Method for treating semiconductor substrate layer and method for manufacturing solar cell
Surface oxidation treatment on single-crystal silicon wafers enhances the uniformity of phosphoric acid spreading, addressing uneven gettering and improving solar cell efficiency and longevity.
Patent Information
- Application Number
- JP2024523469
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2022-02-28
- Filing Date
- 2022-12-23
- Publication Date
- 2024-10-10
- Estimated Expiration
- 2042-12-23
AI Technical Summary
The non-uniform spread of phosphoric acid during chain spray gettering on single-crystal silicon wafers leads to uneven gettering, affecting the photovoltaic conversion efficiency and service life of solar cells.
A method involving surface oxidation treatment on single-crystal silicon wafers to enhance lyophilicity, followed by spraying a diffusion liquid and annealing, forming a uniform oxide layer to improve the distribution of diffused ions and impurity removal.
The method ensures uniform spreading of the diffusion liquid, resulting in a more consistent gettering effect and improved photovoltaic conversion efficiency and service life of solar cells.
Smart Images

Figure 2024537419000001_ABST
Abstract
Description
[Technical field]
[0001] This application claims priority to a Chinese patent application filed with the China Patent Office on February 28, 2022, bearing application number 202210189426.0 and entitled "Method for treating semiconductor substrate layer and method for manufacturing solar cell," the entire contents of which are incorporated herein by reference.
[0002] This application relates to the field of solar cell manufacturing, and in particular to methods for processing semiconductor substrate layers and for manufacturing solar cells. [Background technology]
[0003] Solar cells have the advantages of being clean, pollution-free, renewable, and stable in operation. According to the structure, manufacturing process and materials used of solar cells, solar cells are divided into different types, including silicon-based solar cells, multi-element compound thin film solar cells, polymer multilayer modified electrode solar cells, organic solar cells, etc., among which, silicon-based solar cells such as heterojunction solar cells are the most mature. Taking heterojunction solar cells as an example, a semiconductor layer, a transparent conductive layer and a metal electrode are manufactured on one or both sides of an N-type substrate to form a cell, and then multiple cells are interconnected and packaged to form a module, which generates electricity and feeds the electricity back to the power grid through an inverter.
[0004] N-type substrates are usually monocrystalline silicon wafers obtained by cutting monocrystalline silicon rods. In the process of pulling up monocrystalline silicon rods, the segregation coefficient of metal impurities is very small, so that the metal content difference occurs between the front and rear ends of the single silicon rods. In particular, in the prior art, the method of continuous supply and pulling is often used, which can continuously pull up multiple monocrystalline silicon rods, and in a single batch, the metal impurities in the later pulled monocrystalline rods are more than the metal impurities in the earlier pulled monocrystalline rods. When solar cells are manufactured with monocrystalline silicon wafers, due to the presence of metal impurities, the metal impurities will recombine with a minority of carriers, which will affect the photoelectric conversion efficiency, and even affect the conversion efficiency of high-efficiency cells, leading to a decrease in the service life.
[0005] Gettering is an important method to improve the crystal quality of single crystal silicon wafers. Gettering can reduce the content of metal impurities in single crystal silicon wafers and make the quality of single crystal silicon wafers more consistent, so that the conversion efficiency of high-efficiency cells is more concentrated. At present, one of the main methods is phosphoric acid chain spray gettering, which sprays phosphoric acid on the surface of single crystal silicon wafers as a diffusion liquid, and after the phosphoric acid spreads naturally, a doping layer is formed by diffusion annealing. During this process, the metal impurities in the single crystal silicon wafer are precipitated in the doping layer, and finally, the doping layer is removed to achieve the purpose of impurity removal. However, when the substrate single crystal silicon wafer is treated with phosphoric acid chain spray gettering, it is common that phosphoric acid spreads unevenly on the surface of the single crystal silicon wafer, which may result in poor service life and photoelectric conversion efficiency of the final solar cell. Therefore, a solution is needed to solve the problem of uneven phosphoric acid spread. Summary of the Invention [Problem to be solved by the invention]
[0006] The present application provides a method for treating a semiconductor substrate layer and a method for manufacturing a solar cell, which solves the problem of non-uniform spreading of a diffusion liquid. [Means for solving the problem]
[0007] The present application provides a method for treating a semiconductor substrate layer, the method including the steps of providing a single crystal silicon wafer, spraying a diffusion liquid on a surface of the single crystal silicon wafer, and annealing the single crystal silicon wafer, and further including the step of performing a surface oxidation treatment on the single crystal silicon wafer before spraying the diffusion liquid on the surface of the single crystal silicon wafer, the surface oxidation treatment being used to increase the lyophilicity of the surface of the single crystal silicon wafer with respect to the diffusion liquid, thereby improving uniformity of the annealing treatment of the single crystal silicon wafer.
[0008] Optionally, the step of performing a surface oxidation treatment includes a step of injecting an oxygen-containing gas onto the surface of the single crystal silicon wafer.
[0009] Optionally, the oxygen-containing gas comprises ozone.
[0010] Optionally, the concentration of the oxygen-containing gas is between 50 ppm and 300 ppm.
[0011] Optionally, the injection rate of the oxygen-containing gas is 0.5slm to 5slm.
[0012] The injection time of the oxygen-containing gas can be selectably between 5 seconds and 30 seconds.
[0013] Optionally, in the step of surface oxidation treatment, an oxygen-containing gas is injected perpendicularly toward the surface of the single crystal silicon wafer.
[0014] Optionally, an oxide layer is formed on the surface of the single crystal silicon wafer by the surface oxidation treatment, and the method for treating a semiconductor substrate layer further includes the following: by performing a diffusion annealing treatment on the surface of the single crystal silicon wafer, diffusing ions in the diffusion solution diffuse through the oxide layer into a partial thickness of the single crystal silicon wafer, and a doping layer covered by the oxide layer is formed in the partial thickness of the single crystal silicon wafer, and the diffusion annealing treatment is suitable for transferring impurities in the single crystal silicon wafer to the doping layer.
[0015] Optionally, the diffusion annealing process is a chain diffusion annealing process.
[0016] Optionally, an oxide layer is formed on the surface of the single crystal silicon wafer by surface oxidation treatment, and the thickness of the oxide layer is 0.5 nm to 20 nm.
[0017] Optionally, the material of the single crystal silicon wafer comprises single crystal silicon and the material of the oxide layer comprises silicon oxide.
[0018] Optionally, the step of performing a diffusion annealing treatment on the surface of the single crystal silicon wafer includes a heating process, a heat-holding process, and a cooling process, which are performed in sequence, the heat-holding process being suitable for diffusing ions into a partial thickness of the single crystal silicon wafer, and the cooling process being suitable for transferring impurities in the single crystal silicon wafer to a doping layer.
[0019] The temperature during the heat preservation process can be selected between 800℃ and 900℃.
[0020] Optionally, the thickness of the doping layer is between 0.15 μm and 0.3 μm.
[0021] Optionally, the diffusion liquid comprises a phosphoric acid solution.
[0022] Optionally, the concentration of the phosphoric acid solution is between 2% and 12% by weight.
[0023] Optionally, before subjecting the single crystal silicon wafer to a surface oxidation treatment, The method further includes the steps of removing a damaged layer on the surface of the single crystal silicon wafer, dehydrating the surface of the single crystal silicon wafer with a hydrophobic solution after removing the damaged layer on the surface of the single crystal silicon wafer, and drying the single crystal silicon wafer after the dehydration.
[0024] Optionally, the etchant used to remove the damage layer on the surface of the single crystal silicon wafer is NaOH aqueous solution, KOH aqueous solution, or a mixture of HF and HNO3.
[0025] Optionally, the hydrophobic solution comprises an aqueous solution of HF.
[0026] Optionally, the concentration of the aqueous NaOH solution is between 2% and 15% by weight.
[0027] Optionally, the concentration of the KOH aqueous solution is between 2% and 15% by weight.
[0028] Alternatively, a mixed solution of HF and HNO3 is prepared by mixing HF having a concentration of 45% by mass to 50% by mass and HNO3 having a concentration of 60% by mass to 70% by mass in a volume ratio of 1:3 to 1:9.
[0029] Optionally, the method further includes removing the oxide layer after the diffusion annealing process, and removing the doping layer after removing the oxide layer.
[0030] Optionally, the etching solution for removing the oxide layer is an aqueous HCl solution, and the concentration of HCl in the aqueous HCl solution is 4% by mass to 5% by mass.
[0031] Alternatively, the etchant used to remove the doping layer is an aqueous NaOH solution or an aqueous KOH solution; alternatively, a mixed solution of HF and HNO3 is used to both remove the oxide layer and the doping layer.
[0032] Optionally, the concentration of the NaOH aqueous solution is between 2% by weight and 15% by weight; Optionally, the concentration of the KOH solution is between 2% and 15% by weight; Alternatively, a mixed solution of HF and HNO3 is prepared by mixing HF having a concentration of 45% by mass to 50% by mass and HNO3 having a concentration of 60% by mass to 70% by mass in a volume ratio of 1:3 to 1:9.
[0033] Optionally, after removing the doping layer, the method further includes cleaning the single crystal silicon wafer with a neutral cleaning solution.
[0034] Optionally, the neutralizing wash is a mixed solution of HF and HCl.
[0035] The present application further provides a method for manufacturing a solar cell comprising the method for treating a semiconductor substrate layer according to the present application.
[0036] Optionally, the method for manufacturing a solar cell further includes the steps of: performing a texturing process on the semiconductor substrate layer after processing the semiconductor substrate layer; forming a first intrinsic semiconductor layer on one surface of the semiconductor substrate layer after the texturing process, and forming a second intrinsic semiconductor layer on the other surface of the semiconductor substrate layer; forming a first doped semiconductor layer on a side of the first intrinsic semiconductor layer opposite to the semiconductor substrate layer, and forming a second doped semiconductor layer on a side of the second intrinsic semiconductor layer opposite to the semiconductor substrate layer; forming a first transparent conductive film on a side of the first doped semiconductor layer opposite to the semiconductor substrate layer, and forming a second transparent conductive film on a side of the second doped semiconductor layer opposite to the semiconductor substrate layer; and forming a first grid electrode on a side of the first transparent conductive film opposite to the semiconductor substrate layer, and forming a second grid electrode on a side of the second transparent conductive film opposite to the semiconductor substrate layer. Effect of the Invention
[0037] The beneficial effects of the present application are as follows:
[0038] In the method for treating a semiconductor substrate layer in this embodiment, a surface oxidation treatment is performed on the single crystal silicon wafer before spraying the diffusion liquid. The surface oxidation treatment can form an oxide layer in advance on the surface of the single crystal silicon wafer. Since the oxide layer on the surface of the single crystal silicon wafer has better lyophilicity with respect to the diffusion liquid, the diffusion liquid can be spread better when spraying the diffusion liquid, and the diffusion liquid can be spread faster when spraying the diffusion liquid. As a result, the diffusion liquid can be spread more uniformly on the surface of the single crystal silicon wafer. Furthermore, a diffusion annealing process is performed on the surface of the single crystal silicon wafer, and the diffusion ions in the diffusion liquid are diffused into a part of the thickness of the single crystal silicon wafer to form a doped layer in the part of the thickness of the single crystal silicon wafer, and the diffusion annealing process is suitable for transferring the impurities in the single crystal silicon wafer to the doped layer. Since the diffusion liquid spreads more uniformly on the surface of the single crystal silicon wafer, the distribution of the diffusion ions in the doped layer becomes more uniform, and the gettering effect of the doped layer becomes more consistent in different regions, so that the properties of the semiconductor substrate layer are greatly improved.
[0039] In order to more clearly describe the specific embodiments of the present application or the technical solutions in the prior art, the following will briefly describe the drawings that need to be used in the description of the specific embodiments or the prior art. It is obvious that the drawings in the following description are some embodiments of the present application, and those skilled in the art can obtain other drawings based on these drawings without exerting creative efforts. [Brief description of the drawings]
[0040] [Figure 1] 1 is a simplified flow chart of a method for processing a semiconductor substrate layer in one embodiment of the present application. [Diagram 2] 1 is a detailed schematic flow chart of a method for processing a semiconductor substrate layer in accordance with one embodiment of the present application. [Diagram 3] FIG. 1 is a structural schematic diagram of a processing process of a semiconductor substrate layer in one embodiment of the present application. [Figure 4] FIG. 1 is a structural schematic diagram of a processing process of a semiconductor substrate layer in one embodiment of the present application. [Diagram 5] FIG. 1 is a structural schematic diagram of a processing process of a semiconductor substrate layer in one embodiment of the present application. [Figure 6] FIG. 1 is a structural schematic diagram of a processing process of a semiconductor substrate layer in one embodiment of the present application. [Figure 7] FIG. 1 is a structural schematic diagram of a processing process of a semiconductor substrate layer in one embodiment of the present application. [Figure 8]FIG. 1 is a structural schematic diagram of a processing process of a semiconductor substrate layer in one embodiment of the present application. [Figure 9] FIG. 1 is a structural schematic diagram of a processing process of a semiconductor substrate layer in one embodiment of the present application. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0041] As described in the background art, after the substrate single crystal silicon wafer is treated by the method of chain phosphoric acid gettering, the final photoelectric conversion efficiency and the service life of the solar cell may not be ideal.The inventors have researched and found that the specific cause is that in the process of chain phosphoric acid gettering, the phosphoric acid used as the diffusion liquid has poor spreading property and slow spreading speed, and the diffusion speed of the diffusion liquid is slow, so that the phosphoric acid is easily distributed unevenly on the surface of the single crystal silicon wafer, and the gettering is completed locally and corrosion occurs, but the gettering may not be completed in other parts.
[0042] In order to solve the problem of non-uniform spreading of the diffusion liquid, the present application provides a method for treating a semiconductor substrate layer, comprising the steps of providing a single crystal silicon wafer and spraying a diffusion liquid onto a surface of the single crystal silicon wafer, and further comprising the step of performing a surface oxidation treatment on the single crystal silicon wafer before spraying the diffusion liquid onto the surface of the single crystal silicon wafer, the surface oxidation treatment being used to increase the lyophilicity of the single crystal silicon wafer with respect to the diffusion liquid.
[0043] The technical solutions of the present application will be described below clearly and completely with reference to the drawings, but it is clear that the described embodiments are only some embodiments of the present application, and not all embodiments. Based on the embodiments of the present application, all other embodiments obtained by those skilled in the art without creative labor fall within the scope of protection of the present application.
[0044] In the description of this application, the orientations or positional relationships indicated by terms such as "center," "upper," "lower," "left," "right," "vertical," "horizontal," "inner," and "outer" are based on the orientations or positional relationships shown in the drawings, and are merely for the purpose of facilitating and simplifying the description of this application, and do not indicate or imply that such devices or elements must necessarily have a specific orientation, or be configured or operate in a specific orientation, and therefore are not to be understood as limiting this application. Furthermore, the terms "first," "second," and "third" are used for the purpose of description only, and are not to be understood as indicating or implying relative importance.
[0045] In the description of this application, unless otherwise expressly specified or limited, the terms "attach," "connect," and "connect" should be understood in a broad sense, and may be, for example, a fixed connection, a detachable connection, or an integral connection, a mechanical connection, an electrical connection, a direct connection, an indirect connection via an intermediate medium, or an internal communication between two components. The specific meaning of the above terms in this specification can be understood by those skilled in the art depending on the situation.
[0046] In addition, the technical features according to each embodiment of the present application described below may be combined with each other as long as they are not mutually contradictory.
[0047] Example 1 This embodiment provides a method for treating a semiconductor substrate layer, and referring to FIG. Step S1 of providing a single crystal silicon wafer; Step S2 of performing a surface oxidation treatment on the single crystal silicon wafer; Step S3 of spraying a diffusion liquid onto the surface of the single crystal silicon wafer; and step S4 of performing a diffusion annealing treatment on the surface of the single crystal silicon wafer.
[0048] In the present application, the surface oxidation treatment is used to increase the lyophilicity of the single crystal silicon wafer to a diffusion liquid, which is used to form a doping layer and remove metal impurities in the single crystal silicon wafer during the diffusion annealing step.
[0049] In the method for treating a semiconductor substrate layer in this embodiment, a surface oxidation treatment is performed on a single crystal silicon wafer before spraying a diffusion liquid. An oxide layer can be formed in advance on the surface of the single crystal silicon wafer by the surface oxidation treatment. Since the oxide layer on the surface of the single crystal silicon wafer has better lyophilicity with respect to the diffusion liquid, the diffusion liquid can be better spread when spraying the diffusion liquid, and the diffusion liquid can be spread faster when spraying the diffusion liquid. As a result, the diffusion liquid can be spread more uniformly on the surface of the single crystal silicon wafer, the uniformity of the annealing treatment of the single crystal silicon wafer can be improved, and the properties of the semiconductor substrate layer can be greatly improved.
[0050] In this embodiment, referring to FIG. 2, before the surface oxidation treatment of the single crystal silicon wafer, The method further includes step A1 of removing a damaged layer on the surface of the single crystal silicon wafer, step A2 of dehydrating the surface of the single crystal silicon wafer with a hydrophobic solution after removing the damaged layer on the surface of the single crystal silicon wafer, and step A3 of drying the single crystal silicon wafer after the dehydration.
[0051] In this embodiment, referring to FIG. 2, after the diffusion annealing treatment, the method further includes a step S5 of removing the doping layer.
[0052] Hereinafter, a detailed explanation will be given with reference to FIGS.
[0053] Referring to FIG. 3, a single crystal silicon wafer 100 is provided.
[0054] The material of the monocrystalline silicon wafer 100 includes monocrystalline silicon. In other embodiments, the material of the monocrystalline silicon wafer is germanium or other semiconductor materials such as silicon germanium. The material of the semiconductor substrate layer may be other semiconductor materials.
[0055] In this embodiment, the conductivity type of the single crystal silicon wafer 100 is N-type, and the conductivity type of the semiconductor substrate layer formed thereafter is N-type, and the semiconductor substrate layer is used for a solar cell. In other embodiments, the conductivity type of the single crystal silicon wafer is P-type.
[0056] In this embodiment, the surface of the single crystal silicon wafer 100 has a damage layer 110. In one specific embodiment, the single crystal silicon wafer 100 has damage layers 110 on both the front and back sides. The damage layers 110 are generated during the process of cutting a single crystal raw material to form the single crystal silicon wafer 100.
[0057] Referring to FIG. 4, the damaged layer 110 (FIG. 3) on the surface of the single crystal silicon wafer 100 is removed.
[0058] In this embodiment, the process of removing the damaged layer 110 includes a wet etching process, and in one specific embodiment, the etchant used to remove the damaged layer 110 on the surface of the single crystal silicon wafer 100 is a NaOH aqueous solution, a KOH aqueous solution, or a mixed solution of HF and HNO3. When the etchant used to remove the damaged layer on the surface of the single crystal silicon wafer is a NaOH aqueous solution, the concentration of the NaOH aqueous solution is 2% by mass to 15% by mass; when the etchant used to remove the damaged layer on the surface of the single crystal silicon wafer is a KOH aqueous solution, the concentration of the KOH aqueous solution is 2% by mass to 15% by mass; when the etchant used to remove the damaged layer on the surface of the single crystal silicon wafer is a mixed solution of HF and HNO3, the mixed solution of HF and HNO3 is prepared with a volume ratio of 1:3 to 1:9, with HF having a concentration of 45% by mass to 50% by mass and HNO3 having a concentration of 60% by mass to 70% by mass.
[0059] Referring to FIG. 5, after removing the damaged layer 110 on the surface of the single crystal silicon wafer 100, the surface of the single crystal silicon wafer is dehydrated with a hydrophobic solution.
[0060] The hydrophobic solution comprises an aqueous solution of HF.
[0061] In some other embodiments, when the etching solution used to remove the damaged layer 110 is a NaOH solution or a KOH solution, the method further includes removing the remaining etching solution with a neutralizing solution before the dehydration process. The neutralizing solution is a mixed solution of HF and HCl.
[0062] Referring to FIG. 6, after the dehydration process, the single crystal silicon wafer 100 is dried.
[0063] 7, a surface oxidation treatment is performed on the single crystal silicon wafer 100. The surface oxidation treatment forms an oxide layer 120 on the surface of the single crystal silicon wafer 100. The surface oxidation treatment can increase the uniformity of the diffusion liquid that spreads on the surface of the initial semiconductor layer 100 when a diffusion liquid is sprayed on the surface of the single crystal silicon wafer 100 thereafter.
[0064] In one embodiment, the thickness of the oxide layer 120 is between 0.5 nm and 20 nm, and may be, for example, 0.5 nm, 1 nm, or 2 nm.
[0065] The oxide layer 120 itself is so thin that it does not affect the diffusion of diffusing ions in the diffusion solution through the oxide layer 120 in the subsequent diffusion annealing step.
[0066] When the material of the monocrystalline silicon wafer is monocrystalline silicon, the material of the oxide layer 120 is silicon oxide.
[0067] The step of performing the surface oxidation treatment includes a step of injecting an oxygen-containing gas onto the surface of the single crystal silicon wafer 100 .
[0068] Specifically, the oxygen-containing gas may be, for example, ozone, which has a relatively good oxidizing ability.
[0069] In one embodiment, the concentration of the oxygen-containing gas is 50 ppm to 300 ppm, for example, 50 ppm, 100 ppm, 150 ppm, 200 ppm, 250 ppm, or 300 ppm. If the concentration of the oxygen-containing gas is too low, the oxidation rate will be slow and the process efficiency will be reduced, and if the concentration of the oxygen-containing gas is too high, the oxidation rate will be too high and it will be difficult to control relatively well during oxidation.
[0070] In one embodiment, the injection rate of the oxygen-containing gas is 0.5 slm to 5 slm (standard liter per minute), for example, 0.5 slm, 1 slm, 2 slm, 4 slm or 5 slm. If the injection rate of the oxygen-containing gas is too slow, the oxidation rate will be slow and the process efficiency will be reduced, and if the injection rate of the oxygen-containing gas is too fast, the oxidation rate will be too fast, which makes it difficult to control relatively well during oxidation, and furthermore, the oxygen-containing gas will be insufficiently utilized and wasteful.
[0071] In one embodiment, the injection time of the oxygen-containing gas is 5 seconds to 30 seconds, for example, 5 s, 10 s, 15 s, 20 s, 25 s, or 30 s. If the injection time of the oxygen-containing gas is too short, the oxidation is insufficient, the thickness of the oxide layer 120 becomes too thin, the uniformity of the oxide layer 120 becomes poor, and the degree of improvement in the uniformity of the diffusion liquid spreading on the surface of the single crystal silicon wafer is low. If the injection time of the oxygen-containing gas is too long, the oxide layer 120 becomes too thick, which is unfavorable to the diffusion of the diffusion ions in the diffusion liquid.
[0072] The oxygen-containing gas is preferably sprayed in a direction perpendicular to the single crystal silicon wafer 100 .
[0073] In some embodiments, an oxygen-containing gas is sprayed onto both opposing sides of the single crystal silicon wafer 100 to form an oxide layer 120 on both opposing sides of the single crystal silicon wafer 100 .
[0074] Referring to FIG. 8 , a diffusion liquid is sprayed onto the surface of the single crystal silicon wafer 100, and then a diffusion annealing process is performed on the surface of the single crystal silicon wafer 100. Diffusion ions in the diffusion liquid diffuse through the oxide layer 120 to a portion of the thickness of the single crystal silicon wafer 100, and a doping layer 130 is formed on the oxide layer 120 in a portion of the thickness of the single crystal silicon wafer 100. The diffusion annealing process is suitable for moving impurities in the single crystal silicon wafer 100 to the doping layer 130.
[0075] Since the doped layer 130 has a higher solid solubility for metal impurities than the initial semiconductor layer, the metal impurities gradually move from the portion of the initial semiconductor layer where the doped layer 130 is not formed to the doped layer 130. In this embodiment, after the diffusion annealing process, the oxide layer 120 is also doped with diffusing ions, and when the material of the oxide layer 120 is silicon oxide and the diffusing ions are phosphorus ions, the oxide layer 120 is formed into an oxide layer 120' doped with diffusing ions after the diffusion annealing process, and the oxide layer 120' is phosphorus silicate glass (PSG).
[0076] In this embodiment, the step of spraying the diffusion liquid on the surface of the single crystal silicon wafer is specifically to spray phosphoric acid on the surface of the initial semiconductor layer, and the phosphoric acid is allowed to naturally spread on the surface of the initial semiconductor layer, where the concentration of the phosphoric acid solution is 2% by mass to 12% by mass.
[0077] In some embodiments, the diffusion liquid is sprayed on both opposing sides of the single crystal silicon wafer 100 to form the doped layers 130 on both opposing sides of the single crystal silicon wafer 100 .
[0078] In this embodiment, the diffusion annealing process includes a heating process, a heat-holding process, and a cooling process, which are performed in sequence, the heat-holding process is suitable for diffusing the diffusing ions to a thickness of a portion of the single crystal silicon wafer, and the cooling process is suitable for transferring the impurities in the single crystal silicon wafer to the doping layer. In this embodiment, the diffusion annealing process is a chain diffusion annealing process performed in a chain diffusion annealing furnace.
[0079] The time for the temperature rise process is 50s to 100s, for example, 50s, 60s, 70s, 80s, 90s, and 100s. The temperature rise process is heating from room temperature to 800°C to 900°C, for example, 800°C, 850°C, and 900°C. The temperature in the heat retention process is maintained at 800°C to 900°C. The time for the cooling process is 50s to 100s, for example, 50s, 60s, 70s, 80s, 90s, and 100s. The temperature in the cooling process is reduced by 300°C to 500°C from the temperature in the heat retention process.
[0080] In this embodiment, the material of the initial semiconductor layer 100 is single crystal silicon, and the doped layer 130 is a silicon layer doped with phosphorus. The thickness of the doped layer 130 is 0.15 μm to 0.3 μm, for example, 0.15 μm, 0.2 μm, 0.25 μm, or 0.3 μm.
[0081] Because the diffusion liquid spreads more evenly on the surface of the single crystal silicon wafer, the distribution of the diffusion ions in the doping layer becomes more uniform, and the gettering effect of the doping layer becomes more consistent in different regions.
[0082] Referring to FIG. 9, the oxide layer 120' is removed, and after the oxide layer 120' is removed, the doping layer 130 is removed to form a semiconductor substrate layer 200.
[0083] In this embodiment, the etchant for removing the oxide layer 120' is an HCl aqueous solution, and the concentration of the HCl aqueous solution is 4% by weight to 5% by weight, for example, 4% or 5%. In this embodiment, the process for removing the doped layer 130 includes a wet etching process. In one specific embodiment, the etchant used for removing the doped layer 130 is an NaOH aqueous solution or a KOH aqueous solution. When the etchant used for removing the doped layer 130 is an NaOH aqueous solution, the concentration of the NaOH aqueous solution is 2% by weight to 15% by weight, and when the etchant used for removing the doped layer 130 is an KOH aqueous solution, the concentration of the KOH aqueous solution is 2% by weight to 15% by weight.
[0084] In another embodiment, a mixture of HF and HNO3 is used to remove both the oxide layer 120' and the doping layer 130. When the mixture of HF and HNO3 is used as the etchant to remove the oxide layer 120 and the doping layer 130, the mixture of HF and HNO3 is prepared by mixing 45% to 50% by weight of HF and 60% to 70% by weight of HNO3 in a volume ratio of 1:3 to 1:9.
[0085] Because the gettering effect of the doping layer is more consistent in different regions, the removal effect of impurities in the semiconductor substrate layer after removing the doping layer is better.
[0086] In some other embodiments, after removing the doping layer, the method further comprises cleaning the single crystal silicon wafer with a neutralizing cleaning solution, where the neutralizing cleaning solution is a mixed solution of HF and HCl.
[0087] Finally, drying is performed to complete the processing of the semiconductor substrate layer 200.
[0088] The unoxidized single crystal silicon wafer was used as a comparison group, and the relative values of the test results of the semiconductor substrate layer obtained by the processing method of this embodiment are as follows (the unoxidized single crystal silicon wafer is used as the reference value): [Table 1]
[0089] As can be seen, after the oxidation treatment, the average minority carrier lifetime and the minimum minority carrier lifetime of the semiconductor substrate layer are both significantly improved, and the maximum minority carrier lifetime and the efficiency of the produced battery are also improved to a certain extent.
[0090] Example 2 This embodiment provides a method for manufacturing a solar cell including the method for treating a semiconductor substrate layer according to the first embodiment.
[0091] In this embodiment, the method for manufacturing a solar cell further includes the steps of: performing a texturing process on the semiconductor substrate layer after processing the semiconductor substrate layer; forming a first intrinsic semiconductor layer on one surface of the semiconductor substrate layer after the texturing process, and forming a second intrinsic semiconductor layer on the other surface of the semiconductor substrate layer; forming a first doped semiconductor layer on the first intrinsic semiconductor layer opposite to the semiconductor substrate layer, and forming a second doped semiconductor layer on the second intrinsic semiconductor layer opposite to the semiconductor substrate layer; forming a first transparent conductive film on the first doped semiconductor layer opposite to the semiconductor substrate layer, and forming a second transparent conductive film on the second doped semiconductor layer opposite to the semiconductor substrate layer; forming a first grid electrode on the first transparent conductive film opposite to the semiconductor substrate layer, and forming a second grid electrode on the second transparent conductive film opposite to the semiconductor substrate layer.
[0092] Because the impurities in the semiconductor substrate layer are more effectively removed, the solar cell finally formed by the solar cell manufacturing method of this embodiment has higher photoelectric conversion efficiency and longer service life.
[0093] Obviously, the above examples are merely illustrative and are not limiting. Those skilled in the art can make various other changes or modifications based on the above description. It is not necessary and cannot be possible to cover all the embodiments here. And, the obvious changes or modifications derived in this way are also within the scope of protection of the present invention. [Explanation of symbols]
[0094] 100 Single crystal silicon wafers 110 Damage Layer 120 Oxide layer 120' Oxide layer 130 Doping layer 200 Semiconductor substrate layer
Claims
1. 1. A method for treating a semiconductor substrate layer, comprising the steps of: providing a single crystal silicon wafer; spraying a diffusion liquid onto a surface of the single crystal silicon wafer; and annealing the single crystal silicon wafer, a step of performing a surface oxidation treatment on the single crystal silicon wafer before spraying a diffusion liquid on the surface of the single crystal silicon wafer, the surface oxidation treatment being used to increase the lyophilicity of the surface of the single crystal silicon wafer with respect to the diffusion liquid, thereby increasing uniformity of an annealing treatment of the single crystal silicon wafer.
2. The step of performing the surface oxidation treatment includes a step of spraying an oxygen-containing gas onto the surface of the single crystal silicon wafer, Preferably, the oxygen-containing gas comprises ozone; Preferably, the concentration of the oxygen-containing gas is 50 ppm to 300 ppm; Preferably, the injection velocity of the oxygen-containing gas is between 0.5 slm and 5 slm; Preferably, the injection time of the oxygen-containing gas is 5 seconds to 30 seconds, 2. The method for treating a semiconductor substrate layer according to claim 1, wherein the oxygen-containing gas is preferably sprayed perpendicularly toward the surface of the single crystal silicon wafer in the surface oxidation step.
3. an oxide layer is formed on the surface of the single crystal silicon wafer by the surface oxidation treatment, a step of performing a diffusion annealing treatment on the surface of the single crystal silicon wafer, whereby diffusing ions in the diffusion solution diffuse through the oxide layer into a partial thickness of the single crystal silicon wafer, and a doping layer is formed in the partial thickness of the single crystal silicon wafer, the doping layer being covered by the oxide layer; and the diffusion annealing treatment is suitable for moving impurities in the single crystal silicon wafer to the doping layer; 2. A method according to claim 1, characterized in that the diffusion annealing process is preferably a chain diffusion annealing process.
4. The thickness of the oxide layer is 0.5 nm to 20 nm; 4. A method for treating a semiconductor substrate layer according to claim 3, characterized in that the material of the monocrystalline silicon wafer preferably comprises monocrystalline silicon and the material of the oxide layer preferably comprises silicon oxide.
5. the step of performing a diffusion annealing treatment on the surface of the single crystal silicon wafer includes a temperature increasing process, a temperature maintaining process, and a cooling process, which are performed in sequence, the temperature maintaining process being suitable for diffusing the diffusing ions to a thickness of a portion of the single crystal silicon wafer, and the cooling process being suitable for moving impurities in the single crystal silicon wafer to the doping layer; Preferably, the temperature in the heat-retaining step is 800°C to 900°C; 4. The method of claim 3, wherein the doping layer has a thickness of 0.15 μm to 0.3 μm.
6. The diffusion liquid includes a phosphoric acid solution, The method for treating a semiconductor substrate layer according to any one of the preceding claims, characterized in that the concentration of the phosphoric acid solution is preferably between 2% and 12% by weight.
7. Before performing a surface oxidation treatment on the single crystal silicon wafer, removing a damaged layer on a surface of the single crystal silicon wafer; removing the damaged layer on the surface of the single crystal silicon wafer, and then dehydrating the surface of the single crystal silicon wafer with a hydrophobic solution; and drying the single crystal silicon wafer after the dehydration treatment. Preferably, the etching solution used to remove the damaged layer on the surface of the single crystal silicon wafer is an aqueous NaOH solution, an aqueous KOH solution, or an aqueous solution of HF and HNO 3 A mixed solution of Preferably, the hydrophobic solution comprises an aqueous HF solution; Preferably, the concentration of the NaOH aqueous solution is 2% by mass to 15% by mass, Preferably, the concentration of the KOH aqueous solution is 2% by mass to 15% by mass; Preferably, the HF and HNO 3 The mixed solution is a mixture of HF having a concentration of 45% by mass to 50% by mass and HNO having a concentration of 60% by mass to 70% by mass. 3 6. The method for treating a semiconductor substrate layer according to claim 1, wherein the volume ratio of the components is 1:3 to 1:
9.
8. After the diffusion annealing treatment, removing the oxide layer; removing the doping layer after removing the oxide layer; Preferably, the etching solution for removing the oxide layer is an aqueous HCl solution, and the concentration of HCl in the aqueous HCl solution is 4% by mass to 5% by mass; Preferably, the etchant used to remove the doping layer is an aqueous NaOH solution or an aqueous KOH solution; Preferably, both the removal of the oxide layer and the removal of the doping layer are performed using HF and HNO 3 Using a mixed solution of Preferably, the concentration of the NaOH aqueous solution is 2% by mass to 15% by mass, Preferably, the concentration of the KOH aqueous solution is 2% by mass to 15% by mass; Preferably, the HF and HNO 3 The mixed solution is a mixture of HF having a concentration of 45% by mass to 50% by mass and HNO having a concentration of 60% by mass to 70% by mass. 3 4. The method for treating a semiconductor substrate layer according to claim 3, characterized in that the above is prepared in a volume ratio of 1:3 to 1:
9.
9. After removing the doping layer, the method further includes cleaning the single crystal silicon wafer with a neutral cleaning solution; 9. The method of claim 8, wherein the neutralizing cleaning solution is a mixture of HF and HCl.
10. A method for producing a solar cell, comprising the method for treating a semiconductor substrate layer according to any one of claims 1 to 9.
11. After processing the semiconductor substrate layer, texturing the semiconductor substrate layer; forming a first intrinsic semiconductor layer on one side of the semiconductor substrate layer and a second intrinsic semiconductor layer on the other side of the semiconductor substrate layer after the texturing process; forming a first doped semiconductor layer on a side of the first intrinsic semiconductor layer opposite the semiconductor substrate layer, and forming a second doped semiconductor layer on a side of the second intrinsic semiconductor layer opposite the semiconductor substrate layer; forming a first transparent conductive film on a side of the first doped semiconductor layer opposite to the semiconductor substrate layer, and forming a second transparent conductive film on a side of the second doped semiconductor layer opposite to the semiconductor substrate layer; 11. The method of claim 10, further comprising the steps of: forming a first grid electrode on a side of the first transparent conductive film opposite the semiconductor substrate layer; and forming a second grid electrode on a side of the second transparent conductive film opposite the semiconductor substrate layer.
Citation Information
Patent Citations
Coating source diffusion method and diffusion device capable of improving diffusion uniformity
CN103824761A
Manufacture of silicon semiconductor device
JP1998172913A
Manufacturing method of photoelectric conversion device
JP2006351995A
Manufacturing method of semiconductor substrate for optical power generating body
JP2012190974A
Photovoltaic device and method of manufacturing the same, and photovoltaic module
JP2014093418A