Compositions and methods for extracting metals using non-aqueous solvents

A two-step method using specific DES and oxidizing agents effectively addresses the challenges of metal extraction from electronic waste by selectively dissolving metals, including gold, with reduced environmental impact and improved recovery rates.

JP2024536092APending Publication Date: 2024-10-04アルゴ ナチュラル リソーシーズ リミテッド
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
JP2024518786
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2021-09-27
Filing Date
2022-09-26
Publication Date
2024-10-04

AI Technical Summary

Technical Problem

Existing methods for extracting metals from solid materials, particularly electronic waste, face challenges such as high cost, low selectivity, and sensitivity to water, using DES with iodine as an oxidizing agent, which oxidizes a wide range of metals including gold, making recovery complicated.

Method used

A two-step process using different DES and oxidizing agents, where a first oxidizing agent with a reduction potential ≤ +0.50V (e.g., Fe(III) salt) is used to dissolve most metals, followed by a second oxidizing agent with a higher potential (e.g., iodine) to target gold, minimizing gold loss and improving selectivity.

Benefits of technology

The process achieves high metal recovery rates with low environmental impact, reducing water consumption and energy use, and allows selective extraction of valuable metals like gold, overcoming the limitations of traditional hydrometallurgical methods.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024536092000001_ABST
    Figure 2024536092000001_ABST
Patent Text Reader

Abstract

The present invention relates to compositions and methods for extracting metals from solid materials using non-aqueous solvents and oxidizing agents. The methods and compositions of the present invention are useful for selectively extracting metals from solid materials, particularly e-waste materials.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to compositions and methods for the extraction of metals from solid materials using deep eutectic solvents (DES) and oxidants. The methods and compositions of the present invention are useful for selectively extracting metals from solid materials, particularly e-waste materials. [Background technology]

[0002] Deep eutectic solvents (DES) are formed by the complexation of certain components to provide a homogeneous mixture that melts at a single temperature below the melting point of any of the constituent components. Examples of components that can be complexed to form DESs are quaternary ammonium salts and hydrogen bond donors. Since their discovery, DES have found several applications including dissolving metal oxides and chlorides. In this regard, WO02 / 26701 discloses the preparation of various DES and their use as battery electrolytes, as solvents for metal oxides, as components for electrolytic polishing and electrodeposition of metals, and as solvents for chemical reactions. It was later discovered that naturally occurring metals, such as gold, silver, copper, nickel, tin, lead, aluminum, and iron, could be dissolved when DES was combined with an oxidizing agent in the form of iodine (Abbott et al., Electrocatalytic recovery of elements from complex mixtures using deep eutectic solvents, Green Chem., 2015, 17, pp 2172-2179). Iodine is poorly soluble in water, making it unsuitable for most aqueous chemistries. However, it is highly soluble in DES, and once solubilized, it is capable of oxidizing a wide range of metals.

[0003] The ability of DES to dissolve naturally occurring metals has potential applications in the field of metal extraction, where hydrometallurgical processes that often use strong inorganic acids or toxic chemicals such as cyanide or mercury, as well as energy-intensive high-temperature smelting processes, are currently used. However, the use of DES in combination with iodine to dissolve native metals has drawbacks, including the high cost of iodine, its relatively low metal selectivity due to its ability to oxidize a wide range of metals, and its sensitivity to added water. In light of the above, there is a need for compositions including DES and oxidizing agents that address these shortcomings. Additionally, there is a need for processes for extracting metals from solid materials that have improved selectivity for certain metals, thus simplifying the post-process recovery of these metals. This is particularly true for the extraction of metals from high-value components of electronic waste (e-waste), such as printed circuit boards (PCBs), central processing units (CPUs), and random access memories (RAMs), where the recovery of high-value metals, such as gold, is complicated by the presence of other metals. Summary of the Invention

[0004] The present invention addresses and overcomes the shortcomings of the prior art by providing a composition for extracting metals from solid materials comprising a DES and an oxidizing agent. The composition is capable of dissolving many metals, but may not be able to dissolve some metals, including gold. The present invention also provides a method for extracting metals from solid materials using the composition. In addition to the above, the present invention provides a two-step process for extracting metals from a solid material, in which the solid material is first contacted with a composition comprising a DES and a first oxidizing agent, and in a second step, contacted with a composition comprising a DES and a second oxidizing agent, the first oxidizing agent and the second oxidizing agent being different. Viewed from a first aspect, the present invention provides a method for extracting one or more metals from a solid material, comprising the steps of: (i) a first deep eutectic solvent (DES) formed by reaction of a first quaternary ammonium salt with a first hydrogen bond donor in a molar ratio of 4:1 to 1:20; and First Oxidant contacting the solid material with a first leaching solution comprising: A first leaching step comprising: (ii) a second DES formed by reaction of a second quaternary ammonium salt with a second hydrogen bond donor in a molar ratio of 4:1 to 1:20; and Second Oxidant contacting the first leached solid material with a second leaching solution comprising: A second leaching step comprising: wherein the first oxidant and the second oxidant are different. The method is targeted.

[0005] Viewed from a second aspect, the present invention provides a method for extracting one or more metals from a solid material, comprising the steps of: (i) deep eutectic solvents (DESs) formed by the reaction of quaternary ammonium salts with hydrogen bond donors in molar ratios ranging from 4:1 to 1:20; and First Oxidant contacting the solid material with a leach solution comprising: comprising a leaching step, The method is directed to a method wherein the first oxidant has a reduction potential less than or equal to +0.50 V and / or the first oxidant is an Fe(III) salt, a Cu(II) salt, a Te(IV) salt, a Cr(III) salt, or a Mn(VII) salt.

[0006] Viewed from a third aspect, the present invention provides a method for producing a composition comprising: a deep eutectic solvent formed by reaction of a first quaternary ammonium salt with a first hydrogen bond donor in a molar ratio of 4:1 to 1:20; and First Oxidant 1. A composition for extracting one or more metals from a solid material comprising: the reduction potential of the first oxidant is less than or equal to +0.50 V and / or the first oxidant is an Fe(III) salt, a Cu(II) salt, a Te(IV) salt, a Cr(III) salt, or a Mn(VII) salt; The present invention relates to compositions. Preferred features of the invention are set out in the dependent claims set out hereinafter. [Brief description of the drawings]

[0007] [Figure 1A] FIG. 1 shows the depth to which Cu, Ni, and Au deposits on resin are etched by immersing the resin in a DES containing choline chloride and ethylene glycol (known in the art as E200) in a 1:2 stoichiometric ratio + 1M FeCl3 according to Example 1. [Figure 1B] FIG. 1 shows the depth to which Cu, Ni, and Au deposits on resin are etched by immersing the resin in E200+0.5M I2 according to Example 1. [Diagram 2] FIG. 1 shows the normalized percentage of each metal leached during the leaching process described in Example 2. [Diagram 3] FIG. 1 shows the normalized percentage of each metal leached during the leaching process described in Example 2. [Figure 4] FIG. 1 shows the normalized percentage of each metal leached during the leaching process described in Example 2. [Diagram 5] FIG. 1 shows the normalized percentage of each metal leached during the leaching process described in Example 2. [Figure 6] FIG. 13 shows the mass percentage lost during treatment of E-waste with different oxidants at different temperatures according to Example 3. [Figure 7] FIG. 13 shows the effect of temperature, water content, DES:solids ratio, and time to leaching on <1.2 mm E-waste according to Example 4. [Figure 8] FIG. 1 shows the normalized percentage of each metal leached during the leaching process described in Example 5. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0008] The present inventors have disclosed a composition comprising a DES and an oxidizing agent, and a method for extracting one or more metals from a solid material using the composition. The composition demonstrates high oxidizing agent stability and is capable of dissolving many metals, including the majority of metals commonly present in electronic solid waste materials, but the composition is unable to dissolve some metals, including gold. The method for extracting metals from a solid material using the composition provides a gold-rich material after the solid material is contacted with the composition. The inventors have further developed a two-step process for efficient and selective extraction of metals from solid materials, the process comprising a first step of contacting the solid material with a composition comprising a DES and a first oxidizing agent. The material remaining after contacting the solid material with this composition is enriched in the metals that are not dissolved in the first step. In a second step, the solid material from the first step is contacted with a composition comprising a DES and a second oxidizing agent different from the first oxidizing agent. The second step may dissolve the metals left in the solid material after the first step. As is clear from the language used herein, the invention is not limited to a two-step treatment with a DES and an oxidizing agent, but may include one or more additional such steps using the same or different DES and oxidizing agent performed before, between and / or after the steps described herein.

[0009] DES is a non-aqueous solvent, which means that the compositions and methods of the present invention have very low water consumption. The low vapor pressure of DES also means that the method can be carried out at high temperatures without producing significant volatile organic compounds or particulate emissions and with minimal solvent loss due to evaporation. These relatively good properties mean that DES is user-friendly. The present invention provides a low carbon, low energy and environmentally friendly method for treating metal-bearing solid materials such as electronic waste (e-waste) or Waste Electrical and Electronic Equipment (WEEE). The method can replace environmentally damaging hydrometallurgical processes, which often use strong inorganic acids or toxic chemicals such as cyanide or mercury, as well as the energy intensive high temperature smelting processes commonly used to recycle such materials. Furthermore, the present invention provides high metal recovery from polymetallic feedstocks, enabling complex metal recovery at a relatively low cost compared to capital intensive high temperature smelting processes. In addition to the above advantages, the two-stage process of the present invention provides an efficient and selective process for recovering valuable metals contained in solid materials, producing either single elemental metal products or mixed metal products that can be tailored to meet market needs.

[0010] (definition) Oxidizing Agent - When a particular compound is referred to herein as an oxidizing agent (e.g., FeCl3), this means that when the oxidizing agent is dissolved in the DES, it will react with a counter ion (e.g., Cl - ) may vary, so refers to the form of oxidizing agent added to the composition. Viewed from a first aspect, the present invention provides a method for extracting one or more metals from a solid material, comprising the steps of: (i) a first deep eutectic solvent (DES) formed by reaction of a first quaternary ammonium salt with a first hydrogen bond donor in a molar ratio of 4:1 to 1:20; and First Oxidant contacting the solid material with a first leaching solution comprising: A first leaching step comprising: (ii) a second DES formed by reaction of a second quaternary ammonium salt with a second hydrogen bond donor in a molar ratio of 4:1 to 1:20; and Second Oxidant contacting the first leached solid material with a second leaching solution comprising: A second leaching step comprising: wherein the first oxidant and the second oxidant are different. A method is provided.

[0011] (Oxidizing agent) The oxidizing agent of the present invention may oxidize one or more metals in the solid material to an oxidized form, resulting in dissolution of the metals in the DES. The oxidizing agent of the present invention is thus an additional component to the components that form the DES (described below), and the oxidizing agent does not form part of the DES itself. The oxidizing agent may be added to the leach solution after the DES is formed from the quaternary ammonium salt and the hydrogen bond donor. In the first aspect of the invention, the first and second oxidizing agents are not particularly limited, other than that they are different. The ability of an oxidizing agent to oxidize and / or dissolve a given metal may depend on the reduction potential of the oxidizing agent. Thus, the first and second oxidizing agents of the invention may have different reduction potentials. For example, the reduction potential of the second oxidizing agent may be more positive than the reduction potential of the first oxidizing agent. A first oxidizing agent with a less positive reduction potential may not be able to oxidize (and therefore dissolve) a certain metal. This allows for selective dissolution of a certain metal at each step of the method. For example, the first oxidizing agent may be an oxidizing agent that cannot or does not oxidize gold, while the second oxidizing agent may be an oxidizing agent that oxidizes gold.

[0012] The reduction potential of the first oxidizing agent may be less than or equal to +0.50 V, may be between −1.00 V and +0.50 V, may be between 0 V and +0.50 V, may be between 0 V and +0.49 V, such as 0 V, +0.1 V, +0.2 V, +0.3 V, 0.4 V, or +0.49 V. Oxidizing agents with reduction potentials in these ranges may not be able to oxidize (and therefore dissolve) certain metals, including gold. The reduction potential of the second oxidant may be greater than or equal to +0.50 V, may be between +0.50 V and +2.0 V, may be between +0.51 V and +2.0 V, may be between +1.0 V and +2.0 V, for example +1.0 V, +1.1 V, +1.2 V, +1.3 V, +1.4 V, +1.5 V, +1.6 V, +1.7 V, +1.8 V, +1.9 V, or +2.0 V. Oxidants with reduction potentials in these ranges may be able to oxidize (and therefore dissolve) certain metals, including gold.

[0013] The first oxidizing agent may be a Fe(III) salt, a Cu(II) salt, a Te(IV) salt, a Cr(III) salt, or a Mn(VII) salt, preferably a Fe(III) salt or a Cu(II) salt, more preferably a Fe(III) salt. The first oxidizing agent may be preferably FeCl3, FeF3, FeBr3, FeI3, Fe(CN)6, Fe(SCN)3, Fe(NO3)3, Fe(SO4)3, Fe(OH)3, Fe(C2H3O2)3, CuCl2, CuF2, CuBr2, CuI2, Cu(NO3)2, CuSO4, CuO, Cu(OH)2, TeCl4, TeF4, TeBr4, TeI4, TeO2, or KMnO4, more preferably the first oxidizing agent is FeCl3 or CuCl2, even more preferably the first oxidizing agent is FeCl3. These oxidizing agents may not be able to oxidize (and therefore dissolve) certain metals, including gold. The first oxidizing agent of the present invention is 0.001 mol dm -3 ~2.5mol dm -3 , preferably 0.01 mol dm -3 ~2mol dm -3 , more preferably 0.1 mol dm -3~1.5mol dm -3 , e.g. 0.1 mol dm -3 , 0.25 mol dm -3 , 0.5 mol dm -3 , 0.75 mol dm -3 , 1 mol dm -3 , 1.25 mol dm -3 , or 1.5 mol dm -3 may be present in a concentration of

[0014] The second oxidant may be I2, or SeCl4, SeF4, SeBr4, SeI4, SeO2, preferably the second oxidant is iodine (I2). These oxidants may be capable of oxidizing (and therefore dissolving) certain metals, including gold. When iodine is the second oxidant, an additional benefit of the two-stage process is that less DES and iodine composition (which are more expensive) are required compared to processes in which only DES and iodine composition are used to extract the metals, due to less overall metal leaching after the first stage. Recovery of gold from the DES in the second stage may be greatly simplified since little or no other metals are contained in the DES at this stage. This is an important benefit of the process, since gold recovery is the key economic driver for the extraction of metals. The second oxidizing agent of the present invention is 0.001 mol dm -3 ~2.5mol dm -3 , preferably 0.01 mol dm -3 ~2mol dm -3 , more preferably 0.1 mol dm -3 ~1.5mol dm -3 , e.g. 0.1 mol dm -3 , 0.25 mol dm -3 , 0.5 mol dm -3 , 0.75 mol dm -3 , 1 mol dm -3 , 1.25 mol dm -3 , or 1.5 mol dm -3 may be present in a concentration of

[0015] (Deep eutectic solvent) The deep eutectic solvents of the present invention are prepared by reacting or combining or complexing a quaternary ammonium salt with a hydrogen bond donor. In the first aspect of the present invention, the first and second quaternary ammonium salts are not particularly limited and may be any capable of forming a DES with a hydrogen bond donor as described below. The first and second quaternary ammonium salts may each independently be a compound of formula (I). [ka] (I) (In the formula, R 1 , R 2 , R 3 , and R 4 each independently represents H, a substituted or unsubstituted C1-C5 alkyl group, a substituted or unsubstituted C6-C 10 Cycloalkyl groups, substituted or unsubstituted C6-C 12 Aryl groups, substituted or unsubstituted C7-C 12 is an alkaryl group, or R 1 and R 2 form a substituted or unsubstituted 5- to 11-membered ring together with the N atom to which they are attached, R 3 and R 4 is as already defined, X - is NO3 - , F - , Cl - , Br - , I - , BF4 - , ClO4 - , SO3CF3 - , bitartaric acid, dihydrogen citrate, or COOCF3 - and Substituted means that the groups are OH, SH, SR 5 , Cl, Br, F, I, NH2, CN, NO2, COO - , COOR 5 , CHO, COR 5 , and OR 5(wherein R 5 , H, C1-C 10 Alkyl or C1-C 10 is a cycloalkyl group.

[0016] The first and second quaternary ammonium salts may each independently be a compound of formula (I), R 1 , R 2 , and R 3 are each independently H or an unsubstituted C1-C4 alkyl group; R 4 is a substituted or unsubstituted C1-C4 alkyl group, and X - and "substituted" is as defined above. More preferably, R 1 , R 2 , and R 3 are each independently H or an unsubstituted C alkyl group; R 4 is a substituted or unsubstituted C1-C4 alkyl group, where substituted means that the group is, for example, OR 5 , COO - , and COOR 5 (wherein R 5 , H, C1-C 10 Alkyl, or C1-C 10 is a cycloalkyl group, X - is as defined above). For example, the first and second quaternary ammonium salts may each independently be choline chloride, choline hydroxide, choline acetate, choline bitartrate, choline dihydrogen citrate, betaine, betaine HCl, ammonium chloride, methylammonium chloride, ethylammonium chloride, tetrabutylammonium chloride, or ethanolamine hydrochloride, preferably the first and second quaternary ammonium salts are choline chloride.

[0017] The first and second hydrogen bond donors of the present invention are not particularly limited and may be any of the above-mentioned quaternary ammonium salts capable of forming a DES. The first and second hydrogen bond donors are each independently represented by the formula R6 COOH, R 7 R 8 N.H., R. 9 CZNH2, R 10 OH or HO-R 11 It may be a compound of —OH. (In the formula, R 6 , R 7 , R 8 , and R 10 each independently represents H, a substituted or unsubstituted C1-C8 alkyl group, a substituted or unsubstituted C1-C8 alkenyl group, a substituted or unsubstituted aryl group, or a substituted or unsubstituted C7-C 12 is an alkaryl group, and R 11 is a substituted or unsubstituted C1-C 11 is an alkyl group, Substituted means OH, SR5, Cl, Br, F, I, NH2, CN, NO2, 3,4-dihydroxy-2H-furan-5-one, CONR 5 , COOR 5 , C.O.R. 5 , and OR 5 (wherein R 5 , H, C1-C 10 Alkyl, or C1-C 10 a cycloalkyl group, R 9 is R 6 or NHR 12 and R 12 is H or a C1-C6 alkyl group, and Z is O or S.

[0018] The first and second hydrogen bond donors are each independently represented by the formula R 6 COOH, R 9 CZNH2 or HO-R 11 In the formula, R 6 , R 9 , Z, and R 11 is as defined above) The first and second hydrogen bond donors are each independently represented by the formula R 6 COOH, R9 CZNH2 or HO-R 11 The compound may be a compound having the formula: R 6 is a substituted or unsubstituted C1-C6 alkyl group, a substituted or unsubstituted C1-C6 alkenyl group, or a substituted or unsubstituted aryl group; R 9 is a substituted or unsubstituted C1-C6 alkyl group, a substituted or unsubstituted C1-C6 alkenyl group, or NHR 12 where R 12 is H or a substituted or unsubstituted C1-C6 alkyl group, and Z is O, and R 11 is a substituted or unsubstituted C1-C8 alkyl group, Substituted means OH, CONR 5 , COOR 5 , C.O.R. 5 , and OR 5 (wherein R 5 is H, a C1-C6 alkyl, or a C1-C6 cycloalkyl group)

[0019] The first and second hydrogen bond donors are each independently represented by the formula R 6 COOH, R 9 CZNH2 or HO-R 11 The compound may be a compound having the formula: R 6 is a substituted or unsubstituted C1-C5 alkyl group, a substituted or unsubstituted C1-C4 alkenyl group, or a substituted or unsubstituted aryl group; R 9 is a substituted or unsubstituted C1-C5 alkyl group, or a substituted or unsubstituted C1-C4 alkenyl group, or NHR 12 where R 12 is H or a C1-C6 alkyl group and Z is O, and R 11 is a substituted or unsubstituted C1-C5 alkyl group, Substituted means OH, CONR 5 , COOR5 , C.O.R. 5 , and OR 5 (wherein R 5 is H or a C1-C6 alkyl group) The first and second hydrogen bond donors are each independently represented by the formula R 6 COOH or HO-R 11 The compound may be a compound having the formula: R 6 is a substituted or unsubstituted C1-C5 alkyl group, a substituted or unsubstituted C1-C4 alkenyl group, or a substituted or unsubstituted aryl group; R 11 is a substituted or unsubstituted C1-C5 alkyl group, Substituted means OH, CONR 5 , and COOR 5 (wherein R 5 is H or a C1 alkyl group)

[0020] The first and second hydrogen bond donors each independently have the formula HO-R 11 The compound may be a compound having the formula: R 11 OH and COOR 5 (wherein R 5 is H or a C1 alkyl group) For example, the first and second hydrogen bond donors can each independently be ethylene glycol, glycerol, 1,2-propanediol, 1,3-propanediol, 1,4-butanediol, 1,5-pentanediol, urea, oxalic acid, malonic acid, levulinic acid, lactic acid, citric acid, maleic acid, malonamide, acetamide, oxalic acid dihydrate, ascorbic acid, glutaric acid, glycolic acid, mandelic acid, succinic acid, tartaric acid, or phenol, preferably the first and second hydrogen bond donors are ethylene glycol. The molar ratio of the first quaternary ammonium salt to the first hydrogen bond donor is not particularly limited, except that it must be a ratio that results in the formation of a DES when the first quaternary ammonium salt and the first hydrogen bond donor are combined. The molar ratio of the first quaternary ammonium salt to the first hydrogen bond donor may be 4:1 to 1:20, preferably 3.5:1 to 1:15, more preferably 2.5:1 to 1:10, more preferably 2:1 to 1:4, for example 2:1, 1:1, 1:2, 1:3, or 1:4.

[0021] The molar ratio of the second quaternary ammonium salt to the second hydrogen bond donor is not particularly limited, except that it must be a ratio that results in the formation of a DES when the second quaternary ammonium salt and the second hydrogen bond donor are combined. The molar ratio of the second quaternary ammonium salt to the second hydrogen bond donor may be 4:1 to 1:20, preferably 3.5:1 to 1:15, more preferably 2.5:1 to 1:10, more preferably 2:1 to 1:4, for example 2:1, 1:1, 1:2, 1:3, or 1:4. The inventors have found that a DES comprising choline chloride and ethylene glycol in a 1:2 stoichiometric ratio (known in the art as E200) is advantageous for carrying out the steps of the present invention. The DES can be diluted with aqueous and / or organic solvents ranging from 0% dilution up to 75% dilution (w / w). The diluent may be one or more selected from the group consisting of water, ethanol, acetonitrile, dichloromethane, or acetone. The DES may be hygroscopic and may inherently contain a certain amount of water, for example 2% (w / w). The DES may be further diluted with water to a total mass of water of, for example, 16% (w / w).

[0022] (Process parameters) The solid material may be any solid material including a metal. The solid material may be a solid waste material, such as an electronic waste material, for example, a printed circuit board. The metal in the solid material is not particularly limited and may be any metal known to those skilled in the art. For example, the metal may include one or more selected from the group consisting of aluminum, steel, copper, nickel, tin, lead, palladium, zinc, silver, chromium, cobalt, vanadium, indium, mercury, antimony, gallium, beryllium, molybdenum, cadmium, and gold. The first liquid phase may contain any or all of the above metals, or the first liquid phase may contain any or all of the above metals except gold, the second liquid phase may contain any or all of the above metals, or the second liquid phase may contain only gold.

[0023] Prior to carrying out the leaching step, the solid material may be comminuted by crushing, grinding or chopping to reduce its particle size. This may improve the efficiency of the leaching process by reducing the amount of DES and oxidant required to extract the metal. The solid material may be comminuted to a particle size of less than 10 mm, preferably less than 1.2 mm, for example between 10 μm and 1 mm. In an embodiment, the solid material is comminuted and separated into two fractions using a sieve with a pore size of 1.2 mm before the DES treatment. Furthermore, aluminum and steel may be removed before carrying out the leaching step, for example by mass spectrometry / eddy current / magnetic separation techniques. This may also improve the efficiency of the leaching process. In the first and second leaching steps, the ratio of DES plus oxidant to metal in the solid material may be 1:50-100:1 (w:w), 1:40-75:1, 1:30-50:1, 1:25-25:1, or 1:20-10:1, for example 1:20, 1:15, 1:10, 1:5, 1:1, 5:1, or 10:1 (w:w).

[0024] In the first and second leaching steps, the ratio of DES to solid material may be 1:50 to 100:1 (v / w), 1:10 to 50:1, 1:5 to 40:1, 1:1 to 30:1, 2:1 to 25:1, for example 2:1, 3:1, 4:1, 5:1, 10:1, 15:1, 20:1, or 25:1 (v / w). In the first and second leaching steps, the solid material may be leached at a temperature between 10°C and 120°C, between 40°C and 110°C, between 50°C and 100°C, for example at 50, 55, 60, 65, 70, 75, 80, 85, 90, 95, or 100°C. In the first and second leaching steps, the solid material may be leached for 5 minutes to 240 hours, preferably between 1 hour to 144 hours, more preferably between 6 hours to 96 hours, more preferably between 12 hours to 48 hours, more preferably between 18 hours to 36 hours, for example 18, 24, 30, or 36 hours. In an embodiment, the solid material may be leached at a temperature between 10°C and 120°C for 5 minutes to 240 hours, preferably at 80°C for 24 hours.

[0025] In certain embodiments of the first aspect of the invention, the first and second quaternary ammonium salts may each independently be choline chloride, choline hydroxide, choline acetate, choline bitartrate, choline dihydrogen citrate, betaine, betaine HCl, ammonium chloride, methylammonium chloride, ethylammonium chloride, tetra-butylammonium chloride, or ethanolamine hydrochloride, preferably the first and second quaternary ammonium salts are choline chloride; the first and second hydrogen bond donors may each independently be ethylene glycol, glycerol, 1,2-propanediol, 1,3-propanediol, 1,4-butanediol, 1,5-pentanediol, urea, oxalic acid, malonic acid, levulinic acid, lactic acid, citric acid, maleic acid, malonamide urea, acetamide, oxalic acid dihydrate, ascorbic acid, glutaric acid, glycolic acid, mandelic acid, succinic acid, tartaric acid, or phenol, preferably the first and second hydrogen bond donors are ethylene glycol; The molar ratio of the first and second quaternary ammonium salts to the first and second hydrogen bond donors may be from 4:1 to 1:20, preferably from 2:1 to 1:4; The reduction potential of the first oxidizing agent may be less than or equal to +0.50 V, and / or the first oxidizing agent may be an Fe(III) salt, a Cu(II) salt, a Te(IV) salt, a Cr(III) salt, or a Mn(VII) salt, preferably the first oxidizing agent is an Fe(III) salt or a Cu(II) salt, preferably FeCl3 or CuCl2, more preferably the first oxidizing agent is FeCl3, and The reduction potential of the second oxidizing agent may be greater than or equal to +0.50 V, and / or the second oxidizing agent may be I2, or SeCl4, SeF4, SeBr4, SeI4, SeO2, preferably the second oxidizing agent is I2.

[0026] In certain embodiments of the first aspect of the present invention, the first and second quaternary ammonium salts are choline chloride, the first and second hydrogen bond donors are ethylene glycol, the molar ratios of the first quaternary ammonium salt to the first hydrogen bond donor and the second quaternary ammonium salt to the second hydrogen bond donor are both 1:2, the reduction potential of the first oxidant is less than or equal to +0.50 V, and / or the first oxidant is an Fe(III) salt or a Cu(II) salt, preferably FeCl3 or CuCl2; and the reduction potential of the second oxidant is greater than or equal to +0.50 V, and / or the second oxidant is I2. The method of the present invention may further comprise recovering one or more metals from the first liquid phase; and / or recovering one or more metals from the second liquid phase. The method for recovering metals from the solution according to the present invention is not particularly limited and may be any of those known to the skilled artisan. Metals may be recovered individually or together with other metals. Recovery processes may include processes whereby metals are recovered from the solution using solvent extraction, precipitation (e.g., cementation), and / or electrochemical reactions (e.g., electrowinning). In a particular embodiment, gold is recovered by the addition of activated carbon (e.g., Jacobi PICAGOLD® G210AS).

[0027] During the leaching step, the oxidizing agent oxidizes the metals in the solid material and the oxidizing agent may be reduced so that it can no longer be oxidized. The method of the present invention may therefore further comprise a step of regenerating the oxidizing agent. The regenerating step may be performed after the leaching step or may be performed simultaneously with the leaching step so that the oxidizing agent is regenerated in situ. The oxidizing agent may be regenerated by any means known to the skilled person. For example, the oxidizing agent may be regenerated by bubbling oxygen into the leaching solution or into the liquid phase resulting from the leaching step. This method may be particularly advantageous when the oxidizing agent is an Fe(III) salt, a Cu(II) salt, a Te(IV) salt, a Cr(III) salt or a Mn(VII) salt, for example when the oxidizing agent is FeCl3. The oxidizing agent may be regenerated using an electrochemical reaction, for example by inserting an electrode into the leaching solution or into the liquid phase resulting from the leaching step and applying a voltage. The method of the invention may further comprise filtering and / or cleaning and / or drying the solid material after each leaching step. These additional steps may improve the efficiency of any subsequent leaching steps.

[0028] Viewed from a second aspect, the present invention provides a method for extracting one or more metals from a solid material, comprising the steps of: (i) deep eutectic solvents (DESs) formed by the reaction of quaternary ammonium salts with hydrogen bond donors in molar ratios ranging from 4:1 to 1:20; and First Oxidant contacting the solid material with a leach solution comprising: comprising a leaching step, The method further comprises the step of: providing a first oxidant having a reduction potential less than or equal to +0.50 V; and / or the first oxidant is an Fe(III) salt, a Cu(II) salt, a Te(IV) salt, a Cr(III) salt, or a Mn(VII) salt. Viewed from a third aspect, the present invention provides a method for producing a method for manufacturing a semiconductor device comprising: a deep eutectic solvent formed by reaction of a first quaternary ammonium salt with a first hydrogen bond donor in a molar ratio of 4:1 to 1:20; and First Oxidant A composition for leaching one or more metals from a solid material comprising: The composition is provided wherein the reduction potential of the first oxidant is less than or equal to +0.50 V and / or the first oxidant is an Fe(III) salt, a Cu(II) salt, a Te(IV) salt, a Cr(III) salt, or a Mn(VII) salt.

[0029] The descriptions of the features of the first aspect (including the descriptions of the first oxidant, the deep eutectic solvent, and the process parameters) are equally applicable to the second and third aspects of the invention. In this regard, the reduction potential of the first oxidizing agent may be less than or equal to +0.50 V, may be between −1.00 V and +0.50 V, may be between 0 V and +0.50 V, such as 0 V, +0.1 V, +0.2 V, +0.3 V, +0.4 V, or +0.5 V, and may be between 0 V and +0.49 V. Oxidizing agents having reduction potentials in these ranges may not be able to oxidize (and therefore dissolve) certain metals, including gold. The reduction potential of the second oxidant may be greater than or equal to +0.50 V, may be between +0.50 V and +2.0 V, may be between +0.51 V and +2.0 V, may be between +1.0 V and +2.0 V, for example +1.0 V, +1.1 V, +1.2 V, +1.3 V, +1.4 V, +1.5 V, +1.6 V, +1.7 V, +1.8 V, +1.9 V, or +2.0 V. Oxidants with reduction potentials in these ranges may be able to oxidize (and therefore dissolve) certain metals, including gold.

[0030] The first oxidizing agent may be a Fe(III) salt, a Cu(II) salt, a Te(IV) salt, a Cr(III) salt, or a Mn(VII) salt, preferably a Fe(III) salt or a Cu(II) salt, more preferably a Fe(III) salt. The first oxidizing agent may be preferably FeCl3, FeF3, FeBr3, FeI3, Fe(CN)6, Fe(SCN)3, Fe(NO3)3, Fe(SO4)3, Fe(OH)3, Fe(C2H3O2)3, CuCl2, CuF2, CuBr2, CuI2, Cu(NO3)2, CuSO4, CuO, Cu(OH)2, TeCl4, TeF4, TeBr4, TeI4, TeO2, or KMnO4, more preferably the first oxidizing agent is FeCl3 or CuCl2, even more preferably the first oxidizing agent is FeCl3. These oxidizing agents may not be able to oxidize (and therefore dissolve) certain metals, including gold. The first oxidizing agent of the present invention is 0.001 mol dm -3 ~2.5mol dm -3 , preferably 0.01 mol dm -3 ~2mol dm -3 , more preferably 0.1 mol dm -3~1.5mol dm -3 , e.g. 0.1 mol dm -3 , 0.25 mol dm -3 , 0.5 mol dm -3 , 0.75 mol dm -3 , 1 mol dm -3 , 1.25 mol dm -3 , or 1.5 mol dm -3 may be present in a concentration of EXAMPLES

[0031] (Reduction potential) The reduction potentials of the oxidants listed in this application were measured as formal reduction potentials in the respective DES using an Ag reference electrode in AgCl (0.1 M). (Leaching efficiency) Leaching efficiency (i.e., the percentage of each metal recovered during the leaching step) was determined by leaching the solid material remaining after the leaching step with aqua regia for 24 hours to dissolve all remaining metals. The concentrations of metals in aqua regia were determined via inductively coupled plasma mass spectroscopy (ICP-MS).

[0032] Example 1 Metal dissolution by DES+FeCl3 and DES+I2 The objective of the study was to determine whether Au could be dissolved in DES+FeCl3 or DES+I2 when in close proximity to Cu and Ni, other metals commonly found in E-waste. The DES was formed by combining choline chloride and ethylene glycol in a 1:2 stoichiometric ratio with heating at 50° C. and stirring until a clear homogenous liquid was formed. This DES is known in the art as E200. To form E200+1M FeCl3, FeCl3 was added to E200 (1 L) to achieve a concentration of 1 M FeCl3 with stirring at 50° C. until all solids were dissolved. To form E200+0.5M I2, I2 was added to E200 (1 L) to achieve a concentration of 0.5 M I2 with stirring at 50° C. until all solids were dissolved.

[0033] Polished resin blocks made from Araldite 2020 resin (E), containing adjacent deposits of Cu, Ni, and Au metals at approximately 1 mm thickness, were supplied by RS Components Pty Ltd. Resin blocks were immersed in 200 mL of E200+1M FeCl3 prepared as described above for 40 minutes at 50° C., and individual resin blocks were immersed in 200 mL of E200+0.5M I2 prepared as described above for 40 minutes at 50° C. At time intervals of 0, 5, 10, 20, and 40 minutes, blocks were removed, washed with deionized water, and washed with acetone. The etch depths of Cu, Ni, and Au were measured before at these time intervals using a Zeta™ Instruments Zeta 2000 optical profiler using built-in Zeta3D software version 1.8.5. In this regard, a baseline was created by measuring the height of the metal relative to the resin before treatment with the DES formulation. The metal height was measured during and after treatment, and the etch depth was determined by calculating the difference between the measured height and the baseline. The results are shown in Table 1 below and in Figures 1A and 1B.

[0034] [Table 1] As shown in Table 1 and Figures 1A and 1B, Cu and Ni were dissolved using both DES formulations. Au was dissolved when I2 was used as the oxidizer in E200, but Au was not dissolved when FeCl3 was used as the oxidizer in E200.

[0035] Example 2 A two-stage leaching process performed on crushed e-waste E-waste containing a mixture of commercially available PCBs, CPUs, RAM sticks, connectors, and other high grade E-waste materials was investigated for bulk dissolution using the two-stage DES leaching process of the present invention. E-waste was supplied by PMS Handelskontor GmbH, crushed and processed using their VeRoLiberator® technology. The as-supplied material was sieved through a 1.2 mm pore sieve to separate the <1.2 mm and ≥1.2 mm fractions. A NdFeB supermagnet encased in a plastic sheath was passed through both fractions to remove ferrous material. A typical distribution of metals for each of the sized fractions, prior to ferrous material removal, can be seen in Table 2: [Table 2]

[0036] The fraction was split into 50.0 g batches and combined with pre-heated DES1 formulation in the DES:solid ratio stated in Table 3 and stirred at 80° C. on a hot plate stirrer using a magnetic stir bar for 24 hours. The DES1 formulation was pre-heated as in Example 1 above. During this 24 hour period, 5.0 mL aliquots were taken and analyzed by inductively coupled plasma mass spectrometry (ICP-MS). The ICP-MS used was a Thermo Scientific™ iCAP™ qc Quadrupole ICP-MS with a Cetac™ ASX520 autosampler using Qtegra™ software version 2.10.3324.131.

[0037] The resulting solid was vacuum filtered, washed with hot deionized water until all DES1 was removed from the solid, and then dried in a vacuum oven for 24 hours at 50°C. This dried material was then transferred to a pre-heated DES2 formulation at the DES2:solid ratio described in Table 3 and stirred on a hot plate stirrer at 80°C for 24 hours using a magnetic stir bar. The DES2 formulation was prepared as in Example 1 above. The resulting solid was vacuum filtered, washed using ethanol, then washed with hot deionized water until all DES2 was removed from the solid, and then dried in a vacuum oven for 24 hours at 50°C. Due to the heterogeneity of the E-waste material, the total dissolution of metals was calculated by dissolving the remaining solid residue in aqua regia at a liquid to solid ratio of 5:1 for 24 hours at room temperature and analyzing using ICP-MS. The percentage leaching values ​​listed in Tables 4-7 were calculated by calibrating the metal concentrations (as measured by ICP-MS) at each time interval against the starting concentrations and the concentrations in aqua regia (both measured by ICP-MS).

[0038] [Table 3]

[0039] The percentages of Al, Ni, Cu, Ag, Sn, Au, and Pb leached in EW001-EW004 are shown in Tables 4-7 below, respectively. [Table 4] [Table 5] [Table 6] [Table 7] Figures 2-5 show the percentage of Al, Ni, Cu, Ag, Sn, Au, and Pb leached during treatment with DES1 and DES2 in experiments EW001, EW002, EW003, and EW004, respectively. As can be seen, treatment with DES1, in the presence of a less positive oxidant, leaches up to 100% of Al, Ni, Cu, Ag, Sn, and Pb and little or no Au, while treatment with DES2, in the presence of a different, more positive oxidant, leaches over 90% of Au.

[0040] Example 3 Effect of different oxidants and temperatures A series of mass loss experiments were conducted designed to investigate the total mass loss for the <1.2 mm E-waste fraction prepared as in Example 2 as a function of time and DES formulation. Table 8 shows data from ten individual experiments involving the treatment of 10.00 g of the <1.2 mm E-waste fraction using the DES formulations listed in column 2 of columns 2-4 for the times listed in each row of column 1. Each timed experiment was run independently on 10.00 g of the <1.2 mm E-waste material, and the mass of the E-waste material remaining was measured after vacuum filtration of the DES formulation, washing with deionized water, and then subsequently drying under vacuum at 50° C. for 24 hours.

[0041] [Table 8] The data in Table 8 are presented graphically in Figure 6. This figure shows that lower temperatures result in a slower initial rate of mass loss, but similar total mass loss after 24 hours. The rate and total mass loss are approximately the same when CuCl2 and FeCl3 are used as oxidizers at the same temperatures.

[0042] Example 4 Effect of temperature, water content, DES:solid ratio, and time of DES1-E200+1M FeCl3 on the leaching of <1.2mm E-waste Effect of temperature, moisture content, DES:solids ratio, and time on the effectiveness of DES1 (E200+1M FeCl3) in leaching E-waste samples ground using a hammer mill to achieve a <2.0mm size fraction after passing a range of wedge bar screens spanning from 50mm to 2.0mm. Typical assays of the resulting material can be seen in Table 9 and were collected using ICP-MS (Thermo Scientific™ iCAP™ qc Quadrupole ICP-MS with a Ceta™ ASX520 autosampler using Qtegra™ software version 2.10.3324.131).

[0043] [Table 9] The recovery of metals from this <2.0 mm E-waste material was investigated through a series of tests carried out on approximately 10.0 g samples of E-waste material. In all cases, the DES formulation E200+1M FeCl3 was used. The baseline wt% water, i.e. the amount of water in the DES formulation before water was added, was measured to be 2.0 wt%. An additional 14 wt% water was gravimetrically added to the pre-made E200+1M FeCl3 and stirred for 5 minutes at room temperature using a magnetic stir bar. The total water content was measured using a Mettler Toledo® Titrator Compact V20S volumetric Karl Fischer Titrator.

[0044] The study was carried out using the matrix described in Table 10. Analysis was carried out using ICP-MS as described in Example 2. Values ​​greater than 100% are due to small sample heterogeneities. The process was carried out using a 250 mL round bottom flask with magnetic stirring using a Radley's Carousel 6 Plus™ system 34. [Table 10] As can be seen from Table 10 and Figure 7, Au did not leach under any conditions. Large amounts of Cu, Zn, Sn, and Ag were leached under all conditions. Zn leaching appeared to be the most sensitive to changing conditions. Increasing the temperature and leaching time improved the leaching percentage.

[0045] Example 5 Two-stage leaching process carried out on crushed e-waste Pretreatment of e-waste before extraction Grinding of e-waste materials: The materials were ground to a particle size below 1.2 mm. Steel Removal: Steel was removed by magnetic separation techniques.

[0046] Extraction using deep eutectic solvents Stage 1 leaching: E-waste solid material containing copper, nickel, tin, lead, silver, and gold is sent into the first leaching tank, where it is treated with choline chloride (1 mol equivalent) and ethylene glycol (2 mol equivalent), as well as FeCl3 (1 mol dm -3 ), the ratio of DES+FeCl3 to solid material was 15:1 w / w. The solid material was contacted with the DES+FeCl3 formulation at 80°C for 24 hours resulting in efficient metal recovery: Cu: 99.7%, Ni: 99%, Sn: 92%, Pb: 98%, Ag: 99%. 0% of Au was leached using this formulation resulting in Au-rich solid material. The leached solid material from this stage was filtered, washed and dried. The liquid phase containing the leached metals was transferred to a separate tank for metal recovery.

[0047] Stage 2 Leaching: The cleaned and dried leached solid material is transferred into a second leaching tank where it is treated with choline chloride (1 mol equiv.) and ethylene glycol (2 mol equiv.), as well as I2 (0.5 mol dm -3), which was formed from the leaching of the leached solid material. The ratio of DES+I2 to the solid material was 3:1 w / w. The objective of this second leaching is to recover Au from the solid material. Contacting the solid material with the DES+I2 formulation at 80°C for 24 hours resulted in a 99% Au recovery and also allowed the recovery of any residual metals contained in the solid residue. The leached solid material from this stage was filtered, washed and sent for waste. The liquid phase containing the leached metals was transferred to a separate tank for metal recovery. Data from this leaching process can be seen in Figure 8.

Claims

1. 1. A method for extracting one or more metals from a solid material, comprising the steps of: (i) a first deep eutectic solvent (DES) formed by reaction of a first quaternary ammonium salt with a first hydrogen bond donor in a molar ratio of 4:1 to 1:20; and First Oxidant contacting the solid material with a first leach solution comprising: A first leaching step comprising: (ii) a second DES formed by reaction of a second quaternary ammonium salt with a second hydrogen bond donor in a molar ratio of from 4:1 to 1:20; and Second Oxidant contacting the first leached solid material with a second leaching solution comprising: A second leaching step comprising: wherein the first oxidant and the second oxidant are different. method.

2. The method of claim 1 , wherein the first and second oxidants have different reduction potentials.

3. 3. The method of claim 1 or 2, wherein the reduction potential of the second oxidant is more positive than the reduction potential of the first oxidant.

4. The method according to any one of claims 1 to 3, wherein the reduction potential of the first oxidant is less than or equal to +0.50V, preferably between -1.00V and +0.50V.

5. The method according to any one of claims 1 to 4, wherein the reduction potential of the second oxidant is greater than or equal to +0.50V, preferably between +0.50V and +2.0V.

6. The method of any one of claims 1 to 5, wherein the first oxidizing agent is incapable of oxidizing Au(0).

7. The method of any one of claims 1 to 6, wherein the second oxidizing agent oxidizes Au(0).

8. 8. The method according to any one of claims 1 to 7, wherein the first oxidant is a Fe(III) salt, a Cu(II) salt, a Te(IV) salt, a Cr(III) salt, or a Mn(VII) salt, preferably a Fe(III) salt or a Cu(II) salt, more preferably a Fe(III) salt.

9. The first oxidant is FeCl 3 , FeF 3 , FeBr 3 , FeI 3 , Fe(CN) 6 , Fe(SCN) 3 , Fe(NO 3 ) 3 , Fe(SO 4 ) 3 , Fe(OH) 3 , Fe(C 2 H 3 O 2 ) 3 , CuCl 2 , CuF 2 , CuBr 2 , CuI 2 , Cu(NO 3 ) 2 , CuSO 4 , CuO, Cu(OH) 2 , TeCl 4 , TeF 4 , TeBr 4 , TeI 4 , TeO 2 , or KMnO 4 and more preferably, the first oxidant is FeCl 3 or CuCl 2 and even more preferably, the first oxidant is FeCl 3 The method according to any one of claims 1 to 8, wherein

10. The second oxidant is I 2 , or SeCl 4 , SeF 4 , SeBr 4 , SeI 4 , SeO 2 and preferably the second oxidant is I 2 The method according to any one of claims 1 to 9, wherein

11. The method of any one of claims 1 to 10, wherein the first and second quaternary ammonium salts are each independently a compound of formula (I). 【Chemistry 1】 (I) (In the formula, R 1 , R 2 , R 3 , and R 4 each independently represents H, substituted or unsubstituted C 1 -C 5 Alkyl group, substituted or unsubstituted C 6 -C 10 Cycloalkyl group, substituted or unsubstituted C 6 -C 12 Aryl group, substituted or unsubstituted C 7 -C 12 is an alkaryl group, or R 1 and R 2 form a substituted or unsubstituted 5- to 11-membered ring together with the N atom to which they are attached; R 3 and R 4 is as already defined, X - No. 3 - , F - , Cl - , B - , I - , B.F. 4 - , ClO 4 - , S.O. 3 CF 3 - , bitartaric acid, dihydrogen citrate, or COOCF 3 - and Substituted means that the group is not OH, SH, SR 5 , Cl, Br, F, I, NH 2 , C.N., N.O. 2 , COO - , COOR 5 , CHO, COR 5 , and OR 5 (wherein R 5 is H, C 1 -C 10 Alkyl or C 1 -C 10 is a cycloalkyl group)

12. 12. The method of any one of claims 1 to 11, wherein the first and second quaternary ammonium salts are each independently choline chloride, choline hydroxide, choline acetate, choline bitartrate, choline dihydrogen citrate, betaine, betaine HCl, ammonium chloride, methylammonium chloride, ethylammonium chloride, tetrabutylammonium chloride, or ethanolamine hydrochloride, preferably the first and second quaternary ammonium salts are choline chloride.

13. The first and second hydrogen bond donors are each independently represented by the formula R 6 COOH, R 7 R 8 N.H., R. 9 CZNH 2 , R 10 OH or HO-R 11 The method according to any one of claims 1 to 12, wherein the compound is -OH. (In the formula, R 6 , R 7 , R 8 , and R 10 each independently represents H, substituted or unsubstituted C 1 -C 8 Alkyl group, substituted or unsubstituted C 1 -C 8 an alkenyl group, a substituted or unsubstituted aryl group, or a substituted or unsubstituted C 7 -C 12 is an alkaryl group, and R 11 is a substituted or unsubstituted C 1 -C 11 is an alkyl group, Substituted means that the group is selected from the group consisting of OH, SR 5 , Cl, Br, F, I, NH 2 , C.N., N.O. 2 , 3,4-dihydroxy-2H-furan-5-one, CONR 5 , COOR 5 , C.O.R. 5 , and OR 5 (wherein R 5 is H, C 1 -C 10 Alkyl, or C 1 -C 10 is a cycloalkyl group), R 9 is R 6 or NHR 12 and R 12 is H or C 1 -C 6 is an alkyl group, and Z is O or S; R 11 is a substituted or unsubstituted C 1 -C 11 is an alkyl group)

14. 14. The method of any one of claims 1 to 13, wherein the first and second hydrogen bond donors are each independently ethylene glycol, glycerol, 1,2-propanediol, 1,3-propanediol, 1,4-butanediol, 1,5-pentanediol, urea, oxalic acid, malonic acid, levulinic acid, lactic acid, citric acid, maleic acid, malonamide, acetamide, oxalic acid dihydrate, ascorbic acid, glutaric acid, glycolic acid, mandelic acid, succinic acid, tartaric acid, or phenol, preferably the first and second hydrogen bond donors are ethylene glycol.

15. The method according to any one of claims 1 to 14, wherein the molar ratio of the first quaternary ammonium salt to the first hydrogen bond donor is from 4:1 to 1:20, preferably from 2:1 to 1:

4.

16. The method according to any one of claims 1 to 15, wherein the molar ratio of the second quaternary ammonium salt to the second hydrogen bond donor is from 4:1 to 1:20, preferably from 2:1 to 1:

4.

17. The first oxidant is 0.001 mol dm -3 ~2.5 mol dm -3 , preferably 1 mol dm -3 The method according to any one of claims 1 to 16, wherein the compound is present in a concentration of

18. The second oxidant is 0.001 mol dm -3 ~1.5 mol dm -3 , preferably 0.5 mol dm -3 The method according to any one of claims 1 to 17, wherein the compound is present in a concentration of

19. 19. A method according to any one of the preceding claims, wherein in the first leaching step the ratio of DES plus first oxidant to metal in the solid material is from 1:50 to 100:1 (w:w).

20. 20. The method of any one of the preceding claims, wherein in the second leaching step the ratio of DES plus second oxidant to metal in the solid material is from 1:50 to 100:1 (w:w).

21. 21. The method according to any one of claims 1 to 20, wherein in the first leaching step the ratio of DES to solid material is from 1:50 to 100:1 (v / w).

22. A method according to any one of the preceding claims, wherein in the second leaching step the ratio of DES to solid material may be from 1:50 to 100:1 (v / w).

23. 23. A method according to any one of the preceding claims, wherein in the first and second leaching steps, the solid material is leached at a temperature of from 10°C to 120°C for a period of from 5 minutes to 240 hours.

24. the first and second quaternary ammonium salts are each independently choline chloride, choline hydroxide, choline acetate, choline bitartrate, choline dihydrogen citrate, betaine, betaine HCl, ammonium chloride, methylammonium chloride, ethylammonium chloride, tetra-butylammonium chloride, or ethanolamine hydrochloride, preferably the first and second quaternary ammonium salts are choline chloride; the first and second hydrogen bond donors are each independently ethylene glycol, glycerol, 1,2-propanediol, 1,3-propanediol, 1,4-butanediol, 1,5-pentanediol, urea, oxalic acid, malonic acid, levulinic acid, lactic acid, citric acid, maleic acid, malonamide urea, acetamide, oxalic acid dihydrate, ascorbic acid, glutaric acid, glycolic acid, mandelic acid, succinic acid, tartaric acid, or phenol, preferably the first and second hydrogen bond donors are ethylene glycol; the molar ratio of said first and second quaternary ammonium salts to said first and second hydrogen bond donors is preferably from 4:1 to 1:20, more preferably from 2:1 to 1:4; The reduction potential of the first oxidant is less than or equal to +0.50 V, and preferably the first oxidant is FeCl 3 and The reduction potential of the second oxidant is greater than or equal to +0.50 V, and preferably the second oxidant is I 2 That is, 24. The method according to any one of claims 1 to 23.

25. the first and second quaternary ammonium salts are choline chloride, the first and second hydrogen bond donors are ethylene glycol, the molar ratio of the first quaternary ammonium salt to the first hydrogen bond donor and the second quaternary ammonium salt to the second hydrogen bond donor is 1:2, the reduction potential of the first oxidizing agent is less than or equal to +0.50 V, and / or the first oxidizing agent is an Fe(III) salt or a Cu(II) salt, preferably an Fe(III) salt, and the reduction potential of the second oxidizing agent is greater than or equal to +0.50 V, and / or the second oxidizing agent is an I 2 That is, 25. The method according to any one of claims 1 to 24.

26. recovering one or more metals from the first liquid phase; and / or Recovering one or more metals from the second liquid phase. The method of any one of claims 1 to 25, further comprising:

27. 27. The method of any one of claims 1 to 26, further comprising filtering, cleaning and drying the first leached solid material prior to the second leaching step.

28. 1. A method for extracting one or more metals from a solid material, comprising the steps of: (i) a deep eutectic solvent (DES) formed by the reaction of a quaternary ammonium salt with a hydrogen bond donor in a molar ratio of 4:1 to 1:20; and First Oxidant contacting the solid material with a leach solution comprising comprising a leaching step, 13. A method according to claim 12, wherein the reduction potential of the first oxidant is less than or equal to +0.50 V and / or the first oxidant is an Fe(III) salt, a Cu(II) salt, a Te(IV) salt, a Cr(III) salt, or a Mn(VII) salt.

29. a deep eutectic solvent formed by reaction of a first quaternary ammonium salt with a first hydrogen bond donor in a molar ratio of from 4:1 to 1:20; and First Oxidant 1. A composition for leaching one or more metals from a solid material comprising:

1. A composition, wherein the first oxidant has a reduction potential less than or equal to +0.50 V and / or the first oxidant is an Fe(III) salt, a Cu(II) salt, a Te(IV) salt, a Cr(III) salt, or a Mn(VII) salt.

Citation Information

Patent Citations

  • Recovery apparatus of metal, and recovery method of metal

    JP2023022934A

  • Extraction of rare earth elements with deep eutectic solvents

    WO2018167130A1