Surface coating layer for drones and manufacturing method thereof, and drone

The surface coating layer on drones, comprising an adhesive, antioxidant, and heat-insulating layers, addresses low-temperature resistance and oxidation issues, enhancing their performance in firefighting by providing thermal protection and directional fire extinguishing capabilities.

JP2024540807AActive Publication Date: 2024-11-06KUNMING UNIV OF SCI & TECH
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
JP2024518262
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2021-11-19
Filing Date
2022-10-08
Publication Date
2024-11-06
Estimated Expiration
2042-10-08

AI Technical Summary

Technical Problem

Conventional drones used for firefighting face challenges with low-temperature resistance, oxidation issues, and inadequate directional fire extinguishing capabilities, especially in high-temperature environments like forest fires, limiting their effectiveness in extinguishing fires from a distance.

Method used

A surface coating layer for drones comprising an adhesive layer, antioxidant layer, oxygen transmission barrier layer, and heat-insulating temperature-lowering layer, made from lightweight materials like resin and ceramic composites, enhances high-temperature resistance and fire extinguishing capabilities.

Benefits of technology

The coating layer provides improved thermal protection and oxidation resistance, allowing drones to operate effectively in high-temperature environments and accurately extinguish fires from a distance, extending their operational lifespan.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024540807000001_ABST
    Figure 2024540807000001_ABST
Patent Text Reader

Abstract

This application provides a surface coating layer for a drone and a manufacturing method thereof, and a drone, the coating layer includes at least an adhesive layer, an anti-oxidation layer, an oxygen transmission barrier layer, and a heat insulating temperature reducing layer, the coating layer is manufactured on the surface of the drone body, or the surface of the drone body is covered by a composite material substrate, the drone body is manufactured from a lightweight material, the composite material substrate includes a resin-based composite material substrate and a ceramic-based composite material substrate, the adhesive layer has a thickness of 20-200 μm, the oxygen transmission barrier layer has a thickness of 20-100 μm, and the heat insulating temperature reducing layer has a thickness of 80-1000 μm. In this application, the extremely low thermal conductivity, high reflectance, and extremely strong oxygen transmission barrier properties of the materials of each layer in the coating layer are combined to provide the drone body with oxidation resistance, improve the operating temperature of the drone, and ensure that it can be used for fire rescue and can be used for a long time.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to the technical field of material application, and in particular to a surface coating layer for a drone and a manufacturing method thereof, and a drone. [Background technology]

[0002] With in-depth research and application of unmanned aerial vehicles, their maximum takeoff weight has now reached more than 10 tons. Low-altitude unmanned aerial vehicles can be used at fire rescue sites to carry out tasks such as firefighting, personnel rescue, communication connection and material transportation, which can effectively reduce the risks posed by traditional pilots when carrying out missions. In addition, low-altitude unmanned aerial vehicles are small in volume and easy to operate when carrying out fire rescue in cities, and there are fewer restrictions on takeoff locations, making them more suited to modern development trends. However, in order to effectively reduce the weight of the aircraft itself and increase the amount of material it can carry, in the prior art, low-altitude aircraft fuselages are usually manufactured using different types of resin-based composite materials or ceramic-based composite materials. Resin-based composite materials have problems such as a low melting point, poor high-temperature resistance, and being prone to failure due to corrosion caused by smoke at the fire site, which limits their application at the site of large-scale fires and high-temperature fires. Ceramic-based composite materials, such as silicon carbide fiber reinforced silicon carbide, carbon fiber reinforced carbon, carbon fiber reinforced silicon carbide, and silicon carbide fiber reinforced carbon ceramic composite materials, have a melting point of over 2000°C and have advantages such as low density, high plasticity, and high specific strength similar to resin-based composite materials, but have the disadvantage of being oxidized when exposed to air at high temperatures, causing failure.

[0003] In addition, in recent years, fires have frequently broken out in forest and grassland areas in the southwestern region of China, and the fires are fierce and develop rapidly, causing serious losses in areas where fires have occurred over a large area. Conventional fire extinguishers have a remarkable effect on fires at close range or with small fire sources, but generally cannot be effective against fires that are strong and distant. Conventional fire extinguishing drones do not have a strong directional extinguishing ability at the fire site, and cannot efficiently extinguish fires at long distances from the fire site. Summary of the Invention [Problem to be solved by the invention]

[0004] In view of the above problems in the prior art, the present invention provides a surface coating layer for a drone, a manufacturing method thereof, and a drone, mainly to solve the problems of the poor high-temperature resistance and poor ability to accurately extinguish fires at long distances of the conventional drones. [Means for solving the problem]

[0005] In order to achieve the above and other objects, the present invention employs the following technical means.

[0006] The surface coating layer for the drone includes at least an adhesive layer, an anti-oxidation layer, an oxygen transmission barrier layer, and a heat insulating and cooling layer; Manufactured on the surface of a drone body or covered by a composite material substrate; The drone body is constructed of lightweight materials; The composite material substrate includes a resin-based composite material substrate and a ceramic-based composite material substrate, the adhesive layer has a thickness of 20 to 200 μm, the oxygen transmission barrier layer has a thickness of 20 to 100 μm, and the heat insulating temperature reducing layer has a thickness of 80 to 1000 μm.

[0007] Preferably, the resin-based composite substrate is a fiber-reinforced material based on an organic polymer, the fiber-reinforced material being one of glass fiber, carbon fiber, basalt fiber and aramid.

[0008] Preferably, the ceramic composite substrate is one of silicon carbide fiber reinforced silicon carbide, carbon fiber reinforced carbon, carbon fiber reinforced silicon carbide, and silicon carbide fiber reinforced carbon.

[0009] Preferably, the lightweight material is at least one selected from a carbon fiber braid, a titanium alloy, and an aluminum alloy, and the internal parts of the drone and the lightweight material are bonded together by ethylene propylene rubber.

[0010] Preferably, the raw material of the adhesive layer is a material having a thermal expansion coefficient close to that of the lightweight material, and is at least one selected from aluminum, iron, magnesium, calcium, silicon, tantalum, vanadium, yttrium, zirconium, hafnium, niobium, molybdenum and tungsten.

[0011] Preferably, a thermal expansion coefficient buffer layer having a thickness of 30 to 50 μm is further provided between the oxygen transmission blocking layer and the thermal insulation temperature reducing layer of the ceramic composite material substrate.

[0012] Preferably, the oxygen transmission barrier layer has a thermal expansion coefficient of 3×10 -6 K -1 ~6×10 -6 K -1 and the thermal expansion coefficient of the thermal expansion coefficient buffer layer is between 6×10 -6 K -1 ~9×10 -6 K -1 The thermal expansion coefficient of the adiabatic cooling layer is between 9×10 -6 K -1 ~11×10 -6 K -1 It is between.

[0013] Preferably, the thermal expansion coefficient buffer layer is a RETa3O9 ceramic, where RE is one or more of rare earth elements.

[0014] Preferably, the anti-oxidation layer is a mixture of one or more of Al2O3, SiO2, Ta2O5, Nb2O5, ZrO2, Mo2O5 and WO3.

[0015] Preferably, the oxygen transmission barrier layer is a rare earth tantalate ceramic material or a rare earth tantalum / niobate ceramic material.

[0016] Preferably, the rare earth tantalate ceramic material is ATaO4 spherical powder, where A is Al, Fe or a rare earth element; The rare earth tantalum / niobate ceramic material is RETa 1-x Nb x O4 ceramic material, where RE is one or more of the rare earth elements, 0 <x<1である。

[0017] Preferably, the thermal insulating temperature reducing layer is a rare earth niobate ceramic material, a rare earth tantalate ceramic material or a rare earth tantalum / niobate ceramic material.

[0018] Preferably, the rare earth niobate ceramic material is RE3NbO7 spherical powder; the rare earth tantalate ceramic material is a RE3TaO7 ceramic; The rare earth tantalum / niobate ceramic material is RE3Ta 1-y Nb y O7, RE is one or more of the rare earth elements, 0 <y<1である。

[0019] According to the present application: Producing and forming an adhesive layer on the upper surface of a ceramic composite substrate by a low-temperature thermal spraying method, or producing and forming an adhesive layer on the upper surface of a resin composite substrate or a drone body by an electron beam physical vapor deposition method; placing the adhesive layer in air to oxidize it and form an oxidation prevention layer; forming an oxygen transmission barrier layer on the surface of the oxidation prevention layer by an atmospheric plasma spraying method; and forming a heat insulating layer on the surface of the oxygen transport barrier layer by an atmospheric plasma spraying method.

[0020] Preferably, the step of forming a thermal insulating temperature reducing layer on the surface of the oxygen transport barrier layer of the ceramic composite substrate by an atmospheric plasma spraying method includes: forming a thermal expansion coefficient buffer layer on the surface of the oxygen transport barrier layer by an atmospheric plasma spraying method; and forming the heat insulating temperature reducing layer on the surface of the thermal expansion coefficient buffer layer by an atmospheric plasma spraying method.

[0021] Preferably, the process parameters of the low temperature spraying method include: compressed nitrogen gas as working gas, spraying pressure as 0.66 MPa, spraying distance as 30 mm, spraying temperature as 800° C., and powder feed rate as 40 g / min; The process parameters of the atmospheric plasma spraying method include: power of the spray gun is 30-50 kW, distance of the spray gun is 80-160 mm, gas flow rate of argon gas is 3-10 slpm, gas flow rate of hydrogen gas is 3-10 slpm, supply rate is 30-50 g / min, speed of the spray gun is 80-300 mm / s, and spraying time is 1-20 min.

[0022] Preferably, the process parameters of the electron beam physical vapor deposition method are as follows: during the deposition process, the substrate temperature is 300 to 500° C., the target-substrate distance is 200 to 400 mm, the incidence angle is 30° to 50°, the electron acceleration voltage is 20 to 30 kV, and the vacuum degree is 5×10 -3 The pressure in the vacuum chamber is less than 10 Pa, and the deposition rate is 50 to 150 nm / min. The substrate includes a ceramic composite substrate, a resin composite substrate, or a drone body.

[0023] Preferably, the step of placing the adhesive layer in air to oxidize it and form an oxidation prevention layer includes: The method includes a step of placing the adhesive layer in air, heating it to oxidize it, and forming an oxidation-resistant layer, in which the heating temperature is 30 to 300° C. and the thickness of the oxidation-resistant layer is 20 μm or less.

[0024] According to the present application, there is provided a drone including a drone body, a central control module, and an information acquisition module, a temperature detection module, a pressure control module, a drone module, and a high-efficiency firefighting module, each of which is connected to the central control module, The information acquisition module acquires information related to a target extinguishing point to form a first data set, and transmits the first data set to the central control module; The temperature detection module collects temperature distribution conditions in the fire scene to form a second data set, and sends the second data set to the central control module; The pressure control module monitors the pressure state of the high-efficiency fire extinguishing device and controls the high-efficiency fire extinguishing device in real time; The drone module includes a remote controller, an aircraft power control device, and a fire extinguishing drone, the remote controller controls the fire extinguishing drone to perform the fire extinguishing mission transmitted from the central control module, the aircraft power control device provides flight power to the fire extinguishing drone, and the fire extinguishing drone performs the fire extinguishing mission to extinguish a target fire location; The high-efficiency fire-fighting module includes the high-efficiency fire-extinguishing device and a helmet, the high-efficiency fire-extinguishing device is loaded with extinguishing material to extinguish a fire at a fire site, and the helmet protects the high-efficiency fire-extinguishing device; The central control module includes a data storage unit, a mission issuing unit, and an analysis processing unit, the data storage unit stores the first data set and the second data set, the mission issuing unit issues a fire extinguishing mission to the drone module based on the first data set, the analysis processing unit analyzes and processes the second data set to obtain an analysis result on the location information of the fire source and the point before the fire spreads, and then extinguishes the fire according to a predetermined fire extinguishing strategy; The drone body is manufactured from a lightweight material, and the lightweight material is coated with a coating layer; The coating layer includes at least an adhesive layer, an anti-oxidation layer, an oxygen transmission barrier layer, and a heat insulating and temperature reducing layer; The coating layer is manufactured on the surface of the drone body or is covered on the surface of the drone body by a composite material substrate; The composite substrate includes a resin-based composite substrate and a ceramic-based composite substrate, and the adhesive layer has a thickness of 20 to 200 μm, the oxygen transmission barrier layer has a thickness of 20 to 100 μm, and the heat insulating temperature reducing layer has a thickness of 80 to 1000 μm.

[0025] Preferably, the predetermined extinguishing strategy comprises: Use the temperature detection module to collect the temperature distribution situation of the target extinguishing point, and analyze the specific location information of the fire source and the point before the fire spreads; The pressure control module is used to control the high-efficiency fire fighting module to perform directional extinguishing, which includes first extinguishing the point before the fire spreads, and then extinguishing the source of the fire.

[0026] Preferably, analyzing and processing the second data set to obtain analysis results regarding the fire source and the points before the fire spreads involves obtaining a temperature change graph based on the temperature detection situation, combining with the Beidou positioning system to obtain detailed on-site temperature distribution situation, and finding the specific locations of the fire source and the points before the fire spreads.

[0027] Preferably, the drone body includes a load-bearing panel for mounting the drone aircraft, a stable holder for protecting the safety of the fire extinguisher, a balance stabilizer for maintaining the drone aircraft in a balanced and stable state, and an aircraft propeller for providing the drone aircraft with a flight lift force.

[0028] Preferably, the aircraft propeller is made of woven carbon fibre.

[0029] Preferably, the relevant information includes fire start time, fire location, fire type and fire prediction grade.

[0030] Preferably, the extinguishing material is a highly efficient compressible extinguishing foam.

[0031] Preferably, the highly efficient compressible foam extinguishing agent is non-toxic and harmless, and the reactants obtained by reacting with the combustion material are also non-toxic and harmless substances.

[0032] Preferably, the helmet includes an inner layer made from a fire-resistant, explosion-proof polymeric material and an outer layer made from an erosion-resistant material.

[0033] Preferably, the drone further includes a display module for displaying a fire extinguishing scene screen and the remaining power amount of the fire extinguishing drone in real time. Effect of the Invention

[0034] As described above, the surface coating layer for a drone and the manufacturing method thereof, as well as the drone of the present application, have the following beneficial effects.

[0035] In this application, a drone body is manufactured using a lightweight material, and a coating layer is coated on the body. The coating layer includes at least an adhesive layer, an anti-oxidation layer, an oxygen transmission barrier layer, and an insulating temperature-reducing layer, thereby providing the drone with the effects of insulating temperature-reducing, oxygen transmission-blocking, and anti-oxidation, and effectively improving the limit operating temperature and oxidation resistance of the lightweight material, allowing the drone to be used in high-temperature, highly corrosive environments such as fire rescue, enabling low-altitude flight, and extending its service life. When the above-mentioned coating layer is used as a material for the body of a fire rescue drone, due to the advantages of its low thermal conductivity and multi-layer structure improving the effect of insulating temperature-reducing, it can ensure that the internal parts of the aircraft are below their limit operating temperature in the usage environment of a fire scene, so that it can be used effectively for a long period of time. [Brief description of the drawings]

[0036] [Figure 1] 1 is a schematic diagram of a surface coating layer for a drone in one embodiment of the present application. FIG. [Diagram 2] This is a microstructure diagram of a surface coating layer for a drone in one embodiment of the present application after being heated at 800°C. [Diagram 3] FIG. 2 is a schematic diagram of a surface coating layer for a drone in another embodiment of the present application. [Figure 4]FIG. 2 is a schematic diagram of a surface coating layer for a drone in another embodiment of the present application. [Diagram 5] FIG. 1 is a system schematic diagram of a drone in one embodiment of the present application. [Figure 6] FIG. 1 is a schematic diagram of a drone module in one embodiment of the present application. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0037] Hereinafter, the embodiments of the present invention will be described with reference to specific examples, but those skilled in the art can easily understand other advantages and effects of the present invention from the contents disclosed in this specification. The present invention may be implemented or applied in other different specific embodiments, and various modifications or changes may be made to each detail in this specification based on different perspectives and applications without departing from the spirit of the present invention. In addition, the following examples and features in the examples may be combined with each other as long as they are not inconsistent.

[0038] It should be noted that the drawings provided in the following examples are merely for illustrative purposes of explaining the basic concept of the present invention, and the drawings are not drawn according to the number, shape and dimensions of components when actually implemented, but only components related to the present invention are shown, and the shape, number and ratio of each component when actually implemented can be changed arbitrarily, and the layout form of the components can also become more complex.

[0039] Example 1 In this application, a surface coating layer for a drone and a manufacturing method thereof are presented. As shown in FIG. 1, in the embodiment of this application, the surface coating layer for a drone is covered on the surface of the drone body by a resin-based composite material substrate, and the resin-based composite material substrate is a fiber-reinforced material based on an organic polymer, and glass fiber is used as the reinforcing fiber. An adhesive layer having a thickness of 30 μm, an oxygen transmission barrier layer having a thickness of 50 μm, and an insulating temperature-reducing layer having a thickness of 1000 μm are sequentially manufactured on the resin-based composite material substrate, and silicon (Si) is used as the adhesive layer, LuTa is used as the oxygen transmission barrier layer, and LuTa is used as the oxygen transmission barrier layer. 0.5 Nb 0.5O4 was used, and Lu3Ta was used as the adiabatic cooling layer. 0.3 Nb 0.7 An O7 ceramic coating layer was used.

[0040] Specifically, (1) a silicon (Si) adhesive layer with a thickness of 30 μm is manufactured on the surface of a glass fiber substrate by electron beam physical vapor deposition. In the electron beam physical vapor deposition process, the silicon (Si) of the adhesive layer is used as a target to deposit an adhesive layer on the upper surface of the glass fiber substrate. The temperature of the glass fiber substrate is 350°C, the target-substrate distance is 300 mm, the incidence angle is 30°, the electron acceleration voltage is 20 kV, and the vacuum degree is 2 × 10 -3 The pressure was less than 1 Pa and the deposition rate was 100 nm / min.

[0041] (2) The silicon (Si) adhesion layer is oxidized in air to obtain a SiO2 oxidation prevention layer with a thickness of less than 1 μm, and then a 50 μm-thick oxygen transmission barrier layer LuTa is applied to the surface of the oxidation prevention layer by atmospheric plasma spraying. 0.5 Nb 0.5 First, the raw materials Lu2O3, Nb2O5 and Ta2O5 were used to prepare spherical LuTaO4 ceramic layers by high-temperature solid-state method. 0.5 Nb 0.5 The O4 spherical powder was produced and sprayed onto LuTa by atmospheric plasma spraying using a spray gun. 0.5 Nb 0.5 In the process of spraying the O4 spherical powder, argon gas was used as the protective gas and hydrogen gas was used as the combustion gas, the power of the spray gun was 45 kW, the distance of the spray gun was 130 mm, the gas flow rates of the argon gas and hydrogen gas were 45 / 12 slpm and 40 / 10 slpm, respectively, the supply speed was 60 g / min, the speed of the spray gun was 200 mm / s, and the spraying time was 2 min.

[0042] (3) LuTa using atmospheric plasma spraying 0.5 Nb 0.5 Lu3Ta is a reflective thermal insulation layer with a thickness of 1000 micrometers on the surface of the O4 ceramic oxygen transmission barrier layer. 0.3 Nb 0.7The O7 ceramic coating layer was produced by using Lu2O3, Nb2O5 and Ta2O5 as raw materials and forming spherical Lu3Ta by high-temperature solid-state method. 0.3 Nb 0.7 O7 spherical powder was produced and sprayed onto Lu3Ta by atmospheric plasma spraying using a spray gun. 0.3 Nb 0.7 In the process of spraying the O7 spherical powder, argon gas was used as the protective gas and hydrogen gas was used as the combustion gas, the power of the spray gun was 43 kW, the distance of the spray gun was 140 mm, the gas flow rates of the argon gas and hydrogen gas were 42 / 12 slpm and 45 / 15 slpm respectively, the supply rate was 50 g / min, the speed of the spray gun was 100 mm / s, and the spraying time was 20 min.

[0043] Example 2 In this application, a surface coating layer for a drone and a manufacturing method thereof are presented. As shown in FIG. 1, in the embodiment of this application, the surface coating layer for a drone is covered on the surface of the drone body by a resin-based composite material substrate, and the resin-based composite material substrate is a fiber-reinforced material based on an organic polymer, and carbon fiber is used as the reinforcing fiber. In the resin-based composite material substrate, an adhesive layer having a thickness of 100 μm, an oxygen transmission barrier layer having a thickness of 75 μm, and an insulating temperature-reducing layer having a thickness of 100 μm are sequentially manufactured, and aluminum is used as the adhesive layer, and Tm 1 / 4 Yb 1 / 4 Lu 1 / 4 Sc 1 / 4 Ta 0.8 Nb 0.2 O4 was used, and Y3Ta was used as the adiabatic cooling layer. 0.5 Nb 0.5 An O7 ceramic coating layer was used.

[0044] Specifically, (1) an aluminum adhesive layer with a thickness of 100 μm is manufactured on the surface of a glass fiber substrate by electron beam physical vapor deposition. In the electron beam physical vapor deposition process, the aluminum of the adhesive layer is used as a target to deposit the adhesive layer on the upper surface of the substrate. The temperature of the substrate is 350°C, the target-substrate distance is 300 mm, the incidence angle is 30°, the electron acceleration voltage is 20 kV, and the vacuum degree is 2 × 10-3 The pressure was less than 1 Pa and the deposition rate was 100 nm / min.

[0045] (2) The aluminum adhesive layer is oxidized in air to obtain an Al2O3 oxidation prevention layer with a thickness of less than 1 μm, and then an oxygen transmission barrier layer Tm with a thickness of 75 μm is formed on the surface of the oxidation prevention layer by atmospheric plasma spraying. 1 / 4 Yb 1 / 4 Lu 1 / 4 Sc 1 / 4 Ta 0.8 Nb 0.2 The O4 ceramic layer was first fabricated using Sc2O3, Tm2O3, Yb2O3, Lu2O3, Nb2O5 and Ta2O5 as raw materials, and spherical Tm 1 / 4 Yb 1 / 4 Lu 1 / 4 Sc 1 / 4 Ta 0.8 Nb 0.2 O4 spherical powder was produced and sprayed with an air plasma spraying gun to produce Tm 1 / 4 Yb 1 / 4 Lu 1 / 4 Sc 1 / 4 Ta 0.8 Nb 0.2 In the process of spraying the O4 spherical powder, argon gas was used as the protective gas and hydrogen gas was used as the combustion gas, the power of the spray gun was 45 kW, the distance of the spray gun was 130 mm, the gas flow rates of the argon gas and hydrogen gas were 45 / 12 slpm and 40 / 10 slpm, respectively, the supply speed was 60 g / min, the speed of the spray gun was 200 mm / s, and the spraying time was 20 min.

[0046] (3) Atmospheric plasma spraying method 1 / 4 Yb 1 / 4 Lu 1 / 4 Sc 1 / 4 Ta 0.8 Nb 0.2 A reflective thermal insulation layer, Y3Ta, 100 micrometers thick, is applied to the surface of the O4 ceramic oxygen barrier layer. 0.5 Nb 0.5 The O7 ceramic coating layer was produced by using Y2O3, Nb2O5 and Ta2O5 as raw materials and producing spherical Y3Ta by high-temperature solid-state method. 0.5Nb 0.5 O7 spherical powder was produced and sprayed onto Lu3Ta by atmospheric plasma spraying using a spray gun. 0.3 Nb 0.7 In the process of spraying the O7 spherical powder, argon gas was used as the protective gas and hydrogen gas was used as the combustion gas, the power of the spray gun was 43 kW, the distance of the spray gun was 140 mm, the gas flow rates of the argon gas and hydrogen gas were 42 / 12 slpm and 45 / 15 slpm respectively, the supply rate was 50 g / min, the speed of the spray gun was 100 mm / s, and the spraying time was 2 min.

[0047] Example 3 In this application, a surface coating layer for a drone and a manufacturing method thereof are presented. As shown in FIG. 1, in the embodiment of this application, the surface coating layer for a drone is covered on the surface of the drone body by a resin-based composite material substrate, and the resin-based composite material substrate is a fiber-reinforced material based on an organic polymer, and basalt fiber is used as the reinforcing fiber. An adhesive layer having a thickness of 50 μm, an oxygen transmission barrier layer having a thickness of 80 μm, and an insulating temperature-reducing layer having a thickness of 600 μm are sequentially manufactured on the resin-based composite material substrate, and a tantalum-niobium-molybdenum alloy is used as the adhesive layer, and a YTa 0.5 Nb 0.5 O4 was used, and YGdDyTa 0.5 Nb 0.5 An O7 ceramic coating layer was used.

[0048] Specifically, (1) a tantalum-niobium-molybdenum alloy adhesive layer with a thickness of 50 μm is manufactured on the surface of a glass fiber substrate by electron beam physical vapor deposition. In the electron beam physical vapor deposition process, the tantalum-niobium-molybdenum alloy of the adhesive layer is used as a target to deposit the adhesive layer on the upper surface of the substrate. The substrate temperature is 350°C, the target-substrate distance is 300 mm, the incidence angle is 30°, the electron acceleration voltage is 20 kV, and the vacuum degree is 2×10 -3 The pressure was less than 1 Pa and the deposition rate was 100 nm / min.

[0049] (2) Oxidizing the tantalum-niobium-molybdenum alloy adhesive layer in air to obtain a corresponding oxide oxidation prevention layer with a thickness of less than 1 μm, and then forming an oxygen transmission barrier layer YTa 0.5 Nb 0.5 The O4 ceramic layer was first fabricated using Y2O3, Nb2O5 and Ta2O5 as raw materials and spherical YTa 0.5 Nb 0.5 O4 spherical powder was produced and sprayed with YTa by air plasma spraying using a spray gun. 0.5 Nb 0.5 In the process of spraying the O4 spherical powder, argon gas was used as the protective gas and hydrogen gas was used as the combustion gas, the power of the spray gun was 45 kW, the distance of the spray gun was 130 mm, the gas flow rates of the argon gas and hydrogen gas were 45 / 12 slpm and 40 / 10 slpm, respectively, the supply speed was 60 g / min, the speed of the spray gun was 200 mm / s, and the spraying time was 2 min.

[0050] (3) YTa by atmospheric plasma spraying 0.5 Nb 0.5 A 600 micrometer thick reflective thermal insulation layer of YGdDyTa is applied to the surface of the O4 ceramic oxygen transmission barrier. 0.5 Nb 0.5 The O7 ceramic coating layer was produced by using Dy2O3, Gd2O3, Y2O3, Nb2O5 and Ta2O5 as raw materials to produce spherical YGdDyTa by high-temperature solid-state method. 0.5 Nb 0.5 O7 spherical powder was produced and sprayed with YGdDyTa by air plasma spraying using a spray gun. 0.5 Nb 0.5 In the process of spraying the O7 spherical powder, argon gas was used as the protective gas and hydrogen gas was used as the combustion gas, the power of the spray gun was 43 kW, the distance of the spray gun was 140 mm, the gas flow rates of the argon gas and hydrogen gas were 42 / 12 slpm and 45 / 15 slpm respectively, the supply rate was 50 g / min, the speed of the spray gun was 100 mm / s, and the spraying time was 12 min.

[0051] Example 4 In this application, a surface coating layer for a drone and a manufacturing method thereof are presented. As shown in FIG. 1, in the embodiment of this application, the surface coating layer for a drone is covered on the surface of the drone body by a resin-based composite material substrate, and the resin-based composite material substrate is a fiber-reinforced material based on an organic polymer, and aramid is used as the reinforcing fiber. In the resin-based composite material substrate, an adhesive layer having a thickness of 60 μm, an oxygen transmission barrier layer having a thickness of 60 μm, and an insulating temperature-reducing layer having a thickness of 720 μm are sequentially manufactured, and the adhesive layer is made of zirconium-silicon alloy, and the oxygen transmission barrier layer is made of SmTa. 0.2 Nb 0.8 O4 was used, and SmEuGdTa 0.2 Nb 0.8 An O7 ceramic coating layer was used.

[0052] Specifically, (1) a zirconium-silicon alloy adhesive layer with a thickness of 50 μm is produced on the surface of a glass fiber substrate by electron beam physical vapor deposition. In the electron beam physical vapor deposition process, a zirconium-silicon alloy is used as a target to deposit an adhesive layer on the upper surface of the substrate. The substrate temperature is 350°C, the target-substrate distance is 300 mm, the incidence angle is 30°, the electron acceleration voltage is 20 kV, and the vacuum degree is 2 × 10 -3 The pressure was less than 1 Pa and the deposition rate was 100 nm / min.

[0053] (2) Oxidizing the zirconium-silicon alloy adhesive layer in air to obtain a corresponding oxide oxidation prevention layer with a thickness of less than 1 μm, and then spraying an oxygen transmission barrier layer SmTa with a thickness of 60 μm on the surface of the oxidation prevention layer by atmospheric plasma spraying. 0.2 Nb 0.8 The O4 ceramic layer was first fabricated using Sm2O3, Nb2O5 and Ta2O5 as raw materials and spherical SmTa 0.2 Nb 0.8 O4 spherical powder was produced and sprayed with SmTa by air plasma spraying using a spray gun. 0.2 Nb 0.8In the process of spraying the O4 spherical powder, argon gas was used as the protective gas and hydrogen gas was used as the combustion gas, the power of the spray gun was 45 kW, the distance of the spray gun was 130 mm, the gas flow rates of the argon gas and hydrogen gas were 45 / 12 slpm and 40 / 10 slpm, respectively, the supply speed was 60 g / min, the speed of the spray gun was 200 mm / s, and the spraying time was 2 min.

[0054] (3) SmEuGdTa by atmospheric plasma spraying 0.2 Nb 0.8 A 720 micrometer thick reflective thermal insulation layer of SmEuGdTa is applied to the surface of the O7 ceramic oxygen barrier layer. 0.2 Nb 0.8 The O7 ceramic coating layer was produced by using Sm2O3, Gd2O3, Eu2O3, Nb2O5 and Ta2O5 as raw materials to produce spherical SmEuGdTa 0.2 Nb 0.8 O7 spherical powder was produced and sprayed with SmEuGdTa by air plasma spraying using a spray gun. 0.2 Nb 0.8 In the process of spraying the O7 spherical powder, argon gas was used as the protective gas and hydrogen gas was used as the combustion gas, the power of the spray gun was 43 kW, the distance of the spray gun was 140 mm, the gas flow rates of the argon gas and hydrogen gas were 42 / 12 slpm and 45 / 15 slpm respectively, the supply rate was 50 g / min, the speed of the spray gun was 100 mm / s, and the spraying time was 15 min.

[0055] Example 5 In this application, a surface coating layer for a drone and a manufacturing method thereof are presented. As shown in FIG. 1, in the embodiment of this application, the surface coating layer for a drone is covered on the surface of the drone body by a resin-based composite material substrate, and the resin-based composite material substrate is a fiber-reinforced material based on an organic polymer, and glass fiber is used as the reinforcing fiber. An adhesive layer having a thickness of 30 μm, an oxygen transmission barrier layer having a thickness of 50 μm, and an insulating temperature-reducing layer having a thickness of 500 μm are sequentially manufactured on the resin-based composite material substrate, and silicon (Si) is used as the adhesive layer, LuTa is used as the oxygen transmission barrier layer, and LuTa is used as the oxygen transmission barrier layer.0.5 Nb 0.5 O4 was used, and Lu3Ta was used as the adiabatic cooling layer. 0.3 Nb 0.7 An O7 ceramic coating layer was used.

[0056] Specifically, (1) a silicon (Si) adhesive layer with a thickness of 30 μm is manufactured on the surface of a glass fiber substrate by electron beam physical vapor deposition. In the electron beam physical vapor deposition process, the silicon (Si) of the adhesive layer is used as a target to deposit an adhesive layer on the upper surface of the glass fiber substrate. The temperature of the glass fiber substrate is 350°C, the target-substrate distance is 300 mm, the incidence angle is 30°, the electron acceleration voltage is 20 kV, and the vacuum degree is 2 × 10 -3 The pressure was less than 1 Pa and the deposition rate was 100 nm / min.

[0057] (2) The silicon (Si) adhesion layer is oxidized in air to obtain a SiO2 oxidation prevention layer with a thickness of less than 1 μm, and then a 50 μm-thick oxygen transmission barrier layer LuTa is applied to the surface of the oxidation prevention layer by atmospheric plasma spraying. 0.5 Nb 0.5 First, the raw materials Lu2O3, Nb2O5 and Ta2O5 were used to prepare spherical LuTaO4 ceramic layers by high-temperature solid-state method. 0.5 Nb 0.5 The O4 spherical powder was produced and sprayed onto LuTa by atmospheric plasma spraying using a spray gun. 0.5 Nb 0.5 In the process of spraying the O4 spherical powder, argon gas was used as the protective gas and hydrogen gas was used as the combustion gas, the power of the spray gun was 45 kW, the distance of the spray gun was 130 mm, the gas flow rates of the argon gas and hydrogen gas were 45 / 12 slpm and 40 / 10 slpm, respectively, the supply speed was 60 g / min, the speed of the spray gun was 200 mm / s, and the spraying time was 2 min.

[0058] (3) LuTa using atmospheric plasma spraying 0.5 Nb 0.5 Lu3Ta is a 500 micrometer thick reflective thermal insulation layer on the surface of the O4 ceramic oxygen barrier layer. 0.3 Nb 0.7The O7 ceramic coating layer was produced by using Lu2O3, Nb2O5 and Ta2O5 as raw materials and forming spherical Lu3Ta by high-temperature solid-state method. 0.3 Nb 0.7 O7 spherical powder was produced and sprayed onto Lu3Ta by atmospheric plasma spraying using a spray gun. 0.3 Nb 0.7 In the process of spraying the O7 spherical powder, argon gas was used as the protective gas and hydrogen gas was used as the combustion gas, the power of the spray gun was 43 kW, the distance of the spray gun was 140 mm, the gas flow rates of the argon gas and hydrogen gas were 42 / 12 slpm and 45 / 15 slpm respectively, the supply rate was 50 g / min, the speed of the spray gun was 100 mm / s, and the spraying time was 10 min.

[0059] Example 6 In this application, a surface coating layer for a drone and a manufacturing method thereof are presented. As shown in FIG. 1, in the embodiment of this application, the surface coating layer for a drone is covered on the surface of the drone body by a resin-based composite material substrate, and the resin-based composite material substrate is a fiber-reinforced material based on an organic polymer, and carbon fiber is used as the reinforcing fiber. An adhesive layer having a thickness of 100 μm, an oxygen transmission barrier layer having a thickness of 75 μm, and an insulating temperature-reducing layer having a thickness of 500 μm are sequentially manufactured on the resin-based composite material substrate, and aluminum is used as the adhesive layer, and Tm 1 / 4 Yb 1 / 4 Lu 1 / 4 Sc 1 / 4 Ta 0.8 Nb 0.2 O4 was used, and Y3Ta was used as the adiabatic cooling layer. 0.5 Nb 0.5 An O7 ceramic coating layer was used.

[0060] Specifically, (1) an aluminum adhesive layer with a thickness of 100 μm is manufactured on the surface of a glass fiber substrate by electron beam physical vapor deposition. In the electron beam physical vapor deposition process, the aluminum of the adhesive layer is used as a target to deposit the adhesive layer on the upper surface of the substrate. The temperature of the substrate is 350°C, the target-substrate distance is 300 mm, the incidence angle is 30°, the electron acceleration voltage is 20 kV, and the vacuum degree is 2 × 10-3 The pressure was less than 1 Pa and the deposition rate was 100 nm / min.

[0061] (2) The aluminum adhesive layer is oxidized in air to obtain an Al2O3 oxidation prevention layer with a thickness of less than 1 μm, and then an oxygen transmission barrier layer Tm with a thickness of 75 μm is formed on the surface of the oxidation prevention layer by atmospheric plasma spraying. 1 / 4 Yb 1 / 4 Lu 1 / 4 Sc 1 / 4 Ta 0.8 Nb 0.2 The O4 ceramic layer was first fabricated using Sc2O3, Tm2O3, Yb2O3, Lu2O3, Nb2O5 and Ta2O5 as raw materials, and spherical Tm 1 / 4 Yb 1 / 4 Lu 1 / 4 Sc 1 / 4 Ta 0.8 Nb 0.2 O4 spherical powder was produced and sprayed with an air plasma spraying gun to produce Tm 1 / 4 Yb 1 / 4 Lu 1 / 4 Sc 1 / 4 Ta 0.8 Nb 0.2 In the process of spraying the O4 spherical powder, argon gas was used as the protective gas and hydrogen gas was used as the combustion gas, the power of the spray gun was 45 kW, the distance of the spray gun was 130 mm, the gas flow rates of the argon gas and hydrogen gas were 45 / 12 slpm and 40 / 10 slpm, respectively, the supply speed was 60 g / min, the speed of the spray gun was 200 mm / s, and the spraying time was 20 min.

[0062] (3) Atmospheric plasma spraying method 1 / 4 Yb 1 / 4 Lu 1 / 4 Sc 1 / 4 Ta 0.8 Nb 0.2 A 500 micrometer thick reflective thermal insulation layer, Y3Ta, is applied to the surface of the O4 ceramic oxygen barrier layer. 0.5 Nb 0.5 The O7 ceramic coating layer was produced by using Y2O3, Nb2O5 and Ta2O5 as raw materials and producing spherical Y3Ta by high-temperature solid-state method. 0.5Nb 0.5 O7 spherical powder was produced and sprayed onto Lu3Ta by atmospheric plasma spraying using a spray gun. 0.3 Nb 0.7 In the process of spraying the O7 spherical powder, argon gas was used as the protective gas and hydrogen gas was used as the combustion gas, the power of the spray gun was 43 kW, the distance of the spray gun was 140 mm, the gas flow rates of the argon gas and hydrogen gas were 42 / 12 slpm and 45 / 15 slpm respectively, the supply rate was 50 g / min, the speed of the spray gun was 100 mm / s, and the spraying time was 10 min.

[0063] Comparative Example 1 In this application, a surface coating layer for a drone and a manufacturing method thereof are presented. As shown in FIG. 1, in the embodiment of this application, the surface coating layer for a drone is covered on the surface of the drone body by a resin-based composite material substrate, and the resin-based composite material substrate is a fiber-reinforced material based on an organic polymer, and glass fiber is used as the reinforcing fiber. An adhesive layer having a thickness of 30 μm and an oxygen transmission barrier layer having a thickness of 50 μm are sequentially manufactured on the resin-based composite material substrate, and silicon (Si) is used as the adhesive layer and LuTa (LuTa) is used as the oxygen transmission barrier layer. 0.5 Nb 0.5 O4 was used.

[0064] Specifically, (1) a silicon (Si) adhesive layer with a thickness of 30 μm is manufactured on the surface of a glass fiber substrate by electron beam physical vapor deposition. In the electron beam physical vapor deposition process, the silicon (Si) of the adhesive layer is used as a target to deposit an adhesive layer on the upper surface of the glass fiber substrate. The temperature of the glass fiber substrate is 350°C, the target-substrate distance is 300 mm, the incidence angle is 30°, the electron acceleration voltage is 20 kV, and the vacuum degree is 2 × 10 -3 The pressure was less than 1 Pa and the deposition rate was 100 nm / min.

[0065] (2) The silicon (Si) adhesion layer is oxidized in air to obtain a SiO2 oxidation prevention layer with a thickness of less than 1 μm, and then a 50 μm-thick oxygen transmission barrier layer LuTa is applied to the surface of the oxidation prevention layer by atmospheric plasma spraying. 0.5 Nb 0.5First, the raw materials Lu2O3, Nb2O5 and Ta2O5 were used to prepare spherical LuTaO4 ceramic layers by high-temperature solid-state method. 0.5 Nb 0.5 The O4 spherical powder was produced and sprayed onto LuTa by atmospheric plasma spraying using a spray gun. 0.5 Nb 0.5 In the process of spraying the O4 spherical powder, argon gas was used as the protective gas and hydrogen gas was used as the combustion gas, the power of the spray gun was 45 kW, the distance of the spray gun was 130 mm, the gas flow rates of the argon gas and hydrogen gas were 45 / 12 slpm and 40 / 10 slpm, respectively, the supply speed was 60 g / min, the speed of the spray gun was 200 mm / s, and the spraying time was 2 min.

[0066] Comparative Example 2 In this application, a surface coating layer for a drone and a manufacturing method thereof are presented. As shown in FIG. 1, in the embodiment of this application, the surface coating layer for a drone is covered on the surface of the drone body by a resin-based composite material substrate, and the resin-based composite material substrate is a fiber-reinforced material based on an organic polymer, and carbon fiber is used as the reinforcing fiber. An oxygen transmission barrier layer having a thickness of 75 μm and an insulating temperature-reducing layer having a thickness of 500 μm are sequentially manufactured on the resin-based composite material substrate, aluminum is used as the adhesive layer, and Tm 1 / 4 Yb 1 / 4 Lu 1 / 4 Sc 1 / 4 Ta 0.8 Nb 0.2 O4 was used, and Y3Ta was used as the adiabatic cooling layer. 0.5 Nb 0.5 An O7 ceramic coating layer was used.

[0067] Specifically, (1) a 75-micrometer-thick oxygen transmission barrier layer, Tm 1 / 4 Yb 1 / 4 Lu 1 / 4 Sc 1 / 4 Ta 0.8 Nb 0.2The O4 ceramic layer was first fabricated using Sc2O3, Tm2O3, Yb2O3, Lu2O3, Nb2O5 and Ta2O5 as raw materials, and spherical Tm 1 / 4 Yb 1 / 4 Lu 1 / 4 Sc 1 / 4 Ta 0.8 Nb 0.2 O4 spherical powder was produced and sprayed with an air plasma spraying gun to produce Tm 1 / 4 Yb 1 / 4 Lu 1 / 4 Sc 1 / 4 Ta 0.8 Nb 0.2 In the process of spraying the O4 spherical powder, argon gas was used as the protective gas and hydrogen gas was used as the combustion gas, the power of the spray gun was 45 kW, the distance of the spray gun was 130 mm, the gas flow rates of the argon gas and hydrogen gas were 45 / 12 slpm and 40 / 10 slpm, respectively, the supply speed was 60 g / min, the speed of the spray gun was 200 mm / s, and the spraying time was 20 min.

[0068] (2) Atmospheric plasma spraying method 1 / 4 Yb 1 / 4 Lu 1 / 4 Sc 1 / 4 Ta 0.8 Nb 0.2 A 500 micrometer thick reflective thermal insulation layer, Y3Ta, is applied to the surface of the O4 ceramic oxygen barrier layer. 0.5 Nb 0.5 The O7 ceramic coating layer was produced by using Y2O3, Nb2O5 and Ta2O5 as raw materials and producing spherical Y3Ta by high-temperature solid-state method. 0.5 Nb 0.5 O7 spherical powder was produced and sprayed onto Lu3Ta by atmospheric plasma spraying using a spray gun. 0.3 Nb 0.7In the process of spraying the O7 spherical powder, argon gas was used as the protective gas and hydrogen gas was used as the combustion gas, the power of the spray gun was 43 kW, the distance of the spray gun was 140 mm, the gas flow rates of the argon gas and hydrogen gas were 42 / 12 slpm and 45 / 15 slpm respectively, the supply rate was 50 g / min, the speed of the spray gun was 100 mm / s, and the spraying time was 10 min.

[0069] The compositions of the material systems manufactured in the above Examples 1-6 and Comparative Examples 1-2 are shown in Table 1. The softening temperature and adiabatic temperature drop gradient of the materials were tested. The test process was to heat the surface of the material coating layer and test the temperature of the surface and the interface between the substrate and the coating layer. The softening temperature was the temperature at which the resin-based composite material softened and separated from the coating layer, and the adiabatic temperature drop gradient was the temperature difference between the surface and the interface of the coating layer when softened. The inherent softening temperatures of the glass fiber, carbon fiber, basalt fiber, and aramid-reinforced resin-based materials used in this application are 140°C, 145°C, 120°C, and 94°C, respectively.

[0070] [Table 1]

[0071] [Table 2]

[0072] As shown in Table 2, the gradient coating layers manufactured for different types of resin-based composite materials can improve their operating temperature by 100 to 600 ° C by providing excellent thermal insulation protection performance, while the comparative example material in which the gradient composite coating layer of the present application is not manufactured can improve a certain adiabatic temperature drop gradient, but the performance is obviously insufficient. In addition, in Comparative Example 2, when no adhesive layer was manufactured, the coating layer peeled off after the coating material underwent two thermal cycles, and the thermal cycle life of the other materials all exceeded 20 times. Figure 2 shows the microstructure diagram of the manufactured composite gradient coating layer after heating at 800 ° C. As shown in Figure 2, the layers are tightly bonded, which proves that the bonding strength of the coating layer is strong and there are no obvious cracks or pores.

[0073] Example 7 In the present invention, a surface coating layer for drones and its manufacturing method are presented. As shown in Fig. 3, in the embodiment of the present application, the surface coating layer for drones is covered on the surface of the drone body by a ceramic composite material substrate, and the ceramic composite material substrate is silicon carbide fiber reinforced silicon carbide. On the silicon carbide fiber reinforced silicon carbide substrate, a bonding layer with a thickness of 100 μm, an oxidation prevention layer with a thickness of less than 1 μm, an oxygen transmission barrier layer with a thickness of 30 μm, a thermal expansion coefficient buffer layer with a thickness of 30 μm and an adiabatic temperature reduction layer with a thickness of 100 μm are sequentially manufactured, and the material of the bonding layer is metal tantalum Ta, the oxygen transmission barrier layer is a rare earth tantalate RETaO4 ceramic material, RE is Yb, and the thermal expansion coefficient buffer layer is a RETa3O9 ceramic, RE is Tm.

[0074] Specifically, (1) a tantalum (Ta) adhesive layer with a thickness of 100 μm is produced on the upper surface of a silicon carbide fiber reinforced silicon carbide substrate by a low-temperature thermal spraying method. In the low-temperature thermal spraying process, compressed nitrogen gas is used as the working gas, the spraying pressure is 0.66 MPa, the spraying distance is 30 mm, the spraying temperature is 800°C, and the powder feed rate is 40 g / min. After the sprayed tantalum (Ta) adhesive layer material is placed in the air, the metallic tantalum is oxidized, and a dense tantalum oxide (Ta2O5) oxidation prevention layer with a thickness of less than 1 μm can be formed on the surface of the material.

[0075] (2) A 30-micrometer-thick oxygen transmission barrier layer, YbTaO4 ceramic material, was manufactured on the surface of a dense tantalum oxide Ta2O5 oxidation prevention layer by atmospheric plasma spraying. First, Yb2O3 and Ta2O5 were used as raw materials, and spherical YbTaO4 powder was manufactured by a high-temperature solid-phase method. In the process of spraying the oxygen transmission barrier layer by atmospheric plasma spraying, argon gas was used as the protective gas and hydrogen gas was used as the combustion gas. During spraying, the power of the spray gun was 42kW, the distance of the spray gun was 100mm, the gas flow rates of argon gas and hydrogen gas were 40 / 12slpm and 45 / 10slpm, respectively, the supply speed was 50g / min, the speed of the spray gun was 300mm / s, and the spraying time was 1min.

[0076] (3) A 30-micrometer-thick TmTa3O9 ceramic coating layer, which is a thermal expansion coefficient buffer layer, was manufactured on the surface of the YbTaO4 ceramic oxygen transmission barrier layer by the atmospheric plasma spraying method. First, Tm2O3 and Ta2O5 were used as raw materials, and spherical TmTa3O9 spherical powder was manufactured by the high-temperature solid-phase method. In the process of spraying the thermal expansion coefficient buffer layer by the atmospheric plasma spraying method, argon gas was used as the protective gas, hydrogen gas was used as the combustion gas, the power of the spray gun was 46kW, the distance of the spray gun was 150mm, the gas flow rates of argon gas and hydrogen gas were 42 / 12slpm and 40 / 10slpm, respectively, the supply speed was 30g / min, the speed of the spray gun was 300mm / s, and the spraying time was 2min.

[0077] (4) A 200-micrometer-thick thermal insulation cooling ceramic layer, Tm3TaO7 ceramic coating layer, was manufactured on the surface of the TmTa3O9 ceramic thermal expansion coefficient buffer layer by atmospheric plasma spraying. First, Tm2O3 and Ta2O5 were used as raw materials, and spherical Tm3TaO7 spherical powder was manufactured by a high-temperature solid-phase method. In the process of spraying the thermal insulation cooling layer by atmospheric plasma spraying, argon gas was used as the protective gas, hydrogen gas was used as the combustion gas, the power of the spray gun was 46kW, the distance of the spray gun was 150mm, the gas flow rates of argon gas and hydrogen gas were 42 / 12slpm and 40 / 10slpm, respectively, the supply speed was 30g / min, the speed of the spray gun was 300mm / s, and the spraying time was 2min.

[0078] Example 8 In this application, a surface coating layer for drones and its manufacturing method are presented. As shown in FIG. 3, in the embodiment of this application, the surface coating layer for drones is covered on the surface of the drone body by a ceramic composite material substrate, and the ceramic composite material substrate is silicon carbide fiber reinforced silicon carbide. On the silicon carbide fiber reinforced carbon substrate, an adhesive layer with a thickness of 200 μm, an anti-oxidation layer with a thickness of less than 1 μm, an oxygen transmission barrier layer with a thickness of 50 μm, a thermal expansion coefficient buffer layer with a thickness of 50 μm, and an adiabatic temperature reduction layer with a thickness of 100 μm are sequentially manufactured, and the material of the adhesive layer is metal tantalum Ta, the oxygen transmission barrier layer is a rare earth tantalate RETaO4 ceramic coating layer, RE is Yb and Lu, and the thermal expansion coefficient buffer layer is a RETa3O9 ceramic, RE is La, Ho, and Tm.

[0079] Specifically, (1) a tantalum (Ta) adhesive layer with a thickness of 200 μm is produced on the upper surface of a silicon carbide fiber reinforced silicon carbide substrate by a low-temperature thermal spraying method. In the low-temperature thermal spraying process, compressed nitrogen gas is used as the working gas, the spraying pressure is 0.66 MPa, the spraying distance is 30 mm, the spraying temperature is 800°C, and the powder feed rate is 40 g / min. After the sprayed tantalum (Ta) adhesive layer material is placed in the air, the metallic tantalum is oxidized, and a dense tantalum oxide (Ta2O5) anti-oxidation layer with a thickness of less than 1 μm can be formed on the surface of the material.

[0080] (2) A 50-micrometer-thick oxygen barrier layer, Yb 1 / 2 Lu 1 / 2 The TaO4 ceramic coating layer was manufactured. First, the raw materials Lu2O3, Yb2O3 and Ta2O5 were used to prepare spherical Yb 1 / 2 Lu 1 / 2 In the process of producing TaO4 spherical powder and spraying the oxygen transmission barrier layer using the atmospheric plasma spraying method, argon gas was used as the protective gas and hydrogen gas was used as the combustion gas. During spraying, the power of the spray gun was 42 kW, the distance of the spray gun was 100 mm, the gas flow rates of argon gas and hydrogen gas were 40 / 12 slpm and 45 / 10 slpm, respectively, the supply speed was 50 g / min, the speed of the spray gun was 300 mm / s, and the spraying time was 2 min.

[0081] (3) Air plasma spraying of Yb 1 / 2 Lu 1 / 2 The TaO4 ceramic oxygen barrier layer is covered with a 50-micrometer-thick thermal expansion buffer layer, La 1 / 3 Ho 1 / 3 Tm 1 / 3 The Ta3O9 ceramic coating layer was manufactured. First, La2O3, Ho2O3, Tm2O3 and Ta2O5 were used as raw materials, and spherical La was fabricated by a high-temperature solid-state method. 1 / 3 Ho 1 / 3 Tm 1 / 3 In the process of producing Ta3O9 spherical powder and spraying a thermal expansion coefficient buffer layer by atmospheric plasma spraying, argon gas was used as the protective gas and hydrogen gas was used as the combustion gas, the power of the spray gun was 46kW, the distance of the spray gun was 150mm, the gas flow rates of argon gas and hydrogen gas were 42 / 12slpm and 40 / 10slpm respectively, the supply rate was 30g / min, the speed of the spray gun was 300mm / s, and the spraying time was 3min.

[0082] (4) Atmospheric plasma spraying method 1 / 3 Ho 1 / 3 Tm 1 / 3A 100-micrometer-thick Y3TaO7 ceramic coating layer, which is an adiabatic temperature-reducing ceramic layer, was manufactured on the surface of a Ta3O9 ceramic thermal expansion coefficient buffer layer. First, Y2O3 and Ta2O5 were used as raw materials, and spherical Y3TaO7 spherical powder was manufactured by a high-temperature solid-phase method. In the process of spraying the adiabatic temperature-reducing ceramic layer by an atmospheric plasma spraying method, argon gas was used as the protective gas, hydrogen gas was used as the combustion gas, the power of the spray gun was 46kW, the distance of the spray gun was 150mm, the gas flow rates of argon gas and hydrogen gas were 42 / 12slpm and 40 / 10slpm, respectively, the supply speed was 30g / min, the speed of the spray gun was 300mm / s, and the spraying time was 2min.

[0083] Example 9 In this application, a surface coating layer for drones and its manufacturing method are presented. As shown in FIG. 3, in the embodiment of this application, the surface coating layer for drones is covered on the surface of the drone body by a ceramic composite material substrate, and the ceramic composite material substrate is carbon fiber reinforced silicon carbide. On the carbon fiber reinforced silicon carbide substrate, an adhesive layer with a thickness of 150 μm, an oxidation prevention layer with a thickness of less than 1 μm, an oxygen transmission barrier layer with a thickness of 35 μm, a thermal expansion coefficient buffer layer with a thickness of 35 μm, and an adiabatic temperature reduction layer with a thickness of 1000 micrometers are sequentially manufactured, and the material of the adhesive layer is metal tantalum Ta, the oxygen transmission barrier layer is a rare earth tantalate RETaO4 ceramic coating layer, RE is Sc, and the thermal expansion coefficient buffer layer is a RETa3O9 ceramic, RE is La.

[0084] Specifically, (1) a tantalum (Ta) adhesive layer with a thickness of 150 μm is produced on the upper surface of a silicon carbide fiber reinforced silicon carbide substrate by a low-temperature thermal spraying method. In the low-temperature thermal spraying process, compressed nitrogen gas is used as the working gas, the spraying pressure is 0.66 MPa, the spraying distance is 30 mm, the spraying temperature is 800°C, and the powder feed rate is 40 g / min. After the sprayed tantalum (Ta) adhesive layer material is placed in the air, the metallic tantalum is oxidized, and a dense tantalum oxide (Ta2O5) oxidation prevention layer with a thickness of less than 1 μm can be formed on the surface of the material.

[0085] (2) An ScTaO4 ceramic coating layer, which is an oxygen transmission barrier layer, was manufactured with a thickness of 35 micrometers on the surface of a dense tantalum oxide Ta2O5 oxidation prevention layer by atmospheric plasma spraying. First, Sc2O3 and Ta2O5 were used as raw materials, and spherical ScTaO4 spherical powder was manufactured by a high-temperature solid-phase method. In the process of spraying the oxygen transmission barrier layer by atmospheric plasma spraying, argon gas was used as the protective gas and hydrogen gas was used as the combustion gas, the power of the spray gun during spraying was 42kW, the distance of the spray gun was 100mm, the gas flow rates of argon gas and hydrogen gas were 40 / 12slpm and 45 / 10slpm, respectively, the supply speed was 50g / min, the speed of the spray gun was 300mm / s, and the spraying time was 2min.

[0086] (3) A LaTa3O9 ceramic coating layer, which is a thermal expansion coefficient buffer layer with a thickness of 35 micrometers, was manufactured on the surface of the ScTaO4 ceramic oxygen transmission barrier layer by the atmospheric plasma spraying method. First, La2O3 and Ta2O5 were used as raw materials, and spherical LaTa3O9 spherical powder was manufactured by a high-temperature solid-phase method. In the process of spraying the thermal expansion coefficient buffer layer by the atmospheric plasma spraying method, argon gas was used as the protective gas, hydrogen gas was used as the combustion gas, the power of the spray gun was 46kW, the distance of the spray gun was 150mm, the gas flow rates of argon gas and hydrogen gas were 42 / 12slpm and 40 / 10slpm, respectively, the supply speed was 30g / min, the speed of the spray gun was 300mm / s, and the spraying time was 3min.

[0087] (4) A 1000-micrometer-thick YLaDyTaO7 ceramic coating layer, which is an adiabatic temperature-reducing ceramic layer, was manufactured on the surface of a LaTa3O9 ceramic thermal expansion coefficient buffer layer by atmospheric plasma spraying. First, Y2O3, La2O3, Dy2O3, and Ta2O5 were used as raw materials, and spherical YLaDyTaO7 spherical powder was manufactured by a high-temperature solid-phase method. In the process of spraying the adiabatic temperature-reducing ceramic layer by atmospheric plasma spraying, argon gas was used as the protective gas, hydrogen gas was used as the combustion gas, the power of the spray gun was 46kW, the distance of the spray gun was 150mm, the gas flow rates of argon gas and hydrogen gas were 42 / 12slpm and 40 / 10slpm, respectively, the supply speed was 30g / min, the speed of the spray gun was 300mm / s, and the spraying time was 10min.

[0088] Example 10 In this application, a surface coating layer for a drone and a manufacturing method thereof are presented. As shown in FIG. 3, in the embodiment of this application, the surface coating layer for a drone is covered on the surface of the drone body by a ceramic composite material substrate, and the ceramic composite material substrate is carbon fiber reinforced carbon. On the carbon fiber reinforced carbon substrate, an adhesive layer having a thickness of 170 μm, an anti-oxidation layer having a thickness of less than 1 μm, an oxygen transmission barrier layer having a thickness of 35 μm, a thermal expansion coefficient buffer layer having a thickness of 40 μm, and an insulating temperature reduction layer having a thickness of 500 micrometers are sequentially manufactured, and the material of the adhesive layer is metal tantalum Ta, the oxygen transmission barrier layer is a rare earth tantalate RETaO4 ceramic coating layer, where RE is Sc, Yb, and Lu, and the thermal expansion coefficient buffer layer is RETa3O9 ceramic, where RE is La, Ho, Er, and Tm.

[0089] Specifically, (1) a tantalum (Ta) adhesive layer with a thickness of 170 μm is produced on the upper surface of a silicon carbide fiber reinforced silicon carbide substrate by a low-temperature thermal spraying method. In the low-temperature thermal spraying process, compressed nitrogen gas is used as the working gas, the spraying pressure is 0.66 MPa, the spraying distance is 30 mm, the spraying temperature is 800°C, and the powder feed rate is 40 g / min. After the sprayed tantalum (Ta) adhesive layer material is placed in the air, the metal tantalum is oxidized, and a dense tantalum oxide (Ta2O5) oxidation prevention layer with a thickness of less than 1 μm can be formed on the surface of the material.

[0090] (2) A 35-micrometer-thick oxygen barrier layer, Sc, is applied to the surface of the dense tantalum oxide (Ta2O5) oxidation prevention layer by air plasma spraying. 1 / 3 Yb 1 / 3 Lu 1 / 3 The TaO4 ceramic coating layer was produced. First, Sc2O3, Lu2O3, Yb2O3 and Ta2O5 were used as raw materials, and spherical Sc was fabricated by a high-temperature solid-state method. 1 / 3 Yb 1 / 3 Lu 1 / 3 In the process of producing TaO4 spherical powder and spraying the oxygen transmission barrier layer using the atmospheric plasma spraying method, argon gas was used as the protective gas and hydrogen gas was used as the combustion gas. During spraying, the power of the spray gun was 42 kW, the distance of the spray gun was 100 mm, the gas flow rates of argon gas and hydrogen gas were 40 / 12 slpm and 45 / 10 slpm, respectively, the supply speed was 50 g / min, the speed of the spray gun was 300 mm / s, and the spraying time was 2 min.

[0091] (3) Sc by atmospheric plasma spraying 1 / 3 Yb 1 / 3 Lu 1 / 3 The TaO4 ceramic oxygen barrier layer is covered with a 40-micrometer-thick thermal expansion buffer layer called La 1 / 4 Ho 1 / 4 Tm 1 / 4 Er 1 / 4 The Ta3O9 ceramic coating layer was manufactured. First, Er2O3, La2O3, Ho2O3, Tm2O3 and Ta2O5 were used as raw materials, and spherical La was fabricated by a high-temperature solid-state method. 1 / 4 Ho 1 / 4 Tm 1 / 4Er 1 / 4 In the process of producing Ta3O9 spherical powder and spraying a thermal expansion coefficient buffer layer by atmospheric plasma spraying, argon gas was used as the protective gas and hydrogen gas was used as the combustion gas, the power of the spray gun was 46kW, the distance of the spray gun was 150mm, the gas flow rates of argon gas and hydrogen gas were 42 / 12slpm and 40 / 10slpm respectively, the supply rate was 30g / min, the speed of the spray gun was 300mm / s, and the spraying time was 3min.

[0092] (4) Atmospheric plasma spraying method 1 / 4 Ho 1 / 4 Tm 1 / 4 Er 1 / 4 A 500-micrometer-thick Y3TaO7 ceramic coating layer, which is an adiabatic temperature-reducing ceramic layer, was manufactured on the surface of a Ta3O9 ceramic thermal expansion coefficient buffer layer. First, Y2O3 and Ta2O5 were used as raw materials, and spherical Y3TaO7 spherical powder was manufactured by a high-temperature solid-phase method. In the process of spraying the adiabatic temperature-reducing ceramic layer by an atmospheric plasma spraying method, argon gas was used as the protective gas, hydrogen gas was used as the combustion gas, the power of the spray gun was 46kW, the distance of the spray gun was 150mm, the gas flow rates of argon gas and hydrogen gas were 42 / 12slpm and 40 / 10slpm, respectively, the supply speed was 30g / min, the speed of the spray gun was 300mm / s, and the spraying time was 10min.

[0093] Comparative Example 3 In this application, a surface coating layer for drones and its manufacturing method are presented. As shown in FIG. 1, in the embodiment of this application, the surface coating layer for drones is covered on the surface of the drone body by a ceramic composite material substrate, and the ceramic composite material substrate is silicon carbide fiber reinforced carbon. On the silicon carbide fiber reinforced carbon substrate, an adhesive layer with a thickness of 200 μm, an anti-oxidation layer with a thickness of less than 1 μm, an oxygen transmission barrier layer with a thickness of 50 μm, and an adiabatic cooling layer with a thickness of 100 micrometers are sequentially manufactured, and the material of the adhesive layer is metal tantalum Ta, the oxygen transmission barrier layer is a rare earth tantalate RETaO4 ceramic coating layer, RE is Yb and Lu, and the thermal expansion coefficient buffer layer is a RETa3O9 ceramic, RE is La, Ho, and Tm.

[0094] Specifically, (1) a tantalum (Ta) adhesive layer with a thickness of 200 μm is produced on the upper surface of a silicon carbide fiber reinforced silicon carbide substrate by a low-temperature thermal spraying method. In the low-temperature thermal spraying process, compressed nitrogen gas is used as the working gas, the spraying pressure is 0.66 MPa, the spraying distance is 30 mm, the spraying temperature is 800°C, and the powder feed rate is 40 g / min. After the sprayed tantalum (Ta) adhesive layer material is placed in the air, the metallic tantalum is oxidized, and a dense tantalum oxide (Ta2O5) anti-oxidation layer with a thickness of less than 1 μm can be formed on the surface of the material.

[0095] (2) A 50-micrometer-thick oxygen barrier layer, Yb 1 / 2 Lu 1 / 2 The TaO4 ceramic coating layer was manufactured. First, the raw materials Lu2O3, Yb2O3 and Ta2O5 were used to prepare spherical Yb 1 / 2 Lu 1 / 2In the process of producing TaO4 spherical powder and spraying the oxygen transmission barrier layer using the atmospheric plasma spraying method, argon gas was used as the protective gas and hydrogen gas was used as the combustion gas. During spraying, the power of the spray gun was 42 kW, the distance of the spray gun was 100 mm, the gas flow rates of argon gas and hydrogen gas were 40 / 12 slpm and 45 / 10 slpm, respectively, the supply speed was 50 g / min, the speed of the spray gun was 300 mm / s, and the spraying time was 2 min.

[0096] (3) Yb, an oxygen barrier layer, is used in the atmospheric plasma spraying method. 1 / 2 Lu 1 / 2 A 100-micrometer-thick Y3TaO7 ceramic coating layer, which is an adiabatic temperature-reducing ceramic layer, was manufactured on the surface of the TaO4 ceramic coating layer. First, Y2O3 and Ta2O5 were used as raw materials, and spherical Y3TaO7 spherical powder was manufactured by a high-temperature solid-phase method. In the process of spraying the adiabatic temperature-reducing ceramic layer by an atmospheric plasma spraying method, argon gas was used as the protective gas, hydrogen gas was used as the combustion gas, the power of the spray gun was 46kW, the distance of the spray gun was 150mm, the gas flow rates of argon gas and hydrogen gas were 42 / 12slpm and 40 / 10slpm, respectively, the supply speed was 30g / min, the speed of the spray gun was 300mm / s, and the spraying time was 2min.

[0097] Comparative Example 4 In this application, a surface coating layer for drones and its manufacturing method are presented. As shown in FIG. 3, in the embodiment of this application, the surface coating layer for drones is covered on the surface of the drone body by a ceramic composite material substrate, and the ceramic composite material substrate is carbon fiber reinforced silicon carbide. On the carbon fiber reinforced silicon carbide substrate, an oxygen transmission barrier layer having a thickness of 35 μm, a thermal expansion coefficient buffer layer having a thickness of 35 μm, and a heat insulating temperature reduction layer having a thickness of 1000 micrometers are sequentially manufactured, and the material of the adhesive layer is metal tantalum Ta, the oxygen transmission barrier layer is a rare earth tantalate RETaO4 ceramic coating layer, RE is Sc, and the thermal expansion coefficient buffer layer is a RETa3O9 ceramic, RE is La.

[0098] Specifically, (1) an ScTaO4 ceramic coating layer, which is an oxygen transmission barrier layer with a thickness of 35 micrometers, was manufactured on the surface of the substrate by the atmospheric plasma spraying method, and first, Sc2O3 and Ta2O5 were used as raw materials, and spherical ScTaO4 spherical powder was manufactured by the high-temperature solid-phase method. In the process of spraying the oxygen transmission barrier layer by the atmospheric plasma spraying method, argon gas was used as the protective gas, and hydrogen gas was used as the combustion gas, and the power of the spray gun during spraying was 42kW, the distance of the spray gun was 100mm, the gas flow rates of argon gas and hydrogen gas were 40 / 12slpm and 45 / 10slpm, respectively, the supply speed was 50g / min, the speed of the spray gun was 300mm / s, and the spraying time was 2min.

[0099] (2) A LaTa3O9 ceramic coating layer, which is a thermal expansion coefficient buffer layer with a thickness of 35 micrometers, was manufactured on the surface of the ScTaO4 ceramic oxygen transmission barrier layer by the atmospheric plasma spraying method. First, La2O3 and Ta2O5 were used as raw materials, and spherical LaTa3O9 spherical powder was manufactured by a high-temperature solid-phase method. In the process of spraying the thermal expansion coefficient buffer layer by the atmospheric plasma spraying method, argon gas was used as the protective gas, hydrogen gas was used as the combustion gas, the power of the spray gun was 46kW, the distance of the spray gun was 150mm, the gas flow rates of argon gas and hydrogen gas were 42 / 12slpm and 40 / 10slpm, respectively, the supply speed was 30g / min, the speed of the spray gun was 300mm / s, and the spraying time was 3min.

[0100] (3) A 1000-micrometer-thick YLaDyTaO7 ceramic coating layer, which is an adiabatic temperature-reducing ceramic layer, was manufactured on the surface of a LaTa3O9 ceramic thermal expansion coefficient buffer layer by atmospheric plasma spraying. First, Y2O3, La2O3, Dy2O3, and Ta2O5 were used as raw materials, and spherical YLaDyTaO7 spherical powder was manufactured by a high-temperature solid-phase method. In the process of spraying the adiabatic temperature-reducing ceramic layer by atmospheric plasma spraying, argon gas was used as the protective gas, hydrogen gas was used as the combustion gas, the power of the spray gun was 46kW, the distance of the spray gun was 150mm, the gas flow rates of argon gas and hydrogen gas were 42 / 12slpm and 40 / 10slpm, respectively, the supply speed was 30g / min, the speed of the spray gun was 300mm / s, and the spraying time was 10min.

[0101] The specific compositions of the material systems manufactured in the above Examples 7 to 10 are shown in Table 3. In order to characterize the performance of the above Examples and Comparative Examples, tests were conducted on the number of thermal cycles required for their failure, the oxidation weight loss rate, and the adiabatic temperature drop gradient. The thermal cycle test process involves heating the surface of the coating layer to 1000°C using a flame, keeping it warm for 3 minutes, and then cooling for 2 minutes, and repeating this cycle until the coating layer peels off or the oxidation weight loss of the material exceeds 10%. After weighing the mass of the material system before (W1) and after (W2) the total number of thermal cycles, (W1-W2) / W1×100% is the oxidation weight loss rate, and the temperature difference between the surface temperature of the coating layer during the first test and the temperature at the contact interface between the substrate and the coating layer is the adiabatic temperature drop gradient of the coating material, and the results are shown in Table 4.

[0102] [Table 3]

[0103] [Table 4]

[0104] The test results show that the material with a complete coating system has excellent insulating and cooling effects and can be used for a long time in a temperature environment of 1000°C, preventing the oxidation and depletion of the above-mentioned base material. On the other hand, the material without a complete coating system has a large difference in thermal expansion coefficient and weak bonding strength, so it will deplete early and cannot meet the needs of use.

[0105] Example 11 As shown in Figure 4, in this embodiment, the lightweight material for manufacturing the drone body is selected from carbon fiber braid, and the internal parts of the drone and the carbon fiber braid body are bonded with ethylene propylene rubber, and the specific manufacturing process is to cover the surface of the drone with ethylene propylene rubber, and then cover the surface of the drone with the lightweight material housing of the drone body. The carbon fiber braid material is used as the substrate, and a coating layer consisting of "adhesive layer + antioxidant layer + oxygen transmission barrier layer + heat insulation temperature reduction layer" is manufactured on the surface of the substrate, and the specific steps are as follows (1) to (4).

[0106] (1) A silicon (Si) adhesive layer with a thickness of 50 micrometers was fabricated on the surface of a carbon fiber braid by electron beam physical vapor deposition. During the deposition process, the substrate temperature was 350°C, the target-substrate distance was 300 mm, the incidence angle was 30°, the electron acceleration voltage was 20 kV, and the vacuum degree was 2×10 -3 The pressure was less than 1 Pa and the deposition rate was 100 nm / min.

[0107] (2) After the Si coating layer was produced, it was placed in air and heated at 300°C to oxidize it, obtaining a 10 micrometer-thick SiO2 coating layer, i.e., an oxidation-resistant layer.

[0108] (3) An oxygen transmission barrier layer-YbTaO4 ceramic coating layer with a thickness of 50 micrometers was produced on the surface of the oxidation prevention layer by atmospheric plasma spraying. First, Yb2O3 and Ta2O5 were used as raw materials to produce spherical YbTaO4 spherical powder by high-temperature solid-phase method, and then the YbTaO4 spherical powder was used to produce the YbTaO4 ceramic coating layer by atmospheric plasma spraying technology. The process parameters of the atmospheric plasma spraying were: spray gun power 42kW, spray gun distance 120mm, argon gas and hydrogen gas flow rates 40 / 12slpm and 45 / 10slpm respectively, feed rate 45g / min, spray gun speed 200mm / s, spraying time 2min.

[0109] (4) A 300-micrometer-thick thermal insulation layer-La3NbO7 ceramic coating layer was produced on the surface of the oxygen transmission barrier layer by atmospheric plasma spraying. First, La2O3 and Nb2O5 were used as raw materials to produce spherical La3NbO7 spherical powder by high-temperature solid-phase method, and then the La3NbO7 spherical powder was used to produce the La3NbO7 ceramic coating layer by atmospheric plasma spraying technology. The process parameters of the atmospheric plasma spraying were: spray gun power 43kW, spray gun distance 120mm, argon gas and hydrogen gas flow rates 42 / 12slpm and 45 / 15slpm respectively, feed rate 50g / min, spray gun speed 100mm / s, spraying time 10min.

[0110] FIG. 5 shows how the thermal conductivity of the coating system (not including ethylene propylene rubber) produced on the surface of the carbon fiber braided body of the lightweight material of this embodiment changes with temperature. As shown in FIG. 5, the thermal conductivity increases slightly with increasing temperature, but the thermal conductivity of the entire material system is extremely low, between 0.32 and 0.48 W / m / K, proving that this coating layer has excellent high-temperature thermal insulation protection effect.

[0111] FIG. 6 shows the microstructure diagram of the coating system produced in this embodiment. As shown in FIG. 6, the anti-oxidation layer is very thin, consisting only of the black area on the surface of the adhesive layer. Also, as can be seen from FIG. 3, the materials between each coating layer are tightly bonded, with no obvious cracks, proving that the manufacturing process of this application can produce a coating material with extremely strong bonding strength.

[0112] Example 12 As shown in FIG. 4, in this embodiment, the lightweight material for manufacturing the drone body is selected from TC4 titanium alloy material, and the TC4 titanium alloy material is used as the substrate. A coating layer consisting of "adhesive layer + anti-oxidation layer + oxygen transmission barrier layer + heat insulating temperature reduction layer" is manufactured on the surface of the substrate. The specific steps are as follows (1) to (4).

[0113] (1) An aluminum (Al) adhesive layer with a thickness of 50 micrometers was fabricated on the surface of TC4 titanium alloy material by electron beam physical vapor deposition. During the deposition process, the substrate temperature was 400°C, the target-substrate distance was 300 mm, the incidence angle was 45°, the electron acceleration voltage was 22 kV, and the vacuum degree was 3×10 -3 The pressure was less than 1 Pa and the deposition rate was 100 nm / min.

[0114] (2) After the Al coating layer was produced, it was placed in air and heated at 100°C to oxidize it, obtaining an Al2O3 coating layer with a thickness of less than 10 micrometers, i.e., an oxidation-resistant layer.

[0115] (3) An oxygen barrier layer, an AlTaO4 ceramic layer, 50 micrometers thick, was fabricated on the surface of the oxidation prevention layer by atmospheric plasma spraying. First, Lu2O3, Yb2O3 and Ta2O5 were used as raw materials, and spherical Yb 0.5 Lu 0.5 TaO4 spherical powder was produced and then Yb 0.5 Lu 0.5 TaO4 spherical powder was used to coat Yb 0.5 Lu 0.5A TaO4 ceramic coating layer was produced, and the process parameters of the atmospheric plasma spraying were as follows: spray gun power 42 kW, spray gun distance 120 mm, argon gas and hydrogen gas flow rates 40 / 12 slpm and 45 / 10 slpm respectively, feed rate 45 g / min, spray gun speed 200 mm / s, and spraying time 2 min.

[0116] (4) A Y3NbO7 ceramic coating layer, which is an adiabatic temperature-reducing layer with a thickness of 350 micrometers, was produced on the surface of the oxygen transmission barrier layer by atmospheric plasma spraying. First, Y2O3 and Nb2O5 were used as raw materials to produce spherical Y3NbO7 spherical powder by high-temperature solid-phase method, and then the Y3NbO7 spherical powder was used to produce a Y3NbO7 ceramic coating layer by atmospheric plasma spraying technology. The process parameters of the atmospheric plasma spraying were: power of the spray gun was 43kW, distance of the spray gun was 100mm, gas flow rates of argon gas and hydrogen gas were 42 / 12slpm and 45 / 15slpm, respectively, feed rate was 40g / min, speed of the spray gun was 100mm / s, and spraying time was 11min.

[0117] (Example 13) As shown in FIG. 4, in this embodiment, an aluminum alloy material is selected as a lightweight material for manufacturing a drone body, and the aluminum alloy material is used as the substrate. A coating layer consisting of an "adhesive layer + anti-oxidation layer + oxygen transmission blocking layer + heat insulating temperature reducing layer" is manufactured on the surface of the substrate. The specific steps are as follows (1) to (4).

[0118] (1) An aluminum (Al) adhesive layer with a thickness of 20 micrometers was produced on the surface of an aluminum alloy material by electron beam physical vapor deposition. During the deposition process, the substrate temperature was 400°C, the target-substrate distance was 300 mm, the incidence angle was 45°, the electron acceleration voltage was 22 kV, and the vacuum degree was 3×10 -3 The pressure was less than 1 Pa and the deposition rate was 100 nm / min.

[0119] (2) After the Al coating layer was produced, it was placed in air and heated at 100°C to oxidize it, obtaining an Al2O3 coating layer with a thickness of less than 10 micrometers, i.e., an oxidation-resistant layer.

[0120] (3) An oxygen transmission barrier layer-AlTaO4 ceramic layer with a thickness of 100 micrometers was produced on the surface of the oxidation prevention layer by atmospheric plasma spraying. First, Al2O3 and Ta2O5 were used as raw materials to produce spherical AlTaO4 spherical powder by high-temperature solid-phase method, and then the AlTaO4 spherical powder was used to produce an AlTaO4 ceramic coating layer by atmospheric plasma spraying technology. The process parameters of the atmospheric plasma spraying were: spray gun power 42kW, spray gun distance 120mm, argon gas and hydrogen gas flow rates 40 / 12slpm and 45 / 10slpm respectively, feed rate 45g / min, spray gun speed 200mm / s, spraying time 5min.

[0121] (4) A 600-micrometer-thick Sm3NbO7 ceramic coating layer, which is an adiabatic cooling layer, was produced on the surface of the oxygen transmission barrier layer by atmospheric plasma spraying. First, Sm2O3 and Nb2O5 were used as raw materials to produce spherical Sm3NbO7 spherical powder by high-temperature solid-phase method, and then the Sm3NbO7 ceramic coating layer was produced using the Sm3NbO7 spherical powder by atmospheric plasma spraying technology. The process parameters of the atmospheric plasma spraying were: power of the spray gun was 43kW, distance of the spray gun was 100mm, gas flow rates of argon gas and hydrogen gas were 42 / 12slpm and 45 / 15slpm, respectively, feed rate was 40g / min, speed of the spray gun was 100mm / s, and spraying time was 20min.

[0122] Example 14 As shown in FIG. 4, in this embodiment, an aluminum alloy material is selected as a lightweight material for manufacturing a drone body, and the aluminum alloy material is used as the substrate. A coating layer consisting of an "adhesive layer + anti-oxidation layer + oxygen transmission blocking layer + heat insulating temperature reducing layer" is manufactured on the surface of the substrate. The specific steps are as follows (1) to (4).

[0123] (1) A tantalum (Ta) adhesive layer with a thickness of 100 micrometers was fabricated on the surface of an aluminum alloy material by electron beam physical vapor deposition. During the deposition process, the substrate temperature was 400°C, the target-substrate distance was 300 mm, the incidence angle was 45°, the electron acceleration voltage was 22 kV, and the vacuum degree was 3×10 -3 The pressure was less than 1 Pa and the deposition rate was 100 nm / min.

[0124] (2) After the tantalum coating layer was prepared, it was placed in air and heated at 30°C to oxidize it, obtaining a Ta2O5 coating layer with a thickness of less than 10 micrometers, i.e., an oxidation-resistant layer.

[0125] (3) A 50 micrometer-thick oxygen transmission barrier layer-YTaO4 ceramic layer was produced on the surface of the oxidation prevention layer by atmospheric plasma spraying. First, Y2O3 and Ta2O5 were used as raw materials to produce spherical YTaO4 spherical powder by high-temperature solid-phase method, and then the YTaO4 spherical powder was used to produce a YTaO4 ceramic coating layer by atmospheric plasma spraying technology. The process parameters of the atmospheric plasma spraying were: spray gun power 42kW, spray gun distance 120mm, argon gas and hydrogen gas flow rates 40 / 12slpm and 45 / 10slpm respectively, feed rate 45g / min, spray gun speed 200mm / s, spraying time 2min.

[0126] (4) An 80-micrometer-thick Y3NbO7 ceramic coating layer, which is an adiabatic temperature-reducing layer, was produced on the surface of the oxygen transmission barrier layer by atmospheric plasma spraying. First, Y2O3 and Nb2O5 were used as raw materials to produce spherical Y3NbO7 spherical powder by high-temperature solid-phase method, and then the Y3NbO7 spherical powder was used to produce a Y3NbO7 ceramic coating layer by atmospheric plasma spraying technology. The process parameters of the atmospheric plasma spraying were: power of the spray gun was 43kW, distance of the spray gun was 100mm, gas flow rates of argon gas and hydrogen gas were 42 / 12slpm and 45 / 15slpm, respectively, feed rate was 40g / min, speed of the spray gun was 100mm / s, and spraying time was 3min.

[0127] Example 15 As shown in FIG. 4, in this embodiment, the lightweight material for manufacturing the drone body is selected from TC4 titanium alloy material, and the TC4 titanium alloy material is used as the substrate. A coating layer consisting of "adhesive layer + anti-oxidation layer + oxygen transmission barrier layer + heat insulating temperature reduction layer" is manufactured on the surface of the substrate. The specific steps are as follows (1) to (4).

[0128] (1) A zirconium-hafnium alloy (ZrHf) adhesive layer with a thickness of 60 micrometers was fabricated on the surface of TC4 titanium alloy material by electron beam physical vapor deposition. During the deposition process, the substrate temperature was 400°C, the target-substrate distance was 300 mm, the incidence angle was 45°, the electron acceleration voltage was 22 kV, and the vacuum degree was 3×10 -3 The pressure was less than 1 Pa and the deposition rate was 100 nm / min.

[0129] (2) After the ZrHf coating layer was prepared, it was placed in air and heated at 280°C to be oxidized, resulting in a ZrO2 / HfO2 coating layer with a thickness of less than 10 micrometers, i.e., an oxidation-resistant layer.

[0130] (3) A 50-micrometer-thick oxygen barrier layer (Sm 1 / 3 Yb 1 / 3 Ho 1 / 3First, the raw materials Ho2O3, Sm2O3, Yb2O3 and Ta2O5 were used to fabricate spherical (Sm 1 / 3 Yb 1 / 3 Ho 1 / 3 )TaO4 spherical powder was produced, and then (Sm 1 / 3 Yb 1 / 3 Ho 1 / 3 )TaO4 spherical powder was used to produce (Sm 1 / 3 Yb 1 / 3 Ho 1 / 3 ) A TaO4 ceramic coating layer was produced, and the process parameters of the atmospheric plasma spraying were: spray gun power 42 kW, spray gun distance 120 mm, argon gas and hydrogen gas flow rates 40 / 12 slpm and 45 / 10 slpm respectively, feed rate 45 g / min, spray gun speed 200 mm / s, and spraying time 2 min.

[0131] (4) A 250 micrometer thick insulating layer (Sm 1 / 3 Yb 1 / 3 Ho 1 / 3 The raw materials were Ho2O3, Sm2O3, Yb2O3 and Nb2O5, and spherical (Sm 1 / 3 Yb 1 / 3 Ho 1 / 3 )3NbO7 spherical powder was produced and then (Sm 1 / 3 Yb 1 / 3 Ho 1 / 3 )3NbO7 spherical powder was used to produce (Sm 1 / 3 Yb 1 / 3 Ho 1 / 3 )3NbO7 ceramic coating layer was produced, and the process parameters of atmospheric plasma spraying were: spray gun power 43 kW, spray gun distance 100 mm, argon gas and hydrogen gas flow rates 42 / 12 slpm and 45 / 15 slpm respectively, feed rate 40 g / min, spray gun speed 100 mm / s, and spraying time 9 min.

[0132] (Example 16) As shown in FIG. 4, in this embodiment, a carbon fiber braided material is selected as a lightweight material for manufacturing a drone body, and the carbon fiber braided material is used as a substrate. A coating layer consisting of an adhesive layer, an anti-oxidation layer, an oxygen transmission barrier layer, and a heat insulating temperature reducing layer is manufactured on the surface of the substrate. The specific steps are as follows: (1) to (4).

[0133] (1) A calcium-magnesium (CaMg) adhesive layer with a thickness of 75 micrometers was fabricated on the surface of a carbon fiber braid by electron beam physical vapor deposition. During the deposition process, the substrate temperature was 350°C, the target-substrate distance was 300 mm, the incidence angle was 30°, the electron acceleration voltage was 20 kV, and the vacuum degree was 2×10 -3 The pressure was less than 1 Pa and the deposition rate was 100 nm / min.

[0134] (2) After the CaMg coating layer was produced, it was placed in air and heated at 120°C to cause oxidation, obtaining a CaO / MgO coating layer with a thickness of 10 micrometers, i.e., an oxidation-resistant layer.

[0135] (3) A 75-micrometer-thick oxygen barrier layer - Yb 1 / 4 Lu 1 / 4 Y 1 / 4 Sc 1 / 4 The TaO4 ceramic coating layer was fabricated. First, Yb2O3, Lu2O3, Y2O3, Sc2O3 and Ta2O5 were used as raw materials, and spherical Yb 1 / 4 Lu 1 / 4 Y 1 / 4 Sc 1 / 4 TaO4 spherical powder was produced and then Yb 1 / 4 Lu 1 / 4 Y 1 / 4 Sc 1 / 4 TaO4 spherical powder was used to coat Yb 1 / 4 Lu 1 / 4 Y 1 / 4 Sc 1 / 4A TaO4 ceramic coating layer was produced, and the process parameters of the atmospheric plasma spraying were as follows: spray gun power 42 kW, spray gun distance 120 mm, argon gas and hydrogen gas flow rates 40 / 12 slpm and 45 / 10 slpm respectively, feed rate 45 g / min, spray gun speed 200 mm / s, and spraying time 3 min.

[0136] (4) A 420-micrometer thick insulating layer (Yb 1 / 4 Lu 1 / 4 Y 1 / 4 Sc 1 / 4 The raw materials were Yb2O3, Lu2O3, Y2O3, Sc2O3 and Nb2O5, and spherical (Yb 1 / 4 Lu 1 / 4 Y 1 / 4 Sc 1 / 4 )3NbO7 spherical powder was produced, and then (Yb 1 / 4 Lu 1 / 4 Y 1 / 4 Sc 1 / 4 )3NbO7 spherical powder was used to produce (Yb 1 / 4 Lu 1 / 4 Y 1 / 4 Sc 1 / 4 )3NbO7 ceramic coating layer was produced, and the process parameters of atmospheric plasma spraying were: spray gun power 43 kW, spray gun distance 120 mm, argon gas and hydrogen gas flow rates 42 / 12 slpm and 45 / 15 slpm respectively, feed rate 50 g / min, spray gun speed 100 mm / s, and spraying time 15 min.

[0137] Comparative Example 5 In this comparative example, a carbon fiber braid material was used as a substrate, and a coating layer consisting of an "adhesive layer" was produced on the surface of the substrate according to the method of Example 11.

[0138] Comparative Example 6 In this comparative example, a titanium alloy was used as a substrate, and a coating layer consisting of an "adhesive layer + anti-oxidation layer" was produced on the surface of the substrate according to the method of Example 11.

[0139] Comparative Example 7 In this comparative example, a carbon fiber braid material was used as a substrate, and a coating layer consisting of "adhesive layer + antioxidant layer + oxygen transmission barrier layer" was produced on the surface of the substrate according to the method of Example 11.

[0140] The coating system structure and the specific material composition and thickness of each coating layer of the above Examples 11-16 and Comparative Examples 5-7 are shown in Table 5. In order to detect the protective and insulating effect of the surface coating layers made of different material systems on the lightweight material, tests were conducted on the limit operating temperature (high temperature resistance performance), the corresponding adiabatic temperature drop gradient and anti-oxidation performance of the surface coating layers. The specific test process is to heat the surface of the material manufactured with different coating layers, and observe the temperature at which the material melts to obtain the high temperature resistance performance (limit operating temperature) of the material. The material is kept warm for 60 seconds at the limit operating temperature, and the temperature of the contact interface between the lightweight material and the coating layer is measured by a thermocouple. The temperature difference between the surface temperature and the interface temperature is the adiabatic temperature drop gradient. The mass of the material before and after the test is measured, and the masses before and after the test are Z1 and Z2, respectively. The oxidation weight gain rate of the material is (Z2-Z1) / Z1×100%, and the higher the weight gain rate, the worse its anti-oxidation performance. (The oxidation temperature of the carbon fiber used in the embodiment of the present invention is 350°C, the limit operating temperature of the aluminum alloy is 660°C, and the limit operating temperature of the titanium alloy is 520°C)

[0141] [Table 5]

[0142] Based on the above experimental method, performance such as the limit operating temperature, temperature drop gradient, and oxidation weight gain rate were determined for each of Examples 11 to 16 and Comparative Examples 5 to 7, and the results are shown in Table 6 below.

[0143] [Table 6]

[0144] Experimental results and analysis As can be seen from Table 6, in Examples 11-16, after a complete coating system is manufactured on the surface of the lightweight material substrate, the limit operating temperature of the lightweight material is greatly improved, its adiabatic temperature reduction effect is excellent, and the adiabatic temperature reduction gradient can be effectively controlled by adjusting the thickness of each coating layer, so that the lightweight material can be used at a higher temperature for a long time, and the high temperature oxidation ablation resistance of the material can be effectively improved. Comparing Example 11 with Comparative Examples 5-7, the limit operating temperature of the material of Example 11 is higher than that of Comparative Examples 5-7, the adiabatic temperature reduction effect is better, and the antioxidant ability is stronger, and the mass loss of the material of Comparative Example 5 is very significant, which is due to the mass loss after the oxidative sublimation of the carbon fiber, the performance of the material of Comparative Example 6 is better than that of Comparative Example 5, and the performance of the material of Comparative Example 7 is better than that of Comparative Example 6, which shows that the setting of the oxygen transmission barrier layer and the adiabatic temperature reduction layer can further improve the high temperature resistance performance, adiabatic temperature reduction ability and antioxidant ability of the material.

[0145] (Example 17) As shown in FIG. 5, the present application provides a drone, which includes a drone body, a central control module 3, and an information acquisition module 1, a temperature detection module 2, a pressure control module 4, a drone module 5, and a high-efficiency firefighting module 6, which are respectively connected to the central control module 3; The information acquisition module 1 acquires relevant information of the target extinguishing point, including fire occurrence time, fire location, fire type, and fire prediction grade, and then forms a first data set, and sends the first data set to the central control module; The temperature detection module 2 collects the temperature distribution situation of the fire scene to form a second data set, and sends the second data set to the central control module; The pressure control module 4 monitors the pressure state of the high-efficiency fire extinguishing device and controls the high-efficiency fire extinguishing device in real time.

[0146] The drone body is made of a lightweight material, which is at least one selected from a carbon fiber braid, a titanium alloy, and an aluminum alloy. The lightweight material is used as a substrate, and an adhesive layer, an antioxidant layer, an oxygen transmission barrier layer, and a heat insulating temperature reducing layer are sequentially formed on the substrate by the method of the above-mentioned Examples 11 to 16. The internal parts of the drone and the lightweight material body are bonded by ethylene propylene rubber, and the specific manufacturing process is to cover the surface of the drone with ethylene propylene rubber, and then cover the surface of the drone with the lightweight material housing of the drone body. In addition, a coating layer may be formed on the resin-based composite material substrate or the ceramic-based composite material substrate by the method of Examples 1 to 10, and the substrate may be further covered on the surface of the drone body. The adhesive layer has a thickness of 20 to 200 μm, the oxygen transmission barrier layer has a thickness of 20 to 100 μm, the heat insulating temperature reducing layer has a thickness of 80 to 1000 μm, and the antioxidant layer has a thickness of less than 20 μm.

[0147] As shown in FIG. 6, the drone module 5 includes a remote controller, an aircraft power control device, and a fire extinguishing drone, where the remote controller controls the fire extinguishing drone to carry out the fire extinguishing mission issued from the central control module, the aircraft power control device provides flight power to the fire extinguishing drone, and the fire extinguishing drone carries out the fire extinguishing mission to extinguish the target fire location.

[0148] The high-efficiency firefighting module 6 includes a high-efficiency fire extinguishing device and a helmet. The high-efficiency fire extinguishing device is loaded with a high-efficiency compressible foam extinguishing agent as an extinguishing material to extinguish a fire scene. The high-efficiency compressible foam extinguishing agent is non-toxic and harmless, and the reactants obtained by reacting with the combustion material are also non-toxic and harmless substances. The helmet protects the high-efficiency fire extinguishing device and includes an inner layer made of a fire-resistant and explosion-proof polymer material and an outer layer made of an erosion-resistant material.

[0149] The central control module 3 includes a data storage unit 7, a mission issuing unit 8 and an analysis processing unit 9, the data storage unit 7 stores the first data set and the second data set, the mission issuing unit issues a fire extinguishing mission to the drone module according to the first data set, the analysis processing unit 9 analyzes and processes the second data set to obtain a temperature change graph according to the temperature detection situation, and combines with the Beidou positioning system to obtain a detailed on-site temperature distribution situation to find the specific location of the fire source and the point before the fire spreads, and then extinguishes the fire according to a predetermined fire extinguishing strategy; Use the temperature detection module to collect the temperature distribution situation of the target extinguishing point, and analyze the specific location information of the fire source and the point before the fire spreads; The pressure control module is used to control the high-efficiency fire fighting module to perform directional extinguishing, first extinguishing the point before the fire spreads, and then extinguishing the source of the fire.

[0150] The drone body includes a load-bearing panel for mounting the drone aircraft, a stable holder for protecting the safety of the fire extinguisher, a balance stabilizer for maintaining the drone aircraft in a balanced and stable state, and an aircraft propeller for providing the drone aircraft with a flight lift force. The aircraft propeller is made of woven carbon fiber with high strength and low mass, and a high-temperature resistant lightweight coating layer is applied to the surface of the propeller.

[0151] The specific implementation process of this embodiment is as follows: steps 1 to 5.

[0152] In step 1, the information acquisition module 1 acquires information such as the fire occurrence time, fire location, fire type, and fire prediction grade of the target extinguishing point, forms a first data set, and sends the first data set to the central control module; In step 2, the data storage unit of the central control module 3 receives and stores the first data set, and the mission issuing unit issues a firefighting mission to the drone module based on all the information in the first data set.

[0153] In step 3, after the remote controller of the drone module 5 receives the fire extinguishing mission, it controls the fire extinguishing drone to perform the fire extinguishing mission, by first providing flight power to the fire extinguishing drone via the aircraft power control device, and then controlling the flight distance and flight attitude of the fire extinguishing drone via the remote controller to fly from the fire center to the target extinguishing point.

[0154] In step 4, the temperature detection module 2 starts to work, collects the temperature distribution situation at the fire scene to form a second data set, and then sends the second data set to the central control module, and the analysis processing unit of the central control module analyzes and processes the second data set, obtains a temperature change graph based on the temperature detection situation, and combines with the Beidou positioning system to obtain detailed on-site temperature distribution situation, and finds the specific locations of the fire source and the points before the fire spreads.

[0155] In step 5, the pressure control module 4 controls the high-efficiency fire extinguishing device of the high-efficiency firefighting module to spray high-efficiency compressible foam extinguishing agent to perform directional extinguishing, first extinguishing the point before the fire spreads, and then extinguishing the source of the fire. After completing the extinguishing mission, the central control module 3 issues a return control command, and the remote controller controls the fire extinguishing drone to fly back to the fire center, thereby completing the fire extinguishing mission.

[0156] In recent years, the research and application of rescue drones has not been widely spread, and it has been widely applied in various fields of society, especially in the firefighting field, the application of drones is becoming more and more. In recent years, in the southwestern region of China and other areas, fires often occur in forests and grasslands, and the fires are fierce and develop rapidly, causing serious losses in areas where fires occur over a large area. The traditionally used fire extinguishers have a significant fire-extinguishing effect on fires at close range or with small fire sources, but generally cannot exert their power on fires at long distances and with strong fires. In the prior art, firefighting drones generally carry fire extinguishers and fly quickly to the fire site, spray extinguishing agents to extinguish the fire in advance, and play a role in timely suppression of fire behavior. Compared with firefighting teams, their only advantages are that they have a fast fire extinguishing response speed and can quickly arrive at the fire scene to extinguish the fire, but the directional extinguishing ability for the fire is not strong, the extinguishing effect is not good, and the entire fire extinguishing process is not intelligent and efficient enough.

[0157] In the embodiment of the present application, not only can the fire extinguishing mission be intelligently issued based on the collected information such as the fire occurrence time, fire location, fire type and fire forecast grade of the target extinguishing point, but also after the fire extinguishing drone arrives at the fire scene, it does not directly carry out the fire extinguishing work without planning, but first detects the temperature distribution situation of the fire scene by the temperature detection module, obtains a temperature change graph, and combines with the Beidou positioning system to obtain the detailed on-site temperature distribution situation, finds the specific location of the fire source and the point before the fire spreads, and then extinguishes the fire in a directional and efficient manner, so that the extinguishing effect is better, the efficiency is higher and the intelligence is higher. The highly efficient compressible fire extinguishing foam used for extinguishing is non-toxic and harmless, and the reactants obtained by reacting with the combustion material are also non-toxic and harmless materials, which can effectively guarantee the life and safety of animals, evacuees and firefighters at the fire scene. The drone's structural components are all made of high-temperature resistant materials, so that the fire extinguishing drone can continue to operate in a high-temperature environment, and the fire extinguishing drone will not deform or burn, which further ensures the extinguishing effect.

[0158] (Example 18) This embodiment is basically the same as embodiment 17, with the difference being that when the fire is strong and the long-distance fire extinguishing effect is not significant, the temperature detection module detects the exact location of the fire source, and the remote controller controls the drone module to fly toward the fire source, and the pressure control module controls the high-efficiency fire extinguishing device to perform explosion, thereby rapidly controlling the fire behavior by performing fixed-time fixed-point explosion extinguishing for the fire source.

[0159] The specific implementation process of this embodiment is the same as that of the seventeenth embodiment, except for the following points:

[0160] In step 5, the pressure control module 4 controls the high-efficiency fire extinguishing device of the high-efficiency firefighting module to spray high-efficiency compressible foam extinguishing agent to perform directional extinguishing, first extinguishing the point before the fire spreads, and then extinguishing the fire source. If the long-distance fire extinguishing effect is not significant and the fire is still strong, the temperature detection module detects the exact location of the fire source, controls the remote controller to fly toward the fire source, and controls the high-efficiency fire extinguishing device to perform blasting through the pressure control module, thereby rapidly controlling the fire behavior by performing fixed-point blasting extinguishing at the fire source, and then dispatches the candidate fire extinguishing drone to continue extinguishing the remaining fire. After all open flames are extinguished, the fire extinguishing mission is completed.

[0161] When using a fire extinguishing drone to extinguish a long-distance fire, unexpected situations may occur, such as a sudden increase in wind volume that gradually intensifies the fire, and the fire behavior cannot be controlled by long-distance extinguishing. In such a case, the fire source can be quickly and efficiently extinguished by directly using the blast extinguishing method, thereby avoiding the fire continuing to expand and causing more serious losses. Although blast extinguishing will result in the loss of the fire extinguishing drone, the uncontrollable fire behavior can be controlled in a timely manner, the impact of the fire can be reduced, and the safety of evacuees and firefighters can be ensured, and its value is greater than the economic value of a single fire extinguishing drone itself.

[0162] (Example 19) This embodiment is basically the same as embodiment 17, with the difference being that after the fire extinguishing drone completes the fire extinguishing mission and extinguishes all open flames at the fire scene, it will again collect the temperature distribution situation at the scene through the temperature detection module, and determine the points with a temperature higher than 60°C as rekindling points where the fire may rekindle, and then the fire extinguishing drone will carry out directional extinguishing on these rekindling points one by one until their temperature drops below 40°C.

[0163] The specific implementation process of this embodiment is the same as that of the seventeenth embodiment, except for the following points:

[0164] In step 5, the pressure control module 4 controls the high-efficiency fire extinguishing device of the high-efficiency firefighting module to spray high-efficiency compressible foam extinguishing agent to perform directional extinguishing, first extinguishing the points before the fire spreads, and then extinguishing the source of the fire. After the fire extinguishing mission is completed, the temperature detection module collects the temperature distribution situation at the scene again, and determines that the points with a temperature higher than 60°C are re-ignition points where the fire may re-ignite. The remote controller of the drone module 5 controls the fire extinguishing drones to fly one by one at points 2 meters above these re-ignition points, and perform directional extinguishing again until the temperature of all the re-ignition points drops below 40°C. Finally, the central control module 3 issues a return control command, and the remote controller controls the fire extinguishing drones to fly back to the fire center, and the fire extinguishing mission is completed.

[0165] According to the actual situation, in many cases of forest or mountain fires, open flames will re-ignite immediately after being extinguished. Therefore, after the fire extinguishing drone has extinguished all open flames, the temperature detection module will detect all points with a temperature higher than 60°C and carry out secondary extinguishing, thereby avoiding the occurrence of re-ignition and causing more serious losses, and effectively improving the extinguishing effect of the fire extinguishing drone.

[0166] (Example 20) This embodiment is basically the same as Example 17, and the difference is that the intelligent fire extinguishing drone system further includes a display module for displaying the fire extinguishing scene screen and the remaining power amount of the fire extinguishing drone in real time.

[0167] The specific implementation process of this embodiment is the same as that of the seventeenth embodiment, except for the following points:

[0168] In step 5, the pressure control module 4 controls the high-efficiency fire extinguishing device of the high-efficiency firefighting module to spray high-efficiency compressible foam extinguishing agent to perform directional extinguishing, first extinguishing the point before the fire spreads, and then extinguishing the source of the fire. During the extinguishing process, the display module can display the fire extinguishing site screen and the remaining power of the fire extinguishing drone in real time. After completing the fire extinguishing mission, the central control module issues a return control command, and the remote controller controls the fire extinguishing drone to fly back to the fire center, and the fire extinguishing mission is completed.

[0169] The display module allows workers to check the screen of the firefighting site in real time, allowing them to clearly understand the progress and effect of the firefighting. When an emergency occurs, they can take timely response measures. It also allows workers to check the remaining power of the firefighting drone, so that they can promptly call back the firefighting drone when the power is about to run out, preventing the drone from losing power and breaking down.

[0170] The above embodiments are merely illustrative of the principles and effects of the present application, and are not intended to limit the present invention. Those skilled in the art may modify or change the above embodiments without departing from the spirit and scope of the present application. Therefore, all equivalent modifications or changes made by those skilled in the art without departing from the spirit and technical ideas disclosed in the present application shall still be included in the scope of the claims of the present application.

Claims

1. At least an adhesive layer, an anti-oxidation layer, an oxygen transmission barrier layer, and a heat insulating and temperature reducing layer are included, A surface coating layer for a drone, which is manufactured on a surface of a drone body or is covered on the surface of the drone body by a composite material substrate, The drone body is constructed of lightweight materials; The composite substrate includes a resin-based composite substrate and a ceramic-based composite substrate, the adhesive layer has a thickness of 20 to 200 μm, the oxygen transmission barrier layer has a thickness of 20 to 100 μm, and the heat insulating temperature reducing layer has a thickness of 80 to 1000 μm. Surface coating layer for drones.

2. The resin-based composite substrate is a fiber-reinforced material based on an organic polymer, and the fiber-reinforced material is one of glass fiber, carbon fiber, basalt fiber, and aramid; The surface coating layer for a drone according to claim 1 .

3. The ceramic composite substrate is one of silicon carbide fiber reinforced silicon carbide, carbon fiber reinforced carbon, carbon fiber reinforced silicon carbide, and silicon carbide fiber reinforced carbon; The surface coating layer for a drone according to claim 1 .

4. The lightweight material is at least one selected from a carbon fiber braid, a titanium alloy, and an aluminum alloy, and the internal parts of the drone and the lightweight material are bonded with ethylene propylene rubber. The surface coating layer for a drone according to claim 1 .

5. The raw material of the adhesive layer is a material having a thermal expansion coefficient close to that of the lightweight material, and is at least one selected from aluminum, iron, magnesium, calcium, silicon, tantalum, vanadium, yttrium, zirconium, hafnium, niobium, molybdenum and tungsten; The surface coating layer for a drone according to claim 1 .

6. A thermal expansion coefficient buffer layer having a thickness of 30 to 50 μm is further provided between the oxygen transmission barrier layer and the thermal insulation temperature reducing layer of the ceramic composite substrate. The surface coating layer for a drone according to claim 1 .

7. The thermal expansion coefficient of the oxygen transmission barrier layer is 3×10 -6 K -1 ~6×10 -6 K -1 and the thermal expansion coefficient of the thermal expansion coefficient buffer layer is between 6×10 -6 K -1 ~9×10 -6 K -1 and the thermal expansion coefficient of the adiabatic temperature-reducing layer is between 9×10 -6 K -1 ~11 x 10 -6 K -1 Between The surface coating layer for a drone according to claim 6.

8. The thermal expansion coefficient buffer layer is RETa 3 O 9 Ceramic, RE being one or more of rare earth elements; The surface coating layer for a drone according to claim 6.

9. The oxidation prevention layer is made of Al 2 O 3 , SiO 2 , Ta 2 O 5 , Nb 2 O 5 , ZrO 2 , Mo 2 O 5 and W.O. 3 A mixture of one or more of The surface coating layer for a drone according to claim 1 .

10. the oxygen transmission barrier layer is a rare earth tantalate ceramic material or a rare earth tantalum / niobate ceramic material; The surface coating layer for a drone according to claim 1 .

11. The rare earth tantalate ceramic material is ATaO 4 A is a spherical powder, A is Al, Fe or a rare earth element, The rare earth tantalum / niobate ceramic material is 1-x Nb x O 4 A ceramic material, where RE is one or more of the rare earth elements, and 0<x<1; The surface coating layer for a drone according to claim 10.

12. The thermal insulating temperature reducing layer is a rare earth niobate ceramic material, a rare earth tantalate ceramic material, or a rare earth tantalum / niobate ceramic material; The surface coating layer for a drone according to claim 1 .

13. The rare earth niobate ceramic material is 3 NbO 7 It is a spherical powder, The rare earth tantalate ceramic material is RE 3 TaO 7 It is ceramic, The rare earth tantalum / niobate ceramic material is 3 T 1-y Nb y O 7 where RE is one or more rare earth elements, and 0<y<1. The surface coating layer for a drone according to claim 12.

14. Producing and forming an adhesive layer on the upper surface of a ceramic composite substrate by a low-temperature thermal spraying method, or producing and forming an adhesive layer on the upper surface of a resin composite substrate or a drone body by an electron beam physical vapor deposition method; placing the adhesive layer in air to oxidize it and form an oxidation prevention layer; forming an oxygen transmission barrier layer on the surface of the oxidation prevention layer by an atmospheric plasma spraying method; and forming a heat insulating layer on the surface of the oxygen transport barrier layer by an atmospheric plasma spraying method. A method for producing a surface coating layer for a drone, comprising:

15. The step of forming a thermal insulating temperature reducing layer on the surface of the oxygen transport barrier layer by an atmospheric plasma spraying method on the ceramic composite substrate includes: forming a thermal expansion coefficient buffer layer on the surface of the oxygen transport barrier layer by an atmospheric plasma spraying method; and forming the heat insulating temperature reducing layer on the surface of the thermal expansion coefficient buffer layer by an atmospheric plasma spraying method. The method for producing a surface coating layer for a drone according to claim 14.

16. The process parameters of the low temperature spraying method include: compressed nitrogen gas as working gas, spraying pressure as 0.66 MPa, spraying distance as 30 mm, spraying temperature as 800° C., and powder feed rate as 40 g / min; The process parameters of the atmospheric plasma spraying method include: the power of the spray gun is 30-50 kW, the distance of the spray gun is 80-160 mm, the gas flow rate of the argon gas is 3-10 slpm, the gas flow rate of the hydrogen gas is 3-10 slpm, the supply rate is 30-50 g / min, the speed of the spray gun is 80-300 mm / s, and the spraying time is 1-20 min. The method for producing a surface coating layer for a drone according to claim 14.

17. The process parameters of the electron beam physical vapor deposition method are as follows: the temperature of the substrate is 300 to 500° C., the target-substrate distance is 200 to 400 mm, the incidence angle is 30° to 50°, the electron acceleration voltage is 20 to 30 kV, and the vacuum degree is 5×10 -3 Pa or less, and a deposition rate of 50 to 150 nm / min; and the substrate includes a ceramic composite substrate, a resin composite substrate, or a drone body; The method for producing a surface coating layer for a drone according to claim 14.

18. The step of placing the adhesive layer in air to oxidize it and form an oxidation prevention layer includes: The adhesive layer is placed in air and heated to oxidize it, thereby forming an oxidation-resistant layer, the heating temperature being 30 to 300° C., and the thickness of the oxidation-resistant layer being 20 μm or less. The method for producing a surface coating layer for a drone according to claim 14.

19. A drone including a drone body, a central control module, and an information acquisition module, a temperature detection module, a pressure control module, a drone module, and a high-efficiency firefighting module, each of which is connected to the central control module, The information acquisition module acquires information related to a target extinguishing point to form a first data set, and transmits the first data set to the central control module; The temperature detection module collects temperature distribution conditions in the fire scene to form a second data set, and sends the second data set to the central control module; The pressure control module monitors the pressure state of the high-efficiency fire extinguishing device and controls the high-efficiency fire extinguishing device in real time; The drone module includes a remote controller, an aircraft power control device, and a fire extinguishing drone, the remote controller controls the fire extinguishing drone to perform the fire extinguishing mission issued from the central control module, the aircraft power control device provides flight power to the fire extinguishing drone, and the fire extinguishing drone performs the fire extinguishing mission to extinguish a target fire location; The high-efficiency fire-fighting module includes the high-efficiency fire-extinguishing device and a helmet, the high-efficiency fire-extinguishing device is loaded with extinguishing material to extinguish a fire at a fire site, and the helmet protects the high-efficiency fire-extinguishing device; The central control module includes a data storage unit, a mission issuing unit, and an analysis processing unit, the data storage unit stores the first data set and the second data set, the mission issuing unit issues a fire extinguishing mission to the drone module based on the first data set, the analysis processing unit analyzes and processes the second data set to obtain an analysis result on the location information of the fire source and the point before the fire spreads, and then extinguishes the fire according to a predetermined fire extinguishing strategy; The drone body is manufactured from a lightweight material, and the lightweight material is coated with a coating layer; The coating layer includes at least an adhesive layer, an anti-oxidation layer, an oxygen transmission barrier layer, and a heat insulating and temperature reducing layer; The coating layer is manufactured on the surface of the drone body or is covered on the surface of the drone body by a composite material substrate; The composite material substrate includes a resin-based composite material substrate and a ceramic-based composite material substrate, the adhesive layer has a thickness of 20 to 200 μm, the oxygen transmission barrier layer has a thickness of 20 to 100 μm, and the heat insulating temperature reducing layer has a thickness of 80 to 1000 μm. A drone characterized by

20. The predetermined fire extinguishing strategy comprises: Using the temperature detection module to collect the temperature distribution situation of the target extinguishing point, and analyze the specific location information of the fire source and the point before the fire spreads; Using the pressure control module to control the high-efficiency fire fighting module to perform directional extinguishing, first extinguishing the point before the fire spreads, and then extinguishing the source of the fire; The drone of claim 19.

21. Analyzing and processing the second data set to obtain an analysis result on the fire source and the point before the fire spreads includes obtaining a temperature change graph based on the temperature detection situation, combining with the Beidou positioning system to obtain a detailed on-site temperature distribution situation, and finding the specific location of the fire source and the point before the fire spreads. The drone of claim 19.

22. The drone body includes a load-bearing panel for mounting the drone aircraft, a stable holder for protecting the safety of the fire extinguisher, a balance stabilizer for maintaining the drone aircraft in a balanced and stable state, and an aircraft propeller for providing the drone aircraft with a flight lift force; The drone of claim 19.

23. The aircraft propeller is made of woven carbon fiber.

23. The drone of claim 22.

24. The relevant information includes fire occurrence time, fire location, fire type, and fire forecast grade; The drone of claim 19.

25. The extinguishing material is a highly efficient compressible foam extinguishing agent; The drone of claim 19.

26. The highly efficient compressible foam fire extinguishing agent is non-toxic and harmless, and the reactants obtained by reacting with the combustion material are also non-toxic and harmless substances.

26. The drone of claim 25.

27. The helmet includes an inner layer made of a fire-resistant, explosion-resistant polymeric material and an outer layer made of an erosion-resistant material. The drone of claim 19.

28. Further includes a display module for displaying the fire extinguishing site screen and the remaining power of the fire extinguishing drone in real time; The drone of claim 19.

Citation Information

Patent Citations

  • Rare earth tantalate (RE3TaO7) thermal barrier coating and preparation method thereof

    CN111908921A

  • Structure of thermal barrier coating, and method for manufacturing thermal barrier coating

    JP2006117975A