Resin-coated aluminum pigment, coating, and ink

A resin-attached aluminum pigment with controlled surface roughness and thickness improves adhesion and chemical resistance, addressing the limitations of conventional methods by enhancing design and alkali resistance.

JP2024169313APending Publication Date: 2024-12-05ASAHI KASEI KOGYO KABUSHIKI KAISHA
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
JP2024064948
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-05-24
Filing Date
2024-04-12
Publication Date
2024-12-05

AI Technical Summary

Technical Problem

Conventional methods for improving the alkali resistance and design properties of aluminum pigments do not adequately address the contribution of resin layer thickness to these qualities.

Method used

A resin-attached aluminum pigment with a specific range of average surface roughness and thickness of the resin layer, achieved by coating aluminum particles with a polymer containing radically polymerizable double bonds, is developed, ensuring excellent adhesion and chemical resistance.

Benefits of technology

The resin-attached aluminum pigment exhibits enhanced design properties, adhesion, and chemical resistance, particularly against alkalis, by controlling the resin layer's surface roughness and thickness within specified ranges.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024169313000001_ABST
    Figure 2024169313000001_ABST
Patent Text Reader

Abstract

To provide a resin-coated aluminum pigment that offers superior designability and exhibits superior adhesion and chemical resistance.SOLUTION: A resin-coated aluminum pigment comprises aluminum particles whose surfaces are coated with a resin containing a polymer of a monomer and / or oligomer with one or more radical-polymerizable double bonds. In the resin-coated aluminum pigment, the resin layer surface has an average surface roughness Ra of 0.1-5.0 nm.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a resin-deposited aluminum pigment, and to paints and inks containing the resin-deposited aluminum pigment. [Background technology]

[0002] Aluminum pigments have been used for a long time in metallic paints, printing inks, plastics, etc., to obtain a cosmetic effect that emphasizes a metallic feel. By coating these aluminum pigments with resin, it is possible to improve the alkali resistance test. In particular, thin-film aluminum with an average particle size of 20 μm or less and a particle thickness of 0.2 μm or less has excellent design properties.

[0003] As a method for improving the alkali resistance of aluminum pigments as described above, a method of subjecting the aluminum pigments to a specific surface treatment has been proposed. For example, Patent Document 1 describes that by setting the ratio of the resin mass per unit mass of the resin-adhered aluminum pigment to the total surface area of ​​the particles of the resin-adhered aluminum pigment within a specified range, the design tends to be excellent and the alkali resistance also tends to be excellent. However, there is no description of the contribution of the thickness of the resin layer to the design.

[0004] Patent Document 2 describes a method for producing a resin-coated metal pigment in which 0.1 to 50 parts by weight of resin is attached to the surface of the metal pigment per 100 parts by weight of the metal pigment, and describes that the desired resin-coated metal pigment can be obtained by promoting physical dispersion by applying an external action such as ultrasonic irradiation during the resin coating process. However, there is no description of the contribution that the thickness of the resin layer can make to the design.

[0005] Patent Document 3 describes that a pigment having excellent chemical resistance to chemicals such as alkalis can be provided by setting the ratio of the total area of ​​resin particles having an equivalent circle diameter of 25 nm or more on the surface of the coating resin that coats the surface of the aluminum particles to a specific range. However, there is no description of the contribution of the thickness of the resin layer to the design.

[0006] Patent Document 4 describes an aluminum pigment capable of providing a metallic coating film having excellent design and adhesion, and a method for producing the same. However, there is no description of the contribution of the thickness of the resin layer to the design, and no description of alkali resistance. [Prior art documents] [Patent documents]

[0007] [Patent Document 1] JP 2018-135455 A [Patent Document 2] Patent Publication No. 2012-162733 [Patent Document 3] International Publication No. 2018 / 047360 [Patent Document 4] JP 2002-226733 A Summary of the Invention [Problem to be solved by the invention]

[0008] An object of the present invention is to provide a resin-adhered aluminum pigment that has not necessarily been fully realized in the prior art as described above, and to provide a resin-adhered aluminum pigment that has excellent design properties, adhesion, and chemical resistance. [Means for solving the problem]

[0009] As a result of intensive research to solve the above-mentioned problems, the inventors have discovered that by setting the average surface roughness of the resin layer surface of a resin-adhered aluminum pigment and / or the thickness of the resin-adhered layer within a predetermined range, a resin-adhered aluminum pigment can be obtained that has excellent design properties, adhesion, and chemical resistance to chemicals such as alkalis, and have completed the present invention. That is, the gist of the present invention is as follows. [1] A resin-adhered aluminum pigment in which the surfaces of aluminum particles are coated with a resin containing a polymer of a monomer and / or oligomer having one or more radically polymerizable double bonds, and the average surface roughness Ra of the resin layer surface of the resin-adhered aluminum pigment is 0.1 to 5.0 nm. [2] The resin-adhered aluminum pigment according to the above [1], wherein the thickness τ of the resin-adhered layer measured by cross-sectional observation is 10 nm to 20 nm. [3] A resin-adhered aluminum pigment in which the surfaces of aluminum particles are coated with a resin containing a polymer of a monomer and / or oligomer having one or more radically polymerizable double bonds, and the thickness τ of the resin-adhered layer measured by cross-sectional observation is 10 nm to 20 nm. [4] The resin mass per unit mass of the resin-attached aluminum pigment (A(g / g)) and the total surface area per unit mass of the aluminum particles (SSA(m 2 / g)) ((A) / (SSA)) is 0.0077g / m 2 ~0.025g / m 2 The resin-adhered aluminum pigment according to the above item [1]. [5] The resin-adhered aluminum pigment according to the above [1], wherein the average cross-sectional thickness τ' of the aluminum particles is 0.03 μm to 0.2 μm. [6] The resin-adhered aluminum pigment according to the above [5], wherein the average particle diameter d50 of the aluminum particles is 5 μm to 15 μm. [7] A paint containing the resin-adhered aluminum pigment according to any one of [1] to [6] above. [8] An ink containing the resin-adhered aluminum pigment according to any one of [1] to [6] above. Effect of the Invention

[0010] According to the present invention, it is possible to provide a resin-adhered aluminum pigment that has not necessarily been fully realized in the prior art, and it is possible to provide a resin-adhered aluminum pigment that has excellent design properties, adhesion, and chemical resistance. [Brief description of the drawings]

[0011] [Figure 1] 1 is an example of a TEM photograph of the resin-coated metal pigment of Example 1. [Diagram 2] 2 is an example of a TEM photograph of the resin-coated metal pigment of Comparative Example 1. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0012] Hereinafter, an example of a preferred embodiment of the present invention will be described. However, the following embodiment is merely an example for explaining the present invention, and the present invention is not limited to the following embodiment.

[0013] The resin-adhered aluminum pigment of the present invention has excellent adhesion and chemical resistance while maintaining excellent design properties.

[0014] The resin-adhered aluminum pigment of the present invention has a structure in which the surfaces of aluminum particles are coated with a resin containing a polymer of a monomer and / or oligomer having one or more radically polymerizable double bonds. The specific shapes of the aluminum particles that are the raw material for the resin-adhered aluminum pigment of the present invention will be described below.

[0015] The aluminum particles used in the present invention are not limited in type, and may be those generally used as aluminum pigments, and may have a flat shape such as a scaly, angular, rounded, etc. If high designability (e.g., characteristics such as brightness, brilliance, flip-flop feel, and hiding power) is to be maintained, the effect of the present invention will be more pronounced if high design grade (vapor deposition metallic paint or ink grade) aluminum particles (hereinafter sometimes referred to as flake aluminum powder) are used.

[0016] The method for producing aluminum particles is not particularly limited, but can be obtained by grinding granular powder or small pieces of metallic aluminum together with a few percent of a grinding aid by a mechanical method such as a stamp mill method, a dry ball mill method, a wet ball mill method, an attritor method, or a vibrating ball mill method. Examples of methods for producing highly decorative aluminum particles include the method described in WO 99 / 54074, and the flake-shaped aluminum powder obtained by this method, which has a smooth surface and uniform thickness, can be particularly preferably used as the raw material for the aluminum pigment of the present invention.

[0017] The particle size of the aluminum particles used as the raw material for the resin-adhered aluminum pigment of the present invention varies depending on the application. When the resin-adhered aluminum pigment of the present invention is used for paints and printing inks, aluminum particles with an average particle size d50 (μm) of about 1 to 100 μm can be suitably used. In addition, applications in which high designability of metal pigments is particularly required recently include automobiles, general home appliances, and information appliances such as mobile phones, and in these applications, metal pigments are used to paint metals such as iron and magnesium alloys or plastics. In order to ensure high designability, the preferred average particle size (d50) of the aluminum particles of the resin-adhered aluminum pigment of the present invention used for these applications is 5 to 35 μm, and more preferably 5 to 15 μm.

[0018] The average particle size d50 (μm) of the aluminum particles of the present invention can be measured using a general laser diffraction / scattering type particle size distribution measuring device, and can be measured, for example, as follows. The average particle size (d50) of the particles of the flaky aluminum powder is measured using a laser diffraction / scattering type particle size distribution measuring device (LA-300 / Horiba, Ltd.) Mineral spirits can be used as the measurement solvent. It is preferable that the resin-adhered aluminum pigment sample is subjected to ultrasonic dispersion for 2 minutes as a pretreatment, then placed in a dispersion tank and the measurement is started after confirming that the appropriate concentration has been achieved.

[0019] The average cross-sectional thickness τ' (μm) of the aluminum particles can be determined by using an FE-SEM image of the cross section of the coating film and measuring it using image analysis software. Specifically, 100 particles are randomly selected from an FE-SEM image of the cross section of the coating film, the cross-sectional thickness of the particles is automatically measured, and the arithmetic average value of the 100 particles is calculated. The average cross-sectional thickness τ' (μm) of the aluminum particles of this embodiment is preferably 0.03 μm to 0.2 μm.

[0020] The specific composition and shape of the resin adhered to the surface of the resin-adhered aluminum pigment of the present invention will be described below.

[0021] The resin adhered to the resin-adhered aluminum pigment of the present embodiment is not particularly limited, but is preferably a polymer of a monomer and / or oligomer having one or more radically polymerizable double bonds.

[0022] The monomer having one or more radically polymerizable double bonds is not particularly limited, and conventionally known monomers can be used. Specific examples of the monomer having one or more radically polymerizable double bonds include, but are not limited to, unsaturated carboxylic acids (e.g., acrylic acid, methacrylic acid, itaconic acid, fumaric acid, citraconic acid, crotonic acid, maleic acid, or maleic anhydride), mono- or diesters of phosphorus or phosphonic acid (e.g., 2-methacryloyloxyethyl phosphate, di-2-methacryloyloxyethyl phosphate, tri-2-methacryloyloxyethyl phosphate, 2- ... ethyl phosphate, di-2-acryloyloxyethyl phosphate, tri-2-acryloyloxyethyl phosphate, diphenyl-2-acryloyloxyethyl phosphate, dibutyl-2-methacryloyloxyethyl phosphate, dioctyl-2-acryloyloxyethyl phosphate, 2-methacryloyloxypropyl phosphate, bis(2-chloroethyl)vinyl phosphonate, diallyl dibutyl phosphonosuccinate, 2-methacryloyloxyethyl phosphate acrylate, 2-acryloxyethyl phosphate), coupling agents (e.g., γ-methacryloxypropyltrimethoxysilane, 3-acryloxypropyltrimethoxysilane, vinyltrichlorosilane, vinyltriethoxysilane, vinyltrimethoxysilane, vinyltris(β-methoxyethoxy)silane, isopropylisostearoyldiacryl titanate, acetoalkoxyaluminum diisopropylate, zircoaluminate), nitriles of unsaturated carboxylic acids (e.g., acrylonitrile, methacrylonitrile), or esters of unsaturated carboxylic acids (e.g., methyl acrylate, ethyl acrylate, n-butyl acrylate, 2-ethylhexyl acrylate, lauryl acrylate, stearyl acrylate, hydroxyethyl acrylate, 2-hydroxypropyl acrylate, methoxyethyl acrylate, butoxyethyl acrylate, glycidyl acrylate, cyclohexyl acrylate, 1,6-hexanediol diacrylate, 1,4-Butadiol diacrylate, triethylene glycol diacrylate, ethylene glycol dimethacrylate, triethylene glycol dimethacrylate, neopentyl glycol dimethacrylate, trimethylolpropane triacrylate, tetramethylolpropane tetraacrylate, tetramethylolpropane methane triacrylate, trimethylolpropane trimethacrylate, tetramethylolmethane trimethacrylate, di-trimethylolpropane tetraacrylate, pentaerythritol tetraacrylate, di-pentaerythritol tetraacrylate, Lithritol hexaacrylate, di-pentaerythritol pentaacrylate, di-pentaerythritol pentaacrylate monopropionate, triacrylformal, methyl methacrylate, ethyl methacrylate, n-butyl methacrylate, 2-ethylhexyl methacrylate, lauryl methacrylate, stearyl methacrylate, hydroxyethyl methacrylate, 2-hydroxypropyl methacrylate, methoxyethyl methacrylate, butoxyethyl methacrylate, glycidyl methacrylate, cyclohexyl methacrylate, and the like can be preferably used. Furthermore, cyclic unsaturated compounds (e.g., cyclohexene) and aromatic unsaturated compounds (e.g., styrene, α-methylstyrene, vinyltoluene, divinylbenzene, cyclohexene vinyl monoxide, divinylbenzene monoxide, vinyl acetate, vinyl propionate, allylbenzene, or diallylbenzene) can also be suitably used. The oligomer having one or more radically polymerizable double bonds can be a polymer of these monomers.

[0023] In the method for producing a resin-deposited aluminum pigment of the present embodiment described below, it is preferable to use a polymerization initiator. The polymerization initiator is generally known as a radical generator, and the type thereof is not particularly limited. Examples of the polymerization initiator include, but are not limited to, peroxides such as benzoyl peroxide, lauroyl peroxide, and bis-(4-t-butylcyclohexyl)peroxydicarbonate, and azo compounds such as 2,2'-azobis-isobutyronitrile, 2,2'-azobis-2,4-dimethylvaleronitrile, and 2,2'-azobis-4-methoxy-2,4-dimethylvaleronitrile. The amount of the polymerization initiator used is not particularly limited since it is adjusted depending on the reaction rate of each radically polymerizable monomer, but is preferably 0.1 to 25 parts by mass with respect to 100 parts by mass of the aluminum pigment.

[0024] During the resin polymerization of the resin-adhered aluminum pigment of this embodiment described below, it is preferable to add a reversible addition-fragmentation chain transfer agent (hereinafter referred to as a RAFT agent) together with the polymerization initiator to control the molecular weight of the reaction product, thereby performing living radical polymerization. This polymerization is superior in productivity compared to other living radical polymerizations in that (1) it is applicable to a variety of monomers and (2) it is applicable to a wide range of reaction conditions. Examples of RAFT agents used to obtain the resin layer of the resin-adhered aluminum pigment of the present invention include, but are not limited to, dithiocarbonates such as O-ethyl-S-(1-phenylethyl)dithiocarbonate, O-ethyl-S-(2-propoxyethyl)dithiocarbonate, and O-ethyl-S-(1-cyano-1-methylethyl)dithiocarbonate; dithioesters such as cyanoethyl dithiopropionate, benzyl dithiopropionate, benzyl dithiobenzoate, and acetoxyethyl dithiobenzoate; dithiocarbamates such as S-benzyl-N,N-dimethyldithiocarbamate and benzyl-1-pyrrolecarbodithioate; and trithiocarbonates such as dibenzyl trithiocarbonate and S-cyanomethyl-S-dodecyl trithiocarbonate. The RAFT agent used is preferably selected from the most suitable ones depending on the reactivity of the monomers, and in particular, dithiocarbamates and dithiocarbonates are suitable for the polymerization of acrylic acid esters, and dithioesters are suitable for the polymerization of methacrylic acid esters. The RAFT agent is preferably used in an amount of 0.1 to 30 parts by weight, more preferably 1.0 to 10 parts by weight, per 100 parts by weight of the total amount of resin. By using an amount of 0.1 part by weight or more, it is possible to suppress the tendency of the average molecular weight of the reaction product to become high, and by using an amount of 30 parts by weight or less, it is possible to suppress the tendency of the average molecular weight of the reaction product to become low.

[0025] The solvent is not limited to the following examples, but any organic solvent used to disperse a metal pigment in an organic solvent may be used as long as it is inactive against the metal pigment, and examples of the organic solvent include aliphatic hydrocarbons such as hexane, heptane, octane, and mineral spirits, aromatic hydrocarbons such as benzene, toluene, xylene, and solvent naphtha, ethers such as tetrahydrofuran and diethyl ether, alcohols such as ethanol, 2-propanol, and butanol, esters such as ethyl acetate and butyl acetate, glycols such as propylene glycol and ethylene glycol, glycol ethers such as propylene glycol monomethyl ether, propylene glycol monoethyl ether, ethylene glycol monoethyl ether, and ethylene glycol monobutyl ether, and glycol esters such as propylene glycol monomethyl ether acetate, propylene glycol monoethyl ether acetate, and ethylene glycol monomethyl ether acetate. These organic solvents may be used alone or in combination of two or more. The amount of the organic solvent used is preferably an amount that gives a solids concentration of the metal pigment of 1 to 40% by weight. In the present invention, the organic solvent is also used as a reaction solvent when forming a resin by polymerizing the monomer and / or oligomer having one or more double bonds in the molecule.

[0026] When producing a resin-attached aluminum pigment, a shear external action and a vibration external action may be used in combination as an external action. The shear external action refers to the action of applying high shear force to promote physical dispersion when dispersing a metal pigment in an organic solvent and when adding a monomer to the dispersion, and examples of the method for this include a method of dispersing a metal pigment or a monomer using a stirrer, a disperser, a vibration generator, or an ultrasonic generator. When a vibration generator or an ultrasonic generator is used, the dispersion or the slurry liquid during the polymerization reaction is mechanically vibrated strongly, and an action of promoting physical dispersion occurs. In particular, high-speed dispersion using a stirrer is more preferable because the surface of the vapor deposition-like aluminum pigment is not destroyed.

[0027] The resin-adhered aluminum pigment of the present invention is characterized by maintaining high designability due to the high smoothness and thin film formation of the resin-adhered layer compared to conventional thin film aluminum pigments. This is thought to be because the thin film aluminum pigment can be made into a monodisperse state under high speed stirring and the molecular weight can be controlled at a low molecular weight state by RAFT polymerization, which allows both high smoothness and thin film formation to be achieved. This uniformity can be evaluated by measuring the thickness τ of the resin layer of the resin-coated pigment and the average surface roughness Ra.

[0028] The average surface roughness Ra of the resin layer surface of the resin-adhered aluminum pigment of the present invention is preferably 0.1 to 5.0 nm, more preferably 0.1 to 4.5 nm, even more preferably 0.1 to 2.6 nm, and most preferably 0.1 to 2.5 nm. Among these, the upper limit of the average surface roughness Ra is preferably the above-mentioned upper limit, more preferably 2.5 nm, even more preferably 2.2 nm, and most preferably 2.0 nm. In addition, the lower limit of the average surface roughness Ra may be 0.3 nm, 0.5 nm, 0.7 nm, or 0.9 nm depending on the case. When the average surface roughness Ra is equal to or less than the above-mentioned upper limit, the regular reflectance of light on the surface of the coating film using the resin-adhered aluminum pigment is high, so that the coating film shows extremely excellent light brightness and also has good flop properties. The average surface roughness Ra referred to in the present invention can be calculated by a surface morphology observation method using a general atomic force microscope. Specifically, it is calculated, for example, by the following method. An atomic force microscope (hereinafter abbreviated as AFM) (e.g., Dimensioin Icon (manufactured by Bruker)) can be used to observe the surface morphology of metal pigments. For example, the resin-coated aluminum pigment sample is ultrasonically cleaned with excess methanol and chloroform, vacuum dried, dispersed again in acetone, dropped onto a silicon wafer, and naturally dried. The surface roughness is quantified using AFM for resin-coated metal pigments that do not overlap with other resin-coated metal pigments, with a measurement field of 2 μm and 512 pixels, divided into 16 sections, and a third-order plane fit is performed on each section, and the calculated average value is defined as the "average surface roughness Ra (nm)". The terminology for surface roughness is based on JIS-B-0601:2013.

[0029] In the resin-adhered aluminum pigment of the present invention, the thickness τ of the resin-adhered layer measured by cross-sectional observation of the resin-adhered aluminum pigment is preferably 5 to 30 nm, more preferably 10 nm to 20 nm. The upper limit of the thickness τ of the resin-adhered layer is even more preferably 18 nm, and most preferably 16 nm. When the thickness τ of the resin-adhered layer is within the above range, it exhibits extremely excellent design properties, and also has good adhesion and chemical resistance.

[0030] The average film thickness τ of the resin layer in the present invention is calculated, for example, as follows. First, as a pretreatment, the resin-adhered aluminum pigment is ultrasonically cleaned with excess methanol and chloroform, then vacuum dried, dispersed and cleaned again in acetone, and then naturally dried. Then, it is embedded in epoxy resin and completely cured, after which it is trimmed and cut into pieces, and the cross section is observed with a transmission electron microscope (hereinafter abbreviated as TEM) to observe the interface between the resin coating layer and the aluminum pigment. Observation is performed in four fields of view at 200,000 times magnification per field, and the area of ​​the coating layer is measured from the outline of the entire resin layer using known image analysis software (for example, Image-ProPLUS ver.7.0 (manufactured by Media Cybernetics)), and the arithmetic average value of these four fields of view is defined as the [arithmetic average film thickness τ].

[0031] (I) The mass of resin per unit mass of the resin-attached aluminum pigment (A (g / g)) and the total surface area of ​​aluminum particles per unit mass of the resin-attached aluminum pigment (SSA (m 2 / g) ((A) / (SSA)) (1)Resin mass (A(g / g)) The resin mass per unit mass of the resin-adhered aluminum pigment (A (g / g)) is the calculated mass (g) of resin adhering to 1 g of the resin-adhered aluminum pigment. The total surface area of ​​the particles per unit mass of resin-bonded aluminum pigment (SSA(m 2 / g) is the sum of the areas of aluminum particles in 1 g (m 2 ). The ratio (A) / (SSA) in the resin-bonded aluminum pigment of the present invention is preferably 0.0077 g / m 2 ~0.025g / m 2 When the ratio (A) / (SSA) is within the above range, the amount of resin relative to the aluminum particles is appropriate. When the ratio (A) / (SSA) is equal to or greater than the lower limit of the above range, the alkali resistance is prevented from decreasing, and when the ratio is equal to or less than the upper limit of the above range, the resin layer is easily controlled, and deterioration in color tone is prevented.

[0032] In the present invention, A (g / g) and SSA (m 2 / g) can be measured, for example, by the following method. 1 g of the resin-attached aluminum pigment of the present invention is weighed into a 100 ml beaker, 50 ml of petroleum benzene is added, and the pigment is thoroughly dispersed. The pigment is then heated for 1 hour in a thermostatic water bath at 40°C. The heated dispersion is filtered and thoroughly washed with acetone before being collected. The solid sample obtained after filtration is dried in a desiccator for 90 minutes or more. A portion of the dried sample is analyzed by thermogravimetry and differential thermal TG-DTA to determine the resin mass per unit mass of the resin-attached aluminum pigment (A (g / g)).

[0033] SSA of aluminum particles (m 2 / g) is the total surface area per gram of aluminum particles and is calculated using the following formula: SSA(m 2 / g) = 2 × (0.4 / τ'(μm))

[0034] The above SSA(m 2 The method for calculating the viscosity (g) is described, for example, on pages 16 to 22 of Aluminum Paint and Powder, J.D. Edwards & R.I. Wray, 3rd Edition, Reinhold Publishing Corp., New York (1955).

[0035] In addition, the resin-adhered aluminum pigment of the present invention has a more dense and uniform resin coating on the surface of the aluminum particles than conventional aluminum pigments, improving the chemical resistance in the coating film. When the color difference ΔE is calculated according to 6.3.19 of JIS-Z-8781 (2017) to evaluate the chemical resistance, it is preferable that ΔE is less than 1.0.

[0036] The resin-adhered aluminum pigments of the present invention can be used in paints and inks. Paints containing the resin-adhered aluminum pigment of the present invention can be suitably used for automobiles, general home appliances, information appliances such as mobile phones, printing, and for coating substrates such as metals such as iron and magnesium alloys, and plastics, and can exhibit high design properties. Inks containing the resin-adhered aluminum pigment of the present invention can be suitably used for metallic paints, printing inks, paints for kneading into plastics, and can exhibit high design properties.

[0037] In addition, additives commonly used in the paint industry, such as pigments, dyes, wetting agents, dispersants, color separation inhibitors, leveling agents, slip agents, rheology control agents, viscosity modifiers, antiskinning agents, antigelling agents, defoamers, thickeners, anti-sagging agents, mildew inhibitors, ultraviolet absorbers, film-forming assistants, and surfactants, may be added as appropriate to paints or inks containing the novel resin-adhered aluminum pigment of the present invention. EXAMPLES

[0038] The present invention will now be described in detail with reference to examples. In the following description, "%" indicates "% by weight."

[0039] Example 1 100 g of commercially available aluminum paste (manufactured by Asahi Kasei Corporation, SB-10 "average particle size 10 μm, non-volatile content 74 mass%"; aluminum particles of the present invention) was placed in a four-neck flask with a volume of 1 liter, 500 g of mineral spirits was added, and the mixture was stirred for 3 hours while bubbling nitrogen gas, and the temperature in the system was raised to 70 ° C. Next, 1.11 g of acrylic acid was added and stirring was continued for 30 minutes at 70 ° C. Next, 7.83 g of trimethylolpropane trimethacrylate, 0.87 g of di-trimethylolpropane tetraacrylate, 2.0 g of 2,2'-azobis-2,4-dimethylvaleronitrile (polymerization initiator), 0.5 g of bis(dodecylsulfonylthiocarbonyl) disulfide (RAFT agent), and 50 g of mineral spirits were added dropwise over 1 hour (i.e., dropwise was adopted as the addition method, and the dropwise addition time was 1 hour), and polymerization was performed for a total of 8 hours while maintaining the temperature in the system at 70 ° C. The amount of unreacted trimethylolpropane trimethacrylate and di-trimethylolpropane tetraacrylate in the filtrate sampled at this point was analyzed by gas chromatography, and it was found that more than 99% of the added amount had reacted. After the polymerization was completed, the treated slurry was filtered to obtain a resin-attached aluminum pigment. The heating residue of the aluminum pigment (according to JIS-K-5910) was 56.1% by weight.

[0040] Example 2 A resin-adhered aluminum pigment was obtained in the same manner as in Example 1, except that the amounts of trimethylolpropane trimethacrylate and di-trimethylolpropane tetraacrylate were changed to 12.6 g and 0.14 g, respectively.

[0041] Example 3 A resin-adhered aluminum pigment was obtained in the same manner as in Example 1, except that the mineral spirits were changed to 150 g.

[0042] Example 4 An ultrasonic disperser was attached directly to the outside of the 1-liter four-neck flask used in Example 1, and ultrasonic waves were applied to the slurry liquid inside. A resin-coated aluminum paste was obtained in the same manner as in Example 1, except that ultrasonic waves with a frequency of 40 kHz and an output of 12 W were irradiated during polymerization using this ultrasonic disperser. The non-volatile content of this paste according to JIS-K-5910 was 50.1% by weight.

[0043] Example 5 A resin-adhered aluminum pigment was obtained in the same manner as in Example 1, except that the aluminum paste used in Example 1 was changed to 100 g (manufactured by Asahi Kasei Corporation, FD-5060 "average particle size 6 μm, non-volatile content 72 mass%"; aluminum particles of the present invention), 5.31 g of trimethylolpropane trimethacrylate, and 0.59 g of di-trimethylolpropane tetraacrylate.

[0044] Example 6 A resin-adhered aluminum pigment was obtained in the same manner as in Example 1, except that in Example 3, the amounts of trimethylolpropane trimethacrylate and di-trimethylolpropane tetraacrylate were changed to 10.62 g and 1.18 g, respectively.

[0045] Example 7 A resin-adhered aluminum pigment was obtained in the same manner as in Example 1, except that the aluminum paste used in Example 1 was changed to 100 g (manufactured by Asahi Kasei Corporation, BS-120 "average particle size 13 μm, non-volatile content 65 mass%"; aluminum particles of the present invention), 4.95 g of trimethylolpropane trimethacrylate, and 0.55 g of di-trimethylolpropane tetraacrylate.

[0046] Example 8 A resin-adhered aluminum pigment was obtained in the same manner as in Example 5, except that the amounts of trimethylolpropane trimethacrylate and di-trimethylolpropane tetraacrylate were changed to 7.2 g and 0.8 g, respectively.

[0047] Example 9 A resin-adhered aluminum pigment was obtained in the same manner as in Example 1, except that the amounts of trimethylolpropane trimethacrylate, di-trimethylolpropane tetraacrylate, and divinylbenzene were changed to 6.83 g, 0.87 g, and 1.0 g, respectively.

[0048] Example 10 A resin-adhered aluminum pigment was obtained in the same manner as in Example 2, except that the dropping time was changed to 0.5 hours.

[0049] Example 11 A resin-adhered aluminum pigment was obtained in the same manner as in Example 2, except that the addition method was changed from dropwise addition to lump-sum addition.

[0050] Comparative Example 1 100g of commercially available aluminum paste (manufactured by Asahi Kasei Corporation, SB-10 "average particle size 10μm, non-volatile content 74% by mass") was placed in a 1L four-neck flask, 500g of mineral spirits was added, and the mixture was stirred for 1 hour while bubbling nitrogen gas, and the temperature in the system was raised to 70°C. Next, 1.11g of acrylic acid was added and the mixture was stirred for 30 minutes at 70°C. Next, 12.6g of trimethylolpropane trimethacrylate, 0.14g of di-trimethylolpropane tetraacrylate, 2.0g of 2,2'-azobis-2,4-dimethylvaleronitrile (polymerization initiator), and 50g of mineral spirits were added dropwise with a metering pump over 1 hour (i.e., the addition method was dropwise, and the drop time was 1 hour), and the mixture was polymerized for a total of 8 hours while maintaining the temperature in the system at 70°C. During the polymerization reaction, ultrasonic waves with a frequency of 42 kHz and an output of 180 W were indirectly irradiated to the mixture in the four-neck flask for about 3 minutes every 15 minutes using a commercially available ultrasonic cleaner. The amount of unreacted trimethylolpropane trimethacrylate and di-trimethylolpropane tetraacrylate in the filtrate sampled at this point was analyzed by gas chromatography, and it was found that more than 99% of the added amount had reacted. After the polymerization was completed, the treated slurry was filtered to obtain a resin-adhered aluminum pigment. The heating residue of the aluminum pigment (according to JIS-K-5910) was 55.6% by weight.

[0051] Comparative Example 2 A resin-adhered aluminum pigment was obtained in the same manner as in Comparative Example 1, except that the amounts of trimethylolpropane trimethacrylate and di-trimethylolpropane tetraacrylate were changed to 7.83 g and 0.87 g, respectively.

[0052] Comparative Example 3 A resin-adhered aluminum pigment was obtained in the same manner as in Comparative Example 1, except that the aluminum paste used in Comparative Example 1 was changed to 100 g (manufactured by Asahi Kasei Corporation, FD-5060, "average particle size 6 μm, non-volatile content 72 mass%"), 7.20 g of trimethylolpropane trimethacrylate, and 0.80 g of di-trimethylolpropane tetraacrylate.

[0053] Comparative Example 4 A resin-adhered aluminum pigment was obtained in the same manner as in Comparative Example 1, except that the aluminum paste used in Comparative Example 1 was changed to 100 g (BS-120 manufactured by Asahi Kasei Corporation, "average particle size 13 μm, non-volatile content 65 mass %), 4.95 g of trimethylolpropane trimethacrylate, and 0.55 g of di-trimethylolpropane tetraacrylate.

[0054] Comparative Example 5 A resin-adhered aluminum pigment was obtained in the same manner as in Comparative Example 1, except that the dropping time was changed to 0.5 hours.

[0055] Comparative Example 6 A resin-adhered aluminum pigment was obtained in the same manner as in Comparative Example 5, except that the addition method in Comparative Example 1 was changed from dropwise addition to lump-sum addition.

[0056] [Evaluation 1 (resin mass (A(g / g)) and total surface area (SSA(m 2 / g) ((A) / (SSA))) (1)Resin mass (A(g / g)) 1 g of the resin-adhered aluminum pigment obtained in the Examples and Comparative Examples was weighed into a 100 ml beaker, 50 ml of petroleum benzene was added and thoroughly dispersed, then the pigment was heated in a 40°C thermostatic water bath for 1 hour. The heated dispersion was filtered and thoroughly washed with acetone before being collected. The solid sample obtained after filtration was dried in a desiccator for 90 minutes or more. A portion of the dried sample was analyzed by thermogravimetry and differential thermal TG-DTA to determine the resin mass per unit mass of the resin-adhered aluminum pigment (A (g / g)). (2) Total surface area of ​​aluminum particles (SSA(m 2 / g)) (Total surface area of ​​particles SSA(m 2 / g) = 2 × (0.4 / τ' (μm)). The average thickness τ' (μm) can be determined by measuring an FE-SEM image of the cross section of the coating film, which will be described later, using image analysis software.

[0057] [Evaluation 2 (Measurement of the average particle diameter d50 of aluminum particles)] The average particle size (d50) of the aluminum particles was measured using a laser diffraction / scattering type particle size distribution analyzer (LA-300 / HORIBA, Ltd.). Mineral spirits was used as the measurement solvent. The measurements were carried out in accordance with the equipment's instruction manual, but it should be noted that the aluminum particles used as samples were ultrasonically dispersed for 2 minutes as a pretreatment, then placed in the dispersion tank and measurements were started after confirming that the appropriate concentration had been achieved. After the measurement was completed, d50 was automatically displayed.

[0058] [Evaluation 3 (Measurement of the average cross-sectional thickness τ' of aluminum particles)] (1) Preparation of painted panels Using the aluminum pigments obtained in the Examples and Comparative Examples, metallic base paints were prepared according to the following compositions. Aluminum pigment: 2g Thinner (Musashi Paint Co., Ltd., product name "Plaace Thinner No. 2726"): 50g Acrylic resin (Musashi Paint Co., Ltd., product name "Plaace No. 7160"): 33g The above paint was applied to an ABS resin plate using an air spray device so that the dry film thickness was 20 μm, and then dried in an oven at 60° C. for 30 minutes to obtain a metallic base-coated plate. A top coat paint prepared according to the following composition was applied onto the metallic base coated plate using an air spray device. -Hitaroid Varnish 3685S (Hitachi Chemical): 25g Mixed thinner (solvent mixing ratio: toluene: 45% by mass, butyl acetate: 30% by mass, ethyl acetate: 20% by mass, 2-acetoxy-1-methoxypropane: 5% by mass): 20g Duranate TPA100 (Asahi Kasei Chemicals): 5g After the above coating, the plate was dried in an oven at 60° C. for 30 minutes to obtain a coated plate for evaluation.

[0059] (2) Cross-section of the coating Using the coated evaluation plates produced as described above, cross sections of the coating film were prepared according to the following procedure. Using scissors, the coated plate for evaluation was cut into pieces measuring 2 cm square. The cut 2 cm square coated evaluation panels were repeatedly cut along the cross section of the coating using a large rotary microtome (RV-240, manufactured by Yamato Koki Kogyo Co., Ltd.) to remove the microscopic aluminum-acrylic resin protruding from the cross section. The cross-section of the coating film obtained above was subjected to ion milling using an ion milling device (JEOL Ltd. / IB-09010CP) set up so as to be able to irradiate the ion beam up to a portion 20 μm away from the cross-section of the coating film, and a cross-section of the coating film for obtaining an FE-SEM image, as described below, was prepared.

[0060] (3) Obtaining particle cross-sections (FE-SEM images) The coating cross-section (coated plate) obtained in the above ((2) Preparation of coating cross-section) was attached parallel to the SEM sample stage, and a field emission type FE-SEM (Hitachi / S-4700) was used to obtain an FE-SEM image of the coating cross-section. The conditions for FE-SEM observation and acquisition were adjusted so that the acceleration voltage was set to 5.0 kV and the image magnification was 10,000 times. In addition, before acquiring (capturing) the FE-SEM image, electronic axis alignment processing was performed to prevent distortion of the boundary between the aluminum particles and the acrylic resin in the FE-SEM image.

[0061] (4) Analysis (measurement of average particle thickness on particle cross section) Using the FE-SEM images (10,000x) obtained by the procedure for obtaining particle cross sections (FE-SEM images) described above ((1)-(3)) and image analysis software Win Roof version 5.5 (MITANI CORPORATION), the particle thicknesses at the cross sections of the aluminum particles were measured and the average thickness was calculated. The FE-SEM image for measuring the particle thickness in the cross section of an aluminum particle was displayed, and the ROI line was selected and aligned with the 5 μm scale of the image, and the length and unit were entered and set using the registration / change. Next, the image of the cross-section of the aluminum particle on which the thickness measurement was to be performed was displayed, a rectangular ROI was selected, and the rectangular ROI was aligned with the cross-section of the particle, and binary processing was performed. Next, the subject was asked to select the measurement item of the vertical chord length, and then the measurement was carried out. The value automatically measured by the image analysis software (vertical chord length value) was displayed on the image. In this manner, using the image analysis software Win Roof version 5.5, 100 particles having an average particle diameter within ±50% of the average particle diameter: d50 described below (IV) average particle diameter: d50 were selected, the thickness of the cross section of the aluminum particles was automatically measured, and the arithmetic mean value of the 100 particles was calculated to determine the average cross-sectional thickness τ' of the particles.

[0062] [Evaluation 4 (Measurement of the average film thickness τ of the resin-adhered aluminum pigment surface)] First, as a pretreatment, the resin-coated metal pigment was ultrasonically cleaned with excess methanol and chloroform, then vacuum dried, dispersed and washed again in acetone, and naturally dried. It was then embedded in epoxy resin and completely cured, after which it was trimmed and cut into sections, and the cross sections were observed with a transmission electron microscope (hereinafter abbreviated as TEM) to observe the surface irregularities of the resin coating layer. Four fields of view, each 1 μm wide, were observed, and the area of ​​the coating layer was measured using image analysis software Image-ProPLUS ver.7.0 (Media Cybernetics), to detect the outline of the entire resin layer, measure the area, and calculate the arithmetic average value of the four fields of view, which was taken as τ.

[0063] [Evaluation 5 (measurement of average surface roughness Ra of resin-adhered aluminum pigment surface)] Using an atomic force microscope (AFM), a line profile (300 scans) of one visual field of 4 μm square of the resin-coated metal pigment was obtained. This was divided into 16 sections, and a third-order tilt correction was performed to obtain the arithmetic average surface roughness. The same operation was performed for a total of four or more visual fields, and the arithmetic average value was calculated and taken as Ra.

[0064] [Evaluation 6 (Evaluation of coating adhesion and chemical resistance)] Using the resin-adhered aluminum pigments obtained in Examples 1 to 9 and Comparative Examples 1 to 6, metallic paints were prepared according to the following compositions. Resin-attached aluminum pigment: 1.3g (solid weight) Thinner (a mixture of 30 parts butyl acetate, 45 parts toluene, 20 parts isopropyl alcohol, and 5 parts ethyl cellosolve): (D) g (the total amount of the resin-attached aluminum pigment and (D) was adjusted to 33 g.) Clear (a mixture of 29 parts of Acrydic A-166 (DIC), 3 parts of nitrocellulose (industrial nitrocellulose 1 / 2AS, Companhia Nitro Qumica Brasileira), and 68 parts of the above thinner) (binder resin component): 42g The resulting coating composition was spray-coated onto an ABS resin plate to a film thickness of 15 μm, and then dried at 55° C. for 30 minutes to prepare a coated plate for evaluation. Using the above-mentioned coating plates for evaluation, the adhesion, chemical resistance, and gloss retention were evaluated.

[0065] (Adhesion of coating film) Using the coated plate prepared above, cellophane tape (registered trademark: CT405AP-18, manufactured by Nichiban Co., Ltd.) was attached to the coating film and pulled at a 45 degree angle, and the degree of peeling of the metal pigment particles was visually observed. Depending on the observation results, the following evaluation was made. ○ (Good): No peeling △ (Acceptable): Slight peeling × (Not acceptable): Peeling occurs

[0066] (Chemical resistance of coating film) The lower half of the coated plate prepared above was immersed in a beaker containing 2.5N NaOH aqueous solution and left at 23°C for 24 hours. After the test, the coated plate was washed with water and dried, and the immersed and unimmersed parts were color-measured according to condition d (8-d method) of JIS-Z-8722 (1982), and the color difference ΔE was calculated according to JIS-Z-8730 (1980) 6.3.2. The color difference ΔE was evaluated as follows (the smaller the value, the better). ○ (Good): Less than 1.0 △ (Acceptable): 1.0 or more and less than 2.0 × (not allowed): 2.0 or more

[0067] [Evaluation 7: FF properties (brightness, lustre) and hiding power of coating film] (1) Preparation of painted panels Using the resin-adhered aluminum pigments obtained in Examples 1 to 11 and Comparative Examples 1 to 6, metallic paints were prepared according to the following compositions. Resin-bonded aluminum pigment: 5.0g Thinner (Kansai Paint Co., Ltd., product name "Acrydic 2000GL"): 13.0g Acrylic resin (Kansai Paint Co., Ltd., product name "Acrydic 2000"): 97.0g Next, the metallic base paint was applied to a PET film using a 3 mil applicator and dried at room temperature for 30 minutes to obtain a metallic base-coated plate.

[0068] (2) Measurement of ΔF / F (brightness, luminosity) The paint prepared above was applied to a PET sheet, and the ΔF / F property of the coating film was evaluated using a variable angle colorimeter (manufactured by Suga Test Instruments Co., Ltd.). The incident angle was set at 45 degrees, and the light receiving angle of 15 degrees (L15), which is close to the regular reflection light, and the light receiving angle of 60 degrees (L60), which is close to the base color, were measured, excluding the light in the specular reflection area reflected by the coating film surface of the coating plate for evaluation. The ratio (L15 / L60) was taken as the FF property.

[0069] (3) Judgment of concealment Concealment The coating film formed by applying the above-mentioned paint to a PET sheet was visually evaluated. Specifically, the above-mentioned paint was prepared using a standard aluminum paste and a resin-coated aluminum paste, and two painted strips were drawn onto a PET sheet, and a light was shone on the unpainted side to evaluate the hiding power. (The standard aluminum paste pigment is the aluminum pigment before it is resin-coated.) ◎: Has the same hiding power as the standard aluminum paste pigment. ◯: Slightly lower hiding power than the standard aluminum paste pigment. △: The hiding power is low compared to the standard aluminum paste pigment. ×: The hiding power is significantly reduced compared to the standard aluminum paste pigment.

[0070] The results of evaluations 1 to 7 are shown in Table 1. [Table 1]

Claims

1. A resin-attached aluminum pigment in which the surfaces of aluminum particles are coated with a resin containing a polymer of a monomer and / or an oligomer having one or more radically polymerizable double bonds, The resin-adhered aluminum pigment has a resin layer surface having an average surface roughness Ra of 0.1 to 5.0 nm.

2. The resin-adhered aluminum pigment according to claim 1, wherein the thickness τ of the resin-adhered layer measured by cross-sectional observation is 10 nm to 20 nm.

3. A resin-attached aluminum pigment in which the surfaces of aluminum particles are coated with a resin containing a polymer of a monomer and / or an oligomer having one or more radically polymerizable double bonds, A resin-adhered aluminum pigment, the thickness τ of a resin-adhered layer being 10 nm to 20 nm as measured by cross-sectional observation.

4. The resin mass per unit mass of the resin-attached aluminum pigment (A (g / g)) and the total surface area per unit mass of the aluminum particles (SSA (m 2 / g)) ((A) / (SSA)) is 0.0077 g / m 2 ~0.025g / m 2 2. The resin-adhered aluminum pigment according to claim 1,

5. 2. The resin-adhered aluminum pigment according to claim 1, wherein the aluminum particles have an average cross-sectional thickness τ' of 0.03 μm to 0.2 μm.

6. The resin-adhered aluminum pigment according to claim 5, wherein the average particle diameter d50 of the aluminum particles is 5 μm to 15 μm.

7. A paint comprising the resin-adhered aluminum pigment according to any one of claims 1 to 6.

8. An ink comprising the resin-adhered aluminum pigment according to any one of claims 1 to 6.

Citation Information

Patent Citations

  • Novel aluminum pigment

    JP2002226733A

  • Resin coated metal pigment and method of producing the same

    JP2012162733A

  • Resin-attached aluminum pigment, coating material composition, coating film, article having the coating film, ink composition and printed matter

    JP2018135455A

  • Resin coated aluminum pigment

    WO2018047360A1