Metal oxide products for producing cathode active materials for lithium-ion rechargeable batteries

A metal oxide product with controlled primary and secondary particle sizes addresses the low discharge capacity and capacity drop issues in existing nickel-based transition metal oxides, enhancing the performance of cathode active materials for lithium ion rechargeable batteries.

JP2024539971AActive Publication Date: 2024-10-31UMICORE(BE)
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
JP2024524708
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2021-10-25
Filing Date
2022-10-20
Publication Date
2024-10-31
Estimated Expiration
2042-10-20

AI Technical Summary

Technical Problem

Existing nickel-based transition metal oxides used as precursors for cathode active materials in lithium ion rechargeable batteries exhibit low first discharge capacity (DQ1) and significant capacity drop (QF), which are critical issues for hybrid electric vehicle applications.

Method used

A metal oxide product comprising specific compositions and particle size distributions, with primary particles having a first D50 of at most 0.10 μm and D99 of up to 0.30 μm, and secondary particles with a second D50 of at least 2.0 μm, ensuring improved flowability and bulk density, is used as a precursor for cathode active materials.

Benefits of technology

The solution results in cathode active materials with enhanced first discharge capacity and reduced capacity reduction, optimizing performance for lithium ion rechargeable batteries.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024539971000001_ABST
    Figure 2024539971000001_ABST
Patent Text Reader

Abstract

1. A metal oxide product for producing a positive electrode active material for a lithium ion rechargeable battery, the metal oxide product comprising one or more oxides of one or more metals M', M' being: Ni with a content x of 20.0 mol % to 100.0 mol % relative to M', Co with a content y of 0.0 mol % to 60.0 mol % relative to M', Mn with a content z of 0.0 mol % to 80.0 mol % relative to M', and D with a content a of 0.0 mol % to 5.0 mol % relative to the total atomic content of M', D being selected from the group consisting of Al, B, Ba, Ca, Cr, Fe, Mg, and D comprising at least one element from the group consisting of Mo, Nb, S, Si, Sr, Ti, Y, V, W, Zn, and Zr, wherein x, y, z, and a are measured by ICP such that x+y+z+a=100.0 mol%, and the metal oxide product comprises secondary particles each comprising a plurality of primary particles, the primary particles having a first particle size distribution determined by analysis of images taken by CS-SEM, the first particle size distribution having a first D50 at most 0.10 μm and a first D99 at most 0.30 μm.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to metal oxides applicable for the preparation of cathode active materials for lithium-ion rechargeable batteries, and in particular to nickel-based transition metal oxides applicable as precursors for cathode active materials. [Background technology]

[0002] In preparing such active cathode materials, a precursor such as a hydroxide, carbonate or oxide containing the desired transition metal element is typically mixed with a Li source and then subjected to a heat treatment to engage in a solid-state reaction to yield a lithiated transition metal oxide.

[0003] Very fine nickel-based transition metal oxides containing primary particles with an average size of 0.4 μm are known from US Patent Application Publication No. 2010196761. However, the properties of the precursor have an influence on the properties of the final cathode active material produced therefrom. For example, the metal oxides containing primary particles of US Patent Application Publication No. 2010196761 have a low first discharge capacity DQ1 and a high capacity fade QF. High DQ1 and QF are important for the use of the cathode active material in rechargeable lithium-ion batteries suitable for (hybrid) electric vehicle applications.

[0004] An object of the present invention is to provide a metal oxide for producing a positive electrode active material, which can produce a positive electrode active material with improved first discharge capacity and capacity decrease. Summary of the Invention [Means for solving the problem]

[0005] The object of the present invention is a metal oxide product for producing a positive electrode active material of a lithium-ion rechargeable battery, the metal oxide product comprising one or more oxides of one or more metals M′, M′ being: Ni with a content x of 20.0 mol% to 100.0 mol% relative to M'; Co with a content y of 0.0 mol% to 60.0 mol% relative to M'; Mn having a content z of 0.0 mol% to 80.0 mol% relative to M'; D with a content a of 0.0 mol % to 5.0 mol % relative to the total atomic content of M', where D contains at least one element selected from the group consisting of Al, B, Ba, Ca, Cr, Fe, Mg, Mo, Nb, S, Si, Sr, Ti, Y, V, W, Zn, and Zr; x, y, z, and a are measured by ICP and x+y+z+a=100.0 mol %, and the metal oxide product comprises secondary particles each comprising a plurality of primary particles; The primary particles have a first particle size distribution, the first particle size distribution being accompanied by a metal oxide product having a first D50 of up to 0.10 μm and a first D99 of up to 0.30 μm.

[0006] The first particle size distribution is determined in this case by cross-sectional SEM image analysis. The first particle size distribution is determined as a cumulative particle size distribution. This can be done in an automated manner by image analysis software, but can also be done manually. To obtain sufficient accuracy, the first particle size distribution is determined for at least 1000 primary particles.

[0007] To calculate the D50 and D99 of the first particle size distribution, a cross-sectional SEM image of the transition metal oxide precursor particles contained in the metal oxide product should be referenced, showing clear edges of the primary particles. Primary particles are selected from the image while avoiding particles that are truncated by the frame. The area enclosed by the edges of each individual primary particle is used to calculate the equivalent diameter, which is defined as the diameter of a disk whose area is equal to the area of ​​the particle.

[0008] D50 is defined as the equivalent diameter at 50% number distribution of the cumulative particle size distribution. Similarly, D99 is defined as the equivalent diameter at 99% of the cumulative particle size distribution.

[0009] Due to the fact that the primary particles are part of larger secondary particles, the oxide product has a much better flowability compared to oxide products that only have such primary particles. As a result, the oxide product according to the invention has a lower agglomeration tendency and, as a result, a higher bulk density. This has the advantage that the oxide product takes up less space in the process equipment, in particular in the equipment for carrying out the above-mentioned heat treatment, and, as a result, the process equipment has a higher processing capacity.

[0010] Various embodiments according to the present invention are disclosed in the claims and the specification. The embodiments and examples described in the claims and the specification can be freely combined with each other unless expressly specified otherwise. Throughout this specification, when any numerical range is provided, the range also includes the end values, unless expressly specified otherwise.

[0011] In a preferred embodiment, the first D50 is at most 0.10 μm.

[0012] In a preferred embodiment, the first D99 is at most 0.30 μm.

[0013] In a preferred embodiment, the first D50 is at least 0.05 μm, preferably at least 0.06 μm.

[0014] In a preferred embodiment, the first D50 is at most 0.09 μm.

[0015] In a preferred embodiment, said first D99 is at least 0.15 μm, preferably at least 0.17 μm.

[0016] In a preferred embodiment, the first D50 is at most 0.27 μm.

[0017] As stated above, the metal element content of the metal oxide product is represented as x, y, z, and a as defined above, satisfying x+y+z+a=100.0 mol%, which is true for all embodiments described herein.

[0018] In a preferred embodiment, x≦99.0 mol%, for example, 85.0 mol%≦x≦99.0 mol%.

[0019] In a preferred embodiment, x≦95.0 mol % and y≧5.0 mol %.

[0020] In a preferred embodiment, 75.0 mol%≦x≦85.0 mol%, and 5.0 mol%≦y≦15.0 mol%, and more preferably still, 5.0 mol%≦z≦15.0 mol%.

[0021] In preferred embodiments, 50.0 mol%≦x≦80.0 mol%, for example, x is 55.0, 60.0, 65.0, 70.0, or 75.0 mol%, and 10.0 mol%≦y≦40.0 mol%, for example, y is 15.0, 20.0, 25.0, 30.0, or 35.0 mol%.

[0022] In preferred embodiments, 20.0 mol%≦x≦45.0 mol%, for example, x is 25.0, 30.0, 35.0, or 40.0 mol%.

[0023] In a preferred embodiment, 0.0 mol%≦y≦5.0 mol%, for example, y is 1.0, 2.0, 3.0, or 4.0 mol%.

[0024] In a preferred embodiment, 20.0 mol%≦x≦25.0 mol%, and 1.0 mol%≦y≦3.0 mol%, and more preferably, 70.0 mol%≦z≦80.0 mol%.

[0025] In a preferred embodiment, the one or more oxides of the one or more metals M' constitute at least 80% by weight, preferably at least 90% by weight, of the metal oxide product.

[0026] In a preferred embodiment, the primary particles consist of the one or more oxides of the one or more metals M'.

[0027] In a preferred embodiment, x<100 mol % and said one or more oxides of said one or more metals M' are mixed metal oxides.

[0028] As used herein, mixtures of single metal oxides are not considered mixed metal oxides; only oxide compounds that contain cations of two or more different metal elements are considered mixed metal oxides.

[0029] Alternatively, a mixed metal oxide may be defined as a metal oxide in which the metal elements exist in a mixed state at the atomic level.

[0030] Alternatively, a mixed metal oxide may be defined as a metal oxide in which each particle of the metal oxide contains all of the metal elements present in the metal oxide.

[0031] By mixed salt solution is meant a solution in which salts of different metal elements are present in the same solvent, whether or not an explicit mixing step has taken place.

[0032] In a preferred embodiment, the metal oxide product has a second particle size distribution as determined by laser diffraction particle size analysis, the second particle size distribution having a second D50, the second D50 being at least 2.0 μm, preferably at least 3.5 μm.

[0033] If this value is respected, it is ensured that the flowability of the metal oxide product is sufficiently good to obtain a high bulk density.

[0034] In a preferred embodiment, the metal oxide product has a second particle size distribution as determined by laser diffraction particle size analysis, the second particle size distribution having a second D50, the second D50 being at most 20 μm, preferably at most 15 μm, more preferably at most 12.5 μm.

[0035] This ensures sufficiently good lithiation for subsequent heat treatment, which can otherwise be problematic due to the long diffusion length of Li.

[0036] For completeness, it is noted that D50 is defined as the equivalent diameter at 50% of a second particle size distribution when expressed as a cumulative volumetric particle size distribution. Similarly, D99 is defined as the equivalent diameter at 99% of that second particle size distribution.

[0037] In a preferred embodiment, the secondary particles are spherical, which further helps to obtain good flowability.

[0038] The present invention further relates to a method for producing an active cathode material for a lithium-ion rechargeable battery, in which a metal oxide product according to the present invention is used as a source of the one or more metals M' in the active cathode material.

[0039] Preferably, in the method, the metal oxide product is mixed with a source of Li and the mixture is heat treated at 500° C. or above.

[0040] The present invention further relates to the use of the metal oxide product according to the invention in the manufacture of a positive electrode active material for a lithium-ion rechargeable battery. [Brief description of the drawings]

[0041] [Figure 1a] 1 is a CS-SEM image of Example 1 (EX1). [Figure 1b] 1 is a CS-SEM image of Comparative Example 1 (CEX1). [Figure 1c] 1 is a CS-SEM image of Example 4 (EX4). [Figure 1d] 1 is a CS-SEM image of Example 5 (EX5). DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0042] In the following detailed description, preferred embodiments are described to enable the practice of the invention. Although the invention is described with reference to these specific preferred embodiments, it will be understood that the invention is not limited to these preferred embodiments. The invention includes numerous alternatives, modifications, and equivalents that will be apparent from a consideration of the following detailed description and the accompanying drawings.

[0043] A) ICP analysis The amount of metal elements, e.g., Ni, Mn, and Co, in the precursor, i.e., in the metal oxide product, is measured by Inductively Coupled Plasma (ICP) method by using Agillent ICP 720-ES (Agilent Technologies). 2 grams of powder sample is dissolved in 10 mL of high-purity hydrochloric acid (at least 37 wt% HCl with respect to the total weight of the solution) in an Erlenmeyer flask. The flask is covered with glass and heated on a hot plate at 380 °C until the precursor is completely dissolved. After cooling to room temperature, the solution in the Erlenmeyer flask is poured into a 250 mL volumetric flask. Then, the volumetric flask is filled with deionized water up to the 250 mL mark, followed by complete homogenization. An appropriate amount of the solution is taken out with a pipette and transferred to a 250 mL volumetric flask for the second dilution, and the volumetric flask is filled with an internal standard and 10% hydrochloric acid up to the 250 mL mark, followed by homogenization. Finally, this 50 mL solution is used for ICP measurement.

[0044] B) Particle size B1) Secondary particle size analysis The particle size distribution (PSD) of the transition metal oxide precursor powders, i.e., the metal oxide products, is measured by laser diffraction particle size analysis using a Malvern Mastersizer 3000 equipped with a Hydro MV wet dispersion accessory after dispersing each powder sample in an aqueous medium. Sufficient sonication and stirring are applied and appropriate surfactants are introduced to improve the dispersion of the powder. The median diameter, i.e., D50, is defined as the particle diameter at 50% of the cumulative volume percent distribution obtained from the Malvern Mastersizer 3000 as measured by Hydro MV. Similarly, the D99 of this particle size distribution is defined as the equivalent diameter at 99% of this cumulative particle size distribution.

[0045] This particle size distribution is also referred to herein as the second particle size distribution.

[0046] B2) Primary particle size analysis The primary particle diameter is calculated by using MountainsLab® Expert Version 8.0.9286 (Digital Surf) according to the following steps: Step 1) Perform CS-SEM (cross-sectional scanning electron microscope) analysis: The cross section of the transition metal oxide precursor described herein is prepared by ion beam cross section polishing (CP) equipment JEOL (IB-0920CP). This equipment uses argon gas as the beam source. To prepare the test piece, a small amount of transition metal oxide precursor powder is mixed with resin and hardener, and then the mixture is heated on a hot plate for 10 minutes. After heating, it is placed in the ion beam equipment for cutting, and the settings are adjusted to the standard procedure of a voltage of 6.5 kV for a duration of 3 hours. The morphology of the positive electrode active material is analyzed by scanning electron microscopy (SEM) technique. This measurement is 9.6×10 -5 This is performed using a JEOL JSM7100F under a high vacuum environment of 100 Pa. Step 2) Load the file containing the cross-sectional SEM image of the transition metal oxide precursor obtained from step 1) at a magnification of 10,000 times. The image should have suitable contrast and brightness so that the edges of the primary particles can be clearly observed. Step 3) Set the scale according to the SEM magnification. Step 4) The area of ​​the center of the secondary particle is extracted by setting the position to 25% left and bottom, and 75% right and top. Step 5) Set edge detection in particle analysis, then set no filter with preprocessing and Height pruning <5%. Step 6) Refine the detection by selecting Remove Particles on Edges, thereby removing particles that are truncated by frame lines. Step 7) Select the statistical results and obtain the primary particle size by selecting the equivalent diameter parameter.

[0047] When particles appear porous in the CS-SEM images, pores with equivalent diameters larger than 0.40 μm are excluded from the measurement to determine the mechanical limit at which a pore is counted as a particle.

[0048] Here, the cumulative primary particle size distribution of the primary particles is obtained based on individual diameters of at least 1000 primary particles from at least one secondary particle.

[0049] This particle size distribution is also referred to herein as the first particle size distribution.

[0050] The D50 of this particle size distribution is defined as the equivalent diameter at 50% of this cumulative particle size distribution. Similarly, the D99 of this particle size distribution is defined as the equivalent diameter at 99% of this cumulative particle size distribution.

[0051] C) Coin Cell Test C1) Coin cell fabrication For the preparation of the positive electrode, a slurry containing the positive electrode active material powder, conductive agent (Super P, Timcal), binder (KF#9305, Kureha) in a weight ratio of 90:5:5, and solvent (NMP, Mitsubishi) is prepared by using a high-speed homogenizer. The homogenized slurry is spread onto one side of an aluminum foil using a doctor blade coater with a gap of 230 μm. The foil coated with the slurry is dried in an oven at 120° C. and then pressed using a calendaring tool. It is then dried again in a vacuum oven to completely remove the residual solvent in the electrode film. The coin cell is assembled in an argon-filled glove box. A separator (Celgard 2320) is placed between the positive electrode and a piece of lithium foil used as the negative electrode. 1M LiPF in EC:DMC (1:2) is added to the aluminum foil. 6 is used as the electrolyte and dropped between the separator and the electrode, and the coin cell is then completely sealed to prevent leakage of the electrolyte.

[0052] C2) Test method Each coin cell is cycled at 25° C. using a Toscat-3100 computer-controlled galvanostatic cycling station (Toyo). The coin cell test schedule used to evaluate the samples is detailed in Table 1. The definition of 1C current is 160 mA / g.

[0053] The first discharge capacity DQ1 is measured in constant current mode (CC). The capacity fade rate (QF) is calculated by the following formula:

number

[0054] D) Bulk density The bulk density of the precursor material powder, i.e., the metal oxide product, is determined by measuring the mass of the powder flowing into a graduated cylinder having a specific volume. The precursor bulk density is calculated according to the following formula:

number

[0055] The invention is further illustrated by the following (non-limiting) examples.

[0056] Comparative Example 1 CEX1 was obtained by a spray pyrolysis and spray drying process carried out as follows. 1) Preparation of Feed Solution: NiCl at a total concentration of 110 g / L with Ni, Mn, and Co in a Ni:Mn:Co ratio of 0.6:0.2:0.2. 2 , MnCl 2 , and CoCl 2 A feed solution was prepared containing the solution. 2) Spray pyrolysis: The feed solution prepared from step 1) was sprayed into a heated chamber at 650 °C to oxidize the salts and form mixed metal oxide powders. The chamber volume was approximately 8.8 m 3 and the feed rate was 30 L / h. 3) Washing: The mixed metal oxide powder from step 2) was washed with water (25 wt.% solids) to remove impurities such as Cl residues. 4) Slurry formulation: A slurry was prepared by mixing the washed powder from step 3) with a dispersant (Dolapix CA, Zschimmer & Schwarz, DE) to have 70 wt. % solids and 2 wt. % dispersant in water. 5) Wet bead mill: The slurry prepared in step 4) was wet bead milled in water with a specific milling energy of 200 kWh / T. The milling media was 1 mm diameter Y-stabilized ZrO 2 The median diameter of the milled powder particles obtained by laser diffraction was 0.71 μm. 6) Spray drying: The milled slurry prepared in step 5) was spray dried through a two fluid nozzle with an inlet temperature of 170°C and an outlet temperature of 100°C. 7) Heating: The spray dried powder obtained from step 6) was heated for 5 hours in a furnace at 500° C. under oxygen atmosphere. The result of this step was a heated precursor powder labeled Comparative Example 1.

[0057] Comparative Example 1 was composed of secondary particles having a plurality of primary particles, and the primary particle size (first particle size distribution) D50 determined according to the method described in the primary particle size analysis was 0.11 μm, D99 was 0.35 μm, the secondary particle (second particle size distribution) D50 was 15.1 μm, and the bulk density was 0.8 gr / cm 3 It was.

[0058] CEX1 is not according to the invention.

[0059] Example 1 EX1 was prepared according to the same method as CEX1, except that in step 5) the wet bead mill specific grinding energy was 1300 kWh / T. The median diameter of the milled powder particles in the slurry after step 5, obtained by laser diffraction method, was 0.28 μm.

[0060] EX1 is composed of secondary particles having a plurality of primary particles, and the primary particle size (first particle size distribution) D50 determined according to the method described in the primary particle size analysis was 0.08 μm, D99 was 0.20 μm, the secondary particle (second particle size distribution) D50 was 12.6 μm, and the bulk density was 1.5 gr / cm 3 It was.

[0061] Comparative Example 2 CEX2.1 was obtained by solid-state reaction between a lithium source and a transition metal-based precursor, carried out as follows. 1) Mixing: The precursor powder CEX1 and LiOH as the lithium source were homogeneously mixed in an industrial blending device with a lithium to metal Me (Li / Me) ratio of 1.05 to obtain mixtures (Me=Ni, Mn, Co). 2) Heating: The mixture from step 1) was heated under oxygen atmosphere at 840° C. for 15 hours. The heated powder was crushed, classified, and sieved to obtain the lithiated product, i.e., the cathode active material powder.

[0062] CEX2.2 was prepared according to the same method as CEX2.1, except that the Li / Me ratio in step 1) was 1.03 and the heating temperature in step 2) was 860°C.

[0063] CEX2.1 and CEX2.2 are not according to the invention.

[0064] Example 2 EX2.1 according to the present invention was prepared following the same procedure as CEX2.1, except that the precursor powder used in step 1) was EX1 instead of CEX1.

[0065] EX2.2 according to the present invention was prepared following the same procedure as CEX2.2, except that the precursor powder used in step 1) was EX1 instead of CEX1.

[0066] Example 3 EX3 is a solution in which the feed solution in step 1) is NiCl 2 EX3 was prepared according to the same method as EX1, except that it contained only 1.5 g / cm 3 It is a NiO precursor with a bulk density of

[0067] Example 4 EX4 was obtained by a spray pyrolysis and spray drying process carried out as follows. 1) Preparation of Feed Solution: NiCl at a total concentration of 110 g / L with Ni, Mn, and Co in a Ni:Mn:Co ratio of 0.8:0.1:0.1. 2 , MnCl 2 , and CoCl 2 A feed solution was prepared containing the solution. 2) Spray pyrolysis: The feed solution prepared from step 1) was sprayed into a heated chamber at 680 °C to oxidize the salts and form mixed metal oxide powders. The chamber volume was approximately 8.8 m 3 and the feed rate was 30 L / h. 3) Washing: The mixed metal oxide powder from step 2) was washed with water (25 wt.% solids) to remove impurities such as Cl residues. 4) Slurry formulation: A slurry was prepared by mixing the washed powder from step 3) with a dispersant (Dolapix CA, Zschimmer & Schwarz, DE) to have 60 wt. % solids and 2 wt. % dispersant in water. 5) Wet bead mill: The slurry prepared in step 4) was wet bead milled in water with a specific milling energy of 1500 kWh / T. The milling media was Y-stabilized ZrO with a diameter of 0.3 mm. 2 The median diameter of the milled powder particles obtained by laser diffraction was 0.25 μm. 6) Spray drying: The milled slurry prepared in step 5) was spray dried by a rotary atomizer at an inlet temperature of 250°C and an outlet temperature of 100°C. 7) Heating: The spray dried powder obtained from step 6) was heated in an oven at 500° C. under oxygen atmosphere for 5 hours. The result of this step was a heated precursor powder labeled EX4.

[0068] EX4 is composed of secondary particles with multiple primary particles, and the primary particle size (first particle size distribution) D50 determined according to the method described in Primary Particle Size Analysis was 0.05 μm, D99 was 0.28 μm, the secondary particle (second particle size distribution) D50 was 12.4 μm, and the bulk density was 1.4 gr / cm 3 It was.

[0069] Example 5 EX5 was obtained by a spray pyrolysis and spray drying process carried out as follows. 1) Preparation of Feed Solution: NiCl at a total concentration of 110 g / L with Ni, Mn, and Co in a Ni:Mn:Co ratio of 0.22:0.76:0.02.2 , MnCl 2 , and CoCl 2 A feed solution was prepared containing the solution. 2) Spray pyrolysis: The feed solution prepared from step 1) was sprayed into a heated chamber at 600 °C to oxidize the salts and form mixed metal oxide powders. The chamber volume was approximately 8.8 m 3 and the feed rate was 30 L / h. 3) Washing: The mixed metal oxide powder from step 2) was washed with water (25 wt.% solids) to remove impurities such as Cl residues. 4) Slurry formulation: A slurry was prepared by mixing the washed powder from step 3) with a dispersant (Dolapix CA, Zschimmer & Schwarz, DE) to have 67 wt. % solids and 2 wt. % dispersant in water. 5) Wet bead mill: The slurry prepared in step 4) was wet bead milled in water with a specific milling energy of 2130 kWh / T. The milling media was Y-stabilized ZrO with a diameter of 0.3 mm. 2 The median diameter of the milled powder particles obtained by laser diffraction was 0.22 μm. 6) Spray drying: The milled slurry prepared in step 5) was spray dried through a high pressure nozzle with an inlet temperature of 250°C and an outlet temperature of 100°C. 7) Heating: The spray dried powder obtained from step 6) was heated in an oven at 500° C. under oxygen atmosphere for 5 hours. The result of this step was a heated precursor powder labeled EX5.

[0070] EX5 is composed of secondary particles having a plurality of primary particles, and the primary particle size (first particle size distribution) D50 determined according to the method described in Primary Particle Size Analysis was 0.067 μm and D99 was 0.159 μm. The secondary particle (second particle size distribution) D50 was 7.6 μm and the bulk density was 0.8 gr / cm 3 It was. [Table 2]

[0071] Table 2 summarizes the primary particle size distributions of precursors CEX1 and EX1, as well as the preparation conditions and electrochemical properties of CEX2.1, CEX2.2, EX2.1, and EX2.2. The average primary particle size distribution D50 of EX1 is 0.08 μm, which is smaller than that of CEX1, which is 0.11 μm. Primary particle SEM images of EX1 and CEX1 are shown in Figure 1b and Figure 1a, respectively.

[0072] The cathode active materials EX2.1 and EX2.2 produced from the precursor EX1 show higher DQ1 and lower QF than the cathode active materials CEX2.1 and CEX2.2 produced from the precursor CEX1. The precursor having a first particle size distribution D50 of at least 0.05 μm and at most 0.10 μm and a D99 of at least 0.15 μm and at most 0.30 μm is suitable for achieving the objectives of the present invention, providing an cathode active material with an improved first discharge capacity of at least 174 mAh / g and a capacity fade of at most 17% / 100 cycles.

Claims

1. 1. A metal oxide product for producing an active cathode material for a lithium-ion rechargeable battery, the metal oxide product comprising one or more oxides of one or more metals M′, wherein M′ is: Ni with a content x of 20.0 mol% to 100.0 mol% relative to M'; Co with a content y of 0.0 mol% to 60.0 mol% relative to M'; Mn with a content z of 0.0 mol % to 80.0 mol % relative to M'; D with a content a of 0.0 mol % to 5.0 mol % relative to the total atomic content of M', D including at least one element selected from the group consisting of Al, B, Ba, Ca, Cr, Fe, Mg, Mo, Nb, S, Si, Sr, Ti, Y, V, W, Zn, and Zr; x, y, z, and a are measured by ICP and x+y+z+a=100.0 mol %, and the metal oxide product comprises secondary particles each comprising a plurality of primary particles; the primary particles have a first particle size distribution; The metal oxide product, wherein the first particle size distribution has a first D50 up to 0.10 μm and a first D99 up to 0.30 μm.

2. 2. The metal oxide product of claim 1, wherein the first D50 is at least 0.05 μm and the first D99 is at least 0.15 μm.

3. 3. The metal oxide product of claim 1 or 2, wherein the first D50 is at least 0.06 μm and at most 0.09 μm.

4. 4. The metal oxide product according to any one of claims 1 to 3, wherein the first D99 is at least 0.17 μm and at most 0.28 μm.

5. 5. The metal oxide product according to any one of claims 1 to 4, wherein x≦95.0 mol% and y≧5.0 mol%.

6. 6. The metal oxide product according to any one of claims 1 to 5, wherein 50.0 mol%≦x≦80.0 mol% and 10.0 mol%≦y≦40.0 mol%.

7. A metal oxide product according to any one of the preceding claims, wherein said one or more oxides of said one or more metals M' constitute at least 80% by weight, preferably at least 90% by weight of said metal oxide product.

8. 8. A metal oxide product according to any one of the preceding claims, wherein the primary particles consist of the one or more oxides of the one or more metals M'.

9. 9. A metal oxide product according to any one of the preceding claims, wherein x<100 mol % and said one or more oxides of said one or more metals M' are mixed metal oxides.

10. 10. The metal oxide product of any one of claims 1 to 9, wherein the metal oxide product has a second particle size distribution as determined by laser diffraction particle size analysis, the second particle size distribution having a second D50, the second D50 being at least 2 μm.

11. 11. The metal oxide product of any one of claims 1 to 10, wherein the metal oxide product has a second particle size distribution as determined by laser diffraction particle size analysis, the second particle size distribution having a second D50, the second D50 being up to 15 μm.

12. The metal oxide product according to any one of claims 1 to 11, wherein the secondary particles are spherical.

13. A method for producing an active cathode material for a lithium-ion rechargeable battery, wherein the metal oxide product according to any one of claims 1 to 12 is used as a source of said one or more metals M'.

14. 14. The method of claim 13, wherein the metal oxide product is mixed with a source of Li and heat treated at 500°C or higher.

Citation Information

Patent Citations

  • Positive electrode active material, production method therefor, positive electrode composite material using positive electrode active material, positive electrode for nonaqueous electrolyte secondary battery and nonaqueous electrolyte secondary battery

    JP2016201209A

  • Positive electrode active substance for nonaqueous electrolyte secondary cell, method for producing same, and nonaqueous electrolyte secondary cell using positive electrode active substance

    WO2014010448A1

  • Precursor, method for manufacturing precursor, positive electrode material, method for manufacturing positive electrode material, and lithium-ion secondary cell

    WO2020209239A1