Magnetic Nanoparticles for Sample Separation

Uniform silica-coated magnetic nanoparticles with controlled aggregation address the aggregation issues of existing technologies, facilitating efficient nucleic acid separation and preparation for diagnostics and sequencing, reducing labor and costs.

JP2024537005APending Publication Date: 2024-10-10AGILENT TECHNOLOGIES INC
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
JP2024516478
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2021-09-30
Filing Date
2022-09-30
Publication Date
2024-10-10

AI Technical Summary

Technical Problem

Existing silica-coated magnetic nanoparticles for nucleic acid purification suffer from ill-defined silica surfaces and aggregation issues, leading to inefficient and labor-intensive sample preparation processes that delay test results and increase costs in diagnostic and research applications.

Method used

The development of uniform silica-coated magnetic nanoparticles with a conformal coating thickness of 1.5 to 2 nm, allowing for the formation of optimally sized clusters through controlled aggregation, enhancing binding efficiency and stability in aqueous dispersions.

Benefits of technology

The solution provides stable, efficient separation and purification of nucleic acids, enabling rapid and reliable sample preparation for diagnostic assays like QRT-PCR and next-generation sequencing, reducing labor and cost by normalizing nucleic acid concentrations for high-throughput sequencing.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024537005000001_ABST
    Figure 2024537005000001_ABST
Patent Text Reader

Abstract

Magnetic nanoparticles and compositions for the simple and reliable production of purified nucleic acids from a variety of sample formats for diagnostic and research applications, as well as methods for their manufacture, are provided. The present invention provides silica-coated magnetic nanoparticles with a high ability to remain dispersed, and a method for producing the silica-coated magnetic nanoparticles, which comprises incubating an aqueous dispersion of the freshly produced particles at room temperature for a period of time to produce clusters of silica-coated magnetic nanoparticles. The resulting clusters are of an optimal size for the extraction of viral RNA from human clinical samples. The magnetic nanoparticles comprise a core and a coating, the core being Fe 3 O 4 or other magnetic material, the coating having a thickness of about 1.5 nm to about 2 nm. The magnetic nanoparticles are useful in preparing nucleic acids for analysis by separating the nucleic acids from other components and normalizing the nucleic acid concentration.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] (CROSS REFERENCE TO RELATED APPLICATIONS) This application claims priority to International Application No. PCT / US2021 / 052974, filed September 30, 2021, with the U.S. Patent and Trademark Office as the receiving office, and is incorporated by reference herein in its entirety.

[0002] The present invention relates to silica-coated magnetic nanoparticles, compositions comprising such magnetic nanoparticles, and techniques for using such magnetic nanoparticles and compositions to separate analytes from biological samples. [Background technology]

[0003] Magnetic particles with various surface modifications are used to separate molecules from biological samples for analysis and processing. The molecules to be analyzed are separated from other components in the sample by binding the desired molecules to the magnetic particles, capturing the particles with the molecules bound to them from the rest of the sample by applying an external magnetic field, washing the particles to remove impurities, and finally recovering the desired molecules with water or a low ionic strength buffer.

[0004] Magnetic particles used for biomolecule separation typically have magnetic iron oxide in their core. Magnetic iron oxide particles are commonly present as magnetite (Fe3O4), maghemite (γ-Fe2O3) or hematite (Fe2O3). Magnetic particles can be coated, for example, with silica, and a wide particle size distribution is expected, ranging from tens or hundreds of nanometers to several microns. Many synthetic methods for making silica-coated magnetic particles result in material with poorly defined (non-uniform) silica surfaces and / or produce large aggregates that settle out of suspension and are difficult to handle. Therefore, it is necessary to mix the particles before and during the protocol to maximize biomolecule binding and recover high purity material.

[0005] More specifically, silica-coated magnetic particles can be used to isolate nucleic acids from biological samples. The first example of the capture of nucleic acids from a sample using silica was presented by Vogelstein [1]. He found that nucleic acids bind tightly to silica glass in the presence of chaotropic salts. The bound nucleic acids could be washed with aqueous organic solvents to remove impurities while remaining bound to the silica. The nucleic acids were then released from the silica upon exposure to low ionic strength buffers. By developing reproducible synthetic methods to make very small or optimally small silica-coated "nanoparticles" (NPs), nucleic acids can be captured on silica surfaces, washed to remove impurities, and eluted with low ionic strength buffers without the attendant problems of aggregation and subsequent precipitation.

[0006] The above nanoparticles NPs can be used for various nucleic acid purification protocols. For example, diagnostic methods can be developed that rely on enrichment of RNA from the SARS-CoV-2 virus, the pathogen of the Covid-19 disease. The resulting RNA can be detected by quantitative reverse transcription polymerase chain reaction (QRT-PCR). Various other viral and bacterial infectious agents, such as Flu-A, Flu-B and Legionella (which causes Legionnaires' disease), respectively, can be detected using various analytical tools once highly purified nanoparticle NP-based nucleic acids are provided.

[0007] Additionally, next-generation sequencing (NGS) protocols can be streamlined, resulting in higher sample throughput, by using nanoparticles NP to adjust each NGS library to the same specific target concentration, called "normalization." Normalizing multiple NGS libraries that vary in concentration allows them to be pooled before loading onto the sequencing instrument. This process allows multiple NGS libraries to be sequenced in a single sequencing run, maximizing data collection and minimizing sequencing instrument costs.

[0008] There are several existing approaches to normalize NGS libraries with varying concentrations. These include nucleic acid quantification by spectrophotometry, fluorimetry, quantitative PCR, or electrophoresis, followed by calculation of the desired concentration, and then diluting all samples to the normalized concentration. Other approaches to nucleic acid normalization include kits sold by companies such as Corning Life Sciences. Corning's "AxyPrep Mag PCR Normalizer" protocol states that 10 μL of bead mixture has a binding capacity for 200 ng of input library DNA. The protocol recommends that "to minimize variability at each data point, the input DNA should be at least 3-4 times more than the desired amount of DNA. For example, if the desired eluted DNA concentration is 2 ng / μL, the input sample should be at least 8 ng / μL." It is very difficult to achieve these amounts of library DNA in a sequencing project, for example 400 ng of DNA from a library recovery volume of 50 μL or a concentration of 200 nM. This is especially true when the DNA used for NGS library synthesis is, by its nature, of poor quality, such as DNA recovered from formalin-fixed, paraffin-embedded (FFPE) samples.

[0009] Agilent Technologies (Santa Clara, CA) currently offers kits for generating next-generation sequencing libraries, such as the "SureSelectXT Target Enrichment System." The SureSelectXT method generates libraries with non-normalized DNA amounts ranging from 10 nM to approximately 50 nM. These DNA amounts are estimated to be too low to use the AxyPrep Mag PCR Normalizer kit.

[0010] The use of nucleic acid-based diagnostics and sequencing in research and medical diagnostics is increasing, but preparation of nucleic acids prior to analysis is a significant cost component for nucleic acid analytical techniques such as real-time PCR, nucleic acid sequencing and hybridization testing. Sample preparation delays test results and limits the ability of laboratories with adequately trained personnel to perform these assays. Current sample preparation processes are laborious, time-consuming and require laboratory capacity.

[0011] There remains a need for magnetic nanoparticles and compositions for simply and reliably producing purified nucleic acids from a variety of sample formats for diagnostic and research applications. [Prior art documents] [Non-patent literature]

[0012] [Non-Patent Document 1] Vogelstein, B. and Gillespie, D., Proc. Nalt. Acad. Sci. USA, vol. 76(2), pp. 615-619, 1979. Summary of the Invention

[0013] In one embodiment of the present invention, a stable aqueous dispersion of magnetic particles is provided. Each individual magnetic nanoparticle is comprised of a magnetic core and a uniform conformal coating surrounding the core. The uniform conformal coating has a thickness of about 1.5 nm to about 2 nm. The average total diameter of the individual uniform conformally coated magnetic nanoparticles is about 10 nm to about 20 nm. In some examples, small clusters of magnetic nanoparticles are formed in the dispersion, with an average cluster size of about 50 to about 190 nm. In some examples, the clusters have an average cluster size of about 10 to about 1000 nm, e.g., about 300 nm, in the dispersion.

[0014] In another aspect of the present invention, a method for preparing silica-coated magnetic nanoparticles is provided. Fe3O4 nanoparticles are provided in an alcohol mixture, and a silicate solution is added while sonicating the mixture. The thickness of the silica coating on the magnetic nanoparticles may be adjusted by varying the amount of silicate added.

[0015] In some examples of using co-precipitation methods to produce Fe3O4 particles, the method excludes oxygen during the Fe3O4 co-precipitation reaction to minimize / eliminate the formation of unwanted Fe2O3. In some examples, the coating thickness is selected to (1) protect the Fe3O4 core from further oxidation to Fe2O3, (2) completely cover the magnetic core, and (3) change the surface chemistry of the resulting core-shell particle to contain a high density of silanol groups (Si-OH) that make the final particle more amenable to binding to nucleic acids. Coating thickness and surface area have been found to be important parameters regarding the use and efficiency of the present magnetic particles for purifying nucleic acids from biological samples.

[0016] In another aspect, methods are provided for maintaining an aqueous dispersion of nanoparticles described herein for a clustering time that results in the formation of stable, optimally sized clusters ("aged" nanoparticles). For example, the nanoparticles can be maintained at room temperature or 20°C-30°C for a clustering time that may be as little as one month, or as little as two, three, four, five, six, seven, or eight months, such that the individual magnetic nanoparticles form clusters having a selected value or range of average cluster size (e.g., diameter). For example, the average cluster size can be at least about 200 nm, or at least about 220 nm, or at least about 235 nm, or at least about 250 nm, or at least about 260 nm, and / or the average cluster size can be at most about 400 nm, or at most about 370 nm, or at most about 350 nm, or at most about 320 nm, or at most about 300 nm, or at most about 290 nm. It is expressly contemplated that any of the above minimum and maximum values ​​may be combined to form a selected range, such as a range of about 200 nm to about 400 nm, or a range of about 250 nm to about 350 nm. Enhanced detection of nucleic acids in human clinical samples is achieved by using aged nanoparticles as compared to "unaged" nanoparticles. In some embodiments, aged nanoparticles form clusters having an average cluster size of about 250 nm, about 255 nm, about 260 nm, about 265 nm, about 270 nm, about 275 nm, about 280 nm, about 285 nm, about 290 nm, about 295 nm, about 300 nm, about 305 nm, about 310 nm, about 315 nm, or about 320 nm, and it is contemplated that any of these values ​​may be combined to form a range. Each of the above approximate values ​​is also contemplated as a disclosure of a specific value and is set forth herein.

[0017] In another aspect, a method for preparing nucleic acids for analysis is provided. The method includes the steps of mixing a sample containing nucleic acids with a binding medium and a magnetic nanoparticle composition as described herein in a container, binding the nucleic acids to the coating of the magnetic nanoparticles, separating the nanoparticles from the liquid in the container by using a magnetic field, removing the liquid from the container and retaining the nucleic acid-bound magnetic nanoparticles in the container, contacting the nucleic acid-bound magnetic nanoparticles with a washing liquid to remove impurities while the magnetic nanoparticles remain attracted to the magnet or while the magnetic nanoparticles remain attracted again by the magnetic field after dispersing the magnetic nanoparticles, and then removing the washing liquid, and finally adding an elution medium to recover the nucleic acids released from the magnetic nanoparticles. The nucleic acids are removed from the container, thereby obtaining a nucleic acid preparation.

[0018] As another aspect of the invention, a method is provided for obtaining RNA from a biological sample and preparing the RNA for analysis. The method includes placing a biological sample containing RNA in a container, the biological sample being a cell or a virus. The biological sample is contacted with guanidine thiocyanate (GTC) and proteinase K to create a sample mixture, and the sample mixture is incubated at an elevated temperature for a sample preparation time. A neat alcohol and a magnetic nanoparticle composition (embodiments described herein) are added to the sample mixture in the container. The method also includes mixing the sample mixture with the magnetic nanoparticles, incubating for a second incubation time, and then applying a magnetic force to separate the magnetic nanoparticles from the supernatant in the container. The supernatant is removed from the container without disturbing the separated magnetic nanoparticles, and the separated magnetic nanoparticles are washed one or more times with an alcohol solution. The separated magnetic nanoparticles are dried, and an elution medium is added to the container and mixed with the magnetic nanoparticles. After an elution time to elute the RNA from the magnetic nanoparticles to create an elution solution, the elution solution is removed from the container.

[0019] These and other features and advantages of the present methods and compositions will become apparent from the following detailed description, taken in conjunction with the appended claims. [Brief description of the drawings]

[0020] [Figure 1A] FIG. 1A illustrates one embodiment for the preparation of silica-coated magnetic nanoparticles according to the present technique. [Figure 1B] FIG. 1B illustrates one embodiment for the preparation of silica-coated magnetic nanoparticles according to the present technique. [Figure 2A] FIG. 2A is an electron micrograph showing individual silica-coated Fe3O4 nanoparticles and the typical cluster size formed by unripened particles in an aqueous dispersion. [Figure 2B] FIG. 2B is an electron micrograph showing individual silica-coated Fe3O4 nanoparticles and the typical cluster size formed by unripened particles in an aqueous dispersion. [Figure 2C] FIG. 2C shows laser diffraction data of silica-coated magnetic nanoparticles according to the present technique. [Figure 2D] FIG. 2D is a TEM image of the silica-coated magnetic nanoparticles prepared in Example 1. [Figure 2E] FIG. 2E is a TEM image of the silica-coated magnetic nanoparticles prepared in Example 1. [Figure 2F] FIG. 2F is a TEM image of the silica-coated magnetic nanoparticles prepared in Example 1. [Figure 2G] FIG. 2G is a TEM image of the silica-coated magnetic nanoparticles prepared in Example 1. [Figure 2H] FIG. 2H is a TEM image of the silica-coated magnetic nanoparticles prepared in Example 1. [Figure 2I] FIG. 2I is a TEM image of the silica-coated magnetic nanoparticles prepared in Example 1. [Diagram 3] Figure 3 shows the full spectrum of silica-coated magnetic nanoparticles by FT-IR spectroscopy. Fe-O stretching vibrations at about 580 cm-1 and Si-O-Si stretching vibrations at about 1100 cm-1 are clearly observed. [Figure 4-1]Figure 4-1 shows a series of IR spectra highlighting the increase in the Si-O to Fe-O peak ratio as the volume of TEOS used in the silica coating process (0.5 ml to 2.5 ml) increases. The higher the Si-O to Fe-O peak ratio signal, the thicker the silica shell formed on the Fe3O4 nanoparticle core. [Figure 4-2] FIG. 4-2 shows a continuation of FIG. 4-1. [Diagram 5] FIG. 5 is a graph showing that the thickness of the silica coating increases linearly with increasing amounts of TEOS. [Figure 6] Figure 6 is a scanning electron microscope (SEM) image of silica-coated magnetic nanoparticles from the present technology at a magnification of 250,000 times. The particles were produced using 1.5 ml of TEOS and ultrasonic treatment. [Figure 7] Figure 7 shows a transmission electron microscope (TEM) image of silica-coated magnetic nanoparticles produced by this technique. Typical Fe3O4 cores range from 7 to 10 nm. The average thickness of the silica coating on the particles was about 1.6 nm when 1.5 ml of TEOS was used. The prominent crystal lattice of Fe3O4 visible inside the core indicates that the nanoparticles were not oxidized during synthesis. [Figure 8A] Figure 8A shows the results of diagnostic quantitative reverse transcription polymerase chain reaction (QRT-PCR). Using manual (Figures 8A-C) and automated (Figures 8D-F) protocols and multiple lots of magnetic silica nanoparticles, viral RNA was recovered from samples and analyzed by diagnostic QRT-PCR. [Figure 8B] Figure 8B shows the results of diagnostic quantitative reverse transcription polymerase chain reaction (QRT-PCR). Using manual (Figures 8A-8C) and automated (Figures 8D-8F) protocols and multiple lots of magnetic silica nanoparticles, viral RNA was recovered from samples and analyzed by diagnostic QRT-PCR. [Figure 8C]Figure 8C shows the results of diagnostic quantitative reverse transcription polymerase chain reaction (QRT-PCR). Using manual (Figures 8A-8C) and automated (Figures 8D-8F) protocols and multiple lots of magnetic silica nanoparticles, viral RNA was recovered from samples and analyzed by diagnostic QRT-PCR. [Figure 8D] Figure 8D shows the results of diagnostic quantitative reverse transcription polymerase chain reaction (QRT-PCR). Using manual (Figures 8A-8C) and automated (Figures 8D-8F) protocols and multiple lots of magnetic silica nanoparticles, viral RNA was recovered from samples and analyzed by diagnostic QRT-PCR. [Figure 8E] Figure 8E shows the results of diagnostic quantitative reverse transcription polymerase chain reaction (QRT-PCR). Using manual (Figures 8A-8C) and automated (Figures 8D-8F) protocols and multiple lots of magnetic silica nanoparticles, viral RNA was recovered from samples and analyzed by diagnostic QRT-PCR. [Figure 8F] Figure 8F shows the results of diagnostic quantitative reverse transcription polymerase chain reaction (QRT-PCR). Using manual (Figures 8A-8C) and automated (Figures 8D-8F) protocols and multiple lots of magnetic silica nanoparticles, viral RNA was recovered from samples and analyzed by diagnostic QRT-PCR. [Figure 9] Figure 9 shows NGS-related "normalization" results. The data presented is electrophoresis and next-generation sequencing data metric validation where normalization as defined below is achieved. [Figure 10] FIG. 10 is a photograph of magnetic separation of silica-coated magnetic nanoparticles from a stable suspension using a small magnet. [Figure 11A] FIG. 11A shows the results of normalization of NGS libraries analyzed by various parameters. [Figure 11B] FIG. 11B shows the results of normalization of NGS libraries analyzed by various parameters. [Figure 11C] FIG. 11C shows the results of normalization of NGS libraries analyzed by various parameters. [Figure 11D] FIG. 11D shows the results of normalization of NGS libraries analyzed by various parameters. [Figure 11E] FIG. 11E shows the results of normalization of NGS libraries analyzed by various parameters. [Figure 11F] FIG. 11F shows the results of normalization of NGS libraries analyzed by various parameters. [Figure 11G] FIG. 11G shows the results of normalization of NGS libraries analyzed by various parameters. [Figure 11H] FIG. 11H shows the results of normalization of NGS libraries analyzed by various parameters. [Figure 11I] FIG. 11I shows the results of normalization of NGS libraries analyzed by various parameters. [Figure 11J] FIG. 11J shows the results of normalization of NGS libraries analyzed by various parameters. [Figure 12A] FIG. 12A shows that the size of the nanoparticle clusters increased upon aging. [Figure 12B] FIG. 12B shows that the size of the nanoparticle clusters increased upon aging. [Figure 13A] FIG. 13A shows that the size of the nanoparticle clusters increased upon aging. [Figure 13B] FIG. 13B shows that the size of the nanoparticle clusters increased upon aging. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0021] The present technology is best understood from the following detailed description when read in conjunction with the accompanying drawings, in which features are not necessarily drawn to scale.

[0022] The silica-coated magnetic nanoparticles (also abbreviated herein as "nanoparticles NP") of the present disclosure are surprisingly effective in isolating nucleic acids from samples. The silica coating provides a hydrophilic matrix, greatly reducing non-specific binding in important applications such as nucleic acid purification.

[0023] In some embodiments, the technique is used to enrich RNA obtained from a cell or viral sample as part of a quantitative reverse transcription polymerase chain reaction (QRT-PCR) detection assay. By way of example, the technique can be used to enrich RNA from SARS-CoV-2 or other viral pathogens prior to detecting the RNA by QRT-PCR. In some embodiments, the technique is used to enrich human RNA, human DNA, and bacterial DNA. For example, the technique may be used to enrich and detect DNA from respiratory pathogens such as Legionella pneumophila (the agent of Legionnaires' disease). In some embodiments, the technique is used to normalize DNA libraries prior to next generation sequencing (NGS). In some embodiments, the technique is used to normalize DNA or RNA samples prior to analysis of the samples.

[0024] Referring to FIG. 1A, the present technology provides a magnetic nanoparticle 100 including a core 10 and a uniform conformal coating 20 on the core 10 that substantially encapsulates the core 10. In one example, the coating 20 completely encapsulates the core 10. The core 10 can be made of a metal, alloy, or metal oxide, and the coating can be made of silica. In one example, the core 10 can be Fe3O4, and the coating includes silica. In one example, the silica coating is substantially non-porous. The ratio of the core diameter to the coating thickness and the properties of the coating surface can be such that the analytes in the sample solution can optimally bind to the coating surface of the magnetic nanoparticles 100, resulting in aggregation of multiple magnetic nanoparticles 100. The magnetic nanoparticles 100 with the analytes bound to the coating surface can then be rapidly removed from the sample solution by applying a magnetic field to the sample solution with the magnetic nanoparticles 100.

[0025] FIG. 1A illustrates one embodiment of the preparation of the magnetic nanoparticles 100. In one example, the magnetic nanoparticles 100 can include a size of about 9 nm to about 40 nm, such as about 20 nm to about 30 nm. The core 10 can include a diameter of about 5 nm to about 20 nm, such as about 7 nm to about 15 nm or less, such as about 10 nm to about 15 nm or less, such as about 8.8 nm or less, about 8 nm or less, or about 7.9 nm. The coating 20 substantially encapsulates the core 10. In some examples, the coating 20 can include a thickness of about 0.5 nm to about 7.5 nm, about 1 nm to about 2 nm, such as about 1.5 nm to about 2 nm. FIG. 1B illustrates a magnetic nanoparticle 100 having a coating thickness of about 2.5 nm and a particle size of about 15 nm.

[0026] As shown in Figures 2A and 2B, the ratio of core diameter to thickness of silica coating 20 in combination with the properties of silica coating 20 allows magnetic nanoparticles 100 to aggregate and form clusters. In one example, the clusters can be about 10 nm to about 1000 nm, such as about 20 nm to about 500 nm, about 100 nm to about 500 nm, about 200 nm to about 500 nm, about 250 nm to about 450 nm, about 275 nm to about 325 nm (e.g. about 300 nm), about 30 nm to about 400 nm, about 40 nm to about 300 nm. Figure 2C shows laser diffraction data measured using a Malvern Panalytical Mastersizer 3000, showing the particle size distribution of nanoparticles NP in a typical aqueous dispersion. Individual particles of clusters up to about 1 micron in diameter are present in the dispersion, with an average cluster size of 128 to 174 nm in diameter. The nanoparticles in this example were "unripe".

[0027] The nanoparticles NPs exhibit high magnetic susceptibility in manual and automated workflows, where timing and efficiency of magnetic particle capture are critical and are particularly desirable in automated platforms that require rapid and quantitative particle recovery during capture, washing and elution steps.

[0028] In some embodiments, the nanoparticle core is composed mostly or entirely of a crystal lattice of Fe3O4. In some embodiments, the nanoparticle core is composed mostly or entirely of nanoscale single crystals of magnetite (Fe3O4) or single domain magnetic nanoparticles of Fe3O4 that exhibit paramagnetic properties.

[0029] In some instances, the nanoparticle NP has a molecular weight of at least 10 2 / g, for example at least about 110m 2 / g ~ approx. 180m 2 / g or at least about 110m 2 / g ~ approx. 130m 2 / g Brunauer-Emmett-Teller (BET) surface area. The BET surface area of ​​the nanoparticles NP can be measured by nitrogen adsorption. For example, nitrogen adsorption / desorption isotherms can be measured at liquid nitrogen temperature (-196 ° C) using a Micromeritics ASAP2020 volumetric adsorption analyzer to measure mesoporosity.

[0030] The silica-coated magnetic nanoparticles described herein can be used directly or functionalized to meet the needs of a particular application. Functional groups such as carboxylate, epoxide, and tosylate can be included or added to the silica coating, and such functional groups can be a convenient method for covalent functionalization. As a further example, the silica coating can be modified by incorporating one or more types of organic groups into the silica matrix. The organic groups can covalently functionalize the surface and / or pores of the silica coating. As another example, polymers can functionalize the silica surface by simple coating or covalent bonding.

[0031] The coating of the silica magnetic nanoparticles described herein can include pores that extend to the surface of the magnetic nanoparticle. The coating can be modified with functional groups both inside and outside the pores. In some examples, the coating further includes reactive chemical moieties that are configured to bind to analytes such as nucleic acids.

[0032] The present technology provides a composition that can include a plurality of magnetic nanoparticles as described herein. The plurality of magnetic nanoparticles has an average particle size of about 15 nm or less, or about 12 nm or less, or about 11 nm or less. The composition is a stable suspension of the magnetic nanoparticles in a liquid medium, such as water. In some examples, the magnetic nanoparticles are present in the stable suspension at a concentration of 3-30 g / L, or 10-20 g / L, or about 13 g / L.

[0033] In some examples, the nanoparticles remain suspended at a temperature of 25° C. for at least 6 months, or at least 9 months. In some examples, the nanoparticles are held for an aggregation time before being used, shipped to a user, or sold for general or specific use. The aggregation time is selected so that the nanoparticles form clusters of a desired size or characteristics. Exemplary aggregation times include at least about 1 month, at least about 2 months, at least about 3 months, at least about 4 months, at least about 6 months, at least about 8 months, or more. Alternatively, exemplary aggregation times include at least about 18 months, at least about 12 months, at least about 10 months, at least about 8 months, at least about 6 months, at least about 5 months, or less. It is contemplated that any of the above minimum and maximum values ​​can be combined to form a range, provided that the minimum value is less than the maximum value. In some examples, a general use is to separate an analyte, such as RNA, from a sample. In some examples, a specific use is to normalize the amount of nucleic acid obtained from a sample.

[0034] The present technology also includes stable suspensions that the magnetic nanoparticles are packaged in. The magnetic particles or compositions described herein can be provided in a sealed package whose internal volume is an aqueous suspension of the nanoparticles.

[0035] The present technology provides a method for producing silica-coated magnetic nanoparticles. The present method for producing silica-coated magnetic nanoparticles involves the addition of a base (e.g., ammonia or NaOH) at room temperature under an inert atmosphere to form Fe 3+ / Fe 2+ The synthesis of magnetic iron oxide from aqueous salt solutions involves the synthesis of Fe3O4 particles using a co-precipitation method. The size, shape and composition of the magnetic nanoparticles depend on the type of salt used (e.g. chloride, sulfate, nitrate), Fe 3+ / Fe 2+ The ratio of Fe+ to FeO+ depends on the reaction temperature and pH value. If the synthesis conditions are kept constant, the final properties of the synthesized magnetite nanoparticles are completely reproducible. The advantages of this technique in the formation of Fe3O4 nanoparticles include rapid particle formation, use of inexpensive solvents, magnetic separation for product isolation, controlled particle size and morphology, reproducible magnetic properties, and the ability to synthesize nanoparticles on a larger industrial scale. In some examples, the concentration of Fe+ used in the coprecipitation method is less than 0.1M, or less than 0.05M, or less than 0.02M, e.g., 0.01M.

[0036] The method was as follows: 3+ / Fe 2+ Fe with a molar ratio of about 2 / 1 3+ and Fe 2+ In some instances, the aqueous solution of Fe ions is 3+ The concentration of Fe in the aqueous solution is about 2 to about 50 mM. 2+The concentration of is about 1 to about 25 mM. The aqueous solution can be prepared by dissolving FeCl3 and FeCl2 in deionized, deoxygenated water, although other iron salts can be used for dissolution. The water can be deoxygenated by any suitable technique, such as sparging with an inert gas, sonication, and / or stirring for a sufficient deoxygenation time prior to mixing the water with the iron salt. The deoxygenation time is generally at least 2 hours, although longer or shorter times may be used.

[0037] Fe 3+ and Fe 2+ The aqueous solution of ions may be further sonicated and optionally adjusted to about 35° C. (e.g., by heating the aqueous solution from room temperature). A base may be added to the heated aqueous solution under an inert atmosphere. In some examples, suitable bases include ammonia, sodium hydroxide, and the like. The base is added in an amount sufficient to form Fe3CO4 cores from the aqueous solution. For example, the base may be added in a molar excess of 2-fold or more (e.g., 4-fold or 8-fold). As a result of adding a sufficient amount of base, a mixture including Fe3CO4 nanoparticles and alkaline water is formed. In some examples, the base may be added dropwise to the aqueous solution, optionally while stirring and / or sonicating the aqueous solution.

[0038] The mixture is maintained under an inert atmosphere without stirring for a settling time during which the Fe3O4 nanoparticles settle out of the alkaline water. In some examples, the settling time is overnight or about 12 hours. In other examples, the settling time is at least 4, 6, 8, 12, or 18 hours, and / or is no more than 60, 48, 36, 24, or 20 hours. The above values ​​can be combined to create a range of settling times. After the settling time, most of the alkaline water is removed from the mixture by suction. This results in a concentrated mixture of Fe3O4 nanoparticles in alkaline water.

[0039] A deoxygenated alcohol is added to the concentrated mixture to create an aqueous alcohol mixture. The aqueous alcohol mixture is stirred and sonicated to suspend the Fe3O4 nanoparticles. In some instances, additional base is added to the aqueous alcohol mixture prior to further processing.

[0040] The silicate solution is added to the aqueous alcohol mixture while sonicating and maintaining an inert atmosphere. The silica coating thickness can be controlled by the amount of reactants used. The silicate solution may be added dropwise slowly to the aqueous alcohol mixture, for example over 30-90 minutes, while the mixture is stirred and sonicated. The silicate solution includes tetraethyl orthosilicate (TEOS) and an alcohol. In some examples, the silicate solution is anhydrous.

[0041] The mixture is stirred under an inert atmosphere for a coating time during which a silica coating forms on the Fe3O4 nanoparticles. In some examples, the coating time is overnight or about 12 hours. In other embodiments, the coating time is at least 4, 6, 8, 12, or 18 hours, and / or is no more than 60, 48, 36, 24, or 20 hours. The above values ​​can be combined to create a range of coating times.

[0042] The silica-coated Fe3O4 nanoparticles are separated from the alcohol-aqueous mixture by any suitable separation technique. In some examples, the Fe3O4 nanoparticles are separated from the aqueous-alcohol mixture by magnetic capture. The silica-coated Fe3O4 nanoparticles can be washed with methanol or other alcohol or solvent. The separated silica-coated Fe3O4 nanoparticles can be dried, for example, by vacuum drying. A powder of silica-coated Fe3O4 nanoparticles is formed by drying. In some examples, a powder including silica-coated Fe3O4 nanoparticles is formed without grinding or mechanically separating the nanoparticles.

[0043] The resulting dried nanoparticles may be dispersed in deoxygenated water to form a composition. In some instances, the composition is a stable suspension. The resulting particle suspension may be aged for up to six months to allow the average cluster size of the nanoparticles to increase from an average of 125 nm to 260 nm.

[0044] The technology also includes a method for preparing nucleic acids for analysis by isolating the nucleic acids from a sample. In some examples, the method includes mixing a sample containing nucleic acids with a binding medium and a magnetic nanoparticle composition described herein in a container. The nucleic acids bind to the coating of the magnetic nanoparticles. After a binding time, the nucleic acid-bound magnetic nanoparticles are separated from the binding medium in the container. The nucleic acid-bound magnetic nanoparticles are contacted with a wash solution to remove unwanted impurities and then with an elution medium, thereby separating the bound nucleic acids from the magnetic nanoparticles. The magnetic nanoparticles are attracted by a magnet, and the resulting clarified solution containing the desired nucleic acids is removed from the container, thereby obtaining a nucleic acid preparation.

[0045] The magnetic nanoparticles and compositions described herein have many uses, such as for the separation of analytes, such as small molecules, proteins, and / or nucleic acids from biological samples. The magnetic nanoparticles and compositions may be used as carriers for chemical or biological species, including, for example, precious metal particles, small organic or inorganic molecules, DNA, peptides or polypeptides (e.g., antibodies and other proteins), and whole cells. Applications for such carriers may include magnetic resonance imaging (MRI), optical imaging, targeted drug delivery, and cell delivery.

[0046] The present technology provides a method for preparing nucleic acids for analysis. The method includes mixing a sample containing nucleic acids with a binding medium and a magnetic nanoparticle composition described herein in a container. The nucleic acids bind to the coating of the magnetic nanoparticles. After a binding time, the nucleic acid-bound magnetic nanoparticles are separated from the binding medium in the container. In some examples, the nucleic acid-bound magnetic nanoparticles are then washed with a washing medium that includes aqueous alcohol or various water-miscible organic solvents, such as acetonitrile, acetone, and sulfolane. Most of the liquid (binding medium and / or washing medium) is then removed from the container, taking care to retain the nucleic acid-bound magnetic nanoparticles in the container. The nucleic acid-bound magnetic nanoparticles are contacted with an elution medium, thereby separating the bound nucleic acids from the magnetic nanoparticles. The nucleic acids are removed from the container, thereby obtaining a nucleic acid preparation.

[0047] The coating of the magnetic nanoparticles may include binding sites configured to selectively bind to a nucleic acid or another analyte.

[0048] The isolation of nucleic acids from a sample is illustrative of the case when other analytes, for example small molecules such as pharmaceuticals, proteins or polypeptides, lipids, or other analytes, may be isolated.

[0049] The method may be used to normalize the amount of nucleic acid obtained from a sample, where the sample comprises an input amount of nucleic acid and the magnetic nanoparticle composition has binding capacity for an output amount of nucleic acid, the output amount being less than the input amount.

[0050] The magnetic nanoparticle composition may have a normalization factor of 0.8 to 1.2, where the normalization factor refers to the concentration value of nucleic acid recovered from the magnetic silica nanoparticles after exposure to a high concentration of nucleic acid divided by the concentration value of nucleic acid recovered from the magnetic silica nanoparticles after exposure to a low concentration of nucleic acid. Ideally, for compositions prepared for NGS, the normalization factor is approximately 1.0.

[0051] The nucleic acid preparation comprises a nucleic acid having a length within a predetermined length range. In some examples, the minimum nucleotide length is 50 nucleotides (hereinafter, nt), or 70 nt, or 75 nt, or 80 nt, or 100 nt, or 150 nt, or 200 nt, or 500 nt, or 2,000 nt, or 5,000 nt, or 10,000 nt, or 50,000 nt, or 100,000 nt. The maximum nucleotide may be 2 million nt, or 1 million nt, or 500,000 nt, or 200,000 nt, or 75,000 nt, or 25,000 nt, or 12,500 nt, or 6,000 nt, or 3,000 nt, or 1,500 nt, or 750 nt, or 400 nt, or 250 nt. Any of the above minimum and maximum values ​​can be combined to form a desired nucleotide length range, provided that the minimum value is less than the maximum value.

[0052] The method may be used where the input sample contains small amounts of nucleic acid, for example less than 1,000 ng, or less than 500 ng, or less than 200 ng, or less than 100 g, or less than 50 ng.

[0053] The present technology provides a method for obtaining RNA from a biological sample and preparing the RNA for analysis. In this method, a biological sample containing RNA is placed in a container. The biological sample may be a cell or a virus.

[0054] The method includes contacting the biological sample with guanidine thiocyanate (GTC) and proteinase K to form a sample mixture and incubating for a sample preparation time (e.g., up to 10 minutes or about 5 minutes) at an elevated temperature (e.g., about 60° C.). The GTC and proteinase K may be added separately or may be premixed and added together. After the sample preparation time, neat alcohol is added to the sample mixture in the container, and one of the magnetic nanoparticle compositions described herein is also added to the sample mixture in the container. The sample mixture and the magnetic nanoparticles are mixed and incubated for a second incubation time (e.g., up to 10 minutes or about 5 minutes).

[0055] After the second incubation period, a magnetic force is applied to separate the magnetic nanoparticles from the supernatant in the container. The supernatant is removed from the container without disturbing the separated magnetic nanoparticles, and the magnetic nanoparticles are washed one or more times with an alcohol solution. A suitable alcohol solution may contain 80% v / v or more lower alcohols, such as methanol, ethanol, n-propanol, isopropanol, or mixtures thereof. A variety of non-alcoholic organic solvents that are miscible with water are also effective for washing purposes and are known to those skilled in the art. Some of these include, but are not limited to, acetonitrile, acetone, and sulfolane. The separated magnetic nanoparticles are dried, and an elution medium is added to the container. The magnetic nanoparticles are mixed with the elution medium for an elution time (e.g., less than 10 minutes), and then the RNA is eluted from the magnetic nanoparticles to create an eluate. The eluate containing the RNA is removed from the container, and the RNA may then be subjected to analysis, such as quantitative reverse transcription polymerase chain reaction (QRT-PCR) for diagnostic and research purposes, or may be modified to serve as a substrate for nucleotide sequencing, such as Sanger and NGS sequencing. Alternatively, the removed eluate may be placed in a second container and sealed and stored at low temperature, such as for shipment or subsequent analysis.

[0056] In some examples, one, some or all steps of the above method are performed by an automated device.

[0057] (term) It should be understood that the terminology used herein is for the purpose of describing particular embodiments only, and is not intended to be limiting. Defined terms are in addition to the technical and scientific meaning of the defined terms as commonly understood and accepted in the art of the present disclosure.

[0058] The terms "nucleic acid" and "polynucleotide" are used interchangeably herein to describe a polymer of any length, e.g., greater than about 10 bases, greater than about 100 bases, greater than about 500 bases, greater than 1000 bases, greater than 10,000 bases, or more, composed of nucleotides, e.g., deoxyribonucleotides or ribonucleotides, or a synthetically produced compound capable of sequence-specific hybridization with a naturally occurring nucleic acid, e.g., capable of participating in Watson-Crick base pairing interactions, as well as, e.g., two naturally occurring nucleic acids. Naturally occurring nucleotides include guanine, cytosine, adenine, thymine, and uracil (G, C, A, T, and U, respectively).

[0059] The terms "complementarity," "complementary strand," or "complementary nucleic acid sequence" refer to a nucleic acid strand that is related to the base sequence of another nucleic acid strand by Watson-Crick base pairing rules. In general, two sequences are complementary if one sequence can hybridize in an antiparallel sense to the other sequence, such that the 3' end of each sequence hybridizes to the 5' end of the other sequence and each A, T / U, G, and C of one sequence aligns with each T / U, A, C, and G of the other sequence.

[0060] The term "duplex" refers to at least two sequences that undergo Watson-Crick base pairing in a fully or partially complementary manner to form a stable complex between all or most of their nucleotides. The terms "annealing" and "hybridization" are used interchangeably to refer to the formation of a stable duplex.

[0061] In the context of nucleotide sequences, the terms "hybridization" and "hybridization" are used interchangeably herein. The ability of two nucleotide sequences to hybridize to each other is based on the degree of complementarity of the two nucleotide sequences, which in turn is based on the proportion of matched complementary nucleotide pairs. The more nucleotides in a given sequence that are complementary to another sequence, the more stringent the hybridization conditions are, and the more specific the hybridization of the two sequences is. Higher stringency can be achieved by increasing the temperature, increasing the proportion of cosolvent, decreasing salt concentration, etc.

[0062] As used herein and in the appended claims, and when given its ordinary meaning, the terms "substantial" or "substantially" mean within the limits or degree acceptable to one of ordinary skill in the art. For example, "substantially canceled" means that one of ordinary skill in the art would consider the cancellation acceptable.

[0063] As used herein and in the appended claims, and when added to its ordinary meaning, the terms "approximately" and "about" mean within acceptable limits or amounts to one of ordinary skill in the art. The term "about" generally refers to ±15% of the stated number. For example, "about 10" can indicate a range of 8.5 to 11.5. For example, "about the same" means that the compared items would be considered the same by one of ordinary skill in the art.

[0064] In this disclosure, numerical ranges are inclusive of the numbers defining the range. It should be recognized that chemical structures and formulas may be extended or expanded for illustrative purposes.

[0065] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as commonly understood by those working in the field to which this disclosure belongs.

[0066] Before various embodiments are described, it should be understood that the technology of the present disclosure is not limited to the particular embodiments described, and as such may vary. It should be understood that the terminology used herein is for the purpose of describing particular embodiments only, and is not intended to be limiting, since the scope of the present disclosure will be limited only by the appended claims.

[0067] As disclosed herein, a number of ranges of values ​​are provided, and unless clearly contrary by context, it is understood that each intervening value, to the tenth of the unit of the lower limit, between the upper and lower limits of that range is also specifically disclosed.

[0068] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as commonly understood by one of ordinary skill in the art to which this disclosure belongs. Although any methods and materials similar or equivalent to those described herein may also be used in the practice or testing of the present technology, some exemplary methods and materials are described herein.

[0069] All patents and publications mentioned herein are expressly incorporated by reference.

[0070] As used in this specification and the appended claims, the terms "a," "an," and "the" include singular and plural referents unless the context clearly dictates otherwise. Thus, for example, "a moiety" includes one moiety and multiple moieties. EXAMPLES

[0071] Example 1 In this example, silica-coated magnetic nanoparticles (nanoparticles NP) are produced using the methods described above and below. An exemplary procedure for the synthesis of Fe3O4 nanoparticles on a 1 g scale was carried out as follows: 400 ml of DI water was thoroughly deoxygenated for 2 hours using hard N2 purging, mechanical stirring and sonication. After deoxygenation, 2.508 g of FeCl3 (9.24 mM) and 0.919 g of FeCl2 (4.62 mM) were added under nitrogen atmosphere and further purging / sonication was performed. During the course of sonication, the temperature of the water increased to 35°C. Then, 10 ml of 28% ammonia solution (0.18 M, which is about 4 molar excess required to completely convert iron to magnetite) was quickly added to the rapidly stirred and sonicated solution. The solution immediately turned black and precipitation of nanoparticles was observed. The sonication was stopped and the mixture was stirred under nitrogen atmosphere for an additional 4 hours. The particles were then left under nitrogen atmosphere without stirring until the next day. The nanoparticles settled to the bottom of the flask, resulting in a clear top aqueous layer and a black bottom layer consisting of magnetic Fe3O4 nanoparticles.

[0072] The next day, the precipitated Fe3O4 nanoparticles were isolated by aspirating off the clear top layer of ammonia / water. The remaining solvent (100 ml) was left behind. 300 ml of deoxygenated ethanol was then added to this black slurry. The particles were stirred and sonicated for 1 hour to resuspend the nanoparticles. While sonicating, 1.5 ml of TEOS was mixed with 80 ml of absolute ethanol, placed in a dropping funnel under a nitrogen purge and attached to the flask. The flask was purged under a stream of N2 and then sealed. An additional 5 ml of ammonia solution (28%) was then added to this black nanoparticle suspension. The mixture was sonicated again and mechanically stirred for 10 minutes under a stream of nitrogen. The TEOS solution was then added dropwise to the stirred and sonicated nanoparticles over approximately 60 minutes. After addition of the TEOS solution, slow stirring was continued overnight under N2.

[0073] The next day, a magnet was used to separate the nanoparticles at the bottom of the flask. The clear ethanol / water mixture was decanted away from the nanoparticles held in place by the magnet. The silica-coated Fe3O4 nanoparticles were washed twice with fresh methanol and magnetically separated. The nanoparticles were then dried under a stream of nitrogen to a powder and then dispersed in 100 ml of deoxygenated water. The nanoparticles were thoroughly sparged with nitrogen, sonicated, and sealed under an inert atmosphere to yield a 1.3 wt% aqueous solution of nanoparticles.

[0074] Silica-coated Fe3O4 nanoparticle samples were isolated as dry particles for various analyses. Scanning electron microscopy (SEM) was used to image the particles and estimate the degree of aggregation and overall size of individual particles. Figures 2A-2B are scanning electron microscopy (SEM) images of silica-coated magnetic nanoparticles from the present technique. Figure 2C shows laser diffraction data of silica-coated magnetic nanoparticles from the present technique.

[0075] The use of current techniques, including sonication during synthesis, helps disperse the nanoparticle cores, thereby allowing for a uniform silica coating to occur and preventing premature particle aggregation. SEM estimates indicate that the final silica-coated Fe3O4 nanoparticles are 10-15 nm in diameter. This suggests that the coating structure on the core consists of internal Fe3O4 nanoparticles approximately 7-10 nm in diameter incorporating a uniform external silica shell approximately 1.5 nm thick. These sizes were confirmed using high-resolution TEM.

[0076] Examples 1-1, 1-2, and 1-3 were prepared using the above technique with different amounts of TEOS solution. The silica-coated Fe3O4 nanoparticles were analyzed by IR and TEM and found to have very desirable size characteristics and SiO:FeO ratios. Figures 2D and 2E are TEM images of Example 1-1, Figures 2F and 2G are TEM images of Example 1-2, and Figures 2H and 2I are TEM images of Example 1-3. The following table shows the average shell thickness and average core particle size of each of these examples.

[0077] [Table 1] In the above table, the amount of TEOS used in the reaction is shown in volume and equivalent amount. The ratio of SiO to FeO in the resulting silica-coated nanoparticles was determined by IR analysis. The shell thickness and core particle size were determined based on TEM analysis.

[0078] Analysis of dried silica-coated Fe3O4 nanoparticles using Brunauer-Emmett-Teller (BET) theory showed that 105m 2 / g, e.g., 113-127 m2 / g, which is in good agreement with the estimated diameter of the particles. Analysis of the nanoparticles was performed using FT-IR spectroscopy both before and after functionalization with a silica shell. FT-IR analysis of the uncoated Fe3O4 nanoparticles showed a 580 cm -1 and 630 cm -1 Two overlapping bands at 3400 cm−1 were observed, which are associated with the metal-oxygen Fe–O stretching vibrations of the crystal lattice of the Fe3O4 magnetic phase. After coating the nanoparticles with silica, these bands also contain a band at 3400 cm−1 originating from the OH and Si–O stretching of the silica in the SiO2 shell. -1 , 1094cm -1 , and 467 cm -1 (See Figure 3.) The emergence of new modes confirms the encapsulation of the nanoparticles by a thin shell of silica.

[0079] Two other batches of silica-coated nanoparticles were prepared in the same manner as in Example 1-1 and the coating thickness was evaluated. As shown in the table below, this procedure resulted in silica-coated nanoparticles with very consistent coating thickness and little batch-to-batch variability.

[0080] [Table 2] Example 2 In this example, silica-coated nanoparticles were prepared according to the procedure described in Example 1, except that different amounts of silicate were used in the procedure. The following table summarizes the five different embodiments of magnetic nanoparticles prepared in this example.

[0081] [Table 3]

[0082] [Table 4] The silica-coated magnetic nanoparticles were analyzed by FT-IR. Figures 4-1 and 4-2 show the spectra. The particles of various embodiments have different silica coating thicknesses. IR analysis showed that the silica coating thickness increases linearly with increasing TEOS amount.

[0083] FIG. 5 is a graph showing that silica coating thickness increases linearly with increasing amounts of TEOS.

[0084] Figure 6 is a scanning electron microscope (SEM) image of silica-coated magnetic nanoparticles from the present technology at a magnification of 250,000 times. The particles were produced using 1.5 ml of TEOS and ultrasonic treatment.

[0085] Figure 7 shows a transmission electron microscope (TEM) image of silica-coated magnetic nanoparticles produced by this technique. Individual silica-coated magnetic nanoparticles are visible. Particle agglomerations are also visible. Typical Fe3O4 cores are in the range of 7-10 nm. The average thickness of the silica coating on the particles was about 1.6 nm when 1.5 ml of TEOS was used. Inside the core, the Fe3O4 crystal lattice is visible, indicating that the nanoparticles were not oxidized during synthesis or transport.

[0086] Example 3 In this example, several lots of silica-coated magnetic nanoparticles were prepared based on the procedure described in Example 1, thereby producing Examples 3-1 to 3-14. The surface area of ​​some of these examples was measured by Brunauer-Emmett-Teller (BET) surface area and was approximately 113 m 2 / g ~ approx. 127m 2 / g.

[0087] [Table 5] Example 4 In this example, RNA was recovered from samples using the magnetic nanoparticles of the present disclosure in both manual and automated protocols. In these methods, 75 μL aliquots of biological samples containing RNA were pipetted into 0.2 ml strip tubes. 75 μL of guanidine thiocyanate (GTC) containing lysis buffer and 2 μL of proteinase K (20 mg / ml) were added to each tube. The tubes were capped, mixed by vortexing, and rotated. The tubes were incubated at 60° C. for 5 minutes. After incubation, 75 μL of 100% EtOH was added to each tube along with 2 μL of magnetic nanoparticles having a particle size of 10.38 nm based on a core particle size of 8.82 nm and a coating thickness of 1.56 nm. The tubes were capped, mixed, briefly rotated, and incubated at room temperature for 5 minutes. During this second incubation period, the RNA from the samples was bound to the silica-coated magnetic nanoparticles.

[0088] After the second incubation period, the tube was placed on a magnet for 5 minutes. All supernatant was then removed from the tube without disturbing the nanoparticle pellet. 200 μL of washing medium (80% EtOH) was added to the pellet in the tube. The washing medium was removed without disturbing the nanoparticle pellet, and the washing and removal steps were repeated. The nanoparticle pellet was incubated at room temperature for 3 minutes to dry the nanoparticles.

[0089] Then, 75 μL of elution medium preheated to 65 °C was added to the tube and pipetted up and down several times to mix the nanoparticles while avoiding the generation of air bubbles. The tube was left for 2 min, the nanoparticles were captured by a magnet, and the eluate containing the RNA was collected and transferred to a new tube. The new tube was capped and placed on ice.

[0090] Example 5 In this example, RNA was recovered from samples using the magnetic nanoparticles of the present disclosure using a manual protocol. Figure 8A shows a comparison of six nanoparticle (nanoparticle NP) lots for viral RNA extraction using the manual workflow.

[0091] Final concentrations of SARS-CoV-2 N1 and N2 targets were 10 per microliter 5 , 10 4 , 10 3 , 10 2 Contrived samples were prepared by spiking SARS-CoV-2 armored synthetic RNA into nasal swabs (NS) collected in VTM at 1, 10, 1 and 0.5 copies. RNA extraction was performed using 75ul of each dilution in duplicate according to the NAP manual protocol. Briefly, 75ul of each sample was mixed with 75ul of lysis buffer and 2ul of proteinase K, incubated at RT for 5 min and 60°C for 5 min, then 75ul of 100% ethanol containing 2ul of nanoparticle beads was added. The following six nanoparticle lots were used in this experiment: Example 3-3, Example 3-5, Example 3-6, Example 3-7, Example 3-8, and Example 3-9. Samples were mixed and incubated at RT for 5 min to allow the nucleic acids to bind to the magnetic beads, then the tubes were transferred to a magnetic stand and the beads were collected at the bottom side of the tube (RNA remains bound to the magnetic beads at this step). After aspirating the supernatant, the beads were washed twice with 80% ethanol, dried for 3 min at RT, and RNA was eluted with 30 ul of low TE buffer (10 mM Tris, 0.1 mM EDTA, pH 8.0).

[0092] Five ul of each extracted RNA sample was used in a multiplex QRT-PCR reaction using primers and probes specific for SARS-CoV-2 N1 and N2 targets and the human RNase P gene. The assay was performed on an Agilent AriaMx Real-Time PCR System. The amplification curves for N1, N2 and RP targets are shown in Figure 8A, Figure 8B and Figure 8C, and the corresponding Cq values ​​are shown in Tables A, B and C. No significant differences were observed among the six nanoparticle lots, with a 10 5 QRT-PCR detection of SARS-CoV2 N1 and N2 RNA targets and human RP at ~0.5 copies / ul was demonstrated.

[0093] [Table 6]

[0094] [Table 7]

[0095] [Table 8] Example 6 In the following examples, the magnetic nanoparticles of the present disclosure were used to recover RNA from samples in an automated protocol. Figures 8D, 8E, and 8F show a comparison of six nanoparticle lots for viral RNA extraction using an automated workflow.

[0096] Final concentrations of SARS-CoV-2 N1 and N2 targets were 10 per microliter 5 , 10 4 , 10 3 , 10 2Artificial samples were prepared by spiking SARS-CoV-2 armored synthetic RNA into nasal swabs (NS) collected in viral transfer medium (VTM) at 10, 1, and 0.5 copies. RNA extraction was performed using 75 ul of each dilution. Briefly, 75 ul of each sample was mixed with 75 ul of lysis buffer and 2 ul of proteinase K, incubated at RT for 5 min, and then transferred to the Bravo instrument for automated processing. The following nanoparticle lots were used in this experiment: Example 3-2, Example 3-3 (from two different vials, referred to as 3-3a, 3-3b), Example 3-4, Example 3-5, and Example 1-1B. RNA was eluted with 30 ul of low TE buffer (10 mM Tris, 0.1 mM EDTA, pH 8.0).

[0097] Five ul of each extracted RNA sample was used in a multiplex QRT-PCR reaction using primers and probes specific for SARS-CoV-2 N1 and N2 targets and the human RNase P gene. The assay was performed on an Agilent AriaMx Real-Time PCR System. The amplification curves for N1, N2 and RP targets are shown in Figure 8D, Figure 8E and Figure 8F, and the corresponding Cq values ​​are shown in Tables D, E and F. No significant differences were observed among the six nanoparticle lots, with a 10 5 QRT-PCR detection of SARS-CoV2 N1 and N2 RNA targets and human RP at ~0.5 copies / ul was demonstrated.

[0098] [Table 9]

[0099] [Table 10]

[0100] [Table 11] Example 7 In this experiment, the effect of nanoparticle NP aging on the average cluster size was evaluated. Figures 12A and 12B show the increase in cluster size upon aging of a nanoparticle composition of the present disclosure up to 218 days. Table H shows the values ​​measured at the indicated time points.

[0101] [Table 12] 13A and 13B show another experiment demonstrating the increase in cluster size upon aging another nanoparticle composition of the present disclosure out to 109 days. Table I shows the values ​​measured at the indicated time points.

[0102] [Table 13] These experiments show that the nanoparticle mode size increases over time as the clusters plateau at about 300 nm, and more specifically, at about 260 nm. Nanoparticle compositions containing clusters of this size were used in exemplary RNA isolation / QRT-PCR assays and NGS normalization.

[0103] Example 8 In this example, the effect of nanoparticle NP aging on nucleic acid extraction efficiency was evaluated by comparing QRT-PCR analysis of RNA isolated using 2-week and 14-week old nanoparticle NP. Nucleic acids were extracted from 14 nasopharyngeal (nanoparticle NP) clinical samples, of which 8 had been found to be positive for human metapneumovirus (hMPV) and 6 for human parainfluenza virus type 3 (hPIV3). The amount of extracted viral RNA was assessed by QRT-PCR on an AriaMx Real-Time PCR system using Brilliant III QRT-PCR reagents, ABI TaqMan Microbiology Assays (primers and probes for detecting hMPV or hPIV3) and 2 μl of each RNA sample in a 20 μl PCR reaction. Results were analyzed using AriaMx v1.5 software (ΔCq values ​​for each sample were calculated as [ΔCq=Cq2 weeks-Cq14 weeks]). The data are shown in the table below.

[0104] As shown in Table G, 10 of 14 samples (71%) extracted with 14-week-old NPs showed an improvement of more than 0.5 Cq (ΔCq1 = 3-fold difference in RNA yield).

[0105] [Table 14] This experiment demonstrated that the 14 week old nanoparticle NP composition (the "mature" nanoparticle NP composition) provided significant improvements in viral RNA yields from clinical samples as measured by QRT-PCR.

[0106] Example 9 In the following examples, DNA samples for NGS, which have different concentrations and are referred to as "libraries," were "normalized," meaning that all DNA concentrations obtained after normalization are approximately equal, regardless of the DNA concentration to which the magnetic silica nanoparticles were exposed.

[0107] All the following steps were performed at 4°C.

[0108] Add 10 µL of magnetic nanoparticles (0.1 µg / mL; 1 µg) and 60 µL of DNA binding medium to tubes A1-H1 (nanoparticle lot CS-019A) and A2-H2 (nanoparticles CS-019B) and mix by pipetting.

[0109] Add 20 µL of the 10 nM DNA library to tubes A1-D1 and tubes A2-D2, add 20 µL of the 100 nM DNA library to tubes E1-H1 and tubes E2-H2, mix by pipetting, and immediately capture the particles.

[0110] The captured particles are washed once with 150 μL of 80% EtOH, the supernatant is removed, the particles are dried, 10 μL of 10 mM Tris-0.1 mM EDTA (pH 8.0) is added, mixed, the particles are immediately captured, and the supernatant is subjected to electrophoretic analysis (HSD1000 TapeStation).

[0111] Figure 9 shows the results of the TapeStation analysis. Despite using different concentrations of nucleic acids in the DNA libraries as input for the normalization method, the normalization factor was 1.1 for CS-019A and 1.0 for CS-019B. The average DNA concentrations in tubes A1-D1 and E1-H1 (CS-019A) were 9.4 nM and 10.4 nM, respectively. Dividing 10.4 by 9.4 gives a normalization factor of approximately 1.1. The average DNA concentrations in tubes A2-D2 and E2-H2 (CS-019B) were 9.8 nM and 9.7 nM, respectively. Dividing 9.8 by 9.7 gives a normalization factor of approximately 1.0.

[0112] Example 10 In this example, DNA samples (or libraries) for NGS with different concentrations were normalized. This example further shows that NGS protocols can be improved by normalizing nucleic acid libraries with varying concentrations using nanoparticles NP, resulting in higher sample throughput and reduced sequencing time and costs. NGS instrument platforms generally require a specific concentration of nucleic acid to be loaded onto the sequencing instrument. If the concentration is too low or too high, the output and quality of the sequence data will be reduced. There are several existing approaches to normalize nucleic acids for NGS with varying concentrations. These include nucleic acid quantification by spectrophotometry, fluorometry, quantitative PCR, or electrophoresis, followed by calculation of the desired concentration and further dilution of all samples to the normalized concentration. The following NGS data comparison shows that the quality of nanoparticle NP normalization is equal or better than that of electrophoresis (Agilent TapeStation instrument).

[0113] The normalization procedure described in Example 8 was used with silica-coated magnetic nanoparticles prepared according to Example 1 (nanoparticle lot CS-019).

[0114] The results are shown in Figures 11A-11J. In these figures, BN refers to the nanoparticle NP normalized library and TS refers to the TapeStation normalized library. Figure 11A shows the results of the TapeStation analysis.

[0115] Figure 11B shows "bam counts", which are the number of sequence reads that mapped to each targeted feature, such as genes, exons, transcripts, etc. Bam counts were lower but more uniform in the nanoparticle NP-normalized library compared to the TS-normalized library.

[0116] FIG. 11C shows the complexity of the normalized libraries, which reflect the amount of bias introduced by a given experimental design. In terms of library complexity, the ideal is a highly complex library that faithfully reflects the original complexity of the raw material. Nanoparticle NP normalization and TS normalization yielded equal complexity, as indicated by the nearly equal coefficients of variation. The nanoparticle NP normalized and TS normalized libraries are equally complex.

[0117] Figure 11D shows the uniformity of the normalized libraries, which is the percentage of target base positions where the read depth exceeds the average regional target coverage depth a specified number of times. The nanoparticle NP normalized libraries were more uniform than the TS normalized libraries.

[0118] FIG. 11E shows the coverage of the normalized library. The number of times a particular base in the target region is represented in the sequence data is called the coverage or coverage depth. The number before the "fold" is the coverage (the average number of times the genome is sequenced). For example, if you perform 30x whole genome sequencing (WGS), "30x" means that the whole genome is sequenced 30 times on average. At both 20x and 30x coverage, nanoparticle NP normalization and TS normalization show equal results.

[0119] Figure 1IF shows the "fold 80" base pair penalty. This is the number of additional sequencing folds required to ensure that 80% of the target bases achieve average coverage. The lower the on-target rate or the higher the fold-80, the more capture inefficiencies and wasted sequencing. The average "fold 80" for nanoparticle NP normalization was 3, whereas the average "fold 80" for TS normalization was 3.25. This means that nanoparticle NP normalized libraries require less sequencing compared to TS normalized libraries. The lower the number of fold 80s, the better the results.

[0120] FIG. 11G shows overlap in normalized libraries. If multiple sequencing reads map to the exact same location, including the 3' and 5' coordinates, they are considered overlapping reads. The overlap rate is the percentage of marked map reads in a particular data set. In contrast to overlapping reads, overlapping reads do not provide additional information and are removed from sequencing data during bioinformatics analysis, a process known as deduplication. Nanoparticle NP normalization and TS normalization give equal overlap values.

[0121] Figure 11H shows AT / GC dropout. The AT / GC dropout metric indicates the degree of insufficient coverage of a particular region based on AT or GC content. For the nanoparticle NP-normalized library and the TS-normalized library, the values ​​of these metrics were equal.

[0122] Figure 11I shows the average insert size. The insert size is the length that is sequenced and the length of DNA (or RNA) that is "inserted" between the adaptors. For the nanoparticle NP normalized library, the average insert size was 220 bp, and for the TS normalized library, the average insert size was 190 bp, with a difference of 30 bp higher for the nanoparticle NP normalized library.

[0123] Figure 11J shows the on-target values ​​of the normalized libraries. Percent on-target bases is the number of bases that map to the target region, and percent on-target reads includes all sequencing reads that overlap the target region by even one base. The more bases or reads that fall within the target region, the higher the overall on-target percentage, indicating high probe specificity, high quality probes, and efficient target enrichment based on hybridization. The difference between the nanoparticle NP-normalized library and the TS-normalized library was only 0.03%.

[0124] It should be noted that in view of this disclosure, the methods, compositions, and systems can be implemented according to the present technology. Moreover, the various components, materials, structures, and parameters are included as examples only, and not in any limiting sense. In view of this disclosure, the present technology can be implemented into other applications, and the components, materials, structures, and devices for implementing these applications can be determined while remaining within the scope of the appended claims.

Claims

1. 1. A composition comprising magnetic nanoparticles in a liquid medium, The magnetic nanoparticles each include a magnetic core and a coating on the core, the coating having a thickness of about 1 nm to about 2 nm, and the magnetic nanoparticles in the composition have a thickness of about 110 nm. 2 / g ~ approx. 130m 2 / g Brunauer-Emmett-Teller (BET) surface area, said composition comprising clusters of individual magnetic nanoparticles, said clusters having an average cluster size of about 250 nm to about 350 nm.

2. The composition of claim 1 , wherein the coating has a thickness of about 1.5 nm to about 2.0 nm.

3. The magnetic nanoparticles are about 113 m 2 / g ~ approx. 127m 2 The composition of claim 1 having a BET surface area of ​​1 / g.

4. The composition of claim 1 , wherein the individual magnetic nanoparticles have an average total diameter of about 15 nm or less.

5. The composition of claim 1, wherein the individual magnetic nanoparticles have an average total diameter of about 10 to about 15 nm.

6. The composition of claim 1 , wherein the core of the magnetic nanoparticles has an average diameter of about 10 nm or less.

7. The core is Fe, which exhibits paramagnetism. 3 O 4 The composition of claim 1 , wherein the nanoparticle is a single domain magnetic nanoparticle of

8. 2. The composition of claim 1, wherein the core is a nanoscale single crystal of magnetite.

9. The core is Fe 2 O 3 The composition of claim 1 , wherein the composition is substantially free of

10. The composition of claim 1 , wherein the coating comprises silica.

11. The composition of claim 1 , wherein the coating further comprises a binding site that binds to an analyte.

12. The composition of claim 11 , wherein the analyte is a nucleic acid.

13. The composition of claim 1 , wherein the liquid medium is water.

14. The composition of claim 13, wherein the composition is a stable aqueous dispersion.

15. The composition of claim 13 , wherein the composition comprises clusters of the magnetic nanoparticles dispersed in the water.

16. 16. The composition of claim 15, wherein the clusters have an average cluster size of about 300 nm.

17. The composition of claim 1, wherein the composition is a stable suspension of the magnetic nanoparticles, and the magnetic nanoparticles are present at a concentration of about 3 to about 30 g / L.

18. 18. The composition of claim 17, wherein the magnetic nanoparticles remain suspended for at least six months at a temperature of about 25°C.

19. A stable suspension of magnetic nanoparticles packaged in a sealed package, comprising: the magnetic nanoparticles comprising a core and a coating on the core, the coating having a thickness of about 1 nm to about 2 nm; The suspension, wherein the interior volume of said sealed package is substantially free of oxygen.

20. 1. A method for producing silica-coated magnetic nanoparticles, comprising: Fe in deionized deoxygenated water 3+ / Fe 2+ Fe with a molar ratio of about 2 / 1 3+ and Fe 2+ preparing an aqueous solution of ions; sonicating the aqueous solution; Fe from the aqueous solution 3 O 4 is precipitated, thereby 3 O 4 forming a mixture including nanoparticles, and precipitating the mixture; adding a deoxygenated alcohol and a silicate to the mixture; The Fe 3 O 4 forming a silica coating on the nanoparticles; The silica-coated Fe 3 O 4 Isolating the nanoparticles; and A method comprising:

21. Fe in the aqueous solution 3+ The concentration of Fe in the aqueous solution is 2 to 50 mM. 2+ 21. The method of claim 20, wherein the concentration is 1 to 25 mM.

22. The aqueous solution is 3 and FeCl 2 21. The method of claim 20, wherein the compound is prepared by dissolving in deionized and deoxygenated water.

23. 21. The method of claim 20, further comprising adding a base to the aqueous solution under an inert atmosphere.

24. 24. The method of claim 23, wherein the base is ammonia and the base is added in a 2-fold or greater molar excess.

25. The mixture is maintained without stirring under an inert atmosphere for a settling time during which the Fe 3 O 4 maintaining the mixture such that nanoparticles are precipitated; and After the settling period, most of the water is removed from the mixture, thereby 3 O 4 concentrating or removing said mixture of nanoparticles; 24. The method of claim 23, further comprising:

26. 24. The method of claim 23, further comprising stirring under the inert atmosphere for the duration of the coating.

27. The method of claim 20, wherein the settling time and / or the coating time is from about 8 hours to about 24 hours.

28. 21. The method of claim 20, further comprising adding additional base to the mixture prior to adding the anhydrous silicate solution.

29. 21. The method of claim 20, wherein the silicate is added dropwise to the mixture while stirring and sonicating the mixture.

30. The Fe 3 O 4 The nanoparticles are separated from the mixture by magnetic capture, and the method comprises: 3 O 4 21. The method of claim 20, further comprising washing the nanoparticles.

31. The separated silica-coated Fe 3 O 4 The nanoparticles are dried under vacuum, thereby forming the silica-coated Fe 3 O 4 21. The method of claim 20, further comprising vacuum drying to form a powder of the nanoparticles.

32. 32. The method of claim 31, further comprising dispersing the powder in deoxygenated water, sparging with an inert gas, and sonicating before sealing in a package under an inert atmosphere.

33. To form clusters of individual magnetic nanoparticles having an average cluster size of about 250 nm to about 350 nm, silica-coated Fe 3 O 4 21. The method of claim 20, further comprising maintaining the nanoparticles for a clustering time.

34. During the clustering time, the silica-coated Fe is exposed to a temperature of 20° C. to 30° C. 3 O 4 The method of claim 33, wherein the nanoparticles are maintained.

35. 34. The method of claim 33, wherein the clustering time is at least one month.

36. 1. A method for preparing nucleic acids for analysis, comprising: mixing a sample containing nucleic acid with a binding medium and a magnetic nanoparticle composition in a vessel, the magnetic particle composition comprises a plurality of magnetic nanoparticles comprising a core and a coating on the core, the coating having a thickness of about 1.5 nm to about 2 nm; mixing, whereby the nucleic acid binds to the coating of the magnetic nanoparticles; After the binding time, separating the nucleic acid-bound magnetic nanoparticles from the liquid in the container using a magnet; removing the liquid from the container to retain the nucleic acid-bound magnetic nanoparticles within the container; washing the nanoparticles to remove impurities while the nanoparticles remain attracted to the magnet within the container; removing the cleaning medium; contacting the nucleic acid-bound magnetic nanoparticles with an elution medium, thereby separating the bound nucleic acid from the magnetic nanoparticles; Separating the magnetic nanoparticles from the nucleic acid-containing liquid in the container using a magnet; removing the nucleic acid from the vessel, thereby obtaining a nucleic acid preparation; and A method comprising:

37. the sample comprises an input amount of the nucleic acid; 37. The method of claim 36, wherein the magnetic nanoparticle composition has binding capacity for an output amount of nucleic acid, the output amount being less than the input amount.

38. 37. The method of claim 36, further comprising washing the nucleic acid-bound magnetic nanoparticles with a washing medium comprising at least 80% v / v alcohol.

39. 37. The method of claim 36, wherein the coating of the magnetic nanoparticles comprises binding sites configured to bind to the nucleic acid.

40. 37. The method of claim 36, wherein the magnetic nanoparticle composition has a normalization factor of 0.8 to 1.2, the normalization factor being a ratio of a first amount of output from a first sample to a second amount of output from a second sample, the first sample being

41. 37. The method of claim 36, wherein the output amount is within 10% of a predetermined output amount of the magnetic nanoparticle composition.

42. 37. The method of claim 36, wherein the nucleic acid preparation comprises nucleic acids having lengths within a predetermined length range.

43. 37. The method of claim 36, wherein the input sample comprises less than 200 ng of nucleic acid.

44. 37. The method of claim 36, wherein the input sample comprises less than 50 ng of nucleic acid.

45. 37. The method of claim 36, wherein said steps of said method are performed by automated equipment.

46. 1. A method for obtaining nucleic acid from a biological sample and preparing the nucleic acid for analysis, comprising: placing a nucleic acid-containing biological sample in a container to form a sample mixture, the biological sample being a cell or a virus; adding to the vessel a magnetic nanoparticle composition responsive to the sample mixture, the magnetic nanoparticle composition comprising a plurality of magnetic nanoparticles comprising a core and a coating on the core, the coating having a thickness of about 1.5 nm to about 2 nm; mixing the sample mixture with the magnetic nanoparticles and incubating for an incubation time; Separating the magnetic nanoparticles from the sample mixture; and adding a dissolution medium to the container and mixing the magnetic nanoparticles with the dissolution medium; removing the elution solution from the vessel after an elution period during which nucleic acids are eluted from the magnetic nanoparticles to form an elution solution; and A method comprising:

47. contacting the biological sample with guanidine thiocyanate (GTC) and proteinase K to form the sample mixture; incubating the sample mixture at an elevated temperature for a sample preparation time; adding neat alcohol to the sample mixture in the container; 47. The method of claim 46, further comprising:

48. applying a magnetic force to separate the magnetic nanoparticles from the supernatant in the container; removing the supernatant from the vessel without disturbing the separated magnetic nanoparticles; washing the separated magnetic nanoparticles one or more times with an alcohol solution; 47. The method of claim 46, wherein the magnetic nanoparticles are separated from the sample mixture by:

49. 47. The method of claim 46, wherein the elution time is less than 10 minutes.

50. placing the removed eluate in a second container; sealing the second container; and storing the second container at a low temperature; and 47. The method of claim 46, further comprising:

51. 47. The method of claim 46, wherein the sample preparation time and / or the incubation time is about 10 minutes or less.

52. 47. The method of claim 46, wherein the alcohol solution comprises about 80% v / v or more alcohol.

53. 47. The method of claim 46, wherein the nucleic acid is RNA.

54. 47. The method of claim 46, wherein the nucleic acid is DNA.