Production method of nickel sulfate aqueous solution

The method enhances nickel sulfate solution production by employing pressurized oxidation leaching and controlled pH adjustments to separate and recover nickel from neutralized precipitates, addressing inefficiencies in existing processes and improving recovery rates.

JP2024170245APending Publication Date: 2024-12-06SUMITOMO METAL MINING CO LTD

Patent Information

Application Number
JP2023087303
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-05-26
Publication Date
2024-12-06

AI Technical Summary

Technical Problem

Existing methods for producing nickel sulfate solutions face challenges in achieving high nickel recovery rates from neutralized precipitates produced during the iron removal process without increasing costs, as they often result in the precipitation of nickel hydroxide along with iron hydroxide, leading to inefficiencies in nickel recovery.

Method used

A method involving pressurized oxidation leaching, oxidative neutralization, and controlled pH adjustments during dissolution steps to separate and recover nickel from neutralized precipitates, utilizing a series of solid-liquid separation processes and solvent extraction to enhance nickel recovery.

Benefits of technology

The method effectively recovers more nickel from neutralized precipitates without significant cost increases, improving the overall efficiency and purity of the nickel sulfate solution production process.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024170245000001_ABST
    Figure 2024170245000001_ABST
Patent Text Reader

Abstract

To provide a production method of a nickel sulfate aqueous solution which can recover nickel with a high recovery rate without spending great cost.SOLUTION: A production method of a nickel sulfate aqueous solution includes: a pressurization oxidation leaching step of charging raw material slurry including nickel sulfide into an autoclave to subject the slurry to oxidation leaching treatment under high temperature and pressure to thereby produce a leachate including the nickel sulfate aqueous solution; an iron removal step of subjecting leached slurry including the leachate and a leaching residue to oxidation neutralization treatment to produce a neutralization precipitate including iron hydroxide; a first solid-liquid separation step of performing solid-liquid separation of iron-removed slurry obtained in the iron removal step to remove an iron-removed primary precipitate including the neutralization precipitate and the leaching residue to thereby obtain a crude nickel sulfate aqueous solution; and a dissolution step of adding sulfuric acid to the iron-removed primary precipitate to dissolve nickel hydroxide contained in the neutralization precipitate. In the dissolution step, a pH of a liquid phase is adjusted so as to be in a range of 2.3 to 3.0.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for producing an aqueous nickel sulfate solution. [Background technology]

[0002] Nickel sulfate is used for a wide range of applications, including nickel plating, aluminum coloring, catalysts, and positive electrode materials for secondary batteries. For example, a pressurized oxidation leaching method is used as a method for producing nickel sulfate, in which a nickel sulfide raw material is charged into a pressure vessel called an autoclave and leaching is performed under high temperature and high pressure. Examples of nickel sulfide raw materials include nickel matte produced by dry smelting, and nickel-cobalt mixed sulfide (MS) produced by adding a sulfurizing agent to nickel and cobalt sulfates produced by high pressure acid leaching, which adds sulfuric acid and high pressure steam to a slurry of nickel oxide ore with a low Ni content and leaches valuable metals nickel and cobalt as sulfates under high temperature and high pressure. In the above-mentioned leaching process, impurities such as iron are leached out in addition to nickel, which is the target metal for production. Therefore, the leachate obtained by the leaching process is subjected to an oxidation neutralization process in which the iron is removed as a neutralized precipitate, and then impurities that cannot be removed in the iron removal process are removed in a solvent extraction process or the like to produce a high-purity aqueous nickel sulfate solution.

[0003] For example, Patent Document 1 discloses a technology in which an aqueous solution of crude nickel sulfate obtained by dissolving a nickel raw material in a sulfuric acid solution in a nickel refining process contains iron, aluminum, chromium, zinc, arsenic, and phosphorus, which are problematic when producing nickel sulfate crystals, and in which sodium hydroxide or hydrated lime is added as a pH adjuster while blowing air into the aqueous solution of crude nickel sulfate charged in a reaction tank, thereby separating and removing impurities mainly consisting of iron as a neutralized precipitate, and then purifying the obtained de-ironized liquid in a solvent extraction process. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] JP 2006-225217 A DISCLOSURE OF THEINVENTION [Problem to be solved by the invention]

[0005] In the above iron removal treatment, the pH during treatment is generally set to be relatively high in order to more reliably remove the iron contained in the aqueous solution of crude nickel sulfate. Therefore, the neutralized precipitate contains hydroxide of nickel, the target metal, precipitated together with hydroxide of iron. Therefore, sulfuric acid is added to the neutralized precipitate separated and removed to dissolve the nickel, and then the nickel is recovered by solid-liquid separation.

[0006] As described above, by dissolving the neutralized precipitate separated and removed in the iron removal step with sulfuric acid and then performing solid-liquid separation, it is possible to recover a certain amount of nickel precipitated together with the iron content, but the dissolution residue after dissolution with sulfuric acid still contains nickel, and there has been a demand for a further increase in the nickel recovery rate. The dissolution residue is discharged outside the nickel sulfate production process. The present invention has been made in view of the above circumstances, and an object of the present invention is to provide a method for producing an aqueous nickel sulfate solution that can recover a large amount of nickel from the neutralized precipitate generated in the iron removal step without incurring too much cost. [Means for solving the problem]

[0007] In order to achieve the above object, the method for producing an aqueous nickel sulfate solution according to the present invention comprises a pressurized oxidation leaching step of charging a raw material slurry containing nickel sulfide into an autoclave and performing an oxidation leaching treatment under high temperature and high pressure to produce a leachate consisting of an aqueous nickel sulfate solution; a de-ironizing step of performing an oxidation neutralization treatment on a leach slurry consisting of the leachate and a leach residue to produce a neutralized precipitate containing iron hydroxide; a first solid-liquid separation step of performing solid-liquid separation of the de-ironizing slurry obtained in the de-ironizing step to remove the neutralized precipitate and a de-ironizing primary precipitate consisting of the leach residue to obtain an aqueous crude nickel sulfate solution; and a dissolution step of adding sulfuric acid to the de-ironizing primary precipitate to dissolve nickel hydroxide contained in the neutralized precipitate, wherein the pH of the liquid phase in the dissolution step is adjusted to a range of 2.3 to 3.0. Effect of the Invention

[0008] According to the present invention, it is possible to recover a larger amount of nickel from the neutralized precipitate generated during the production of an aqueous nickel sulfate solution without incurring significant costs. [Brief description of the drawings]

[0009] [Figure 1] FIG. 1 is a block flow diagram of an embodiment of a method for producing an aqueous nickel sulfate solution according to the present invention. [Diagram 2] FIG. 2 is a vertical cross-sectional view of an autoclave preferably used in the pressurized oxidation leaching process of FIG. 1. [Diagram 3] FIG. 1 is a schematic flow diagram of a production facility capable of suitably carrying out a method for producing nickel sulfate according to the present invention. [Figure 4] FIG. 1 is a graph plotting the ratio of the amount of insoluble nickel dissolved to the amount of iron from the deironated primary sediment (amount of insoluble Ni / Fe dissolved) with pH on the horizontal axis when the deironated primary sediment is repulped at various pH levels in the dissolution step of a nickel sulfate production method according to an embodiment of the present invention. [Diagram 5]FIG. 1 is a graph plotting the time required to filter, with a filter press, slurries obtained by repulping the iron-removed primary sediment at various pH values ​​in the dissolution step of a nickel sulfate production method according to an embodiment of the present invention, and the Fe concentration of the filtrate (nickel recovery solution), with pH on the horizontal axis. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0010] Hereinafter, an embodiment of the method for producing a nickel sulfate aqueous solution according to the present invention will be described in detail. The method for producing a nickel sulfate aqueous solution according to the embodiment of the present invention uses nickel-cobalt mixed sulfide (MS: mixed sulfide) consisting of a mixture of nickel sulfide (NiS) and cobalt sulfide (CoS) as a raw material containing nickel sulfide. The typical composition of this nickel-cobalt mixed sulfide on a dry basis is about 50 to 60 mass% nickel, 4 to 6 mass% cobalt, and 30 to 34 mass% sulfur, and contains magnesium, iron, copper, zinc, etc. as impurities.

[0011] Nickel-cobalt mixed sulfide can be produced by treating nickel oxide ore such as low-grade limonite ore by a hydrometallurgical process. Specifically, this hydrometallurgical process mainly comprises a process of subjecting an ore slurry prepared by adding water to nickel oxide ore to a high pressure acid leaching (HPAL) process to produce a leachate containing nickel and cobalt, a process of adding a neutralizing agent to the leachate to separate and remove impurities such as iron in the form of a neutralized precipitate, and a process of producing a nickel-cobalt mixed sulfide by blowing a sulfurizing agent such as hydrogen sulfide gas into the neutralized final solution after the neutralized precipitate is separated and removed. The method for producing nickel sulfate according to an embodiment of the present invention treats the nickel-cobalt mixed sulfide obtained by the hydrometallurgical process in a raw material preparation process, a pressure oxidation leaching process, a deironization process, a first solid-liquid separation process, a solvent extraction process, a crystallization process, a dissolution process, and a second solid-liquid separation process, as shown in the block flow of FIG. 1. Each of these steps will now be described in detail.

[0012] 1. Method for producing nickel sulfate aqueous solution (1) Raw material preparation process In the raw material preparation step, a raw material slurry having a solid content concentration (also called a slurry concentration) of about 200 to 300 g / L is prepared by adding water to the raw material nickel-cobalt mixed sulfide at a predetermined ratio and mixing. The nickel recovery liquid separated in the second solid-liquid separation step described below is preferably used repeatedly as the water to be added. The nickel-cobalt mixed sulfide contains 0.1 to 1 mass % of iron.

[0013] (2) Pressure oxidation leaching process In the pressurized oxidation leaching process, an autoclave is used in which a cylindrical pressure vessel 1 as shown in Fig. 2 is laid horizontally with its central axis facing horizontally, and the vessel is partitioned into a plurality of reaction chambers 3a to 3e by a plurality of partition walls 2 (four partition walls 2 are shown in Fig. 2) with their upper openings. The raw material slurry prepared in the raw material preparation process is charged into the most upstream reaction chamber 3a of this autoclave, and while the raw material slurry is allowed to overflow the upper ends of the plurality of partition walls 2 and transferred sequentially to the downstream reaction chambers, high-pressure air is blown into each of the reaction chambers 3a to 3e through a gas discharge pipe 5 having an outlet below the stirring blades of a stirrer 4 provided in each of the reaction chambers, thereby causing an oxidation reaction under high temperature and pressure, for example, at a pressure of about 1.0 to 2.0 MPaG and a temperature of about 140 to 200°C, to carry out the leaching process.

[0014] By the above leaching treatment, nickel and cobalt contained in the nickel-cobalt mixed sulfide are leached together with some of the impurities, and a leaching slurry consisting of a leaching solution of nickel sulfate aqueous solution with a pH of about 1 to 2 and a leaching residue is produced. Since the above oxidation reaction is exothermic, the autoclave is provided with a device for cooling the leaching slurry with cooling water. The produced leaching slurry is discharged from the autoclave and the pressure is reduced to almost atmospheric pressure in a flash tank, and then the leaching slurry is de-ironized in the next de-ironization process.

[0015] (3) Iron removal process In the iron removal process, air is blown into the leaching slurry as an oxidizing agent to remove the Fe contained in the leaching solution. 2+Fe 3+ The leachate is oxidized to 100% by weight, and a neutralizing agent such as slaked lime, calcium carbonate, or sodium hydroxide is added to cause the oxidation neutralization reaction shown in Chemical Formula 1 below. As a result, a neutralized precipitate consisting of Fe(OH)3 is produced from impurities mainly consisting of iron contained in the leachate constituting the leach slurry. Among the above neutralizing agents, slaked lime is preferred because it can improve the filterability of the precipitate by producing gypsum. [Chemical formula 1] 4FeSO4+4Ca(OH)2+O2+2H2O→4Fe(OH)3+4CaSO4

[0016] In this iron removal step, if the pH of the liquid phase during the oxidation neutralization reaction is too low, iron hydroxide is not generated much, and iron remains in the aqueous solution of crude nickel sulfate. Conversely, if the pH of the liquid phase during the oxidation neutralization reaction is too high, nickel hydroxide, which is the target metal to be produced, is generated by the neutralization reaction shown in the following chemical formula 2, and the distribution rate of nickel to the aqueous solution of crude nickel sulfate decreases. Therefore, in this iron removal step, the pH of the liquid phase is preferably adjusted to 2.6 to 5.9, more preferably 4.0 to 5.5. This makes it possible to sufficiently remove iron, an impurity contained in the leachate, while suppressing a decrease in the distribution rate of nickel to the aqueous solution of crude nickel sulfate. [Chemical formula 2] NiSO4+Ca(OH)2 →Ni(OH)2+CaSO4

[0017] (4) First solid-liquid separation step In the first solid-liquid separation step, the deironized slurry obtained by subjecting the leaching slurry to an oxidation neutralization treatment in the previous deironization step is introduced into a solid-liquid separation means such as a filter press to perform solid-liquid separation. This separates and removes the primary deironized precipitate consisting of a mixture of the leaching residue and the neutralized precipitate, thereby obtaining a crude nickel sulfate aqueous solution.

[0018] (5) Solvent extraction process In the solvent extraction step, the crude nickel sulfate aqueous solution obtained by separating and removing the solids in the first solid-liquid separation step in the previous step is subjected to a solvent extraction treatment to remove impurities such as cobalt. This results in a high-purity nickel sulfate aqueous solution. There is no particular limitation on the organic solvent used in this solvent extraction, but it is preferable to use an organic phosphoric acid-based acidic organic extractant such as PC-88A manufactured by Daihachi Chemical Industry Co., Ltd.

[0019] (6) Crystallization process In the crystallization step, nickel sulfate crystals are produced by crystallizing the high-purity nickel sulfate aqueous solution obtained in the previous solvent extraction step. There is no particular limitation on the method of crystallization, and for example, a method in which the high-purity nickel sulfate aqueous solution is introduced into a crystallization tank and heated under reduced pressure to evaporate water and crystallize nickel sulfate can be preferably adopted. Note that when nickel sulfate is used to manufacture a positive electrode material for a secondary battery, the high-purity nickel sulfate aqueous solution can be used as it is without going through this crystallization step.

[0020] (7) Melting process Since the neutralized precipitate produced in the above-mentioned deironization step contains coprecipitated nickel hydroxide, the deironized primary precipitate as the solid content separated in the above-mentioned first solid-liquid separation step contains this nickel hydroxide. Therefore, in the dissolution step, the deironized primary precipitate separated in the first solid-liquid separation step is repulped by adding an aqueous sulfuric acid solution to dissolve the nickel hydroxide contained in the deironized primary precipitate. This makes it possible to recover the nickel contained in the neutralized precipitate. In this dissolution step, the pH of the liquid phase obtained when the deironized primary precipitate is repulped by adding an aqueous sulfuric acid solution to the deironized primary precipitate is adjusted to within the range of 2.3 to 3.0. If the pH of this liquid phase is higher than 3.0, the recovery of nickel becomes insufficient, and conversely, if the pH of this liquid phase is lower than 2.3, the iron hydroxide is also dissolved and the particles constituting the neutralized precipitate become small in diameter, resulting in poor solid-liquid separability.

[0021] (8) Second solid-liquid separation step In the second solid-liquid separation step, the deironized secondary precipitate slurry, which is mainly composed of leaching residue and iron hydroxide obtained after the treatment in the previous dissolution step, is introduced into a solid-liquid separation means such as a filter press, and the deironized secondary precipitate is subjected to solid-liquid separation to obtain a nickel recovery solution. The deironized secondary precipitate obtained by solid-liquid separation is discharged out of the system, while the nickel recovery solution is used as repulping water or washing water in each step in the nickel sulfate production process system, and is preferably used repeatedly as an aqueous solution for preparing a raw material slurry in the above-mentioned raw material preparation step.

[0022] 2. Solid-liquid separability in solid-liquid separation process As described above, in the first solid-liquid separation step and the second solid-liquid separation step, the slurry containing the neutralized precipitate mainly composed of iron hydroxide produced in the iron removal step and the leaching residue produced in the pressure oxidative leaching step is subjected to solid-liquid separation, preferably using a filter such as a filter press, to separate and remove the solids. When performing solid-liquid separation of the slurry using a filter such as a filter press, an operation of forming a cake layer on the surface of the filter cloth using a filter aid such as diatomaceous earth or perlite may be performed.

[0023] Specifically, there is a precoat method in which a clear liquid with a filter aid dispersed therein is introduced into the filter before the slurry to be filtered is introduced into the filter, thereby forming a layer of the filter aid on the surface of the filter cloth in advance, and a body feed method in which the slurry to be filtered is introduced into the filter in a state in which the filter aid is dispersed, thereby forming a cake layer consisting of the filter aid and the solid content to be filtered on the surface of the filter cloth.

[0024] By adopting the above-mentioned precoating method and / or body feed method, it is possible to reduce the filtration resistance, suppress clogging of the filter medium, and increase the clarity of the filtrate. On the other hand, in the manufacturing method of nickel sulfate according to the embodiment of the present invention, the solid content contained in the slurry to be filtered contains not only the neutralized precipitate made of iron hydroxide as described above, but also the leaching residue, so it is presumed that the filterability is improved. While the neutralized precipitate made of iron hydroxide generally has a three-dimensional mesh-like entangled form, the leaching residue is the remaining part of the mixture of NiS and CoS, and is therefore presumed to be fine particles having a porous form. For this reason, it is also considered that the leaching residue plays the role of a filter aid similar to diatomaceous earth and perlite made of porous materials.

[0025] If the oxidation reaction is promoted in the pressure oxidative leaching process, in addition to the leaching reaction of metals, the leached iron is more likely to be oxidized to trivalent iron, resulting in the hydrolysis reaction shown in chemical formula 3 below, which increases the amount of hematite (Fe2O3) produced. Since the hematite produced under high temperature and pressure in the pressure oxidative leaching process is generally finer than the iron hydroxide produced at about 50°C in the deferronization process, if the oxidation reaction is promoted in the pressure oxidative leaching process, the proportion of hematite in the deferronization primary sediment becomes relatively high, which may deteriorate the filterability in the first solid-liquid separation process and the second solid-liquid separation process. [Chemical formula 3] 2Fe 3+ +3H2O→Fe2O3+6H +

[0026] Therefore, in the pressure oxidation leaching step, it is preferable to keep the redox potential relatively low. Specifically, it is preferable to adjust the redox potential of the liquid phase (based on a silver / silver chloride electrode) in the pressure oxidation leaching step to 500 mV or less. This makes it possible to prevent the oxidation reaction in the pressure oxidation leaching step from proceeding excessively, thereby suppressing excessive precipitation of hematite. If the redox potential in the pressure oxidation leaching step is too low, the leaching reaction of the metal becomes insufficient. Therefore, it is preferable to adjust the redox potential of the liquid phase (based on a silver / silver chloride electrode) in the pressure oxidation leaching step to 410 mV or more, and to prevent the precipitation of thiosulfate ions (SO3 2- From the viewpoint of suppressing the generation of .alpha.-Hexazoline, it is more preferable to adjust the voltage to a value exceeding 480 mV. EXAMPLES

[0027] A high-purity nickel sulfate aqueous solution was produced from the raw material nickel-cobalt mixed sulfide (MS) using a production facility as shown in Figure 3. Specifically, a raw material slurry prepared by adding water to MS was charged into the most upstream reaction chamber 3a of an autoclave, which has a structure in which a cylindrical pressure vessel 1 as shown in Figure 2 is laid horizontally and the inside is divided into five reaction chambers 3a to 3e by four partition walls 2 with an open top, via a raw material slurry supply pipe 6, and the slurry was transferred to the downstream reaction chambers in sequence by overflowing the upper end of the partition wall 2, while stirring with a stirrer 4 in each reaction chamber and blowing in high-pressure air through a gas blowing pipe 5, thereby performing a pressurized oxidation leaching treatment under high temperature and high pressure of a pressure of 1.8 to 1.9 MPaG and a temperature of 140 to 180°C to produce a leaching slurry consisting of a leachate and a leach residue (pressurized oxidation leaching process).

[0028] The leaching slurry produced in the autoclave was extracted through an extraction pipe 7 installed in the reaction chamber 3e and reduced in pressure to approximately atmospheric pressure in a flash tank 8, after which it was charged via a first relay tank 9A into a deironization reaction tank 10, where air was blown in as an oxidizing agent and slaked lime was added as a neutralizing agent. Although only one deironization reaction tank 10 is shown in Fig. 1, in reality the pH was raised stepwise using multiple consecutive reaction tanks. As a result, a neutralized precipitate was produced in the final reaction tank at a pH of 4.7 to 5.3 (deironization process).

[0029] The deironized slurry containing the neutralized precipitate produced in the deironization reaction tank 10 was transferred to the second relay tank 9B, and then introduced into the first filter press 12 via the first slurry pump 11 to separate the neutralized precipitate and the primary deironized precipitate consisting of the leaching residue, thereby obtaining a crude nickel sulfate aqueous solution (first solid-liquid separation step).The obtained crude nickel sulfate aqueous solution was introduced into the mixer settler 13 and subjected to a solvent extraction treatment to obtain a high-purity nickel sulfate aqueous solution (solvent extraction step).

[0030] On the other hand, the deironized primary precipitate was recovered in a repulping tank 14, and then an aqueous sulfuric acid solution was added thereto for repulping, and steam was blown in to heat the precipitate to approximately 60°C to dissolve the insoluble nickel contained in the neutralized precipitate (dissolving step). The resulting deironized secondary precipitate slurry was introduced into a second filter press 16 via a second slurry pump 15, and the deironized secondary precipitate, which mainly consisted of leaching residue and iron hydroxide, was separated to obtain a nickel recovery solution (second solid-liquid separation step).

[0031] In the above dissolution step, the pH of the liquid phase was changed in various ways when repulping with an aqueous sulfuric acid solution. The amounts of iron and insoluble nickel dissolved from the deironization primary sediment when the pH of the liquid phase was changed were analyzed by fluorescent X-ray analysis, and the ratio of insoluble nickel to iron (insoluble Ni / Fe dissolved amount ratio) was obtained. The results are plotted in a graph shown in FIG. 4, with the horizontal axis representing the pH of the liquid phase. From the graph in FIG. 4, it can be seen that the lower the pH of the liquid phase is in the range of about 2.1 to 3.2, the higher the insoluble Ni / Fe dissolved amount ratio is, and therefore, more insoluble nickel can be recovered. More specifically, the ratio of insoluble nickel to iron (insoluble Ni / Fe dissolved amount ratio) was calculated using the following formula.

[0032] [Calculation formula] Insoluble Ni / Fe solubility ratio = (Insoluble nickel content (wt%) of the deironized primary sediment / Iron content (wt%) of the deironized primary sediment) - (Insoluble nickel content (wt%) of the deironized secondary sediment / Iron content (wt%) of the deironized secondary sediment)

[0033] The insoluble nickel content was calculated by subtracting the water-soluble nickel content from the total nickel content. The water-soluble nickel content was calculated by boiling 1 g of the sample in 100 mL of water for 30 minutes, filtering the sample, measuring the nickel concentration of the filtrate by ICP emission spectrometry, multiplying the nickel concentration by the volume of the liquid to calculate the weight of water-soluble nickel, and converting it into the water-soluble nickel content.

[0034] On the other hand, when the pH of the liquid phase was changed as described above, the time required for filtration in the second filter press was measured, and the Fe concentration of the nickel recovery liquid (Fe-free secondary filtrate) obtained by this filtration was analyzed by X-ray fluorescence analysis. The results are plotted on a graph in FIG. 5, with the pH of the liquid phase on the horizontal axis. From the graph in FIG. 5, it can be seen that when the pH decreases, iron dissolves along with insoluble nickel. It can also be seen that the time required for filtration in the second filter press becomes critically long at pH levels below 2.3, with the boundary being pH 2.3. This is thought to be due to the fact that the particle size of the undissolved precipitate becomes smaller due to the dissolution of iron, and the filterability in the second filter press decreases. From the results of FIG. 4 and FIG. 5, it can be seen that when the iron-free primary precipitate is repulped with an aqueous sulfuric acid solution in the dissolution process, the pH of the liquid phase is preferably set to 2.3 or higher. [Explanation of symbols]

[0035] 1. Pressure vessels 2 Bulkhead 3a, 3b, 3c, 3d, 3e reaction chamber 4 Mixer 5 Gas discharge tube 6 Raw slurry supply piping 7 Extraction tube 8. Flash Tank 9A 1st relay tank 9B Second relay tank 10 Iron removal reaction tank 11 No. 1 slurry pump 12 First filter press 13 Mixer Settler 14 Repulping tank 15 No. 2 slurry pump 16 Second filter press

Claims

1. The present invention relates to a method for producing an aqueous nickel sulfate solution, the method comprising the steps of: a pressurized oxidation leaching step of charging a raw material slurry containing nickel sulfide into an autoclave and subjecting it to an oxidation leaching treatment under high temperature and high pressure to produce a leachate consisting of an aqueous nickel sulfate solution; a de-ironizing step of subjecting a leach slurry consisting of the leachate and a leach residue to an oxidation neutralization treatment to produce a neutralized precipitate containing iron hydroxide; a first solid-liquid separation step of subjecting the de-ironizing slurry obtained in the de-ironizing step to solid-liquid separation to remove the neutralized precipitate and a de-ironizing primary precipitate consisting of the leach residue to obtain an aqueous crude nickel sulfate solution; and a dissolution step of adding sulfuric acid to the de-ironizing primary precipitate to dissolve the nickel hydroxide contained in the neutralized precipitate, the dissolution step being characterized in that the pH of the liquid phase is adjusted to a range of 2.3 to 3.

0.

2. 2. The method for producing a nickel sulfate aqueous solution according to claim 1, wherein the pressure leaching step comprises blowing high-pressure air into the raw material slurry to perform the oxidative leaching treatment under conditions of a pressure of 1 to 2 MPaG and a temperature of 140 to 200° C.

3. 2. The method for producing an aqueous nickel sulfate solution according to claim 1, wherein the iron removal step comprises blowing air into the leached slurry to perform an oxidation treatment and adding a neutralizing agent to perform a neutralizing treatment.

4. 2. The method for producing an aqueous nickel sulfate solution according to claim 1, wherein the pH of the liquid phase in the iron removal step is adjusted to a range of 2.6 to 5.

9.

5. 5. The method for producing an aqueous nickel sulfate solution according to claim 1, wherein the nickel sulfide is a mixed sulfide containing nickel and cobalt produced by a hydrometallurgical process using nickel oxide ore as a raw material.

Citation Information

Patent Citations

  • Method for leaching nickel from iron removal precipitate

    JP2006283163A

  • Method for recovering nickel

    JP2013253273A

  • Method for producing crude nickel sulfate solution

    JP2018150183A

  • Pressure oxidation leaching method and method for producing nickel sulfate

    JP2019178013A

  • Manufacturing method of nickel sulfide, and wet smelting method of nickel oxide ore

    JP2020193386A

Cited By

  • Eliminator unit, scrubber device equipped therewith, and exhaust gas treatment method using the scrubber device.

    JP2026144638A