SiC single crystal formed by using a CVD method.
[0072] [Manufacturing method for SiC semiconductor device] Next, a method for manufacturing a SiC semiconductor device will be described. FIG. 6 is a flow chart showing an example of a method for manufacturing a SiC semiconductor device 7, showing steps S90 to S140. In step S90, a SiC single crystal epitaxial layer 4 is epitaxially grown on the surface of a SiC single crystal substrate 2, and in step S100, a circuit pattern of components 5 of a semiconductor device and the like is formed on the surface of the SiC single crystal epitaxial layer 4, and a surface protection layer for protecting the circuit pattern is formed with resin or the like. Thereafter, in step S110, the back surface side opposite to the surface on which the circuit pattern is formed is ground, and the SiC polycrystalline substrate 1 is thinned to form a ground surface 16 (back grinding process). The substrate in the state in which the process up to step S110 has been completed is the substrate 6 for a SiC semiconductor device shown in FIG. 3. After the process of step S110, in step S120, a drain electrode 8 is formed as a back surface electrode on the ground surface 16 of the substrate 6 for a SiC semiconductor device, resulting in a SiC semiconductor device 7. Before forming the back electrode, the ground surface 16 may be subjected to surface treatment such as polishing.
[0073] Thereafter, in step S130, the surface protection layer protecting the circuit pattern of the SiC semiconductor device 7 is removed, and in step S140, dicing is performed by using a rotating diamond blade or the like to cut the SiC semiconductor device 7 into dies.
[0074] The process flow from manufacturing the SiC polycrystalline substrate 1 to manufacturing the semiconductor is as shown in steps S10 to S140, but existing inspection steps and processing steps such as contact hole formation and probe inspection may be further carried out as appropriate.
[0075] In the manufacturing process of the SiC semiconductor device 7, after the components 5 of the semiconductor element are formed on the SiC single crystal epitaxial layer 4, back grinding is performed. In particular, the SiC semiconductor device 7 is often used in a vertical power device in which the current flow direction is the thickness direction of the substrate, and a thinning process by back grinding is performed after mounting a front circuit pattern in the manufacturing process of the vertical power device. In this process, it is necessary to remove about 40 to 60% of the original thickness of the SiC polycrystalline substrate 1. For example, in a SiC polycrystalline substrate with a diameter of 6 inches, when the thickness of the substrate is 350 μm, a thickness of about 150 to 200 μm is removed by grinding, so the amount of SiC polycrystalline is large, and grinding is generally adopted, which has a higher thinning processing efficiency than polishing. For example, in a substrate for a SiC semiconductor device using a SiC single crystal substrate that is not bonded to a SiC polycrystalline substrate, the warp of the substrate after thinning the SiC single crystal substrate by back grinding can be suppressed to about 1 mm or less. By keeping it within this range, it becomes possible to process the substrate without any problems in the subsequent processes. In contrast, when a SiC bonded substrate 3 is used in which a SiC polycrystalline substrate 1 and a SiC single crystal substrate 2 are bonded together, and the SiC polycrystalline substrate 1 is thinned by back grinding, the warpage of the substrate significantly exceeds 1.0 mm, for example, in the conventional technology in which no heat treatment process is performed.
[0076] In this embodiment, by performing a heat treatment process between the separation process and the grinding process, the warpage of the substrate after the thinning process of the SiC polycrystalline substrate by back-grinding can be suppressed to approximately 1.0 mm or less. EXAMPLES
[0077] The present invention will be explained in more detail below by showing examples, but the present invention is not limited to the following examples in any way.
[0078] [Example 1] <Preparation of SiC polycrystalline substrate 1> A seed substrate formed in a disk shape made of carbon was used as a base substrate, and a SiC polycrystalline film having a thickness of 2 mm was formed on the surface of the base substrate by chemical vapor deposition (CVD) (step S10). Methylchlorosilane was used as the source gas, and hydrogen and nitrogen gases were used as the carrier gas. The growth temperature in this chemical vapor deposition was 1400°C. Thereafter, the base substrate was heated and removed in an air atmosphere at 1000°C by a combustion method, and a disk-shaped SiC polycrystalline film 100 having a diameter of 6 inches was produced (step S20).
[0079] The SiC polycrystalline film 100 was heat-treated using an atmosphere-controlled heating furnace (step S30). The heating temperature was 1700°C, the heating temperature was held for 24 hours, and the atmosphere in the furnace was an argon gas atmosphere. During the heat treatment, the warpage of the SiC polycrystalline film 100 was corrected using a graphite correction tool 200, a graphite ring-shaped tool 400, and a graphite weight 300b. At this time, the SiC polycrystalline film 100 was first placed on the correction tool 200, the upper surface of which was the correction surface 210. The radius of curvature of the correction surface 210 was 4 m, and a convex spherical surface 110 with a protruding center of the SiC polycrystalline film 100 was placed on the correction surface 210. A ring-shaped jig 400 having an outer diameter of 150 mm, an inner diameter of 100 mm, and a plate thickness of 2 mm was placed on the SiC polycrystalline film 100 placed on the correction jig 200 in this way, and a cylindrical weight 300b weighing 4 kg was further placed on the ring-shaped jig 400. By arranging in this way, the spherical surface 110 of the SiC polycrystalline film 100 was deformed so as to be in close contact with the correction surface 210, and a force was applied in the opposite direction to the warping direction of the SiC polycrystalline film 100, so that the heat treatment was performed while maintaining the warped state in the opposite direction. The warping direction of the SiC polycrystalline film 100 before being placed on the correction jig 200 can be determined by using a shape measuring device such as the above-mentioned three-dimensional measuring device, as well as by various simple measurements and visual inspection.
[0080] Thereafter, the surface of the SiC polycrystalline film 100 was ground and polished to be flattened (steps S40, S50), to obtain a SiC polycrystalline substrate 1 having a diameter of 6 inches (about 150 mm) and a thickness of 350 μm.
[0081] <Preparation of SiC bonded substrate 3> The manufactured SiC polycrystalline substrate 1 was used to manufacture a SiC bonded substrate 3. The SiC single crystal substrate to be bonded to the SiC polycrystalline substrate 1 was a 350 μm thick, 6 inch (about 150 mm) diameter SiC single crystal substrate manufactured by the improved Lely process with a main surface orientation of <0001> The SiC bonded substrate 3 was manufactured using a disk-shaped substrate of 4H polytype. The SiC bonded substrate 3 was manufactured using a separation technique using ablation of hydrogen atoms (also called Smart Cut (registered trademark)) described in Patent Document 1.
[0082] (Step S60) Hydrogen ions were implanted into the bonding surface of the SiC single crystal substrate to be bonded to the SiC polycrystalline substrate 1, forming a hydrogen ion implanted layer at a depth of 1.0 μm from the bonding surface. The SiC single crystal substrate and the SiC polycrystalline substrate 1 were attracted by an electrostatic chuck and set in the chamber. Next, the electrostatic chuck was moved to align the relative positions of the SiC single crystal substrate and the SiC polycrystalline substrate 1 so that the two substrates would come into contact in the correct positional relationship during the room temperature bonding process. Next, the chamber was filled with 2×10 -6 The chamber was evacuated to a vacuum of 10 Pa. Next, a neutral argon atomic beam was uniformly irradiated onto the entire surface of the SiC single crystal substrate to be bonded and the entire surface of the SiC polycrystalline substrate 1 to be bonded using a FAB gun, removing the oxide film and adsorption layer on both surfaces to be bonded, exposing the bonds and making them active. Next, while maintaining the vacuum at room temperature, the electrostatic chuck was moved within the chamber, bringing the surfaces to be bonded of the SiC single crystal substrate and the surfaces to be bonded of the SiC polycrystalline substrate 1 into contact with each other in a vacuum state within the chamber, directly bonding them through covalent bonds, to obtain a bonded substrate.
[0083] (Step S70) Next, using a furnace, the bonded substrate was heated to 1000°C in an inert atmosphere filled with argon gas to form a microbubble layer in the hydrogen ion implanted layer, and the SiC single crystal substrate 2 was separated at the microbubble layer, and the thin plate-shaped SiC single crystal substrate 2 with a thickness of 1.0 μm was transferred to the SiC polycrystalline substrate 1.
[0084] (Step S80) The surface of the SiC single crystal substrate 2 exposed in step S70 was processed by CMP polishing so as to be smooth, thereby obtaining a SiC bonded substrate 3.
[0085] <Preparation of Substrate 6 for SiC Semiconductor Device> Next, a substrate 6 for a SiC semiconductor device was produced. Using the SiC bonded substrate 3 produced by the above method, a SiC single crystal epitaxial layer 4 was formed to a thickness of 20 μm on the surface of the SiC single crystal substrate 2 by chemical vapor deposition (step S90). Then, a circuit pattern was formed as a component 5 of a semiconductor device on the surface of the SiC single crystal epitaxial layer 4, and the circuit pattern was protected with a resin or the like (step S100). Then, back grinding was performed to grind the exposed surface side of the SiC polycrystalline substrate 1, and a ground surface 16 was formed (step S110). For back grinding, a grinder manufactured by DISCO was used to grind the back surface of the SiC polycrystalline substrate 1. A grinding wheel with a diameter of 200 mm and number 7000 was used as the grinding wheel.
[0086] <Measurement of warpage of grinding surface 16> The warpage of the SiC semiconductor device substrate 6 was measured using a three-dimensional measuring device EMS-3D 300XY manufactured by COMS Corporation. First, the ground surface 16 of the SiC semiconductor device substrate 6 was suctioned on the non-full surface, and the ground surface 16 was held so that the constituent element 5 of the semiconductor element of the SiC semiconductor device substrate 6 faces upward, and height difference data was obtained. Next, the warpage was calculated as the sum of the maximum distance and the minimum distance from the reference plane. The warpage was measured in the state before grinding in step S110, the state in which the back grinding amount of the SiC polycrystalline substrate 1 in step S110 was 150 μm (43% of the thickness of the SiC polycrystalline substrate 1), the state in which the back grinding amount of the SiC polycrystalline substrate 1 was 175 μm (50% of the thickness of the SiC polycrystalline substrate 1), and the state in which the back grinding amount of the SiC polycrystalline substrate 1 was 200 μm (57% of the thickness of the SiC polycrystalline substrate 1). The measurement results are shown in Table 1.
[0087] A non-full surface is an adsorption surface that can adsorb and hold one or three points on the measurement surface to be measured for warpage without changing the original shape of the substrate. Since the entire surface to be measured is not adsorbed, using a non-full surface makes it possible to measure warpage.
[0088] [Example 2] In Example 2, the warpage of the SiC polycrystalline substrate 1 produced in Example 1 was evaluated. First, for back grinding evaluation, the SiC polycrystalline substrate 1 was subjected to back grinding under the same conditions as in step S110 in Example 1. In addition, the warpage of the ground surface 13 was measured by suctioning and holding the ground surface 13 on the non-full suction surface of the opposite surface 12 of the SiC polycrystalline substrate 1 before the back grinding, and in the states where the back grinding amount of the SiC polycrystalline substrate 1 was 150 μm (43% of the thickness of the SiC polycrystalline substrate 1), 175 μm (50% of the thickness of the SiC polycrystalline substrate 1), and 200 μm (57% of the thickness of the SiC polycrystalline substrate 1). The measurement results are shown in Table 1.
[0089] [Example 3], [Example 4] In Example 3, the radius of curvature of the correction surface 210 of the correction tool 200 in the heat treatment step was changed to 3.5 m. In Example 4, the heat treatment temperature in the heat treatment step was changed to 1800° C. The warpage of the SiC polycrystalline substrate 1 produced under the same conditions as those for producing the SiC polycrystalline substrate 1 in Example 1 was evaluated. As in Example 2, the back grinding process was performed, and the opposite surface 12 and the ground surface 13 were adsorbed and held by the non-entire adsorption surface, and the warpage of the opposite surface 12 and the ground surface 13 was measured. That is, the warpage of the ground surface 13 was measured in the opposite surface 12 of the SiC polycrystalline substrate 1 before the back grinding process, and in the state where the back grinding amount of the SiC polycrystalline substrate 1 was 150 μm (43% of the thickness of the SiC polycrystalline substrate 1), 175 μm (50% of the thickness of the SiC polycrystalline substrate 1), and 200 μm (57% of the thickness of the SiC polycrystalline substrate 1). The measurement results are shown in Table 1.
[0090] [Comparative Example 1] Except for not carrying out the heat treatment process of step S30, the SiC polycrystalline substrate 1, the SiC bonded substrate 3 and the substrate 6 for a SiC semiconductor device were manufactured in the same manner as in Example 1, and the warpage of the manufactured substrate 6 for a SiC semiconductor device was measured. The measurement results are shown in Table 1.
[0091] [Comparative Example 2] The warpage of the SiC polycrystalline substrate 1 produced in Comparative Example 1 was measured in the same manner as in Example 2. The measurement results are shown in Table 1.
[0092] [Comparative Example 3] The warpage of the SiC bonded substrate 3 produced in Comparative Example 1 was measured. Specifically, the SiC bonded substrate 3 was subjected to a back grinding process under the same conditions as in step S110 of Example 1. The warpage of the back surface 14 of the SiC bonded substrate 3 before the back grinding process, and the ground surface 15 of the SiC bonded substrate 3 with the back surface grinding amount of 150 μm (43% of the thickness of the SiC polycrystalline substrate 1), 175 μm (50% of the thickness of the SiC polycrystalline substrate 1), and 200 μm (57% of the thickness of the SiC polycrystalline substrate 1) were measured. The warpage was measured by suctioning and holding the back surface 14 and the ground surface 15 on the non-entire suction surface. The measurement results are shown in Table 1.
[0093] [Comparative Example 4] In Comparative Example 4, the straightening jig 200, the ring-shaped jig 400, and the weight 300b were not used in the heat treatment process, and the heat treatment was performed without straightening the warpage of the SiC polycrystalline film 100. The SiC polycrystalline substrate 1 was produced under the same conditions as those for producing the SiC polycrystalline substrate 1 in Example 1, and the warpage of the SiC polycrystalline substrate 1 was evaluated. The opposite surface 12 of the SiC polycrystalline substrate 1 before the back-grinding process and the ground surface 13 after the back-grinding process was performed as in Example 2 were sucked and held on the non-entire chucking surface, and the warpage of the opposite surface 12 and the ground surface 13 were measured. The measurement results are shown in Table 1.
[0094] [Table 1]
[0095] (Results and Discussion) The SiC semiconductor device substrate 6 is composed of a SiC polycrystalline substrate 1, a SiC single crystal substrate 2, a SiC single crystal epitaxial layer 4, and a semiconductor element component 5. Among these, the thickness of the SiC polycrystalline substrate 1 is sufficiently larger than the others, and the SiC polycrystalline substrate 1 is directly processed in the back grinding, so it is understood that the SiC polycrystalline substrate 1 has a large effect on warpage. In addition, in the results of Table 1, in any of the cases of the SiC semiconductor device substrate 6, the SiC bonded substrate 3, and the SiC polycrystalline substrate 1, the degree of warpage after back grinding ("after BG processing" in Table 1) was considerably larger than the warpage before back grinding ("before BG processing" in Table 1). From this, it is necessary to improve the warpage of the substrate caused by back grinding after the back grinding of the SiC single crystal substrate 1. Comparing Examples 1 to 4 and Comparative Examples 1 to 4 in Table 1, it was found that the warpage can be improved by subjecting the SiC polycrystalline substrate 1 to heat treatment.
[0096] In Comparative Examples 1 to 3, the warpage after back grinding exceeds 1 mm in each of the SiC semiconductor device substrate 6, the SiC bonded substrate 3, and the SiC polycrystalline substrate 1, because no heat treatment process is performed. The warpage after back grinding of the SiC semiconductor device substrate 6, the SiC bonded substrate 3, and the SiC polycrystalline substrate 1 is almost the same. From this result, it is inferred that the warpage after back grinding of the SiC semiconductor device substrate 6 is essentially caused by the polycrystalline SiC substrate 1. And, from the results of Examples 1 to 4, it was found that the warpage after back grinding of the SiC semiconductor device substrate 6 can be improved by improving the warpage of the SiC polycrystalline substrate 1 alone after back grinding by heat treatment.
[0097] Furthermore, by performing heat treatment while maintaining the state in which the warpage of SiC polycrystalline film 100 was corrected using correction jig 200, ring-shaped jig 400, and weight 300b, i.e., while applying a force in the opposite direction to the direction of the warpage of SiC polycrystalline film 100, the degree of warpage could be improved compared to the case in which heat treatment was performed without correcting the warpage of SiC polycrystalline film 100 (Examples 1 to 4, Comparative Example 4).
[0098] As described above, this embodiment can reduce the warpage of a 6-inch substrate after backgrinding by backgrinding to 1 mm or less, and this embodiment can provide a manufacturing method that can achieve this by a heat treatment process characterized by a long time and high temperature, and is therefore industrially useful. The heat treatment conditions that can reduce the warpage of a 6-inch substrate after backgrinding by backgrinding to 1 mm or less are a heat treatment temperature of 1600° C. or more and less than 2000° C., and a temperature holding time of 3 hours or more. In addition, by performing heat treatment while maintaining a state in which the warpage of the SiC polycrystalline film is corrected, the warpage of the substrate after backgrinding by backgrinding can be further alleviated. [Explanation of symbols]
[0099] 1,1A...SiC polycrystalline substrate, 2...SiC single crystal substrate, 3,3A...SiC bonded substrate, 4...SiC single crystal epitaxial layer, 5...component of semiconductor element, 6...SiC semiconductor device substrate, 7...SiC semiconductor device, 8...drain electrode, 11...front surface, 12...opposite surface, 13,15,16...ground surface, 14...back surface, 51...source electrode, 52...gate electrode, 53...gate insulating film, 54...N + source, 55... P well, 100... SiC polycrystalline film, 110, 120... spherical surface, 200, 200a... correction jig, 210, 210a... correction surface, 220, 220a, 320, 320a... center, 230, 230a... outer periphery, 300, 300a, 300b... weight, 310, 310a... spherical surface, 310b... lower surface, 330, 330a... outer periphery, 400... ring-shaped jig, 500... carbon sheet.
Claims
1. In order, a support substrate made of polycrystalline SiC; A SiC single crystal substrate bonded to a surface of the support substrate; A SiC single crystal epitaxial layer formed on a surface of the SiC single crystal substrate; A substrate for a SiC semiconductor device in which a component of a semiconductor element is formed on the SiC single crystal epitaxial layer, a surface of the support substrate that is not joined to the SiC single crystal substrate is a ground surface; A substrate for a SiC semiconductor device, wherein the amount of warping of the ground surface relative to the diameter of the ground surface is 0.17 mm / inch or less.
2. 2. The substrate for a SiC semiconductor device according to claim 1, wherein the amount of warping of the ground surface is 1.0 mm or less.
3. A support substrate made of polycrystalline SiC; a SiC single crystal substrate bonded to a surface of the support substrate; and A SiC bonded substrate, in which a surface of the support substrate that is not bonded to the SiC single crystal substrate is back-ground to grind the thickness of the support substrate by 40 to 60% to form a ground surface, and in this state, the amount of warping of the ground surface relative to the diameter of the ground surface is 0.17 mm / inch or less.
4. 4. The SiC bonded substrate according to claim 3, wherein the amount of warping of the ground surface is 1.0 mm or less.
5. The SiC bonded substrate according to claim 3, A SiC bonded substrate, in which a surface of the support substrate that is not bonded to the SiC single crystal substrate is back-ground to grind the thickness of the support substrate by 40 to 50% to form a ground surface, and in this state, the amount of warping of the ground surface with respect to a diameter of the ground surface is 0.085 mm / inch or less.
6. A SiC polycrystalline substrate is used as the support substrate in a SiC bonded substrate in which a support substrate made of SiC polycrystalline and a SiC single crystal substrate bonded to a surface of the support substrate are laminated, A SiC polycrystalline substrate, in which a surface of the support substrate that is not joined to the SiC single crystal substrate is back-ground to grind the thickness of the support substrate by 40 to 60% to form a ground surface, the amount of warping of the ground surface relative to a diameter of the ground surface being 0.17 mm / inch or less.
7. The SiC polycrystalline substrate according to claim 6 , wherein the amount of warping of the ground surface is 1.0 mm or less.
8. The SiC polycrystalline substrate according to claim 6, A SiC polycrystalline substrate, in which a surface of the support substrate that is not joined to the SiC single crystal substrate is back-ground to grind the thickness of the support substrate by 40 to 50% to form a ground surface, the amount of warping of the ground surface relative to a diameter of the ground surface is 0.085 mm / inch or less.
9. A method for manufacturing a SiC polycrystalline substrate for use as the support substrate in a SiC bonded substrate in which a support substrate made of SiC polycrystalline and a SiC single crystal substrate bonded to a surface of the support substrate are stacked, comprising: a film formation step of forming a SiC polycrystalline film on a seed substrate; a separation step of separating the seed substrate and the SiC polycrystalline film after the film forming step; a heat treatment step of heat-treating the SiC polycrystalline film by maintaining the temperature at 1600° C. or more and less than 2000° C. after the separation step; a grinding and polishing step of grinding and polishing the SiC polycrystalline film to process it into the support substrate after the heat treatment step, In the heat treatment step, the SiC polycrystalline film is heat-treated while maintaining a state in which a force is applied in a direction opposite to a warping direction of the SiC polycrystalline film.
10. The method for producing a SiC polycrystalline substrate according to claim 9 , wherein in the heat treatment step, a force in the opposite direction is applied to the SiC polycrystalline film placed on a correction jig.
11. 10. The method for producing a SiC polycrystalline substrate according to claim 9, wherein the heat treatment step is a step of holding the SiC polycrystalline film at a temperature between 1700° C. and 1800° C. for 3 hours or more.
Citation Information
Patent Citations
Method for producing silicon carbide composite substrate, and method for producing semiconductor substrate
JP2017055022A
Semiconductor substrate manufacturing method
JP2017112336A
Silicon carbide single crystal substrate, silicon carbide epitaxial substrate and silicon carbide semiconductor device manufacturing method
JP2020181994A
Manufacturing method of silicon carbide polycrystal substrate
JP2021070609A
Rare earth-containing sic substrate, and sic composite substrate using same
WO2022168372A1