Preparation method and application of modified hopcalite catalyst
The modified hopcalite catalyst with CuAl2O4 and MnAl2O4 composite oxide structure addresses the high cost and low-temperature activity issues of noble metal and conventional hopcalite catalysts by enhancing Cu2+ and Mn4+ dispersion, achieving 100% CO conversion at room temperature.
Patent Information
- Application Number
- JP2024526759
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2022-09-27
- Filing Date
- 2022-12-05
- Publication Date
- 2024-10-31
- Estimated Expiration
- 2042-12-05
AI Technical Summary
Existing noble metal catalysts for CO combustion are costly, limiting their commercial application, and conventional hopcalite catalysts face challenges in achieving high low-temperature activity due to limited dispersion of Cu2+ and Mn4+ on the surface.
A modified hopcalite catalyst with a CuAl2O4 and MnAl2O4 composite oxide structure is developed, enhancing Cu2+ and Mn4+ dispersion through Al doping, forming a stable spinel structure for improved low-temperature activity.
The modified catalyst achieves 100% CO conversion at room temperature with enhanced low-temperature activity and reduced preparation costs, demonstrating improved catalytic stability and efficiency.
Smart Images

Figure 2024540340000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to the technical field of catalysts for catalytic combustion CO. [Background technology]
[0002] In industrial production and construction practice, equipment generates large amounts of CO due to incomplete combustion. Colorless and odorless CO gas is highly likely to bind with hemoglobin in human blood, leading to extremely serious and irreversible consequences such as hemiplegia, aphasia, and even death due to lack of oxygen to the brain. In common application scenarios such as coal-fired boilers and factory equipment operation and oxidative decomposition of materials, carbon monoxide poisoning accidents are frequent, making the treatment of CO an urgent task.
[0003] Up to now, the catalysts used for CO catalytic combustion are mainly precious metal catalysts, but due to their high cost, the commercial application of precious metal catalysts is greatly restricted. Therefore, the development of non-precious metal catalysts with high low-temperature activity, high stability and low cost will greatly promote the progress of commercial application of catalytic combustion.
[0004] Hopcalite catalysts, which are non-precious metal catalysts and are mainly composed of Cu, Mn oxides and their composite oxides, have shown high reaction activity in the study of catalytic combustion activity. Hopcalite catalysts, which are mainly composed of MnO2 and CuO, are widely used in the sealed cabins of submarines and can convert CO to CO2 around the combustion chamber at 320°C. This reaction has the advantage of not generating secondary toxic pollutants (Christopher et al. Applied Catalysis B: Environmental, 2017, (203) 533-540). Since conventional hopcalite catalysts are made of CuMn2O4 spinel composed of Cu and Mn, most of the Cu and Mn elements are mainly present in the catalyst as carriers, and the Cu atoms that can be dispersed and liberated on the surface of the catalyst to form catalytic reaction active centers are also present. 2+ and Mn 4+ Therefore, it is difficult to obtain the desired low temperature catalytic activity with the hopcalite catalyst. Summary of the Invention [Problem to be solved by the invention]
[0005] The present invention aims to provide a modified hopcalite catalyst in which Al is doped to form a new spinel structure with Cu and Mn to act as a carrier, allowing more Cu2+ and Mn4+ to be scattered on the catalyst surface, and thus the catalyst has a stable structure, good low-temperature catalytic activity, and high catalytic stability; a preparation method for the catalyst with a simple process and high product stability; and an application method for the catalyst. [Means for solving the problem]
[0006] In order to achieve one of the above objects, the present invention provides the following technical solutions.
[0007] A modified hopcalite catalyst containing a composite oxide consisting of CuAl2O4, MnAl2O4 and oxides of Cu and Mn.
[0008] In some embodiments of the present invention, the Cu, Mn oxide is CuMnO2.
[0009] In some examples of the present invention, the ratio of the amounts of Cu, Mn and Al in the composite oxide is 1-10:1-10:0.2-5.
[0010] The ratio of the amounts of Cu, Mn and Al is preferably 5:1:0.2-3, and more preferably 5:1:0.5-1.
[0011] In order to achieve the second object above, the present invention provides the following technical solutions.
[0012] The preparation method of said catalyst includes the following steps: co-precipitating a mixed solution containing Cu ions, Mn ions and Al ions, and roasting the obtained precipitate.
[0013] In some embodiments of the present invention, the mixed solution is an acid solution containing a compound of Cu, a compound of Mn, and a compound of Al.
[0014] Preferably, the acid solution is a nitric acid solution.
[0015] In some embodiments of the present invention, the roasting temperature is between 300 and 500°C.
[0016] In some embodiments of the present invention, the roasting time is 6 to 10 hours.
[0017] In some embodiments of the present invention, the co-precipitation is carried out under alkaline conditions.
[0018] Preferably, the alkaline conditions are pH=8 to 9, more preferably pH=8 to 8.5.
[0019] In some embodiments of the present invention, the co-precipitating alkali is the precipitating agent, and the alkali is one or more of sodium hydroxide, sodium carbonate, and ammonia.
[0020] In some embodiments of the present invention, the alkali has a concentration of 0.3 to 3 mol L -1 is located.
[0021] Preferably, the alkali has a concentration of 1.5 to 2.5 mol L. -1 is located.
[0022] In some embodiments of the present invention, the co-precipitation is at a temperature of 10-30°C.
[0023] Preferably, the coprecipitation is carried out at a temperature of 15 to 20°C.
[0024] In some examples of the present invention, after coprecipitation, the mixed solution is allowed to stand for 10 to 20 hours.
[0025] In some examples of the present invention, the ratio of the amounts of Cu, Mn and Al in the composite oxide is 1-10:1-10:0.2-5.
[0026] Preferably, the ratio of the amounts of Cu, Mn and Al is 5:1:0.5-1.
[0027] In some embodiments of the present invention, the mixed solution has a total concentration of metal ions of 0.5 to 1.5 mol L -1 is located.
[0028] In some embodiments of the present invention, the Cu compound is either copper nitrate (Cu(NO3)2·3H2O) and / or copper sulfate (CuSO4).
[0029] In some embodiments of the present invention, the Mn compound is either manganese nitrate (MnN2O6·4H2O) and / or manganese nitrate solution (Mn(NO3)2).
[0030] In some embodiments of the present invention, the compound of Al is either aluminum nitrate (Al(NO3)3·9H2O).
[0031] In some embodiments of the present invention, the preparation procedure of the mixed solution includes dissolving the copper source, the manganese source and the aluminum source in distilled water in order to obtain the mixed solution.
[0032] In order to achieve the above three objects, the present invention provides the following technical solutions.
[0033] The catalyst described above or the catalyst prepared according to the above preparation method is applied to CO catalytic combustion.
[0034] In some embodiments of the present invention, the catalyst has a particle size of 20-60 mesh.
[0035] Specifically, in the above application, the low temperature oxidation of CO is at a temperature of 20°C. Effect of the Invention
[0036] (1) In the present invention, a new hopcalite catalyst for CO combustion was obtained. (2) Compared with the conventional hopcalite catalyst, the present invention also dopes the existing hopcalite catalyst with Al2O3 to improve the dispersion of the active center components Cu2+ and Mn4+. At the same time, the doping effect of the metal ions improves the bonding strength between CO and Cu and Mn, thereby significantly improving the low-temperature activity and contact efficiency of the catalyst. (3) In the present invention, the catalyst has a low-temperature activity used in the CO catalytic combustion reaction that is higher than that of the conventional hopcalite catalyst, and can achieve 100% conversion of CO at room temperature of 20°C. (4) Doping with Al can improve the low-temperature catalytic activity of the catalyst, while further reducing the preparation cost of hopcalite catalyst. The preparation process of coprecipitation is easy to operate and has strong feasibility. [Brief description of the drawings]
[0037] [Figure 1] XRD spectrum of Example 5 [Diagram 2] Comparison of Example 5 and commercial Hopcalite catalyst H2-TPR DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0038] The present invention will now be described in detail in conjunction with examples. It should be understood that the above examples and drawings are merely for illustrative purposes only and do not constitute any limitations on the scope of the present invention. Any suitable transformation or combination consistent with the object of the present invention is included in the claims of the present invention.
[0039] The catalysts used in each of the examples below were prepared according to the following procedures.
[0040] Add appropriate amounts of copper nitrate, manganese nitrate and aluminum nitrate to appropriate amounts of distilled water and mix thoroughly to obtain a transparent metal ion mixed solution. The amount of each raw material is such that the molar ratio of Cu:Mn:Al is 5:1:x, where x = 0~1. In the obtained mixed solution, the total concentration of metal ions is 1 mol L -1 The solution should be 2 mol L. -1The NaOH solution is used as a precipitant, and under stirring conditions, the metal ion mixture and NaOH precipitant are simultaneously dropped into a 5L beaker to co-precipitate and react, the reaction temperature is room temperature, pH=8~8.5, and the dropping speed of both is adjusted during titration to adjust the pH of the reaction solution. When the metal ion solution is completely dropped, the drop of NaOH precipitant is immediately stopped, followed by stirring at room temperature for 2h, and then allowed to stand for aging for 15h. The obtained precipitate is filtered and then washed to about pH=7, the obtained filter cake is dried in air at 100℃, and then roasted at 400℃ for 6~10h to obtain CuO-MnO2-xAl2O3 catalyst, and the sieved 20~60 mesh catalyst granules are used for fixed bed CO catalytic combustion reaction.
[0041] In each of the following examples, the process of the combustion reaction using a fixed bed CO catalyst is as follows:
[0042] Five grams of the sieved catalyst granules were loaded into a fixed-bed reactor and preactivated with air at 350°C for about 6 hours. The temperature of the bed was then adjusted to the required reaction temperature and the catalyst was then pumped at a rate of 30 mL min -1 CO is fed into a fixed-bed reactor through a mass flowmeter at a flow rate of 0.01 to carry out catalytic combustion reaction, and the reaction product gas is directly fed into a gas chromatograph for detection. The catalytic combustion reaction temperature is 20-200°C, and the Al doping amount (calculated as metal ion Al / (Cu+Mn)%) in the CuO-MnO2-xAl2O3 catalyst is 0-30%. EXAMPLES
[0043] The combustion reaction activity of the CO catalyst is examined against commercial hopcalite catalyst. -1 A mixed gas consisting of 1.6% CO, 21.4% oxygen and 77.0% nitrogen was passed through the reactor at a reaction air flow rate of 360 h -1 The CO catalytic combustion reaction is carried out under normal pressure and a reaction temperature of 15°C. After the temperature has stabilized for 15 minutes, sampling is started. Online analysis is performed using a TCD detector on an SC-2000 gas chromatograph, and the CO conversion rate of the reaction product is evaluated using the following formula. X CO(%) = ([CO] in -[CO] out ) / [CO] in *100% X CO :CO conversion rate, [CO] in : CO concentration at the reactor inlet; [CO] out : CO concentration at the reactor outlet
[0044] When the error of the three sampling results is less than 1%, the collection at the temperature is completed, and the average conversion rate of the three samples is taken as the conversion rate at the temperature. Next, the temperature is raised at a rate of 5°C per sampling, and the reaction is terminated when the CO conversion rate reaches 100%.
[0045] The reaction results showed that the CO conversion rate reached 100% at 125°C after the mixer entered the catalyst bed layer. EXAMPLES
[0046] A Cu-Mn-Al composite oxide was prepared with a molar ratio of Cu:Mn:Al = 5:1:0.2 and used as a catalyst. It was reacted in a fixed-bed reactor at 30 mL min -1 A mixed gas consisting of 1.6% CO, 21.4% oxygen and 77.0% nitrogen was passed through the reactor at a reaction air flow rate of 360 h -1 The combustion reaction using CO as a catalyst was carried out under normal pressure and at a reaction temperature of 15°C. After the temperature had stabilized for 15 minutes, sampling was started and online analysis was performed using a TCD detector on an SC-2000 gas chromatograph.
[0047] The reaction results showed that the CO conversion rate reached 100% at 85°C after the mixer entered the catalyst bed layer. EXAMPLES
[0048] A Cu-Mn-Al composite oxide with a molar ratio of Cu:Mn:Al = 5:1:0.4 was prepared and used as a catalyst. It was reacted in a fixed-bed reactor at 30 mL min -1 A mixed gas consisting of 1.6% CO, 21.4% oxygen and 77.0% nitrogen was passed through the reactor at a reaction air flow rate of 360 h -1The combustion reaction using CO as a catalyst was carried out under normal pressure and at a reaction temperature of 15°C. After the temperature had stabilized for 15 minutes, sampling was started and online analysis was performed using a TCD detector on an SC-2000 gas chromatograph.
[0049] The reaction results showed that the CO conversion rate reached 100% at 55°C after the mixer entered the catalyst bed layer. EXAMPLES
[0050] A Cu-Mn-Al composite oxide with a molar ratio of Cu:Mn:Al = 5:1:0.6 was prepared and used as a catalyst. It was reacted in a fixed-bed reactor at 30 mL min -1 A mixed gas consisting of 1.6% CO, 21.4% oxygen and 77.0% nitrogen was passed through the reactor at a reaction air flow rate of 360 h -1 The combustion reaction using CO as a catalyst was carried out under normal pressure and at a reaction temperature of 15°C. After the temperature had stabilized for 15 minutes, sampling was started and online analysis was performed using a TCD detector on an SC-2000 gas chromatograph.
[0051] The reaction results showed that the CO conversion rate reached 100% at 35°C after the mixer entered the catalyst bed. EXAMPLES
[0052] A Cu-Mn-Al composite oxide with a molar ratio of Cu:Mn:Al = 5:1:0.8 was prepared and used as a catalyst. It was reacted in a fixed-bed reactor at 30 mL min -1 A mixed gas consisting of 1.6% CO, 21.4% oxygen and 77.0% nitrogen was passed through the reactor at a reaction air flow rate of 360 h -1 The combustion reaction using CO as a catalyst was carried out under normal pressure and at a reaction temperature of 15°C. After the temperature had stabilized for 15 minutes, sampling was started and online analysis was performed using a TCD detector on an SC-2000 gas chromatograph.
[0053] The reaction results showed that the CO conversion rate reached 100% at 20°C after the mixer entered the catalyst bed layer. EXAMPLES
[0054] A Cu-Mn-Al composite oxide with a molar ratio of Cu:Mn:Al = 5:1:1 was prepared as a catalyst. It was then run at 30 mL min -1 A mixed gas consisting of 1.6% CO, 21.4% oxygen and 77.0% nitrogen was passed through the reactor at a reaction air flow rate of 360 h -1 The combustion reaction using CO as a catalyst was carried out under normal pressure and at a reaction temperature of 15°C. After the temperature had stabilized for 15 minutes, sampling was started and online analysis was performed using a TCD detector on an SC-2000 gas chromatograph.
[0055] The reaction results showed that the CO conversion rate reached 100% after the mixer entered the catalyst bed at 45°C. EXAMPLES
[0056] The process of preparing Cu-Mn-Al composite oxide was mainly studied when the molar ratio of Cu:Mn:Al was 5:1:0.2, 5:1:0.4, 5:1:0.6, 5:1:0.8, and 5:1:1, respectively, for commercial hopcalite catalyst. The XRD spectrum shown in Figure 1 was obtained by reproducing the X-ray diffraction of the catalyst in Example 5, which has the best low-temperature activity. As shown in the figure, the main crystal form in the Cu-Mn-Al catalyst is a structure in which Cu, Mn, and Al are bonded together to form a spinel. At the same time, the CuMnO2 composite oxide was formed. It was found that after the Al element was added, the CuMn2O4 spinel structure was replaced by CuAl2O4 or MnAl2O4 in the newly formed Cu-Mn-Al composite oxide catalyst, and the dispersion of Cu and Mn was improved, resulting in better catalytic activity. The results of H2-TPR also verified this rule. In Example 5, the catalyst and commercial hopcalite catalyst were heated and reduced through the H2 procedure, and the H2-TPR comparison spectrum shown in Figure 2 was obtained. The figure shows that the Cu-Mn catalyst can be reduced more easily by doping with Al. This is because the Cu in the catalyst 2+ , Mn 2+At the same time, the doping of Al effectively reduces the interaction between the active component and the carrier, and the free Cu as the active component on the catalyst surface is reduced. 2+ , Mn 4+ This improves the degree of dispersion of the catalyst, thereby improving the low-temperature reducibility of the catalyst and improving the reaction activity of catalytic combustion.
[0057] The above examples are merely preferred implementation methods of the present invention, and the claims of the present invention are not limited to the above examples, and all technical solutions consistent with the concept of the present invention are included in the claims of the present invention. Improvements and modifications made by ordinary skilled in the art without departing from the principles of the present invention are also included in the claims of the present invention.
Claims
1. A method for preparing a modified hopcalite catalyst, comprising the steps of: A solution containing a copper source, a manganese source and an aluminum source is mixed to obtain a mixed solution, and the mixed solution is co-precipitated under alkaline conditions to obtain a precipitate, and the obtained precipitate is roasted to obtain the modified hopcalite catalyst. The mixture solution is co-precipitated under alkaline conditions at 10 to 30°C.
2. The preparation method of modified hopcalite catalyst according to claim 1, characterized in that: The copper source is an acid solution of a compound containing Cu ions, the manganese source is an acid solution of a compound containing Mn ions, and the aluminum source is an acid solution of a compound containing Al ions.
3. The method for preparing modified hopcalite catalyst according to claim 2, wherein the acid solution of the compound of Cu ion comprises copper nitrate and / or copper sulfate.
4. 3. The method for preparing a modified hopcalite catalyst according to claim 2, wherein the acid solution of a compound containing Mn ions contains manganese nitrate.
5. The method for preparing modified hopcalite catalyst according to claim 2, characterized in that the acid solution of the compound of Al ion contains aluminum nitrate.
6. The method for preparing modified hopcalite catalyst according to any one of claims 1 to 5, characterized in that the ratio of the amount of Cu in the copper source, the amount of Mn in the manganese source, and the amount of Al in the aluminum source is (1-10):(1-10):(0.2-5).
7. The preparation method of modified hopcalite catalyst according to claim 6, characterized in that the ratio of the amount of Cu in said copper source, the amount of Mn in said manganese source, and the amount of Al in said aluminum source is 5:1:(0.2-1).
8. The preparation method of modified hopcalite catalyst according to claim 7, characterized in that the ratio of the amount of Cu in said copper source, the amount of Mn in said manganese source, and the amount of Al in said aluminum source is 5:1:(0.5-1).
9. The method for preparing a modified hopcalite catalyst according to any one of claims 1 to 5, characterized in that the roasting temperature is 300 to 500°C and the roasting time is 6 to 10 hours.
10. The preparation method of modified hopcalite catalyst according to any one of 1 to 5, characterized in that the alkaline conditions include pH=8-9, using alkali as precipitant, and the concentration of alkali is 1-3 mol / L.
11. 6. A method for preparing the modified hopcalite catalyst according to any one of 1 to 5, characterized in that the mixed solution is co-precipitated under alkaline conditions at 15 to 20°C.
12. 6. A method for preparing a modified hopcalite catalyst according to any one of 1 to 5, characterized in that the mixed solution is co-precipitated under alkaline conditions and allowed to stand for 10 to 20 hours to obtain the precipitate.
13. A modified hopcalite catalyst prepared by the method according to any one of claims 1 to 12.
14. Application of the modified hopcalite catalyst of claim 13 in catalytic combustion of CO.
Citation Information
Patent Citations
Preparing method of copper-series low-temperature conversion catalyst
CN109621967A
Production of gas purification catalyst
JP1978116290A
Exhaust gas purification catalyst
WO2018123862A1