Film for cell pouch and method of storing thereof
A cell pouch film with a sealant, metal, and outer layer, stored at 48-57°C, addresses slip agent leakage and agglomeration issues, ensuring surface roughness and moldability, thus improving process efficiency and reliability.
Patent Information
- Application Number
- JP2024083392
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2024-05-09
- Filing Date
- 2024-05-22
- Publication Date
- 2024-12-05
- Estimated Expiration
- 2044-05-22
AI Technical Summary
Cell pouch films used in electric vehicles and energy storage systems face issues with slip agent leakage and agglomeration, leading to contamination and reduced process efficiency, necessitating a film with improved moldability and reduced slip agent leakage.
A cell pouch film comprising a sealant layer with a slip agent, a metal layer, and an outer layer, stored at a controlled temperature of 48-57°C, which minimizes slip agent leakage and agglomeration, ensuring surface roughness within specific parameters (Rt 13-20 μm and Rz 10-15 μm) and maintains high moldability.
The film effectively prevents excessive slip agent leakage and agglomeration, enhancing moldability and process efficiency by controlling storage temperature, thereby reducing defects and improving product reliability.
Smart Images

Figure 2024169379000001_ABST
Abstract
Description
[Technical field]
[0001] The present specification relates to a film for a cell pouch and a method for storing the same.
[0002] CROSS-REFERENCE TO RELATED APPLICATIONS This application claims priority based on Korean Patent Application No. 10-2023-0066379, filed on May 23, 2023, the entire contents of which are incorporated by reference into this application. This application claims priority based on Korean Patent Application No. 10-2024-0061080, filed on May 9, 2024, the entire contents of which are incorporated herein by reference.
[0003] State-sponsored research and development explanation This research was carried out through the following national projects: - Department name: Ministry of Trade, Industry and Energy, Project management (specialized) agency name: Korea Institute for Industrial Technology Evaluation and Management, Research project name: Material parts packaging type (best company), Research project name: Development of next-generation secondary battery pouch that can realize more than twice the high adhesive strength (60℃), Project execution agency name: Yurimura Chemical Co., Ltd., Project number: 20022450, Project unique number: 1415185612 [Background technology]
[0004] Pouch-type batteries, which are generally used in electric vehicles, have the advantages of being easier to change shape and having a higher energy density than cylindrical or prismatic batteries. A cell pouch is an exterior material that encases the electrodes and electrolyte of a battery, and must meet the required characteristics such as adhesion between layers made of a metal thin film and a polymer, heat fusion strength, electrolyte resistance, airtightness, moisture permeability, and moldability. In particular, cell pouches must have high moldability in order to be applied to large batteries such as electric vehicles (EVs) and energy storage systems (ESSs). For this reason, a slip agent is essential as an additive for improving moldability in cell pouches, and the slip agent provides moldability by flowing to the surface of the outermost layer of the pouch depending on the temperature and pressure after production. However, if an excessive amount of slip agent flows out, the slip agent particles aggregate, causing contamination during the process and a rapid decrease in process efficiency. Therefore, there is a need to develop a cell pouch film that can prevent the aggregation of the slip agent and provide high moldability. Summary of the Invention [Problem to be solved by the invention]
[0005] The problem to be solved by the present disclosure is to provide a cell pouch film having excellent formability and reduced slip agent leakage, and a method for storing the same. [Means for solving the problem]
[0006] One embodiment of the present disclosure includes a sealant layer that includes a slip agent; a metal layer formed on the sealant layer; and an outer layer formed on the metal layer; A film for a cell pouch comprising: The film is stored at a temperature of 48 to 57°C for 30 days, and then, when a lubricant inspection device is used in which a 1.3 kgf cubic metal is wrapped in a black pouch having a matte black appearance and an outer layer made of nylon, the front surface of the black pouch is rubbed against the sealant layer or outer layer of the film at a speed of 400 mm / 10 s, the slip agent that has flowed out of the film and exuded white stripes on the black pouch has a surface roughness of Rt 13 to 20 μm and Rz 10 to 15 μm.
[0007] Another embodiment of the present disclosure provides a cell pouch including the cell pouch film.
[0008] Another embodiment of the present disclosure provides a method for storing the cell pouch film according to any one of the above aspects, the method including a step of storing the film at a temperature of 48 to 57°C. Effect of the Invention
[0009] According to an embodiment of the present disclosure, by controlling the storage temperature after manufacturing the film for cell pouch, it is possible to improve the efficiency of the slip agent by minimizing the phenomenon of the slip agent overflowing to the surface even though the film contains a small amount of slip agent. Therefore, the film according to the present disclosure exhibits excellent formability and prevents the overflow of the slip agent, thereby preventing the occurrence of defects in the process due to the slip agent. [Brief description of the drawings]
[0010] [Figure 1] 1 shows the results of measuring the surface roughness of Example 1, Example 2, and Comparative Example 4 in Test Example 1. [Diagram 2] 1 is an image of the lubricant inspection device used in Test Example 2. [Diagram 3] 13 is an image of a black pouch after a lubricant inspection in Test Example 2. [Figure 4] FIG. 1 is a diagram showing the evaluation criteria (S, A, B grades) for the lubricant inspection in Test Example 2. [Figure 5A] 1 shows the results of particle size analysis of particles formed by agglomeration of slip agent in Example 1 (storage temperature 50° C.) after lubricant testing in Test Example 2 (80x magnification). [Figure 5B] 1 shows the results of particle size analysis of particles formed by agglomeration of slip agent in Example 1 (storage temperature 50° C.) after lubricant testing in Test Example 2 (450x magnification). [Figure 6A] 1 shows the results of particle size analysis of particles formed by aggregation of slip agent in Comparative Example 4 (storage temperature 45° C.) after lubricant inspection in Test Example 2 (80x image). [Figure 6B] 1 shows the results of particle size analysis of particles formed by aggregation of slip agent in Comparative Example 4 (storage temperature 45° C.) after lubricant inspection in Test Example 2 (450x magnification). DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0011] DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS Hereinafter, preferred embodiments of the present disclosure will be described in detail with reference to the accompanying drawings.
[0012] The embodiments of the present disclosure disclosed herein are merely illustrative and are not to be construed as being limited to the embodiments described herein, as the present disclosure may be implemented in various forms. The present disclosure can be modified in various ways and can have various forms, and the embodiments are not intended to limit the present disclosure to the specific disclosed forms, but should be understood to include all modifications, equivalents, or alternatives within the spirit and technical scope of the present disclosure.
[0013] The singular expression includes the plural expression unless the context clearly indicates otherwise. In this application, the terms "comprise" or "have" are intended to indicate the presence of features, numbers, steps, operations, components, parts, or combinations thereof described in the specification, and do not exclude the presence or additional possibility of one or more other features, numbers, steps, operations, components, parts, or combinations thereof.
[0014] In this specification, the term "cell" refers to a battery, and has the broadest meaning including all types of batteries such as secondary batteries such as lithium ion batteries and lithium polymer batteries, and portable storage batteries.
[0015] In this specification, the term "cell pouch" has the broadest meaning including all laminated films processed into a bag or box shape in consideration of gas barrier properties, bendability, electrolyte resistance, thermal adhesiveness, etc., in order to house the cell components, in which the cell components, such as a positive electrode, a negative electrode, and a separator, are impregnated with an electrolyte and stored therein.
[0016] In this specification, "formability" means a property that a film for a cell pouch can be processed into a desired shape without cracks or tears when processed into a predetermined shape and can maintain the shape. For example, the formability can be evaluated by applying a pressure of 0.3 MPa to a test piece obtained by cutting the film for a cell pouch and measuring the maximum depth at which no cracks or tears occur when the film is molded into a cup shape. More specifically, if none of ten of ten identical film test pieces are broken, the deeper depth is applied, and if even one test piece is broken, the depth just before the break may be defined as the maximum height. For example, the formability may be evaluated using a rectangular parallelepiped molding cup (entrance size: 16 cm x 9 cm). More specifically, the formability may be evaluated using the GS-S5 model manufactured by GWANGSHIN HI-TECH.
[0017] One embodiment of the present disclosure provides a film for a cell pouch, the film including a sealant layer, a metal layer formed on the sealant layer, and an outer layer formed on the metal layer, the sealant layer including a slip agent, and the film is stored at a temperature of 48 to 57° C. for 30 days, and then when a front surface of the black pouch is rubbed against the sealant layer or the outer layer of the film at a speed of 400 mm / 10 s using a lubricant inspection device having a shape in which a 1.3 kgf cubic metal is wrapped in a black pouch having a matt black appearance and an outer layer made of nylon, the surface roughness of a portion where the slip agent has oozed out of the film and formed white stripes on the black pouch satisfies Rt 13 to 20 μm and Rz 10 to 15 μm.
[0018] According to an embodiment of the present disclosure, the film may be stored at a temperature of 48 to 57° C., and the storage temperature can be adjusted to prevent excessive outflow and aggregation of the slip agent. Specifically, the storage temperature may be 48° C. or more, 49° C. or more, 50° C. or more, 51° C. or more, 52° C. or more, 53° C. or more, or 54° C. or more, and 57° C. or less, 56° C. or less, 55° C. or less, 54° C. or less, 53° C. or less, 52° C. or less, or 51° C. or less. If the storage temperature exceeds 57° C., moldability may decrease, and if it is less than 48° C., the slip agent may overflow and aggregate, causing process defects and reducing product reliability.
[0019] In one embodiment, the storage period during storage may be 10 to 300 days. Specifically, the storage period may be 10 days or more, 20 days or more, 30 days or more, 40 days or more, 50 days or more, 60 days or more, 70 days or more, 80 days or more, 90 days or more, 100 days or more, 150 days or more, 200 days or more, or 250 days or more, and may be 300 days or less, 200 days or less, 100 days or less, 90 days or less, 80 days or less, 70 days or less, 60 days or less, 50 days or less, 40 days or less, 30 days or less, 20 days or less, or 10 days or less.
[0020] In one embodiment, the relative humidity during storage may be 5% to 25%. In this disclosure, the term "relative humidity (RH)" refers to the ratio of the amount of water vapor currently contained in the air to the maximum saturated water vapor pressure that a given volume of air can contain, expressed as a percentage (%).
[0021] In one embodiment, the surface roughness of the film is a parameter representing the state in which the slip agent contained in the sealant layer of the film flows out to the sealant layer and the outer layer, respectively, and some of the slip agent aggregates. In the present disclosure, the surface roughness refers to the degree of fine irregularities present on the surface. Among the surface roughness parameters, Rt is the maximum height roughness, which is measured by measuring the vertical distance between two parallel lines that are parallel to the center line and pass through the highest and lowest points of the roughness curve within the cut-off length of the cut-off portion. Rz is the ten point median height, which is measured by measuring the distance between the average height of the maximum peak to the fifth peak and the average depth of the maximum valley to the fifth valley.
[0022] In one embodiment, the black pouch used in the measurement of the surface roughness is a pouch (manufacturer: Kurimura Chemical Co., Ltd.) with a matte black appearance and an outer layer made of nylon. When the black pouch is rubbed, the slip agent that flows out of the film may bleed onto the front surface of the black pouch as the front surface of the black pouch and the sealant layer or outer layer of the film rub against each other, forming white stripes. The present disclosure has found that when the film containing a slip agent in the sealant layer exhibits the above-mentioned surface assembly range, a small amount of slip agent flows out, forming small aggregate particles, while still exhibiting high moldability. From this viewpoint, when measured by the above method, the surface roughness of the part where the white stripes are formed may satisfy Rt 13 to 20 μm and Rz 10 to 15 μm. Here, the surface roughness may be a value when the sealant layer is rubbed once or the outer layer is rubbed five times repeatedly in the same direction. Specifically, the surface roughness Rt (μm) may be 13 or more, 14 or more, 15 or more, 16 or more, 17 or more, 18 or more, or 19 or more, and 20 or less, 19 or less, 18 or less, 17 or less, 16 or less, 15 or less, or 14 or less. The surface roughness Rz (μm) may be 10 or more, 11 or more, 12 or more, 13 or more, or 14 or more, and 15 or less, 14 or less, 13 or less, 12 or less, or 11 or less. A film having surface roughness Rt and Rz outside the above ranges may have agglomerated particles of more than 60 μm on the surface of the sealant layer due to excessive outflow of slip agent during a lubricant test, and the friction coefficient and moldability of the sealant layer may be low.
[0023] In one aspect, the film according to one embodiment may be stored at a temperature of 48 to 57°C for 30 days, and then, when the front surface of the black pouch of the lubricant inspection device is rubbed against the sealant layer or outer layer of the film at a speed of 400 mm / 10 s using the same lubricant inspection device as described above, the average diameter of the largest agglomerated particle of the slip agent present in the part where the slip agent flows out of the film and exudes to form white stripes on the black pouch may be 60 μm or less. Here, the agglomerated particle of the slip agent means a particle formed by agglomeration of the flowed out slip agent. The more the slip agent flows out, the larger the particle size becomes. The largest agglomerated particle of the agglomerated particle of the slip agent means the largest agglomerated particle of the formed agglomerated particles, and the average diameter means the average diameter measured for one agglomerated particle. Specifically, the largest agglomerate particle of the slip agent may refer to the largest agglomerate particle of 100% or less, 98% or less, 96% or less, 94% or less, 92% or less, 90% or less, 88% or less, 86% or less, 84% or less, 82% or less, or 80% or less of the total agglomerate particles of the slip agent. Alternatively, the largest agglomerate particle of the slip agent may refer to the largest agglomerate particle of the agglomerate particles included in an image taken by a scanning electron microscope (SEM). Here, the size of the agglomerate particles of the slip agent may be a value when the sealant layer is rubbed once or the outer layer is rubbed five times repeatedly in the same direction. More specifically, the size of the agglomerate particles of the slip agent may be 60 μm or less, 50 μm or less, or 40 μm or less. In one embodiment, the size of the agglomerate particles can be confirmed from a microscope image.
[0024] In one aspect, the film according to one embodiment may have a formability of 15 to 25 mm after storage for 30 days at a temperature of 48 to 57° C. Here, the formability is measured by applying a pressure of 0.3 MPa to the film and measuring the maximum depth at which the film does not break when molded into one cup (16 cm×9 cm). More specifically, the formability may be 15 mm or more, 16 mm or more, 17 mm or more, 18 mm or more, 19 mm or more, 20 mm or more, 21 mm or more, 22 mm or more, or 23 mm or more, and may be 25 mm or less, 24 mm or less, 23 mm or less, 22 mm or less, 21 mm or less, or 20 mm or less.
[0025] In one aspect, the film according to one embodiment may have a friction coefficient of 0.15 to 0.5 when the friction coefficient is evaluated as follows after storing the film according to one embodiment at a temperature of 48 to 57°C for 30 days: (a) a cell pouch is manufactured using the film according to one embodiment of the present disclosure, and then the cell pouch is cut to a size of 200 mm x 100 mm to prepare a test piece, and the test piece is attached flat to the bottom of a friction coefficient measuring device. (b) Next, a test piece of the same cell pouch as the above, having a size of 70 mm x 60 mm, is fixed to a friction coefficient measuring tool. (c) Next, a tool provided in the friction coefficient measuring device is sandwiched between the two pouches so as to abut against both of the two pouches, and then the bottom of the friction coefficient measuring device is moved at a speed of 15 mm / 1 s for 55 seconds to measure the friction coefficient between the sealant layers of the pouches. In one embodiment, the friction coefficient measuring device may be a CF-800XS model manufactured by Labsink. Specifically, the friction coefficient may be 0.15 or more, 0.2 or more, 0.25 or more, or 0.3 or more, and may be 0.5 or less, 0.4 or less, 0.35 or less, 0.3 or less, 0.25 or less, or 0.2 or less.
[0026] In the present disclosure, the material and thickness of each layer of the film are not particularly limited as long as they can be manufactured into a film for a cell pouch, and may include, for example, the following configurations.
[0027] In the present disclosure, the sealant layer means an inner layer that is bonded by heat after the cell is built in to provide sealing properties. As an example, the sealant layer may include a thermal adhesive resin, i.e., a sealing resin for thermal adhesion. Specifically, the sealant layer may include one or more selected from the group consisting of polyolefins such as polypropylene (PP) and polyethylene (PE), copolymers, terpolymers or derivatives thereof, and ethylene vinyl acetate (EVA). The copolymer or terpolymer may include an ethylene / propylene copolymer or an ethylene / propylene / butadiene terpolymer. As an example, the sealant layer may have a thickness of 20 μm to 100 μm. The sealant layer may be composed of a plurality of layers.
[0028] In the present disclosure, the slip agent refers to an additive for reducing the friction coefficient and imparting lubricity and moldability to the surface of the film. In one embodiment, the slip agent may include one or more of a wax-based, an amide-based, a siloxane, and a silicone. Specifically, the slip agent may be an oleic acid amide-based slip agent. More specifically, the slip agent may include one or more of erucamide, behenamide, stearamide, and oleamide.
[0029] In one embodiment, the film may include 0.1 to 20 weight percent of a slip agent based on the total weight of the sealant layer. Specifically, the film may contain at least 0.1 wt.%, at least 0.2 wt.%, at least 0.3 wt.%, at least 0.4 wt.%, at least 0.5 wt.%, at least 0.6 wt.%, at least 0.7 wt.%, at least 0.8 wt.%, at least 0.9 wt.%, at least 1 wt.%, at least 2 wt.%, at least 3 wt.%, at least 4 wt.%, at least 5 wt.%, at least 6 wt.%, at least 7 wt.%, at least 8 wt.%, at least 9 wt.%, at least 12 wt.%, at least 15 wt.%, at least 17 wt.%, or at least 19 wt.%, and may contain at most 20 wt.%, at most 17 wt.%, at most 15 wt.%, at most 13 wt.%, at most 10 wt.%, at most 9 wt.%, at most 8 wt.%, at most 7 wt.%, at most 6 wt.%, at most 5 wt.%, at most 4 wt.%, at most 3 wt.%, at most 2 wt.%, at most 1 wt.%, or at most 0.5 wt.% of the slip agent based on the total weight of the sealant layer. If the slip agent is added in an amount exceeding the above range, the sealing strength may be reduced, the winding state may be poor, and the physical properties may become non-uniform over time. Also, if the slip agent is added in an amount less than the above range, the moldability may be reduced.
[0030] In the present disclosure, the outer layer means a layer having heat resistance, abrasion resistance, chemical resistance, etc. to protect the metal layer. In one embodiment, the outer layer may include one selected from the group consisting of polybutylene adipate terephthalate (PBAT), polybutylene succinate (PBS), polyhydroxy aldehyde (PHA), polylactic acid (PLA), thermoplastic starch (TPS), polyvinyl alcohol (PVA), polycaprolactam (PCL), polyethylene (PE), polypropylene (PP), ethylene vinyl acetate (EVA), ethylene vinyl alcohol (EVOH), polyvinylidene chloride (PVDC), polyethylene terephthalate (PET), and nylon. More specifically, the outer layer may include one or more resins selected from nylon resin, polyethylene terephthalate (PET), polybutylene terephthalate (PBT), etc. In one embodiment, the outer layer may have a thickness of 5 μm to 40 μm. The outer layer may be composed of a plurality of layers.
[0031] In this specification, the metal layer refers to a barrier layer having a function of blocking water vapor or air from outside the battery, gas generated inside the battery, and / or moisture. In one embodiment, the metal layer may further include a surface treatment layer uniformly coated on one or both sides. In one embodiment, the metal layer may be a metal thin film or a metal deposition layer. The metal thin film may be a metal foil. The metal deposition layer may be formed by vacuum-depositing a metal on a separate plastic film, for example, a film such as polyethylene terephthalate (PET), polyethylene (PE), or polypropylene (PP).
[0032] As an example, the metal of the metal layer is not particularly limited as long as it has the above-mentioned barrier performance, and examples thereof include one or more selected from the group consisting of aluminum (Al), iron (Fe), copper (Cu), magnesium (Mg), nickel (Ni), tin (Sn), zinc (Zn), indium (In), and tungsten (W) (single metal or mixture of single metals), or an alloy of two or more selected from the group consisting of aluminum or its alloy, titanium or its alloy, tungsten or its alloy, molybdenum or its alloy, copper or its alloy, and stainless steel. More specifically, it may include aluminum. As an example, the surface treatment layer may be a surface treatment layer made of phosphoric acid, chromium, zirconium, cerium, lanthanum, scandium, yttrium, etc. to provide corrosion resistance of the metal.
[0033] In one embodiment, the metal layer may have a thickness of 20 μm to 80 μm. If the thickness of the metal layer is less than 20 μm, pinholes, microcracks, etc. may occur during processes such as molding, making it difficult to ensure safety, and if the thickness of the metal layer is more than 80 μm, the energy density may be reduced during battery fabrication.
[0034] An embodiment of the present disclosure may further include an adhesive layer between the metal layer and the outer layer for bonding the metal layer and the outer layer. Also, an embodiment of the present disclosure may further include an adhesive layer between the sealant layer and the metal layer for bonding the metal layer and the sealant layer. Specifically, the adhesive layer may be an adhesive layer and / or an extruded resin layer. For example, the adhesive layer may include one or more of an epoxy adhesive, a polyurethane adhesive, a phenolic resin adhesive, a polyolefin adhesive, and a polyester adhesive. In one embodiment, the adhesive layer may have a thickness of 0.5 μm to 10 μm. For example, the extruded resin layer may include an olefin resin such as a polypropylene resin. In one embodiment, the extruded resin layer may have a thickness of about 5 to 80 μm.
[0035] One embodiment of the present disclosure can provide a cell pouch including the above-described film for a cell pouch.
[0036] Another embodiment of the present disclosure may provide a method for storing the above-mentioned cell pouch film, comprising storing the film at a temperature of 48 to 57° C. Specifically, the storage temperature may be 48° C. or more, 49° C. or more, 50° C. or more, 51° C. or more, 52° C. or more, 53° C. or more, or 54° C. or more, and may be 57° C. or less, 56° C. or less, 55° C. or less, 54° C. or less, 53° C. or less, 52° C. or less, or 51° C. or less. If the storage temperature exceeds 57° C., moldability may decrease, and if it is less than 48° C., the slip agent may overflow and aggregate, causing process defects and decreasing product reliability.
[0037] In one embodiment, the storage period of the storage step may be 10 days or more, specifically, 10 days or more, 20 days or more, 30 days or more, 40 days or more, 50 days or more, 60 days or more, 70 days or more, 80 days or more, 90 days or more, 100 days or more, 150 days or more, 200 days or more, or 250 days or more, and may be 300 days or less, 200 days or less, 100 days or less, 90 days or less, 80 days or less, 70 days or less, 60 days or less, 50 days or less, 40 days or less, 30 days or less, or 20 days or less.
[0038] In one embodiment, the relative humidity during the storage stage may be between 5% and 25%.
[0039] The present disclosure will be described in more detail with reference to the following examples. However, it will be obvious to those skilled in the art that these examples are merely for the purpose of illustrating the disclosure and should not be construed as limiting the scope of the present disclosure.
[0040] [Production Example] An example of the present disclosure was prepared by the following method.
[0041] A 25 μm outer layer of polyethylene terephthalate film was formed on one side of a 60 μm thick metal layer made from a metal roll of aluminum foil, and a 80 μm sealant layer was formed by laminating a non-oriented polypropylene film containing an amide-based slip agent in an amount of 0.1 to 20 wt % based on the total weight of the sealant layer on the other side of the metal layer, to produce a film for a cell pouch.
[0042] As an example of the present disclosure, a film for a cell pouch can be manufactured using an outer layer in which a 12 μm polyethylene terephthalate film and a 25 μm nylon film are laminated to the outer layer, and it was confirmed that in this case as well, the results of the test example described below were the same.
[0043] [Test Example 1] In order to confirm the surface roughness depending on the storage temperature during storage of the films produced in the above Production Examples, the following experiment was carried out.
[0044] First, a lubricant testing device was prepared by wrapping the surface of a cubic metal (iron) (weight: approximately 1.3 kg) in a black pouch (manufacturer: Kurimura Chemical Co., Ltd.). The film manufactured in the above manufacturing example, cut to a size of 50 mm x 240 mm, was fixed on a flat surface with the sealant layer facing up, and the black pouch of the device was rubbed once against the sealant layer of each film stored at different storage temperatures at a speed of 400 mm / 10 s. Next, the area where the slip agent had leaked out of the film and formed white stripes on the black pouch was cut into 1 x 1 cm pieces. 2 The sample was cut to the size of 10 mm and attached flat to a slide glass using double-sided tape, and the surface roughness was measured using a surface roughness measuring device (e.g., NV-2200 3D profiler, Nano Systems) and an analysis program (NanoMap, Nano Systems).
[0045] Among these, the results of Examples 1 and 2 and Comparative Example 4 are shown in FIG.
[0046] [Table 1]
[0047] As shown in the above results, it can be confirmed that in Examples 1 and 2 of the present disclosure, the surface roughness Rt falls within the range of 13 to 20 μm and the surface roughness Rz falls within the range of 10 to 15 μm by adjusting the storage temperature.
[0048] [Test Example 2] In order to confirm the aggregation state, friction coefficient, and moldability of the slip agent according to the surface roughness of the film according to one embodiment of the present disclosure, the following experiments were carried out on Examples 1 and 2 and Comparative Examples 1 to 4 whose surface roughness was confirmed in Test Example 1, and the measured values are shown in Tables 2 to 9. At this time, the moldability, lubricant test, and friction coefficient of each film were measured at room temperature on day 0, and then the results were observed while storing the films at each set storage temperature for 90 days.
[0049] Lubricant Inspection The lubricant test is to measure the amount or agglomeration state of the slip agent flowing out onto the surface of the sealant layer or outer layer of the film for the cell pouch. The same lubricant tester as that used for the surface roughness measurement was prepared, and the prepared film was cut into a size of 50 mm x 240 mm, fixed on a flat surface with the sealant layer or outer layer facing upward, and rubbed against the sealant layer or outer layer of each prepared film at a speed of 400 mm / 10 s. The test was repeated once when the sealant layer was rubbed, and five times when the outer layer was rubbed. Next, the area where the slip agent flowed out from each film and oozed out to form white stripes on the black pouch was photographed using a scanning electron microscope (SEM, manufacturer: HITACHI, product name: SU3500), and the size of the agglomerated particles of the slip agent was confirmed and evaluated by scanning visual inspection. Figure 2 is a photograph of the lubricant inspection device used in the experiment, and Figure 3 is an image of the black pouch after the experiment, where it can be seen that a white stripe has formed at the top of the black pouch. As shown in Figure 4, the results of visual evaluation were graded as follows: if a white stripe was found only on one side of the edge and there were few scratches over most of the area, it was rated as Grade S; if two lines were found on the edge (white stripe area) and there were scratches on the slip agent, it was rated as Grade A (A+, A0 or A-); if two lines were found on the corners and the slip agent was applied over the entire surface, it was rated as Grade B.
[0050] In addition, when analyzing the SEM images, the number of the largest agglomerated particles of slip agent present in the area where the slip agent had leaked out and formed white streaks on the black pouch was selected and their average diameter was determined.
[0051] Measurement of the coefficient of friction Each prepared film was cut to a size of 200 x 100 mm, and the friction coefficient of each film was measured using a friction coefficient measuring device (manufacturer: Labsink, product name: CF-800XS). Specifically, a test piece of each film was prepared to a size of 200 mm x 100 mm and attached flatly to the bottom of the friction coefficient measuring device, and then a test piece of the same film, 70 mm x 60 mm in size, was attached to a jig equipped in the friction coefficient measuring device, and the jig was connected to the equipment with a string. The jig was placed on the equipment so that the two films were in contact with each other, and the bottom of the equipment was moved at a speed of 15 mm / 1 s for 55 seconds, during which the film of the jig fixed with the string did not move, and the friction coefficient between the two films was measured.
[0052] Measurement of formability Each prepared film was cut to a size of 200 x 100 mm, placed on a cup-shaped mold (manufacturer: GWANGSHIN HI-TECH, model: GS-S5) and molded into a cup shape by applying a pressure of 0.3 MPa, and the maximum depth at which no cracks or tears occurred during molding was measured. In this case, if none of the 10 samples of the same film specimen were broken, a deeper depth was applied, and if even one sample was broken, the depth just before that was defined as the maximum height.
[0053] Comparative Example 1 [Table 2]
[0054] Comparative Example 2 [Table 3]
[0055] Comparative Example 3 [Table 4]
[0056] Comparative Example 4 [Table 5]
[0057] Example 1 [Table 6]
[0058] Example 2 [Table 7]
[0059] Comparative Example 5 [Table 8]
[0060] Figures 5A, 5B, 6A, and 6B show the results of particle size analysis of the aggregated particles formed by the slip agent that flowed out after the lubricant test. Figures 5A and 5B are images of the film of Example 1 in the table, and the average diameter of the largest aggregated particles present in the SEM image was 39.2 μm. Figures 6A and 6B are images of the film of Comparative Example 4 in the table. The average diameter of the largest aggregated particles present in the SEM image of Comparative Example 4 in Figure 6A was 40.9 μm, and the average diameter of the largest aggregated particles present in the SEM image of Comparative Example 4 in Figure 6B was 97.5 μm.
[0061] The results are summarized in the table below.
[0062] [Table 9]
[0063] As can be seen from the above results, unlike Comparative Examples 1 to 4, Examples 1 and 2 of the present disclosure satisfied the surface roughness Rt range of 13 to 20 μm and Rz range of 10 to 15 μm, and thus the size of the agglomerated particles of the slip agent present on the surface of the sealant layer during the lubricant test was reduced to 60 μm or less. Furthermore, it can be confirmed that Examples 1 and 2 maintain the friction coefficient of the sealant layer at 0.15 or more, and the moldability is improved by about 40% compared to room temperature (day 0), showing excellent moldability even though a small amount of slip agent flows out.
[0064] [Test Example 3] Films were produced according to the above Production Examples, and by adjusting the storage temperature, Examples 3 and 4 were prepared in which the film surface roughness Rt was within the range of 13 to 20 μm and Rz was within the range of 10 to 15 μm, and Comparative Examples 5 to 8 were prepared in which the film surface roughness was outside the above range. In order to confirm the cohesion state, friction coefficient, and moldability of the slip agent according to the surface roughness of the film, the surface roughness, lubricant test, friction coefficient, and moldability of each film were measured in the same manner as described in Test Examples 1 and 2, and the measured values are shown in Table 10.
[0065] [Table 10]
[0066] As a result, Examples 3 and 4 of the present disclosure, which satisfy the surface roughness ranges of Rt 13 to 20 and Rz 10 to 15, both received an S grade in the lubricant test and showed a high friction coefficient of 0.2 or more. Furthermore, although Examples 3 and 4 contain the same amount of slip agent as Comparative Examples 5 to 8, it can be confirmed that the outflow amount of the slip agent is adjusted to satisfy the surface roughness range, and the moldability is remarkably excellent.
[0067] The present disclosure can provide the following embodiments as examples.
[0068] [First embodiment] a sealant layer, which includes a slip agent; a metal layer formed on the sealant layer; and an outer layer formed on the metal layer; A film for a cell pouch comprising: The film is a film for a cell pouch, and after storing the film at a temperature of 48 to 57°C for 30 days, when a lubricant testing device is used in which a 1.3 kgf cubic metal is wrapped in a black pouch having a matt black appearance and an outer layer made of nylon, and the front surface of the black pouch is rubbed against the sealant layer or outer layer of the film at a speed of 400 mm / 10 s, the surface roughness of the part where the slip agent has oozed out of the film and formed white streaks on the black pouch satisfies Rt 13 to 20 μm and Rz 10 to 15 μm.
[0069] [Second embodiment] The film according to the first embodiment, wherein after storing the film at a temperature of 48 to 57°C for 30 days, when a lubricant testing device is used to rub the front surface of a 1.3 kgf cubic metal pouch having a matt black appearance and an outer layer made of nylon against the sealant layer or outer layer of the film at a speed of 400 mm / 10 s, the slip agent that has leaked out of the film and exuded white streaks on the black pouch has an average diameter of the largest agglomerated particle of 60 μm or less.
[0070] [Third embodiment] The film according to the first or second embodiment, wherein the friction coefficient of the sealant layer after storage at a temperature of 48 to 57° C. for 30 days is 0.15 to 0.5.
[0071] [Fourth embodiment] The film has a formability of 15 to 25 mm after storage for 30 days at a temperature of 48 to 57°C; The film according to any one of the first to third embodiments, wherein the formability is measured by applying a pressure of 0.3 MPa to the film and measuring the maximum depth at which the film does not break when molded into one cup.
[0072] [Fifth embodiment] The film according to any one of the first to fourth embodiments, wherein the film is intended to be stored at a temperature of 48 to 57°C.
[0073] [Sixth embodiment] The film according to any one of the first to fifth embodiments, wherein the film contains 0.1 to 20% by weight of a slip agent based on the total weight of the sealant layer.
[0074] [Seventh embodiment] The film according to any one of the first to sixth embodiments, wherein the slip agent includes at least one of a wax-based agent, an amide-based agent, a siloxane agent, and a silicone agent.
[0075] [Eighth embodiment] The film according to any one of the first to seventh embodiments, wherein the metal layer contains at least one selected from the group consisting of aluminum or an alloy thereof, titanium or an alloy thereof, tungsten or an alloy thereof, molybdenum or an alloy thereof, copper or an alloy thereof, and stainless steel.
[0076] [Ninth embodiment] The film according to any one of the first to eighth embodiments, wherein the outer layer includes one selected from the group consisting of polybutylene adipate terephthalate (PBAT), polybutylene succinate (PBS), polyhydroxy aldehyde (PHA), polylactic acid (PLA), thermoplastic starch (TPS), polyvinyl alcohol (PVA), polycaprolactam (PCL), polyethylene (PE), polypropylene (PP), ethylene vinyl acetate (EVA), ethylene vinyl alcohol (EVOH), polyvinylidene chloride (PVDC), polyethylene terephthalate (PET), and nylon.
[0077] [Tenth embodiment] The film according to any one of the first to ninth embodiments, wherein the sealant layer contains a thermal adhesive resin.
[0078] [Eleventh embodiment] A method for storing the cell pouch film according to any one of the first to tenth embodiments, A storage method comprising the step of storing the film at a temperature of 48 to 57°C.
[0079] [Twelfth embodiment] The storage method according to the eleventh embodiment, wherein the storage period of the above steps is 10 to 300 days.
[0080] [Thirteenth embodiment] The storage method according to the eleventh or twelfth embodiment, wherein the relative humidity during storage in the above step is 5% to 25%.
Claims
1. a sealant layer comprising a slip agent; a metal layer formed on the sealant layer; and an outer layer formed on the metal layer; A film for a cell pouch comprising: The film is a film for a cell pouch, which is stored at a temperature of 48 to 57°C for 30 days, and then, when a lubricant inspection device is used to rub the front surface of a black pouch having a matt black appearance and an outer layer made of nylon, against the sealant layer or outer layer of the film at a speed of 400 mm / 10 s, the surface roughness of the part where the slip agent has oozed out of the film and formed white stripes on the black pouch satisfies Rt 13 to 20 μm and Rz 10 to 15 μm.
2. 2. The film according to claim 1, wherein, after storing the film at a temperature of 48 to 57° C. for 30 days, when a front surface of a black pouch made of 1.3 kgf cubic metal with a matt black appearance and an outer layer made of nylon is rubbed against the sealant layer or outer layer of the film at a speed of 400 mm / 10 s using a lubricant inspection device, the front surface of the black pouch is rubbed against the sealant layer or outer layer of the film at a speed of 400 mm / 10 s., the slip agent leaked from the film and exuded white streaks on the black pouch.
3. 10. The film of claim 1, wherein the film has a coefficient of friction of the sealant layer of 0.15 to 0.5 after storage at a temperature of 48 to 57°C for 30 days.
4. The film has a formability of 15 to 25 mm after storage for 30 days at a temperature of 48 to 57°C; The film according to claim 1 , wherein the formability is measured by applying a pressure of 0.3 MPa to the film and measuring the maximum depth at which the film does not break when molded into one cup.
5. 10. The film of claim 1, wherein the film is for storage at a temperature of 48-57°C.
6. 10. The film of claim 1, wherein the film comprises 0.1 to 20 weight percent of a slip agent, based on the total weight of the sealant layer.
7. 10. The film of claim 1, wherein the slip agent comprises one or more of wax-based, amide-based, siloxane, and silicone.
8. 2. The film of claim 1, wherein the metal layer comprises at least one selected from the group consisting of aluminum or an alloy thereof, titanium or an alloy thereof, tungsten or an alloy thereof, molybdenum or an alloy thereof, copper or an alloy thereof, and stainless steel.
9. The outer layer may be made of polybutylene adipate terephthalate (PBAT), polybutylene succinate (PBS), polyhydroxy aldehyde (PHA), polylactic acid (PLA), thermoplastic starch (TPS), polyvinyl alcohol (PVA), polycaprolactam (PCL), polyethylene (PE), polypropylene (PP), ethylene vinyl acetate (ethylene vinyl acetate), or the like.
2. The film of claim 1, comprising one selected from the group consisting of polyvinyl acetate (EVA), ethylene vinyl alcohol (EVOH), polyvinylidene chloride (PVDC), polyethylene terephthalate (PET), and nylon.
10. The film of claim 1 , wherein the sealant layer comprises a thermal adhesive resin.
11. A method for storing the cell pouch film according to any one of claims 1 to 10, comprising: A method of storage comprising storing the film at a temperature of 48-57°C.
12. The method according to claim 11, wherein the storage period in each step is from 10 to 300 days.
13. The method for storing according to claim 11, wherein the relative humidity during storage in said step is 5% to 25%.
Citation Information
Patent Citations
Polypropylene-based composite film, laminate using same, packaging pouch for battery exterior, and retort packaging pouch
WO2018088257A1
Sealant film