Enhanced ultra-thin and ultra-low density films for EUV lithography and methods for manufacturing same
Carbon nanotube-based pellicle films with plasma treatment address the challenges of high EUV transmission and mechanical strength, enabling effective EUV lithography by achieving over 92% transmission and temperature resistance up to 600°C.
Patent Information
- Application Number
- JP2024516720
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2021-09-28
- Filing Date
- 2022-09-27
- Publication Date
- 2024-10-02
AI Technical Summary
Existing EUV pellicle films face challenges in achieving high EUV transmission, mechanical strength, and temperature tolerance, particularly for large sizes, making them unsuitable for advanced EUV lithography applications.
Development of carbon nanotube-based pellicle films with a specific interconnecting network structure and plasma treatment to enhance mechanical properties and EUV transmission, using filtration-based methods to form uniform films.
The carbon nanotube films achieve EUV transmission exceeding 92%, are temperature-resistant up to 600°C, and exhibit enhanced mechanical strength, suitable for large-scale EUV lithography applications.
Smart Images

Figure 2024535841000001_ABST
Abstract
Description
[Technical field]
[0001] CROSS-REFERENCE TO RELATED APPLICATIONS This application claims priority to U.S. Provisional Patent Application No. 63 / 249,113, filed September 28, 2021. The disclosures of each of these documents, including the specification, drawings, and claims, are hereby incorporated by reference in their entirety.
[0002] The present disclosure relates generally to thin films and thin film devices used in semiconductor microchip manufacturing, and more particularly to ultra-thin, ultra-low density, nanostructured, free-standing pellicle films with enhanced mechanical properties for extreme ultraviolet (EUV) lithography, and methods for making such pellicles and pellicle films. [Background technology]
[0003] A pellicle is a protective device. Pellicles cover photomasks and are used in semiconductor microchip manufacturing. Photomasks can refer to opaque plates with holes or transparencies that allow light to filter in a defined pattern. Such photomasks can be widely used in photolithography and the manufacture of integrated circuits. As a master template, photomasks are used to generate patterns on a substrate (usually a thin slice of silicon known as a wafer in semiconductor chip manufacturing).
[0004] In semiconductor manufacturing, particle contamination can be a significant problem. Photomasks are protected from particles by a pellicle, a thin transparent film that is stretched over a mounted frame over the patterned side of the photomask. The pellicle is close to the mask but far enough away that small to medium sized particles that land on the pellicle are too out of focus to print. In recent years, the microchip manufacturing industry has realized that pellicles can protect photomasks from damage resulting from sources other than particles and contaminants.
[0005] Extreme ultraviolet lithography is an advanced optical lithography technique that uses the EUV wavelength range (more specifically, 13.5 nm wavelength). It allows semiconductor microchip manufacturers to pattern the most delicate features at a resolution of 7 nm or less to place many more transistors without increasing the size of the space required. EUV photomasks work by reflecting light. The reflection of light is achieved by using multiple alternating layers of molybdenum and silicon. When the EUV light source is powered on, the EUV light first hits the pellicle film, passes through the pellicle film, then reflects back from underneath the photomask, hits the pellicle film once more, and continues on its path to print the microchip. Some of the energy is absorbed during this process, which can result in heat being generated, absorbed, and stored. The temperature of the pellicle can rise to 600-1000 degrees Celsius or higher.
[0006] While heat resistance is important, the pellicle must also be highly transparent to EUV light to ensure the passage of reflected light and the light pattern from the photomask.
[0007] In 2016, a polysilicon-based EUV pellicle was developed after decades of research and efforts, but the EUV transmittance was only 78% for a simulated relatively low-power 175 watt EUV source. The desire for increased transistor density poses further technical challenges for EUV pellicle developers, with stringent requirements for higher transmittance, lower transmittance variation, higher temperature tolerance, and strong mechanical strength.
[0008] Attempts have been made to target higher EUV transmittance (e.g., 90%, 95%, or even 98%) by introducing carbon nanotubes (CNTs) into the formation of pellicle films. However, in order to produce and utilize thin films with higher EUV transmittance in EUV lithography scanner chambers, further improvement in the mechanical strength of the film is required, since any pressure disturbance or mechanical vibration during product packaging, transportation, and scanner pump-down and venting may cause irreparable damage to the film. Thus, existing technologies are unable to manufacture and provide pellicle films with high EUV transmittance with sufficient mechanical strength for use in EUV lithography scanners.
[0009] Additionally, the demand for significantly larger film sizes for EUV scanners, e.g., full size pellicle films of 110 mm x 140 mm or more, poses further challenges regarding mechanical strength requirements while maintaining an ultra-thin, high EUV transmission state.
[0010] Therefore, in the prior art, the three factors of high transmittance of EUV light, ultra-thin pellicle film, and strong mechanical strength, which are characterized in one embodiment, are often contradictory in themselves, significantly inhibiting the development of EUV pellicles.
[0011] Existing methods for increasing membrane film strength are ineffective in producing such thin films. Summary of the Invention
[0012] According to an embodiment of the present disclosure, a uniquely structured nanotube film is disclosed, which comprises a plurality of carbon nanotubes randomly crossed to form an interconnected network structure in a planar orientation, the interconnected network structure having a thickness from a lower limit of at least 3 nm to an upper limit of up to 100 nm, and a minimum EUV transmittance of 92% or greater.
[0013] According to another aspect of the disclosure, in some embodiments, the thickness is between a lower limit of 3 nm and an upper limit of 40 nm.
[0014] According to another aspect of the disclosure, in some embodiments, the thickness is between a lower limit of 3 nm and an upper limit of 20 nm.
[0015] According to yet another aspect of the present disclosure, in some embodiments, the average thickness of the interconnect network structure is between 10.7 nm and 11.9 nm.
[0016] According to further aspects of the present disclosure, in some embodiments, the EUV transmittance reaches greater than 95%.
[0017] According to yet another aspect of the present disclosure, in some embodiments, the EUV transmittance reaches greater than 98%.
[0018] According to a further aspect of the present disclosure, the plurality of carbon nanofibers further comprises single-walled carbon nanotubes and multi-walled carbon nanotubes, where the single-walled carbon nanotubes have one wall, the double-walled carbon nanotubes have two walls, and the multi-walled carbon nanotubes have three or more walls.
[0019] According to another embodiment of the present disclosure, single-walled carbon nanotubes account for 20-40% of all carbon nanotubes, double-walled carbon nanotubes account for 50% or more of all carbon nanotubes, and the remaining carbon nanotubes are multi-walled carbon nanotubes.
[0020] According to a further aspect of the present disclosure, the nanotube film is further treated by a plasma treatment.
[0021] According to a further aspect of the present disclosure, the plasma treatment of the nanostructured film selects a gas from hydrogen or oxygen.
[0022] According to another aspect of the present disclosure, the pellicle is subjected to a plasma treatment.
[0023] According to another aspect of the present disclosure, plasma treatment of the pellicle applies an active gas selected from oxygen, hydrogen, or air.
[0024] According to another aspect of the present disclosure, the plasma treatment is mild, defined by treatment time interval, treatment power, and gas type.
[0025] According to a further embodiment of the present disclosure, the treatment time interval is 1 to 60 seconds, and a preferred treatment time interval is 5 to 20 seconds.
[0026] According to one embodiment of the present disclosure, the plasma treatment is performed by applying a power of 15 watts to 35 watts.
[0027] According to a further aspect of the present disclosure, the plasma processing power is between 15 Watts and 20 Watts.
[0028] According to one embodiment of the present disclosure, the plasma treatment of a small size 10 mm x 10 mm pellicle film may be in the range of 15 watts to 35 watts, and the treatment time interval does not exceed 50 seconds.
[0029] According to another aspect of the present disclosure, the plasma treatment of a small size 10 mm x 10 mm pellicle film may preferably be in the range of 15 watts to 20 watts, with the treatment time interval being 5 to 20 seconds.
[0030] According to one embodiment of the present disclosure, the plasma treatment applies a power of 15 to 25 watts to a full-size or larger pellicle film.
[0031] According to another aspect of the present disclosure, the plasma treatment applies a power of 22 watts or less for a full size or larger pellicle film.
[0032] According to another embodiment of the present disclosure, the plasma treatment applies a power of 10 to 20 watts to a full-size or larger ultra-thin pellicle film having a light transmittance of more than 89% at 550 nm.
[0033] According to another embodiment of the present disclosure, the plasma treatment applies 15 to 16 watts of power to a full-size or larger ultra-thin pellicle film with a 550 nm light transmittance of greater than 89%.
[0034] According to one aspect of the present disclosure, the plasma treatment time interval is 25 seconds or less for a full size pellicle film.
[0035] According to another aspect of the present disclosure, the plasma treatment time interval is 22 seconds or less for a full size pellicle film.
[0036] According to another further embodiment of the present disclosure, for a full size or larger ultra-thin pellicle film having a light transmittance of more than 89% at 550 nm, the plasma treatment time interval is 6 to 15 seconds.
[0037] According to yet another further aspect of the present disclosure, for a full-size or larger ultra-thin pellicle film having a light transmittance of more than 89% at 550 nm, the plasma treatment time interval is 6 to 15 seconds.
[0038] According to a further aspect of the present disclosure, for full size or larger ultra-thin pellicle films with optical transmittance at 550 nm of greater than 89%, the plasma treatment time interval is 6 seconds or 10 seconds.
[0039] The present disclosure will be further described in the following detailed description with reference to a number of drawings, which are mentioned as non-limiting examples of preferred embodiments of the present disclosure, in which like characters represent like elements throughout the several views of the drawings. [Brief description of the drawings]
[0040] [Figure 1] 1 shows a flow chart for fabricating a plasma treated nanotube pellicle film according to an illustrative embodiment. [Diagram 2]1 shows a scanning electron microscope (SEM) image of the microstructure of an untreated CNT film, according to an exemplary embodiment. [Diagram 3] 1 shows a time course study of average light transmittance versus plasma treatment, and the average percent change in light transmittance, measured at a wavelength of 550 nm, for oxygen plasma treated 10 mm×10 mm films, according to an exemplary embodiment. [Figure 4] 1 shows a time course study of average light transmittance versus plasma treatment and the average percent change in light transmittance measured at a wavelength of 550 nm for hydrogen treated 10 mm×10 mm films according to an exemplary embodiment. [Diagram 5] 1 shows a time course study of plasma treatment versus film deflection measured at a constant 2 Pascal pressure for an oxygen plasma treated 10 mm×10 mm film according to an exemplary embodiment. [Figure 6] 1 shows a time course study of plasma treatment versus film deflection measured at a constant 2 Pascal pressure for a hydrogen plasma treated 10 mm×10 mm film according to an exemplary embodiment. [Figure 7] 1 shows a time course study of plasma treatment versus measured film rupture pressure for oxygen plasma treated films according to an exemplary embodiment. [Figure 8] 13 illustrates a plasma treatment vs. measured film rupture pressure over time study for hydrogen plasma treated samples, according to an example embodiment. [Figure 9] 1 shows a time course study of plasma treatment versus film rupture flow rate for an oxygen plasma treated nanotube film, according to an example embodiment. [Figure 10] 1 shows a time course study of plasma treatment versus film rupture flow rate for a hydrogen plasma treated nanotube film, according to an example embodiment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0041] Through one or more of its various aspects, the embodiments and / or specific features, subcomponents, or processes of the present disclosure are intended to demonstrate one or more of the advantages specifically discussed above and below.
[0042] A pellicle may refer to a thin transparent film that protects a photomask during semiconductor microchip fabrication. A pellicle contemplates a protection device having a boundary frame and a central opening. Both the boundary and the opening are covered by a continuous thin film over at least a portion of the boundary and over the entire opening. The central portion of such thin film over the opening is freestanding. A pellicle may act as a dust cover to prevent particles and contaminants from falling onto the photomask during fabrication. However, the pellicle must be transparent enough to allow EUV light to pass through for lithography. A higher level of light transmission is required for more effective lithography.
[0043] Furthermore, pellicles for EUV lithography require large (e.g., greater than 110×140 mm) free-standing thin-film materials with extreme and unique properties. A full-size EUV pellicle can refer to a pellicle device having a free-standing film that covers an aperture of 110 mm×140 mm or larger.
[0044] In addition to being highly transparent to EUV radiation, the pellicle must be resistant to temperatures in excess of 600°C, be mechanically robust, and withstand handling, transportation, pumping down, and venting operations during the photolithography process. It is also desirable to have gas permeability, yet the ability to retain micrometer-sized particles. Given the number of high-level properties required, effective EUV pellicles have traditionally been difficult to manufacture.
[0045] In this aspect, carbon nanotubes are proposed as a possible starting material for forming pellicles for this EUV pellicle application due to their excellent thermal and mechanical properties and ability to form porous films.
[0046] Carbon nanotubes and carbon nanotube films Carbon nanotubes (CNTs) typically come in several different varieties, including, but not limited to, single-walled CNTs (SWCNTs), double-walled CNTs (DWCNTs), multi-walled CNTs (MWCNTs), and coaxial nanotubes. They may exist substantially purely of one variety, or often in combination with other varieties. Individual CNTs may intersect with several others. Collectively, many CNTs can form a mesh-like, free-standing microstructured thin film. As the names suggest, SWCNTs have one or a single wall, DWCNTs have two walls, and MWCNTs have three or more walls.
[0047] Furthermore, among several possible methods of producing free-standing films, a filtration-based approach was utilized to produce films ranging from small size films to films large and uniform enough for EUV lithography, or even larger than a full-sized pellicle. This filtration-based method allows for the rapid production of films of CNTs as well as other high aspect ratio nanoparticles and nanofibers, such as boron nitride nanotubes (BNNTs) or silver nanowires (AgNWs). Because this approach separates the nanoparticle synthesis method from the film production method, different kinds of nanotubes made by virtually any method may be used. Different types of nanotubes can be mixed in any desired ratio, such as a mixture of two or more CNTS selected from SWCNTs, DWCNTs, and MWCNTs. Filtration is a self-leveling process in the sense that non-uniformities in film thickness during the filtration process are self-corrected by local permeability variations, and is therefore a highly desirable film formation process and a promising candidate for the production of highly uniform films.
[0048] After film formation, the pellicle film on the pellicle boundary or transport frame is plasma treated with a selected gas and plasma treatment time interval to enhance the film's mechanical properties, reduce film deflection, and increase the film break pressure and flow rate when the film breaks.
[0049] Plasma treatment is widely used to clean, activate, etch, and coat material surfaces in various technical fields for various purposes. Different purposes include promoting surface adhesion, wettability, and hydrophilicity. Low power plasma treatments, such as 100 watts for 10 seconds, on stacks of polyvinyl alcohol densified 100-layer CNT sheets drawn from CNT forests showed improvements in d Young's modulus and tensile strength when tested with a Surfx Atomflo™ 400 plasma system, while treatments at higher powers, such as 140 watts for 30 seconds, actually reduced the Young's modulus and tensile strength of the sheets.
[0050] FIG. 1 shows a flow chart for fabricating a plasma treated nanotube pellicle film according to an example embodiment.
[0051] As illustrated in Figure 1, a free-standing carbon nanotube-based pellicle film may be created by a filtration-based method. In operation 101, a catalyst is removed from carbon nanotubes (CNTs) to be used to form an aqueous suspension. In an example, prior to dispersion in the suspension, the CNTs may be chemically purified to reduce the concentration of catalyst particles to less than 1 wt%, or preferably less than 0.5 wt%, as measured by thermogravimetric analysis. Catalyst removal is not limited to any particular process or procedure, and any suitable process may be used to achieve the desired results.
[0052] In operation 102, an aqueous suspension is prepared using the purified CNTs such that the purified CNTs are uniformly dispersed in water. When preparing one or more CNT suspensions, the carbon nanotube material can be mixed with a selected solvent to uniformly disperse the nanotubes in the final solution as a suspension. Mixing can include mechanical mixing (e.g., using a magnetic stir bar and stir plate), ultrasonic mixing (e.g., using an immersion ultrasonic probe), or other methods. In some examples, the solvent can be a protic or aprotic polar solvent, such as water, isopropyl alcohol (IPA), and aqueous alcohol mixtures, such as 60, 70, 80, 90, 95% IPA, N-methyl-2-pyrrolidone (NMP), dimethyl sulfide (DMS), and combinations thereof. In examples, a surfactant can also be included to aid in the uniform dispersion of the carbon nanofibers in the solvent. Examples of surfactants include, but are not limited to, anionic surfactants.
[0053] Carbon nanofiber films are typically formed from one of MWCNTs, DWCNTs, or SWCNTs. Carbon nanofiber films may also include mixtures of two or more types of CNTs (i.e., SWCNTs, DWCNTs, and / or MWCNTs) with varying ratios between the different types of CNTs.
[0054] Each of these three different types of carbon nanotubes (MWCNT, DWCNT, and SWCNT) has different properties. In one example, single-wall carbon nanotubes can be more conveniently dispersed in water or water containing a solvent (i.e., most of the nanotubes are suspended separately and are not adsorbed onto other nanotubes) for subsequent formation into sheets of randomly oriented carbon nanotubes. This ability to uniformly disperse individual nanotubes in water or water containing a solvent can result in the production of more planarly uniform nanotube films that are formed by removing the water and solvent from the nanofiber suspension. This physical uniformity can also improve the uniformity of properties across the film (e.g., uniform radiation penetration into the film).
[0055] As used herein, the term "nanofiber" refers to a fiber having a diameter of less than 1 μm. As used herein, the terms "nanofiber" and "nanotube" are used interchangeably and both include single-walled carbon nanotubes, double-walled carbon nanotubes, and / or multi-walled carbon nanotubes (where the carbon atoms are linked together to form a cylindrical structure).
[0056] In an example, the aqueous CNT suspension initially formed in operation 102 may have a purity of at least greater than 85% SWCNT. The remainder may be a mixture of DWCNT, MWCNT, and / or catalyst. In other examples, dispersed CNT suspensions may be prepared with different ratios of different types of CNT, such as about 20% / 75% DWCNT / SWCNT, about 50% / 45% DWCNT / SWCNT, about 70% / 20% DWCNT / SWCNT (with the remainder being MWCNT). In an example, an anionic surfactant may be used as a catalyst in the suspension.
[0057] In operation 103, the CNT suspension is then further refined to remove any aggregated or stuck CNTs from the initial mixture. In an example, different morphologies of CNTs (undispersed or aggregated vs. well-dispersed) may be separated from the suspension by centrifugation. Centrifugation of the surfactant-suspended carbon nanotubes before proceeding to the next filtration step may help reduce the turbidity of the suspension solution to ensure full dispersion of the carbon nanotubes within the final suspension solution. However, aspects of the present disclosure are not limited in this respect and other separation methods or processes may be used.
[0058] In operation 104, the CNT supernatant from operation 103 is then filtered through a filtration membrane to form a CNT web (a continuous sheet of film of intersecting CNTs).
[0059] In an example, one approach to making a CNT film is to deposit nanotubes in a random pattern on a filter using water or other fluid. A homogeneously dispersed CNT-containing mixture is passed or forced through the filter, leaving the nanotubes on the surface of the filter to form a nanotube structure or film. The size and shape of the resulting film is determined by the size and shape of the desired filtering area of the filter, while the thickness and density of the film are determined by the quantity of nanotube material used in the process and the permeability of the filtering membrane to the components of the input CNT material, since the impermeable components are trapped on the surface of the filter. If the concentration of nanotubes dispersed in the fluid is known, the mass of nanotubes deposited on the filter can be determined from the amount of fluid passing through the filter, and the average areal density of the film can be determined by dividing the nanotube mass by the total filtering area. The filter selected is usually not permeable to any CNTs.
[0060] The filter-formed CNT films can be combinations of SWCNTs, DWCNTs, and / or MWCNTs in different compositions.
[0061] The CNT film is then removed from the filtration membrane in operation 105. More specifically, the carbon nanofibers may be randomly crossed to form an interconnected network structure in a planar orientation to form a thin CNT film.
[0062] In operation 106, the lifted CNT film is then collected using a collector frame and transferred and mounted directly onto virtually any solid substrate (e.g., the pellicle boundary with the aperture defined). The CNT film is attached to the pellicle boundary and covers the aperture to form a pellicle. Mounting the transferred film onto a metal frame or silicon frame with an aperture as small as 1×1 cm may be useful. For practical EUV scanners, there is a high demand for much larger sized films. In FIG. 2, a scanning electron microscope (SEM) image of a CNT film prepared according to FIG. 1 according to an exemplary embodiment is shown. A full-sized pellicle for EUV lithography scanning may require an ultra-thin free-standing film with a size of typically 110×140 mm or larger based on current industry standards.
[0063] In operation 107, the CNT film is further treated by plasma. In the plasma treatment, a selected active gas or gas precursor is used with a predetermined treatment power and treatment time interval. Many gases can be considered and applied to generate the plasma. The plasma treatment power and treatment time interval vary depending on the actual application. After operation 107 is completed, in operation 108, the method for manufacturing the plasma treated nanotube pellicle film is completed.
[0064] Characterization of the CNT film with or without plasma treatment (eg, its mechanical strength, strain testing, permeability testing, strain at constant pressure or during pumping down conditions) may be performed.
[0065] Exemplary embodiments of the present disclosure provide filtered CNT pellicle films having structures distinct from known prior art that exhibit properties that meet or exceed certain aspects of EUV lithography requirements, including, without limitation, EUV transmission (EUVT), EUVT uniformity, low distortion, and mechanical strength (under pressure changes).
[0066] The exemplary structure of the pellicle film results in an extremely thin pellicle film that allows for very high EUVT (e.g., greater than 92%, 95%, or even 98%) while being extremely temperature resistant (e.g., resistant to temperatures in excess of 600° C.) and mechanically robust. In an example, the minimum EUVT can be 92% or greater.
[0067] Although the above disclosure has been shown with respect to CNTs and aqueous solutions, aspects of the present disclosure are not so limited and different nanotubes (eg, boron nitride nanotubes (BNNTs)) may be used according to the same principles.
[0068] The aforementioned thin films may be conformally coated by various methods, such as, but not limited to, e-beam, chemical vapor deposition, atomic layer deposition, spin coating, dip coating, spray coating, sputtering, DC sputtering, and RF sputtering. The material may be a metallic element including any one of the following: silicon, SiO2, SiON, boron, ruthenium, boron, zirconium, niobium, molybdenum, rubidium, yttrium, YN, Y2O3, strontium, and / or rhodium. The material may be any one of a metal, a metal oxide, or a nitride. However, aspects of the present disclosure are not limited thereto and a combination of materials may be used in the coating.
[0069] Plasma treatment Plasma treatment is a known technique used in various scientific and technological fields as well as manufacturing processes. It is generally used with various combinations of active gases, gas precursors, gas mixtures, treatment energies, and treatment time intervals to clean, activate, modify hydrophilicity, etch, or prepare surfaces for subsequent attachment of other materials. Plasma treatment with one or more inappropriate parameters, under optimal or suboptimal conditions, can produce unsatisfactory results on the target surface or cause irreversible damage to the target or target surface, including destruction of the target or target surface. Effective treatments can also be specified or specifically tailored for any surface.
[0070] In an exemplary embodiment of the present disclosure, the pellicle is placed in a 25 cm x 25 cm enclosure or chamber. The chamber is then closed and purged with oxygen, hydrogen, nitrogen gas, or air at a low rate of 25 sccm (standard cubic centimeters per second) due to the high pressure and high sensitivity of the ultra-thin nanotube film to gas flow. In one example, the plasma treatment can be performed in a low pressure environment, such as 0.2-0.3 Pascal, and the treatment temperature can be room or ambient temperature. Further, radio frequency power in the range of 1-100 watts is applied for 1-600 seconds. The chamber can then be slowly vented for 5 minutes to overnight to remove the sample.
[0071] Multiple samples were prepared for each test group and multiple measurements were made on the same samples.
[0072] Thin Film Thickness Exemplary embodiments of the present disclosure are further analyzed for their thickness, which is important to determine and ensure high EUVT. More specifically, a Dimension Icon AFM instrument was first calibrated against a National Institute of Standards and Technology (NIST) traceable standard. CNT pellicle films with an area of approximately 90 μm×90 μm were selected for AFM 2D and 3D height imaging. Step height analysis was performed to measure the film thickness. Three measurements were taken from three carbon nanotube film samples, with readings of 11.8 nm, 10.6 nm, and 11.4 nm, respectively. The average thickness of the test objects was approximately 11.3±0.6 nm (10.7 nm to 11.9 nm).
[0073] Furthermore, thickness values of 3 nm to 100 nm, 3 nm to 40 nm, and 3 nm to 20 nm were obtained based on additional sets of measurements.
[0074] Additionally, in other samples, the thickness values may be 3 nm to 100 nm, 3 nm to 40 nm, and 3 nm to 20 nm, but the embodiments of the present application are not limited thereto, and the range may be 3 nm to 5 nm at the lower end and 20 nm to 100 nm at the upper end.
[0075] Given the much higher mechanical strength exhibited by DWCNT-dominated CNT pellicle films, they can be constructed extremely thin to enable higher EUVT values without sacrificing mechanical strength or integrity for use in EUV scanners.
[0076] Visible and EUV transmittance The EUV transmittance of the samples was measured using the current industry standard 13.5 nm wavelength. EUVT maps were generated based on the EUV scanning results to demonstrate and measure the variation and / or uniformity of the transmittance.
[0077] The filtered CNT pellicle films generally showed high EUV transmission of >92%, and in some cases >95% or even >98%. For example, a scan across a full-sized pellicle film sample (approximately 110 mm x 144 mm) showed an average transmission of 96.69 ± 0.15%, while a scan of the 1.5 mm x 1.5 mm central area yielded an average transmission of 96.75 ± 0.03%.
[0078] Plasma treated pellicle films (film size: 10 mm x 10 mm) are measured for light transmittance at 550 nm and compared to the untreated negative control. Both oxygen treated and hydrogen treated films have improved transmittance. As shown in Figures 3 and 4, the improvement ranges from about 0.8% up to about 3%. The improvement correlates well with the treatment time, which ranges from 5 seconds to 60 seconds (see, e.g., Figures 3 and 4).
[0079] The visible light transmittance and EUV transmittance of post-plasma treated pellicle films with sizes of 110 cm x 140 mm or larger can be measured by the same method. The full size pellicle film treated with 15 watts oxygen plasma shows a 1.4% and 1.7% improvement in visible light transmittance at 6 second and 8 second treatment time intervals, respectively.
[0080] Mechanical properties of CNT pellicles for EUV lithography Exemplary embodiments of the present application provide a CNT pellicle with sufficient and satisfactory mechanical strength for product transportation and handling, and the pellicle can withstand any desired pressure changes surrounding its application environment (e.g., without limitation, an EUV lithography scanner environment).
[0081] A commonly applied mechanical characterization has been the bulge test, which measures the deflection of a film against flow pressure. For example, a film for testing can be mounted on the flat surface of the interface (pellicle film mounted on pellicle interface), and a baseline of the film can be established without any air or gas flow impact on the film. An initial flow of gas, preferably an inert gas, can then be applied at a low, steady pressure, directed perpendicularly to the central region of the film to create a localized surface bulge. The gas pressure continues to increase gradually to further deform the film until the pressure reaches a predetermined value (2 Pascals for 2 Pa strain test). This value can also be a flow rate of less than about 10 sccm, less than 3.5 mbar / sec, or any scanner pump-down or venting condition. The distance between the highest tip of the deformed film and its baseline can be measured. The results can be recorded as the strain at 2 Pa. Strain tests can be performed at various pressures other than 2 Pa.
[0082] Increasing the applied gas flow pressure may eventually cause the film to rupture. This pressure may be recorded as the rupture pressure, and the deflection of the film just prior to rupture may be referred to as the rupture deflection. The gas flow rate at the time of film rupture may be obtained and may be referred to as the rupture flow rate. Additionally, the deflection of the thin film may be intentionally adjusted by methods such as, but not limited to, tension adjustment by physical or chemical means.
[0083] Plasma Surface Treatment and Enhanced Mechanical Properties One or more exemplary embodiments of the present disclosure are described in detail below and illustrated in FIGS.
[0084] 5-10 illustratively show the change in mechanical properties of a 10 mm×10 mm nanotube film after plasma treatment with either oxygen or hydrogen at various treatment times from 5 to 60 seconds using 20 watts of radio frequency (RF) power, according to an illustrative embodiment. According to an illustrative embodiment, the 10 mm×10 mm film shows reduced deflection when loaded at a constant flow of 2 Pa for short treatment time intervals. The 10 mm×10 mm film breaks at higher flow pressures and higher flow rates. Furthermore, both oxygen and hydrogen treatments of the 10 mm×10 mm film reduce the film deflection by more than 100% on average for a 10 second treatment, as shown in FIGS. 5 and 6, and increase the break pressure and break flow rate by more than 60% on average for a 5 second treatment, as shown in FIGS. 7-10. As illustratively shown, the benefit of plasma treatment in terms of break pressure decreases beyond a 30 second treatment time interval.
[0085] Studies with low and high RF power are summarized in Table 1 below. [Table 1]
[0086] A set of 10 mm x 10 mm nanotube films were subjected to a constant 8 second oxygen plasma treatment at various RF power levels. The 20 watt treatment results show a similar reduction in film deflection and an increase in the rupture pressure and light transmission measured at 550 nm when compared to previous studies of film density or percentage of transmittance at 550 nm. As illustrated in Table 1, higher power treatments of 25 watts and above showed a reduction in film deflection, but the films became more brittle with a dramatic reversal in the film rupture pressure. The films became very brittle and could not withstand the plasma treatment when treated with RF powers of 40 watts and above.
[0087] For a full-size ultra-thin pellicle film, the details of a series of plasma treatments using different active gases, different plasma powers, and different treatment time intervals are shown below and in Table 2. [Table 2]
[0088] Guided by the results of the 10 mm x 10 mm film study, full-size ultra-thin pellicles took two different routes for oxygen plasma treatment. From Table 2, they did not survive further reductions in plasma treatment power and treatment time interval. They were easily broken when subjected to 6 seconds of treatment under 18 or 20 watts of applied power. Oxygen plasma treatment for 10 seconds with 15 watts of power could not prevent the ultra-thin film from breaking before the completion of the treatment process. However, oxygen plasma treatment for 6 and 8 seconds with 15 watts of power kept the film intact and the optical transmittance at a wavelength of 550 nm increased by about 1.4% and 1.7%, respectively, while the deflection of the film decreased by about 20% and 23%, respectively.
[0089] When oxygen is replaced with air, the same treatment regime of 15 watts and 6 seconds has nearly the same results, as shown in Table 2.
[0090] A very mild hydrogen plasma treatment, as exemplarily outlined in row 8 of Table 2 provided above, did not significantly improve the deflection of the film, with the deflection decreasing by 3.3%.
[0091] Full-sized ultrathin pellicles were exposed to the same plasma treatment chamber using nitrogen as the active gas, and the optical transmittance at 550 nm increased, moving in the opposite direction of decreasing the EUVT when compared to untreated.
[0092] The illustrations of the embodiments described herein are intended to provide a general understanding of the various embodiments. The illustrations are not intended to serve as a complete description of all of the elements and features of the products and methods constituting the products or methods described herein. Many other embodiments may become apparent to those skilled in the art upon review of the present disclosure. Since other embodiments may be utilized and derived from the present disclosure, structural and logical substitutions and changes may be made without departing from the scope of the present disclosure. Furthermore, the illustrations are merely representative and may not be drawn to scale. Certain proportions within the illustrations may be exaggerated, while other proportions may be minimized. Thus, the present disclosure and figures should be considered illustrative rather than limiting.
[0093] One or more embodiments of the present disclosure may be referred to herein, individually and / or collectively, by the term "invention" merely for convenience and without any intention to spontaneously limit the scope of the present application to any particular invention or inventive concept. In addition, although specific embodiments have been illustrated and described herein, it will be understood that any subsequent arrangements designed to achieve the same or similar purpose may be substituted for the specific embodiment shown. The present disclosure is intended to cover any and all subsequent adaptations or variations of the various embodiments. Combinations of the foregoing embodiments, as well as other embodiments not specifically described herein, will be apparent to one of ordinary skill in the art upon review of this description.
[0094] The Abstract of the Disclosure is submitted with the understanding that it will not be used to interpret or limit the scope or meaning of the claims. In addition, the foregoing Detailed Description may group or describe various features together in a single embodiment for the purpose of streamlining the disclosure. This disclosure should not be interpreted as reflecting an intention that the claimed embodiments require more features than are expressly recited in each claim. Rather, as the following claims reflect, the inventive subject matter may be directed to less than all of the features of any of the disclosed embodiments. Thus, the following claims are incorporated into the Detailed Description, with each claim standing on its own as defining the separately claimed subject matter.
[0095] The foregoing disclosed subject matter should be considered as illustrative and not limiting, and the appended claims are intended to cover all such modifications, extensions, and other embodiments that fall within the true spirit and scope of the present disclosure. Accordingly, to the maximum extent permitted by law, the scope of the present disclosure should be determined by the broadest permissible interpretation of the following claims and their equivalents, and should not be limited or restricted by the foregoing detailed description.
Claims
1. 1. An extreme ultraviolet (EUV) photolithographic nanotube film, comprising: A plurality of nanotubes randomly crossed to form an interconnected network structure in a planar orientation, the interconnected network structure comprising: a) having a thickness of at least 3 nm and up to an upper limit of 100 nm and a minimum EUV transmission of 92%; b) the plurality of nanotubes being plasma treated using an active gas, a treatment power, and a treatment time interval; The EUV photolithographic nanotube film comprising:
2. 10. The EUV photolithographic nanotube film of claim 1, wherein said thickness ranges from said lower limit of 3 nm to said upper limit of 40 nm.
3. 10. The EUV photolithographic nanotube film of claim 1, wherein said thickness ranges from said lower limit of 3 nm to said upper limit of 20 nm.
4. 10. The EUV photolithographic nanotube film of claim 1, wherein the average thickness of the interconnected network structure is between 10.7 nm and 11.9 nm.
5. 10. The EUV photolithographic nanotube film of claim 1, wherein the EUV transmittance reaches 95% or more.
6. the plurality of nanotubes further comprising single-walled carbon nanotubes, double-walled carbon nanotubes, and multi-walled carbon nanotubes; 10. The EUV photolithographic nanotube film of claim 1, wherein the number of walls of the single-walled carbon nanotube is 1, the number of walls of the double-walled carbon nanotube is 2, and the number of walls of the multi-walled carbon nanotube is 3 or more.
7. 7. The EUV photolithographic nanotube film of claim 6, wherein the single-walled carbon nanotubes account for 20-40% of all nanotubes, the double-walled carbon nanotubes account for 50% or more of all nanotubes, and the remaining nanotubes are multi-walled carbon nanotubes.
8. 10. The EUV photolithographic nanotube film of claim 1, wherein the film has a free-standing portion with an area size of 10 mm x 10 mm or greater.
9. 10. The EUV photolithographic nanotube film of claim 1, wherein the film has a free-standing portion with an area size of 110 mm x 140 mm or greater.
10. A method for improving extreme ultraviolet (EUV) photolithographic nanotube films, comprising: Obtaining a film having a plurality of carbon nanotubes randomly crossed to form an interconnected network structure in a planar orientation, the interconnected network structure having a thickness of at least 3 nm to a maximum of 100 nm and a minimum EUV transmittance of 88%, attached to a boundary having an aperture and covering the entire aperture of the boundary; subjecting the film to a plasma treatment using an active gas, a treatment power of 35 watts or less, and a treatment time interval of 30 seconds or less; The method comprising:
11. The method of claim 10, wherein the film has a thickness from the lower limit of 3 nm to the upper limit of 40 nm.
12. The method of claim 10, wherein the film has a thickness from the lower limit of 10 nm to the upper limit of 20 nm.
13. The method of claim 10, wherein the average thickness of the film is between 10.7 nm and 11.9 nm.
14. The method of claim 10, wherein the active gas is oxygen, hydrogen, or atmospheric air.
15. The method of claim 10, wherein the nanotube film has a free-standing portion with a side area of at least 10 mm by 10 mm.
16. 10. The EUV photolithographic nanotube film of claim 1, wherein the plasma treatment power does not exceed 35 Watts for a treatment time interval of 30 seconds or less.
17. The method of claim 10 , wherein the nanotube film has a free-standing portion with an area size of at least 110 mm by 140 mm.
18. 20. The method of claim 17, wherein the plasma treatment power does not exceed 18 Watts for the treatment time interval of 10 seconds or less.
19. 20. The method of claim 17, wherein the plasma treatment power does not exceed 16 Watts for the treatment time interval of 10 seconds or less.
20. 18. The method of claim 17, wherein the active gas is oxygen gas, the treatment power is 15 watts, and the treatment time interval is 8 seconds or less.
21. The nanotubes further include single-walled carbon nanotubes, double-walled carbon nanotubes, and multi-walled carbon nanotubes; 11. The method of claim 10, wherein each of said single-walled carbon nanotubes has one wall, each of said double-walled carbon nanotubes has two walls, and each of said multi-walled carbon nanotubes has three or more walls.
22. 22. The method of claim 21, wherein the single-walled carbon nanotubes comprise 20-40% of all carbon nanotubes, the double-walled carbon nanotubes comprise 50% or more of all carbon nanotubes, and the remaining carbon nanotubes are multi-walled carbon nanotubes.
Citation Information
Patent Citations
Metallic wire or capillary equipped with carbon nanotube and method of depositing carbon nanotube
JP2005035841A
Carbon nanotube aggregate and production method for the same
JP2015017029A
Method for forming pellicle
JP2018194838A
Method for forming EUVL pellicle
JP2021107916A
Robust, high transmission pellicle for extreme ultraviolet lithography systems
US20210132490A1