High strength, high hardness reinforced wear resistant steel and its manufacturing method

A high-strength, high-hardness wear-resistant steel with optimized composition and microstructure addresses machining difficulties and phase transformation issues, offering enhanced mechanical and wear resistance, suitable for harsh conditions.

JP2024538834AActive Publication Date: 2024-10-23BAOSHAN IRON & STEEL CO LTD
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
JP2024526668
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2021-11-03
Filing Date
2022-11-02
Publication Date
2024-10-23
Estimated Expiration
2042-11-02

AI Technical Summary

Technical Problem

Existing wear-resistant steels face challenges with low strength and hardness, making machining difficult and prone to plastic-induced phase transformation, while requiring high hardness for harsh conditions.

Method used

A high-strength, high-hardness reinforced wear-resistant steel with optimized chemical composition, including C, Si, Mn, Cr, Al, RE, W, Mo, Ni, Nb, V, and Ti, and a microstructure of martensite + bainite + retained austenite + carbide, facilitating easy processing and enhanced wear resistance through TRIP effect.

Benefits of technology

The steel exhibits excellent mechanical performance, machinability, thermal stability, and welding performance, with improved wear resistance and toughness, maintaining hardness during use, and resisting high temperatures.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024538834000001_ABST
    Figure 2024538834000001_ABST
Patent Text Reader

Abstract

The present invention discloses a high-strength, high-hardness reinforced wear-resistant steel containing Fe and unavoidable impurities, and further containing, in mass percent, at least one of C: 0.22-0.33%, Si: 0.10-1.00%, Mn: 0.50-1.80%, Cr: 0.80-2.30%, Al: 0.010-0.10%, RE: 0.01-0.10%, W: 0.01-1.0%; and Mo: 0.01-0.80%, Ni: 0.01-1.00%, Nb: 0.005-0.080%, V: 0.01-0.20%, and Ti: 0.001-0.50%. The present invention also discloses a method for producing the high-strength, high-hardness reinforced wear-resistant steel, comprising the steps of: (1) smelting and casting; (2) heating; (3) rolling; and (4) the cooling start temperature of the first cooling is (Ar3'+5) to (Ar3'+50)°C, and M 90 <Final cooling temperature s , online quenching with cooling rate of 2~15℃ / s; then air cooling to room temperature.​
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a steel material and a manufacturing method thereof, and more particularly to a wear-resistant steel material and a manufacturing method thereof. [Background technology]

[0002] Wear-resistant steel has the characteristics of high strength and high wear resistance, and its performance is very excellent. It can be effectively used in mining, agriculture, cement production, ports, electricity, metallurgy and other fields, for example, in manufacturing mechanical products such as bulldozers, loaders, excavators, dump trucks, grabs, stack feeders and the like, and has a wide range of application prospects.

[0003] In recent years, the development of wear-resistant steels has progressed rapidly, and at present, the martensitic wear-resistant steel is the most commonly used. In such wear-resistant steels, the mechanical properties are generally improved by increasing the carbon content and adding appropriate amounts of alloying elements such as chromium, molybdenum, nickel, vanadium, boron, etc., and making full use of phase transformation strengthening after heat treatment.

[0004] However, when working conditions are relatively severe, it is often necessary to adopt wear-resistant steel plates with extremely high hardness. Due to the ultra-high hardness of such wear-resistant steels, the requirements for processing equipment such as mechanical cutting, drilling, bending, etc. are very high, making machining extremely difficult, and causing great difficulties for users.

[0005] Based on this, the present invention aims to obtain a new high-strength, high-hardness reinforced wear-resistant steel in response to the shortcomings and defects of existing wear-resistant steels: it has a lower hardness than existing conventional ultra-high hardness wear-resistant steel plates, which can bring great convenience to users in machining; during actual use, such high-strength, high-hardness reinforced wear-resistant steel is prone to plasticity-induced phase transformation, which can significantly increase the hardness of the steel plate and further improve the wear resistance of the steel plate; due to this effect, the high-strength, high-hardness reinforced wear-resistant steel of the present invention can obtain higher mechanical and wear resistance than wear-resistant steel plates of the same hardness level during actual use. Summary of the Invention [Problem to be solved by the invention]

[0006] One of the objectives of the present invention is to provide a high-strength, high-hardness reinforced wear-resistant steel which has excellent mechanical properties, and at the same time, excellent machinability, thermal stability and weldability, achieves a combination of high hardness and high toughness, has excellent machinability, and also has excellent mechanical properties and good wear resistance during actual use, and has very good prospects for popularization and application value. [Means for solving the problem]

[0007] The high-strength, high-hardness reinforced wear-resistant steel of the present invention is easy to process and provides convenience for general mechanical processing. During use, the steel obtains excellent toughness and wear resistance through plasticity-induced phase transformation, and has excellent performance, making it suitable for wide application in wear-resistant parts in engineering machinery.

[0008] In order to achieve the above object, the present invention provides a high-strength, high-hardness reinforced wear-resistant steel containing Fe and unavoidable impurities, and further containing, in mass percent, at least one of C: 0.22-0.33%, Si: 0.10-1.00%, Mn: 0.50-1.80%, Cr: 0.80-2.30%, Al: 0.010-0.10%, RE: 0.01-0.10%, W: 0.01-1.0%; and Mo: 0.01-0.80%, Ni: 0.01-1.00%, Nb: 0.005-0.080%, V: 0.01-0.20%, and Ti: 0.001-0.50%.

[0009] Furthermore, in the high-strength, high-hardness reinforced wear-resistant steel according to the present invention, the mass percentages of the chemical elements are C: 0.22-0.33%, Si: 0.10-1.00%, Mn: 0.50-1.80%, Cr: 0.80-2.30%, Al: 0.010-0.10%, RE: 0.01-0.10%, W: 0.01-1.0%; and at least one of Mo: 0.01-0.80%, Ni: 0.01-1.00%, Nb: 0.005-0.080%, V: 0.01-0.20%, and Ti: 0.001-0.50%, with the remainder being Fe and unavoidable impurities.

[0010] In the present invention, the high-strength, high-hardness reinforced wear-resistant steel according to the present invention mainly contains C, Si elements and Mn, Cr alloying elements, and may contain Mo, Ni, and other precious metal elements as required, thereby keeping the cost of the alloy low while ensuring the performance of the steel material.

[0011] In the high strength and high hardness reinforced wear-resistant steel of the present invention, the design principles of each chemical element are as follows: C: In the high-strength, high-hardness reinforced wear-resistant steel according to the present invention, C is the most basic and most important element in the wear-resistant steel, and adding an appropriate amount of C element can increase the strength and hardness of the steel material, and further improve the wear resistance of the steel material. However, it should be noted that C element also has an adverse effect on the toughness and welding performance of the steel material at the same time, so the content of C element in the steel needs to be reasonably controlled. Based on this, and taking into account the effect of the content of C element on the performance of the wear-resistant steel, in the high-strength, high-hardness reinforced wear-resistant steel according to the present invention, the mass percentage of C element is controlled to 0.22-0.33%, more preferably 0.23-0.28%. In some embodiments, the mass percentage of C is 0.22-0.31%. In some embodiments, the mass percentage of C is 0.23-0.31%. In some embodiments, the mass percentage of C is 0.23-0.30%.

[0012] Si: In the high-strength, high-hardness reinforced wear-resistant steel according to the present invention, Si can dissolve in ferrite and austenite, and can increase their hardness and strength, but if the Si element content is too high, the toughness of the steel material will drop sharply. At the same time, the Si element has a stronger affinity with O than Fe, and is prone to generate low-melting silicates during welding, which increases the fluidity of slag and molten metal and affects welding quality. In consideration of this, the content of the Si element in the steel should not be too high. Based on this, in the high-strength, high-hardness reinforced wear-resistant steel according to the present invention, the mass percentage of the Si element is controlled to 0.10-1.00%. In some embodiments, the mass percentage of Si is 0.10-0.80%. In some embodiments, the mass percentage of Si is 0.15-0.80%. In some embodiments, the mass percentage of Si is 0.15-0.65%.

[0013] Mn: In the high-strength, high-hardness reinforced wear-resistant steel according to the present invention, adding an appropriate amount of Mn element can strongly improve the hardenability of the steel material and reduce the transformation temperature of the steel material and the critical cooling rate of the steel material. However, if the content of Mn element in the steel is too high, not only does the grains tend to become coarse, but also increases the tempering brittleness susceptibility of the steel, and segregation and cracks are easily generated in the cast slab, which reduces the performance of the steel plate, so it should be noted that the content of Mn element in the steel should not be too high. Based on this, in the high-strength, high-hardness reinforced wear-resistant steel according to the present invention, the mass percentage of Mn element is controlled to 0.50-1.80%, preferably 1.05-1.65%. In some embodiments, the mass percentage of Mn is 1.00-1.80%. In some embodiments, the mass percentage of Mn is 1.10-1.80%. In some embodiments, the mass percentage of Mn is 1.10-1.80%. In some embodiments, the weight percent of Mn is between 1.15 and 1.80%. In some embodiments, the weight percent of Mn is between 0.65 and 1.65%.

[0014] Cr: In the high-strength, high-hardness reinforced wear-resistant steel according to the present invention, the Cr element can reduce the critical cooling rate and improve the hardenability of the steel. Cr is present in the steel as (Fe,Cr)3C, (Fe,Cr)7C3 and (Fe,Cr) 23 It can form various carbides such as C7, effectively increasing the strength and hardness of the steel. In addition, by adding an appropriate amount of Cr to the steel, it is possible to prevent or alleviate the precipitation and aggregation of carbides during tempering, thereby improving the tempering stability of the steel. Based on this, and taking into account the beneficial effects of the Cr element, the mass percentage of the Cr element in the high-strength, high-hardness reinforced wear-resistant steel according to the present invention may be controlled to 0.80-2.30%, more preferably 1.25-2.10%. In some embodiments, the mass percentage of Cr is 1.10-2.20%. In some embodiments, the mass percentage of Cr is 1.10-2.00%. In some embodiments, the mass percentage of Cr is 1.15-2.00%. In some embodiments, the mass percentage of Cr is 0.95-2.10%.

[0015] Al: In the high-strength, high-hardness reinforced wear-resistant steel according to the present invention, the Al element forms fine, hardly soluble AlN particles with the N element in the steel, and can refine the crystal grains of the steel. By adding an appropriate amount of the Al element to the steel, the crystal grains of the steel can be effectively refined, N and O in the steel can be fixed, the sensitivity of the steel to notches can be reduced, the aging phenomenon of the steel can be reduced or eliminated, and the toughness of the steel can be increased. Based on this, in the high-strength, high-hardness reinforced wear-resistant steel according to the present invention, the mass percentage of the Al element is controlled to 0.010-0.10%, more preferably 0.035-0.080%. In some embodiments, the mass percentage of Al is 0.010-0.080%. In some embodiments, the mass percentage of Al is 0.015-0.075%. In some embodiments, the mass percentage of Al is 0.015-0.070%. In some embodiments, the mass percentage of Al is 0.025-0.080%.

[0016] RE: In the high strength, high hardness reinforced wear-resistant steel according to the present invention, the addition of an appropriate amount of rare earth can reduce the segregation of elements such as sulfur and phosphorus, improve the shape, size and distribution of nonmetallic inclusions, and at the same time refine the crystal grains and increase the hardness. In addition, rare earth increases the bending strength ratio, which is advantageous for improving the toughness of low alloy high strength steel and can improve the thermal stability of steel plate. However, it should be noted that the content of rare earth in steel should not be too high, since if the content of rare earth in steel is too high, serious segregation may occur, which may deteriorate the quality and mechanical performance of the cast slab. Based on this, in the high strength, high hardness reinforced wear-resistant steel according to the present invention, the mass percentage of RE is controlled to 0.01-0.10%, more preferably 0.03-0.10%. In some embodiments, the mass percentage of RE is 0.025-0.080%.

[0017] W: In the high-strength, high-hardness reinforced wear-resistant steel according to the present invention, tungsten can improve the tempering stability and thermal strength of the steel, and can play a role in refining certain crystal grains. In addition, tungsten can form hard carbides to improve the wear resistance of the steel. Thus, in order to exert the beneficial effects of tungsten, the mass percentage of W element is controlled to 0.01-1.0%, more preferably 0.05-0.85%, in the high-strength, high-hardness reinforced wear-resistant steel according to the present invention. In some embodiments, the mass percentage of W is 0.05-0.85%.

[0018] Mo: In the high-strength, high-hardness reinforced wear-resistant steel according to the present invention, the addition of an appropriate amount of Mo can effectively refine the crystal grains and increase the strength and toughness of the steel. Mo exists in the solid solution phase and the carbide phase in the steel, so that the Mo-containing steel simultaneously plays the role of solid solution strengthening and carbide dispersion strengthening. In addition, Mo is an element that reduces temper brittleness, and the temper stability of the material can be improved by adding an appropriate amount of Mo element to the steel. Based on this, in the high-strength, high-hardness reinforced wear-resistant steel according to the present invention, if added, the mass percentage of Mo element is controlled to 0.01-0.80%, preferably 0.08-0.55%.

[0019] Ni: In the high-strength, high-hardness reinforced wear-resistant steel according to the present invention, Ni can be dissolved with Fe in any ratio, and can improve the low-temperature toughness of the steel by refining the ferrite grains, and can play a role in significantly lowering the cold brittle transformation temperature. However, if the Ni content in the steel is too high, the oxide scale on the surface of the steel plate is difficult to remove, which is likely to lead to a significant increase in production costs, so it should be noted that the Ni content in the steel should not be too high. Based on this, in the high-strength, high-hardness reinforced wear-resistant steel according to the present invention, if added, the mass percentage of Ni element is controlled to 0.01-1.00%, preferably 0.25-0.85%.

[0020] Nb: In the high-strength, high-hardness reinforced wear-resistant steel of the present invention, the addition of an appropriate amount of Nb element can play the role of refining crystal grains and precipitation strengthening, and contribute significantly to improving the toughness of the material; Nb element can effectively increase the strength and toughness of steel material by refining crystal grains, and can also improve and improve the performance of steel material by precipitation strengthening and phase transformation strengthening, so Nb has become one of the most effective strengthening agents in high-strength low-alloy structural steel; Nb is also a strong carbon compound and nitrogen compound forming element, and can strongly suppress the growth of austenite crystal grains. Based on this, in the high-strength, high-hardness reinforced wear-resistant steel of the present invention, if added, the mass percentage of Nb element is controlled to 0.005-0.080%, preferably 0.01-0.045%.

[0021] V: In the high-strength, high-hardness reinforced wear-resistant steel according to the present invention, the addition of an appropriate amount of V element can effectively refine the grains and prevent the growth of austenite grains from becoming coarse during the heating stage of the steel billet, which can further refine the grains of the steel during the subsequent multiple rolling processes and further increase the strength and toughness of the steel material. Based on this, in the high-strength, high-hardness reinforced wear-resistant steel according to the present invention, if added, the mass percentage of V element is controlled to 0.01-0.20%, preferably 0.03-0.15%.

[0022] Ti: In the high-strength, high-hardness reinforced wear-resistant steel of the present invention, Ti is one of the elements that strongly form carbides, and Ti element can combine with C element to form fine TiC particles. Among them, TiC particles are small and can be distributed at grain boundaries, thereby realizing the effect of refining crystal grains; TiC particles are also hard and can improve the wear resistance of steel. Based on this, and taking into account the beneficial effect of Ti element, in the high-strength, high-hardness reinforced wear-resistant steel of the present invention, if added, the mass percentage of Ti element is controlled to 0.001-0.50%, preferably 0.015-0.45%.

[0023] More preferably, in the high-strength, high-hardness reinforced wear-resistant steel according to the present invention, the mass percentages of the chemical elements satisfy the following: C: 0.22-0.31%, Si: 0.10-0.80%, Mn: 1.00-1.80%, Cr: 1.10-2.20%, and Al: 0.010-0.080%.

[0024] More preferably, in the high-strength, high-hardness reinforced wear-resistant steel according to the present invention, the mass percentages of the chemical elements satisfy C: 0.23-0.31%, Si: 0.15-0.80%, Mn: 1.10-1.80%, Cr: 1.10-2.00%, and Al: 0.015-0.075%.

[0025] Most preferably, in the high-strength, high-hardness reinforced wear-resistant steel according to the present invention, the mass percentages of the chemical elements satisfy the following: C: 0.23-0.30%, Si: 0.15-0.65%, Mn: 1.15-1.80%, Cr: 1.15-2.00%, and Al: 0.015-0.070%.

[0026] Furthermore, in the high-strength, high-hardness reinforced wear-resistant steel according to the present invention, the unavoidable impurities include P≦0.030% and / or S≦0.010%.

[0027] In the present invention, both P and S are unavoidable impurities, and in order to ensure the quality of the wear-resistant steel, the lower the content of the impurity elements in the steel, the better, as long as conditions permit. Both P and S are harmful elements, and their contents should be strictly controlled. Therefore, in the high-strength, high-hardness reinforced wear-resistant steel of the present invention, the unavoidable impurity elements are controlled to satisfy P≦0.030% and / or S≦0.010%.

[0028] Furthermore, in the high-strength, high-hardness reinforced wear-resistant steel according to the present invention, the microstructure is martensite + bainite + retained austenite + carbides.

[0029] Furthermore, in the high strength, high hardness reinforced wear resistant steel according to the present invention, the volume fraction of retained austenite is ≧5%, and the volume fraction of martensite is ≦90%. In some embodiments, in the high strength, high hardness reinforced wear resistant steel according to the present invention, the volume fraction of retained austenite is 5-15%, and the volume fraction of martensite is 60-90%. In some embodiments, in the high strength, high hardness reinforced wear resistant steel according to the present invention, the volume fraction of retained austenite is 5.3-12.0%, for example, 5.5-8.5%, and the volume fraction of martensite is 70-88%, for example, 77.5-85.6%.

[0030] Compared with ordinary low-alloy steel plates with the same hardness level, the high-strength, high-hardness reinforced wear-resistant steel of the present invention has a microstructure that is different from the currently common martensite structure, and instead has a microstructure of martensite + bainite + retained austenite + carbide.

[0031] Based on the above microstructure, the mechanical properties of the high-strength, high-hardness reinforced wear-resistant steel of the present invention can be ensured, and this high-strength, high-hardness reinforced wear-resistant steel has a relatively low hardness, which brings great convenience to users in mechanical processing and is suitable for easy processing situations.

[0032] In addition, during actual use, the high-strength, high-hardness reinforced wear-resistant steel of the present invention has excellent wear resistance, which is mainly due to the occurrence of the TRIP (phase transformation induced plasticity) effect during use, that is, since this steel plate contains a certain proportion of austenite in addition to a certain amount of martensite or bainite, when the steel plate is impacted, struck, or worn during use, a plasticity induced phase transformation occurs, which greatly increases the strength and hardness of the steel plate and further improves the wear resistance of the steel plate. Due to this effect, the high-strength, high-hardness reinforced wear-resistant steel of the present invention can obtain higher mechanical and wear resistance during actual use than ordinary wear-resistant steel plates of the same hardness level.

[0033] In addition, the high-strength, high-hardness reinforced wear-resistant steel of the present invention has a special microstructure and contains added RE and W elements, so that it can obtain a certain degree of high temperature resistance, and the loss of hardness of this steel plate is not significant even at high temperatures.

[0034] Furthermore, the high-strength, high-hardness reinforced wear-resistant steel according to the present invention has a Brinell hardness of 400 to 500 HBW, a tensile strength of 1200 to 1600 MPa (for example, 1300 to 1600 MPa), an elongation of 10 to 15%, and a Charpy V-type longitudinal impact energy at -40°C of >40 J.

[0035] In some embodiments, the high strength, high hardness reinforced wear resistant steel according to the present invention has a Brinell hardness of 420 to 480 HBW, a tensile strength of 1220 to 1450 MPa, an elongation of 10 to 15%, and a Charpy V-type longitudinal impact energy at -40°C of >40 J, for example, 41 to 60 J.

[0036] In some embodiments, the high strength, high hardness reinforced wear resistant steel according to the present invention has a yield strength of 800 to 1000 MPa, for example, 830 to 980 MPa. In some embodiments, the high strength, high hardness reinforced wear resistant steel according to the present invention has a bending strength ratio of ≦0.75, preferably ≦0.70.

[0037] In some embodiments, the high strength, high hardness reinforced wear resistant steel according to the present invention is measured to have a Brinell hardness of the steel plate surface that is 10% or more higher, preferably 13% or more higher than the Brinell hardness of the steel plate before the test, after being subjected to an impact energy strike of 550 J. In some embodiments, the high strength, high hardness reinforced wear resistant steel according to the present invention is measured to have a Brinell hardness of the steel plate surface that is ≧480 HBW, for example, 480 to 560 HBW, after being subjected to an impact energy strike of 550 J.

[0038] Accordingly, another object of the present invention is to provide a simple and feasible method for producing a high-strength, high-hardness reinforced wear-resistant steel, the high-hardness reinforced wear-resistant steel produced by this method has excellent comprehensive performance, a Brinell hardness of 400-500 HBW, a tensile strength of 1200-1600 MPa (e.g., 1300-1600 MPa), an elongation of 10-15%, and a Charpy V-type longitudinal impact energy of >40 J at -40°C, and has very good prospects for popularization and application value.

[0039] In order to achieve the above object, the present invention provides a method for producing the high-strength, high-hardness reinforced wear-resistant steel, comprising the following steps: (1) Smelting and foundry; (2) heating; (3) Rolling; (4) The initial cooling start temperature is (Ar3'+5)~(Ar3'+50)℃, and M 90 <Final cooling temperature s , online quenching with cooling rate of 2~15℃ / s; then air cooling to room temperature.

[0040] In the manufacturing method of the high-strength, high-hardness reinforced wear-resistant steel according to the present invention, each smelting raw material is added according to the compounding ratio of the chemical components designed by the inventors, and the high-strength, high-hardness reinforced wear-resistant steel can be obtained by sequentially going through the steps of smelting, casting, heating, rolling and online quenching.

[0041] In the online quenching process in the above step (4) of the present invention, the initial cooling may be water cooling or oil cooling.

[0042] ​ In the present invention, Ar3' represents the temperature at which austenite begins to transform into ferrite during online quenching, and B s indicates the temperature at which the Bainite begins to transform, and M 90 represents the temperature at which the martensite volume ratio is 90%.

[0043] Furthermore, in the manufacturing method described in the present invention, in step (2), the slab heating temperature is controlled to 1030 to 1230° C. and kept at that temperature for 1 to 3 hours. In some embodiments, the slab heating temperature is controlled to 1050 to 1210° C. and kept at that temperature for 1 to 3 hours.

[0044] Furthermore, in the manufacturing method described in the present invention, the slab heating temperature is controlled to 1030 to 1180°C in the step (2).

[0045] Accordingly, in some other embodiments, it is more preferable to control the heating temperature to 1030-1160°C; most preferably, the heating temperature is controlled to 1030-1140°C to improve production efficiency and prevent excessive growth of austenite grains and serious oxidation of the slab surface.

[0046] Furthermore, in the manufacturing method according to the present invention, in step (3), the rough rolling temperature is controlled to 930 to 1180° C., and the finish rolling temperature is controlled to 870 to 970° C. In some embodiments, in step (3), the rough rolling temperature is controlled to 950 to 1150° C., and the finish rolling temperature is controlled to 885 to 955° C.

[0047] Furthermore, in the manufacturing method according to the present invention, in step (3), the rough rolling temperature is controlled to 930 to 1130°C, and the finish rolling temperature is controlled to 875 to 945°C.

[0048] Furthermore, in the manufacturing method according to the present invention, in step (3), the rolling reduction in the rough rolling stage is controlled to more than 35%, and the rolling reduction in the finish rolling stage is controlled to more than 55%. Furthermore, in the manufacturing method according to the present invention, in step (3), the rolling reduction in the rough rolling stage is controlled to 35 to 75%, and the rolling reduction in the finish rolling stage is controlled to 55 to 80%.

[0049] More preferably, in some other embodiments, in order to obtain better implementation effects, the present invention controls the rough rolling temperature to 930-1110°C, the rolling reduction in the rough rolling stage to 38% or more, the finish rolling temperature to 875-935°C, and the rolling reduction in the finish rolling stage to 58% or more.

[0050] Most preferably, in step (3), the rough rolling temperature during rolling is controlled to 935 to 1105° C., the rolling reduction in the rough rolling stage is controlled to more than 40%, the controlled fine rolling temperature is controlled to 875 to 930° C., and the rolling reduction in the fine rolling stage is controlled to more than 60%.

[0051] Furthermore, in the production method according to the present invention, in step (4), the cooling start temperature of the initial cooling is (Ar3'+5) to (Ar3'+45)°C, and (M 90 +5℃)<Final cooling temperature<(B s -15℃) and the cooling rate is 2~12℃ / s.

[0052] In some other embodiments, the initial cooling start temperature is (Ar3'+5) to (Ar3'+40) °C, and the final cooling temperature is (M 90 +5℃)<Final cooling temperature<(B s The temperature may be controlled so as to satisfy the above condition (−20° C.) and the cooling rate may be controlled to be 2 to 11° C. / s.

[0053] Most preferably, the initial cooling start temperature is (Ar3'+5) to (Ar3'+38) ° C., and the final cooling temperature is (M 90 +5℃)<Final cooling temperature<(B s The cooling rate may be controlled to be 3 to 11°C / s.

[0054] In some embodiments, the final cooling temperature is between 350 and 450°C. In some embodiments, the high strength, high hardness reinforced wear resistant steel of the present invention has a thickness of 9 to 25 mm.

[0055] The high-strength, high-hardness reinforced wear-resistant steel and its manufacturing method according to the present invention have the following advantages and beneficial effects compared to the prior art: (1) When designing the chemical composition, the high-strength, high-hardness reinforced wear-resistant steel of the present invention has fully optimized alloy components, mainly adding C, Si elements and Mn, CI alloy elements, and appropriately adding Mo, Ni and other precious metal elements as necessary, thereby keeping the alloy cost low and ensuring the performance of the steel material. (2) From the viewpoint of microstructure, the high strength and high hardness reinforced wear resistant steel of the present invention has a microstructure of martensite + bainite + retained austenite + carbide (wherein the volume fraction of martensite is <90%, the volume fraction of retained austenite is >5%, and the rest is bainite and carbide), which generates the TRIP effect in the steel plate during use, thereby increasing the hardness and wear resistance of the steel plate and further improving the practicality and service life of the steel plate. In addition, the hard phases such as carbides of Ti, Cr, Mo, and W, which are uniformly distributed in large quantities, can further improve the wear resistance and service life of the steel plate. (3) The high-strength, high-hardness reinforced wear-resistant steel of the present invention has a lower hardness than conventional martensitic wear-resistant steels, which brings great convenience to users in machining and is suitable for easy processing; and due to the addition of RE and W elements, the high-strength, high-hardness reinforced wear-resistant steel of the present invention has a certain high temperature resistance, and even at high temperatures, the steel plate does not lose much of its hardness.

[0056] From the above, the present invention scientifically designs carbon, alloy components and their compounding ratios under reasonable production process conditions, reduces the alloy cost, and the production process is simple and feasible, which is favorable for industrial production; accordingly, the high-strength, high-hardness reinforced wear-resistant steel of the present invention has excellent mechanical properties (such as hardness, strength, elongation, impact toughness and a certain high temperature resistance), processing performance and usability, with a Brinell hardness of 400-500HBW, a tensile strength of 1200-1600MPa (for example, 1300-1600MPa), an elongation of 10-15%, and a Charpy V-type longitudinal impact energy of >40J at -40℃, and has very good popular prospects and application value. [Brief description of the drawings]

[0057] [Figure 1] FIG. 1: Metallographic micrograph of the high-strength, high-hardness reinforced wear-resistant steel produced in Example 3. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0058] The high-strength, high-hardness reinforced wear-resistant steel and its manufacturing method according to the present invention will be further interpreted and explained below by combining specific examples, but these interpretations and explanations are not intended to unduly limit the configuration of the embodiments of the present invention.

[0059] Examples 1 to 8 The high-strength, high-hardness reinforced wear-resistant steels of Examples 1 to 8 were all produced by the following process: (1) Smelting and casting were carried out according to the chemical composition ratios shown in Table 1. (2) Heating: The obtained slab was heated, and the slab heating temperature was controlled to 1030 to 1230°C and kept at that temperature for 1 to 3 hours; of course, the slab heating temperature may be controlled preferably to 1030 to 1180°C. (3) Rolling: The heated slab is rolled, and the rough rolling temperature is controlled to 930-1180°C, the finish rolling temperature is controlled to 870-970°C, the rolling reduction in the rough rolling stage is controlled to more than 35%, and the rolling reduction in the finish rolling stage is controlled to more than 55%; of course, when the rolling reduction in the rough rolling stage is controlled to more than 35% and the rolling reduction in the finish rolling stage is controlled to more than 55%, the rough rolling temperature may be preferably controlled to 930-1130°C, and the finish rolling temperature may be preferably controlled to 875-945°C. (4) The initial cooling start temperature is ((Ar3'+5)~(Ar3'+50)℃, and M 90 <Final cooling temperature s , online quenching with a cooling rate of 2-15°C / s; then air-cooling to room temperature; of course, it is preferable that the initial cooling start temperature is (Ar3'+5)-(Ar3'+50)°C and the final cooling temperature is (M 90 +5℃)<Final cooling temperature<(B s -15℃) and the cooling rate is controlled to be 2 to 12℃ / s. ​

[0060] The high-strength, high-hardness reinforced wear-resistant steels of Examples 1 to 8 according to the present invention were all produced by the above-mentioned process, and their chemical compositions and related process parameters all satisfied the design specification control requirements of the present invention.

[0061] Table 1 shows the mass percentage of each chemical element in the high-strength, high-hardness reinforced wear-resistant steels of Examples 1 to 8.

[0062] [Table 1]

[0063] Specific process parameters in each step of the above-mentioned manufacturing method for the high-strength, high-hardness reinforced wear-resistant steels of Examples 1 to 8 are shown in Tables 2-1 and 2-2.

[0064] [Table 2-1]

[0065] [Table 2-2]

[0066] Note: In Table 2-2, Ar3' represents the temperature at which austenite begins to transform into ferrite during on-line quenching of the test steel, and B s represents the temperature at which bainite begins to transform, and M 90 represents the temperature at which the martensite volume ratio is 90%.

[0067] The finally obtained high-hardness strengthened wear-resistant steels of Examples 1 to 8 were sampled, and the high-hardness strengthened wear-resistant steel samples of Examples 1 to 8 were observed and analyzed. The observation revealed that the microstructure of all the high-hardness strengthened wear-resistant steels of Examples 1 to 8 was martensite + bainite + retained austenite + carbide. A metallographic photograph of Example 3 is shown in FIG.

[0068] Accordingly, further analysis was performed on the microstructures of the high hardness strengthened wear resistant steels of Examples 1 to 8 to obtain the volume fractions of the retained austenite structure and the volume fractions of the martensite structure. Here, the volume fractions of the retained austenite structure were all >5% and the volume fractions of the martensite structure were all <90%, and the results of the volume fractions of the retained austenite structure are shown in Table 3 below.

[0069] [Table 3]

[0070] It can be seen from Table 3 above that the high-strength, high-hardness reinforced wear-resistant steels of Examples 1 to 8 according to the present invention have a volume fraction of retained austenite of 5.6 to 8.3%.

[0071] After completing the microstructural observation of the high strength, high hardness reinforced wear resistant steels of the above-mentioned Examples 1 to 8 of the present invention, the mechanical performance of the high strength, high hardness reinforced wear resistant steel samples of Examples 1 to 8 was further tested to obtain the mechanical performance parameters of the high hardness reinforced wear resistant steels of Examples 1 to 8. The obtained test results are shown in Table 4 below.

[0072] The test procedures for correlation mechanical performance are as follows: Tensile test: A tensile performance test was carried out at room temperature using an SCL 233200 kN room temperature tensile tester based on the GB / T 228.1 standard, and the tensile strength and elongation at room temperature of the high-strength, high-hardness reinforced wear-resistant steel samples of Examples 1 to 8 were measured.

[0073] Cold bending test: The high-strength, high-hardness reinforced wear-resistant steels of Examples 1 to 8 were subjected to bending tests at room temperature, and corresponding results were obtained; bending tests were performed at room temperature using a YJW-2000 electric hydraulic dedicated server bending tester in accordance with the GB / T232 standard; after the bending test, the samples were observed without using a magnifying device, and if no cracks were found on the outer surface, they were rated as "passed."

[0074] Brinell hardness test: The Brinell hardness test was performed at room temperature using an SCL 246 Brinell hardness tester according to the GB / T 231.1 standard. The high strength, high hardness reinforced wear-resistant steel samples of Examples 1 to 8 were each subjected to a hardness test at the surface position to obtain the Brinell hardness of the corresponding Example.

[0075] After obtaining the Brinell hardness of the high-hardness reinforced wear-resistant steel samples of Examples 1 to 8, the steel plate of each Example was struck with an impact energy of 550 J using a homemade hammer equipment, and then the Brinell hardness of the steel plate surface was measured to obtain the Brinell hardness after reinforcement.

[0076] Impact test: An SCL 186750J instrumented impact tester was used at -40°C to perform impact performance tests according to GB / T 229. The impact toughness of each of the high-strength, high-hardness reinforced wear-resistant steel samples of Examples 1 to 8 was tested, and the corresponding impact energy was obtained.

[0077] Table 4 shows the results of the mechanical performance tests at the surface positions of the high-strength, high-hardness reinforced wear-resistant steels of Examples 1 to 8.

[0078] [Table 4]

[0079] Note: Hardness after strengthening: The Brinell hardness of the steel plate surface measured after striking the sample steel plate with 550J impact energy using a homemade hammer equipment.

[0080] From Table 4 above, the high-strength, high-hardness reinforced wear-resistant steels of Examples 1 to 8 according to the present invention not only have extremely excellent mechanical performance and properties such as high strength, high hardness, and high elongation, but also have excellent low-temperature impact toughness, with a yield strength of 835 to 980 MPa, a tensile strength of 1240 to 1415 MPa, an elongation of 12 to 15%, a surface Brinell hardness of 422 to 475 HBW, and a Charpy V-type longitudinal impact energy at -40°C of 42 to 57 J.

[0081] The high-hardness, high-hardness reinforced wear-resistant steels of Examples 1 to 8 according to the present invention had good Brinell hardness even after reinforcement, and the Brinell hardness of the steel plates of each Example after reinforcement, measured after striking the sample steel plate with an impact energy of 550 J using a homemade hammer equipment, was 493 to 545 HBW.

[0082] Accordingly, the high-strength, high-hardness reinforced wear-resistant steels of Examples 1 to 8 according to the present invention all had very good cold bending performance, no cracks were observed on the outer surface of the samples after the bending test, and all were "passed." The steel plate according to the present invention has an extremely low yield strength, and therefore has very good forming processability, such as bending the steel plate, compared to normal wear-resistant steels of the same hardness level.

[0083] In view of the above, in the high-strength, high-hardness reinforced wear-resistant steel of the present invention, a wear-resistant steel with a microstructure of martensite + bainite + retained austenite + carbide is obtained through rational chemical element composition design and compounding optimization technology; this high-strength, high-hardness reinforced wear-resistant steel has excellent mechanical properties (e.g., hardness, strength, elongation, impact toughness and a certain degree of high temperature resistance) and at the same time has good processing performance and usability.

[0084] The high-strength, high-hardness reinforced wear-resistant steel of the present invention is not only easy to process and convenient for ordinary machining, but also has excellent toughness and wear resistance during use, and can be widely used in wear-resistant parts in engineering machinery.

[0085] In addition, the prior art portion in the scope of protection of the present invention is not limited to the examples described in the present application documents, but includes, but is not limited to, all prior art, prior patent documents, prior published publications, prior published uses, etc. that are not inconsistent with the aspects of the present invention and can be incorporated into the scope of protection of the present invention.

[0086] In addition, the combination methods of each technical feature in this application are not limited to the combination methods described in the claims of this application or the combination methods described in the specific examples, and all technical features described in this application may be freely combined or combined in any manner as long as there are no contradictions between them.

[0087] It should be noted that the above are only specific examples of the present invention, and the present invention is not limited to the above examples, and it is obvious that there are many similar variations thereto. All modifications directly derived or conceived by those skilled in the art from the disclosure of the present invention are included in the protection scope of the present invention.

Claims

1. A high-strength, high-hardness, reinforced wear-resistant steel containing Fe and unavoidable impurities, Further, the high-strength, high-hardness reinforced wear-resistant steel contains, in mass percent, at least one of C: 0.22-0.33%, Si: 0.10-1.00%, Mn: 0.50-1.80%, Cr: 0.80-2.30%, Al: 0.010-0.10%, RE: 0.01-0.10%, W: 0.01-1.0%; and Mo: 0.01-0.80%, Ni: 0.01-1.00%, Nb: 0.005-0.080%, V: 0.01-0.20%, and Ti: 0.001-0.50%.

2. The mass percentages of each chemical element are C: 0.22-0.33%, Si: 0.10-1.00%, Mn: 0.50-1.80%, Cr: 0.80-2.30%, Al: 0.010-0.10%, RE: 0.01-0.10%, W: 0.01-1.0%; and at least one of Mo: 0.01-0.80%, Ni: 0.01-1.00%, Nb: 0.005-0.080%, V: 0.01-0.20%, and Ti: 0.001-0.50%, with the remainder being Fe and unavoidable impurities. High strength, high hardness reinforced wear-resistant steel according to claim 1.

3. The mass percentages of each chemical element are: C: 0.22-0.31%, Si: 0.10-0.80%, Mn: 1.00-1.80%, Cr: 1.10-2.20%, Al: 0.010-0.080%; or the mass percentages of each chemical element are: C: 0.23-0.31%, Si: 0.15-0.80%, Mn: 1.10-1.80%, 3. The high-strength, high-hardness reinforced wear-resistant steel according to claim 1 or 2, wherein the mass percentages of the chemical elements are as follows: C: 0.23-0.30%, Si: 0.15-0.65%, Mn: 1.15-1.80%, Cr: 1.15-2.00%, Al: 0.015-0.070%.

4. 3. High strength, high hardness reinforced wear resistant steel according to claim 1 or 2, characterized in that the mass percentages of the chemical elements have one or more of the following characteristics: The C content is 0.23-0.28%; the Si content is 0.15-0.65%; the Mn content is 1.05-1.65%; the Cr content is 1.25-2.10%; and the Al content is 0.035-0.080%.

5. 3. The high-strength, high-hardness, reinforced wear-resistant steel according to claim 1, wherein the unavoidable impurities include P≦0.030% and / or S≦0.010%.

6. 3. The high-strength, high-hardness reinforced wear-resistant steel according to claim 1, having a microstructure of martensite + bainite + retained austenite + carbides.

7. 3. The high-strength, high-hardness reinforced wear-resistant steel according to claim 1 or 2, wherein the volume fraction of retained austenite is ≧5%, and the volume fraction of martensite is ≦90%; preferably, the volume fraction of retained austenite is 5-15%, and the volume fraction of martensite is 60-90%; more preferably, the volume fraction of retained austenite is 5.3-12.0% or 5.5-8.5%, and the volume fraction of martensite is 70-88% or 77.5-85.6%.

8. 3. High strength, high hardness reinforced wear resistant steel according to claim 1 or 2, having a Brinell hardness of 400-500 HBW, a tensile strength of 1200-1600 MPa, an elongation of 10-15%, a Charpy V-type longitudinal impact energy at -40°C of >40 J; preferably a yield strength of 800-1000 MPa, preferably 830-980 MPa; and preferably a bending strength ratio of ≦0.75, preferably ≦0.

70.

9. A method for producing a high-strength, high-hardness reinforced wear-resistant steel according to any one of claims 1 to 8, comprising the following steps: (1) Smelting and foundry; (2) Heating; (3) rolling; (4) The cooling start temperature of the initial cooling is (Ar3'+5) to (Ar3'+50) ° C., and M 90 <Final cooling temperature <B s , online quenching with a cooling rate of 2-15°C / s; then air cooling to room temperature.

10. The method according to claim 9, wherein in the step (2), the slab heating temperature is controlled to 1030 to 1230° C. and kept at that temperature for 1 to 3 hours.

11. The method according to claim 10, wherein in the step (2), the slab heating temperature is controlled to 1030 to 1180°C.

12. The manufacturing method according to claim 9, wherein in the step (3), the rough rolling temperature is controlled to 930 to 1180 ° C. and the finish rolling temperature is controlled to 870 to 970 ° C.

13. The manufacturing method according to claim 12, wherein in the step (3), the rough rolling temperature is controlled to 930 to 1130 ° C. and the finish rolling temperature is controlled to 875 to 945 ° C.

14. The manufacturing method according to any one of claims 9 to 13, wherein in the step (3), the rolling reduction in the rough rolling stage is controlled to more than 35% and the rolling reduction in the finish rolling stage is controlled to more than 55%.

15. In step (4), the cooling start temperature of the first cooling is (Ar3'+5) to (Ar3'+45) ° C., and (M 90 +5℃)<Final cooling temperature<(B s The method according to claim 9, wherein the cooling rate is from 2 to 12° C. / s.

Citation Information

Patent Citations

  • Steel plate with great heat and abrasion resistance and manufacturing method thereof

    CN103205650A

  • High-hardness low-alloy wear-resistant steel plate and its manufacturing method

    JP2016505094A

  • Case-hardened steel having excellent fatigue characteristics

    WO2014061784A1