Ferritic stainless steel with improved magnetic properties and manufacturing method thereof

A ferritic stainless steel with controlled alloy compositions and manufacturing processes addresses poor responsiveness to low magnetic fields, achieving high magnetic permeability and effective electromagnetic shielding.

JP2024539668AActive Publication Date: 2024-10-29POHANG IRON & STEEL CO LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
JP2024523152
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2021-10-26
Filing Date
2022-10-19
Publication Date
2024-10-29
Estimated Expiration
2042-10-19

AI Technical Summary

Technical Problem

Existing materials with high magnetic permeability exhibit poor responsiveness to low externally applied magnetic fields, leading to inadequate electromagnetic shielding.

Method used

A ferritic stainless steel with controlled alloy compositions and manufacturing processes, including specific ranges for elements like C, Si, Mn, Cr, Mo, and Ti, achieving high magnetic permeability and improved responsiveness to low magnetic fields.

Benefits of technology

The ferritic stainless steel exhibits high magnetic permeability and low coercive force, enhancing electromagnetic shielding effectiveness and corrosion resistance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024539668000001
    Figure 2024539668000001
  • Figure 2024539668000002
    Figure 2024539668000002
  • Figure 2024539668000003
    Figure 2024539668000003
Patent Text Reader

Abstract

The present invention provides a ferritic stainless steel having improved magnetic properties, which exhibits high magnetic permeability in response to a low externally applied magnetic field and thereby increases reactivity to electromagnetic wave shielding, and a method for producing the same. [Solution] The stainless steel of the present invention is characterized by the following components, by weight: C: more than 0% and not more than 0.02%, N: more than 0% and not more than 0.02%, Si: 0.5% to 2.0%, Mn: 0.1% to 0.3%, Cr: 16.0% to 20.1%, Mo: more than 1.0% and not more than 2.0%, Ti: 0.1% to 0.4%, with the balance being Fe (iron) and other unavoidable impurities, and the value of the following formula (1) being 130 or less. Formula (1): 30 + 2500 * ([C] + [N]) - 15 * [Si] + 2.5 * [Cr] + 22 * ​​[Mo] (In formula (1), [C], [N], [Si], [Cr], and [Mo] mean the content (weight%) of each element).
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a ferritic stainless steel having improved magnetic properties and a manufacturing method thereof, and more particularly to a ferritic stainless steel having improved magnetic properties by controlling the alloy components and manufacturing process in order to enhance responsiveness to an externally applied magnetic field, and a manufacturing method thereof. [Background technology]

[0002] In recent years, with the development of technology fields such as smartphones and semi-autonomous vehicles, various electronic devices have come into use, and the use of electromagnetic waves has increased rapidly. This has led to an increase in electromagnetic interference between electronic devices. Electromagnetic interference can cause devices to malfunction or make precise control of the devices difficult. To prevent electronic devices from malfunctioning due to electromagnetic interference, important elements must be isolated with materials that can shield against magnetic fields.

[0003] In the case of shielding from low frequency or magnetic fields, materials with high magnetic permeability have excellent shielding ability, and there is a growing demand for materials that exhibit high magnetic permeability, especially with respect to low externally applied magnetic fields.

[0004] Conventionally, research has been conducted on materials that exhibit high magnetic permeability in response to a strong externally applied magnetic field, but these have the problem of being poor in responsiveness to an externally applied magnetic field. Summary of the Invention [Problem to be solved by the invention]

[0005] The present invention has been made to solve the above problems, and its object is to provide a ferritic stainless steel with improved magnetic properties, which exhibits high magnetic permeability in response to a low externally applied magnetic field, thereby increasing reactivity to electromagnetic wave shielding, and a method for manufacturing the same. [Means for solving the problem]

[0006] The ferritic stainless steel with improved magnetic properties of the present invention is characterized by the following composition, by weight: C: more than 0% and not more than 0.02%, N: more than 0% and not more than 0.02%, Si: 0.5% to 2.0%, Mn: 0.1% to 0.3%, Cr: 16.0% to 20.1%, Mo: more than 1.0% and not more than 2.0%, Ti: 0.1% to 0.4%, with the balance being Fe (iron) and other unavoidable impurities, and the value of the following formula (1) being 130 or less. Formula (1): 30+2500*([C]+[N])-15*[Si]+2.5*[Cr]+22*[Mo] In formula (1), [C], [N], [Si], [Cr], and [Mo] mean the content (wt%) of each element.

[0007] In the ferritic stainless steel of the present invention with improved magnetic properties, the value of the following formula (2) should be 50 or less. Formula (2): 18+800*([C]+[N])-6*[Si]+[Cr]+6*[Mo] In formula (2), [C], [N], [Si], [Cr], and [Mo] mean the content (wt%) of each element.

[0008] The ferritic stainless steel of the present invention may further contain, by weight percent, Nb: more than 0% and 0.1% or less, and Sn: more than 0% and 0.1% or less. Furthermore, the stainless steel of the present invention preferably has a maximum magnetic permeability of 1,000 or more in a 50 Hz frequency band. Furthermore, the stainless steel of the present invention preferably exhibits maximum magnetic permeability when an externally applied magnetic field is 130 A / m or less.

[0009] The ferritic stainless steel of the present invention can have a coercive force of less than 50 A / m under conditions exhibiting maximum magnetic permeability in a 50 Hz frequency band. Moreover, the stainless steel of the present invention preferably has a pitting potential value of 300 mV or more. Furthermore, the ferritic stainless steel of the present invention preferably has a hardness of Hv140 or more.

[0010] The method for producing a ferritic stainless steel having improved magnetic properties according to the present invention is characterized in that the stainless steel has, by weight percent, C: more than 0% and not more than 0.02%, N: more than 0% and not more than 0.02%, Si: 0.5% to 2.0%, Mn: 0.1% to 0.3%, Cr: 16.0% to 20.1%, Mo: more than 1.0% and not more than 2.0%, Ti: 0.1% to 0.4%, and the balance being Fe (iron) and other unavoidable impurities, and the value of the following formula (1) is 130 or less and the value of the following formula (2) is 50 or less, and the method includes the steps of producing a slab, hot rolling the slab at a reheating temperature of 1050 to 1150°C to produce a hot rolled material, cold rolling the hot rolled material to produce a cold rolled material, and final annealing the cold rolled material at 1050 to 1150°C. Formula (1): 30+2500*([C]+[N])-15*[Si]+2.5*[Cr]+22*[Mo] Formula (2): 18+800*([C]+[N])-6*[Si]+[Cr]+6*[Mo] In formulas (1) and (2), [C], [N], [Si], [Cr], and [Mo] mean the content (wt%) of each element.

[0011] In the manufacturing method of the present invention, the cold rolling is preferably carried out at a rolling reduction of 70% or more. Effect of the Invention

[0012] According to one embodiment of the present invention, a component system exhibiting high magnetic permeability is derived, and a ferritic stainless steel having improved magnetic properties and increased reactivity to electromagnetic wave shielding due to high magnetic permeability in response to a low externally applied magnetic field can be provided, as well as a manufacturing method thereof. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0013] The ferritic stainless steel with improved magnetic properties according to one embodiment of the present invention has, by weight%, C: more than 0% and not more than 0.02%, N: more than 0% and not more than 0.02%, Si: 0.5% to 2.0%, Mn: 0.1% to 0.3%, Cr: 16.0% to 20.1%, Mo: more than 1.0% and not more than 2.0%, Ti: 0.1% to 0.4%, with the balance being Fe (iron) and other unavoidable impurities, and the value of the following formula (1) may be 130 or less. Formula (1): 30+2500*([C]+[N])-15*[Si]+2.5*[Cr]+22*[Mo] In formula (1), [C], [N], [Si], [Cr], and [Mo] mean the content (wt%) of each element.

[0014] Hereinafter, the embodiments of the present invention will be described in detail with reference to the accompanying drawings. The following embodiments are presented to fully convey the concept of the present invention to those skilled in the art to which the present invention pertains. The present invention is not limited to the embodiments presented herein and may be embodied in other forms. Throughout the specification, when a part "includes" a certain element, this does not mean that other elements are excluded, but that other elements may be further included, unless otherwise specified. The singular expression includes the plural expression unless otherwise clearly indicated in the context.

[0015] The ferritic stainless steel with improved magnetic properties according to one embodiment of the present invention contains, by weight, C: more than 0% and not more than 0.02%, N: more than 0% and not more than 0.02%, Si: 0.5% to 2.0%, Mn: 0.1% to 0.3%, Cr: 16.0% to 20.1%, Mo: more than 1.0% and not more than 2.0%, Ti: 0.1% to 0.4%, and the remainder being Fe (iron) and other unavoidable impurities. The reasons for limiting the contents of alloying elements in the examples of the present invention will be described below. Unless otherwise specified, the units are % by weight.

[0016] The C (carbon) content is more than 0% and not more than 0.02%. Since C is an impurity element inevitably contained in steel, it is preferable to reduce its content as much as possible. If the C content is excessive, the magnetic properties may deteriorate due to the formation of carbides, resulting in poor magnetic permeability. Furthermore, if the C content is excessive, impurities increase, the elongation decreases, the work hardening exponent n value decreases, and the ductile-brittle transition temperature (DBTT) increases, resulting in poor impact properties. Taking this into consideration, the upper limit of the C content is limited to 0.02%. Taking into consideration the workability and mechanical properties, the upper limit of the C content is preferably 0.01% by weight.

[0017] The N (nitrogen) content is greater than 0% and less than 0.02%. When the N content is excessive, the impurities in the material increase, the elongation decreases, and the ductile-to-brittle transition temperature (DBTT) increases, resulting in a decrease in impact properties. In addition, when the N content is excessive, rod-shaped AlN precipitates are formed, which may cause grain refinement and result in poor core loss. In consideration of this, the upper limit of the N content is limited to 0.02%. In consideration of the workability and mechanical properties, the upper limit of the N content is preferably 0.015% by weight.

[0018] The Si (silicon) content is equal to or greater than 0.5% and equal to or less than 2.0%. Silicon is an element that is effective in improving magnetic permeability against a low externally applied magnetic field. In consideration of this, it is preferable that 0.5% or more of silicon is added. However, if the silicon content is excessive, the elongation rate decreases, the work hardening exponent n value decreases, and silicon-based inclusions increase, resulting in a decrease in workability. In consideration of this, the upper limit of the silicon content is limited to 2.0%. In consideration of workability, the upper limit of the silicon content is preferably 1.0% by weight.

[0019] The Mn (manganese) content is greater than or equal to 0.1% and less than or equal to 0.3%. When the Mn content is low, fine MnS precipitates are formed, which refines the crystal grains and reduces the magnetic property. Therefore, it is preferable to add Mn in an amount of 0.1% or more so that coarse MnS precipitates are formed. However, when the Mn content is excessive, the magnetic property may be deteriorated due to the increase in the fraction of MnS precipitates. Taking this into consideration, the upper limit of the Mn content is limited to 0.3%.

[0020] The Cr (chromium) content is greater than or equal to 16.0% and less than or equal to 20.1%. Cr is an element that forms a passivation film in an oxidizing environment to improve corrosion resistance. Taking this into consideration, it is preferable to add 16.0% or more of Cr. However, if the Cr content is excessive, it promotes the formation of delta (δ) ferrite in the slab, which reduces the elongation rate and impact toughness, and reduces the magnetic permeability. Taking this into consideration, the upper limit of the Cr content is limited to 20.1%.

[0021] The Mo (molybdenum) content is more than 1.0% and not more than 2.0%. Mo is an effective element for increasing the corrosion resistance of stainless steel. Taking this into consideration, it is recommended that 1.0% or more be added. However, if the Mo content is excessive, it may cause grain refinement by segregating at the grain boundaries and inhibiting grain growth, resulting in poor magnetic properties. Taking this into consideration, the upper limit of the Mo content is set to 2.0%.

[0022] The Ti (titanium) content is 0.1% or more and 0.4% or less. Ti is an effective element for improving strength by causing precipitation. Taking this into consideration, it is recommended that Ti be added in an amount of 0.1% or more. However, if the Ti content is excessive, the amount of Ti-based precipitates increases and the crystal grain size does not become large enough, resulting in a problem of reduced magnetic permeability. Taking this into consideration, the upper limit of the Ti content is set to 0.4%.

[0023] The remaining component of the present invention is iron (Fe). However, since unintended impurities may be inevitably mixed in from raw materials or the surrounding environment during normal manufacturing processes, it is not possible to exclude them. Since these impurities are known to anyone skilled in normal manufacturing processes, the contents of all of them are not specifically mentioned in this specification.

[0024] In addition, the ferritic stainless steel with improved magnetic properties according to an embodiment of the present invention may further include, by weight percent, Nb: more than 0% and not more than 0.1%, and Sn: more than 0% and not more than 0.1%.

[0025] The Nb (niobium) content is more than 0% and not more than 0.1%. Nb is an element that forms fine precipitates like Ti. However, since Ti forms a relatively high-temperature phase, fine precipitation can be prevented by heat treatment, but since Nb forms a stable phase at a relatively low temperature, it may be redissolved during hot rolling and cause fine precipitation during annealing. Therefore, if the Nb content is excessive, there is a risk of a decrease in magnetic properties due to fine precipitation, so it is preferable to manage it as an impurity. Taking this into consideration, the upper limit of the Nb content is limited to 0.1%.

[0026] The Sn (tin) content is more than 0% and not more than 0.1%. Sn is an element that forms fine precipitates like Ti. However, Ti forms a relatively high-temperature phase, so fine precipitation can be prevented by heat treatment, but Sn forms a stable phase at a relatively low temperature, so it may be redissolved during hot rolling and cause fine precipitation during annealing. Therefore, if the Sn content is excessive, there is a risk of a decrease in magnetic properties due to fine precipitation, so it is preferable to manage it as an impurity. Taking this into consideration, the upper limit of the Sn content is limited to 0.1%.

[0027] In the ferritic stainless steel with improved magnetic properties according to one embodiment of the present invention, the value of the following formula (1) is 130 or less. Formula (1): 30+2500*([C]+[N])-15*[Si]+2.5*[Cr]+22*[Mo] In formula (1), [C], [N], [Si], [Cr], and [Mo] mean the content (wt%) of each element.

[0028] The present invention provides a ferritic stainless steel with improved magnetic properties, which exhibits high magnetic permeability in response to a low externally applied magnetic field, thereby increasing the reactivity to electromagnetic shielding, and a method for producing the same. When the value of the formula (1) exceeds 130, the stainless steel exhibits a high magnetic permeability in response to a relatively large externally applied magnetic field, and thus the reactivity to electromagnetic shielding decreases. Therefore, it is preferable that the value of the formula (1) is 130 or less. By controlling the value of formula (1) to 130 or less, the ferritic stainless steel with improved magnetic properties according to an embodiment of the present invention may have a maximum magnetic permeability of 1,000 or more in a 50 Hz frequency band. In addition, the externally applied magnetic field required to exhibit the maximum magnetic permeability is 130 A / m or less.

[0029] In the ferritic stainless steel with improved magnetic properties according to one embodiment of the present invention, the value of the following formula (2) may be 50 or less. Formula (2): 18+800*([C]+[N])-6*[Si]+[Cr]+6*[Mo] In formula (2), [C], [N], [Si], [Cr], and [Mo] mean the content (wt%) of each element.

[0030] Coercive force refers to the magnitude of an external magnetic field in the opposite direction required to return a magnetized magnetic material to an unmagnetized state. If the value of the formula (2) exceeds 50, the coercive force becomes high, which may result in poor shielding ability. Therefore, it is preferable that the value of the formula (2) is 50 or less. By controlling the value of formula (2) to 50 or less, the ferritic stainless steel with improved magnetic properties according to one embodiment of the present invention can have a coercive force of less than 50 A / m under conditions exhibiting maximum magnetic permeability in a 50 Hz frequency band. In addition, the ferritic stainless steel with improved magnetic properties according to an embodiment of the present invention may have a pitting potential of 300 mV or more by improving corrosion resistance through controlling the alloy composition and manufacturing process. In addition, the ferritic stainless steel with improved magnetic properties according to an embodiment of the present invention can have a hardness of Hv140 or more by improving strength through controlling the alloy composition and manufacturing process.

[0031] Next, a method for producing a ferritic stainless steel having improved magnetic properties according to another embodiment of the present invention will be described. A method for producing a ferritic stainless steel having improved magnetic properties according to an embodiment of the present invention may include the steps of producing a slab having, by weight percent, C: more than 0% and not more than 0.02%, N: more than 0% and not more than 0.02%, Si: 0.5% to 2.0%, Mn: 0.1% to 0.3%, Cr: 16.0% to 20.1%, Mo: more than 1.0% and not more than 2.0%, Ti: 0.1% to 0.4%, and the balance being Fe (iron) and other unavoidable impurities, the value of the following formula (1) being 130 or less and the value of the following formula (2) being 50 or less, hot rolling the slab at a reheating temperature of 1050 to 1150°C to produce a hot rolled material, cold rolling the hot rolled material to produce a cold rolled material, and final annealing the cold rolled material at 1050 to 1150°C.

[0032] Formula (1): 30+2500*([C]+[N])-15*[Si]+2.5*[Cr]+22*[Mo] In formula (1), [C], [N], [Si], [Cr], and [Mo] mean the content (wt%) of each element. Formula (2): 18+800*([C]+[N])-6*[Si]+[Cr]+6*[Mo] In formula (2), [C], [N], [Si], [Cr], and [Mo] mean the content (wt%) of each element.

[0033] The reasons for the numerical limitations of the component ranges and the component relations of the alloy compositions are as described above. Each manufacturing step will be described in more detail below. First, a slab satisfying the above alloy composition and chemical formula is manufactured, and then it undergoes a series of steps including hot rolling, cold rolling and final annealing.

[0034] The slab is hot rolled at a reheating temperature of 1050 to 1150°C. If the reheating temperature of the slab is too low, the load on the rolling rolls increases, making it difficult to re-decompose the coarse precipitates generated during slab casting, and making it difficult to homogenize the internal structure. In consideration of this, the reheating temperature of the slab should be 1050°C or higher. However, if the reheating temperature is too high, the crystal grain size of the slab may become excessively coarse, and the strength may be deteriorated. In consideration of this, the upper limit of the reheating temperature of the slab is limited to 1150°C.

[0035] The cold rolling is preferably carried out at a reduction of 70% or more. If the reduction is less than 70%, it is difficult to achieve the desired strength. The cold rolled material may be final annealed at 1050 to 1150°C. If the final annealing temperature is low, the required time is long and the manufacturing cost increases. In consideration of this, the final annealing temperature is preferably 1050°C or higher. However, if the final annealing temperature is high, the microstructure may become excessively coarse, and the mechanical properties may be deteriorated. In consideration of this, the final annealing temperature is preferably 1150°C or lower.

[0036] The present invention will be described in more detail with reference to the following examples. However, the description of the examples is for illustrating the implementation of the present invention, and the present invention is not limited by the description of the examples. The scope of the present invention is determined by the matters described in the claims and matters that can be reasonably inferred from the claims. {Example}

[0037] Steels having various chemical compositions as shown in Table 1 below were cast into slabs, and the cast slabs were reheated to 1050°C. The reheated slabs were hot rolled and then cold rolled with a reduction of 70%, followed by annealing at a temperature of 1050°C to produce stainless steel as the final cold rolled product.

[0038] [Table 1]

[0039] The values ​​of formula (1) and formula (2), maximum magnetic permeability, applied magnetic field, coercive force, pitting potential and hardness are shown in Table 2. The value of formula (1) is calculated as 30+2500*([C]+[N])-15*[Si]+2.5*[Cr]+22*[Mo]. In the formula (1), [C], [N], [Si], [Cr], and [Mo] represent the content (wt %) of each element. The value of equation (2) is calculated as 18 + 800 * ([C] + [N]) - 6 * [Si] + [Cr] + 6 * [Mo]. In the formula (2), [C], [N], [Si], [Cr], and [Mo] represent the content (wt %) of each element.

[0040] The magnetic properties of the final cold-rolled product were evaluated by measuring the magnetic field due to the magnetization of the material while gradually increasing the externally applied magnetic field in the 50 Hz frequency band. The maximum magnetic permeability was measured using a non-magnetic magnetic permeability measuring instrument, model name Ferropro FP-5, by contacting a probe with a cross section of a steel sample having a diameter of 20 mm or more and a thickness of 5 mm or more. The pitting potential was measured by applying a potential to a sample immersed in a NaCl solution at a temperature of 30° C. and a concentration of 3.5%. The hardness was measured using a Zwick Roell Vickers hardness tester.

[0041] [Table 2]

[0042] Referring to Table 2, in all of Examples 1 to 7, the value of formula (1) was 130 or less, and the value of formula (2) was 50 or less. Therefore, the maximum magnetic permeability was 1,000 or more in the 50 Hz frequency band, the externally applied magnetic field for showing the maximum magnetic permeability was 130 A / m or less, and the coercive force under the condition of showing the maximum magnetic permeability was less than 50 A / m. That is, it can be seen that Examples 1 to 7 show high magnetic permeability against a low externally applied magnetic field, thereby increasing the reactivity to electromagnetic wave shielding and improving the magnetic properties. Furthermore, Examples 1 to 7 have pitting potential values ​​of 300 mV or more, and hardness of Hv140 or more. That is, Examples 1 to 7 are excellent in corrosion resistance and strength.

[0043] In Comparative Examples 1 to 5, the value of formula (1) did not satisfy 130 or less. Therefore, in Comparative Examples 1 to 5, the externally applied magnetic field for exhibiting the maximum magnetic permeability did not satisfy 130 A / m or less. In addition, in Comparative Examples 1 to 5, the value of formula (2) did not satisfy 50 or less. Therefore, in Comparative Examples 1 to 5, the coercive force did not satisfy less than 50 A / m. That is, it is found that Comparative Examples 1 to 5 have poor reactivity to electromagnetic wave shielding because the externally applied magnetic field is relatively high. In addition, in Comparative Example 4, Mo was not added, and the pitting potential value did not satisfy the requirement of 300 mV or more due to the relatively low level of Cr content. That is, Comparative Example 4 was inferior in corrosion resistance. [Industrial Applicability]

[0044] According to one embodiment of the present invention, a component system exhibiting high magnetic permeability is derived, and a ferritic stainless steel having improved magnetic properties and increased reactivity to electromagnetic shielding due to its large magnetic permeability in response to a low externally applied magnetic field can be provided, and therefore the present invention is found to have industrial applicability.

Claims

1. In weight percent, C: more than 0% and not more than 0.02%, N: more than 0% and not more than 0.02%, Si: 0.5% to 2.0%, Mn: 0.1% to 0.3%, Cr: 16.0% to 20.1%, Mo: more than 1.0% and not more than 2.0%, Ti: 0.1% to 0.4%, and the balance being Fe (iron) and other unavoidable impurities. A ferritic stainless steel having improved magnetic properties, characterized in that the value of the following formula (1) is 130 or less. Formula (1): 30+2500*([C]+[N])-15*[Si]+2.5*[Cr]+22*[Mo] (In formula (1), [C], [N], [Si], [Cr], and [Mo] represent the contents (wt %) of each element.)

2. 2. The ferritic stainless steel having improved magnetic properties according to claim 1, characterized in that the value of the following formula (2) is 50 or less: Formula (2): 18+800*([C]+[N])-6*[Si]+[Cr]+6*[Mo] (In formula (2), [C], [N], [Si], [Cr], and [Mo] represent the contents (wt %) of each element.)

3. The ferritic stainless steel having improved magnetic properties according to claim 1, further comprising, by weight percent, Nb: more than 0% and not more than 0.1%, and Sn: more than 0% and not more than 0.1%.

4. 2. The ferritic stainless steel having improved magnetic properties according to claim 1, wherein the maximum magnetic permeability is 1,000 or more in a 50 Hz frequency band.

5. 2. The ferritic stainless steel having improved magnetic properties according to claim 1, characterized in that the externally applied magnetic field required for exhibiting the maximum magnetic permeability is 130 A / m or less.

6. 2. The ferritic stainless steel with improved magnetic properties according to claim 1, characterized in that the coercive force is less than 50 A / m under conditions showing maximum magnetic permeability in a 50 Hz frequency band.

7. 2. The ferritic stainless steel with improved magnetic properties according to claim 1, characterized in that it has a pitting potential value of 300 mV or more.

8. 2. The ferritic stainless steel having improved magnetic properties according to claim 1, characterized in that the hardness is Hv140 or more.

9. In weight percent, C: more than 0% and not more than 0.02%, N: more than 0% and not more than 0.02%, Si: 0.5% to 2.0%, Mn: 0.1% to 0.3%, Cr: 16.0% to 20.1%, Mo: more than 1.0% and not more than 2.0%, Ti: 0.1% to 0.4%, and the balance being Fe (iron) and other unavoidable impurities. A step of producing a slab, in which the value of the following formula (1) is 130 or less and the value of the following formula (2) is 50 or less; hot rolling the slab at a reheating temperature of 1050 to 1150° C. to produce a hot rolled material; cold rolling the hot rolled material to produce a cold rolled material; The method for producing a ferritic stainless steel having improved magnetic properties comprises a step of final annealing the cold rolled material at 1050 to 1150°C. Formula (1): 30+2500*([C]+[N])-15*[Si]+2.5*[Cr]+22*[Mo] (In formula (1), [C], [N], [Si], [Cr], and [Mo] mean the content (wt%) of each element.) Formula (2): 18+800*([C]+[N])-6*[Si]+[Cr]+6*[Mo] (In formula (2), [C], [N], [Si], [Cr], and [Mo] mean the content (wt%) of each element.)

10. 10. The method for producing a ferritic stainless steel having improved magnetic properties according to claim 9, wherein the cold rolling is performed at a rolling reduction of 70% or more.

Citation Information

Patent Citations

  • Ferritic stainless steel excellent in weldability and corrosion resistance

    JP1990107744A

  • Production of ferritic stainless steel excellent in surface property and small in anisotropy

    JP1999302739A

  • Ferritic stainless steel good in surface property and excellent in corrosion resistance and forming workability

    JP2000001756A

  • Ferritic stainless steel sheet and production method

    WO2022124215A1