Polyester copolymers containing recycled monomers and having improved extrusion processability
A polyester copolymer using recycled bis-2-hydroxyethyl terephthalate and specific diols and acids improves extrusion processability, addressing quality issues and enhancing productivity.
Patent Information
- Application Number
- JP2024520679
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2021-10-08
- Filing Date
- 2022-09-06
- Publication Date
- 2024-10-16
AI Technical Summary
The quality of polyester copolymers produced using recycled bis-2-hydroxyethyl terephthalate deteriorates due to foreign matter and impurities, leading to issues in extrusion processability and article quality.
A polyester copolymer is formulated using recycled bis-2-hydroxyethyl terephthalate, dicarboxylic acids or their derivatives, and diols such as ethylene glycol and comonomers, with specific ratios and reaction conditions to achieve an extrudability coefficient of 1 or more, improving extrusion processability.
The improved extrusion processability reduces roll contamination and outgas generation, enhancing the quality and productivity of polyester copolymer articles.
Smart Images

Figure 2024537855000001 
Figure 2024537855000002 
Figure 2024537855000003
Abstract
Description
[Technical field]
[0001] The present invention relates to polyester copolymers containing recycled monomers and having improved extrusion processability, methods for making same, and articles containing same. [Background technology]
[0002] Polyester is highly suitable for use in large quantities as a material for beverage containers, packaging films, audio and video films, etc., due to its excellent mechanical strength, heat resistance, transparency, and gas barrier properties. It is also widely produced worldwide as an industrial material for medical fibers, tire cords, etc. Polyester sheets and plates have good transparency and excellent mechanical strength, and are widely used as materials for cases, boxes, partitions, store shelves, protective panels, blister packaging, building materials, interior and exterior materials, etc.
[0003] Meanwhile, waste plastics, which account for about 70% of marine pollution, have recently emerged as a serious social problem, and as a result, countries are restricting the use of disposable plastics while at the same time trying to reuse them. There are two main methods for recycling waste plastics. One is to collect, crush, and wash the waste plastics, melt extrude them, re-pelletize them, and use them as raw materials. The other is to use the substance obtained by depolymerizing the waste plastics as a monomer for plastic synthesis. In the latter case, bis-2-hydroxyethyl terephthalate can be obtained by depolymerizing PET or PETG in the waste plastics, and research is underway to use this as a monomer for polyester copolymers.
[0004] However, it is difficult to obtain good quality materials due to foreign matter in waste plastics, and in particular, plastics made from materials obtained by depolymerizing waste plastics often suffer from quality degradation. In particular, when the quality of plastics deteriorates, the quality of products manufactured by extrusion processing also inevitably deteriorates.
[0005] Therefore, the present inventors have confirmed that the quality of the polyester copolymer produced from the material obtained by depolymerizing waste plastics is improved, particularly the extrusion processability, by using recycled bis-2-hydroxyethyl terephthalate as a monomer for the polyester copolymer and adjusting the amount of other monomers used as described below, and thus completed the present invention. Summary of the Invention [Problem to be solved by the invention]
[0006] The present invention provides polyester copolymers containing recycled monomers and having improved extrudability, methods for their preparation, and articles containing same. [Means for solving the problem]
[0007] In order to solve the above problems, the present invention provides the following polyester copolymer: 1) recycled bis-2-hydroxyethyl terephthalate; 2) Acids, including dicarboxylic acids or their derivatives, and 3) A diol containing ethylene glycol and a comonomer is polymerized, In the polyester resin having a structure in which a portion derived from the bis-2-hydroxyethyl terephthalate, an acid portion derived from the dicarboxylic acid or a derivative thereof, and a diol portion derived from the diol are repeated, The polyester copolymer has an extrudability coefficient of 1 or more as determined by the following formula 1: Polyester Copolymer:
[0008]
number
[0009] In the above formula 1, A is the content (wt%) of the portion derived from recycled bis-2-hydroxyethyl terephthalate in the polyester copolymer, B is the content (ppmw) of residual acid (acid) in the polyester copolymer, C is the content (ppmw) of residual recycled bis-2-hydroxyethyl terephthalate in the polyester copolymer; D is the content (area / g) of the oligomer in the polyester copolymer.
[0010] Definition of Terms The copolymer according to the present invention relates to a copolymer prepared by copolymerizing a dicarboxylic acid or its derivative, and a diol containing diethylene glycol and a comonomer, and relates to a polyester copolymer prepared by participating in the reaction of recycled bis-2-hydroxyethyl terephthalate during the copolymerization process.
[0011] The term "derivative" as used herein means a certain portion or unit derived from a specific compound contained in the result of a chemical reaction when the specific compound participates in the chemical reaction. Specifically, the acid portion derived from the dicarboxylic acid or its derivative, and the diol portion derived from the diol, each mean a repeating unit in the polyester copolymer formed by an esterification reaction or a condensation polymerization reaction. Also, the portion derived from bis-2-hydroxyethyl terephthalate means a repeating unit in the polyester copolymer formed by an esterification reaction in the copolymerization reaction.
[0012] Acids including dicarboxylic acids or their derivatives The dicarboxylic acid or its derivative used in the present invention means a main monomer constituting the polyester copolymer together with the diol component. In particular, the dicarboxylic acid includes terephthalic acid, and the physical properties of the polyester copolymer according to the present invention can be improved by terephthalic acid. The terephthalic acid residue can also be formed from a terephthalic acid alkyl ester, preferably dimethyl terephthalic acid.
[0013] The dicarboxylic acid component may further include an aromatic dicarboxylic acid component, an aliphatic dicarboxylic acid component, or a mixture thereof in addition to terephthalic acid. In this case, the dicarboxylic acid component other than terephthalic acid is preferably included in an amount of 30 wt % or less based on the total weight of the entire dicarboxylic acid component.
[0014] The aromatic dicarboxylic acid component may be an aromatic dicarboxylic acid having 8 to 20 carbon atoms, preferably 8 to 14 carbon atoms, or a mixture thereof. Examples of the aromatic dicarboxylic acid include isophthalic acid, naphthalenedicarboxylic acid such as 2,6-naphthalenedicarboxylic acid, diphenyldicarboxylic acid, 4,4'-stilbene dicarboxylic acid, 2,5-furandicarboxylic acid, 2,5-thiophenedicarboxylic acid, etc., but the specific examples of the aromatic dicarboxylic acid are not limited thereto. The aliphatic dicarboxylic acid component may be an aliphatic dicarboxylic acid component having 4 to 20 carbon atoms, preferably 4 to 12 carbon atoms, or a mixture thereof. Examples of the aliphatic dicarboxylic acid include cyclohexanedicarboxylic acid such as 1,4-cyclohexanedicarboxylic acid and 1,3-cyclohexanedicarboxylic acid, phthalic acid, sebacic acid, succinic acid, isodecyl succinic acid, maleic acid, fumaric acid, adipic acid, glutaric acid, azelaic acid, etc., linear, branched or cyclic aliphatic dicarboxylic acid components, but the specific examples of the aliphatic dicarboxylic acid are not limited thereto.
[0015] Specifically, the acid containing the dicarboxylic acid or a derivative thereof may include, in addition to terephthalic acid, any one or more selected from the group consisting of isophthalic acid, dimethyl isophthalate, phthalic acid, dimethyl phthalate, phthalic anhydride, 2,6-naphthalenedicarboxylic acid, dimethyl 2,6-naphthalenedicarboxylate, diphenyldicarboxylic acid, 1,4-cyclohexanedicarboxylic acid, 1,3-cyclohexanedicarboxylic acid, dimethyl 1,4-cyclohexanedicarboxylate, dimethyl 1,3-cyclohexanedicarboxylate, sebacic acid, succinic acid, isodecylsuccinic acid, maleic acid, maleic anhydride, fumaric acid, adipic acid, glutaric acid, and azelaic acid.
[0016] Diol The diol component used in the present invention means a main monomer constituting a polyester copolymer together with the above-mentioned dicarboxylic acid or its derivative. In particular, the diol component includes ethylene glycol and a comonomer, and the comonomer is diethylene glycol, cyclohexanedimethanol, a cyclohexanedimethanol derivative, or a combination thereof. Preferably, the cyclohexanedimethanol derivative is 4-(hydroxymethyl)cyclohexylmethyl 4-(hydroxymethyl)cyclohexanecarboxylate or 4-(4-(hydroxymethyl)cyclohexylmethoxymethyl)cyclohexylmethanol. Preferably, when the polyester resin according to the present invention includes a cyclohexanedimethanol derivative, the polyester resin includes 0.1 to 25 mol % of diol portions derived from 4-(hydroxymethyl)cyclohexylmethyl 4-(hydroxymethyl)cyclohexanecarboxylate and 4-(4-(hydroxymethyl)cyclohexylmethoxymethyl)cyclohexylmethanol based on the total diol portion.
[0017] In addition, preferably, the comonomer may further include 1,2-propanediol, 1,3-propanediol, 2-methyl-1,3-propanediol, 2-methylene-1,3-propanediol, 2-ethyl-1,3-propanediol, 2-isopropyl-1,3-propanediol, 2,2-dimethyl-1,3-propanediol, 1,4-butanediol, 2,3-butanediol, 3-methyl-1,5-pentanediol, 3-methyl-2,4-pentanediol, 1,6-hexanediol, 1,2-cyclohexanediol, 1,4-cyclohexanediol, diethylene glycol, or a mixture thereof.
[0018] The diethylene glycol in the comonomer is a component that contributes to improving the color properties of the polyester copolymer. Preferably, the diethylene glycol residue is contained in an amount of 5 to 50 moles relative to 100 moles of the total diol component residues. More preferably, the diethylene glycol residue is contained in an amount of 6 moles or more, 7 moles or more, or 8 moles or more, and 45 moles or less, 40 moles or less, 35 moles or less, 30 moles or less, 25 moles or less, or 20 moles or less, relative to 100 moles of the total diol component residues.
[0019] The ethylene glycol is a component that contributes to improving the transparency and impact strength of the polyester copolymer. Preferably, the ethylene glycol residue is contained in an amount of 30 to 80 mol relative to 100 mol of the total diol component residues. More preferably, the ethylene glycol residue is contained in an amount of 35 mol or more, 40 mol or more, 45 mol or more, 50 mol or more, or 55 mol or more and 75 mol or less relative to 100 mol of the total diol component residues.
[0020] The cyclohexanedimethanol (e.g., 1,2-cyclohexanedimethanol, 1,3-cyclohexanedimethanol, or 1,4-cyclohexanedimethanol) is a component that contributes to improving the transparency and impact strength of the polyester copolymer produced. Preferably, the cyclohexanedimethanol residue is contained in an amount of 5 to 40 mol relative to 100 mol of the total diol component residues. More preferably, the cyclohexanedimethanol residue is contained in an amount of 7 mol to 35 mol relative to 100 mol of the total diol component residues.
[0021] Recycled bis-2-hydroxyethyl terephthalate The term "recycled bis-2-hydroxyethyl terephthalate" used in the present invention refers to a material obtained from waste plastics that have been recovered after use. Waste plastics from which the bis-2-hydroxyethyl terephthalate can be obtained include PET and PETG. For example, bis-2-hydroxyethyl terephthalate can be obtained from recovered PEG by methods such as glycolysis, hydrolysis, and methanolysis, and these methods are widely known in the art.
[0022] The recycled bis-2-hydroxyethyl terephthalate undergoes various chemical steps in the process of obtaining it from waste plastics, and therefore, when it is used as a monomer for a copolymer, the product quality inevitably deteriorates. In particular, when it is used as a monomer for a polyester copolymer, the color quality deteriorates and a large amount of by-products are generated as described below.
[0023] Therefore, in the present invention, the recycled bis-2-hydroxyethyl terephthalate is used as a main monomer constituting the polyester copolymer according to the present invention, and the polyester copolymer is adjusted to contain 10 to 90% by weight of the residue of the recycled bis-2-hydroxyethyl terephthalate. If the residue of the recycled bis-2-hydroxyethyl terephthalate is less than 10% by weight, the content of the above-mentioned diol is relatively high, which increases the amount of by-products derived from the diol component, especially by-products derived from ethylene glycol, which is one factor in the deterioration of the quality of the polyester copolymer. In addition, if the residue of the recycled bis-2-hydroxyethyl terephthalate exceeds 90% by weight, there is a problem that the color quality and transparency of the polyester copolymer are reduced.
[0024] Polyester Copolymer The polyester copolymer according to the present invention can be prepared by copolymerizing the above-mentioned recycled bis-2-hydroxyethyl terephthalate, dicarboxylic acid or its derivative, ethylene glycol and a comonomer. In this case, the copolymerization can be carried out in sequence through an esterification reaction (step 1) and a polycondensation reaction (step 2).
[0025] The esterification reaction is carried out in the presence of an esterification catalyst, and the esterification catalyst may include a zinc-based compound. Specific examples of such zinc-based catalysts include zinc acetate, zinc acetate dihydrate, zinc chloride, zinc sulfate, zinc sulfide, zinc carbonate, zinc citrate, zinc gluconate, or a mixture thereof. The amount of each starting material used is as described above.
[0026] The esterification reaction is carried out at a rate of 0 to 10.0 kg / cm 2 The esterification reaction can be carried out at a pressure of 0 to 5.0 kg / cm and a temperature of 150 to 300° C. The esterification reaction conditions can be appropriately adjusted depending on the specific properties of the polyester to be produced, the ratio of each component, or the process conditions. Specifically, a preferred example of the esterification reaction conditions is a pressure of 0 to 5.0 kg / cm. 2 , more preferably 0.1 to 3.0 kg / cm2 and the temperature is preferably from 200 to 270°C, more preferably from 240 to 260°C.
[0027] The esterification reaction may be carried out in a batch or continuous manner, and each raw material may be added separately, but it is preferable to add the diol component in the form of a slurry mixed with the dicarboxylic acid component and recycled bis-2-hydroxyethyl terephthalate. The diol component such as isosorbide, which is a solid at room temperature, may be dissolved in water or ethylene glycol and then mixed with the dicarboxylic acid component such as terephthalic acid to prepare a slurry. Alternatively, the dicarboxylic acid component such as terephthalic acid may be mixed with the other diol component after melting isosorbide at 60°C or higher to prepare a slurry. Water may be added to the mixed slurry to increase the fluidity of the slurry.
[0028] The polycondensation reaction can be carried out by reacting the esterification reaction product at a temperature of 150 to 300° C. under reduced pressure conditions of 600 to 0.01 mmHg for 1 to 24 hours.
[0029] Such polycondensation reaction is carried out at a reaction temperature of 150 to 300°C, preferably 200 to 290°C, more preferably 260 to 280°C; and under reduced pressure conditions of 600 to 0.01 mmHg, preferably 200 to 0.05 mmHg, more preferably 100 to 0.1 mmHg. By applying reduced pressure conditions to the polycondensation reaction, glycol, which is a by-product of the polycondensation reaction, can be removed from the system. Therefore, if the polycondensation reaction exceeds the reduced pressure range of 400 to 0.01 mmHg, the removal of the by-product may be insufficient. In addition, if the polycondensation reaction occurs outside the temperature range of 150 to 300°C, if the condensation polymerization reaction proceeds at 150°C or less, glycol, which is a by-product of the polycondensation reaction, cannot be effectively removed from the system, the intrinsic viscosity of the final reaction product is low, and the physical properties of the polyester resin produced are deteriorated, and if the reaction proceeds at 300°C or more, the appearance of the polyester resin produced is likely to be yellow. The polycondensation reaction is carried out for a time required for the intrinsic viscosity of the final reaction product to reach an appropriate level, for example, an average residence time of 1 to 24 hours.
[0030] The polycondensation reaction may use a polycondensation catalyst including a titanium-based compound, a germanium-based compound, an antimony-based compound, an aluminum-based compound, a tin-based compound, or a mixture thereof.
[0031] Examples of the titanium-based compound include tetraethyl titanate, acetyl tripropyl titanate, tetrapropyl titanate, tetrabutyl titanate, 2-ethylhexyl titanate, octylene glycol titanate, lactate titanate, triethanolamine titanate, acetylacetonate titanate, ethyl acetoacetic ester titanate, isostearyl titanate, titanium dioxide, etc. Examples of the germanium-based compound include germanium dioxide, germanium tetrachloride, germanium ethylene glycol oxide, germanium acetate, copolymers thereof, or mixtures thereof. Preferably, germanium dioxide can be used, and as such germanium dioxide, either crystalline or non-crystalline can be used, and glycol-soluble can also be used.
[0032] Meanwhile, the polyester copolymer according to the present invention has an extrudability coefficient of 1 or more in the above formula 1. As described in the examples below, when the extrudability coefficient is 1 or more, the plate-out phenomenon of the roll during extrusion is reduced, outgas is reduced, and extrudability is excellent, and therefore extrusion processability is excellent. On the other hand, when the extrudability coefficient is less than 1, the plate-out phenomenon of the roll during extrusion is increased, productivity is reduced, and outgas is increased, adversely affecting the quality of the manufactured sheet.
[0033] Preferably, the polyester copolymer according to the present invention has an extrudability coefficient of Formula 1 of 1 or more, 2 or more, 3 or more, 4 or more, 5 or more, 6 or more, 7 or more, 8 or more, 9 or more, or 10 or more. Meanwhile, since a higher extrudability coefficient means better extrusion processability, there is no theoretical upper limit, but the extrudability coefficient may be, for example, 200 or less, 190 or less, 180 or less, 170 or less, 160 or less, 150 or less, 140 or less, 130 or less, 120 or less, 110 or less, or 100 or less.
[0034] Meanwhile, in the above Equation 1, the values of the variables A to D are applied with the units removed. For example, in relation to the variable A, when the content of the part derived from the recycled bis-2-hydroxyethyl terephthalate in the polyester copolymer is 50 wt%, A is 50. The variables A to D can be obtained by analyzing the produced polyester copolymer, and the specific method will be embodied in the examples described later.
[0035] Meanwhile, the variable D is the content (area / g) of the oligomer in the polyester copolymer, and specifically, the oligomer means a low molecular weight having a weight average molecular weight of 1,000 or less. A method for measuring the content of the oligomer in the polyester copolymer will be described in detail in the examples below.
[0036] The polyester copolymer according to the present invention has an intrinsic viscosity of 0.50 to 1.0 dl / g, preferably 0.50 to 0.85 dl / g, more preferably 0.55 to 0.80 dl / g or 0.60 to 0.80 dl / g. The method for measuring the intrinsic viscosity will be described in the examples described later.
[0037] The present invention further provides an article comprising the polyester copolymer.
[0038] The polyester copolymer produced by the above-mentioned method can be in the form of chips, pellets, or powder before molding, or can be in the form of a molded product, for example, a film or sheet, formed by another molding process such as extrusion or injection, and is preferably in the form of a film, a heat shrinkable film, a sheet, a profile, or a blown film. Effect of the Invention
[0039] The polyester copolymer according to the present invention described above contains recycled monomers and has excellent extrusion processability, and is applicable to the production of various articles, particularly films. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0040] Hereinafter, preferred examples will be presented for understanding the present invention. However, the following examples are provided only to facilitate understanding of the present invention, and are not intended to limit the scope of the present invention.
[0041] Example 1 Into a 10 L reactor connected to a column and a condenser that can be cooled by water, recycled bis-2-hydroxyethyl terephthalate (689.8 g; hereinafter referred to as "r-BHET"), TPA (terephthalic acid; 2554.5 g), EG (ethylene glycol; 755.4 g), CHDM (1,4-cyclohexanedimethanol; 826.4 g), and DEG (diethylene glycol; 211.1 g) were added, along with TiO2 (1.0 g) as a catalyst, phosphoric acid (phosphoric acid, 1.5 g) as a stabilizer, Clarient's blue toner (0.006 g), and Clarient's red toner (0.004 g).
[0042] Next, nitrogen was injected into the reactor until the reactor pressure was 2.0 kgf / cm above normal pressure. 2 The reactor was pressurized to a high pressure (absolute pressure: 2231.1 mmHg). The temperature of the reactor was then raised to 220°C over 90 minutes, maintained at 220°C for 2 hours, and then raised to 260°C over 2 hours. The temperature of the reactor was then maintained at 260°C until the mixture in the reactor was transparent when observed with the naked eye, and the esterification reaction was allowed to proceed. During this process, by-products were discharged through a column and a condenser. When the esterification reaction was completed, the nitrogen in the pressurized reactor was discharged to the outside, the pressure in the reactor was reduced to normal pressure, and the mixture in the reactor was transferred to a 7L reactor capable of vacuum reaction.
[0043] The pressure of the reactor was then lowered to 5 Torr (absolute pressure: 5 mmHg) over 30 minutes under normal pressure, and the temperature of the reactor was raised to 265°C over 1 hour, and the polycondensation reaction was carried out while maintaining the pressure of the reactor at 1 Torr (absolute pressure: 1 mmHg) or less. The stirring speed was set to be fast at the beginning of the polycondensation reaction, but if the stirring force weakens due to an increase in the viscosity of the reactants as the polycondensation reaction proceeds, or if the temperature of the reactants rises above the set temperature, the stirring speed can be appropriately adjusted. The polycondensation reaction was carried out until the intrinsic viscosity (IV) of the mixture (melt) in the reactor was 0.70 dl / g. When the intrinsic viscosity of the mixture in the reactor reached a desired level, the mixture was discharged outside the reactor and made into strands, which were solidified with a cooling liquid and then granulated to an average weight of about 12 to 14 mg to produce a polyester copolymer.
[0044] Example 2 Into a 10 L reactor connected to a column and a condenser that can be cooled by water, r-BHET (2248.9 g), TPA (1202.5 g), EG (182.6 g), and CHDM (734.8 g) were added, and TiO2 (1.0 g) as a catalyst, phosphoric acid (1.5 g) as a stabilizer, and cobalt acetate (0.7 g) as a coloring agent were added.
[0045] Next, nitrogen was injected into the reactor until the reactor pressure was 2.0 kgf / cm above normal pressure. 2 The reactor was pressurized to a high pressure (absolute pressure: 2231.1 mmHg). The temperature of the reactor was then raised to 220°C over 90 minutes, maintained at 220°C for 2 hours, and then raised to 255°C over 2 hours. The temperature of the reactor was then maintained at 255°C until the mixture in the reactor was transparent when observed with the naked eye, and the esterification reaction was allowed to proceed. During this process, by-products were discharged through a column and a condenser. When the esterification reaction was completed, the nitrogen in the pressurized reactor was discharged to the outside, the pressure in the reactor was reduced to normal pressure, and the mixture in the reactor was transferred to a 7L reactor capable of vacuum reaction.
[0046] The pressure of the reactor was then lowered to 5 Torr (absolute pressure: 5 mmHg) over 30 minutes under normal pressure, and the temperature of the reactor was raised to 285°C over 1 hour, and the polycondensation reaction was carried out while maintaining the pressure of the reactor at 1 Torr (absolute pressure: 1 mmHg) or less. The stirring speed was set to be fast at the beginning of the polycondensation reaction, but if the stirring force weakens due to an increase in the viscosity of the reactants as the polycondensation reaction proceeds, or if the temperature of the reactants rises above the set temperature, the stirring speed can be appropriately adjusted. The polycondensation reaction was carried out until the intrinsic viscosity (IV) of the mixture (melt) in the reactor was 0.70 dl / g. When the intrinsic viscosity of the mixture in the reactor reached a desired level, the mixture was discharged outside the reactor and made into strands, which were solidified with a cooling liquid and then granulated to an average weight of about 12 to 14 mg to produce a polyester copolymer.
[0047] Example 3 A 10 L reactor connected to a column and a water-coolable condenser was charged with r-BHET (3291.8 g), TPA (717.1 g), EG (21.4 g), CHDM (522.5 g), and DEG (311.4 g), TiO2 (1.0 g) as a catalyst, phosphoric acid (1.5 g) as a stabilizer, Clarient blue toner (0.007 g), and Clarient red toner (0.004 g).
[0048] Next, nitrogen was injected into the reactor until the reactor pressure was 2.0 kgf / cm above normal pressure. 2 The reactor was pressurized to a high pressure (absolute pressure: 2231.1 mmHg). The temperature of the reactor was then raised to 220°C over 90 minutes, maintained at 220°C for 2 hours, and then raised to 255°C over 2 hours. The temperature of the reactor was then maintained at 255°C until the mixture in the reactor was transparent when observed with the naked eye, and the esterification reaction was allowed to proceed. During this process, by-products were discharged through a column and a condenser. When the esterification reaction was completed, the nitrogen in the pressurized reactor was discharged to the outside, the pressure in the reactor was reduced to normal pressure, and the mixture in the reactor was transferred to a 7L reactor capable of vacuum reaction.
[0049] The pressure of the reactor was then lowered to 5 Torr (absolute pressure: 5 mmHg) over 30 minutes under normal pressure, and the temperature of the reactor was raised to 285°C over 1 hour, and the polycondensation reaction was carried out while maintaining the pressure of the reactor at 1 Torr (absolute pressure: 1 mmHg) or less. The stirring speed was set to be fast at the beginning of the polycondensation reaction, but if the stirring force weakens due to an increase in the viscosity of the reactants as the polycondensation reaction proceeds, or if the temperature of the reactants rises above the set temperature, the stirring speed can be appropriately adjusted. The polycondensation reaction was carried out until the intrinsic viscosity (IV) of the mixture (melt) in the reactor was 0.70 dl / g. When the intrinsic viscosity of the mixture in the reactor reached a desired level, the mixture was discharged outside the reactor and made into strands, which were solidified with a cooling liquid and then granulated to an average weight of about 12 to 14 mg to produce a polyester copolymer.
[0050] Example 4 A 10 L reactor with a column and a water-coolable condenser was charged with r-BHET (4388.5 g), TPA (151.0 g), EG (45.1 g), CHDM (261.9 g), DEG (239.0 g), CHDM derivative (341.2 g; i) 4-(hydroxymethyl)cyclohexylmethyl 4-(hydroxymethyl)cyclohexanecarboxylate, and ii) 4-(4-(hydroxymethyl)cyclohexylmethoxymethyl)cyclohexylmethanol in a 1:3 molar ratio, GeO2 (1.0 g) as catalyst, phosphoric acid (1.5 g) as stabilizer, blue toner (Clarient) (0.020 g), and red toner (Clarient) (0.008 g).
[0051] Next, nitrogen was injected into the reactor so that the pressure in the reactor was 0.5 kgf / cm above normal pressure. 2The reactor was pressurized to a high pressure (absolute pressure: 1127.8 mmHg). The temperature of the reactor was then raised to 220°C over 90 minutes, maintained at 220°C for 2 hours, and then raised to 260°C over 2 hours. The temperature of the reactor was then maintained at 260°C until the mixture in the reactor was transparent when observed with the naked eye, and the esterification reaction was allowed to proceed. During this process, by-products were discharged through a column and a condenser. When the esterification reaction was completed, the nitrogen in the pressurized reactor was discharged to the outside, the pressure in the reactor was reduced to normal pressure, and the mixture in the reactor was transferred to a 7L reactor capable of vacuum reaction.
[0052] The pressure of the reactor was then lowered to 5 Torr (absolute pressure: 5 mmHg) over 30 minutes under normal pressure, and the temperature of the reactor was raised to 275°C over 1 hour, and the polycondensation reaction was carried out while maintaining the pressure of the reactor at 1 Torr (absolute pressure: 1 mmHg) or less. The stirring speed was set to be fast at the beginning of the polycondensation reaction, but if the stirring force weakens due to an increase in the viscosity of the reactants as the polycondensation reaction proceeds, or if the temperature of the reactants rises above the set temperature, the stirring speed can be appropriately adjusted. The polycondensation reaction was carried out until the intrinsic viscosity (IV) of the mixture (melt) in the reactor was 0.80 dl / g. When the intrinsic viscosity of the mixture in the reactor reached a desired level, the mixture was discharged outside the reactor and made into strands, which were solidified with a cooling liquid and then granulated to an average weight of about 12 to 14 mg to produce a polyester copolymer.
[0053] Example 5 Into a 10 L reactor connected to a column and a condenser that can be cooled by water, r-BHET (1005.9 g), DMT (dimethyl terephthalate; 2304.9 g), EG (874.1 g), CHDM (707.2 g), and DEG (231.3 g) were added, and Mn(II) acetate tetrahydrate (1.5 g) and Sb2O3 (1.8 g) were added as catalysts, and cobalt acetate (0.6 g) was added as a coloring agent.
[0054] Next, nitrogen was injected into the reactor so that the pressure in the reactor was 0.1 kgf / cm above normal pressure. 2 The reactor was pressurized to a high pressure (absolute pressure: 833.6 mmHg). The temperature of the reactor was then raised to 220°C over 90 minutes, maintained at 220°C for 2 hours, and then raised to 240°C over 2 hours. The temperature of the reactor was then maintained at 240°C until the mixture in the reactor was transparent when observed with the naked eye, and the esterification reaction was allowed to proceed. During this process, by-products were discharged through a column and a condenser. When the esterification reaction was completed, the nitrogen in the pressurized reactor was discharged to the outside, the pressure in the reactor was reduced to normal pressure, and the mixture in the reactor was transferred to a 7L reactor capable of vacuum reaction.
[0055] The pressure of the reactor was then lowered to 5 Torr (absolute pressure: 5 mmHg) over 30 minutes under normal pressure, and the temperature of the reactor was raised to 265°C over 1 hour, and the polycondensation reaction was carried out while maintaining the pressure of the reactor at 1 Torr (absolute pressure: 1 mmHg) or less. The stirring speed was set to be fast at the beginning of the polycondensation reaction, but if the stirring force weakens due to an increase in the viscosity of the reactants as the polycondensation reaction proceeds, or if the temperature of the reactants rises above the set temperature, the stirring speed can be appropriately adjusted. The polycondensation reaction was carried out until the intrinsic viscosity (IV) of the mixture (melt) in the reactor was 0.70 dl / g. When the intrinsic viscosity of the mixture in the reactor reached a desired level, the mixture was discharged outside the reactor and made into strands, which were solidified with a cooling liquid and then granulated to an average weight of about 12 to 14 mg to produce a polyester copolymer.
[0056] Example 6 Into a 10 L reactor connected to a column and a condenser that can be cooled by water, r-BHET (2283.5 g), TPA (1221.0 g), IPA (isophthalic acid; 1492.4 g), EG (185.5 g), CHDM (746.2 g), and GeO2 (1.0 g) were added as a catalyst.
[0057] Next, nitrogen was injected into the reactor until the reactor pressure was 2.0 kgf / cm above normal pressure.2 The reactor was pressurized to a high pressure (absolute pressure: 2231.1 mmHg). The temperature of the reactor was then raised to 220°C over 90 minutes, maintained at 220°C for 2 hours, and then raised to 255°C over 2 hours. The temperature of the reactor was then maintained at 255°C until the mixture in the reactor was transparent when observed with the naked eye, and the esterification reaction was allowed to proceed. During this process, by-products were discharged through a column and a condenser. When the esterification reaction was completed, the nitrogen in the pressurized reactor was discharged to the outside, the pressure in the reactor was reduced to normal pressure, and the mixture in the reactor was transferred to a 7L reactor capable of vacuum reaction.
[0058] The pressure of the reactor was then lowered to 5 Torr (absolute pressure: 5 mmHg) over 30 minutes under normal pressure, and the temperature of the reactor was raised to 285°C over 1 hour, and the polycondensation reaction was carried out while maintaining the pressure of the reactor at 1 Torr (absolute pressure: 1 mmHg) or less. The stirring speed was set to be fast at the beginning of the polycondensation reaction, but if the stirring force weakens due to an increase in the viscosity of the reactants as the polycondensation reaction proceeds, or if the temperature of the reactants rises above the set temperature, the stirring speed can be appropriately adjusted. The polycondensation reaction was carried out until the intrinsic viscosity (IV) of the mixture (melt) in the reactor was 0.70 dl / g. When the intrinsic viscosity of the mixture in the reactor reached a desired level, the mixture was discharged outside the reactor and made into strands, which were solidified with a cooling liquid and then granulated to an average weight of about 12 to 14 mg to produce a polyester copolymer.
[0059] Comparative Example 1 Into a 10 L reactor connected to a column and a condenser that can be cooled by water, TPA (3005.3 g), EG (1088.8 g), CHDM (834.3 g), and DEG (211.1 g) were added, along with TiO2 (1.0 g) as a catalyst and phosphoric acid (1.5 g) as a stabilizer.
[0060] Next, nitrogen was injected into the reactor until the reactor pressure was 2.0 kgf / cm above normal pressure. 2The reactor was pressurized to a high pressure (absolute pressure: 2231.1 mmHg). The temperature of the reactor was then raised to 220°C over 90 minutes, maintained at 220°C for 2 hours, and then raised to 255°C over 2 hours. The esterification reaction was then carried out by maintaining the temperature of the reactor at 255°C until the mixture in the reactor was transparent when observed with the naked eye. During this process, by-products were discharged through a column and a condenser. When the esterification reaction was completed, the nitrogen in the pressurized reactor was discharged to the outside, the pressure in the reactor was reduced to normal pressure, and the mixture in the reactor was transferred to a 7L reactor capable of vacuum reaction.
[0061] The pressure of the reactor was then lowered to 5 Torr (absolute pressure: 5 mmHg) over 30 minutes under normal pressure, and the temperature of the reactor was raised to 285°C over 1 hour, and the polycondensation reaction was carried out while maintaining the pressure of the reactor at 1 Torr (absolute pressure: 1 mmHg) or less. The stirring speed was set to be fast at the beginning of the polycondensation reaction, but if the stirring force weakens due to an increase in the viscosity of the reactants as the polycondensation reaction proceeds, or if the temperature of the reactants rises above the set temperature, the stirring speed can be appropriately adjusted. The polycondensation reaction was carried out until the intrinsic viscosity (IV) of the mixture (melt) in the reactor was 0.70 dl / g. When the intrinsic viscosity of the mixture in the reactor reached a desired level, the mixture was discharged outside the reactor and made into strands, which were solidified with a cooling liquid and then granulated to an average weight of about 12 to 14 mg to produce a polyester copolymer.
[0062] Comparative Example 2 A 10 L reactor connected to a column and a water-coolable condenser was charged with TPA (2780.6 g), EG (1495.5 g), CHDM (241.2 g), DEG (159.8 g), and CHDM derivatives (341.2 g; i) 4-(hydroxymethyl)cyclohexylmethyl 4-(hydroxymethyl)cyclohexanecarboxylate, and ii) 4-(4-(hydroxymethyl)cyclohexylmethoxymethyl)cyclohexylmethanol in a molar ratio of 1:3. TiO2 (1.0 g) was added as a catalyst, phosphoric acid (1.5 g) as a stabilizer, and cobalt acetate (0.7 g) as a coloring agent.
[0063] Next, nitrogen was injected into the reactor until the reactor pressure was 2.0 kgf / cm above normal pressure. 2 The reactor was pressurized to a high pressure (absolute pressure: 2231.1 mmHg). The temperature of the reactor was then raised to 220°C over 90 minutes, maintained at 220°C for 2 hours, and then raised to 255°C over 2 hours. The temperature of the reactor was then maintained at 255°C until the mixture in the reactor was transparent when observed with the naked eye, and the esterification reaction was allowed to proceed. During this process, by-products were discharged through a column and a condenser. When the esterification reaction was completed, the nitrogen in the pressurized reactor was discharged to the outside, the pressure in the reactor was reduced to normal pressure, and the mixture in the reactor was transferred to a 7L reactor capable of vacuum reaction.
[0064] The pressure of the reactor was then lowered to 5 Torr (absolute pressure: 5 mmHg) over 30 minutes under normal pressure, and the temperature of the reactor was raised to 260°C over 1 hour, and the polycondensation reaction was carried out while maintaining the pressure of the reactor at 1 Torr (absolute pressure: 1 mmHg) or less. The stirring speed was set to be fast at the beginning of the polycondensation reaction, but if the stirring force weakens due to an increase in the viscosity of the reactants as the polycondensation reaction proceeds, or if the temperature of the reactants rises above the set temperature, the stirring speed can be appropriately adjusted. The polycondensation reaction was carried out until the intrinsic viscosity (IV) of the mixture (melt) in the reactor was 0.85 dl / g. When the intrinsic viscosity of the mixture in the reactor reached a desired level, the mixture was discharged outside the reactor and made into strands, which were solidified with a cooling liquid and then granulated to an average weight of about 12 to 14 mg to produce a polyester copolymer.
[0065] Comparative Example 3 Into a 10 L reactor connected to a column and a condenser that can be cooled by water, TPA (3631.3 g), EG (2780.3 g), DEG (159.7 g), GeO2 (1.0 g) as a catalyst, and phosphoric acid (1.5 g) as a stabilizer were added.
[0066] Next, nitrogen was injected into the reactor until the reactor pressure was 1.0 kgf / cm above normal pressure. 2 The reactor was pressurized to a high pressure (absolute pressure: 1495.6 mmHg). The temperature of the reactor was then raised to 220°C over 90 minutes, maintained at 220°C for 2 hours, and then raised to 265°C over 2 hours. The temperature of the reactor was then maintained at 255°C until the mixture in the reactor was transparent when observed with the naked eye, and the esterification reaction was allowed to proceed. During this process, by-products were discharged through a column and a condenser. When the esterification reaction was completed, the nitrogen in the pressurized reactor was discharged to the outside, the pressure in the reactor was reduced to normal pressure, and the mixture in the reactor was transferred to a 7L reactor capable of vacuum reaction.
[0067] The pressure of the reactor was then lowered to 5 Torr (absolute pressure: 5 mmHg) over 30 minutes under normal pressure, and the temperature of the reactor was raised to 275°C over 1 hour, and the polycondensation reaction was carried out while maintaining the pressure of the reactor at 1 Torr (absolute pressure: 1 mmHg) or less. The stirring speed was set to be fast at the beginning of the polycondensation reaction, but if the stirring force weakens due to an increase in the viscosity of the reactants as the polycondensation reaction proceeds, or if the temperature of the reactants rises above the set temperature, the stirring speed can be appropriately adjusted. The polycondensation reaction was carried out until the intrinsic viscosity (IV) of the mixture (melt) in the reactor was 0.60 dl / g. When the intrinsic viscosity of the mixture in the reactor reached a desired level, the mixture was discharged outside the reactor and made into strands, which were solidified with a cooling liquid and then granulated to an average weight of about 12 to 14 mg to produce a polyester copolymer.
[0068] Comparative Example 4 Into a 10 L reactor connected to a column and a condenser that can be cooled by water, TPA (2300.2 g), NPG (neopentyl glycol; 158.0 g), DEG (202.3 g), GeO2 (1.0 g) as a catalyst, and phosphoric acid (1.5 g) as a stabilizer were added.
[0069] Next, nitrogen was injected into the reactor until the reactor pressure was 2.0 kgf / cm above normal pressure. 2 The reactor was pressurized to a high pressure (absolute pressure: 2231.1 mmHg). The temperature of the reactor was then raised to 220°C over 90 minutes, maintained at 220°C for 2 hours, and then raised to 265°C over 2 hours. The temperature of the reactor was then maintained at 255°C until the mixture in the reactor was transparent when observed with the naked eye, and the esterification reaction was allowed to proceed. During this process, by-products were discharged through a column and a condenser. When the esterification reaction was completed, the nitrogen in the pressurized reactor was discharged to the outside, the pressure in the reactor was reduced to normal pressure, and the mixture in the reactor was transferred to a 7L reactor capable of vacuum reaction.
[0070] The pressure in the reactor was then lowered to 5 Torr (absolute pressure: 5 mmHg) over 30 minutes under normal pressure, and the temperature of the reactor was raised to 280°C over 1 hour, and the polycondensation reaction was carried out while maintaining the pressure in the reactor at 1 Torr (absolute pressure: 1 mmHg) or less. The stirring speed was set to be fast at the beginning of the polycondensation reaction, but if the stirring force weakens due to an increase in the viscosity of the reactants as the polycondensation reaction proceeds, or if the temperature of the reactants rises above the set temperature, the stirring speed can be appropriately adjusted. The polycondensation reaction was carried out until the intrinsic viscosity (IV) of the mixture (melt) in the reactor was 0.70 dl / g. When the intrinsic viscosity of the mixture in the reactor reached a desired level, the mixture was discharged outside the reactor and made into strands, which were solidified with a cooling liquid and then granulated to an average weight of about 12 to 14 mg to produce a polyester copolymer.
[0071] Experimental Example The physical properties of the copolymers prepared in the above examples and comparative examples were evaluated as follows.
[0072] 1) Residue composition The composition (wt%) derived from r-BHET and the composition (mol%) derived from diol residues in the polyester resin were confirmed by dissolving the sample in CDCl3 solvent at a concentration of 3 mg / mL and then measuring the 1H-NMR spectrum obtained at 25°C using a nuclear magnetic resonance device (JEOL, 600 MHz FT-NMR). The composition of diol-derived residues was analyzed in terms of the total composition of all residues derived from diols and the mol% of residues released from each specific diol (DEG and CHDM).
[0073] 2) Intrinsic viscosity After dissolving the polyester copolymer at a concentration of 0.12% in orthochlorophenol (OCP) at 150°C, the intrinsic viscosity was measured using an Ubbelohde viscometer in a thermostatic bath at 35°C. Specifically, the temperature of the viscosity tube was maintained at 35°C, and the efflux time t0 taken for the solvent to pass between specific internal sections of the viscosity tube and the time t taken for the solution to pass through were determined. The t0 and t values were then substituted into Equation 1 to calculate the specific viscosity, and the calculated specific viscosity value was substituted into Equation 2 to calculate the intrinsic viscosity.
[0074]
number
[0075]
number
[0076] 3) HPLC / residual acid, BHET measurement High-performance liquid chromatography was used to measure the amount of unreacted and residual acids and diols in the pellet samples. Specifically, the residual monomers (TPA, DMT, BHET, IPA, etc.) were extracted by reprecipitation.
[0077] The standard solution for HPLC was prepared by dissolving 0.01 g of the monomer to be quantified (TPA, BHET, DMT, IPA, etc.) in 20 mL of MeOH (500 μg / mL), then serially diluting with MeOH to match the range of the calibration curve sample. The sample was pretreated by dissolving approximately 0.1 g of the pellet sample in 1 mL of HFIP (shaker 180 rpm, stirring for 1 hour or more), and after confirming complete dissolution, adding 3 mL of MeOH to reprecipitate.
[0078] In addition, the mobile phase must be set in order to apply liquid chromatography mass spectrometry, so mobile phase A was prepared by mixing distilled water and H3PO4 to a pH of 2, and acetonitrile was used as mobile phase B. The HPLC measurement conditions are summarized as follows.
[0079] -Maker: Mightysil C18(4.0*250mm), (5μm) -Mobile phase:H2O&H3PO4 / acetonitrile(Gradient) -Flow rate: 1.2ml / min -Wavelength for detection:242nm -Retention time: about 30 minutes -Injection volume: 10um After creating a calibration curve using standard solutions, the correlation coefficient (r 2 The linearity was confirmed during the analysis of the samples for accuracy / precision. The acceptance criteria are that the deviation from the theoretical value must be within 20% at the lowest quantification limit, and the deviation from the theoretical value must be within 15% at concentrations other than the lowest quantification limit. 2 (Correlation coefficient) must be 0.98 or higher.
[0080] 4) GC total area / g For quantitative analysis of oligomers and single molecules by pyrolysis of polymer, gas chromatography was used to collect gaseous substances generated under the following pretreatment conditions and converted into the total area / g of the graph.
[0081] The pretreatment conditions were as follows: pellet sample was heated at 260℃ in an air atmosphere for 1 hour, the substances generated during the heating were collected in the GC head space, and the total area of the collected substances was quantified (unit: area / g). The higher the total area / g value, the more unreacted substances and oligomers there are inside the pellet, and the more monomolecular substances generated by thermal decomposition. The area / g of oligomers detected by GC usually means substances with a molecular weight of 1000 or less. The GC measurement conditions are summarized as follows:
[0082] GC Instrument Conditions -Model:Triplus500(Thermo) -Incubation temperature:260℃ -Incubation time: 60 min -Loop temperature: 260℃ -Loop volume: 1mL -Injection time: 0.5 min -Injection mode:standard 5) Extrusion coefficient Applying the above data and Equation 1 herein, the extrudability coefficient was determined.
[0083] 6) Extrusion property 6-1) Plate-out evaluation Using a Breyer apparatus having the following specifications, the samples according to the examples and comparative examples were subjected to extrusion evaluation.
[0084] -Supplier: Breyer GmbH (Germany, December, 2000) -Main extruder:Single screw extruder with or without venting section -Diameter: 45mm -L / D:33:1 The extrusion was evaluated at 260°C to obtain a sheet sample having a thickness of 0.25 to 1 mm, and one hour after the start of sheet extrusion, the plate-out phenomenon of the roll during extrusion was evaluated. The sensory evaluation was performed based on the degree of contamination of the roll after sheet extrusion, as follows:
[0085] -X:No roll contamination after sheet extrusion -△: Small amount of contamination occurs on the roll after extrusion of the sheet -○: Roll contamination after sheet extrusion In the samples prepared as examples and comparative examples, the more unreacted monomers, residual monomers, and oligomers (total area / g) generated by thermal decomposition, the more monomolecules are generated during sheet extrusion, which increases the degree of contamination of the roll and induces a decrease in quality and productivity during sheet extrusion.
[0086] 5-2) Out-gas generation evaluation Using the same equipment, samples prepared from the examples and comparative examples were subjected to extrusion evaluation, and a sensory evaluation was carried out on the out-gas generated when each pellet passed through the extruder and was pressed against the roll.
[0087] -◎: No out gas generation / checked 6 times at 10 minute intervals -○: Almost no out gas generation -△:Out gas occurs slightly -X:out gas occurs continuously 7) Stretchability In order to evaluate the quality of the extruded sheet, the polyester film (0.25 um) produced above was cut into a 10 cm x 10 cm square, and stretched with a stretch ratio (DR) of MD:TD = 1:5 at a stretching temperature of 75 to 95°C while reheating.
[0088] When the quality of the polyester film is deteriorated, the surface of the film is not uniform and fish eyes occur in the stretched film, and the stretching of the part where the fish eyes occur is uneven. In this case, the quality of the stretched film is affected and it is difficult to ensure the desired shrinkage ratio of the stretched film.
[0089] The polyester sheet produced above was cut into a square of 10 cm x 10 cm, and a fish eye sensory evaluation was performed with the naked eye within a stretched film having a stretch ratio (DR) of MD:TD = 1:5.
[0090] -X:fish eye almost none -△: Fish eye occurs slightly -○: Uneven stretching The results are shown in Table 1 below.
[0091] [Table 1]
Claims
1. 1) recycled bis-2-hydroxyethyl terephthalate; 2) acids including dicarboxylic acids or derivatives thereof, and 3) A diol containing ethylene glycol and a comonomer is polymerized, In the polyester resin having a structure in which a portion derived from the bis-2-hydroxyethyl terephthalate, an acid portion derived from the dicarboxylic acid or a derivative thereof, and a diol portion derived from the diol are repeated, The polyester copolymer has an extrudability coefficient of 1 or more as determined by the following Equation 1: Polyester Copolymer: [0010] In the above formula 1, A is the content (wt%) of the portion derived from the recycled bis-2-hydroxyethyl terephthalate in the polyester copolymer, B is the content (ppmw) of residual acid (acid) in the polyester copolymer, C is the content (ppmw) of residual recycled bis-2-hydroxyethyl terephthalate in the polyester copolymer; D is the content (area / g) of the oligomer in the polyester copolymer.
2. the polyester copolymer comprises 10 to 90 weight percent of a portion derived from the recycled bis-2-hydroxyethyl terephthalate; The polyester copolymer according to claim 1.
3. The comonomer is diethylene glycol, cyclohexanedimethanol, a cyclohexanedimethanol derivative, or a combination thereof; The polyester copolymer according to claim 1.
4. The cyclohexanedimethanol derivative is 4-(hydroxymethyl)cyclohexylmethyl 4-(hydroxymethyl)cyclohexanecarboxylate or 4-(4-(hydroxymethyl)cyclohexylmethoxymethyl)cyclohexylmethanol; The polyester copolymer according to claim 3.
5. The comonomer may additionally comprise 1,2-propanediol, 1,3-propanediol, 2-methyl-1,3-propanediol, 2-methylene-1,3-propanediol, 2-ethyl-1,3-propanediol, 2-isopropyl-1,3-propanediol, 2,2-dimethyl-1,3-propanediol, 1,4-butanediol, 2,3-butanediol, 3-methyl-1,5-pentanediol, 3-methyl-2,4-pentanediol, 1,6-hexanediol, 1,2-cyclohexanediol, 1,4-cyclohexanediol, diethylene glycol, or a mixture thereof; The polyester copolymer according to claim 1.
6. The acid containing the dicarboxylic acid or its derivative includes terephthalic acid. The polyester copolymer according to claim 1.
7. The acid containing a dicarboxylic acid or a derivative thereof includes any one or more selected from the group consisting of isophthalic acid, dimethyl isophthalate, phthalic acid, dimethyl phthalate, phthalic anhydride, 2,6-naphthalenedicarboxylic acid, dimethyl 2,6-naphthalenedicarboxylate, diphenyldicarboxylic acid, 1,4-cyclohexanedicarboxylic acid, 1,3-cyclohexanedicarboxylic acid, dimethyl 1,4-cyclohexanedicarboxylate, dimethyl 1,3-cyclohexanedicarboxylate, sebacic acid, succinic acid, isodecylsuccinic acid, maleic acid, maleic anhydride, fumaric acid, adipic acid, glutaric acid, and azelaic acid. The polyester copolymer according to claim 6.
8. The extrudability coefficient is 3 or more. The polyester copolymer according to claim 1.
9. The intrinsic viscosity of the polyester copolymer is 0.50 to 1.0 dl / g. The polyester copolymer according to claim 1.
10. An article comprising the polyester copolymer according to any one of claims 1 to 9.
11. The article is a film, a heat shrink film, a sheet, a profile, or a blown film; The article of claim 10.
Citation Information
Patent Citations
Polyester sheet
JP1998060239A
Polyester particle and production of container by using the same
JP1998204162A
Method for producing modified polyester resin
JP2002220443A
Process for reducing diethylene glycol formation in polyethylene terephthalate
JP2019011453A
KR20200061948A