Pulp-molded product and method for producing the same

By integrating specific fiber types and additives, the pulp molded products achieve enhanced mechanical strength and accelerated dehydration, addressing the issues of low strength and prolonged dehydration times.

JP2024169224AInactive Publication Date: 2024-12-05TOPPAN HOLDINGS INC
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
JP2023086514
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-05-25
Publication Date
2024-12-05
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Pulp molded products often have low mechanical strength and require extended dehydration times during production.

Method used

Incorporating pulp with a fiber diameter of 4 μm or more, fine fibers with a diameter of 10 to 800 nm, a paper strength enhancer such as amphoteric polyacrylamide, and a drainage agent like cation-modified polyacrylamide, along with specific ratios and manufacturing processes involving dehydration and hot pressing.

Benefits of technology

Results in pulp molded products with high mechanical strength and rapid dehydration during production, achieving improved strength and reduced production time.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024169224000001_ABST
    Figure 2024169224000001_ABST
Patent Text Reader

Abstract

To realize a pulp-molded product which has high mechanical strength and can be dehydrated during production in a short time.SOLUTION: A pulp-molded product contains pulp with a fiber diameter of 4 μm or more, fine fibers with a fiber diameter in the range of 10 to 800 nm, a paper strengthening agent, and a drainage agent.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a pulp molded article. [Background technology]

[0002] Paper containers are widely recognized as environmentally friendly containers, and demand for them is growing.

[0003] Pulp molding is a technique for producing molded products from a slurry containing pulp and water. The use of pulp molding can increase the degree of freedom in the shape of paper-based articles such as paper containers. In pulp molding, the pulp in the slurry is generally deposited on a mold to form a pulp layer, which is then dehydrated and dried in an oven. The molded products obtained by this technique, i.e., pulp molded products, are excellent in heat resistance, cold resistance, moisture absorption and release, etc., which are characteristic physical properties of paper-based packaging materials, and have come to be widely used as paper tray containers for food, fixed cushioning materials for fruits, etc. (Patent Document 1).

[0004] However, the low strength of pulp molded products produced by pulp molding can be a problem. Patent Document 2 describes a technique for increasing the strength of pulp molded products. In the technique described in Patent Document 2, a predetermined amount of cellulose nanofibers is added to the pulp slurry relative to the pulp. The cellulose nanofibers are preferably obtained by subjecting the raw cellulose material, which is the raw material, to a chemical modification treatment such as carboxylation, and usually have an average fiber diameter within the range of 3 to 500 nm and an average length-to-diameter ratio within the range of 50 to 1000. In this technique, both the tensile strength and burst strength are improved by adding a predetermined amount of cellulose nanofibers. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] JP 2008-285188 A [Patent Document 2] JP 2018-59254 A Summary of the Invention [Problem to be solved by the invention]

[0006] An object of the present invention is to realize a pulp molded product which has high mechanical strength and can be dehydrated in a short time during production. [Means for solving the problem]

[0007] According to one aspect of the present invention, there is provided a pulp molded product comprising pulp having a fiber diameter of 4 μm or more, fine fibers having a fiber diameter within a range of 10 to 800 nm, a paper strength agent, and a drainage agent.

[0008] According to another aspect of the present invention, there is provided the pulp molded product according to the above aspect, wherein the fine fibers are fine cellulose fibers.

[0009] According to yet another aspect of the present invention, there is provided a pulp molded product according to any one of the above aspects, wherein the paper strength agent is an amphoteric polyacrylamide.

[0010] According to yet another aspect of the present invention, there is provided a pulp molded product according to any of the above aspects, wherein the drainage agent is a cationically modified polyacrylamide.

[0011] According to yet another aspect of the present invention, there is provided a pulp molded product according to any of the above aspects, wherein the fine fibers are fine cellulose fibers, the paper strength agent is an amphoteric polyacrylamide, and the drainage agent is a cationically modified polyacrylamide.

[0012] According to yet another aspect of the present invention, there is provided a pulp molded product according to any of the above aspects, wherein, when the mass of the pulp is 100 parts by mass, the amount of the fine fibers is in the range of 1.0 to 8.0 parts by mass, the amount of the paper strength agent is in the range of 0.1 to 5.0 parts by mass, and the amount of the drainage agent is in the range of 0.1 to 5.0 parts by mass.

[0013] According to yet another aspect of the present invention, there is provided a pulp molded product according to any of the above aspects, wherein the pulp has an average fiber diameter in the range of 15 to 40 μm, and the fine fibers have an average fiber diameter in the range of 50 to 500 nm.

[0014] According to yet another aspect of the present invention, there is provided a pulp molded product according to any of the above aspects, wherein the pulp has an average fiber length in the range of 0.5 to 2.0 mm, and the fine fibers have an average fiber length in the range of 10 to 1500 μm.

[0015] According to yet another aspect of the invention, the density is 0.5 to 1.1 g / m 3 The present invention provides a pulp molded article according to any of the above aspects, which is within the range of

[0016] According to yet another aspect of the present invention, there is provided a pulp molded product according to any of the above aspects, having a thickness in the range of 0.5 to 1.2 mm.

[0017] According to yet another aspect of the present invention, there is provided a pulp molded article according to any one of the above aspects, which is a container.

[0018] According to yet another aspect of the present invention, there is provided a method for producing a pulp molded product, the method including: preparing a slurry containing pulp having a fiber diameter of 4 μm or more, fine fibers having a fiber diameter in the range of 10 to 800 nm, a paper strength agent, a drainage agent, and water; depositing the pulp and the fine fibers on a three-dimensional mold to form a pulp layer; dehydrating the pulp layer to obtain an intermediate molded product; and sandwiching the undried intermediate molded product between a male mold and a female mold and heating it while applying pressure.

[0019] According to yet another aspect of the present invention, there is provided the method according to the above aspect, wherein the fine fibers are fine cellulose fibers.

[0020] According to yet another aspect of the present invention, there is provided a method according to any of the above aspects, wherein the paper strength agent is an amphoteric polyacrylamide.

[0021] According to yet another aspect of the present invention, there is provided a method according to any of the above aspects, wherein the drainage agent is a cationically modified polyacrylamide.

[0022] According to yet another aspect of the present invention, there is provided a method according to any of the above aspects, wherein the fine fibers are fine cellulose fibers, the paper strength agent is an amphoteric polyacrylamide, and the drainage agent is a cationically modified polyacrylamide.

[0023] According to yet another aspect of the present invention, there is provided a method relating to any of the above aspects, wherein, when the mass of the pulp is 100 parts by mass, the amount of the fine fibers is in the range of 1.0 to 8.0 parts by mass, the amount of the paper strength agent is in the range of 0.1 to 5.0 parts by mass, and the amount of the drainage agent is in the range of 0.1 to 5.0 parts by mass.

[0024] According to yet another aspect of the present invention, there is provided a method according to any of the above aspects, wherein the pulp has an average fiber diameter in the range of 15 to 40 μm and the fine fibers have an average fiber diameter in the range of 50 to 500 nm.

[0025] According to yet another aspect of the present invention, there is provided a method according to any of the above aspects, wherein the pulp has an average fiber length in the range of 0.5 to 2.0 mm and the fine fibers have an average fiber length in the range of 10 to 1500 μm.

[0026] According to yet another aspect of the invention, the density is 0.5 to 1.1 g / m 3 The method of any of the above aspects is provided to obtain a molded article within the range of

[0027] According to yet another aspect of the present invention there is provided a method according to any of the above aspects for obtaining a moulded article having a thickness in the range 0.5 to 1.2 mm.

[0028] According to yet another aspect of the present invention there is provided a method according to any of the above aspects for obtaining a container. Effect of the Invention

[0029] According to the present invention, it is possible to realize a pulp molded product which has high mechanical strength and can be dehydrated in a short time during production. [Brief description of the drawings]

[0030] [Figure 1] FIG. 1 is a perspective view showing a pulp molded product according to one embodiment of the present invention. [Diagram 2] FIG. 2 is a schematic diagram showing an example of a manufacturing apparatus that can be used to manufacture the pulp molded product of FIG. [Diagram 3] FIG. 3 is a diagram showing a pulp layer forming process in pulp molding using the apparatus of FIG. [Figure 4] FIG. 4 is a cross-sectional view that illustrates an example of a pulp layer formed on a mold. [Diagram 5] FIG. 5 is a diagram showing a dewatering process in pulp molding using the apparatus of FIG. [Figure 6] FIG. 6 is a diagram showing a conveying process of a pulp layer in pulp molding using the apparatus of FIG. [Figure 7] FIG. 7 is a diagram showing a hot press forming process in pulp molding using the apparatus of FIG. [Figure 8] FIG. 8 is a cross-sectional view that illustrates an example of a pulp molded product obtained by the heat pressing process. [Figure 9] FIG. 9 is a diagram showing a conveying process of a pulp molded product in pulp molding using the apparatus of FIG. [Figure 10]FIG. 10 is a diagram showing a state in which the transport process of FIG. 9 has been completed. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0031] Hereinafter, embodiments of the present invention will be described with reference to the drawings. The embodiments described below are more specific embodiments of any of the above aspects. The following items can be incorporated into each of the above aspects alone or in combination.

[0032] The embodiments described below are merely examples of configurations for embodying the technical idea of ​​the present invention, and the technical idea of ​​the present invention is not limited by the materials, shapes, structures, etc. of the components described below. Various modifications can be made to the technical idea of ​​the present invention within the technical scope defined by the claims.

[0033] In addition, elements having the same or similar functions are given the same reference numerals in the drawings referred to below, and duplicated explanations are omitted. In addition, the drawings are schematic, and the relationship between dimensions in one direction and dimensions in another direction, the relationship between the dimensions of one member and the dimensions of another member, etc. may differ from the actual ones.

[0034] <1> Pulp Molding FIG. 1 is a perspective view showing a pulp molded product according to one embodiment of the present invention. The pulp molded product MP2 shown in Fig. 1 is a container. This pulp molded product MP2 includes a bottom and a side wall, and is open at the top.

[0035] The bottom has a disk shape. The orthogonal projection of the bottom onto a plane perpendicular to the depth direction of the container may have a shape other than a circle, for example, a polygonal shape such as a square.

[0036] The side wall has a cylindrical shape extending upward from the edge of the bottom. The side wall expands in diameter from the bottom toward the opening. The inner and outer surfaces of the side wall may be perpendicular to the upper surface of the bottom. However, the pulp molded product MP2 in which the side wall expands in diameter from the bottom toward the opening is advantageous in realizing high releasability and is easy to stack.

[0037] The pulp molded product MP2 may have various shapes such as a cup shape, a bowl shape, a tray shape, a box shape, etc. The pulp molded product MP2 does not have to be a container as long as it is a three-dimensional molded product, i.e., a molded product having a three-dimensional shape, not a two-dimensional shape like a sheet.

[0038] The pulp molded product MP2 preferably has a thickness in the range of 0.5 to 1.2 mm. That is, the thickness of the wall of the pulp molded product MP2, here the thickness of the bottom and side walls, is preferably in the range of 0.5 to 1.2 mm. The pulp molded product MP2 more preferably has a thickness in the range of 0.6 to 1.2 mm, and further preferably has a thickness in the range of 0.7 to 1.0 mm.

[0039] A thick pulp molded product MP2 is bulky, especially when stacked. Also, increasing the thickness makes it difficult to mold the pulp molded product MP2 into a complex shape. On the other hand, making the walls of the pulp molded product MP2 thin is advantageous in that it allows dehydration and drying during production to be completed in a short time.

[0040] The pulp molded product MP2 has a density of 0.5 to 1.1 g / cm 3 The density of the pulp molded product MP2 is preferably in the range of 0.7 to 1.1 g / cm 3 More preferably, the range is 0.85 to 0.95 g / cm 3 It is more preferable that the ratio is in the range of 1:1.

[0041] When the density is low, it is difficult to achieve good strength. Pulp molded products MP2 with excessively high density usually have low flexibility and are prone to cracking.

[0042] The pulp molded product MP2 has a basis weight of 500 to 1100 g / m 2 and preferably in the range of 616 to 1056 g / m 2 It is more preferable that the ratio is in the range of 1.

[0043] Here, the thickness, density, and basis weight are values ​​obtained by the following method. That is, a square or rectangular test piece is cut out from a portion of the pulp molded product MP2 where the surface is not curved, and the dimensions, mass, and thickness are measured. For example, 10 test pieces each having a strip shape with a width of 15 mm and a length of 145 mm are cut out from the pulp molded product MP2. Then, the width, length, thickness, and mass of each test piece are measured. For example, a digital caliper is used to measure the width, length, and thickness. For example, an electronic balance is used to measure the mass. Then, the thickness, density, and basis weight of each test piece are calculated from the values ​​obtained for each test piece. Then, the above thickness, density, and basis weight are obtained by arithmetically averaging the values ​​obtained for the 10 test pieces.

[0044] The pulp molded product MP2 contains pulp, fine fibers, a paper strength agent, and a drainage agent. The fine fibers are preferably fine cellulose fibers. The components contained in the pulp molded product MP2 will be described below.

[0045] (pulp) The fiber diameter of the pulp is 4 μm or more. The fiber diameter of the pulp is preferably 7 μm or more. The fiber diameter of the pulp is preferably 100 μm or less, and more preferably 80 μm or less. The average fiber diameter of the pulp is preferably in the range of 15 to 40 μm, and more preferably in the range of 17 to 25 μm. Pulp suitable for the pulp molded product MP2 has a fiber diameter within the above range.

[0046] Here, the fiber diameter of the pulp can be measured from an image obtained using a microscope such as an optical microscope, and the average fiber diameter of the pulp can be obtained by arithmetically averaging the fiber diameters measured from the image.

[0047] The pulp molded product MP2 may contain only one type of pulp as the pulp, or may contain multiple types of pulp. For example, the pulp molded product MP2 may contain only a first pulp having an average fiber diameter in the range of 15 to 22 μm as the pulp, or may contain the first pulp and a second pulp having an average fiber diameter in the range of 22 to 40 μm. The proportion of the first pulp in the pulp is preferably 50 mass% or more.

[0048] The average fiber length of the pulp is preferably in the range of 0.5 to 2.0 mm, more preferably in the range of 0.90 to 1.60 mm, and even more preferably in the range of 0.91 to 1.59 mm. By increasing the average fiber length, it becomes possible to complete drying in a shorter time during production. However, if the average fiber length is excessively increased, the strength of the pulp molded product MP2 may decrease.

[0049] Here, the average fiber length of the pulp is a value obtained by the following method. That is, first, a 5 g test piece is obtained from the pulp molded product MP2. Next, the test piece is finely shredded and immersed in 500 mL of water overnight. Then, the test piece is stirred with a stirrer to disintegrate the pulp from each other. In this way, a dispersion containing pulp is obtained. Next, 10 g is taken from the dispersion and diluted with water. This dilution is performed so that the total mass becomes 200 g. Using the sample obtained in this way, fiber length measurement is performed according to JIS P8226-2:2011 "Pulp - Fiber length measurement method by optical automatic analysis method - Part 2: Non-polarized method". The average fiber length of the pulp is the length-weighted average fiber length L L Refers to...

[0050] (Fine Fiber) The fine fibers have a fiber diameter in the range of 10 to 800 nm, and preferably in the range of 10 to 500 nm.

[0051] Fine fibers with a small fiber diameter can fill the gaps between adjacent pulps without interfering with hydrogen bonding between the pulps. Therefore, in order to achieve excellent strength, it is preferable that the fine fibers have a small fiber diameter. However, the fine fibers do not include cellulose nanofibers with an average fiber diameter of less than 10 nm.

[0052] On the other hand, some of the fine fibers may be detached from the pulp layer together with water during the dehydration process in the production of the pulp molded product MP2. Fine fibers with a large fiber diameter are less likely to be detached. Furthermore, fine fibers with a large fiber diameter do not excessively increase the residual moisture content of the pulp layer immediately before the drying process in the production of the pulp molded product MP2. Therefore, fine fibers with a large fiber diameter are advantageous in completing the drying process in a short time in the production of the pulp molded product MP2.

[0053] The average fiber diameter of the fine fibers is preferably in the range of 50 to 500 nm, and more preferably in the range of 100 to 300 nm. The fine fibers suitable for the pulp molded product MP2 have a fiber diameter within the above range.

[0054] Here, the fiber diameter of the fine fibers can be measured from an image obtained using a microscope such as a scanning electron microscope, etc. Also, the average fiber diameter of the fine fibers can be obtained by randomly selecting 20 fine fibers from the image and arithmetically averaging the fiber diameters measured for the selected fine fibers.

[0055] The average fiber length of the fine fibers is preferably within the range of 10 to 1500 μm.

[0056] Here, the average fiber length of the fine fibers refers to the value obtained according to the above-mentioned "Method for obtaining the average fiber length of pulp."

[0057] As described above, the fine fibers are preferably fine cellulose fibers. For example, commercially available "microfibrillated cellulose" can be used as the fine cellulose fibers. For example, the Celish (registered trademark) series (e.g., KY100G, KY100S) manufactured by Daicel Miraize Co., Ltd.; the Valmet (registered trademark) series manufactured by Valmet Co., Ltd.; or the Exilva (registered trademark) series (e.g., Exilva F-01V, Exilva P-01V) manufactured by Borregaard Co., Ltd. can be used as the fine cellulose fibers.

[0058] When the mass of the pulp is taken as 100 parts by mass, the amount of the fine fibers is preferably in the range of 1.0 to 8.0 parts by mass, more preferably in the range of 2.0 to 6.0 parts by mass, and even more preferably in the range of 3.5 to 4.5 parts by mass. If this ratio is reduced, the effect of improving the strength of the pulp molded product MP2 by adding the fine cellulose fibers is reduced. If this ratio is increased, the remaining moisture content of the pulp layer immediately before the drying step during the production of the pulp molded product MP2 increases. Therefore, it may take a longer time to dry the pulp molded product MP2 during the production of the pulp molded product MP2.

[0059] (Paper strength agent) The paper strength enhancer is preferably an amphoteric polyacrylamide. The amphoteric polyacrylamide is a polyacrylamide containing cationic functional groups and anionic functional groups in the molecule to the same extent. The weight average molecular weight of the amphoteric polyacrylamide is, for example, about 2 million to 6 million. When the molecular weight of the paper strength enhancer is increased, the intermolecular force interaction between pulp and pulp becomes stronger, and the effect of improving the paper strength of the pulp tends to increase.

[0060] The paper strength enhancer may be, for example, one commercially available as an "amphoteric polyacrylamide-based paper strength enhancer." Examples of the paper strength enhancer include the DS series (e.g., DS4424) manufactured by Seiko PMC Co., Ltd.; the Polystron (registered trademark) series (e.g., PS-1280) manufactured by Arakawa Chemical Industries Co., Ltd.; or the Hermide (registered trademark) EX-200 series, EX-300 series, EX-400 series, and KS series manufactured by Harima Chemical Industries Co., Ltd.

[0061] When the mass of the pulp is taken as 100 parts by mass, the amount of the paper strength agent is preferably in the range of 0.1 to 5.0 parts by mass, more preferably in the range of 0.1 to 3.0 parts by mass, and even more preferably in the range of 1.0 to 2.5 parts by mass. Use of the paper strength agent can increase the strength of the pulp molded product MP2.

[0062] (Drainage agent) The drainage agent is preferably a cationically modified polyacrylamide. The cationically modified polyacrylamide is a polyacrylamide that contains both cationic and anionic functional groups in the molecule, but contains more cationic functional groups than anionic functional groups. The cationically modified polyacrylamide can be prepared, for example, by Hoffman modification. Since the cationically modified polyacrylamide contains many cationic functional groups, it self-fixes to the pulp. As a result, the pulps are bonded to each other and the gaps between the pulps are enlarged, improving drainage. Such drainage performance can be improved by the cationically modified polyacrylamide containing many cationic functional groups.

[0063] The filtering agent may be, for example, a commercially available "polyacrylamide filtering agent." For example, the filtering agent may be the RD series (e.g., RD-7144) manufactured by Seiko PMC Co., Ltd. or the Polystron (registered trademark) series (e.g., PS-505) manufactured by Arakawa Chemical Industries Co., Ltd.

[0064] When the mass of the pulp is taken as 100 parts by mass, the amount of the filtering agent is preferably in the range of 0.1 to 5.0 parts by mass, more preferably in the range of 0.1 to 1.0 parts by mass, and even more preferably in the range of 0.15 to 0.30 parts by mass. By using the filtering agent, the slurry suction time during the production of the pulp molded product MP2 can be shortened, and productivity can be increased.

[0065] The pulp molded product MP2 has an ISO ring crush compressive strength in the range of, for example, 9.5 to 20.0 kN / m. The ISO ring crush compressive strength of the pulp molded product MP2 is preferably in the range of 9.5 to 16.5 kN / m.

[0066] Here, the ISO ring crush compressive strength of the pulp molded product MP2 is a value obtained by the method specified in JIS P8126:2015 "Compressive strength test method - Ring crush method". The compressive strength is determined by clamping a long and thin test piece bent into a cylindrical (ring-like) shape between parallel upper and lower compression plates, applying a compressive load to cause buckling, obtaining the maximum load, and dividing the obtained maximum load by the length of the test piece. In this test method, the long and thin test piece is prepared by cutting a strip-shaped test piece with a width of 15 mm and a length of 145 mm from the pulp molded product MP2.

[0067] The pulp molded product MP2 with a large ISO ring crush compressive strength is unlikely to buckle even when a large load is applied. However, if the ISO ring crush compressive strength of the pulp molded product MP2 is too large, it becomes more susceptible to breakage when an impact load is applied when dropped, etc.

[0068] The pulp suspension obtained by dispersing the pulp contained in the pulp molded product MP2 in water preferably has a Canadian Standard Freeness (CSF) in the range of 400 to 650 mL, more preferably in the range of 450 to 600 mL. The Canadian Standard Freeness of the pulp suspension is an index that indicates the degree of drainage of the pulp.

[0069] If the Canadian standard freeness is high, the strength of the pulp molded product MP2 tends to decrease. If the Canadian standard freeness is low, the strength of the pulp molded product MP2 increases, but the pulp molded product MP2 is likely to become distorted during drying, which tends to cause unevenness on the surface of the pulp molded product MP2. Also, if the Canadian standard freeness is low, it tends to take a long time to dry during production.

[0070] Here, the above Canadian standard freeness is a value obtained by the following method. First, a test piece is obtained from the pulp molded product MP2, and a dispersion containing pulp is obtained by the same method as above. Next, this dispersion is diluted with water so that the solid content concentration is 0.3 mass % to obtain an aqueous suspension of pulp. Next, using 1 L of this suspension, a measurement specified in JIS P8121-2:2012 "Pulp-Freeness Test Method-Part 2: Canadian Standard Freeness Method" is performed. For this measurement, for example, a Canadian Freeness Tester manufactured by Kumagai Riki Kogyo Co., Ltd. is used. In addition, the measured value is corrected by referring to a correction table for the temperature of the suspension that has been measured in advance. In this manner, the Canadian standard freeness is obtained.

[0071] As described above, the pulp molded product MP2 contains, in addition to pulp, fine fibers, a paper strength agent, and a drainage agent. With this configuration, the pulp molded product MP2 has high mechanical strength and can complete dewatering in a short time during production. As will be demonstrated in the examples described later, if at least one of the fine fibers, paper strength agent, and drainage agent is missing from the pulp molded product MP2, the two effects described above cannot be achieved at the same time.

[0072] <2> Pulp molding manufacturing equipment Next, a manufacturing apparatus that can be used to manufacture the pulp molded product MP2 will be described. FIG. 2 is a schematic diagram showing an example of a manufacturing apparatus that can be used to manufacture the pulp molded product of FIG.

[0073] The manufacturing apparatus 1 shown in FIG. 2 includes a support 10, a first station 20, a second station 30, and a third station 40.

[0074] The support 10 includes a frame and a rail installed on the upper portion thereof.

[0075] The first station includes a container 210 , a lifting device 220 , a cover body 230 , a mold 240 , a moving device 250 , a lifting device 260 , and an upper mold 270 .

[0076] The container 210 is placed within the frame of the support 10. The container 210 is open at the top. The container 210 contains a slurry S containing pulp, fine cellulose fibers, a crosslinking agent, and water.

[0077] The lifting device 220 is attached to the frame of the support 10 above the container 210. The lifting device 220 includes, for example, a hydraulic cylinder. The lifting device 220 supports a cover body 230. The lifting device 220 can raise and lower the cover body 230 at the position of the opening of the container 210.

[0078] The cover body 230 is a hollow body having an opening at the top. A pump (not shown) is connected to the cover body 230.

[0079] The mold 240 is fixed to the opening of the cover body 230. Specifically, the mold 240 is fixed to the opening of the cover body 230 such that one surface of the mold 240 and a space adjacent to the mold 240 are surrounded by the mold 240 and the cover body 230.

[0080] The mold 240 is a mold that is liquid permeable. The mold 240 has a three-dimensional shape. That is, the mold 240 has one or more convex portions and / or one or more concave portions on the surface on which the pulp, etc. are accumulated. Specifically, the outer surface of the mold 240, i.e., the back surface of the surface adjacent to the above-mentioned space, has a shape corresponding to a pulp molded product. Here, the mold 240 is a male mold with a protruding upper surface.

[0081] The mold 240 includes, for example, a mold body having a number of through holes and an outer surface having a shape corresponding to the pulp molded product, and a mesh body arranged on and along the outer surface of the mold body.

[0082] The moving device 250 is movable between the first station 20 and the second station 30 along the rails of the support 10. The moving device 250 includes, for example, a motor as a power source. The moving device 250 is equipped with an elevator device 260, which can be transported between the first station 20 and the second station 30.

[0083] As described above, the lifting device 260 is attached to the moving device 250. The lifting device 260 includes, for example, a hydraulic cylinder. The lifting device 260 supports the upper mold 270. The lifting device 260 can raise and lower the upper mold 270.

[0084] The upper mold 270 is a holder that sandwiches a pulp layer, which will be described later, between itself and the mold 240 and holds the pulp layer by vacuum suction. The lower surface of the upper mold 270 has a shape corresponding to the outer surface of the mold 240. Here, the upper mold 270 is a female mold with a concave lower surface. The upper mold 270 has, for example, a large number of through holes, one end of which is open at the lower surface and the other end of which is connected to a pump.

[0085] The second station 30 is provided near the first station 20. The second station 30 includes a base 310, a lower mold 320, a moving device 330, a pressing device 340, and an upper mold 350.

[0086] The base 310 is placed within the frame of the support 10. On the base 310, a lower mold 320 is placed.

[0087] The lower mold 320 is a mold that is permeable to gas and / or liquid. The upper surface of the lower mold 320 has a shape corresponding to the outer surface of the mold 240. Here, the lower mold 320 is a male mold with a protruding upper surface. The lower mold 320 has, for example, a large number of through holes, and has a smooth surface that has a shape corresponding to the outer surface of the mold 240.

[0088] The moving device 330 is movable between the second station 30 and a fourth station (not shown) along the rails of the support 10. The moving device 330 includes, for example, a motor as a power source. When the moving device 330 is located at the second station 30, the movement of the moving device 330 in the up-down, left-right, and front-rear directions can be restricted by a locking mechanism. In addition, a pressing device 340 is attached to the moving device 330, and the pressing device 340 can be transported between the second station 30 and the fourth station.

[0089] As described above, the press device 340 is attached to the moving device 330. The press device 340 includes, for example, a hydraulic cylinder. The press device 340 supports the upper die 350. The press device 340 can raise and lower the upper die 350.

[0090] The upper mold 350 is a mold that is neither gas permeable nor liquid permeable. The lower surface of the upper mold 350 has a shape corresponding to the outer surface of the mold 240. Here, the upper mold 350 is a female mold with a concave lower surface. The upper mold 350 has a smooth surface that has a shape corresponding to the outer surface of the mold 240.

[0091] The second station 30 further includes a heater and a pump (neither of which are shown). The heater heats both the lower mold 320 and the upper mold 350. The pump is connected to the lower space of the lower mold 320.

[0092] The third station 40 is provided near the second station 30. The third station 40 includes a platform 410, a moving device 420, a lifting device 430, and a holder 440.

[0093] The base 410 is installed within the frame of the support 10. On the base 410, a pulp molded product is placed.

[0094] The moving device 420 is movable between the second station 30 and the third station 40 along the rails of the support 10. The moving device 420 includes, for example, a motor as a power source. The moving device 420 is provided with an elevator device 430, which can be transported between the second station 30 and the third station 40.

[0095] As described above, the lifting device 430 is attached to the moving device 420. The lifting device 430 includes, for example, a hydraulic cylinder. The lifting device 430 supports the holder 440. The lifting device 430 can raise and lower the holder 440.

[0096] The holder 440 is a holder that holds a pulp molded product (described later) by vacuum suction. The lower surface of the holder 440 has a shape corresponding to the outer surface of the mold 240. Here, the holder 440 has a concave lower surface. The holder 440 has, for example, a number of through holes that open at one end at the lower surface and are connected at the other end to a pump.

[0097] <3> Manufacturing method of pulp molded products In a manufacturing method according to one embodiment of the present invention, for example, a pulp molded product MP2 is manufactured using the above-mentioned manufacturing apparatus 1. This will be described with reference to FIGS.

[0098] FIG. 3 is a diagram showing a pulp layer forming step in pulp molding using the apparatus of FIG. 2. FIG. 4 is a cross-sectional view showing an example of a pulp layer formed on a mold. FIG. 5 is a diagram showing a dewatering step in pulp molding using the apparatus of FIG. 2. FIG. 6 is a diagram showing a pulp layer conveying step in pulp molding using the apparatus of FIG. 2. FIG. 7 is a diagram showing a heat press molding step in pulp molding using the apparatus of FIG. 2. FIG. 8 is a cross-sectional view showing an example of a pulp molded product obtained by the heat press step. FIG. 9 is a diagram showing a conveying step of a pulp molded product in pulp molding using the apparatus of FIG. 2. FIG. 10 is a diagram showing a state in which the conveying step of FIG. 9 has been completed.

[0099] In this method, first, a slurry S is prepared. As described above, the slurry S contains pulp, fine fibers, a paper strength agent, a drainage agent, and water. The slurry S is a highly viscous suspension in which the pulp and fine fibers are dispersed in water, and the paper strength agent and the drainage agent are dissolved or dispersed in water.

[0100] The pulp contained in the slurry S has substantially the same characteristics as those described above for the pulp contained in the pulp molded product MP2.

[0101] There is no particular limitation on the type of pulp used in the slurry S. Examples of pulp include wood pulp, non-wood pulp, and waste paper, with wood pulp and non-wood pulp being preferred. From the viewpoint of environmental considerations such as forest conservation and utilization of unused resources, it is preferable to use non-wood pulp.

[0102] Pulps can be classified according to the difference in the preparation method. For example, examples of wood pulp include chemical pulps such as kraft pulp (KP), sulfite pulp (SP), and soda pulp (AP); semi-chemical pulps such as semi-chemical pulp (SCP) and chemi-ground wood pulp (CGP); groundwood pulp (GP), and thermomechanical pulp (TMP). Among these, it is preferable to use chemical pulp. The pulp may be bleached pulp or unbleached pulp.

[0103] Wood pulp can be classified according to the raw material. Examples of wood pulp include coniferous pulp and hardwood pulp. Examples of coniferous pulp include pulp obtained from the fir and pine genus. Examples of hardwood pulp include pulp obtained from the acacia, eucalyptus, beech, and poplar genus (e.g., poplar).

[0104] Non-wood pulp is obtained from fibers extracted from the bark, stems, leaves, and leaf sheaths of plants. Specific examples include pulps obtained from cotton linters, cotton, linen, hemp, ramie, straw, esparto, Manila hemp, sisal, jute, flax, kenaf, bamboo, sugarcane, ganpi, mitsumata, kozo, and mulberry. Among these, bamboo and sugarcane pulps are preferred.

[0105] These pulps can be used alone or in combination of two or more kinds in any desired ratio.

[0106] Pulp has different fiber lengths and the like depending on its raw material and manufacturing method. For example, pulp made from sugarcane generally has a shorter average fiber length than pulp made from bamboo. The average fiber length of pulp can be adjusted by any method, for example, mechanical treatment such as beating or crushing. Thus, pulp having certain characteristics can be obtained, for example, by selecting an appropriate one from multiple types of pulp, or by appropriately combining two or more types of pulp. As the pulp, it is preferable to use non-wood pulp, and it is preferable to use pulp made from sugarcane, pulp made from bamboo, or a combination thereof.

[0107] The pulp content of the slurry S is preferably in the range of 0.01 to 3.0% by mass, more preferably in the range of 0.01 to 0.5% by mass. If the pulp content is low, it is difficult to achieve high productivity. If the pulp content is high, there is a possibility that the thickness of the pulp layer will vary widely.

[0108] The fine fibers contained in the slurry S have substantially the same characteristics as those described above for the fine fibers contained in the pulp molded product MP2.

[0109] As described above for the fine fibers contained in the pulp molded product MP2, the amount of fine fibers contained in the slurry S is preferably in the range of 1.0 to 8.0 parts by mass per 100 parts by mass of pulp, more preferably in the range of 2.0 to 6.0 parts by mass, and even more preferably in the range of 3.5 to 4.5 parts by mass.

[0110] The strength agent contained in the slurry S has substantially the same characteristics as those described above for the strength agent contained in the pulp molded product MP2.

[0111] As described above for the paper strength agent contained in the pulp molded product MP2, the amount of the paper strength agent contained in the slurry S is preferably in the range of 0.1 to 5.0 parts by mass per 100 parts by mass of pulp, more preferably in the range of 0.1 to 3.0 parts by mass, and even more preferably in the range of 1.0 to 2.5 parts by mass.

[0112] The filterage agent contained in the slurry S has substantially the same characteristics as those described above for the filterage agent contained in the pulp molded product MP2.

[0113] As described above for the filterability agent contained in the pulp molded product MP2, the amount of filterability agent contained in the slurry S is preferably in the range of 0.1 to 5.0 parts by mass per 100 parts by mass of pulp, more preferably in the range of 0.1 to 1.0 part by mass, and even more preferably in the range of 0.15 to 0.30 parts by mass.

[0114] The slurry S may further contain other additives. As the additives, organic low molecular weight materials, organic high molecular weight materials, inorganic materials, or combinations thereof may be used, and examples of such additives include agents that impart water resistance or oil resistance (e.g., sizing agents), and the agent may be selected according to the performance requirements of the pulp molded container.

[0115] The proportion of other additives in the total of pulp, fine fibers, paper strength agent, drainage agent, and other additives is preferably 3 mass % or less, and more preferably 1 mass % or less.

[0116] Next, the slurry S is supplied into the container 210. Then, as shown in FIG. 3, the cover body 230 is lowered by the lifting device 220 until the top surface of the mold 240 is positioned sufficiently below the liquid level of the slurry S. In this state, the pump is driven to reduce the pressure in the space surrounded by the cover body 230 and the mold 240. This causes a flow of the slurry S across the mold 240, and a mixture of pulp and fine fibers is deposited on the mold 240. In this manner, a pulp layer MP1 is formed on the mold 240, as shown in FIG. 4.

[0117] Next, while the pump is still running, as shown in FIG. 5, the lifting device 220 lifts the cover body 230 to position the lower part of the mold 240 sufficiently above the liquid level of the slurry S. This reduces the pressure and dewaters the pulp layer MP1. Next, the lifting device 260 is driven to lower the upper mold 270 until its lower surface comes into contact with the pulp layer MP1. Note that the pulp layer MP1 is not shown in FIG. 5. This dewatering process is performed without heating either the upper mold 270 or the mold 240.

[0118] The decompression time in the dehydration step is preferably within the range of 1 to 60 seconds, and more preferably within the range of 1 to 10 seconds.

[0119] The moisture content of the pulp layer MP1 immediately after dehydration is preferably in the range of 40 to 90% by mass, more preferably in the range of 50 to 70% by mass, and even more preferably in the range of 60 to 70% by mass. If the moisture content is low, the movement of the fibers in the in-plane direction in the pulp layer may be insufficient in the heat pressing process. If the moisture content is high, the movement of the fibers in the in-plane direction in the pulp layer may be excessive in the heat pressing process, or the shape retention of the pulp layer MP1 may be insufficient during the period from the end of the dehydration process to the start of the heat pressing process.

[0120] After the decompression and pressurization of the space are stopped, the pump is driven to adsorb and hold the pulp layer MP1 to the upper mold 270. Note that the suction by the pump and upper mold 270 does not cause further dehydration of the pulp layer MP1.

[0121] Next, with the pulp layer MP1 being adsorbed and held by the upper mold 270, the lifting device 260 is driven to lift the upper mold 270 as shown in Fig. 2. This causes the pulp layer MP1 to be peeled off from the mold 240.

[0122] Next, the moving devices 250 and 330 are driven to move the pressing device 340 and the upper mold 350 from the second station 30 to the fourth station, and the lifting device 260 and the upper mold 270 from the first station 20 to the second station 30, as shown in FIG. 6. Then, the lifting device 260 is driven to lower the upper mold 270 until the pulp layer MP1 contacts the lower mold 320. Then, the suction by the pump and the upper mold 270 is stopped, and the pulp layer MP1 is released from the upper mold 270. Next, the lifting device 260 is driven to raise the upper mold 270. In this way, the pulp layer MP1 is transferred from the first station 20 to the second station 30, and the pulp layer MP1 is placed on the lower mold 320.

[0123] Next, the moving devices 250 and 330 are driven to move the lifting device 260 and the upper mold 270 from the second station 30 to the first station 20 as shown in FIG. 2, and the pressing device 340 and the upper mold 350 are moved from the fourth station to the second station 30. Next, the pressing device 340 is driven to lower the upper mold 350 as shown in FIG. 7. Then, the pulp layer MP1 sandwiched between the upper mold 350 and the lower mold 320 is pressurized. At the same time, the heater is driven to heat the pulp layer MP1. Furthermore, at the same time, the pump is driven to suck and remove water and / or water vapor from the space sandwiched between the upper mold 350 and the lower mold 320. This adjusts the surface shape of the pulp layer MP1, and densifies and dries the pulp layer MP1. In this manner, the pulp molded product MP2 shown in FIG. 8 is obtained.

[0124] The moisture content of the pulp layer MP1 immediately before the start of the heat pressing step is substantially equal to the moisture content of the pulp layer MP1 immediately after the completion of the dewatering step.

[0125] In this heat pressing step, the pressing pressure is set to a range of 0.1 to 3.0 MPa. More preferably, the pressing pressure is set to a range of 0.5 to 2.0 MPa. If the pressing pressure is low, a high-density pulp molded product MP2 may not be obtained. The pulp layer MP1 contains pulp and fine fibers with short fiber lengths. Such pulp and fine fibers are likely to move within the pulp layer MP1, particularly when the pressing pressure is excessively high. Therefore, if the pressing pressure is excessively high, the thickness of the pulp molded product MP2 is likely to vary.

[0126] In this heat pressing process, the heating temperature of the pulp layer MP1, i.e., the temperature of the upper mold 350 or the lower mold 320 heated by the heater, is in the range of 130 to 250°C. This temperature is preferably in the range of 150 to 190°C. The pulp layer MP1 contains pulp with short fiber length and fine fibers, so water vapor does not easily escape to the outside. Therefore, if the heating temperature is low, it takes a long time to dry the pulp layer MP1. If the heating temperature is high, the pulp layer MP1 shrinks more as it dries, which may result in greater distortion in the pulp molded product MP2.

[0127] The pressing time in the heat pressing step depends on the heating temperature, the shape of the molded product, etc., but is preferably within the range of 40 to 120 seconds, and more preferably within the range of 50 to 80 seconds.

[0128] Upon completing the above-mentioned hot pressing process, the press device 340 is driven so that the upper die 350 rises, and the pulp molded product MP2 is separated from the upper die 350.

[0129] Next, the moving devices 330 and 420 are driven to move the press device 340 and the upper mold 350 from the second station 30 to the fourth station, and the lifting device 430 and the holder 440 from the third station 40 to the second station 30, as shown in Fig. 9. Subsequently, the lifting device 430 is driven to lower the holder 440 until it comes into contact with the pulp molded product MP2. Air is ejected from inside the lower mold to release the pulp molded product MP2 from the lower mold, and then the pump is driven to adsorb and hold the pulp molded product MP2 on the holder 440. Next, the lifting device 430 is driven to lift the holder 440 while the pulp molded product MP2 is held by suction on the holder 440. Next, the moving devices 330 and 420 are driven to move the lifting device 430 and the holder 440 from the second station 30 to the third station 40, and move the press device 340 and the upper mold 350 from the fourth station to the second station 30, as shown in FIG. 10. Next, the suction by the pump and the holder 440 is stopped, and the pulp molded product MP2 is released from the holder 440. In this way, the pulp molded product MP2 is transferred from the second station 30 to the third station 40, and the pulp molded product MP2 is placed on the platform 410. In this manner, a pulp molded product MP2 is produced.

[0130] Thereafter, as necessary, the pulp molded product MP2 is subjected to post-treatment, such as printing with a pattern or plain printing, coating, or a combination thereof. The coating layer formed by the post-treatment is, for example, a layer containing a chemical that imparts water resistance or oil resistance, a layer filled with a material that imparts heat insulation, a layer foamed with a foaming agent, or a combination thereof. By performing the post-treatment, for example, it is possible to further improve the cosmetic properties of the pulp molded product MP2 or to impart new functions to the pulp molded product MP2.

[0131] According to the above method, it is possible to produce a pulp molded article MP2 that has high mechanical strength and that can be dehydrated completely in a short time during production.

[0132] Furthermore, the pulp molded product MP2 obtained by the above method has excellent surface properties, the reason for which will be explained below.

[0133] If drying is performed using an oven instead of the heat pressing process, the pulp layer will have large unevenness on the surface due to shrinkage. In addition, this method does not densify the pulp layer sufficiently, and therefore the pulp molded product will have high porosity. Therefore, in this case, it is not possible to produce a pulp molded product with excellent surface properties.

[0134] In addition, when drying is performed using an oven after the dehydration step, and the dried product is moistened as necessary and subjected to a heat press treatment, the height difference of the unevenness generated on the surface due to drying can be reduced by the subsequent moistening and heat press treatment. In addition, the porosity can be reduced by the moistening and heat press treatment. However, the height difference of the unevenness generated on the surface due to drying using an oven is very large, so it cannot be sufficiently reduced by the subsequent moistening and heat press treatment. In addition, even if moistening and heat press treatment are performed after drying, it is difficult to sufficiently reduce the porosity.

[0135] In the method described with reference to Figures 2 to 10, the pulp layer MP1 is dried in the heat pressing step. That is, in the above method, the heat pressing step is performed after the dehydration step without going through the drying step. The fibers used are pulp and fine fibers each having the above-mentioned fiber diameter.

[0136] Since no drying step is performed before the heat pressing step, the surface of the pulp layer MP1 does not have large unevenness with large height differences. In the heat pressing step, the upper mold 350 and the lower mold 320 prevent deformation of the pulp layer MP1 due to drying. In addition, since the heat pressing step is performed on the pulp layer MP1 that has a high moisture content and an average fiber length of the pulp within the above-mentioned range, the fibers can move appropriately in the in-plane direction within the pulp layer MP1. The pulp layer MP1 can be densified without causing thickness variations.

[0137] 2 to 10, a pulp-molded product MP2 with excellent surface properties can be manufactured. Specifically, a pulp-molded product MP2 is obtained that has a region on its surface where one or more of the arithmetic mean roughness Ra, the maximum height roughness Rz, and the average length RSm of the roughness curve element are small. Such a pulp-molded product MP2 has excellent cosmetic properties and is easy to form a printed layer or a coating layer on.

[0138] The arithmetic mean roughness Ra is preferably in the range of 2 to 10 μm, more preferably in the range of 2.5 to 4.5 μm. The maximum height roughness Rz is preferably in the range of 10 to 60 μm, more preferably in the range of 15 to 30 μm. The average length RSm of the roughness curvilinear elements is preferably in the range of 90 to 300 μm, more preferably in the range of 90 to 150 μm, and even more preferably in the range of 90 to 130 μm.

[0139] Here, "arithmetic mean roughness Ra," "maximum height roughness Rz," and "average length of roughness curve element RSm" are surface texture parameters defined in JIS B0601: 2001. The surface texture parameters are measured using, for example, a Mitutoyo surface roughness measuring instrument SJ-210 (tip radius 2 μm, measuring force 0.75 mN) under the following conditions. Filter:Gasussian Cutoff λc: 0.25mm Cutoff λs: 8μm Measurement speed: 0.25mm / s Number of sections: 5 A plate-shaped piece is taken from the pulp molded product MP2, measurements are taken at any five points, and the average value is calculated.

[0140] The entire surface of the pulp molded product MP2 may have the above-mentioned surface properties, or only a portion of the surface may have the above-mentioned surface properties. For example, only the area including the portion where post-treatment such as printing is performed may have the above-mentioned surface properties, and the other areas may not have the above-mentioned surface properties. Alternatively, one side of the pulp molded product MP2 may have the above-mentioned surface properties, and the back side may not have the above-mentioned surface properties. Such a structure can be realized, for example, by making the surface properties of the part of the surface of the upper mold 350 and the lower mold 320 that contacts the pulp layer MP1 different from the other areas.

[0141] In addition, according to the method described with reference to Figures 2 to 10, a pulp molded product MP2 having a small standard deviation in basis weight can be manufactured. The standard deviation of the basis weight of the pulp molded product MP2 is preferably 30 g / m 2 More preferably, it is 15 g / m or less. 2 The lower limit of this standard deviation is zero, and according to one example, 2 g / m 2 It is.

[0142] Here, the standard deviation of the basis weight of the pulp molded product MP2 is a value obtained by the following method.

[0143] First, nine test pieces, each of which has a rectangular shape with a width of 15 mm and a length of 40 mm, are cut out from multiple regions located on a certain plane of the pulp molded product MP2. Next, the mass of these test pieces is measured. After that, the mass and area (600 mm2) of each test piece are recorded. 2 The basis weight is calculated from the basis weight thus obtained. The standard deviation is calculated from the basis weight thus obtained.

[0144] Next, nine test pieces are cut out from multiple regions located in another plane of the pulp molded product MP2 in the same manner as above. The masses of these test pieces are also measured, and the basis weights and their standard deviations are calculated.

[0145] If the pulp molded product MP2 has additional surfaces, test pieces are cut out, the masses are measured, and the basis weights and their standard deviations are calculated for each of the remaining surfaces in the same manner as above. The maximum value of these standard deviations is set as the standard deviation of the basis weight of the pulp molded product MP2.

[0146] The inventors believe that the reason why the method described with reference to Figures 2 to 10 (hereinafter referred to as the first method) makes it possible to produce pulp molded products MP2 with a small standard deviation of basis weight is as follows.

[0147] The pulp molded product can also be produced, for example, by the method described below (hereinafter referred to as the second method).

[0148] In the second method, first, a female mold is prepared as a mold. This mold includes a mold body having a large number of through holes and a recessed upper surface corresponding to a shape of a pulp molded product, and a mesh body provided on and along the inner surface of the mold body.

[0149] Next, the mold is placed so that its opening faces upward. A slurry containing pulp and water is then fed into the cavity of the mold to fill the mold. The slurry is then continued to be fed into the mold, and the pulp is deposited on the mesh. The slurry is fed into the mold so that the slurry in the mold is under pressure.

[0150] After a sufficient amount of pulp has accumulated on the mesh, the supply of the slurry into the mold is stopped. Then, the water remaining in the mold is discharged from the mold, for example, by injecting compressed air into the mold.

[0151] Next, the pulp layer is pressed between the cutting mold and the upper mold, which is a male mold, to dehydrate the pulp layer. This dehydration step is performed without heating either the upper mold or the cutting mold. The moisture content of the pulp layer immediately after dehydration is set to be the same as the moisture content of the pulp layer MP1 immediately after dehydration in the first method.

[0152] Next, the pulp layer is adsorbed and held by the upper mold, and in this state the upper mold is raised, whereby the pulp layer is peeled off from the mold.

[0153] Next, the upper mold, which is holding the pulp layer by suction, is moved to the position of the lower mold, which is a female mold. The upper mold is then lowered until the pulp layer comes into contact with the lower mold. After that, the suction is stopped and the pulp layer is released from the upper mold. In this way, the pulp layer is placed on the lower mold.

[0154] Next, the pulp layer is sandwiched between an upper mold and a lower mold for a hot press, and the pulp layer between them is pressurized. At the same time, the heater is driven to heat the pulp layer. At the same time, the pump is driven to suck and remove water and / or water vapor from the space sandwiched between the upper mold and the lower mold. In the second method, a pulp molded product is obtained as described above.

[0155] In the second method, during the period from when the supply of the slurry into the mold is started until the mold is completely filled with the slurry, a flow of the slurry circulating inside the mold may occur. This circulating flow can prevent the settling of the pulp. However, since the second method requires the mold to be filled with the slurry, the mold cannot be designed to allow water to be quickly discharged. Therefore, after the mold is completely filled with the slurry, even if the pressure of the slurry is increased, a circulating flow of the slurry sufficient to prevent the settling of the pulp does not occur, and the slurry in the mold causes the settling of the pulp.

[0156] As a result, the amount of pulp deposited on the sidewall of the mold is greater at the bottom than at the top. If the slurry is supplied until a sufficient amount of pulp is deposited on the top of the sidewall of the mold, an excessive amount of pulp will be deposited at the bottom of the mold. If excessive pulp is deposited, the amount of pulp deposited will vary greatly. For example, there may be a large difference in the amount of pulp deposited near the through holes provided in the mold body and at a position distant from them.

[0157] Thus, the second method causes a large variation in the amount of pulp deposition. During the hot press treatment, the fibers can move in the in-plane direction within the pulp layer, but the movement of each fiber is limited to a narrow range. In other words, the variation in the amount of pulp deposition is not eliminated by the movement of the fibers during the hot press treatment. Therefore, the second method cannot produce a pulp molded product with a small standard deviation in basis weight.

[0158] In contrast, in the first method, a mold 240 is placed on top of the cover body 230, and the composite body is immersed in a slurry S. The depth of the slurry S is much greater than the height of the mold 240. Therefore, even if pulp settles in the slurry S, the pulp concentration does not differ greatly between the upper position and the lower position of the mold 240. Therefore, according to the first method, pulp can be deposited approximately uniformly on the mold 240, and a pulp molded product MP2 with a small standard deviation of basis weight can be manufactured.

[0159] The pulp molded product MP2 has an opening and does not expand in the direction away from the opening. Here, the pulp molded product MP2 has an opening and tapers in the direction away from the opening. With this shape, the volume of the laminate formed by stacking multiple pulp molded products MP2 can be reduced.

[0160] In the first method, if the pulp layer MP1 is sandwiched between one of the upper mold 350 and the lower mold 320 and an elastic body and pressure is applied to the pulp layer MP1 instead of the upper mold 350 and the lower mold 320, the elastic body will deform, and a pulp molded product with excellent surface properties cannot be obtained.

[0161] In the second method, if one of the upper and lower dies used in the hot press treatment is made of an elastic material, it is not possible to obtain a pulp molded product with excellent surface properties. In addition, in this case, the standard deviation of the basis weight becomes large as described above.

[0162] The pulp molded product MP2 is, for example, a container. The pulp molded product MP2 may be an article other than a container. The pulp molded product MP2 may be a three-dimensional product, that is, a product having a three-dimensional shape, not a two-dimensional shape like a sheet.

[0163] 2 to 10 are provided to facilitate understanding of the manufacturing method of a pulp molded product according to one embodiment of the present invention. The above-mentioned method can also be implemented using manufacturing apparatuses having other structures. For example, in the manufacturing apparatus 1, the upper mold 270 and the upper mold 350 are female molds, and the mold 240 and the lower mold 320 are male molds. The upper mold 270 and the upper mold 350 may be male molds, and the mold 240 and the lower mold 320 may be female molds. In this way, various modifications are possible for the above-mentioned manufacturing apparatus 1 and manufacturing method. EXAMPLES

[0164] Specific examples of the present invention are described below. The present invention is not limited to these specific examples. do not have.

[0165] <1> Manufacturing of pulp molded products (Example 1) A slurry containing pulp, fine cellulose fibers, a paper strength agent, a drainage agent, a sizing agent, and water was prepared using a pulper. The pulp content of the slurry was 0.3% by mass.

[0166] The pulp used was bamboo pulp (average fiber diameter 50 μm, average fiber length 1.590 mm) and sugar cane pulp (average fiber diameter 50 μm, average fiber length 0.918 mm). The amount of bamboo pulp per 100 parts by mass of the total amount of pulp was 70 parts by mass, and the amount of sugar cane pulp per 100 parts by mass of the total amount of pulp was 30 parts by mass. The average fiber diameter of the pulp was 50 μm, and the average fiber length of the pulp was 1.406 mm. The fiber diameter of the pulp was in the range of 4 to 100 μm.

[0167] As the fine cellulose fibers, CELISH (registered trademark) KY100G (average fiber diameter 50-500 nm, average fiber length 10-1500 μm) manufactured by Daicel Miraize Co., Ltd. was used. The fiber diameter of the fine cellulose fibers was within the range of 10 to 800 nm. The amount of the fine cellulose fibers (amount based on solid content) per 100 parts by mass of pulp was 4.0 parts by mass.

[0168] The paper strength agent used was Polystron (registered trademark) PS-1280 (amphoteric polyacrylamide) manufactured by Arakawa Chemical Industries, Ltd. The amount of the paper strength agent (amount on a solid content basis) per 100 parts by mass of pulp was 2.0 parts by mass.

[0169] The filter agent used was RD-7144 (cationically modified polyacrylamide) manufactured by Seiko PMC Co., Ltd. The amount of the filter agent (amount based on solid content) per 100 parts by mass of pulp was 0.2 parts by mass.

[0170] The sizing agent used was Sizepine K-903-20 manufactured by Arakawa Chemical Industries, Ltd. The amount of the sizing agent (amount based on solid content) per 100 parts by mass of pulp was 0.3 parts by mass.

[0171] Using this slurry, a pulp molded product was manufactured by the method described with reference to Figures 2 to 10. Here, the dehydration process was performed so that the moisture content of the pulp layer immediately after dehydration was 65 mass%. The heat pressing process was performed at a heating temperature of 180°C, a pressing pressure of 1.2 MPa, and a pressing time of 120 seconds. In the dehydration and heat pressing processes, the clearance between the upper and lower dies was adjusted so that a pulp molded product with a wall thickness of 0.7 mm was obtained. In this manner, a container was produced as a pulp molded product.

[0172] (Example 2) A pulp molded product was produced in the same manner as in Example 1, except that the amount of the paper strength agent (amount on a solids basis) was changed from 2.0 parts by mass to 0.1 parts by mass per 100 parts by mass of pulp.

[0173] (Example 3) A pulp molded product was produced in the same manner as in Example 1, except that the amount of the paper strength agent (amount on a solids basis) was changed from 2.0 parts by mass to 5.0 parts by mass per 100 parts by mass of pulp.

[0174] (Example 4) A pulp molded product was produced in the same manner as in Example 1, except that the amount of the filter agent (amount based on solids) was changed from 0.2 parts by mass to 0.1 parts by mass per 100 parts by mass of pulp.

[0175] (Example 5) A pulp molded product was produced in the same manner as in Example 1, except that the amount of the filter agent (amount based on solids) was changed from 0.2 parts by mass to 5.0 parts by mass per 100 parts by mass of pulp.

[0176] (Example 6) A pulp molded product was produced in the same manner as in Example 1, except that bamboo pulp was used as the pulp instead of the mixture of 70 parts by mass of bamboo pulp and 30 parts by mass of sugar cane pulp.

[0177] (Example 7) A pulp molded product was produced in the same manner as in Example 1, except that a mixture of 80 parts by mass of bamboo pulp and 20 parts by mass of sugar cane pulp was used instead of a mixture of 70 parts by mass of bamboo pulp and 30 parts by mass of sugar cane pulp.

[0178] (Example 8) A pulp molded product was produced in the same manner as in Example 1, except that a mixture of 50 parts by mass of bamboo pulp and 50 parts by mass of sugar cane pulp was used instead of a mixture of 70 parts by mass of bamboo pulp and 30 parts by mass of sugar cane pulp.

[0179] (Example 9) A pulp molded product was produced in the same manner as in Example 1, except that sugar cane pulp was used as the pulp instead of the mixture of 70 parts by mass of bamboo pulp and 30 parts by mass of sugar cane pulp.

[0180] (Example 10) A pulp molded product was produced in the same manner as in Example 1, except that the amount of pulp piled up was adjusted and the clearance between the upper and lower dies was changed from 0.7 mm to 0.6 mm.

[0181] (Example 11) A pulp molded product was produced in the same manner as in Example 1, except that the amount of pulp piled up was adjusted and the clearance between the upper and lower dies was changed from 0.7 mm to 1.2 mm.

[0182] Comparative Example 1 A pulp molded product was produced in the same manner as in Example 1, except that the slurry in Example 1 was changed so as not to contain fine cellulose fibers, paper strength agents, and drainage agents; that is, a "slurry consisting of pulp, sizing agent, and water" was used as the slurry.

[0183] Comparative Example 2 A pulp molded product was produced in the same manner as in Example 1, except that the slurry in Example 1 was changed so as not to contain fine cellulose fibers and a drainage agent, i.e., a "slurry consisting of pulp, a paper strength agent, a sizing agent, and water" was used as the slurry.

[0184] Comparative Example 3 A pulp molded product was produced in the same manner as in Example 1, except that the slurry in Example 1 was changed so as not to contain fine cellulose fibers and paper strength agents, i.e., a "slurry consisting of pulp, a drainage agent, a sizing agent, and water" was used as the slurry.

[0185] Comparative Example 4 A pulp molded product was produced in the same manner as in Example 1, except that the slurry in Example 1 was changed so as not to contain a paper strength agent or a drainage agent; that is, a "slurry consisting of pulp, fine cellulose fibers, a sizing agent, and water" was used as the slurry.

[0186] Comparative Example 5 A pulp molded product was produced in the same manner as in Example 1, except that the slurry in Example 1 was changed so as not to contain fine cellulose fibers, i.e., a "slurry consisting of pulp, a paper strength agent, a drainage agent, a sizing agent, and water" was used as the pulp.

[0187] Comparative Example 6 A pulp molded product was produced in the same manner as in Example 1, except that the slurry in Example 1 was changed so as not to contain a drainage agent; that is, a "slurry consisting of pulp, fine cellulose fibers, a paper strength agent, a sizing agent, and water" was used as the pulp.

[0188] Comparative Example 7 A pulp molded product was produced in the same manner as in Example 1, except that the slurry in Example 1 was changed so as not to contain a paper strength agent; that is, a "slurry consisting of pulp, fine cellulose fibers, a drainage agent, a sizing agent, and water" was used as the pulp.

[0189] Comparative Example 8 A pulp molded product was produced in the same manner as in Example 1, except that cellulose nanofibers were used instead of fine cellulose fibers as the slurry material, and no paper strength enhancer was used. TEMPO-oxidized cellulose nanofibers (product name: Cellenpia (registered trademark)) (average fiber diameter 3 nm, average fiber length 700 nm) manufactured by Nippon Paper Industries Co., Ltd. were used as the cellulose nanofibers. The amount of cellulose nanofibers (amount based on solid content) was 4.0 parts by mass per 100 parts by mass of pulp. "TEMPO-oxidized cellulose nanofibers" are cellulose nanofibers obtained by treating wood fibers with a TEMPO (2,2,6,6-tetramethylpiperidine 1-oxyl) catalyst to convert the primary hydroxyl groups of cellulose into carboxyl groups, and then mechanically defibrating the fibers.

[0190] <2> Evaluation method For each of the pulp molded articles produced in Examples 1 to 11 and Comparative Examples 1 to 8, various measurements were carried out by the methods described above.

[0191] The effect of shortening the slurry suction time was evaluated as follows. Papermaking was carried out using a mesh-shaped mold with a mesh diameter of 0.15 mm x 0.15 mm. The time required for papermaking (i.e., slurry suction time) was evaluated according to the following criteria. 1: The slurry suction time is 40% or more longer than the standard (10 seconds in Comparative Example 1). In other words, the slurry suction time is 14 seconds or more. 2: The slurry suction time is 20% or more longer than the standard (10 seconds in Comparative Example 1). That is, the slurry suction time is 12 seconds or more and less than 14 seconds. 3: The slurry suction time is 10 seconds (Comparative Example 1). 4: The slurry suction time is reduced by 20% compared to the standard (10 seconds in Comparative Example 1). That is, the slurry suction time is 8 seconds or more and less than 10 seconds. 5: The slurry suction time is reduced by 40% compared to the standard (10 seconds in Comparative Example 1). That is, the slurry suction time is 6 seconds or more and less than 8 seconds.

[0192] <3> result Tables 1 to 3 below show the results of various measurements and the evaluation results of the effect of shortening the slurry suction time.

[0193] [Table 1]

[0194] [Table 2]

[0195] [Table 3]

[0196] As is clear from the comparison of Examples 1 to 11 and Comparative Examples 1 to 8, when a pulp molded product was manufactured by blending fine cellulose fibers, a paper strength enhancer, and a drainage agent with pulp, a pulp molded product having high ISO ring crush strength and capable of completing dehydration during manufacturing in a short time could be manufactured. As shown in Comparative Examples 1 to 7, when at least one of the fine cellulose fibers, the paper strength enhancer, and the drainage agent was missing, it was not possible to achieve both of the above two effects. In addition, as shown in Comparative Example 8, when cellulose nanofibers were blended instead of the fine cellulose fibers, the mechanical strength of the pulp molded product could be increased, but the slurry suction time was increased. [Explanation of symbols]

[0197] Reference Signs List 1... manufacturing apparatus, 10... support, 20... first station, 30... second station, 40... third station, 210... container, 220... lifting device, 230... cover body, 240... mold, 250... moving device, 260... lifting device, 270... upper mold, 310... table, 320... lower mold, 330... moving device, 340... press device, 350... upper mold, 410... table, 420... moving device, 430... lifting device, 440... holder, MP1... pulp layer, MP2... pulp molded product, S... slurry.

Claims

1. Pulp having a fiber diameter of 4 μm or more; Fine fibers having a fiber diameter in the range of 10 to 800 nm; A paper strength enhancer; Drainage agent and A pulp molded product containing.

2. 2. The pulp molded product according to claim 1, wherein the fine fibers are fine cellulose fibers.

3. 2. The pulp molded product according to claim 1, wherein the paper strength agent is an amphoteric polyacrylamide.

4. 2. The pulp molded product according to claim 1, wherein the drainage agent is a cationically modified polyacrylamide.

5. 2. The pulp molded product according to claim 1, wherein the fine fibers are fine cellulose fibers, the paper strength agent is an amphoteric polyacrylamide, and the drainage agent is a cationically modified polyacrylamide.

6. The pulp molded product according to claim 5, wherein, when the mass of the pulp is 100 parts by mass, the amount of the fine fibers is in the range of 1.0 to 8.0 parts by mass, the amount of the paper strength agent is in the range of 0.1 to 5.0 parts by mass, and the amount of the drainage agent is in the range of 0.1 to 5.0 parts by mass.

7. 2. The pulp molded product according to claim 1, wherein the pulp has an average fiber diameter in the range of 15 to 40 μm, and the fine fibers have an average fiber diameter in the range of 50 to 500 nm.

8. 2. The pulp molded product according to claim 1, wherein the pulp has an average fiber length in the range of 0.5 to 2.0 mm, and the fine fibers have an average fiber length in the range of 10 to 1500 μm.

9. Density 0.5 to 1.1 g / m 3 2. The pulp molded product according to claim 1, wherein the thickness of the molded product is within the range of 100 μm to 150 μm.

10. 2. The molded pulp product according to claim 1, having a thickness in the range of 0.5 to 1.2 mm.

11. 2. The pulp molded article according to claim 1, which is a container.

12. Preparing a slurry containing pulp having a fiber diameter of 4 μm or more, fine fibers having a fiber diameter in the range of 10 to 800 nm, a paper strength agent, a drainage agent, and water; depositing the pulp and the fine fibers on a three-dimensional mold to form a pulp layer; dehydrating the pulp layer to obtain an intermediate molded product; the undried intermediate molded product is sandwiched between a male mold and a female mold and heated under pressure; A method for producing a pulp molded product comprising the steps of:

13. The method for producing a pulp molded product according to claim 12, wherein the fine fibers are fine cellulose fibers.

14. The method for producing a pulp molded product according to claim 12, wherein the paper strength agent is an amphoteric polyacrylamide.

15. The method for producing a molded pulp product according to claim 12, wherein the drainage agent is a cationically modified polyacrylamide.

16. 13. The method for producing a pulp molded product according to claim 12, wherein the fine fibers are fine cellulose fibers, the paper strength agent is an amphoteric polyacrylamide, and the drainage agent is a cationically modified polyacrylamide.

17. The method for producing a pulp molded product according to claim 16, wherein, when the mass of the pulp is 100 parts by mass, the amount of the fine fibers is in the range of 1.0 to 8.0 parts by mass, the amount of the paper strength agent is in the range of 0.1 to 5.0 parts by mass, and the amount of the drainage agent is in the range of 0.1 to 5.0 parts by mass.

18. 13. The method for producing a pulp molded product according to claim 12, wherein the pulp has an average fiber diameter in the range of 15 to 40 μm, and the fine fibers have an average fiber diameter in the range of 50 to 500 nm.

19. 13. The method for producing a pulp molded product according to claim 12, wherein the pulp has an average fiber length in the range of 0.5 to 2.0 mm, and the fine fibers have an average fiber length in the range of 10 to 1500 μm.

20. Density 0.5 to 1.1 g / m 3 The method for producing a molded pulp product according to claim 12, which produces a molded product having a particle size within the range of 100 to 150 mm.

21. The method for producing a molded pulp product according to claim 12, which produces a molded product having a thickness in the range of 0.5 to 1.2 mm.

22. The method for producing a molded pulp product according to claim 12, which produces a container.

Citation Information