Abrasive backing and method for making same

The abrasive backing, composed of wood fibers, synthetic fibers, and cellulose filaments with latex polymers and crosslinking agents, addresses breakage and tear issues, improving durability and sanding performance.

JP2024538206AInactive Publication Date: 2024-10-18NEENAH INC
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
JP2024523655
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2021-10-21
Filing Date
2022-10-20
Publication Date
2024-10-18
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Abrasive backings used in sanding applications often break after a certain number of cycles, tear easily, and experience reduced strength when soaked or cleaned, leading to decreased material removal rates due to internal heat build-up.

Method used

An abrasive backing comprising a base sheet made of wood fibers, synthetic fibers, and cellulose filaments, saturated with a combination of two or more latex polymers and a crosslinking agent, and coated with a barrier and backside coating to enhance strength and durability.

Benefits of technology

The abrasive backing exhibits improved strength properties, allowing for increased sanding cycles, reduced tear resistance, and maintains strength after soaking, while reducing internal heat build-up and enhancing material removal rates.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024538206000001_ABST
    Figure 2024538206000001_ABST
Patent Text Reader

Abstract

Generally, an abrasive backing is provided. In some embodiments, the abrasive backing includes a base sheet, the base sheet including wood fibers, synthetic fibers, cellulose filaments, a saturant, the saturant including two or more latex polymers and a crosslinker, a first surface and an opposing second surface, a barrier coating adjacent the first surface of the base sheet, and a backside coating adjacent the second opposing surface of the base sheet. Methods of making the abrasive backing are also provided.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present disclosure relates to an abrasive backing having improved strength characteristics.

[0002] A common problem when using abrasive backings in sanding applications is that the backing breaks after a certain number of sanding cycles. It is also common for the backing to break and become unusable after a certain number of folds. When using abrasive backings on sandpaper for power equipment, a large amount of internal heat buildup can adversely affect the material removal rate when using the equipment. Additionally, to wash the sanded material off the grit, the sandpaper is softened or rejuvenated in water, and in doing so, the sandpaper loses some of its strength properties by being soaked or cleaned.

[0003] Thus, there is a need for an abrasive backer that has improved strength properties. Specifically, there is a need for an abrasive backer that allows for an increased number of sanding cycles or folds before the backing breaks. There is also a need for an abrasive backer that increases the material removal rate and maintains its strength properties when soaked or cleaned. Summary of the Invention

[0004] An abrasive backing is generally provided. In some embodiments, the abrasive backing includes a base sheet, the base sheet including wood fibers, synthetic fibers, cellulose filaments, a saturant, the saturant including two or more latex polymers and a crosslinker, a first surface and an opposing second surface, a barrier coating adjacent to the first surface of the base sheet, and a backside coating adjacent to the opposing second surface of the base sheet. The barrier coating can be impermeable to liquid water and allow gas transmission. In some embodiments, the abrasive backing can have two or more barrier coatings applied adjacent to the first surface of the base sheet. The abrasive backing can have grit applied adjacent to a surface of the barrier coating opposite the first surface of the base sheet. The backside coating can be waterproof. In further embodiments, the abrasive backing can have a layer including a plurality of loops or a plurality of hooks on a surface of the backside coating opposite the second surface.

[0005] In some embodiments, the base sheet can include wood fibers, including hardwood fibers, softwood fibers, or combinations thereof. In some embodiments, the base sheet can include wood fibers including a blend of softwood fibers and hardwood fibers, for example, a blend of 30-70% softwood fibers and 70-30% hardwood fibers by weight, each based on the weight of the wood fibers and cellulose filaments in the base sheet. The base sheet can further include jute fibers, straw fibers, cotton fibers, hemp fibers, bagasse fibers, bamboo fibers, reed fibers, sisal fibers, abaca fibers, kenaf fibers, flax fibers, or combinations thereof.

[0006] In further embodiments, the base sheet can have two or more latex polymers in an amount of 55% to 99.9% by weight of the saturant based on the weight of dry solids in the saturant. In some embodiments, two of the two or more latex polymers can be crosslinkable. The saturant can include a third latex polymer. The two or more latex polymers can include a copolymer prepared from monomers including styrene and butadiene. In some embodiments, the latex polymer is selected from latex polymers having a Tg of -40°C to -20°C and a Tg of -12°C to 8°C. The latex polymer can further include a latex polymer having a Tg of 32°C to 52°C. The latex polymer may include 10% to 50% by weight of a latex polymer having a Tg of -40°C to -20°C, 50% to 90% by weight of a latex polymer having a Tg of -12°C to 8°C, and 10% to 50% by weight of a latex polymer having a Tg of 32°C to 52°C, based on the total dry weight of the latex polymer. In further embodiments, the saturant may include a crosslinking agent in an amount of 0.25% to 1.5% by weight of the saturant, based on the weight of the dry solids in the saturant. The crosslinking agent may include an aziridine crosslinking agent, a glyoxal-based crosslinking agent, ammonium zirconium carbonate, carbodiimide, an aliphatic polyglycidyl ether, hexamethoxymethylmelamine, zinc diethyldithiocarbamate, or a combination thereof. For example, the crosslinking agent may include an aziridine crosslinking agent.

[0007] In some embodiments, the base sheet may include cellulose filaments in an amount of 1% to 5% by weight, based on the weight of the wood fibers and cellulose filaments in the base sheet. The cellulose filaments may have an aspect ratio of 200 to 5000 and a width of 30 to 500 nm. Additionally, the base sheet may include 2% to 8% by weight of synthetic fibers, based on the weight of the wood fibers and cellulose filaments in the base sheet. The synthetic fibers may include polyester fibers, such as polyethylene terephthalate (PET) fibers. The abrasive backing may have a basis weight of 75 to 155 gsm.

[0008] A method for forming an abrasive backing is also generally provided. In one embodiment, the method includes providing a base sheet including wood fibers, synthetic fibers, cellulose filaments, and a saturant including two or more latex polymers and a crosslinking agent, applying a barrier coating to a first surface of the base sheet, and applying a backside coating to a second surface of the base sheet opposite the first surface of the base sheet. The method can also include providing a base sheet made from wood fibers, synthetic fibers, and cellulose filaments, saturating the base sheet with a saturant including two or more latex polymers and a crosslinking agent, and drying the saturated base sheet. The method can also include providing a base sheet by forming the base sheet from a fiber matrix including wood fibers, synthetic fibers, and cellulose filaments, and drying the base sheet. The base sheet can then be calendered after saturating the base sheet with the saturant. The method for making an abrasive backing can include other features as described above with respect to the abrasive backing.

[0009] The details of one or more embodiments are set forth in the following description and the annexed drawings. Other features, objects, and advantages will become apparent from the description, and from the claims.

[0010] This application includes references to the accompanying drawings. [Brief description of the drawings]

[0011] [Figure 1A] 1 illustrates an exemplary abrasive backing. [Figure 1B] 1B shows an enlarged view of the exemplary abrasive backing of FIG. 1A taken along line 1B. [Figure 2A-1] Data from examples are provided that demonstrate the abrasive backings described herein. [Figure 2A-2] Data from examples are provided that demonstrate the abrasive backings described herein. [Figure 2B-1] Data from examples are provided that demonstrate the abrasive backings described herein. [Figure 2B-2] Data from examples are provided that demonstrate the abrasive backings described herein.

[0012] Repeat use of reference characters in the present specification and drawings is intended to represent same or analogous features or elements of the invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0013] The present disclosure generally provides an abrasive backing and a method for forming the same. In a particular embodiment, the abrasive backing comprises a base sheet including wood fibers, synthetic fibers, cellulose filaments, and a saturant, the saturant including two or more latex polymers and a crosslinking agent. The base sheet includes a first surface and an opposing second surface. A barrier coating is adjacent to the first surface of the base sheet, and a backside coating is adjacent to the opposing second surface.

[0014] 1A, an exemplary abrasive backing 10 is shown formed from a base sheet 12 having a first surface 11 and a second surface 13. A barrier coating 22 is adjacent to the first surface 11 of the base sheet. A backside coating 20 is adjacent to the second surface 13 of the base sheet 12.

[0015] Figure IB shows an expanded view of the abrasive backing 10 of Figure IA. In the embodiment shown, the base sheet 12 includes a plurality of fibers including softwood fibers 14, hardwood fibers 16, and synthetic fibers 24. The base sheet 12 also includes cellulose filaments 26. The base sheet 12 also includes latex particles 18 provided by two or more polymers in a saturant.

[0016] Each of the components of the abrasive backing 10 provided herein is discussed in more detail below with respect to the abrasive backing and methods of forming the abrasive backing.

[0017] The base sheet 12 includes a plurality of fibers, including wood fibers, synthetic fibers, and cellulose filaments, bound together by a polymeric matrix formed by the reaction of two or more latex polymers with a crosslinking agent. As discussed herein, the polymeric matrix is ​​provided by a saturant that saturates the plurality of fibers in the base sheet. In some embodiments, hydroxyl groups present in the fibers and cellulose filaments can hydrogen bond with pendant groups present in the latex polymer provided in the saturant (e.g., if the latex polymer is carboxylated).

[0018] The wood fibers in the base sheet can include softwood fibers 14, hardwood fibers 16, or blends thereof. In certain embodiments, the wood fibers can include a blend of softwood and hardwood fibers. The base sheet can include 5-95%, 10-90%, 20-80%, or 30-70% softwood fibers by weight, based on the weight of the wood fibers and cellulose filaments in the base sheet. The base sheet can include 5-95%, 10-90%, 20-80%, or 30-70% hardwood fibers by weight, based on the weight of the wood fibers and cellulose filaments in the base sheet.

[0019] Examples of softwood fibers include Northern Bleached Softwood Kraft (NBSK), an example of which is provided in Table 1. In some embodiments, the softwood fibers can have a length-weighted average fiber length of 1.99 to 2.30 mm. Examples of hardwood fibers include Northern Bleached Hardwood Kraft (NBHK), an example of which is provided in Table 2. In some embodiments, the hardwood fibers can have a length-weighted average fiber length of 0.58 to 1.11 mm. In some embodiments, Eucalyptus Bleached Kraft (EuBK) can be used in place of NBHK. [Table 1] [Table 2]

[0020] In some embodiments, the plurality of fibers can include additional fibers. The additional fibers can include jute fibers, straw fibers, cotton fibers, hemp fibers, bagasse fibers, bamboo fibers, reed fibers, sisal fibers, abaca fibers, kenaf fibers, flax fibers, or combinations thereof. The additional fibers can replace 1% or more, 5% or more, 10% or more, 20% or more, 30% or more, or 40% or more, or 50% or more, or 50% or less, 40% or less, 30% or less, 20% or less, 10% or less, or 5% or less by weight of the wood fibers in the base sheet. For example, straw fibers can be used to replace all or a portion of the hardwood fibers that would be used in the hardwood / softwood fiber blend.

[0021] The base sheet 12 can include cellulose filaments. The cellulose filaments can be formed, for example, by untangling wood fibers to provide monofilaments. The cellulose filaments can have an aspect ratio of 200 to 5000 and a width of 30 nm to 500 nm. One exemplary source of cellulose filaments is FILOCELL™ CF, commercially available from Kruger Biomaterials Inc. The cellulose filaments can be provided in the base sheet in an amount of 0.1% to 10%, 0.5% to 7.5%, or 1% to 5% by weight based on the weight of the wood fibers and cellulose filaments in the base sheet.

[0022] The plurality of fibers may include synthetic fibers to provide additional properties to the base sheet. For example, the synthetic fibers may cooperate with the wood fibers to improve the tear resistance of the base sheet. The synthetic fibers may be formed from any suitable material and in any suitable size and shape, so long as the resulting synthetic fibers function as high tensile strength fibers. Examples of such synthetic fibers may include polyolefins (e.g., polyethylene, polypropylene, polybutylene, etc.), polytetrafluoroethylene, polyesters (e.g., polyethylene terephthalate), polyvinyl acetate, polyvinyl chloride acetate, polyvinyl butyral, acrylics (e.g., polyacrylate, polymethyl acrylate, polymethyl methacrylate, etc.), polyamides (e.g., nylon 6, nylon 6 / 6, nylon 4 / 6, nylon 11, nylon 12, nylon 6 / 10, and nylon 12 / 12), polyvinyl chloride, polyvinylidene chloride, polystyrene, polyvinyl alcohol, polyurethane, polylactic acid, and combinations thereof. In a particular embodiment, the synthetic fibers include polyesters such as polyethylene terephthalate (PET) 24. Synthetic PET fibers include those commercially available from Toray Industries, Inc. In some embodiments, the synthetic fibers have a length of 1 mm to 10 mm, or 2 mm to 8 mm. In some embodiments, the synthetic fibers can have a denier of 0.5 dpf (denier per filament) to 6.0 dpf, or 3.0 dpf to 6.0 dpf. The synthetic fibers are provided in the base sheet in an amount of 0.5% to 15%, 1% to 12%, 2% to 10%, or 2% to 8% by weight based on the weight of the wood fibers and cellulose filaments in the base sheet.

[0023] Various additives can be applied to the fibers (e.g., to the dry fibers) during the formation of the fibrous web or after the formation of the base sheet 12. For example, wet strength agents can be used to improve the strength properties of the web as it is being formed. The wet strength agents can be present in an amount of 0.001% to 5% by weight or 0.01% to 2% by weight based on the weight of the wood fibers and cellulose filaments in the base sheet. Wet strength agents are typically water-soluble, cationic oligomeric or polymeric resins that can bond with cellulose fibers. For example, some suitable wet strength agents are polyamine-epichlorohydrin, polyamide epichlorohydrin, or polyamide-amine epichlorohydrin resins (collectively "PAE" resins). In certain embodiments, other wet strength agents can also be used. For example, other suitable wet strength agents can include dialdehyde starch, polyethyleneimine, mannogalactan gum, glyoxal resins, polyisocyanates, and dialdehyde mannogalactans. In some embodiments, the wet strength resin comprises a polyamide-epichlorohydrin (PAE) resin.

[0024] A variety of other additives may also be used in the base sheet 12. The additives may be provided with the fibers during the formation of the base sheet or may be applied to the base sheet with the saturant. Suitable additives may include defoamers, processing aids, surfactants, and dispersants. For example, kaolin pigment may be included in the base sheet to increase opacity. A wide range of pigments and dyes may also be added to impart color to the base sheet. The pigments and dyes may be added during the formation of the base sheet, may be provided with the saturant when the base sheet is saturated, or may be provided as a separate coating on the base sheet after saturation.

[0025] As discussed herein, the plurality of fibers are provided in a polymeric matrix in the base sheet 12. The polymeric matrix is ​​provided by a saturant or saturating composition used to saturate the fibers in forming the base sheet or after the base sheet is formed. In certain embodiments, the saturant is provided after the base sheet is formed by saturating the base sheet. As discussed herein, the polymeric matrix is ​​formed by the use of at least two latex polymers and a crosslinking agent. In certain embodiments, two or more of the at least two latex polymers are crosslinkable so that they can react with the crosslinking agent or with other latex polymers in the saturating agent. The reaction of the latex polymers with the crosslinking agent can occur through heat or by removing water from the saturating agent in the base sheet. In addition to physically bonding the plurality of fibers in the base sheet, one or more of the latex polymers and the crosslinking agent can additionally bond with the plurality of fibers or cellulose filaments, for example, via hydrogen bonding.

[0026] The saturant comprises at least two latex polymers 18, at least three latex polymers, or more. In some embodiments, the saturant comprises three latex polymers. In some embodiments, two or more latex polymers are crosslinkable and form a polymeric matrix when reacted with the crosslinker. In some embodiments, all three of the latex polymers are crosslinkable. Suitable latex polymers include styrene butadiene copolymers (formed from the reaction of primarily styrene and butadiene monomers), styrene acrylic copolymers (formed from the reaction of primarily styrene and (meth)acrylic and / or (meth)acrylate monomers), pure acrylic copolymers (formed from the reaction of primarily (meth)acrylic and / or (meth)acrylate monomers), or mixtures thereof. For example, the pure acrylic copolymer can be a polyacrylate, such as zinc polyacrylate. Other suitable latex polymers include N-methylolacrylamide, ethylene-vinyl acetate copolymer, nitrile rubber, acrylonitrile-butadiene copolymer, poly(vinyl chloride) copolymer, poly(vinyl acetate) copolymer, ethylene-acrylate copolymer, vinyl acetate-acrylate copolymer, neoprene rubber or trans-1,4-polychloroprene, cis-1,4-polyisoprene, butadiene rubber, cis- and trans-1,4-polybutadiene, ethylene-propylene copolymer, or mixtures thereof. In certain embodiments, the latex polymer may be crosslinkable and may include functional groups configured to allow crosslinking of the latex polymer, either with a crosslinking agent, another latex polymer, or both. For example, the latex polymer may include crosslinkable groups such as carboxyl groups, amine groups, pyridyl groups, or combinations thereof. In some embodiments, the crosslinkable latex polymer may include one or more carboxylated styrene butadiene copolymers. In some embodiments, the particle size of the latex polymer particles can range from 100 nm to 300 nm, or from 140 nm to 210 nm.

[0027] In some embodiments, the saturant can include two or more latex polymers 18 in an amount of 55% to 99.9% or 70% to 99.75% by weight based on the weight of dry solids in the saturant. The at least two latex polymers can include a latex polymer having a Tg of -40°C to -20°C and a latex polymer having a Tg of -12°C to 8°C. In certain embodiments, the latex polymer can have a Tg of 32°C to 52°C. For example, the latex polymer can include 10% to 50% by weight of a latex polymer having a Tg of -40°C to -20°C, 50% to 90% by weight of a latex polymer having a Tg of -12°C to 8°C, and 0% (or 10%) to 50% by weight of a latex polymer having a Tg of 32°C to 52°C, based on the total dry weight of the latex polymers in the saturant. Specific properties can be imparted to the base sheet 12 by using polymer latexes that vary according to particle size, gel content, glass transition temperature, and number of crosslinking groups (eg, degree of carboxylation).

[0028] The saturant may include a crosslinking agent. In certain embodiments, the crosslinking agent may include an aziridine crosslinking agent, a glyoxal-based crosslinking agent, ammonium zirconium carbonate, a carbodiimide, an aliphatic polyglycidyl ether, hexamethoxymethylmelamine, zinc diethyldithiocarbamate, or a combination thereof. In certain embodiments, the crosslinking agent may include an aziridine crosslinking agent. The saturant may include a crosslinking agent in an amount of 0.1% to 2.5%, 0.2% to 2%, or 0.25% to 1.5% by weight based on the weight of the dry solids in the saturant. Crosslinking agents with an aziridine backbone covalently bond with molecules having carboxylic acid groups, such as carboxylated styrene butadiene latex, thereby forming a crosslinked network, thus achieving both wet and dry properties.

[0029] Other ingredients may be included in the saturant composition as needed. For example, antioxidant compounds may be included in the saturant composition. Antioxidants help to prevent oxidation of the saturant composition during the curing process. Oxidation may discolor the saturant composition and reduce its final physical properties. Examples of antioxidants include substituted phenolic compounds such as butylated dihydroxyanisole, di-tert-butyl-p-cresol, and propyl gallate. Additional examples of antioxidants include aromatic amines such as di-β-naphthyl paraphenylenediamine and phenyl-β-naphthylamine. When used, antioxidants may be included in the formulation at a concentration of less than 10 wt%, less than 5 wt%, less than 2 wt%, less than 1 wt%, or less than 0.5 wt%, based on the weight of the dry solids in the saturant. In one particular embodiment, a phenolic antioxidant may be included in the saturant composition.

[0030] Additional materials such as fillers, emulsifiers, water repellents, and film-forming resins may be included in the saturate composition as needed. Suitable fillers may include silica or silicates, clays, and borates. Fillers may be included in the saturate in an amount of from greater than 0% to 45% or from 5% to 30% by weight based on the weight of dry solids in the saturate. Fillers (e.g., clays) may act to reduce moisture and air transmission through the base sheet. Examples of suitable clays include No. 1 high brightness kaolin clay, No. 1 high brightness extra fine clay, No. 2 high brightness clay, No. 1 Regular Brightness extra fine clay, No. 1 Regular Brightness clay, No. 2 Regular Brightness clay, and combinations thereof, as provided in Table 3. [Table 3]

[0031] The saturant may also include other additives to provide the desired qualities to the saturated composition. Examples include pH adjusting chemicals or surfactants. Trisodium phosphate may be included in the saturated composition as an emulsifier and / or thickener to help control the pH of the emulsion.

[0032] The barrier coating 22 can be applied onto the base sheet 12 after saturation. The barrier coating 22 can be applied from a composition that can independently include any of the materials discussed above with respect to the saturant composition. Suitable latex polymer binders for the barrier coating can include acrylic latex binders. Suitable polyacrylic latex binders can include polymethacrylates, poly(acrylic acid), poly(methacrylic acid), and copolymers of various acrylic and methacrylic acid esters and free acids, ethylene-acrylate copolymers, and vinyl acetate-acrylate copolymers.

[0033] The saturant and the latex polymer binder for the barrier coating may be the same or different. The latex polymer of the barrier coating is typically selected to adhere or bond well to the surface of the saturated base sheet. Additionally, the latex polymer binder of the barrier coating can be configured to flow sufficiently well during any subsequent calendering (e.g., soft nip calendering or supercalendering). For example, a latex polymer binder having a viscosity in the range of 10 to 100 centipoise can be expected to flow sufficiently well.

[0034] The thickness of the barrier coating 22 may vary depending on the intended use of the resulting adhesive backing. For example, thinner barrier coatings may be used for coarse grit abrasive products, such as abrasives having a particle size of 200 mesh or greater (the term "mesh" is used herein to mean the mesh of a U.S. Standard Sieve). Meanwhile, thicker barrier coatings may be used for finer grit products used for polishing or fine surface finishing. The practical minimum layer thickness is 10 micrometers, while the practical maximum layer thickness is 250 micrometers. However, thinner or thicker layers may be used as needed, provided that the layer is continuous. Inherently stiff thermoplastic polymer compositions will be more useful for coarse grit products, while softer or elastomeric thermoplastic polymer compositions, such as ethylene-vinyl acetate copolymers and polyurethanes, will be more useful for fine grit products, such as fine sanding and polishing cloths.

[0035] In another exemplary barrier coating, a tie layer can be on the first surface and a barrier coating can be on the tie layer, as disclosed in U.S. patent application Ser. No. 14 / 245,342 to Vervacke, entitled "Super Smooth Paper Backing for Fine Grit Abrasives and Methods of Their Application and Use," filed Apr. 4, 2014, which is incorporated by reference herein.

[0036] In certain embodiments, the barrier coating 22 can be impermeable to liquid water and allow gas transmission. In certain embodiments, the barrier coating 22 allows gas and liquid transmission. In some embodiments, the abrasive backing can have two or more barrier coatings applied adjacent to the first surface of the base sheet. An exemplary abrasive backing can include a make coating applied adjacent to the barrier coating and a grit coating applied adjacent to the make coating. In some embodiments, the make coating can include a liquid phenolic resole resin, a hydroxyl-containing polyester, a polyester polyol, an aromatic polyisocyanate, butyl acetate, sorbitan laurate, or a combination thereof. In some embodiments, the make coating includes a liquid phenolic resole resin. The make coating secures the grit to the base sheet 12 of the abrasive backing 10.

[0037] The backside coating 20 can be any suitable layer of a second surface, or a coating on a second surface, that is not configured to have a layer of abrasive particles thereon. Any such backside coating can be used and adapted for a particular application, as known in the art. Such backside coatings can be applied from compositions that can independently include any of the materials discussed above with respect to saturants. In some embodiments, the backside coating 20 can be waterproof, and in some embodiments, can include a layer with multiple loops or multiple hooks (such as Velcro®). A layer with multiple loops or multiple hooks can be discontinuous and provided only as needed to match a sanding device with a corresponding multiple loops (if the backside coating 20 has multiple hooks) or multiple hooks (if the backside coating has multiple loops). The backside coating 20 can include a latex polymer as well as various other additives. Suitable additives can include defoamers, pigments, processing aids, dispersants, and matting agents. In some embodiments, the backside coating 20 can include fillers, such as diatomaceous earth. Diatomaceous earth can enhance the tactile feel of the backside coating 20 when used in hand sanding applications.

[0038] An exemplary abrasive backing 10 can be formed by a method including providing a base sheet 12 including wood fibers, synthetic fibers, cellulose filaments, and a saturant including two or more latex polymers and a crosslinking agent, applying a barrier coating 22 to a first surface 11 of the base sheet 12, and applying a backside coating 20 to a second surface 13 of the base sheet 12 opposite the first surface 11 of the base sheet 12. In a particular embodiment of the abrasive backing, providing the base sheet 12 can include providing a base sheet 12 including wood fibers, synthetic fibers, and cellulose filaments, saturating the base sheet 12 with a saturant including two or more latex polymers and a crosslinking agent, and drying the saturated base sheet 12. In another embodiment, providing the base sheet 12 can include forming the base sheet 12 from a fibrous matrix including wood fibers, synthetic fibers, and cellulose filaments, and drying the base sheet. In some embodiments of the abrasive backing 10, the method of formation can include calendering the base sheet 12.

[0039] In certain embodiments, the abrasive backing 10 is formed by a method that includes a barrier coating 22 that is impermeable to liquid water and allows the transmission of gas. The method can also include a barrier coating 22 that allows the transmission of gas and liquid. There may also be more than one barrier coating 22 applied adjacent to the first surface 11 of the base sheet 12. The abrasive backing 10 can also be formed by a method that includes applying grit adjacent to a surface of the barrier coating 22 opposite the first surface 11 of the base sheet 12. In some embodiments, the abrasive backing 10 is formed by a method that includes a layer comprising a plurality of loops or a plurality of hooks provided on a surface of the backside coating 20 opposite the second surface 13.

[0040] In certain embodiments, the abrasive backing 10 comprises an abrasive backing base paper having a basis weight between 75 and 155 gsm, encompassing between A and C weight abrasive papers.

[0041] To form the base sheet 12, a plurality of fibers, including wood fibers, optional additional fibers, cellulose filaments, and synthetic fibers, are mixed together. The plurality of fibers are generally placed in a conventional papermaking fiber stock prep beater or pulper containing water. The fibrous material stock is typically continuously agitated to form a suspension. If desired, the cellulose filaments and / or wood fibers can also be subjected to one or more refining steps to provide various benefits, including improved tensile and porosity properties of the base sheet. Refining results in an increased amount of intimate contact of the fiber surfaces and can be performed using devices known in the art, such as a disc refiner, a double disc refiner, a Jordan refiner, a Claflin refiner, or a Valley type refiner.

[0042] The resulting fibrous suspension can then be diluted and prepared for formation into a fibrous web using conventional papermaking techniques. For example, a web can be formed by distributing the suspension onto a forming surface (e.g., a wire) and then removing water from the distributed suspension to form a web. This process can include transferring the suspension to a dump chest, machine chest, clean stock chest, low density cleaner, headbox, etc., as known to those skilled in the art. Once formed, the fibrous web can then be dried using any known technique, such as by using convection ovens, radiant heat, infrared radiation, forced air ovens, and heated rolls or cans to produce a base sheet. Drying can also include intensive steam drying followed by contact drying. Drying can also be performed by air drying without the addition of heat energy.

[0043] In some embodiments, the saturant component is provided as a beater add and is therefore present in the fiber suspension used to manufacture the base sheet. In some embodiments, the saturant can be used to saturate an already formed base sheet. Any known saturation technique can be used, such as brushing, submerged nip saturation, doctor blade, spraying, and direct and offset gravure coating. For example, the fibers can be exposed to an excess of solution and then squeezed. Squeezing the excess saturant from the fibers can be accomplished by passing the fibers between rollers. If desired, the excess saturant can be returned to a source for further use. After squeezing out the excess material, the saturated fibers can then be dried. Other suitable techniques for saturating the fibers with the saturant are described in U.S. Pat. No. 5,595,828 to Weber and U.S. Patent Application Publication No. 2002 / 0168508 to Reed, et al., which are incorporated herein by reference in their entireties for all purposes.

[0044] The amount of saturant applied can vary depending on the desired properties of the fibers, such as the desired permeability. Typically, the saturant is present at a "parts pick up" or PPU add-on level of 10% to 40% by weight, and in some embodiments, 10% to 25% by weight. The PPU add-on level is calculated by dividing the dry weight of the saturant applied by the dry weight of the fibers before treatment and multiplying the result by 100. The PPU is calculated according to the formula:

number

[0045] In one particular embodiment, the saturated base sheet 12 is calendered after saturation. Calendering the saturated base sheet can enhance the softness and smoothness of the sheet. If desired, the saturated base sheet 12 can be calendered according to any process. Calendering generally involves pressing the saturated base sheet in a nip formed by first and second calender rolls. The effect of calendering on the saturated base sheet depends on the temperature, the pressure applied, and the duration of the pressure. For purposes herein, calendering can be performed at either ambient or elevated temperatures. Suitable calender pressures can be 50-2000 pounds force per linear inch (pli), 100-1600 pli, 300-1000 pli, or 400-600 pli. Suitable temperatures can be 20°C-240°C, 20°C-140°C, or 20°C-90°C.

[0046] The duration of the calendering can be varied in relation to the nip pressure and / or composition of the calender rolls to produce the desired smoothness of the paper backing of the sheet. For example, softer calender rolls, such as fiber-filled rolls, tend to compress to create a larger contact area in the nip, thus increasing the duration of the calendering. Harder steel rolls compress more, thus reducing the duration of the calendering. In one arrangement, the calendering nip comprises a steel roll and a soft fiber-filled roll. In another arrangement, for example, a production supercalender stack can include more than two rolls, preferably 9-11 rolls, stacked on top of each other in a vertical arrangement. Desirably, the stacked rolls alternate between the steel roll and the fiber-filled roll. In such an arrangement, the paper can be subjected to various pressures, up to 1600 pli, and several nips, for example 1-8, to produce the desired smoothness level.

[0047] The saturated and calendered base sheet 12 can be dried to remove the solvent from the saturated composition. For example, the saturated base sheet 12 can be heated to a temperature of at least 100° C., in some embodiments at least 150° C., such as at least 200° C. Suitable drying techniques can include heating in a conventional oven, microwave, forced air, heated rolls, can, or through-air drying. Drying can also include intensive steam drying followed by contact drying.

[0048] Additionally, the saturated, calendered base sheet 12 can be cured such that the latex polymer reacts with the crosslinking agent of the saturated composition to crosslink and form a three-dimensional polymeric structure. Thus, the crosslinked latex polymer can serve to bond the fibers of the base sheet together either mechanically and / or chemically.

[0049] Regardless of the particular processing step of the base sheet, the base sheet 12 is maintained at a temperature below the softening or melting point temperature of the synthetic fibers such that the synthetic fibers maintain their as-laid shape and physical structure in the final ply sheet orientation (and the resulting abrasive backer laminate). Thus, the structural and physical integrity of the synthetic fibers remains intact within the individual ply sheets to enable the synthetic fibers to provide strength properties to the ply sheets.

[0050] A backside coating 20 and a barrier coating 22 can be applied to the base sheet 12. The backside coating 20 can be customized to provide specific properties. In particular, the backside coating 20 can be printed on, can have a hand-sanded feel, or can be pre-coated for adhesive.

[0051] The abrasive backing 10 also demonstrates a 100% to 200% improvement in wet properties, allowing sandpaper products made from the abrasive backing 10 to retain strength properties while being soaked or cleaned to wash the sanded material off the grit. Without wishing to be bound by a particular theory, it is believed that the improvement is due to the use of a combination of two or more latex polymers, crosslinking agents, wood fibers, cellulose filaments, and synthetic fibers. The latex polymers provide reinforcement to the fibers, thereby enhancing the strength properties and durability of the abrasive backing 10. The improvement in wet sanding properties is also due to the barrier coating and backside coating, which reduce permeability due to the improved sealing of the sheet through the use of a saturant.

[0052] The abrasive backing 10 can withstand the rigors of both hand sanding and power tool applications in both wet and dry sanding applications. The improved strength of the abrasive backing 10 is exhibited in both in-plane and out-of-plane strength properties. This is demonstrated by a root mean square (RMS) tensile index of greater than 95 Nm / g (e.g., 95-100 Nm / g). The out-of-plane peel force is between 150 g force and 1000 g force, or between 450 g force and 750 g force. It is believed that the cellulose filaments and synthetic fibers provide additional tear strength by intertwining and bonding with the wood fibers.

[0053] The abrasive backing 10 has a high release force in the wet state after both 1 hour or 24 hour soak cycles, thereby allowing the abrasive backing to better retain its strength properties after soaking or cleaning. The abrasive backing 10 maintains its strength properties when periodically cleaned in a suitable polar cleaning solvent such as water, thereby improving wet sanding life. The improved backing retains 40%-60% of its dry tensile strength after 1 hour of soaking in water. The improved backing does not require increased refining energy relative to the base sheet, thus allowing the same level of refining with increased densification and strength properties of the backing.

[0054] Sandpapers using the improved abrasive backing 10 are more durable in both hand and power sanding applications. When used with powered equipment, the improved sandpaper will have reduced internal heat buildup and will improve energy transfer from the powered equipment to the material. Thus, when the same grit and make coat are applied to the abrasive backing, the material removal rate will also be improved.

[0055] The abrasive backings will now be further described by the following non-limiting examples. Parts and percentages are on a unit weight basis unless otherwise specified.

[0056] Test Method Sample preparation Specimens were conditioned using TAPPI T402 sp-13 with the additional step of pulling conditioned air through the specimen for a minimum of 20 minutes prior to any of the following test methods.

[0057] Basis weight The weighing was measured using a TAPPI T410, with the test specimens measuring a minimum of 800 in 2 Instead, it is 412.3 in. 2 The total area of ​​the four sheets was 100 mm.

[0058] Caliper Calipers were measured using a TAPPI T411 om-15.

[0059] Tensile strength, Tensile Energy Absorbed (TEA), Elongation, and RMS Tensile Index Tensile strength, TEA, and elongation were measured using TAPPI T494-om-01. RMS tensile is the square of the MD tensile plus the square root of the CD tensile.

[0060] MD aged wet tensile strength and MD aged wet elongation MD aged wet tensile strength and MD aged wet elongation were measured using TAPPI T456 om-15, except that the specimens were aged at 145° F. for 5 minutes before measurement.

[0061] Tear Tear was measured using TAPPI T414 om-21, but results are in grams force for tearing 16 plies instead of 1 ply.

[0062] Gurley Porosity Gurley porosity was measured using a TAPPI T460 using either one sheet or four sheets.

[0063] Wire smoothness Wire smoothness was measured using a TAPPI T538 om-16.

[0064] Peeling Peel was measured using the following procedure:

[0065] The Twing-Albert Vantage NX EJA series testing machine was a properly calibrated testing machine capable of operating in displacement control mode at a constant displacement rate of 30.5 cm / min. The testing machine was equipped with two opposing grips to hold the two ends of a heat seal tape adhered to an abrasive backing specimen. The testing machine load feed device was capable of indicating the total load supported by the specimen, in this case a 500 N load cell was used. This device had essentially no inertial delay at the specified test speed and indicated loads accurate to within ±1% of the indicated value throughout the load range(s) of interest. Data was digitally stored and post-processed. At least five specimens per test condition were tested. The accuracy of all measuring equipment had certified calibrations that were current at the time of use of the equipment. Samples were stored and tested in a standard laboratory atmosphere of 23±3°C and 50±10% relative humidity. 1. The width of each abrasive backing specimen and heat seal tape was 15 mm. 2. Apply the cloth heat seal tape at 45.5gm / cm 2 Heat seal tape was laminated to both sides of the abrasive backing at 312°F ± 12°F by applying a pressure of 0.01 mm for 20 seconds and used to bond opposing sides of the abrasive backing specimens such that the peel force was measured along the central plane of the specimen. 3. After the abrasive backing specimen was heat sealed and before loading into the grip block, peeling was manually initiated by pulling the two strips of heat seal tape away from each other at 180° until at least 2.54 cm had been pre-peeled. 4. The two ends of the heat seal tape on the previously peeled specimen were placed into the grips of the loading machine, making sure the specimen was aligned and centered. 5. The test specimen was loaded at a constant crosshead speed of 30.5 cm / min. 6. Load and displacement values ​​were recorded continuously. After a test distance of 7.5.08 cm, the test load application was stopped. 8. The specimen was unloaded at a constant crosshead speed of 30.5 cm / min. 9. After the specimen was unloaded, the average force in grams was calculated over the entire test distance of 5.08 cm.

[0066] 1 hour wet peel The equipment, test method, and instrument parameters were exactly the same as the stripping method described above, except with the addition of an immersion step. Prior to testing, the specimens were soaked in a 10 g per liter immersion solution of a non-ionic surfactant (C 14 H 22 O(C2H4O) n ) for 1 hour. 1. Samples were blotted with paper towels to remove excess water. 2. The preliminary peeling and load application steps provided in the peeling method were performed on specimens that had been immersed for 1 hour. 3. After the test was completed, the average peel force of the specimens immersed for 1 hour was calculated over the entire 50.8 cm test distance performed in the peel method. 4. The 1 hour wet peel force was reported in grams and the 1 hour wet / dry test ratio was reported as a percentage.

[0067] 24-hour wet peel The 24 hour wet peel was measured using the same test as the 1 hour wet peel, except that the specimens were immersed in the immersion solution for 24 hours instead of 1 hour.

[0068] Sheffield Porosity Sheffield porosity was measured using a TAPPI T547 om-18.

[0069] The smoothness of the felt The smoothness of the felt was measured using a TAPPI T538 om-16.

[0070] Felt Gloss Felt gloss was measured using a TAPPI T480 om-15.

[0071] Turpentine impregnation The following test was used to measure turpentine penetration: The solvent was made by combining xylene with heptane in a 1.3 to 1 volume ratio and adding 0.25 g of Sudan Red IV per 400 ml of total xylene / heptane. 2. The solvent was brushed onto the barrier coated side of the specimen with a 2 inch wide paint brush. 3. The sample was allowed to sit for 10 seconds while coated with the solvent and then wiped off. 4. The penetration level is the rate on a scale of 1, 3, or 4, with 1 representing the least amount of penetration and 4 representing solvent penetration to the other side of the barrier coat.

[0072] density The density was calculated using the weighing weight measured above and the caliper measured above. EXAMPLES

[0073] Example 1 Eight different samples of the coated saturated base sheet were prepared and the properties were then compared between the samples. For each of the samples prepared, the same process was followed but the materials used for both the base sheet and the saturant were changed. Coated saturated basesheet samples were prepared according to the following method:

[0074] An unsaturated basesheet having a composition according to Table 4 was refined for 15 minutes. [Table 4]

[0075] The dry sheets were saturated with a saturant of the composition according to Table 5 to the appropriate pick-up. [Table 5]

[0076] A barrier coating and a backside coating were provided on opposite sides of the base sheet having a composition according to Table 6. [Table 6]

[0077] The characteristics of different abrasive backings are provided in Figures 2A and 2B.

[0078] As shown in Figures 2A and 2B, there are improved properties when comparing control samples A_B30 and A_B35 to the abrasive backings provided herein. For example, the root mean square (RMS) tensile index increases from about 80 Nm / g for A_B30 to a range of 95-100 Nm / g as shown for samples B_P30 and B_P35. This indicates that the abrasive backings can withstand the rigors of both hand sanding and power tool applications in both wet and dry sanding applications. There is also a 15%-30% improvement in strength properties such as in-plane tensile strength and tear, and a 100% improvement in out-of-plane properties such as z-direction tensile and out-of-plane peel force for the saturated sandpaper products.

[0079] The abrasive backing allows for an increased number of sanding cycles before either tensile or tear failure of the abrasive backing. This improvement is shown in Figure 2A, where the sanding strength of sample A_B30 is 219.8 J / m 2 From sample B_P35, 311.9 J / m 2 This improvement is also demonstrated by the average folding endurance of 4,194 folding cycles for the conditioned and unaged B_35P and 6,513 for the conditioned B_35P aged at 120° C. for 30 minutes, as provided in Table 7. [Table 7]

[0080] Example 2 The properties of sample B_P35 were tested on a commercial 3.15 meter wide paper machine. This embodiment of the abrasive backing had a base sheet having a composition according to Base Sheet B in Table 4, and a saturant having a composition according to Saturation Formula P in Table 5. The components of the base sheet according to Table 4 were fed into a paper machine stock delivery system, formed on a Fourdrinier table, wet pressed, dried, and saturated with 28 PPU using a saturant according to Table 5. The barrier coating was applied commercially on a 3.15 meter paper machine and had a composition according to Table 6. The backside coating was applied off-line to sample B_P35_BC and had a composition according to Table 6.

[0081] Property measurements obtained from the tests are provided in Table 8. Property improvements are based on the current corresponding commercial control grades. [Table 8]

[0082] Property measurements of abrasive backing samples and corresponding abrasive backings manufactured by Neenah® Performance Materials and Monadnock Paper Mills, Inc. are provided in Table 9. The corresponding abrasive backings are manufactured on a commercial scale and the data provided is publicly available and publicly available. [Table 9]

[0083] As shown in Table 9, there is an improvement in the RMS tensile index when comparing sample B_P35 to the corresponding products from Neenah® Performance Materials and Monadnock Paper Mills, Inc. For example, there is an increase in the RMS tensile index from 63.8 Nm / g for the Monadnock Paper Mills, Inc. product in Table 9 to 106.1 Nm / g for B_P35. The difference in RMS tensile index between B_P35_BC in Table 8 and B_P35 in Table 9 is due to the backside coating applied to B_P35_BC, which increases the basis weight of B_P35_BC to 115 gsm from the basis weight of 108.7 gsm for B_P35.

[0084] The compositions and methods of the appended claims are not limited in scope by the specific compositions and methods described herein, which are intended as illustrations of some aspects of the claims, and any compositions and methods that are functionally equivalent are intended to fall within the scope of the claims. Various modifications of the compositions and methods in addition to those shown and described herein are intended to be within the scope of the appended claims. Furthermore, only certain representative compositions and method steps disclosed herein are specifically described, but other combinations of compositions and method steps are also intended to be within the scope of the appended claims even if not specifically recited. Thus, combinations of steps, elements, components, or ingredients may or may not be explicitly mentioned herein, but other combinations of steps, elements, components, and ingredients are included even if not explicitly described. As used herein, the term "comprises" and variations thereof are used synonymously with the term "comprises" and variations thereof, and are open-ended and non-limiting terms. Although the terms "comprising" and "including" have been used herein to describe various embodiments, the terms "consisting essentially of" and "consisting of" can be used in place of "comprising" and "including" to provide more specific embodiments of the invention, and are also disclosed. Except in the examples or where otherwise noted, all numbers expressing amounts of ingredients, reaction conditions, and the like used in the specification and claims should at least be understood as not intended to limit the application of the doctrine of equivalents to the scope of the claims, but should be construed in light of the number of significant digits and ordinary rounding approaches.

Claims

1. 1. An abrasive backing, comprising: a base sheet comprising wood fibers, synthetic fibers, cellulose filaments, and a saturant comprising two or more latex polymers and a crosslinking agent, the base sheet having a first surface and an opposing second surface; a barrier coating adjacent to the first surface of the base sheet; a backside coating adjacent the opposing second surface of the base sheet.

2. 10. An abrasive backing according to any one of the preceding claims, wherein the barrier coating is impermeable to liquid water and allows gas transmission.

3. 2. The abrasive backing of any one of the preceding claims, wherein two or more barrier coatings are applied adjacent to the first surface of the base sheet.

4. 10. The abrasive backing of any one of the preceding claims, wherein grit is applied adjacent to a surface of the barrier coating opposite the first surface of the base sheet.

5. 10. An abrasive backing according to any one of the preceding claims, wherein the backside coating is waterproof.

6. 10. An abrasive backing according to any one of the preceding claims, wherein a layer comprising a plurality of loops or a plurality of hooks is provided on a surface of the backside coating opposite the second surface.

7. 10. An abrasive backing according to any one of the preceding claims, wherein the wood fibres comprise hardwood fibres.

8. 10. An abrasive backing according to any one of the preceding claims, wherein the wood fibres comprise softwood fibres.

9. 10. An abrasive backing according to any one of the preceding claims, wherein the wood fibres in the base sheet comprise a blend of softwood fibres and hardwood fibres, the blend comprising 30-70% by weight softwood fibres and 70-30% by weight hardwood fibres, based on the weight of the wood fibres and the cellulose filaments in the base sheet, respectively.

10. 10. The abrasive backing of any one of the preceding claims, wherein the base sheet further comprises jute fibers, straw fibers, cotton fibers, hemp fibers, bagasse fibers, bamboo fibers, reed fibers, sisal fibers, abaca fibers, kenaf fibers, flax fibers, or combinations thereof.

11. 10. An abrasive backing according to any one of the preceding claims, wherein the two or more latex polymers comprise from 55% to 99.9% by weight, based on the weight of dry solids in the saturant.

12. 2. The abrasive backing of any one of the preceding claims, wherein at least two of the two or more latex polymers are crosslinkable.

13. 2. The abrasive backing of claim 1, wherein the saturant further comprises a third latex polymer.

14. 10. The abrasive backing of any one of the preceding claims, wherein the latex polymer is a copolymer prepared from monomers including styrene and butadiene.

15. 10. An abrasive backing according to any one of the preceding claims, wherein the latex polymer is selected from latex polymers having a Tg of from -40°C to -20°C and latex polymers having a Tg of from -12°C to 8°C.

16. 16. The abrasive backing of claim 15, wherein the latex polymer further comprises a latex polymer having a Tg of from 32°C to 52°C.

17. 17. The abrasive backing of claim 15 or 16, wherein the latex polymer comprises, based on the total dry weight of the latex polymer, 10% to 50% by weight of a latex polymer having a Tg of -40°C to -20°C, 50% to 90% by weight of a latex polymer having a Tg of -12°C to 8°C, and 10% to 50% by weight of a latex polymer having a Tg of 32°C to 52°C.

18. 10. An abrasive backing according to any one of the preceding claims, wherein the crosslinking agent comprises from 0.25% to 1.5% by weight of the saturant, based on the weight of the dry solids in the saturant.

19. 10. The abrasive backing of any one of the preceding claims, wherein the crosslinker comprises an aziridine crosslinker, a glyoxal-based crosslinker, ammonium zirconium carbonate, a carbodiimide, an aliphatic polyglycidyl ether, hexamethoxymethylmelamine, zinc diethyldithiocarbamate, or a combination thereof.

20. 10. The abrasive backing of any one of the preceding claims, wherein the crosslinker comprises an aziridine crosslinker.

21. 10. An abrasive backing according to any one of the preceding claims, wherein the cellulose filaments constitute 1% to 5% by weight based on the weight of the wood fibres and the cellulose filaments in the base sheet.

22. 10. An abrasive backing according to any one of the preceding claims, wherein the cellulose filaments have an aspect ratio of 200 to 5000 and a width of 30 to 500 nm.

23. 10. An abrasive backing according to any one of the preceding claims, wherein the synthetic fibres constitute between 2% and 8% by weight based on the weight of the wood fibres and the cellulose filaments in the base sheet.

24. 10. The abrasive backing of any one of the preceding claims, wherein the synthetic fibers comprise polyester fibers.

25. 25. The abrasive backing of claim 24, wherein the synthetic fibers comprise polyethylene terephthalate (PET).

26. 10. An abrasive backing according to any one of the preceding claims and having a basis weight of 75 to 155 gsm.

27. 1. A method of making an abrasive backing, comprising the steps of: providing a base sheet comprising wood fibers, synthetic fibers, cellulose filaments, and a saturant comprising two or more latex polymers and a crosslinking agent; applying a barrier coating to a first surface of the base sheet; and applying a backside coating to a second surface of the base sheet opposite the first surface of the base sheet.

28. Providing the base sheet comprises: Providing a base sheet comprising wood fibers, synthetic fibers, and cellulose filaments; saturating the base sheet with a saturant comprising two or more latex polymers and a crosslinking agent; 30. The method of claim 27, further comprising drying the saturated base sheet.

29. Providing a base sheet forming a base sheet from a fiber matrix including wood fibers, synthetic fibers, and cellulose filaments; 30. The method of claim 28, further comprising drying the base sheet.

30. 30. The method of making an abrasive backing as defined in claim 28 or 29, further comprising calendering the base sheet after saturating the base sheet with a saturating agent.

31. A method of making an abrasive backing according to any one of claims 27 to 30, wherein the barrier coating is impermeable to liquid water and allows gas transmission.

32. The method of making an abrasive backing according to any one of claims 27 to 31, wherein two or more barrier coatings are applied adjacent to the first surface of the base sheet.

33. 33. The method of making an abrasive backing according to any one of claims 27 to 32, wherein grit is applied adjacent to the surface of the barrier coating opposite the first surface of the base sheet.

34. A method of making an abrasive backing according to any one of claims 27 to 33, wherein the backside coating is waterproof.

35. 35. The method of making an abrasive backing according to any one of claims 27 to 34, wherein a layer comprising a plurality of loops or a plurality of hooks is applied to a surface of the backside coating opposite the second surface.

36. 36. The method of making an abrasive backing according to any one of claims 27 to 35, wherein the wood fibers comprise hardwood fibers.

37. 37. A method of making an abrasive backing according to any one of claims 27 to 36, wherein the wood fibers comprise softwood fibers.

38. 38. The method of making an abrasive backing according to any one of claims 27 to 37, wherein the wood fibers in the base sheet comprise a blend of softwood fibers and hardwood fibers, the blend comprising 30 to 70% by weight softwood fibers and 70 to 30% by weight hardwood fibers, based on the weight of the wood fibers and the cellulose filaments in the base sheet, respectively.

39. 39. The method of making an abrasive backing according to any one of claims 27 to 38, wherein the base sheet further comprises jute fibers, straw fibers, cotton fibers, hemp fibers, bagasse fibers, bamboo fibers, reed fibers, sisal fibers, abaca fibers, kenaf fibers, flax fibers, or combinations thereof.

40. 40. The method of making an abrasive backing according to any one of claims 27 to 39, wherein the two or more latex polymers comprise from 55% to 99.9% by weight of the saturant, based on the weight of dry solids in the saturant.

41. The method of making an abrasive backing according to any one of claims 27 to 40, wherein at least two of the two or more latex polymers are crosslinkable.

42. The method of making an abrasive backing according to any one of claims 27 to 41, wherein the saturant further comprises a third latex polymer.

43. The method of making an abrasive backing according to any one of claims 27 to 42, wherein the latex polymer is a copolymer prepared from monomers including styrene and butadiene.

44. 44. The method of making an abrasive backing according to any one of claims 27 to 43, wherein the latex polymer is selected from latex polymers having a Tg of -40°C to -20°C and latex polymers having a Tg of -12°C to 8°C.

45. 45. The method of making an abrasive backing according to any one of claims 27 to 44, wherein the latex polymer further comprises a latex polymer having a Tg of from 32°C to 52°C.

46. 46. ​​The method of making an abrasive backing of claim 44 or 45, wherein the latex polymer comprises, based on the total dry weight of the latex polymer, 10% to 50% by weight of a latex polymer having a Tg of -40°C to -20°C, 50% to 90% by weight of a latex polymer having a Tg of -12°C to 8°C, and 10% to 50% by weight of a latex polymer having a Tg of 32°C to 52°C.

47. 47. The method of making an abrasive backing according to any one of claims 27 to 46, wherein the crosslinking agent comprises 0.25% to 1.5% by weight of the saturant, based on the weight of the dry solids in the saturant.

48. 48. The method of making an abrasive backing according to any one of claims 27 to 47, wherein the crosslinker comprises an aziridine crosslinker, a glyoxal-based crosslinker, ammonium zirconium carbonate, a carbodiimide, an aliphatic polyglycidyl ether, hexamethoxymethylmelamine, zinc diethyldithiocarbamate, or a combination thereof.

49. The method of making an abrasive backing according to any one of claims 27 to 48, wherein the crosslinker comprises an aziridine crosslinker.

50. 50. The method of making an abrasive backing according to any one of claims 27 to 49, wherein the cellulose filaments comprise 1% to 5% by weight based on the weight of the wood fibers and the cellulose filaments in the base sheet.

51. 51. A method of making an abrasive backing according to any one of claims 27 to 50, wherein the cellulose filaments have an aspect ratio of 200 to 5000 and a width of 30 to 500 nm.

52. 52. The method of making an abrasive backing according to any one of claims 27 to 51, wherein the synthetic fibers comprise 2% to 8% by weight based on the weight of the wood fibers and the cellulose filaments in the base sheet.

53. 53. The method of making an abrasive backing according to any one of claims 27 to 52, wherein the synthetic fibers comprise polyester fibers.

54. 54. The method of making an abrasive backing according to any one of claims 27 to 53, wherein the synthetic fibers comprise polyethylene terephthalate (PET).

55. 55. The method of making an abrasive backing according to any one of claims 27 to 54, wherein the abrasive backing has a basis weight of 75 to 155 gsm.

Citation Information

Patent Citations

  • Coated abrasive article containing an electrically conductive backing

    JP1996502695A

  • Abrasive article and methods of making and using same

    JP2008542043A

  • Method for providing a surface of a polishing product, and polishing product

    JP2016508456A

  • Super Smooth Paper Backing for Fine Grit Abrasives and Methods of Their Application and Use

    US20150283676A1

  • Abrasive backers and methods of their formation

    US20150306739A1