Precipitated silica, its production method and its use

The production method for precipitated silica with controlled parameters improves dispersibility and reinforcing properties, addressing the limitations of existing silicas and enhancing tire performance.

JP2024540049APending Publication Date: 2024-10-31EVONIK OPERATIONS GMBH
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
JP2024525197
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2021-10-26
Filing Date
2022-10-17
Publication Date
2024-10-31

AI Technical Summary

Technical Problem

Existing precipitated silicas have limited dispersibility and reinforcing properties, leading to suboptimal wear resistance in tire tread compounds, which affects the life and performance of tires.

Method used

A method for producing precipitated silica with controlled physicochemical parameters, including specific surface area, particle size distribution, and pH management during production, resulting in improved dispersibility and reinforcing properties.

Benefits of technology

The produced silica enhances dispersibility and reinforcing properties, leading to reduced wear and increased tire life without compromising other tire properties.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024540049000020
    Figure 2024540049000020
  • Figure 2024540049000001
    Figure 2024540049000001
  • Figure 2024540049000002
    Figure 2024540049000002
Patent Text Reader

Abstract

The present invention relates to the following physicochemical parameters: CTAB50m 2 / g~450m 2 / g, BET / CTAB ratio <1.3, 5% tailing factor ≥150 nm. The precipitated silica is produced by reaction of water glass with H2SO4 using various ageing steps. The precipitated silica can be used for the production of rubber mixtures.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to precipitated silica, to a process for its preparation and to its use.

[0002] EP 1585704 describes the following physicochemical parameters: CTAB surface area 100~160m 2 / g, BET surface area 100~190m 2 / g, DBP value 180~300g / (100g), Sears Number V215~28ml / (5g), Moisture content 4~8% A precipitated silica having the formula:

[0003] This precipitated silica is produced at a certain AV (alkali number).

[0004] Furthermore, EP 1 764 344 describes the following physicochemical parameters: Relative width of pore size distribution γ 4.0-10.0 (g nm) / ml; BET surface area 90~320m 2 / g, CTAB surface area 100~200m 2 / g, Sears Number V225~40ml / (5g), Sears number V2 / CTAB ratio 0.16~0.28ml / (5m 2 ) and its use in rubber mixtures.

[0005] EP 2473443 describes a method for producing precipitated silica, which comprises the steps of reacting a silicate with an acidifying agent to produce a silica suspension, followed by the steps of separating and drying the suspension, the reaction of the silicate with the acidifying agent being as follows: (i) forming an aqueous initial charge having a pH of 2 to 5; (ii) adding silicate and acidifying agent simultaneously to the initial charge so as to maintain the pH of the reaction medium between 2 and 5; (iii) continuing the addition of silica to the reaction medium while adjusting the addition of acidifying agent until the pH of the reaction medium is between 7 and 10; (iv) adding silicate and an acidifying agent simultaneously to the reaction medium so that the pH of the reaction medium is maintained between 7 and 10; (v) continuing the addition of acidifying agent to the reaction medium while adjusting the addition of silicate until the pH of the reaction medium is between 2.5 and 5.3; (vi) contacting the reaction medium with an acidifying agent and a silicate such that the pH of the reaction medium is maintained between 2.5 and 5.3; (vii) a step of increasing the pH of the reaction medium obtained to a value between 4.7 and 6.3 by adding an alkaline active component, preferably a silicate, this step (vii) being optional if in step (vi) the reaction medium having a pH between 5.0 and 5.3 is contacted with an acidifying agent and a silicate so that the pH of the reaction medium is maintained at 5.0 to 5.3. A method is disclosed that does this.

[0006] Also from EP 2794479 a method for the preparation of silica is described, which comprises reacting a silicate with at least one acid to produce a silica suspension, which suspension is then separated and dried, and the reaction of the silicate with the acid is carried out in the following successive steps: (i) forming an aqueous initial charge having a pH of 2 to 5; (ii) adding silicate and acid simultaneously to the initial charge so as to maintain the pH of the reaction medium between 2 and 5; (iii) stopping the addition of acid and simultaneously continuing the addition of silica to the reaction medium until the pH of the reaction medium is between 7 and 10; (iv) adding silicate and acid simultaneously to the reaction medium so that the pH of the reaction medium is maintained between 7 and 10; (v) stopping the addition of silicate and simultaneously continuing the addition of acid to the reaction medium until the pH of the reaction medium is less than 6. in which in step (ii) the acid used after the gel point has been reached in the reaction medium is a concentrated acid from the group consisting of sulfuric acid having a concentration of at least 80% by weight, acetic acid or formic acid having a concentration of at least 90% by weight, nitric acid having a concentration of at least 60% by weight, phosphoric acid having a concentration of at least 75% by weight and hydrochloric acid having a concentration of 30% by weight.

[0007] US Patent Application Publication No. 2017 / 0044020 states: BET surface area 45~550m 2 / g, CTAB surface area 40~525m 2 / g, a content (C) of polycarboxylic acids and the corresponding carboxylates, expressed as a total carbon content, of at least 0.15% by weight; and Pore ​​distribution range ldp > 0.65 A precipitated silica having the formula:

[0008] EP 1 764 344 describes the following physicochemical parameters: Relative width of pore size distribution γ 4.0-10.0 (g nm) / ml; BET surface area 90~320m 2 / g, CTAB surface area 100~200m 2 / g, Sears Number V225~40ml / (5g), Sears number V2 / CTAB ratio 0.16~0.28ml / (5m 2 ) A precipitated silica having the formula:

[0009] A particular disadvantage of known silicas is their relatively large surface area (specific surface area of ​​about 150 m 2The main problem is the limited dispersibility of silicas (greater than 1000000 / g), especially in so-called green tire mixes, which results in the inability to optimize the reinforcing properties in typical tire tread mixes. This means that the potential reinforcing effect of such silicas cannot be fully exploited due to the lack of optimal dispersibility. Although such silicas are supposed to confer very good wear resistance to tire tread compounds reinforced with them, this is only partially or incompletely achieved.

[0010] The problem addressed by the present invention is to provide a silica which has more advantageous dispersing and reinforcing properties than those known from the prior art, which should allow a reduction in wear, i.e. an optimization of the wear resistance and therefore an increased tire life, without adversely affecting the other properties of the tire.

[0011] The present invention relates to the following physicochemical parameters: CTAB 50m 2 / g~450m 2 / g, preferably 140m 2 / g~450m 2 / g, more preferably 150m 2 / g~350m 2 / g, particularly preferably 180m 2 / g~330m 2 / g, BET / CTAB ratio <1.3, preferably 0.8 to 1.2, more preferably 0.9 to 1.2, particularly preferably 0.9 to 1.1; 5% tailing coefficient ≧150 nm, preferably 150 to 1000 nm, more preferably 170 to 500 nm, particularly preferably 175 to 400 nm The present invention provides a precipitated silica characterized by:

[0012] The Sears number V2 of the precipitated silica according to the present invention can be from 5 to 15 ml / (1.5 g), preferably from 8 to 12 ml / (1.5 g), more preferably from 10 to 12 ml / (1.5 g).

[0013] The precipitated silica according to the invention may have an Ro-Tap value >300 μm of >75% by weight, preferably >80% by weight, more preferably >85% by weight.

[0014] The precipitated silica according to the invention can be used in a compressed form, more preferably in the form of pellets, where at least 50% of the granules obtained from the Ro-Tap>300 μm fraction can have a longest dimension of the granule (defined as "particle length") in terms of height, width or length of 1.0 mm or more, preferably >1.5 mm, more preferably >2.5 mm, particularly preferably >3.0 mm. Particle length is measured with a Keyence VR-5200 3D profilometer.

[0015] To achieve an ideal, relatively dense packing of essentially stabilized aggregates or agglomerates, a certain ratio of relatively coarse aggregates or agglomerates to relatively small aggregates or agglomerates must be established. The denser the packing, the greater the interaction between these particles and the more stable the packing. The proportion of coarse particles can be expressed by the width of the distribution function at the abscissa value of the particle size distribution by CPS at 5% height. This value is expressed as a ratio to the peak maximum of the particle size distribution, which is then multiplied by d 95 This 5% tailing factor therefore represents the desired asymmetry of the particle size distribution. This leads, for example, to the formation of stabilized essential starting structures in rubber mixtures that are hardly destroyed during the mixing operation even at high shear forces, resulting in further reinforcement of the rubber matrix. By limiting the proportion of coarse particles, the dispersion is not deteriorated in such a way that the abrasion resistance is adversely affected.

[0016] The present invention further relates to a method for producing silica according to the invention, the method comprising the steps of: a) forming an initial charge by adding H2SO4 to water at a temperature between 60°C and 90°C until the pH is less than 4; b) adding water glass and H2SO4 simultaneously to the initial charge having a pH of less than 4, with the proviso that 3-55% of the total amount of water glass is used; c) stopping the metered addition of H2SO4; d) continuing the metered addition of water glass until the pH is between 3 and 9, then stopping the addition of water glass; e) subjecting the suspension to aging by stirring for a further 5 to 90 minutes without further addition of H2SO4 or water glass; f) metering water glass and H2SO4 simultaneously at a pH of the suspension above 8; g) stopping the metered addition of water glass after the entire amount of water glass has been added; h) continuing the metered addition of H2SO4 until the pH is less than 5, then stopping the addition of H2SO4; i) filtering and drying the suspension %, characterized in that a water glass having a SiO2 content of more than 20% by weight and a H2SO4 concentration of more than 90% by weight are used, and stirring is constantly performed in the process steps a) to h).

[0017] Instead of H2SO4, other acids such as HCl or CO2 can also be used.

[0018] The present invention further relates to a further process for the preparation of silica according to the invention, which process comprises the steps of: a) forming an initial charge by adding 5-50% by weight of the total amount of water glass to water at a temperature of 45°C to 90°C; b) adding H2SO4 until the pH is less than 3, then stopping the addition of H2SO4; c) subjecting the suspension to aging by stirring for a further 5 to 90 minutes without further addition of H2SO4 or water glass; d) metering water glass until the pH is between 3 and 9, then stopping the addition of water glass; e) subjecting the suspension to aging by stirring for a further 5 to 90 minutes without further addition of H2SO4 or water glass; f) then adding 5 to 50% by weight of the total amount of water glass, and then stopping the addition of water glass; g) subjecting the suspension to aging by stirring for a further 5 to 90 minutes without further addition of H2SO4 or water glass; h) adding H2SO4 until the pH is less than 3, then stopping the addition of H2SO4; i) subjecting the suspension to ageing by stirring for a further 5 to 90 minutes without further addition of H2SO4 or water glass; j) measuring water glass until the pH is between 3 and 9, and then stopping the addition of water glass; k) subjecting the suspension to aging by stirring for a further 5 to 90 minutes without further addition of H2SO4 or water glass; l) then adding the remaining amount of water glass and then stopping the addition of water glass; m) subjecting the suspension to aging by stirring for a further 5 to 90 minutes without further addition of H2SO4 or water glass; n) adding H2SO4 until the pH is between 7.5 and 9.0, and then stopping the addition of H2SO4; o) optionally heating the suspension to 85-95°C; p) subjecting the suspension to aging by stirring for a further 5 to 90 minutes without further addition of H2SO4 or water glass; q) adding H2SO4 until the pH is less than 5, then stopping the addition of H2SO4; r) filtering and drying the suspension. %, characterized in that a water glass having a SiO2 content of more than 20% by weight and a H2SO4 concentration of more than 90% by weight are used, and stirring is constantly performed in the process steps a) to g).

[0019] The filtered and dried silica obtained in process step r) can be pelletized or ground and then pelletized.

[0020] The suspension obtained in process r) can be dried in a spray dryer, for example a spray dryer designed as a nozzle tower or a spin flash dryer.

[0021] The water glass may have a weight modulus of greater than 2.8.

[0022] Instead of H2SO4, other acids such as HCl or CO2 can also be used.

[0023] The invention further provides the use of the silica according to the invention in rubber mixtures, battery separator foils, silicone rubber mixtures, medical applications, dental applications and cosmetic applications.

[0024] The invention further provides the use of the silica according to the invention as a reinforcing agent, carrier, matting agent and free-flow aid.

[0025] The invention further provides a rubber mixture, characterized in that it comprises at least one rubber and at least one precipitated silica according to the invention.

[0026] The rubber mixture according to the invention may comprise a difunctional silane, which may be a sulfur silane, a vinyltriethoxysilane, a vinyltrimethoxysilane, a 3-glycidyloxypropyltriethoxysilane, a 3-glycidyloxypropyltrimethoxysilane, a 3-methacryloyloxypropyltriethoxysilane or a methacryloyloxypropyltrimethoxysilane.

[0027] The sulfur silanes are represented by the formula (I) [(RO)Si-R 3 -] n A (I) where R is the same or different and is a linear unsubstituted or branched unsubstituted (C1-C 10 )-alkyl, preferably (C1-C6)-alkyl, more preferably a methyl or ethyl group, or an alkyl polyether group -(R 1 -O) m -R 2 where R 1are identical or different, branched or unbranched, saturated or unsaturated, aliphatic, divalent C1-C 30 is a hydrocarbon group, m is an average of 1 to 30, R 2 is an unsubstituted or substituted, branched or unbranched, monovalent C1-C 30 -Alkyl, C2-C 30 -Alkenyl, C6-C 30 -Aryl or C7-C 30 - an aralkyl group, R 3 is a bivalent C1-C branched or unbranched, saturated or unsaturated, aliphatic, aromatic or mixed aliphatic / aromatic 30 A is a hydrocarbon group, and when n=2, A is S. x where x=1 to 10, and when n=1, A is SH, SC(=O)R, or SCN. The sulfur silane is preferably bis[3-triethoxysilyl)propyl]tetrasulfide, bis[3-triethoxysilyl)propyl]disulfide, 3-mercaptopropyltriethoxysilane, (EtO)Si-(CH)-SC(O)-CH 15 , (EtO)3Si-(CH2)3-SCN, (C 13 H 27 (OCH2CH2)5-O-)2(CH3O)Si-(CH2)3-SH, or (C 13 H 27 It may be (OCH2CH2)5-O-)2(C2H5O)Si-(CH2)3-SH.

[0028] The rubber mixture may also contain further fillers apart from the silica according to the invention.

[0029] Fillers which can be used in the rubber mixtures according to the invention include the following fillers: - Carbon black: The carbon black used herein can be produced by the lamp black method, the furnace black method, the gas black method or the thermal black method. Carbon black can also be obtained from a regenerative method. Carbon black is generally from 20 to 200 m 2The carbon black can have a BET surface area of ​​1000 nm / g. The carbon black can be optionally doped with, for example, Si. - amorphous silica, preferably precipitated or shaped silica. The amorphous silica has a viscosity of 5 to 1000 m 2 / g, preferably 20 to 400m 2 / g specific surface area (BET surface area) and a primary particle size of 10 to 400 nm. The silica can optionally be in the form of a mixed oxide with other metal oxides, for example oxides of Al, Mg, Ca, Ba, Zn and titanium. - Synthetic silicates, such as aluminum silicate or alkaline earth metal silicates, such as magnesium silicate or calcium silicate. 20-400m 2 / g BET surface area and primary particle size of 10-400 nm. - Synthetic or natural aluminum oxides and hydroxides. - Natural silicates such as kaolin, and other naturally occurring silicas. - Glass fibres and glass fibre products (mats, strands) or glass microbeads.

[0030] Advantageously, amorphous silica, more preferably precipitated silica or silicates, particularly preferably from 20 to 400 m 2 Precipitated silicas having a BET surface area of ​​0.1 to 0.2 g / g can be used in amounts of 5 to 180 parts by weight per 100 parts by weight of rubber.

[0031] The fillers mentioned can be used either alone or in mixtures.

[0032] In a particularly preferred embodiment of the process, 10 to 180 parts by weight of precipitated silica according to the invention, optionally together with 0 to 100 parts by weight of carbon black and 0.1 to 20 parts by weight of a silane, in each case for 100 parts by weight of rubber, can be used to prepare the mixture.

[0033] Both synthetic and natural rubbers are suitable for the preparation of the rubber mixtures according to the invention. Preferred synthetic rubbers are described, for example, in W. Hofmann, Kautschuktechnologie [Rubber Technology], Genter Verlag, Stuttgart 1980. These include: - Polybutadiene (BR), - Polyisoprene (IR), - styrene / butadiene copolymers, such as emulsion-polymerized SBR (E-SBR) or solution-polymerized SBR (S-SBR), preferably having a styrene content of 1% to 60% by weight, more preferably 2% to 50% by weight, relative to the total polymer; - Chloroprene (CR), - Isobutylene / isoprene copolymers (IIR), - butadiene / acrylonitrile copolymers, preferably having an acrylonitrile content of 5% to 60% by weight, preferably 10% to 50% by weight, relative to the total polymer (NBR); - partially or fully hydrogenated NBR rubber (HNBR), - Ethylene / propylene / diene copolymer (EPDM), or the above rubbers, which further contain functional groups, such as carboxyl, silanol or epoxy groups, such as epoxidized NR, carboxyl-functionalized NBR, or silanol-functionalized (-SiOH) or siloxy-functionalized (-Si-OR), amino-functionalized, epoxy-functionalized, mercapto-functionalized, hydroxyl-functionalized SBR, and mixtures of these rubbers. Of particular importance in the production of automobile tire treads are anionically polymerized S-SBR rubbers (solution-polymerized SBR) having a glass transition temperature above -50°C, and mixtures thereof with diene rubbers.

[0034] The rubbers used may more preferably be NR, or functionalized or non-functionalized S-SBR and BR.

[0035] The rubber mixtures according to the invention may contain further rubber auxiliaries, such as accelerators, ageing stabilizers, heat stabilizers, light stabilizers, antiozonants, processing aids, plasticizers, resins, tackifiers, blowing agents, dyes, pigments, waxes, extenders, organic acids, vulcanization retarders, metal oxides, and activators, such as diphenylguanidine, triethanolamine, polyethylene glycol, alkoxy-terminated polyethylene glycol alkyl-O-(CH2-CH2-O) yI -H, where y I = 2 to 25, preferably y I = 2 to 15, more preferably y I = 3 to 10, most preferably y I = 3-6, or may include hexanetriol, which are well known in the rubber industry.

[0036] The rubber auxiliaries can be used in conventional amounts, which are determined by factors such as the application. Conventional amounts can be, for example, from 0.1 to 50 parts by weight per 100 parts by weight of rubber. The crosslinking agents used can be peroxides, sulfur or sulfur donor substances. The rubber mixture according to the invention can further comprise a vulcanization accelerator. Examples of suitable vulcanization accelerators include mercaptobenzothiazoles, sulfenamides, thiurams, dithiocarbamates, thioureas and thiocarbonates. The vulcanization accelerators and sulfur can be used in amounts of 0.1 to 10 parts by weight per 100 parts by weight of rubber, preferably 0.1 to 5 parts by weight per 100 parts by weight of rubber.

[0037] The rubber mixtures according to the invention can be vulcanized at temperatures between 100° C. and 200° C., preferably between 120° C. and 180° C., optionally at pressures between 10 and 200 bar. Mixing of the rubber with the precipitated silica according to the invention and the optional rubber auxiliaries and silanes can be carried out in known mixing units such as rollers, internal mixers and mixing extruders.

[0038] The rubber mixtures according to the invention can be used for the production of moulded articles, for example for the production of tyres, in particular pneumatic tyres or tyre treads, cable sheaths, hoses, power transmission belts, conveyor belts, roller covers, shoe soles, sealing rings and damping elements.

[0039] The advantages of the precipitated silicas according to the invention are their dispersibility and their special reinforcing properties in rubber mixtures.

[0040] Analytical methods for characterization of silica Loss on drying, 2 hours at 105 °C - Determination of loss on drying according to DIN EN ISO 787-2 The weight loss of a sample heated at 105° C. for 2 hours in a drying cabinet is measured.

[0041] The procedure is carried out in accordance with DIN EN ISO 787-2, but with the following specifics: Heat a weighing bottle (with a flanged lid, diameter approximately 80 mm, height approximately 30 ml) at 105 °C for approximately 1 hour with the lid removed. After cooling in a desiccator, cover with the lid. Measure the weight with an accuracy of 0.01 g using a precision balance. Accurately weigh 5-10 g of sample (weight according to bulk density) and spread it on the bottom of the weighing bottle in a uniform layer. Carefully open the weighing bottle and heat it at (105 ± 2) °C for 2 hours in a drying cabinet (the lid is also heated, but the weighing bottle is not yet closed with the lid). The weighing bottle is carefully closed with a lid, cooled in a desiccator and then reweighed to an accuracy of 0.01 g.

[0042] calculation Volatile fraction / % = (EA) x 100% / E E=initial weight / g A=final weight / g pH - pH of silica according to DIN EN ISO 787-9 The procedure is carried out in accordance with DIN EN ISO 787-9, but with the following specifics: The pelleted sample material is powdered with a mortar and pestle and then weighed.

[0043] Prepare a 5% (m / m) water suspension of the analytical sample. For this, use demineralized (DMPA) water.

[0044] Before measuring the pH, the sample suspension is stirred with a mechanical stirrer for at least 5 minutes.

[0045] The pH is measured at 23° C. using a precalibrated Metrohm pH meter type 780 equipped with a pH electrode 6.0228.000 (Metrohm).

[0046] CTAB Surface Area - measured according to ISO 5794-1 G The method is based on the adsorption of an aqueous buffer solution of CTAB (N-cetyl-N,N,N-trimethylammonium bromide) onto the "external" surface of silica, also called the "rubber effective surface". The unadsorbed CTAB is back-titrated with NDSS (dioctyl sulfosuccinate sodium salt solution). The titration end point is indicated by the maximum increase in the turbidity of the solution.

[0047] This procedure is carried out in accordance with ISO 5794-1 G with the following specifics, additions and modifications: During sample preparation, coarse particle samples of silica and silicates are preferably finely ground in a suitable mill or ground in a mortar and pestle and sieved through a 90 μm sieve rather than ground in a mortar and pestle and sieved through a 150 μm sieve as specified in the standard.

[0048] Test sample and CTAB surface area of ​​200 m 2 The suspension of the test sample and the CTAB solution with a surface area of ​​200 m2 or less is stirred for 10 minutes. 2 The suspension with CTAB solution, expected to be at least 100 mg / g, is stirred for 35 minutes as specified in the specification.

[0049] After adsorption, the silica is filtered through a 0.2 μm polyamide filter.

[0050] The filtrate is titrated in a Metrohm Titroprocessor equipped with an autosampler and a Tirando 809. As optical sensor a Metrohm Spectrosense 523 nm is used.

[0051] BET Surface Area (N2, multipoint) - Measurement according to DIN ISO 9277 This method determines the N2 specific surface area of ​​silica by the BET method according to DIN ISO 9277. The measurement is determined by low-temperature adsorption of nitrogen at a defined partial pressure. The analysis is performed at multiple points, and shows an almost linear behavior in the partial pressure range (p / po) of 0.05 to 0.20 when a total of five measurement points are measured.

[0052] The procedure is carried out in accordance with DIN ISO 9277, but with the following specifics: The pelleted samples are carefully crushed with a spatula before being weighed and then heated under vacuum in a MICROMERITICS Vacuum Bakeout Thermostat VacPrep™ 061 at (160+ / -2)°C for 60 minutes.

[0053] To measure the BET surface area, five relative pressure points (p / po) are recorded during the adsorption stage: 0.0500; 0.0875; 0.1250; 0.1625 and 0.2000.

[0054] For the measurements, a MICROMERITICS TriStar 3000 series (3000 / 3020 / 3030) equipped with a static volume measurement method and a Dewar vessel is used.

[0055] Ro-Tap (>300μm) - Sieving analysis according to ISO 5794-1 Annex F The sieving analysis is carried out using a rotary sieving machine (Tyler Analytical Sieving Machine Ro-Tap RX-29 with timer switch). The method is carried out in accordance with ISO 5794-1 Annex F. For the sieving analysis, test sieves with different mesh sizes are stacked (Analytical sieves with metal sieve mesh, ISO 3310-1, nominal mesh size 75 μm, sieve diameter 200 mm, Analytical sieves with metal sieve mesh, ISO 3310-1, nominal mesh size 150 μm, sieve diameter 200 mm, Analytical sieves with metal sieve mesh, ISO 3310-1, nominal mesh size 300 μm, sieve diameter 200 mm). The sieving towers are placed on the analytical sieving machine in the order listed. The determination of the residue on the sieve is carried out as follows: the sample is gently homogenized before the measurement. Weigh 100 g into a beaker with a precision balance to the nearest 0.01 g, and quantitatively transfer the sample onto the top sieve (300 μm). Perform Ro-Tap sieving with a beater for 5 minutes. After sieving, remove the sieving tower and weigh the fractions on the 75 μm and 300 μm sieves.

[0056] Calculation of sieve residue Ro-Tap<75μm(%)=AS×100% / E and Ro-Tap>300μm(%)=A300×100% / E and Ro-Tap>150μm(%)=A150×100% / E where: A300 = Residue on 300 μm sieve (g) AS = residue in sieving dish (g) E=Initial weight (g) It is.

[0057] 5% Tailing Factor - Measurement of particle size distribution and its asymmetry using a disc centrifuge The particle size distribution of silica is measured. The sample to be analysed is dispersed in an aqueous solution and separated according to particle size in a disc centrifuge. The larger and therefore heavier the particle, the faster it moves in the gravitational field of the centrifuge. The particles then pass through a light barrier and the absorption as a function of time is measured. These data are used to calculate the particle size distribution, i.e. the frequency as a function of particle size.

[0058] Note: In order to avoid confusion with the English description, in the explanation of this test method, "," will be written as "."

[0059] device CPS DC24000 Disc Centrifuge Hielscher UP200S ultrasonic finger with S14 sonotrode Cooling bath, e.g. Julabo F12 Fritsch mill; type "Pulverisette 14" with 80 μm sieve analytical balance Luer disposable syringes: 1.0ml and 2.0ml 30ml snap lid vial, d=28mm, h=75mm Magnetic stirrer with stir bar chemicals Ethanol, pA, e.g., Merck Desalinated water Sucrose, powder, 99.7% or more, e.g. Acros Dodecane 99%, e.g. Merck PVC reference standard, e.g. CPS Instruments method Preparation of the disc centrifuge Adjust the disc centrifuge to the desired speed. For precipitated silica, set the speed at 20,000 rpm.

[0060] A running disk centrifuge is filled with the sucrose solution containing the density gradient and covered with a layer of dodecane.

[0061] Generate sugar solutions with different concentrations. The sugar solutions here have concentrations from w=8% to w=24%. A density gradient is formed in 9 steps: 24% / 22% / 20% / 18% / 16% / 14% / 12% / 10% / 8%.

[0062] For each concentration step, 1.6 ml of sugar solution is injected into the disk centrifuge, starting with the highest concentration. Alternatively, two sugar solutions, one with the highest concentration and one with the lowest concentration, can be generated and mixed together in the required ratio in a measuring syringe. Before injection, the syringe must be shaken briefly to mix the sugar solutions. Finally, 0.5 ml of dodecane is injected.

[0063] Sample preparation All precipitated silica samples (including powder samples) are ground in a Fritsch mill prior to measurement. Fumed silica samples are not ground.

[0064] 15 g (±0.5 g) of sample material are now ground in a Fritsch mill.

[0065] 0.75 g (±0.05 g) of the ground material is weighed into a 30 ml snap-cap vial and 15 ml of demineralized water is added.

[0066] The filled snap-cap vial is secured with a clamp to a cooling bath that has been pre-equilibrated to 5° C. (±1° C.). The ultrasonic finger is positioned so that the sonotrode is immersed 5.5 cm (but at least 5 cm) deep into the snap-cap vial, measured from the top of the vial.

[0067] The sample is sonicated for 15 minutes at 100% power and 100% pulse.

[0068] procedure Before starting the measurement, the centrifuge is warmed up at the set speed for at least 30 minutes after the density gradient formation.

[0069] The measurement procedure used is called up in the instrument software. For the silica measurement, the following parameters are established: Sample parameters: Maximum diameter: 5.1 microns Minimum diameter: 0.02 microns Particle density: 2.0g / ml Particle refractive index: 1.44 Particle absorption: 0.001K Non-sphericity: 1.1 Calibration standards parameters: Peak diameter: xxx microns 1) Half height peak width: 0.2 microns 1) Particle density: 1.385g / ml 1) Fluid parameters: Fluid density: 1,045g / ml Refractive index of fluid: 1,344 Fluid Viscosity: 1.2cps (counts / sec) Suggested parameters: Display mode: Weight X-axis scale: Log 1) →Enter the data according to the manufacturer's data depending on the calibration standard material used.

[0070] In the "System Configuration" submenu, set the measurement wavelength to 470 nm.

[0071] Switch to the "Operate Analyser" submenu to analyze the dispersion of the sample. The steps required for the measurement are displayed step by step in the "Instructions" line.

[0072] Before each measurement, the calibration standards are recorded. The corresponding presettings are made in the "Options" submenu of the "Operate Analyser".

[0073] Inject 0.1 ml of each standard or sample suspension. When the measurement signal falls below the baseline, press the "Terminate" button to stop the measurement.

[0074] For each analytical sample, duplicate determinations (including variance) are performed.

[0075] result The raw data curve (absorption measurement) is used to ascertain the weight distribution by application of Mie theory. It is reported as follows: Peak (nm) - the most frequent particle size, which corresponds to the abscissa value of the maximum value of the distribution function; Half height width (d 50 ) (unit: nm) - corresponds to the width at 50% of the maximum value of the distribution function; Mean (weighted average) (nm) - the value on the abscissa of the distribution function that divides the area under the curve into two halves of equal size; Median value (50th weight percentile) (nm) - particle size at 50% of the cumulative curve; d 25 (25th Oversize Weight Percentile) (unit: nm) - The particle size (from the cumulative curve) above which 25% of the distribution falls. d 75 (75th Oversize Weight Percentile) (unit: nm) - The particle size (from the cumulative curve) above which 75% of the distribution falls. d 95 (95th Oversize Weight Percentile) (unit: nm) - The particle size (from the cumulative curve) above which 95% of the distribution falls.

[0076] 5% tailing factor: confirmation of asymmetry of particle size distribution from measurements using a disc centrifuge. The asymmetry is confirmed from the weight-based size distribution (Figure 1). For this, the peak, the distribution width at 5% peak height, and d 95 The relationship with the value is expressed as follows (Figure 1): 5% tailing factor = distribution width at 5% peak height (nm) / (2 x peak (nm)) x d 95 (nm)

[0077] Sears Number V2 - Determination of Sears Number of Hydrophilic Silica By titrating silica with a 0.1 mol / l potassium hydroxide measurement solution in the pH range of 4 to 9, the Sears number can be determined as an index of the number of free silanol groups.

[0078] The measurement method is based on the following chemical reaction, where ≡SiOH represents the silanol groups of silica: ≡SiOH+NaCl → ≡SiONa+HCl HCl+KOH→KCl+H2O.

[0079] procedure: Approximately 10.0 g of powdered, spherical or granular silica is ground uniformly using a Fritsch mill (Pulverisette 14 with 80 μm sieve) at 10,000 rpm for 60 seconds. Approximately 1.50 g of the silica thus treated is weighed to an accuracy of 0.1 mg into a 250 ml beaker and mixed with 150 ml of NaCl solution (β(NaCl)=200 g / L, adjusted to pH 3 with hydrochloric acid c(HCl)=1 mol / l). After the sample is completely wetted, the suspension is dispersed using an Ultra Turrax PT1300D (Polytron) at a speed of 20,000 rpm for 30 seconds.

[0080] Before titration, a pH meter (Methrom pH electrode LL Unitrode, PT1000 type) is calibrated at room temperature with buffer solutions (pH 4.00, pH 7.00 and pH 9.00). First, the initial pH of the suspension is measured with this pH meter, and then, depending on the result, the pH value is adjusted to 4.00 with potassium hydroxide solution (0.1 mol / l) or hydrochloric acid solution (0.1 mol / l). Then, titration is performed with 0.1 mol / l KOH measuring solution until the pH value reaches 9.00. The consumption (ml) of KOH solution from pH 4.00 to pH 9.00 is V pH4-9 A blank value titration (without adding silica) is performed similarly. The solution blank value corresponds to the volume V of potassium hydroxide solution required to titrate a silica-free NaCl solution from pH 4 to pH 9. BL Represents.

[0081] The Sears number for the original substance in ml / (1.5g) is: Sears Number オリジナル =(V pH4-9 -V BL )×T×(1.5g) / E It is calculated from:

[0082] The Sears numbers on a dry matter basis in ml / (1.5g) are: Sears Number 乾物 =(V pH4-9 -V BL )×T×(1.5g) / E×(100 / (100-TV)) where: T = titer of KOH solution used E = initial mass of the sample (g) TV = loss on drying of silica sample (%) It is.

[0083] Sears Number オリジナル corresponds to the Sears number V2. [Brief description of the drawings]

[0084] [Figure 1] FIG. 2 shows particle size distribution on a weight basis.

[0085] Working Example The pH during precipitation is measured at 60° C. unless a different temperature is specified in the experimental description.

[0086] Example 1: A reactor with a propeller agitator system is initially charged with 1474 liters of water and heated to 90°C. This initial charge is adjusted to a pH of 2.3 with sulfuric acid. Within 22 minutes, 220 kg of water glass (density 1.345 kg / l, 27% SiO2, 8% Na2O) and sulfuric acid (density 1.84 kg / l, 96% H2SO4) are added simultaneously to bring the pH of the reaction medium to 2.3. The metered addition of the sulfuric acid is then stopped and the metered addition of water glass (2.55 kg / min) is continued until the pH is 8.1. The reaction medium is aged at 90°C for 15 minutes. Then, within 38 minutes, 379 kg of water glass are added. In the course of this, the metered addition of sulfuric acid is controlled so that the pH of the reaction medium is 9 (measured at 23°C). The addition of the water glass is then stopped and the supply of sulfuric acid is continued until the pH is 2.3 (measured at 23°C). The suspension obtained is filtered, washed as usual with water and subjected to a short drying operation such as spray drying or spin flash drying, and if necessary, the powder thus obtained is pelletized.

[0087] The pelletized silica has the following analytical parameters: [Table 1]

[0088] Example 2: A reactor with a propeller agitator system is initially charged with 1676 L water and 121 kg water glass (density 1.345 kg / l, 27% SiO2, 8% Na2O) and heated to 90°C. 16 kg sulfuric acid (density 1.84 kg / l, 96% H2SO4) are added within 16.7 minutes until a pH of 2.5 is reached. This is followed by an ageing period of 5 minutes and an adjustment of the pH to 6 with water glass (1 kg / min). The ageing period is carried out at 90°C for 30 minutes. Then 120.9 kg water glass are metered in at a rate of 13.33 kg / min. This is followed by an ageing period of a further 5 minutes. Then 16 kg sulfuric acid are metered in at 0.95 kg / min until a pH of 2.5 is reached. The pH is again adjusted to pH 6 with water glass (1 kg / min). This is followed by an ageing period of 15 minutes at temperature. After aging, 120.9 kg of water glass are further metered in at a rate of 13.33 kg / min. This is followed by a further 5 minutes of aging. Then, 7 kg of sulfuric acid are added at a rate of 0.95 kg / min until a pH of 8.5 is reached. This is followed by 30 minutes of aging, at which time further sulfuric acid is added at 0.4 kg / min so as to reach a pH of 3.3 (measured at 23° C.). The suspension obtained is filtered, washed as usual with water and subjected to spin flash drying. The powder thus obtained is then pelletized. The pelletized silica has the following analytical parameters: [Table 2]

[0089] Example 3: A reactor with a propeller agitator system is initially charged with 1700 L water and 122.3 kg water glass (density 1.345 kg / l, 27% SiO2, 8% Na2O) and heated to 53°C. 16 kg sulfuric acid (density 1.84 kg / l, 96% H2SO4) are metered in at a metering rate of 1.9 kg / min until a pH of 2.5 is reached. After the addition, an ageing period of 5 minutes is allowed. Then water glass is metered in at a metering rate of 1 kg / min until a pH of 6 is reached. The mixture is then aged for 30 minutes. After the ageing period, a further 120.9 kg water glass is added within 3.3 minutes. The mixture is then aged for 5 minutes before a further 16 kg sulfuric acid is added at a rate of 1.9 kg / min until a pH of 2.5 is reached. After aging period of 5 minutes, the pH is adjusted to 6 using water glass (1 kg / min). This is followed by aging for 15 minutes and then 120.9 kg of water glass are added to the suspension. This is followed by aging for 5 minutes and then 7 kg of sulfuric acid are added at 1.9 kg / min until a pH of 8.5 is reached. The mixture is then heated to 90° C. within 21 minutes and aged at that temperature for 30 minutes. Sulfuric acid is then metered in at 0.4 kg / min until the pH of the reaction mixture reaches 4.0 (measured at 23° C.).

[0090] The suspension obtained is filtered, washed with water as usual and subjected to spin flash drying. The powder thus obtained is then pelletized. The pelletized silica has the following analytical parameters: [Table 3]

[0091] Example 4: A reactor with a propeller agitator system is initially charged with 1480 liters of water and heated to 84°C. This initial charge is adjusted to a pH of 2.3 with sulfuric acid. Within 22 minutes, 220 kg of water glass (density 1.345 kg / l, 27% SiO2, 8% Na2O) and sulfuric acid (density 1.84 kg / l, 96% H2SO4) are added simultaneously to bring the pH of the reaction medium to 2.3. The metered addition of the sulfuric acid is then stopped and the metered addition of water glass (2.56 kg / min) is continued until a pH of 4.4 is reached. The metered addition of the water glass is stopped and the pH of the suspension rises to 6.0. The reaction medium is aged for 15 minutes at 84°C. Then, 18.7 kg of water glass are metered in at 9.8 kg / min so as to bring the pH to 9 (measured at 23°C). Then, within 35 minutes, 350 kg of water glass are added. During this process, the metered addition of sulfuric acid is controlled so that the pH of the reaction medium is 9 (measured at 23° C.). The addition of water glass is then stopped and the supply of sulfuric acid is continued until the pH is 2.6 (measured at 23° C.). The suspension obtained is filtered, washed as usual with water and subjected to a short drying operation such as spray drying or spin flash drying. If necessary, the powder thus obtained is pelletized.

[0092] The pelletized silica has the following analytical parameters: [Table 4]

[0093] Example 5: A reactor with a propeller agitator system is initially charged with 1477 liters of water and heated to 78°C. This initial charge is adjusted to a pH of 2.3 with sulfuric acid. Within 22 minutes, 220 kg of water glass (density 1.345 kg / l, 27% SiO2, 8% Na2O) and sulfuric acid (density 1.84 kg / l, 96% H2SO4) are added simultaneously to bring the pH of the reaction medium to 2.3. The metered addition of the sulfuric acid is then stopped and the metered addition of water glass (2.56 kg / min) is continued until a pH of 4.3 is reached. The metered addition of the water glass is stopped and the pH of the suspension rises to 6.0. The reaction medium is aged for 15 minutes at 78°C. Then, 27.3 kg of water glass are metered in at 10.1 kg / min so as to reach a pH of 9 (measured at 23°C). Then, within 35 minutes, 350 kg of water glass are added. During this process, the metered addition of sulfuric acid is controlled so that the pH of the reaction medium is 9 (measured at 23° C.). The addition of water glass is then stopped and the supply of sulfuric acid is continued until the pH is 2.7 (measured at 23° C.). The suspension obtained is filtered, washed as usual with water and subjected to a short drying operation such as spray drying or spin flash drying. If necessary, the powder thus obtained is pelletized.

[0094] The pelletized silica has the following analytical parameters: [Table 5]

[0095] Example 6: A reactor with a propeller agitator system is initially charged with 1439 liters of water and heated to 84°C. This initial charge is adjusted to a pH of 2.9 with sulfuric acid. Within 22 minutes, 220 kg of water glass (density 1.345 kg / l, 27% SiO2, 8% Na2O) and sulfuric acid (density 1.84 kg / l, 96% H2SO4) are added simultaneously to bring the pH of the reaction medium to 2.9. The metered addition of the sulfuric acid is then stopped and the metered addition of water glass (2.43 kg / min) is continued until a pH of 4.5 is reached. The metered addition of the water glass is stopped and the pH of the suspension rises to 6.0. The reaction medium is aged for 15 minutes at 84°C and pH 6. Then, within 5 minutes, 49.9 kg of water glass are metered in so that the pH is 9.5 (measured at 23°C). Then, within 35 minutes, 350 kg of water glass are added. During this process, the metered addition of sulfuric acid is controlled so that the pH of the reaction medium is 8.6. The addition of water glass is then stopped and the supply of sulfuric acid is continued until the pH is 2.5 (measured at room temperature). The suspension obtained is filtered, washed as usual with water and subjected to a short drying operation such as spray drying or spin flash drying. If necessary, the powder thus obtained is pelletized.

[0096] The pelletized silica has the following analytical parameters: [Table 6]

[0097] Example 7: A reactor with a propeller agitator system is initially charged with 1446 liters of water and heated to 78°C. This initial charge is adjusted to a pH of 2.9 with sulfuric acid. Within 22 minutes, 220 kg of water glass (density 1.345 kg / l, 27% SiO2, 8% Na2O) and sulfuric acid (density 1.84 kg / l, 96% H2SO4) are added simultaneously to bring the pH of the reaction medium to 2.9. The metered addition of the sulfuric acid is then stopped and the metered addition of water glass (2.35 kg / min) is continued until a pH of 4.7 is reached. The metered addition of the water glass is stopped and the pH of the suspension rises to 6.0. The reaction medium is aged for 15 minutes at 78°C and pH 6. Then, within 5 minutes, 50.1 kg of water glass are metered in so that the pH is 9.5 (measured at 23°C). Then, within 35 minutes, 350 kg of water glass are added. During this process, the metered addition of sulfuric acid is controlled so that the pH of the reaction medium is 8.6. The addition of water glass is then stopped and the supply of sulfuric acid is continued until the pH is 2.6 (measured at 23° C.). The suspension obtained is filtered, washed as usual with water and subjected to a short drying operation such as spray drying or spin flash drying. If necessary, the powder thus obtained is pelletized.

[0098] The pelletized silica has the following analytical parameters: [Table 7]

[0099] Example 8: A reactor with a propeller agitator system is initially charged with 1280 liters of water and heated to 90°C. This initial charge is adjusted to a pH of 2.9 with sulfuric acid. Within 22 minutes, 220 kg of water glass (density 1.345 kg / l, 27% SiO2, 8% Na2O) and sulfuric acid (density 1.84 kg / l, 96% H2SO4) are added simultaneously to bring the pH of the reaction medium to 2.9. The metered addition of the sulfuric acid is then stopped and the metered addition of water glass (2.45 kg / min) is continued until a pH of 8.1 is reached. The metered addition of the water glass is stopped and the reaction medium is aged for 15 minutes at 90°C. Then, 190 kg of water glass are metered in at 10.1 kg / min within 19 minutes. Then, 350 kg of water glass are added within 35 minutes. Then, 1.28 kg / min of sulfuric acid are metered in so that the pH is 2.7 (measured at 23°C). The suspension obtained is filtered, washed as usual with water and subjected to a short drying operation such as spray drying or spin flash drying, and if necessary, the powder thus obtained is pelletized.

[0100] The pelletized silica has the following analytical parameters: [Table 8]

[0101] Comparative Example 1: In Comparative Example 1, ZEOSIL (registered trademark) HRS 1200 MP manufactured by SOLVAY SA was used.

[0102] Comparative Example 2: In Comparative Example 2, ZEOSIL (registered trademark) PREMIUM 200 MP manufactured by SOLVAY SA was used.

[0103] Comparative Example 3: Comparative Example 3 was a re-execution of Example 2 of EP 2794479.

[0104] Comparative Example 4: In Comparative Example 4, ZEOSIL (registered trademark) 1165 MP manufactured by SOLVAY SA was used.

[0105] Example 9: Rubber properties test The terms "unvulcanized rubber mix" and "vulcanized rubber mix" are used interchangeably herein. Table 1 shows the rubber materials used.

[0106] [Table 9]

[0107] The silica used in the rubber mixtures and its analytical values ​​are compared in Table 2.

[0108] [Table 10]

[0109] The formulations used for the rubber mixtures are shown in Table 3. The unit "phr" ("parts per hundred rubber") used herein means parts by weight relative to 100 parts by weight of the raw rubber used.

[0110] [Table 11-1] [Table 11-2]

[0111] The amount of silane required to realize the reinforcing potential of each silica was determined by the rule of three: the higher the specific surface area (CTAB surface area, which is important for rubber-related reinforcing), the more silane is required. 2 This was based on the assumption that 5.8 phr of Si 266 is required for 1000 / g of CTAB surface area.

[0112] General methods for producing rubber mixtures and their vulcanizates are described in "Rubber Technology Handbook", W. Hofmann, Hanser Verlag 1994. In particular, the equipment and mixing methods used for producing the rubber mixtures according to the invention and the reference mixtures are shown in Table 4.

[0113] In preparation for the mixing operation, the plasticizer to be introduced is weighed into a low melting LDPE pouch that can be included in the process. The term "plasticizer" is used in this context synonymously with TDAE (Treated Distilled Aromatic Extract).

[0114] [Table 12-1] [Table 12-2]

[0115] The test specimens and sheets are vulcanized in a conventional vulcanization press at a temperature of 165° C. and a holding pressure of 130 bar. The vulcanization time of the mixture is 20 minutes.

[0116] Rubber testing is performed according to the test methods specified in Table 5.

[0117] [Table 13-1] [Table 13-2]

[0118] The results of the rubber tests are shown in Table 6.

[0119] [Table 14]

[0120] It has been found that the silicas according to the invention can achieve better dispersion compared to the prior art, which results in better reinforcing properties, which is reflected in the reinforcing index: the higher this index, the better the potential reinforcing effect of each silica is exploited.

[0121] Example 10: Study of rubber properties In a further mixing series, comparative example 4 was compared with example 2 according to the invention. For this, they were mixed according to the mixing method in table 4 and tested according to the test method described in table 5. The formulations are shown in table 7.

[0122] The test specimens and sheets are vulcanized in a conventional vulcanization press at a temperature of 165° C. and a holding pressure of 130 bar. The vulcanization time of the mixture is 15 minutes.

[0123] [Table 15]

[0124] [Table 16]

[0125] Example 10 also shows that the silica according to the invention of Example 2 can achieve better dispersion compared to the prior art, which results in better reinforcing properties, which is reflected in the reinforcing index. The higher this index, the better the potential reinforcing effect of each silica is exploited.

Claims

1. The following physicochemical parameters: CTAB 50m 2 / g~450m 2 / g、 BET / CTAB ratio <1.3, 5% tailing factor ≧150 nm Precipitated silica, characterized by:

2. The CTAB is 150m 2 / g~350m 2 2. Precipitated silica according to claim 1, characterized in that:

3. 2. Precipitated silica according to claim 1, characterized in that said BET / CTAB ratio is between 0.9 and 1.

2.

4. 2. Precipitated silica according to claim 1, characterized in that said 5% tailing factor is between 175 and 400 nm.

5. The CTAB is 150m 2 / g to 350m 2 2. Precipitated silica according to claim 1, characterized in that said BET / CTAB ratio is between 0.9 and 1.2 and said 5% tailing factor is between 175 and 400 nm.

6. 2. The method of claim 1, further comprising the steps of: a) Add H to water at a temperature between 60°C and 90°C until the pH is less than 4 2 SO 4 forming an initial charge by adding b) adding water glass and H 2 SO 4 simultaneously, with the proviso that the amount of water glass used is 3-55%; c) H 2 SO 4 ceasing the metered addition of d) continuing the metered addition of water glass until the pH is between 3 and 9, then stopping the addition of water glass; e) H 2 SO 4 ageing the suspension by stirring for an additional 5 to 90 minutes without further addition of water or water glass; f) adding water glass and H2O while the pH of the suspension exceeds 8; 2 SO 4 5. The method of claim 1, g) stopping the metered addition of water glass after the entire amount of water glass has been added; h) H2O until the pH is less than 5 2 SO 4 Continue metered addition of H 2 SO 4 ceasing the addition of i) filtering and drying the suspension wherein more than 20 wt. % SiO 2 Water glass having a content of more than 90% by weight, 2 SO 4 and stirring is constantly carried out in process steps a) to h).

7. 2. The method of claim 1, further comprising the steps of: a) forming an initial charge by adding 5-50% by weight of the total amount of water glass to water at a temperature of 45° C. to 90° C.; b) H2O until the pH is less than 3 2 SO 4 Then, H 2 SO 4 ceasing the addition of c) H 2 SO 4 ageing the suspension by stirring for an additional 5 to 90 minutes without further addition of water or water glass; d) metering in water glass until the pH is between 3 and 9, then stopping the addition of water glass; e) H 2 SO 4 ageing the suspension by stirring for an additional 5 to 90 minutes without further addition of water or water glass; f) then adding 5-50 wt. % of the total amount of water glass, and then stopping the addition of water glass; g) H 2 SO 4 ageing the suspension by stirring for an additional 5 to 90 minutes without further addition of water or water glass; h) H2O until the pH is less than 3 2 SO 4 Then, H 2 SO 4 ceasing the addition of i) H 2 SO 4 ageing the suspension by stirring for an additional 5 to 90 minutes without further addition of water or water glass; j) metering water glass until the pH is between 3 and 9, then stopping the addition of water glass; k) H 2 SO 4 ageing the suspension by stirring for an additional 5 to 90 minutes without further addition of water or water glass; l) then adding 5-50 wt. % of the total amount of water glass, and then stopping the addition of water glass; m) H 2 SO 4 ageing the suspension by stirring for an additional 5 to 90 minutes without further addition of water or water glass; n) H until the pH reaches 7.5-9.0 2 SO 4 Then, H 2 SO 4 ceasing the addition of o) optionally heating the suspension to 85-95°C; p)H 2 SO 4 ageing the suspension by stirring for an additional 5 to 90 minutes without further addition of water or water glass; q) H until the pH is less than 5 2 SO 4 Then, H 2 SO 4 ceasing the addition of r) filtering and drying the suspension. wherein more than 20 wt. % SiO 2 Water glass having a content of more than 90% by weight, 2 SO 4 and stirring is constantly carried out in process steps a) to g).

8. 10. Use of the silica according to claim 1 in rubber mixtures, battery separator foils, silicone rubber mixtures, medical applications, dental applications and cosmetic applications.

9. 2. Use of the silica according to claim 1 as a reinforcing agent, carrier, matting agent and free-flow aid.

10. A rubber mix, characterized in that it comprises at least one rubber and at least one precipitated silica according to claim 1.

Citation Information

Patent Citations

  • Novel method for producing precipitated silica

    JP2013503806A

  • Hydrous silicic acid for rubber reinforcement and filling

    JP2020026364A

  • Precipitated silica and process for producing same

    JP2020519554A