Threaded ends of tubular elements having coatings containing zinc-chromium alloys
The zinc-chromium alloy coating addresses the toxicity and performance limitations of existing coatings by providing enhanced corrosion and adhesive wear resistance for tubular elements, ensuring long-term protection and safety in harsh conditions.
Patent Information
- Application Number
- JP2024521036
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2021-10-07
- Filing Date
- 2022-10-06
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2042-10-06
AI Technical Summary
Existing coatings for tubular elements used in hydrocarbon wells and energy recovery applications, such as zinc-nickel and zinc-cobalt coatings, pose health risks due to toxic alloying elements and have limitations in corrosion and adhesive wear resistance, while zinc-magnesium and zinc-iron coatings face preparation challenges and lower cathodic protection performance.
A zinc-chromium alloy coating is applied to the threaded ends of tubular elements, with zinc as the predominant element, providing enhanced corrosion resistance and adhesive wear protection without the toxicity of nickel or cobalt, and featuring a chromium content that naturally passivates to form chromium oxide, eliminating the need for additional passivation steps.
The zinc-chromium coating offers improved corrosion resistance, reduced health risks, and superior adhesive wear performance, maintaining effectiveness under harsh environments and multiple screwing/unscrewing cycles, outperforming zinc-nickel coatings in terms of white rust resistance and wear durability.
Smart Images

Figure 2024539601000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a threaded end of a tubular element for drilling and / or working hydrocarbon wells, for oil and gas transportation, for hydrogen transportation or storage, for carbon capture or geothermal energy recovery, the threaded end comprising at least one thread, the surface of which is provided with a zinc and chromium based coating as described below.
[0002] The invention also relates to a process for preparing a threaded end of a tubular element, comprising at least one electrodeposition step onto the surface of the threads of said threaded end of an aqueous composition based on one or more zinc salts, one or more chromium salts, one or more surfactants and one or more electrolytes.
[0003] The invention also relates to a tubular threaded joint comprising at least one threaded end of a tubular element, the surface of the thread being covered with a zinc and chromium based coating as described below. [Background technology]
[0004] It is noted that for the purposes of the present invention, a tubular element means any element or accessory having a substantially tubular shape, optionally joinable to another element of the same type, for the drilling and / or working of hydrocarbon wells, for the transportation of oil and gas, for the transportation and / or storage of hydrogen, for the capture of carbon or for the recovery of geothermal energy.
[0005] Also, for the purposes of the present invention, a threaded end of a tubular element means any end element of a tubular element, as defined above, the surface of which is provided with at least one threaded portion, i.e. a thread, by means of which the tubular element can be joined or connected, optionally to another element of the same type, to form a joint or connection.
[0006] A threaded end of a tubular element in the sense of the present invention therefore corresponds to an end element of the tubular element which is provided with at least one threaded surface, which is involved in the connection of the tubular element with other similar or different elements.
[0007] Each of the tubular elements has at least one externally threaded region, i.e. an end provided with a thread extending on its outer circumferential surface, and / or at least one internally threaded region, i.e. an end provided with a thread extending on its inner circumferential surface, which are intended to be joined by being screwed onto a corresponding end of a similar or different element to form a joint or connection.
[0008] Tubular threaded elements of connections are usually joined under defined constraints, more specifically defined torque targets, in order to meet the tightening and sealing requirements imposed by the conditions of use, and may also have to be screwed in and out multiple times, especially during use.
[0009] The conditions of use of such tubular threaded elements give rise to various types of stresses which can be reduced or minimized by the use of films or greases, especially in the sensitive areas used to connect these elements, such as the threaded areas, abutment areas or metal-to-metal sealing surfaces.
[0010] The stresses induced include, in particular, storage safety stresses, which require the application of a storage grease (as opposed to a threading grease, which is applied before use), but there are also solutions using organic or metallic coatings.
[0011] Screwing and unscrewing operations are generally carried out under high axial loads, e.g. under the weight of pipes of several meters in length, typically 10 to 13 meters, that are joined vertically by the threaded joint, which may be aggravated by slight misalignments of the axes of the threaded elements to be joined. This leads to the risk of adhesive wear occurring in the connection elements of the pipes, especially in the threaded and abutment areas and / or metal-to-metal sealing surfaces. It is therefore important to protect these connection elements, especially the threaded areas, against adhesive wear, especially by covering them with a lubricant.
[0012] Furthermore, tubular threaded elements are often stored and then used in harsh environments, such as "offshore" where salt spray is present, or "onshore" where sand, dust, and / or other contaminants are present, so it is common to apply various types of anti-corrosion coatings to the threaded areas, intimate contact surfaces, metal-to-metal sealing surfaces, and surfaces that are subject to stress during threading, which occur in the abutment areas.
[0013] However, their use may not be a long-term solution with regard to environmental standards, since greases complying with the API RP5A3 (American Petroleum Institute) standard can be extruded from the tubular elements and released into the environment or, for example, into wells, causing blockages that require specific cleaning operations.
[0014] To address the issues of sustained corrosion and adhesive wear resistance, as well as environmental considerations, grease substitutes have been used in the prior art.
[0015] Therefore, zinc (Zn) and nickel (Ni) based metallic coatings have been developed to protect the connecting elements of tubular elements, especially the threaded areas, from corrosion and adhesive wear.
[0016] However, although this metal coating offers excellent performance in terms of corrosion resistance and adhesive wear resistance, it has a major drawback in that it is prepared from nickel salts, which are chemicals that are harmful to the human body and are classified as "CMR" substances, i.e. substances that are known to be carcinogenic, mutagenic, and reproductively toxic.
[0017] Thus, although zinc and nickel based metal coatings are commonly used in industry due to their corrosion and adhesive wear resistance properties, at the same time, their toxicity has always resulted in serious long-term risks to the health of many workers.
[0018] Other zinc-based metallic coatings have also been developed to protect the connecting elements of tubular elements from corrosion and condensation wear.
[0019] However, such envisaged metal coatings have proven to be less than a viable solution for a variety of reasons.
[0020] For example, zinc (Zn) and cobalt (Co) coatings, typically with a cobalt content of about 1% by weight, are toxic because their preparation process is based on the use of cobalt salts classified as "CMR" materials.
[0021] Similarly, zinc (Zn) and cadmium (Cd) coatings have the disadvantage of using cadmium salts, which are substances that are harmful to the human body.
[0022] Tin (Sn) and zinc (Zn) based coatings, especially those with a tin content of 70%-80% by weight and a zinc content of 20%-30% by weight, offer advantageous corrosion resistance but suffer from poor heat resistance, especially to high temperatures, and high manufacturing costs. These disadvantages are particularly related to the high tin content used in the preparation of this type of coating.
[0023] Zinc (Zn) and magnesium (Mg) based coatings are themselves obtained by electrodeposition of zinc and magnesium salts in the presence of solvents at high temperatures, typically around 100° C., a preparation process that is difficult to carry out on an industrial scale.
[0024] Zinc (Zn) and iron (Fe) based coatings, especially those with an iron content above 10% by weight, suffer from the drawback of oxidizing to form a red rust which can be confused with the red oxidation of the substrate iron.
[0025] Generally, zinc (Zn) and magnesium (Mg), zinc (Zn) and iron (Fe), or zinc (Zn) and manganese (Mn) based coatings provide less cathodic protection and therefore less corrosion protection than zinc (Zn) and nickel (Ni) based coatings, because the standard redox potentials of the alloying elements (magnesium, manganese, iron) are lower than that of nickel.
[0026] There is therefore a real need to provide a coating that can effectively protect the threaded ends of tubular elements for the drilling and / or working of hydrocarbon wells, oil and gas transportation, hydrogen transportation or storage, carbon recovery or geothermal energy recovery from corrosion and adhesive wear, while overcoming the above-mentioned drawbacks, i.e. with reduced or minimized toxicity. Summary of the Invention [Problem to be solved by the invention]
[0027] It is therefore an object of the present invention to provide a coating with reduced or no toxicity and which does not adversely affect the corrosion and adhesive wear resistance performance due to the nature of the alloying elements, which can effectively protect the threaded elements of a tubular element used to join the tubular element to another similar or dissimilar tubular element. [Means for solving the problem]
[0028] The invention therefore relates in particular to a threaded end of a tubular element for drilling and / or working hydrocarbon wells, transporting oil and gas, transporting or storing hydrogen, recovering carbon or recovering geothermal energy, which comprises at least one thread extending on its outer or inner circumferential surface, which thread is coated with a layer comprising a zinc-chromium (Zn-Cr) alloy, in which zinc (Zn) is the predominant element in weight percent relative to the total weight of the alloy.
[0029] That is, a coating comprising a zinc-chromium (Zn-Cr) alloy, in which zinc (Zn) is the predominant metallic element in weight percent relative to the total weight of the alloy, covers at least one thread of a threaded end of a tubular element as described above.
[0030] Preferably, the threaded end of the tubular element as described above comprises at least one thread extending on its outer or inner circumferential surface and at least one non-threaded portion, preferably including a stop and / or a sealing seat. The thread and the non-threaded portion are covered with a coating comprising a zinc-chromium (Zn-Cr) alloy, where zinc (Zn) is the predominant metallic element in weight percent relative to the total weight of the alloy.
[0031] That is, the zinc-chromium (Zn-Cr) coating according to the present invention covers at least one thread of the threaded end of a tubular element as described above, and preferably covers at least the thread of the threaded end of the tubular element and at least one non-threaded portion, preferably including a stop and / or a sealing seat.
[0032] In the sense of the present invention, in the remainder of the text, a layer comprising a zinc-chromium (Zn-Cr) alloy corresponds both to a coating comprising a zinc-chromium (Zn-Cr) alloy and to a zinc-chromium (Zn-Cr) coating. Thus, in this specification, the terms "layer" and "coating" may be used interchangeably to denote a zinc-chromium alloy deposit according to the invention, covering at least the thread of the threaded end of the tubular element.
[0033] According to the invention, the layer containing a zinc-chromium (Zn-Cr) alloy is different from a superposition of a zinc (Zn) layer and a chromium (Cr) layer.
[0034] It is noted that for the purposes of this invention, "zinc-chromium (Zn-Cr)" alloy refers to a mixture containing zinc and chromium, where zinc represents the base metal, i.e., the metallic element predominantly present in the mixture, and chromium represents the alloying metallic element, i.e., the metallic element intentionally present in or added to the mixture.
[0035] In other words, the chromium in zinc-chromium (Zn-Cr) alloys is not an impurity or an unnecessary metallic element in the alloy.
[0036] That is, chromium represents the predominant alloying metal element, by weight percent, of all alloying metal elements believed to be present in the mixture.
[0037] The zinc-chromium (Zn-Cr) coating according to the invention has the advantage that the chromium salts used in the preparation process are not classified as "CMR" substances, therefore they are non-toxic and workers are less exposed to serious health risks.
[0038] The chromium present in zinc-chromium (Zn-Cr) alloys corresponds to or is trivalent chromium Cr(III).
[0039] Furthermore, the zinc-chromium (Zn-Cr) coating according to the invention can ensure effective protection against corrosion and adhesive wear of the threaded ends of tubular elements, including in very harsh environments such as marine environments, industrial environments, environments receiving high precipitation and / or environments experiencing large temperature changes.
[0040] Thus, the zinc-chromium (Zn-Cr) coatings used in accordance with the present invention effectively provide cathodic protection for the substrate, imparting a good level of corrosion resistance.
[0041] In particular, the chromium contained in the zinc-chromium metal coating according to the invention is naturally passivated to form chromium oxide, which ensures effective protection against corrosion. The natural formation of chromium oxide therefore makes it possible to omit the implementation of an additional passivation step aimed at enhancing the corrosion protection performance of the substrate, which offers time savings from an industrial point of view.
[0042] In addition, the zinc-chromium (Zn-Cr) coating has excellent lubricating properties and can ensure effective protection against adhesive wear of the threaded ends during the continuous operations of screwing and unscrewing tubular elements.
[0043] The zinc-chromium (Zn-Cr) coating used according to the invention also has the advantage that it is less susceptible to wear during continuous screwing operations, thus ensuring corrosion and adhesive wear resistance even after several screwing / unscrewing cycles without the need for additional corrosion and adhesive wear protection.
[0044] This means that the zinc-chromium (Zn-Cr) coating according to the invention can provide protection against corrosion and adhesive wear over the long term, including multiple screwing and unscrewing operations of the tubular elements in harsh environments.
[0045] In particular, the abrasion resistance may be determined by an indentation test, such as a scratch test, which is carried out by applying a load, in particular a ball, with increasing pressure on the surface of the coating until delamination of the coating, i.e. adhesive failure of the coating, occurs. In particular, the critical load at which adhesive failure occurs is measured.
[0046] The threaded end according to the invention therefore exhibits increased resistance to corrosion and adhesive wear, even in the harsh environments mentioned above, including after several screwing-in and screwing-out cycles of the tubular element provided with said end.
[0047] Furthermore, the zinc-chromium (Zn-Cr) coating according to the present invention performs at least as well as zinc-nickel (Zn-Ni) coatings against the appearance of red rust.
[0048] Also, the zinc-chromium (Zn-Cr) coating of the present invention has better performance against the appearance of white rust than zinc-nickel (Zn-Ni) coatings.
[0049] In particular, salt spray tests carried out without passivation of the coating revealed that the zinc-nickel (Zn-Ni) coating showed early appearance of white rust, whereas the zinc-chromium (Zn-Cr) coating according to the invention showed delayed appearance of white rust, even when the coating thickness was reduced by half.
[0050] In the sense of the present invention, the expression "zinc (Zn) is the predominant element in % by weight relative to the total weight of the alloy" means that zinc has the highest content in % by weight among the elements of the alloy.
[0051] According to one embodiment, the threads are coated with a layer comprising a binary zinc-chromium (Zn-Cr) alloy, where zinc (Zn) is the predominant element in weight percent relative to the total weight of the alloy.
[0052] According to the present invention, the term "content" corresponds to the weight concentration of the metallic element in question relative to the concentrations of all elements present in the alloy.
[0053] In other words, the "content" is the weight concentration of the target metal element relative to the total concentration of the mixture.
[0054] According to one embodiment, the zinc (Zn) content is greater than 50% by weight, preferably equal to or greater than 60% by weight, more preferably equal to or greater than 65% by weight, relative to the total weight of the zinc-chromium alloy.
[0055] Preferably, the zinc (Zn) content is 70% by weight to 80% by weight, more preferably 70% by weight to 75% by weight, based on the total weight of the zinc-chromium alloy.
[0056] According to a preferred embodiment of the present invention, the chromium (Cr) content is equal to or greater than 3 wt. %, preferably equal to or greater than 20 wt. %, based on the total weight of the zinc-chromium alloy.
[0057] Preferably, chromium is the only alloying metal element present in the zinc-chromium (Zn-Cr) alloy.
[0058] Preferably, the zinc-chromium (Zn-Cr) alloy is a mixture comprising zinc as the predominant metallic element, by weight % based on the total weight of the alloy, and chromium as an alloying metallic element, preferably chromium as the only alloying metallic element, and optionally one or more metallic or non-metallic impurities.
[0059] It should be noted that for purposes of this invention, "alloying metal element" means an alloying element that is intentionally present in or added to the alloy.
[0060] That is, the alloying metal elements are not impurities.
[0061] That is, the chromium present in the alloy according to the present invention is not an impurity.
[0062] In particular, the zinc-chromium (Zn-Cr) coating according to the invention, which has a chromium content of 3% by weight or more, contains at least one crystalline phase of the Cr-Zn-17 type and exhibits significantly improved corrosion resistance compared to coatings consisting only of zinc.
[0063] According to one embodiment of the present invention, the chromium (Cr) content is 20% by weight to 30% by weight based on the total weight of the zinc-chromium alloy.
[0064] The zinc-chromium (Zn-Cr) coating according to the invention, which has a chromium content of 20% to 30% by weight based on the total weight of the Zn-Cr alloy, has excellent corrosion resistance properties, comparable to or even better than zinc-based coatings, in particular zinc- and nickel-based coatings, whilst having the advantage of being particularly adherent and consistently homogeneous on the surface.
[0065] The quality of the coating according to the invention is therefore significantly improved, especially in terms of adhesion, cohesion and wear resistance, in a case where the chromium content is between 20% and 30% by weight relative to the total weight of the alloy, compared to zinc- and chromium-based coatings with a chromium content strictly less than 20% by weight (<20% by weight) or strictly more than 30% by weight (>30% by weight).
[0066] In particular, zinc-chromium (Zn-Cr) coatings with a chromium content of 20% to 30% by weight contain at least one crystalline phase of the gamma type, which confers corrosion resistance properties five times higher than those of coatings consisting only of zinc (i.e. coatings with a zinc content of 100% by weight relative to the total weight of the coating).
[0067] The advantage of this crystalline phase lies in the fact that it is cubic in centre and therefore shares an element of symmetry with the austenitic crystal lattice of some steels used as substrates, which promotes epitaxial growth and improves adhesion of the coating to the substrate.
[0068] Thus, a zinc-chromium coating according to the invention having a chromium content between 20% and 30% by weight exhibits better adhesion to the substrate than zinc- and chromium-based coatings having a chromium content strictly less than 20% by weight (<20% by weight) or strictly more than 30% by weight (>30% by weight).
[0069] In other words, the zinc-chromium (Zn-Cr) coating according to the present invention, which has a chromium content of 20% to 30% by weight, has a better structure and improved strength.
[0070] Furthermore, zinc-chromium (Zn-Cr) coatings, which have a chromium content of 20% to 30% by weight relative to the total weight of the alloy, have corrosion resistance properties 14 times better than zinc-nickel (Zn-Ni) coatings against white rust.
[0071] According to one embodiment of the present invention, the chromium (Cr) content is 25% by weight to 30% by weight based on the total weight of the zinc-chromium alloy.
[0072] The zinc-chromium (Zn-Cr) coating according to the invention, which has a chromium content of 25% to 30% by weight based on the total weight of the zinc-chromium alloy, withstands loads at least as well as zinc- and nickel-based coatings and at the same time has excellent corrosion resistance properties, especially in aggressive environments.
[0073] The zinc-chromium coating according to the invention, which has a chromium content of 25% to 30% by weight based on the total weight of the zinc-chromium alloy, has better long-term wear resistance than zinc- and nickel-based coatings and at the same time has excellent corrosion resistance properties.
[0074] Advantageously, the chromium (Cr) content is 27% by weight relative to the total weight of the zinc-chromium alloy.
[0075] According to a preferred embodiment of the present invention, the zinc (Zn) content is 70% to 80% by weight, and the chromium (Cr) content is 20% to 30% by weight, based on the total weight of the zinc-chromium alloy.
[0076] According to a preferred embodiment of the invention, the layer comprising a zinc-chromium alloy as described above is a layer made of a binary zinc-chromium alloy.
[0077] According to a preferred embodiment of the invention, the threads are coated with a layer consisting of a binary zinc-chromium (Zn-Cr) alloy, in which zinc (Zn) is the predominant element in % by weight relative to the total weight of the alloy and the chromium (Cr) content is between 20% and 30% by weight relative to the total weight of the alloy.
[0078] According to a preferred embodiment of the invention, a layer comprising a zinc-chromium (Zn-Cr) alloy is electrodeposited.
[0079] Advantageously, zinc and chromium can be deposited on the substrate by electroplating at very high current densities, in particular at deposition rates of the order of 7 μm per minute, which is three times higher than the deposition rate of layers made from zinc-nickel alloys.
[0080] According to one embodiment, the layer comprising a zinc-chromium (Zn-Cr) alloy has a thickness between 4 μm and 20 μm. Such a thickness allows the zinc-chromium layer to be applied more optimally at least to the thread of the threaded end of the tubular element. That is to say, the deposition of the zinc-chromium (Zn-Cr) layer according to the invention is better distributed in the thread and provides improved protection against corrosive and adhesive wear in the case of a thickness in the range of 4 μm to 20 μm. Such a thickness allows an optimal adaptation to the shape of the thread of the end of the tubular element.
[0081] Advantageously, from 4 μm the corrosion protection performance is fully achieved, and up to 20 μm the layer remains dense without allowing brittleness, beyond which the layer may become too thick for the machining clearances of the connections.
[0082] Advantageously, the layer comprising a zinc-chromium (Zn-Cr) alloy has a chromium content between 20% and 30% by weight, preferably between 25% and 30% by weight, relative to the total weight of the zinc-chromium alloy, and a thickness between 4 μm and 20 μm, preferably between 10 μm and 20 μm.
[0083] Zinc-chromium (Zn-Cr) coatings with a chromium content of 20% to 30% by weight, preferably 25% to 30% by weight, relative to the layer weight of the alloy and a thickness of 4 µm to 20 µm, preferably 10 µm to 20 µm, have the advantage of being optimally distributed on the thread and having particularly good adhesion, being consistently homogeneous and wear-resistant whilst having good corrosion properties.
[0084] Advantageously, the layer comprising a zinc-chromium (Zn-Cr) alloy is not coated with a passivation layer comprising trivalent chromium (Cr(III)).
[0085] In particular, the chromium contained in the coating naturally forms chromium oxide, eliminating the need for an additional passivation step to provide enhanced corrosion protection.
[0086] Advantageously, therefore, zinc-chromium coatings are not covered with a passivation layer containing trivalent chromium (Cr(III)).
[0087] Preferably, the threaded end of the tubular element further comprises at least one non-threaded portion coated with a layer comprising a zinc-chromium (Zn-Cr) alloy according to the invention.
[0088] Preferably, the non-threaded portion comprises a stop.
[0089] Preferably, the non-threaded portion comprises a sealing seat.
[0090] According to a preferred embodiment of the invention, the non-threaded part coated with a layer comprising a zinc-chromium (Zn-Cr) alloy according to the invention is provided with a stop and / or a sealing seat.
[0091] Preferably, the threaded end of the tubular element is made of steel.
[0092] Preferably, the steel threaded end of the tubular element as described above comprises at least one thread extending on its outer or inner circumferential surface, the thread being coated with at least one layer comprising a zinc-chromium (Zn-Cr) alloy, the zinc-chromium (Zn-Cr) alloy having a chromium content of 20% to 30% by weight, preferably 25% to 30% by weight, relative to the total weight of the zinc-chromium (Zn-Cr) alloy.
[0093] Preferably, the steel threaded end of the tubular element as described above comprises at least one thread extending on its outer or inner peripheral surface, the thread being coated with at least one layer comprising a zinc-chromium (Zn-Cr) alloy, the zinc-chromium (Zn-Cr) alloy having a chromium content of 20% to 30% by weight, preferably 25% to 30% by weight, relative to the total weight of the zinc-chromium alloy, and a thickness of 4 μm to 20 μm.
[0094] According to one embodiment, the surface of the thread as described above, and optionally the surface of the non-threaded parts, coated with a zinc-chromium (Zn-Cr) coating according to the invention may have a surface roughness, in particular a surface roughness (Ra) of 1.6 μm to 3.2 μm.
[0095] According to one embodiment, the surfaces of the threads and the surfaces of the non-threaded parts, preferably provided with stop portions and / or sealing seats, coated with a zinc-chromium (Zn-Cr) coating according to the invention may have a surface roughness, in particular a surface roughness (Ra) of 1.6 μm to 3.2 μm.
[0096] The surface roughness can be achieved by sandblasting.
[0097] That is, the surface of the thread, and possibly the surface of the non-threaded portion, may be pre-treated with a mechanical treatment, preferably sandblasting.
[0098] Surface roughening can improve the adhesion and wear resistance of zinc-chromium (Zn-Cr) coatings.
[0099] According to a preferred embodiment of the invention, the surface of the thread, preferably including the stop and / or sealing seat, and optionally the non-threaded parts, are pretreated by sandblasting and provided with a zinc-chromium (Zn-Cr) coating with a chromium content of 20% to 30% by weight and preferably with a thickness of 4 μm to 20 μm.
[0100] The invention also relates to the use of a layer comprising a zinc-chromium (Zn-Cr) alloy as described above for protecting at least one threaded end of a tubular element as described above against corrosion and adhesive wear.
[0101] The invention also relates to a process for preparing a threaded end, as described above, of a tubular element for drilling and / or working hydrocarbon wells, for oil and gas transportation, for hydrogen transportation or storage, for carbon recovery or for geothermal energy recovery, comprising at least one electrodeposition step, on at least the surface of the thread of the end, of an aqueous composition comprising one or more zinc salts, one or more chromium salts, one or more electrolytes and one or more surfactants, preferably non-ionic surfactants.
[0102] The process according to the invention makes it possible to deposit a layer comprising at least one zinc-chromium (Zn-Cr) alloy as described above, which is homogeneous, compact and can be evenly distributed over the threads of the threaded end.
[0103] According to one embodiment, the process according to the invention may include a step of preparation of the surface to be coated by mechanical treatment, more preferably by sandblasting.
[0104] Preparation of the surface to be coated by mechanical treatment, preferably sandblasting, can improve the adhesion of the zinc-chromium (Zn-Cr) coating and minimize the risk of the coating becoming embrittled.
[0105] According to one embodiment, the process according to the invention may comprise a step of preparation of the surface of the thread and of the non-threaded part, preferably with the stop and / or sealing seat, by mechanical treatment, preferably sandblasting.
[0106] According to one embodiment, the process according to the invention may comprise a step of sandblasting the surface of the threaded end to be coated, preferably the surface of the thread including the stop and / or sealing seat and the surface of the non-threaded part.
[0107] According to one embodiment, the process according to the invention comprises the steps of sandblasting the surface to be coated and electrochemically depositing the aqueous composition as described above on at least the sandblasted surface of the thread, preferably on the sandblasted surface of the thread and preferably on the sandblasted surface of the non-threaded part comprising the stop and / or sealing seat.
[0108] Furthermore, the resulting zinc-chromium coating has a surface with a homogenous aesthetic appearance.
[0109] According to a preferred embodiment of the invention, the deposition rate of the aqueous composition on the surface to be coated is between 4 μm and 20 μm per minute, preferably between 5 μm and 7 μm per minute.
[0110] The zinc and chromium salts are soluble in aqueous compositions.
[0111] According to the invention, the chromium (Cr) salt is a trivalent chromium Cr(III) salt.
[0112] Preferably, the electrodeposition is at least 30 amps / dm 2 This is done at a current density of .
[0113] In particular, a sufficient stirring speed of the aqueous composition, for example a speed of 0.23 m / s at the cathode, allows advantageously to increase the current density without the risk of causing seizing, which would likely result in a deterioration of the appearance of the zinc-chromium (Zn-Cr) coating according to the invention.
[0114] More preferably, the electrodeposition is at 30 amps / dm 2 ~50 amps / dm 2The current density is
[0115] 30 amps / dm 2 Below this, chromium incorporation is reduced or inhibited and the resulting coating has dark grey specks representing areas that do not contain chromium.
[0116] According to one embodiment, the weight ratio of the chromium salt to the zinc salt is between 0.8 and 1.4.
[0117] Preferably, the surfactant is selected from the group consisting of non-ionic surfactants.
[0118] Preferably, the nonionic surfactant is a (poly)alkoxylated fatty alcohol, in particular a (poly)alkoxylated C-C 40 It is selected from the group consisting of fatty alcohols, in particular poly(ethylene glycol) octyl ether, and oxirane, 2-methyl-, oxirane and polymer, mono(2-naphthonyl) ether.
[0119] The presence of a surfactant in the aqueous composition allows for the deposition of chromium along with the zinc.
[0120] In fact, it has been found that without the use of surfactants, the deposit obtained is free of chromium, in particular because the pH of the cathode increases due to the release of dihydrogen, which results in the formation of zinc hydroxides, which inhibit the diffusion of chromium to the cathode. This absence of chromium deposition can be explained by the presence of a shift in the reduction potential (chromium becomes lower than the zinc reduction potential and / or the water reduction potential).
[0121] Thus, the presence of at least one surfactant can facilitate the diffusion of chromium in the diffusion layer and / or reduce the cathodic overpotential of chromium and / or increase the cathodic overpotential of the electrolysis of water, thereby minimizing the release of dihydrogen and the production of zinc hydroxide.
[0122] Preferably, the concentration of the surfactant is 0.3 mmol / l to 3 mmol / l.
[0123] The brightness of the zinc-chromium (Zn-Cr) coating according to the invention can be adjusted by the concentration of the surfactant.
[0124] Preferably, the brightness of the zinc-chromium (Zn-Cr) coating according to the present invention can be increased by increasing the concentration of the surfactant.
[0125] Preferably, the zinc salt may be selected from zinc sulfate, zinc chloride, and zinc sulfamate. Preferably, the zinc salt is zinc sulfate.
[0126] Preferably, the chromium salt may be selected based on the properties of the zinc salt: if zinc sulfate is preferred, then chromium sulfate is preferentially selected.
[0127] The conductive salt / carrier salt may be selected from the group consisting of sodium sulfate, potassium sulfate, and ammonium sulfate, and mixtures thereof, and is preferably sodium sulfate. The conductive salt / carrier salt can ensure electrical conductivity during the process.
[0128] Preferably, the aqueous composition further comprises one or more amino acids, preferably glycine.
[0129] Glycine can provide a gloss, semi-gloss or matt finish to the zinc-chromium (Zn-Cr) coating of the present invention.
[0130] The content of glycine in the aqueous composition may be from 50 g / l to 75 g / l relative to the total concentration of the composition.
[0131] The glycine content makes it possible to adjust the matt appearance of the zinc-chromium (Zn-Cr) coating according to the invention.
[0132] Preferably, increasing the glycine content and decreasing the surfactant content results in a zinc-chromium (Zn-Cr) coating with a matte appearance.
[0133] Preferably, the glycine content is decreased and the surfactant content is increased, resulting in a lustrous appearance of the zinc-chromium (Zn-Cr) coating.
[0134] When the Zn-Cr coating is shiny on a non-sandblasted surface or semi-glossy on a sandblasted surface, the mechanical properties of the Zn-Cr coating are superior to those of the Zr-Cr coating with a matte appearance.
[0135] The pH of the aqueous composition may be from 1.5 to 3.5, preferably from 2 to 2.5.
[0136] Indeed, if the pH of the aqueous composition is particularly above 3.5, there is an increased risk of precipitation of chromium salts in the bath, which can be minimized at a pH between 1.5 and 3.5.
[0137] The process according to the invention is carried out at a temperature between 35° C. and 45° C. Below 35° C. the effectiveness of the composition may be insufficient, and above 45° C. the chemical components may deteriorate.
[0138] Preferably, the aqueous composition comprises: one or more zinc salts, one or more chromium salts, one or more conductive / carrier salts, preferably sodium sulfate; one or more surfactants, preferably non-ionic surfactants, and Optionally, one or more amino acids, preferably glycine Includes.
[0139] Advantageously, the process according to the invention does not include the additional step of forming a passivating anti-corrosion layer containing trivalent chromium (Cr(III)).
[0140] That is to say, advantageously, the process according to the invention does not include a step of forming a passivating corrosion-resistant conversion layer comprising trivalent chromium (Cr(III)) after deposition of the layer comprising a zinc-chromium alloy.
[0141] Another subject of the invention relates to a tubular element for drilling and / or working hydrocarbon wells, for transporting oil and gas, for transporting or storing hydrogen, for carbon recovery or for geothermal energy recovery, which is provided with a threaded end according to the invention comprising at least one thread extending on its outer or inner circumferential surface, the thread being covered with a layer comprising a zinc-chromium (Zn-Cr) alloy according to the invention, where zinc (Zn) is the predominant element in % by weight relative to the total weight of the alloy.
[0142] The threaded ends are as described above.
[0143] The layer containing the zinc-chromium (Zn-Cr) alloy is as described above.
[0144] The tubular elements have improved corrosion resistance and adhesive wear resistance.
[0145] Preferably, the tubular element is male and has at least one thread extending on its outer circumferential surface.
[0146] More preferably, the tubular element is male and has at least one thread extending on its outer circumferential surface and at least one non-threaded portion, preferably selected from a stop and / or a sealing seat.
[0147] Preferably, the tubular element is female and has at least one thread extending on its inner circumferential surface.
[0148] More preferably, the tubular element is female and has at least one thread extending on its inner circumferential surface and at least one non-threaded portion, preferably selected from a stop and / or a sealing seat.
[0149] According to the invention, the tubular element is provided with an axis of rotation.
[0150] The tubular element according to the invention is in particular made of steel, in particular a steel as described in the API 5CT standard, for example a steel containing a proportion of less than 0.25% carbon, and / or preferably a steel having a grade defined according to the ISO 11960 and ISO 13680 standards, and / or a H40, J55, K55, M65, L80, C90, C95, T95, P110 or Q125 carbon steel, or a martensitic 13Cr or S13Cr steel, or a duplex 22Cr+25Cr steel, or a super duplex 25Cr steel, or an austenitic Fe27Cr steel.
[0151] The invention also relates to the use of a tubular element as described above for drilling and / or working hydrocarbon wells, for transporting oil and gas, for transporting or storing hydrogen, for carbon capture or for geothermal energy recovery.
[0152] Preferably, the invention relates to the use of a tubular element as described above for drilling and / or working a hydrocarbon well.
[0153] The invention also relates to a tubular threaded joint for drilling and / or working hydrocarbon wells, transporting oil and gas, transporting or storing hydrogen, recovering carbon or recovering geothermal energy. The tubular threaded joint comprises a threaded end of a male tubular element having at least one thread extending on its outer circumferential surface and a threaded end of a female tubular element having at least one thread extending on its inner circumferential surface, which are screwed together. At least one threaded end is as described above. In particular, the thread is covered with a layer comprising a zinc-chromium (Zn-Cr) alloy as described above.
[0154] In particular, tubular threaded joints according to the invention are particularly resistant to corrosion and adhesive wear, especially in harsh environments such as those mentioned above.
[0155] Preferably, the two threaded ends are as described above.
[0156] According to one aspect of the invention, the threaded end of the male tubular element has at least one thread extending on its outer circumferential surface, which is covered with a layer comprising a zinc-chromium (Zn-Cr) alloy according to the invention as described above.
[0157] According to one aspect of the invention, the threaded end of the female tubular element has at least one thread extending on its inner circumferential surface, which is coated with a layer comprising a zinc-chromium (Zn-Cr) alloy according to the invention as described above. According to yet another aspect of the invention, the threaded end of the male tubular element has at least one thread extending on its outer circumferential surface which is covered with a layer comprising a zinc-chromium (Zn-Cr) alloy according to the invention, and the threaded end of the female tubular element has at least one thread extending on its inner circumferential surface which is covered with a layer comprising a zinc-chromium (Zn-Cr) alloy according to the invention.
[0158] Preferably, the tubular threaded joint comprises a threaded end of a male tubular element having at least one non-threaded portion with at least one thread and metallic interference extending on its outer circumferential surface, and a threaded end of a female tubular element having at least one non-threaded portion selected from a stop and / or a sealing seat with at least one thread and metallic interference extending on its inner circumferential surface, the threads and the non-threaded portion being covered with a layer comprising a zinc-chromium (Zn-Cr) alloy according to the invention as described above.
[0159] In the context of this specification, terms expressing ranges are intended to include the values in the stated range, unless otherwise indicated.
[0160] Additionally, as used herein, the phrase "at least one" is equivalent to "one or more." [Brief description of the drawings]
[0161] The features of the present invention will now be described in detail with reference to the accompanying drawings. [Figure 1] FIG. 2 is a schematic diagram of a joint resulting from threaded joining of two tubular elements. [Diagram 2] FIG. 2 is an enlarged view of the boxed area A in FIG. [Diagram 3] FIG. 13 shows in detail the cooperation of the threads of two assembled tubular elements. [Figure 4] FIG. 2 shows in detail a connecting element (thread) according to the invention, which is covered with a zinc-chromium coating according to the invention. [Diagram 5] FIG. 2 is a comparison of the time to appearance of a white rust layer of strength 2 and strength 3 on the surface of a zinc-nickel (Zn-Ni) coating and on the surface of a zinc-chromium (Zn-Cr) coating according to the invention after exposure to a salt spray test. [Figure 6] FIG. 1 compares the time it takes for a zinc-nickel (Zn-Ni) coating surface and a zinc-chromium (Zn-Cr) coating according to the invention to be completely covered with a layer of white rust of strength 2 after exposure to a salt spray test. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0162] The threaded joint shown in FIG. 1 comprises a first tubular element with a rotation axis 9 and a male end 1, and a second tubular element with a rotation axis 9 and a female end 2. Each of the two ends 1 and 2 terminates in an end face oriented radially relative to the axis 9 of the threaded joint and has a threaded portion 3 and 4, respectively, which cooperate with each other for mutual assembly by screwing the two elements together. The threaded portions 3 and 4 may be of trapezoidal type or of another type of thread. In the embodiment shown in the figure, the threaded portions have tapered threads at each end of the threaded portion. These tapered shapes extend over a portion of the axial extent of the threaded portion. In particular, the part 10 of the threaded portion having a tapered shape does not cooperate with a complementary thread.
[0163] Additionally, metal-to-metal sealing surfaces (seats) 5, 6 intended to form a liquid-tight seal with one another after the two threaded elements are screwed together and assembled are formed on the male and female ends, respectively, near the threaded portions 3, 4. Finally, the male end 1 terminates in an end face 7 that abuts a corresponding surface 8 formed on the female end 2 when the two ends are screwed together. The surfaces 7 and 8 are called stops.
[0164] In Figure 3 the threads of the threaded portion are shown in detail. Each of the threads comprises a load flank 11 which makes an angle 12 in the range of -5° to +5° with respect to the normal N of the connection axis 10. The load flanks are connected via apexes 13 to assembly flanks 14. In particular, as shown in the figure, the load flanks of the male threaded portion 3 are connected in contact with the corresponding load flanks of the female threaded portion 4 in the final position of assembly.
[0165] Figure 4 shows the male end 1 of a tubular element, where the threaded portion 3 and the sealing surface 5 (seat) are covered with a coating 15 according to the invention, i.e. a zinc-chromium coating comprising a zinc-chromium (Zn-Cr) alloy in which zinc (Zn) is the predominant element in weight percent relative to the total weight of the alloy.
[0166] Preferably, coating 15 has a chromium content of 20% to 30% by weight, more preferably 25% to 30% by weight, and a zinc content of 70% to 80% by weight, more preferably 70% to 75% by weight, based on the total weight of the alloy.
[0167] Exemplary embodiments Threads made of L80 grade carbon steel were electroplated with a semi-bright metallic coating comprising a zinc-chromium (Zn-Cr) alloy with a chromium content of 27 wt.% based on the total weight of the alloy, as described above.
[0168] A semi-bright zinc-chrome coating was obtained from an aqueous composition containing 75 g / l glycine.
[0169] Zinc-chromium coatings were compared with zinc-nickel (Zn-Ni) coatings, where zinc was the predominant element by weight percent, and the nickel content ranged from 10% to 18% by weight. The weight percent was calculated with respect to the total weight of the alloy.
[0170] Tribological tests (scratch and Bowden tests) were performed on the coatings to determine the critical load at which delamination (plastic deformation) of the coating was observed, the initial coefficient of friction, and the number of cycles the coating could withstand.
[0171] Salt spray tests were also conducted on the coatings to determine the corrosion resistance performance of the coatings.
[0172] [Scratch test] The experimental conditions were as follows: a tungsten carbide ball was used, and the coating was applied with increasing loads ranging from 10N to 260N, with a ball movement speed of 4.20mm / s, movement time of 2.38 seconds, ball size of 5mm, and track length of 10mm.
[0173] The results of the scratch test are shown in Table 1.
[0174] [result] [Table 1]
[0175] The scratch test results, shown in Table 1, indicate that the semi-bright zinc-chromium coating withstood loads at least as great as those withstood by zinc-nickel coatings with nickel contents ranging from 10% to 18% by weight relative to the total alloy weight.
[0176] [Bowden test] To evaluate the lubrication properties (friction coefficient) of the coating surface, a commercially available Bowden friction tester (Shinko Engineering Co., Ltd.) was used. The Bowden friction tester applies a load to a tungsten carbide ball as it moves back and forth linearly over the coating formed on a steel plate.
[0177] The coefficient of friction was measured based on the friction force and pressure load.
[0178] [procedure] A tungsten carbide ball was applied to the coating and moved with a pressing load of 30N and 100N, a ball movement speed of 4.20mm / s, a duration of 2.38s, a ball size of 5mm, and a track length of 10mm.
[0179] To evaluate the lubricating properties of the coatings, the initial coefficient of friction was determined.
[0180] To evaluate the abrasion resistance of each coating, the number of cycles (the number of times the ball passes over the surface) was measured for each coating.
[0181] The results are shown in Tables 2 and 3.
[0182] [Bowden test results with a load of 30N] [Table 2]
[0183] The Bowden test results shown in Table 2 show that for a load of 30 N, the zinc-chromium coating according to the present invention has a lower initial coefficient of friction than the zinc-nickel coating.
[0184] Furthermore, the zinc-chromium coating showed the same level of durability as the zinc-nickel coating at a load of 30N.
[0185] [Bowden test results with a load of 100N] [Table 3]
[0186] The results of the Bowden test carried out at a load of 100 N, shown in Table 3, show that the zinc-chromium coating according to the invention is more durable than the zinc-nickel coating.
[0187] As a result, the zinc-chromium coating according to the present invention had better wear resistance than the zinc-nickel coating with a nickel content of 10% to 18% by weight.
[0188] That is, as the load increased, the zinc-chromium (Zn-Cr) coating according to the present invention showed improved durability, i.e., higher wear resistance, compared to the zinc-nickel (Zn-Ni) coating.
[0189] [Salt spray test] For the corrosivity tests, neutral salt spray tests were carried out in a climatic chamber under the following conditions: 35°C, 50 g / l salt solution with density 1.029–1.036 at 25°C and pH 6.5–7.2 at 25°C, collected at an average rate of 1.5 ml / h.
[0190] This test evaluated the appearance of red rust and white rust.
[0191] [Corrosion resistance: Appearance of red rust] The appearance of red rust was evaluated by determining the degree of rust, Re, corresponding to the ratio of the rusted surface area to the total surface area, in ascending order.
[0192] In this case, an intact sample without red rust must meet class Re0 of the ISO 9227 standard.
[0193] The results are shown in Table 4.
[0194] [Table 4]
[0195] The degree of rust after the test is in ascending order from Re0 to Re2, which corresponds to the rusted surface area relative to the total surface area.
[0196] According to the degree of rust, Re0 = 0% rust on the total surface area; Re1 = 0.05% of the total surface area rust, Re2 = 0.5% of the total surface area rust, Re6 = 40%-50% of the total surface area rusted It became.
[0197] Table 4 shows that zinc-chromium (Zn-Cr) coatings are able to inhibit the appearance of red rust at least as well as zinc-nickel coatings.
[0198] [Corrosion resistance: Appearance of white rust] The presence of white rust corresponds to oxidation of the coating, particularly oxidation of the zinc, and was assessed by measuring the time it takes to appear and to completely cover the surface of the coating after exposure to salt spray.
[0199] After exposure to salt spray, the strength of the white rust layer over the coating was classified in ascending order as follows: · White rust intensity 1: corresponds to a thin, light layer of white rust, also known as bloom. White rust of strength 2: corresponds to a layer of white rust in the form of crystals. · White rust intensity 3: corresponds to a very dense layer of white rust.
[0200] [White rust appearance time] Figure 5 compares the time to appearance of white rust layers of strength 2 and strength 3 on the surface of a zinc-nickel coating [Zn-Ni, nickel content 14 wt%, thickness 10 μm] and a zinc-chromium coating [Zn-Cr, chromium content 27 wt%, thickness 5 μm] after exposure to a salt spray test.
[0201] Figure 5 shows that on the surface of the zinc-nickel coating [Zn-Ni, nickel content 14 wt%, thickness 10 μm], a layer of white rust with strength 2 appeared rapidly after 24 hours, whereas on the surface of the zinc-chromium coating [Zn-Cr, chromium content 27 wt%, thickness 5 μm], a layer of white rust with strength 2 appeared only after 170 hours.
[0202] Figure 5 also shows that on the zinc-nickel coating [Zn-Ni, nickel content 14 wt%, thickness 10 μm], a layer of white rust with strength 3 appeared rapidly after 24 hours, whereas on the zinc-chromium coating [Zn-Cr, chromium content 27 wt%, thickness 5 μm], a layer of white rust with strength 3 appeared only after 336 hours.
[0203] [Time until the coating surface is completely covered with white rust] Figure 6 shows the results of a comparison of the time it takes for a zinc-nickel coating [Zn-Ni, nickel content 14 wt%, thickness 10 μm] and a zinc-chromium coating [Zn-Cr, chromium content 27 wt%, thickness 5 μm] to be completely covered by a layer of white rust with strength 2.
[0204] Figure 6 shows that it took 24 hours for a layer of white rust of strength 2 to completely cover the surface of a zinc-nickel coating [Zn-Ni, nickel content 14 wt%, thickness 10 μm], whereas it took 336 hours for the same layer to completely cover the surface of a zinc-chromium coating [Zn-Cr, chromium content 27 wt%, thickness 5 μm].
[0205] [Conclusion] As described above, it has been shown that the zinc-chromium (Zn-Cr) coating according to the present invention has superior performance in terms of the appearance of white rust compared to the zinc-nickel (Zn-Ni) coating.
[0206] As a result, the adhesion of the layer deposited after the zinc-chromium coating was improved.
Claims
1. Threaded end (1, 2) of a tubular element for drilling and / or working hydrocarbon wells, transporting oil and gas, transporting or storing hydrogen, recovering carbon or recovering geothermal energy, comprising at least one thread (3, 4) extending on its outer or inner circumferential surface, characterized in that said thread (3, 4) is coated with a layer (15) comprising a zinc-chromium (Zn-Cr) alloy, in which zinc (Zn) is the predominant element in weight percent relative to the total weight of said zinc-chromium alloy.
2. 2. The threaded end portion (1, 2) of a tubular element according to claim 1, characterized in that the zinc (Zn) content is more than 50% by weight, preferably 60% by weight or more, more preferably 65% by weight or more, based on the total weight of the zinc-chromium alloy.
3. 3. The threaded end portion (1, 2) of a tubular element according to claim 1 or 2, characterized in that the chromium (Cr) content is greater than or equal to 3% by weight, preferably greater than or equal to 20% by weight, relative to the total weight of the zinc-chromium alloy.
4. 4. The threaded end portion (1, 2) of a tubular element according to claim 1, characterized in that the chromium (Cr) content is between 20% and 30% by weight, preferably between 25% and 30% by weight, relative to the total weight of the zinc-chromium alloy.
5. Threaded end portion (1, 2) of a tubular element according to any one of claims 1 to 4, characterized in that said layer (15) is electrochemically deposited.
6. Threaded end portion (1, 2) of a tubular element according to any one of claims 1 to 5, characterized in that the thickness of said layer (15) is between 4 μm and 20 μm, preferably between 10 μm and 20 μm.
7. The threaded end (1, 2) of a tubular element according to any one of claims 1 to 6, characterized in that it further comprises at least one non-threaded portion coated with the layer (15) according to any one of claims 1 to 6.
8. Threaded end portion (1, 2) of a tubular element according to claim 7, characterized in that the non-threaded portion comprises a stop (7, 8) and / or a sealing seat (5, 6).
9. The threaded end portion (1, 2) of a tubular element according to any one of claims 1 to 8, characterized in that it is made of steel.
10. A process for preparing a threaded end (1, 2) of a tubular element according to any one of claims 1 to 9, characterized in that it comprises at least one step of electrodepositing the surface of the threads (3, 4) of said threaded end with an aqueous composition comprising one or more zinc salts, one or more chromium salts, one or more electrolytes and one or more surfactants, preferably one or more non-ionic surfactants.
11. 11. A process according to claim 10, characterized in that it comprises a step of preparing the surface to be coated, preferably by a mechanical treatment, more preferably by sandblasting.
12. A tubular element for drilling and / or working hydrocarbon wells, for oil and gas transportation, for hydrogen transportation or storage, for carbon capture or for geothermal energy recovery, comprising a threaded end portion (1, 2) according to any one of claims 1 to 9.
13. 13. A tubular element according to claim 12, characterized in that it has at least one thread (3) which is male and extends on the outer circumferential surface of said tubular element.
14. 13. A tubular element according to claim 12, characterized in that it is female and has at least one thread (4) extending on the inner circumferential surface of said tubular element.
15. A tubular threaded joint comprising a male tubular element threaded end (1) and a female tubular element threaded end (2), the male tubular element threaded end (1) having a thread extending on its outer circumferential surface and the female tubular element threaded end (2) having at least one thread extending on its inner circumferential surface, the threads of the male tubular element threaded end (1) and the threads of the female tubular element threaded end (2) being screwed together, at least one of the threaded ends being a threaded end according to any one of claims 1 to 9.
Citation Information
Patent Citations
Chromium-base wear-resistant coating layer for metal pipeline and preparation method thereof
CN102676900A
Rust preventive steel sheet excellent in corrosion resistance and formability
JP1994025887A
Steel tube excellent in workability and chemical conversion treatment property
JP1999302862A
Threaded Connection for Pipes and Method for Producing Threaded Connection for Pipes
US20200400255A1
Corrosion resistant steel sheets improved in corrosion resistance and other characteristics
US5510196A