High molecular weight VDF-containing (co)polymers using a new precipitation polymerization process.

The novel precipitation polymerization process addresses the challenge of producing high molecular weight, beta-phase PVDF polymers with enhanced mechanical properties and adhesion, suitable for lithium ion battery components, by controlling temperature, pressure, and eliminating surfactants, resulting in improved cathode binder performance.

JP2024541207AActive Publication Date: 2024-11-08ARKEMA INC
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
JP2024523542
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2021-10-29
Filing Date
2022-10-25
Publication Date
2024-11-08
Estimated Expiration
2042-10-25

Smart Images

  • Figure 2024541207000001_ABST
    Figure 2024541207000001_ABST
Patent Text Reader

Abstract

Vinylidene fluoride (co)polymers having a beta phase strength ratio greater than 5 and polymerization processes for producing vinylidene fluoride based polymers or copolymers are disclosed.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] High molecular weight VDF-containing (co)polymers and methods for making the polymers are disclosed. [Background technology]

[0002] Vinylidene fluoride polymers or copolymers are melt-processable polymers that are produced by a number of different polymerization processes.

[0003] Vinylidene fluoride based polymers are semi-crystalline polymers that contain both crystalline and amorphous regions. The relationship between the amorphous and crystalline regions and the amount of crystalline phase different from the crystalline phase affect the properties of the polymer and determine the end use of a particular resin composition. Increasing the molecular weight improves melt strength and mechanical properties such as toughness and chemical stress crack resistance.

[0004] In the prior art, it is known to obtain high molecular weight PVDF by emulsion polymerization, for example, U.S. Pat. No. 9,202,638 discloses 4s -1 US Patent No. 10,559,828 discloses a PVDF having a melt viscosity of 900 to 1200 kPoise at 232°C and 100 s -1 The fluorine-containing polymers have melt viscosities of 10 to 100 kPoise measured at a shear rate of 100 kPoise, and U.S. Pat. No. 8,785,580 discloses PVDF copolymers having melt viscosities of over 35 kPoise (examples include those having melt viscosities of 56 kPoise and 52 kPoise).

[0005] PVDF has several crystalline phases, designated as α, β, γ, δ, and ε phases, which can be obtained by different processing methods / conditions. PVDF usually forms α phase from the molten state. In α phase, PVDF chains are polarized and the chains stack antiparallel. Antiparallel stacking results in the non-polarity of α phase crystals. β phase crystals are usually formed by cold drawing α phase crystals. In β phase crystals, PVDF chains are polarized and stack parallel. As a result, β phase crystals have the largest dipole moment and are used in ferroelectrics and many other applications. Normal γ phase crystals are produced by heat treating α phase crystals. γ phase crystals have similar polarity as β phase crystals. PVDF beta crystalline phase has attracted more interest due to its piezoelectric properties. A high percentage of β-phase in PVDF can be prepared by tailoring the polymer chains based on the copolymerization of vinylidene fluoride with comonomers such as vinyl fluoride (VF), trifluoroethylene (TrFE), and chlorotrifluoroethylene (CTFE) or through secondary and post-treatment processes such as temperature, pressure, cooling rate, and application of shear forces. Summary of the Invention [Problem to be solved by the invention]

[0006] When latex PVDF is spray dried, particle sizes between 1 μm and 30 μm can be obtained. However, these particles do not contain significant amounts of β-phase. In contrast, the present invention provides particles with an average precipitated particle size between 50 and 2500 μm that are predominantly β-phase. [Means for solving the problem]

[0007] The present invention describes a novel PVDF polymer and a precipitation polymerization process for producing vinylidene fluoride based polymers or copolymers. The PVDF polymer is predominantly in the beta phase (measured by the beta phase crystalline peak intensity ratio: I β(200 / 110) / [I α(020) +I γ(020)] > 5), has a high melting point (above 165 °C) and a raspberry morphology. The polymer is useful for the manufacture of components in lithium-ion batteries.

[0008] Aspects of the invention

[0009] Aspect 1: A crystalline cellulose having a melting temperature of 165°C to 175°C, preferably 168°C to 174°C, a raspberry morphology, and a beta phase intensity ratio (I β(200 / 110) / [I α(020) +I γ(020) ])

[0010] Aspect 2: The polyvinylidene fluoride polymer of aspect 1, having a melt viscosity of 53 to 150 KPoise at 100 s-1 and 900 to 3500 KPoise at 4 s-1.

[0011] Aspect 3: The polyvinylidene fluoride polymer of any one of aspects 1 or 2, having a solution viscosity at 9 wt. % in NMP (measured at 3.36 / s) of at least 7000 cP, preferably greater than 9000 cP.

[0012] Aspect 4: The polyvinylidene fluoride polymer of any one of Aspects 1-3, having a Delta H (first heat) greater than 58 J / g.

[0013] Example 5: The polyvinylidene fluoride polymer of any one of Examples 1-4, wherein the polymer comprises at least 97% by weight of vinylidene fluoride monomer units.

[0014] Embodiment 6: The polyvinylidene fluoride polymer of any one of embodiments 1 to 5, wherein the polymer is a homopolymer.

[0015] Embodiment 7: The polyvinylidene fluoride polymer of any one of embodiments 1 to 5, comprising at least one non-fluorinated monomer.

[0016] Example 8: The polyvinylidene fluoride polymer of example 7, wherein the at least one non-fluorinated monomer comprises at least one of acrylic acid (AA), carboxyethyl acrylate (CEA), and acryloyloxyethyl succinate (AES).

[0017] Embodiment 9: The polyvinylidene fluoride polymer according to any one of embodiments 1 to 8, wherein the polymer is in the form of precipitated particles having an average precipitate particle size having an average size in the range of 50 μm to 2500 μm, preferably 100 μm to 2200 μm.

[0018] Example 10: The polyvinylidene fluoride polymer of any one of Examples 1 to 9, wherein the intensity ratio is greater than 6.

[0019] Aspect 11: A precipitation polymerization process for producing PVDF having a β-phase, comprising the steps of: feeding water to a reactor, purging said reactor with gas to remove oxygen, heating said reactor, charging said reactor with vinylidene fluoride and optional non-fluorinated monomer until a desired pressure is reached, charging an initiator solution to said reactor, and optionally continuously feeding the initiator solution during the polymerization rate, wherein the temperature of the polymerization reaction is kept constant between 50°C and 70°C, and the pressure is maintained at 280 to 40,000 kPa during the reaction, feeding monomer to maintain the pressure, continuing the polymerization reaction until the consumption of VDF reaches a set level, venting excess gas, and recovering the precipitated polymer by collecting the precipitated solid during the polymerization reaction. Including, The method wherein the amount of initiator used in the polymerization is at least 2000 ppm.

[0020]

[0036] Aspect 12. The method of aspect 11, wherein the aqueous initiator solution comprises an inorganic persulfate salt.

[0021] Aspect 13: The method of any one of aspects 11 or 12, wherein the initiator comprises at least one of hydrogen peroxide, sodium persulfate, potassium persulfate, or ammonium persulfate.

[0022] Aspect 14: The method according to any one of aspects 11 to 13, wherein the temperature range is 53°C to 69°C, preferably 58°C to 68°C.

[0023] Embodiment 15: The method according to any one of embodiments 11 to 14, wherein the amount of initiator is from 2000 ppm to 10000 ppm, preferably from 3000 to 8000 ppm, based on the weight of the total monomers.

[0024] Example 16 The method of any one of Examples 11-15, wherein no surfactant is added to the reactor.

[0025] Example 17 The method of any one of Examples 11 to 16, wherein the non-fluorinated monomer is provided at the beginning and / or during the reaction.

[0026] Embodiment 18: The method of any one of embodiments 11 to 17, wherein the amount of non-fluorinated monomer added is from 0.05 to 5 weight percent, preferably from 0.1 to 3 weight percent, based on the total monomers used.

[0027] Example 19: The method of any one of examples 11 to 18, wherein the non-fluorinated monomer comprises at least one non-fluorinated monomer selected from the group consisting of acrylic acid (AA), carboxyethyl acrylate (CEA), and acryloyloxyethyl succinate (AES).

[0028] Aspect 20: A slurry composition for manufacturing a lithium ion battery, comprising the polyvinylidene fluoride polymer according to any one of aspects 1 to 10, an electrode active material, a non-aqueous solvent, and optionally a conductivity-imparting additive and / or a viscosity modifier.

[0029] Embodiment 21: The slurry composition of embodiment 20, comprising: (a): a polyvinylidene fluoride polymer in an amount of 0.5 to 5% by weight, preferably 0.5 to 3% by weight, based on the total weight of (a)+(b)+(c); (b): a conductivity-imparting additive in an amount of 0.5 to 5% by weight, preferably 0.5 to 3% by weight, based on the total weight of (a)+(b)+(c); (c): An electrode active material in an amount of 90-99% by weight, preferably 95-99% by weight.

[0030] Aspect 22: An electrode for a lithium ion battery, obtained by applying the slurry composition according to aspect 21 onto a current collector and drying it.

[0031] Example 23: A lithium ion battery having the electrode of example 22.

[0032] Example 24: An article comprising the polyvinylidene fluoride polymer of any one of Examples 1-10.

[0033] Aspect 25: A method for producing a battery electrode, comprising the steps of: i) providing the polyvinylidene fluoride polymer according to any one of aspects 1 to 10, wherein the polyvinylidene fluoride polymer is in the form of precipitated particles having an average particle size of 50 μm to 2500 μm; ii) combining the polyvinylidene fluoride polymer of step i) with a solvent and an electrode material to provide an electrode-forming composition, wherein the polyvinylidene fluoride polymer is dissolved in a solvent; iii) applying the electrode-forming composition onto at least one surface of a conductive substrate; and iv) Evaporating the solvent in the electrode-forming composition to form a composite electrode layer on the conductive substrate. [Brief description of the drawings]

[0034] [Figure 1] These are the spray dried powder particles from a typical emulsion process. [Diagram 2] Typical powder particles from a suspension process. [Diagram 3] These are particles collected from the precipitation process. [Figure 4] These are the primary particles from a typical emulsion process. [Diagram 5]These are primary particles from the precipitation process exhibiting a raspberry morphology. [Figure 6] FTIR spectrum (alpha form) from a typical emulsion polymerization. [Figure 7] FTIR spectrum (beta type) from precipitation polymerization. [Figure 8] This is a typical wide-angle X-ray diffraction (alpha type) obtained by emulsion polymerization. [Figure 9] Wide-angle X-ray diffraction (beta type) due to precipitation polymerization. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0035] All references cited in this application are incorporated herein by reference. Unless otherwise indicated, all percentages in compositions are percentages by weight.

[0036] The term "polymer" is used to mean both homopolymers and copolymers. "Copolymer" is used to mean a polymer having two or more different monomer units. The polymer may be linear, branched, star, comb, block, crosslinked, or other architecture. The polymer may be homogeneous or heterogeneous and may have a gradient in the distribution of the comonomer units.

[0037] The terms "polyvinylidene fluoropolymer" and "PVDF" refer to polymers formed by the polymerization of at least one vinylidene fluoride monomer, and include homopolymers, copolymers, terpolymers, and higher polymers that are thermoplastic in nature, i.e., they can be formed into useful parts by the application of heat to cause them to flow, as occurs in molding and extrusion processes.

[0038] The present invention describes novel PVDF polymers and methods for producing vinylidene fluoride-based polymers via a precipitation polymerization process. The precipitation polymerization process / technique relies on the formation of polymer aggregates of precipitated polymer particles. The resulting polymer is in the form of porous particles consisting of aggregated non-porous primary particles as observable under magnification (SEM) (referred to herein as "precipitated particles"). In some embodiments of the present invention, the polymer is a vinylidene fluoride homopolymer with a high melting temperature (greater than 165°C by DSC) and an unexpectedly high melt viscosity, a high melting point, and a predominantly β-phase as detected by WAXD (wide angle X-ray diffraction). Homopolymers and copolymers can be produced using the method of the present invention. The present invention can be used in battery applications for electrodes and / or separators. The polymers of the present invention provide excellent peel adhesion in cathode binders. Positive electrodes made using this polymer can be used as part of a lithium ion battery.

[0039] Precipitation Polymerization Reaction Precipitation polymerization, as used in this invention, is a heterogeneous polymerization process that initially begins as a homogeneous system in a continuous phase, and after initiation, the polymer formed becomes insoluble and precipitates. Precipitation occurs as part of the polymerization reaction, not a post-polymerization step. No additives are added to initiate precipitation.

[0040] In a precipitation polymerization process, the following steps are generally followed: Deionized water, optionally a chain transfer agent, and optionally an antifouling agent are first added to the reactor, followed by deoxygenation (removal of oxygen). After the reactor reaches the desired temperature, monomers (vinylidene fluoride and optionally non-fluorinated monomers) are added to the reactor to reach a predetermined pressure. Once the desired reaction pressure is reached, an initiator solution or combination of initiator solutions is added to start and maintain the polymerization reaction. After the desired level of monomer is delivered, the monomer delivery is stopped; however, the initiator charge can be stopped or continued to consume unreacted monomer. After the initiator charge is stopped, the reactor can be cooled and agitation stopped. Polymer precipitates during the polymerization process. The unreacted monomer can be discharged and the precipitated polymer can be collected through a vent or other collection means.

[0041] The precipitation polymerization process can be a batch, semi-batch or continuous polymerization process.

[0042] The reactors used for the polymerization are pressurized polymerization reactors. The reactors are usually equipped with agitators and heat control means. The agitation may be constant or may be varied during the course of the polymerization to optimize process conditions.

[0043] The polymerization temperature may vary depending on the characteristics of the initiator used, but is typically 50-70°C. The polymerization temperature is preferably 53-69°C, more preferably 58-68°C. The polymerization pressure may vary in the range of 280-40,000 kPa depending on the capacity of the reactor, the initiator system selected, and the monomer selection. The polymerization pressure is preferably 2,000-20,000 kPa, and most preferably 3,500-11,000 kPa.

[0044] Surfactants The process of the present invention is carried out in the absence of surfactants.

[0045] CTA A chain-transfer agent ("CTA") may optionally be added to the polymerization to control the molecular weight of the product. The chain-transfer agent may be added to the polymerization all at once at the beginning of the reaction, or may be added in stages or continuously throughout the reaction. The amount and method of addition of the chain-transfer agent depends on the activity of the particular chain-transfer agent used, and the desired molecular weight of the polymer product. A CTA is not required for the polymerization, but if one is used, the amount of chain-transfer agent added to the polymerization reaction is preferably about 0.05 to about 5 weight percent, more preferably about 0.1 to about 2 weight percent, based on the total weight of monomers added to the reaction mixture. Examples of chain-transfer agents useful in the present invention include, but are not limited to: oxygenated compounds such as alcohols, carbonates, ketones, esters, ethers, halocarbons, hydrohalocarbons (chlorocarbons, hydrochlorocarbons, chlorofluorocarbons, hydrochlorofluorocarbons, etc.); ethane, propane. Preferably, the chain-transfer agent is propane or ethyl acetate.

[0046] If desired, a paraffin antifoulant may be used, but is not preferred. Also, any long chain saturated hydrocarbon wax or oil may be used. The reactor charge of paraffin may be from 0.01% to 0.3% by weight of the total weight of monomers used.

[0047] Initiator The reaction can be initiated and maintained by adding any suitable initiator known for the polymerization of fluorinated monomers, including organic peroxides, inorganic peroxides, and hydrogen peroxide. Examples of typical inorganic peroxides include persulfates such as sodium persulfate, potassium persulfate, or ammonium persulfate.

[0048] The amount of initiator required for precipitation polymerization is related to its activity and the temperature used for polymerization. Examples of typical inorganic persulfates include sodium persulfate, potassium persulfate, or ammonium persulfate, which have useful activity in the temperature range of 65°C to 105°C. Radical polymerization requires sufficient radical generation (radical flux) initially to cause polymerization. The total amount of initiator is generally 0.2% to 5.0% by weight of the total monomer weight used in the polymerization, depending on the reaction temperature, the chain transfer agent, and the efficiency of the initiator. Increasing the initial charge to offset slow polymerization reaction rates is a method used in the present invention. High initiator loadings of 0.20 to 2.0%, preferably 0.25 to 1.0%, are used in the present invention. A mixture of one or more initiators as described above can be used to carry out polymerization at a desired rate. Typically, a sufficient amount of initiator is added initially to start the reaction, and then additional initiator can be added, optionally, to maintain polymerization at a convenient or desired rate.

[0049] monomer The present invention relates to the preparation of vinylidene fluoride polymers. The primary monomer used in the present invention (meaning 97% by weight or more of the polymer) is vinylidene fluoride ("VDF"). Other non-fluorinated ethylenically unsaturated monomers may be present ("non-fluorinated monomers"). Polymers formed by polymerization of vinylidene fluoride and optionally non-fluorinated monomers include homopolymers, copolymers, terpolymers, and higher polymers that are thermoplastic in nature, i.e., they can be formed into useful parts by applying heat to cause them to flow, as occurs in molding and extrusion processes.

[0050] The fluoropolymer contains at least 97 weight percent, preferably at least 98 weight percent, more preferably at least 99 weight percent vinylidene fluoride and is thermoplastic. Thermoplastic polymers exhibit a crystalline melting point as measured by differential scanning calorimetry (DSC).

[0051] The non-fluorinated monomers may be added at the beginning and / or during the polymerization reaction.

[0052] The polymer of the present invention may comprise a non-fluorinated monomer unit. Preferably, the polymer may optionally comprise a non-fluorinated monomer having a hydroxyl group, a carboxylic acid functional group or a carboxyl functional group, and most preferably, the non-fluorinated monomer comprises a carboxylic acid functional group. The non-fluorinated monomer may be used in combination with VDF and includes, but is not limited to, one or more of the non-fluorinated monomers of the following formula: [ka] During the ceremony: R1, R2, and R3 each independently represent a hydrogen atom, a linear alkyl group, a branched alkyl group, or a cycloalkyl group having 1 to 8 carbon atoms; R4 and R6 are each independently a bond, and R4 and R6 are each independently a bond or an atomic group having a molecular weight of 500 or less and a main chain of 1 to 18 atoms; when R4 or R6 is hydrogen, the respective R5 or R7 is absent; When R4 and R6 are not hydrogen, R5 and R7 are each one of the following: a carboxylic acid (C(O)OH), an alkali metal carboxylate (COO - M + ), ammonium carboxylate (COO - NH4 + ), alkyl ammonium carboxylates (COO - N(Alk)4 + ), alcohols (OH), amides (C(O)NH2), dialkylamides (C(O)NAlk2), sulfonic acids (S(O)(O)OH), alkali metal sulfonates (S(O)(O)O - M + ), sulfonic acid ammonium salt (S(O)(O)O - NH4 + ), alkyl ammonium sulfonate (S(O)(O)O - N(Alk)4 +), ketones (C(O)), or acetylacetonates (C(O)-CH2-C(O)), or phosphonates (P(O)(OH)2), alkali metal or ammonium phosphonates, preferably R5 and R7 are independently carboxylic acids (C(O)OH), alkali metal carboxylates (COO - M + ), ammonium carboxylate (COO - NH4 + ), alkyl ammonium carboxylates (COO - N(Alk)4 + ), alcohol (OH), amide (C(O)NH2); most preferably, R5 and R7 are independently carboxylic acid (C(O)OH), alkali metal carboxylate (COO - M + ), ammonium carboxylate (COO-NH4+), or alcohol (OH).

[0053] Examples of non-fluorinated monomers include: acrylic acid, methacrylic acid, 2-carboxyethyl acrylate "CEA", acryloyloxypropyl succinate "APS", acryloyloxyethyl succinate "AES", hydroxyethyl (meth)acrylate, hydroxypropyl (meth)acrylate; hydroxyethylhexyl (meth)acrylate, acrylic esters (such as (meth)acrylic acid alkyl esters), vinyl esters (such as vinyl acetate, vinyl propionate, vinyl butyrate); acrylamide, methacrylamide, 6-acrylamidohexanoic acid.

[0054] Useful non-fluorinated monomers include those disclosed in WO2019199753, which is incorporated herein by reference.

[0055] Buffer The polymerization reaction mixture may optionally contain a buffer to maintain a controlled pH throughout the polymerization reaction. The pH is preferably controlled within the range of about 2 to about 8 to minimize undesirable color development in the product.

[0056] The buffer may comprise an organic or inorganic acid or an alkali metal salt thereof, or a base or salt of such an organic or inorganic acid, having at least one pKa and / or pKb value in the range of about 4 to about 10, preferably about 4.5 to about 9.5. Preferred buffers in the practice of the present invention include, for example, phosphate buffers and acetate buffers. A "phosphate buffer" is a salt of phosphoric acid, such as dipotassium hydrogen phosphate. An "acetate buffer" is a salt of acetic acid, such as sodium acetate.

[0057] PVDF Polymer Properties A novel polymer composition is provided by a novel polymerization method. The composition comprises a PVDF polymer. The PVDF polymer of the present invention is characterized by having a melting temperature of 165°C to 175°C, preferably 168°C to 174°C, and having a raspberry morphology.

[0058] The present invention is characterized by the β phase crystal peak intensity ratio: I β(200 / 110) / [I α(020) +I γ(020)

[0023] The present invention provides a polymer having a predominantly β-phase crystallinity, as measured by β-phase crystallinity (β-phase crystallinity) of greater than 5 (preferably greater than 6 using WAXD as described in the examples).

[0059] In one embodiment, the polymer has a melt viscosity of 53 to 150 kPoise at 100 s and 900 to 3500 kPoise at 4 s. The solution viscosity (cP) of the polymer of the invention in a 9% NMP solution (measured at 3.36 / s) is at least 7000 cP, preferably greater than 9000 cP.

[0060] PVDF polymer is thermoplastic and melt processable.

[0061] The PVDF polymer contains at least 97% by weight, preferably at least 99% by weight, of VDF. The PVDF polymer contains up to 100% by weight of VDF. Preferably, the only fluorinated monomer present in the polymer is VDF (vinylidene fluoride).

[0062] When non-fluorinated monomers are used, the amount of non-fluorinated monomers in the PVDF polymer is 0.001-3 weight percent, preferably 0.01-1.5 weight percent. 19 F NMR and 1 It can be measured using 1 H NMR.

[0063] Unexpectedly high delta H. The ΔH in DSC measurements is higher than that from conventional α-phase PVDF, indicating that β-phase structure has developed instead of the conventional α-phase. Preferably, ΔH(melt)(J / g)(1st heat) is 58 or higher.

[0064] The primary particle size of PVDF polymer from precipitation polymerization process has a wide size distribution, measured by number average particle size, ranging from 100nm to 800nm, preferably from 100nm to 700nm, preferably from 200nm to 600nm. In precipitation polymerization, the primary particles aggregate during the polymerization process and grow large enough to precipitate as "precipitated particles". The average precipitate particle size is 50μm to 2500μm, preferably from 100μm to 2200μm, more preferably from 200μm to 1600μm.

[0065] No post-polymerization process is used to solidify the polymer.

[0066] Suspension polymerization is different from precipitation polymerization. Suspension polymerization is a suitable technique for the production of polymer particles. In suspension polymerization, the monomer phase is suspended in the polymerization medium in the form of small droplets by a stirrer and suitable stabilizers, and both the initiator and monomer are insoluble in the polymerization medium, while the initiator is soluble in the monomer, and polymerization occurs in the monomer droplets. Spherical polymer particles with size 50-500 μm by suspension polymerization. In the present invention, the primary particle size is 100 nm-800 nm, and the precipitated particles are 50 μm-2500 μm, preferably 100 μm-2200 μm, more preferably 200 μm-1600 μm.

[0067] The precipitated particle morphology has an irregular surface topography ("raspberry") consisting of agglomerated primary particles with irregular shapes, while the emulsion process yields primary particles with smooth surfaces as can be seen by SEM. Figures 1-4 show the difference in particle morphology between the emulsion and precipitation polymerization processes. Figure 1 shows the average powder particle size on the order of 1-30 μm obtained by spray drying a standard emulsion latex. In contrast, the average particle size recovered from the precipitation polymerization in Figure 3 is on the order of 50-2200 μm. Figure 2 shows the powder particles from a typical suspension. Figures 4 and 5 show the difference in primary particle morphology. Primary latex particles obtained from the standard emulsion process produce round particles with a narrow size distribution in the range of 100-500 nm (as shown in Figure 4). Precipitation polymerization produces precipitated particles composed of a wide range of primary particle sizes, interconnected and agglomerated, with a raspberry morphology (see Figure 5).

[0068] The polymers or copolymers of the present invention can be isolated using standard methods such as filtration or centrifugation and then oven dried for subsequent application or use.

[0069] Preferably, no fluorinated molecules are added to the polymerization process other than the PVDF monomer and the resulting polymer.

[0070] The polymers of the present invention can be used to prepare anodes, cathodes and / or separators for lithium ion batteries.

[0071] The polymers of the present invention, used as binders in cathodes, provide improved adhesion as measured by ASTM D903 with the modifications described below. Peel adhesion strength is measured using a control (melt viscosity 50 kP (100 s -1 PVDF homopolymer by emulsion polymerization at 100° C.), preferably 150% of the control, more preferably 200% of the control. In some embodiments, the peel can be greater than 150 N / m, preferably greater than 160 N / m, and preferably greater than 175 N / m.

[0072] A typical cathode formulation is active material / conductive material / binder: active material accounts for the majority of the total, at 90-99.5% by weight, binder is typically in the range of 0.5-5% by weight, and the ratio of conductive material to binder is 4:1 to 1:4. An example formulation would be 97 / 1.5 / 1.5 active material / conductive material / binder on a dry weight basis.

[0073] Generally, the binder (polymer of the present invention) is pre-dissolved in a solvent (such as NMP or other suitable solvent) at a concentration typically between 5-10% by weight. The conductive carbon additive is first dry mixed with the active material (a lithium-containing metal oxide compound known for use in lithium-ion batteries). The binder solution is mixed with the dry mixture of conductive carbon and active material to form a thick, homogenous paste. Alternatively, the conductive carbon can be mixed with the binder and solvent, and then the active material is added to form the paste. In either case, additional amounts of solvent are added to the paste and mixed to gradually reduce the solids content and viscosity of the slurry. This dilution step is repeated multiple times until the slurry viscosity reaches a level suitable for coating, typically between 3,000-15,000 cP at a shear rate of 1 / s.

[0074] The cathode slurry is then cast onto a current collector to form the cathode using means known in the art. Typical area mass loading of the cathode is 100-300 g / m2, preferably 180-220 g / m2.

[0075] The anode and separator can similarly be manufactured according to methods known in the art using the polymers of the present invention as binders. EXAMPLES

[0076] Characterization methods / conditions: The melt viscosity of the resin was measured by capillary rheometry at 232° C., 100 s−1 and 4 s−1 according to ASTM-D3835.

[0077] Melting temperature measured by differential scanning calorimetry DSC, powder sample. Thermal properties including melting point and delta H were measured according to ASTM D3418 using a TA Instruments DSC Q2000 and LNCS. Polymers made according to the present invention contain a measurable level of crystalline polyvinylidene fluoride as indicated by the presence of a crystalline melting point in the (DSC) experiment. The melting temperature is assigned to the endothermic peak of the second cycle. The heat of fusion is determined in the first cycle. The DSC run is performed in a three step cycle. The cycle starts at -20°C, then ramps at 10°C / min to 210°C and holds for 10 minutes. The sample is then cooled at a rate of 10°C / min to -20°C, then heated at 10°C / min to 210°C.

[0078] Particle size (number average) results are based on scanning electron microscopy (SEM) measurements. SEM was performed on a Hatachi SU8010 SEM. All polymer samples for SEM were dried at room temperature to coat the samples before imaging.

[0079] Intensity ratio and wide-angle X-ray diffraction experiments were performed on a Riraku SmartLab diffraction platform (Cu Kα 1.5418 Å, 40 kV, 40 mA). Samples are loaded into a low background holder for WAXS analysis in reflection mode. The diffractometer used for WAXS analysis is a Riraku SmartLab equipped with a copper X-ray tube (Cu Kα 1.5418 Å) set at 40 kV and 40 mA at the line focus (the X-ray beam is used at the line focus, with dimensions 12 mm long and 1 mm wide). The experiments are performed in theta-theta (reflection) geometry with parallel beam optics (curved parabolic multilayer mirror, converting the naturally diverging X-ray beam into a parallel X-ray beam with very low divergence). 1D reflection mode. The entrance slit (IS) is set at 1 mm aperture, the length limiting slit at 10 mm aperture, and the two receiving slits (RS1 and RS2) at 3 mm aperture. The detector is a Rigaku Hypix3000 used in 1D mode. Data are collected in continuous mode from 5.0° to 80.0° 2θ, with 0.02° steps and a scan speed of 0.5° / min. The ratio of β-PVDF to α-PVDF and / or γ-PVDF was calculated as the intensity ratio: the sum of β-PVDF(200) and β-PVDF(110) divided by the sum of α-PVDF(020) and γ-PVDF(020). β(200 / 110) / [I α(020) +I γ(020) ]=Intensity ratio.

[0080] Solution viscosity is measured at 25°C using a Brookfield viscometer with a Brookfield DVII viscometer SC4-25 spindle at 3.36 s-1. Solution Viscosity Sample Preparation: PVDF resin is dissolved in 1-methyl-2-pyrrolidinone at 9% by weight. The resin / solvent mixture is mixed on a roll mixer at room temperature for a minimum of 72 hours to ensure complete dissolution.

[0081] Examples 1 to 3 The experiment was carried out in a 1.7 L stainless steel reactor to which 1000 g of water was added. The reactor was purged with nitrogen gas. The reactor was sealed and stirring was started at 72 RPM. Stirring was maintained throughout the reaction. The reactor was heated to the desired temperature as shown in Table 1. The reactor was charged with vinylidene fluoride to reach the desired pressure of about 650 psi. After pressurization, the reactor was charged with initiator solution. The initiator solution was 1% potassium persulfate in aqueous initiator solution (ACS grade, from EMD Chemicals). A continuous feed of aqueous initiator solution was added to the reaction to obtain an adequate polymerization rate. The reaction temperature was maintained at the desired temperature and the reaction pressure was maintained at 650 psi by adding vinylidene fluoride as needed. When the amount of VDF consumed reached the desired level, the VDF feed was stopped. Stirring was continued and temperature was maintained for 30 minutes. Stirring and heating were then discontinued. After cooling to room temperature, the excess gas was vented. All solid material produced by the reaction was collected in a suitable receiver. The solid material from the reactor was dried in a convection oven.

[0082] Comparative Example 1 is the same as Example 1 except that it is carried out at 73° C. Comparative Examples 2 and 3 are commercial grade PVDF homopolymers made by typical emulsion polymerization.

[0083] [Table 1A]

[0084] [Table 1B]

[0085] Examples 4 to 6 The experimental procedure is very similar to that described in Examples 1-4. To a 1.7 L stainless steel reactor, 1000 g of water was added. The reactor was purged with nitrogen gas. The reactor was sealed, stirring was started at 72 RPM, and the reactor was heated to 63° C. The reactor was charged with vinylidene fluoride to reach the desired pressure of 650 psi. After pressurization, the reactor was charged with initiator solution. The initiator solution was 1% potassium persulfate in aqueous initiator solution (ACS grade, from EMD Chemicals). A continuous feed of aqueous initiator solution was added to the reaction to obtain an adequate polymerization rate. Comonomers prepared as 1% solutions were added during the reaction. The reaction temperature was maintained at 63° C. and the reaction pressure was maintained at 650 psi by adding vinylidene fluoride and optionally non-fluorinated monomers as needed. When the amount of VDF consumed reached the desired level, the monomer feed was stopped. Stirring was continued and the temperature was maintained for 30 minutes, after which the stirring and heating were discontinued, and after cooling to room temperature the excess gas was vented and the polymeric material produced by the reaction was collected in a suitable receiving vessel.

[0086] [Table 2]

[0087] CEA is 2-carboxyethyl acrylate.

[0088] AA is acrylic acid.

[0089] The PVDF polymer of the present invention can be used to manufacture battery electrodes or battery separators. The dried polymer is used to prepare a cathode slurry.

[0090] Cathode Formulation and Fabrication Here, two examples of laboratory-scale cathode slurry preparation procedures are described. Process #1 first mixes the carbon black with the binder solution and then mixes it with the active material. Process #2 mixes the carbon black and active material as dry powders and then mixes it with the binder solution. Both processes are used in the lithium-ion battery industry. The following procedures are for laboratory scale with a target mix of NMC622 (lithium active material) / SuperP (carbon black) / binder = 97 / 1.5 / 1.5 on a dry basis.

[0091] Slurry Process #1: 0.36g of conductive carbon additive, SuperP-Li from Timcal, was added to 4.50g of 8.0% binder solution and mixed using a centrifugal planetary mixer Thinky AR-310 at 2000 rpm for 120 seconds, three times with 1 minute air cooling in between. Once the conductive carbon was dispersed in the binder solution, 23.28g of active material, Celcore® NMC622 (Umicore) and a small amount of NMP (0.5g) were added to the mixture and typically mixed at 2000 rpm for 60 seconds to form a thick, homogenous paste. A small amount of NMP (0.5g) was then added to the paste and mixed at 2000 rpm for 60 seconds to gradually reduce the slurry solids and viscosity. This dilution step is repeated multiple times until the slurry viscosity reaches a suitable level for coating, typically 3,000-15,000 cP at a shear rate of 1 / s. Typically, the final solids level of the NMC622 / SuperP / binder=97 / 1.5 / 1.5 blend is about 80% by weight.

[0092] Slurry Process #2: 0.36g of conductive carbon additive, such as Timcal's SuperP-Li, was first dry mixed with 23.28g of active material, such as Celcore® NMC622 (Umicore), using a centrifugal planetary mixer Thinky AR-310, for 60 seconds at 1500 rpm, repeated twice. Next, 4.50g of an 8% binder solution was added and mixed to form a thick, homogenous paste, typically at 2000 rpm for 60 seconds. A small amount of NMP (0.5g) was then added to the paste and mixed for 60 seconds / 2000 rpm to gradually reduce the slurry solids and viscosity. This dilution step was repeated multiple times until the slurry viscosity reached a suitable level for coating, typically 3,000-15,000 cP at a shear rate of 1 / s.

[0093] Electrode casting and drying: The cathode slurry was then cast onto an aluminium foil (current collector, 15 μm thick) using an adjustable doctor blade on an automatic film applicator (Elcometer 4340) at a coating speed of 0.3 m / min. The doctor blade gap was adjusted to give a dry thickness of approximately 80 μm, or a mass loading of approximately 200 g / m. 2 The density was empirically adjusted to be 0.001 g / cm. The wet castings were then transferred to a convection oven and dried at 120 °C for 30 min. After drying, the electrodes were calendered using a roll mill (Hohsen HSTK-1515H). The final density of NMC622-based electrodes was typically around 3.4 g / cm. 3 It is.

[0094] Peel adhesion data was obtained from the peel test method described below. For the peel test, cathode samples made using the polymers of the present invention were cut into stripes 1 inch wide and 5-8 inches long. The samples were dried overnight in a vacuum oven at approximately 85°C and stored in a dry room. The peel strength of the cathodes was obtained by a 180° peel test following ASTM D903 with some modifications. The first modification was that the extension rate used was 50 mm / min (peel rate was 25 mm / min). The second modification was that the test samples were dried (as above) prior to the peel test and the peel test was performed in a dry room, since variations in exposure to ambient humidity can have a significant effect on the peel results. The 1 inch wide test stripes were adhered to an alignment plate via 3M 410M double-sided paper tape and the flexible aluminum foil current collector was peeled off with the grips of the testing machine. The mechanical testing machine was an Instron 3343 model equipped with a 10 N load cell. Peel results are reported in N / m.

[0095] [Table 3]

[0096] Comparative Example 2 is a PVDF homopolymer with a melt viscosity of 50 kPoise at 100 s-1 available from Arkema Inc.

[0097] The new VDF-containing polymers have demonstrated very good release results.

Claims

1. It has a melting temperature of 165°C to 175°C, preferably 168°C to 174°C, has a raspberry morphology, and has a β phase intensity ratio (I β(200 / 110) / [I α(020) +I γ(020) ])

2. 2. The polyvinylidene fluoride polymer of claim 1 having a melt viscosity of 53 to 150 KPoise at 100 s-1 and 900 to 3500 KPoise at 4 s-1.

3. 2. The polyvinylidene fluoride polymer of claim 1, having a solution viscosity at 9 wt. % in NMP (measured at 3.36 / s) of at least 7000 cP, preferably greater than 9000 cP.

4. 2. The polyvinylidene fluoride polymer of claim 1 having a Delta H (first heat) greater than 58 J / g.

5. 2. The polyvinylidene fluoride polymer of claim 1, wherein the polymer comprises at least 97% by weight of vinylidene fluoride monomer units.

6. The polyvinylidene fluoride polymer of any one of claims 1 to 5, wherein the polymer is a homopolymer.

7. The polyvinylidene fluoride polymer of any one of claims 1 to 5, comprising at least one non-fluorinated monomer.

8. 8. The polyvinylidene fluoride polymer of claim 7, wherein the at least one non-fluorinated monomer comprises at least one of acrylic acid (AA), carboxyethyl acrylate (CEA), and acryloyloxyethyl succinate (AES).

9. 8. The polyvinylidene fluoride polymer of claim 7, wherein the polymer is in the form of precipitated particles having an average precipitate particle size having an average size in the range of 50 μm to 2500 μm, preferably 100 μm to 2200 μm.

10. 10. The polyvinylidene fluoride polymer of claim 9, wherein the intensity ratio is greater than 6.

11. A precipitation polymerization process for producing PVDF having a β-phase, comprising the following steps: feeding water to a reactor, purging said reactor with gas to remove oxygen, heating said reactor, charging said reactor with vinylidene fluoride and optional non-fluorinated monomer until a desired pressure is reached, charging said reactor with an initiator solution, and optionally continuously feeding the initiator solution during the polymerization rate, wherein the temperature of the polymerization reaction is kept constant between 50° C. and 70° C., and the pressure is maintained between 280 and 40,000 kPa during the reaction, feeding monomers to maintain the pressure, continuing the polymerization reaction until the consumption of VDF reaches a set level, venting excess gas, and recovering the precipitated polymer by collecting the precipitated solid during the polymerization reaction. Including, The method wherein the amount of initiator used in the polymerization is at least 2000 ppm.

12. The method of claim 11 , wherein the aqueous initiator solution comprises an inorganic persulfate.

13. 12. The method of claim 11, wherein the initiator comprises at least one of hydrogen peroxide, sodium persulfate, potassium persulfate, or ammonium persulfate.

14. The method according to claim 11, wherein the temperature range is from 53°C to 69°C, preferably from 58°C to 68°C.

15. A process according to any one of claims 11 to 14, wherein the amount of initiator is from 2000 ppm to 10000 ppm, preferably from 3000 to 8000 ppm, based on the weight of the total monomers.

16. The process according to any one of claims 11 to 14, wherein no surfactant is added to the reactor.

17. The process according to any one of claims 11 to 14, wherein the non-fluorinated monomer is provided at the start of the reaction and / or during the reaction.

18. The process according to any one of claims 11 to 14, wherein the amount of non-fluorinated monomer added is from 0.05 to 5 weight percent, preferably from 0.1 to 3 weight percent, based on the total monomers used.

19. 15. The method of any one of claims 11 to 14, wherein the non-fluorinated monomer comprises at least one non-fluorinated monomer selected from the group consisting of acrylic acid (AA), carboxyethyl acrylate (CEA), and acryloyloxyethyl succinate (AES).

20. A slurry composition for manufacturing a lithium ion battery, comprising the polyvinylidene fluoride polymer according to claim 1, an electrode active material, a non-aqueous solvent, and optionally a conductivity-imparting additive and / or a viscosity modifier.

21. 21. The slurry composition of claim 20 comprising: (a): a polyvinylidene fluoride polymer in an amount of 0.5 to 5% by weight, preferably 0.5 to 3% by weight, based on the total weight of (a)+(b)+(c); (b): a conductivity-imparting additive in an amount of 0.5 to 5 wt. %, preferably 0.5 to 3 wt. %, based on the total weight of (a)+(b)+(c); (c): An electrode active material in an amount of 90-99% by weight, preferably 95-99% by weight.

22. 22. An electrode for a lithium ion battery, obtained by applying the slurry composition according to claim 21 onto a current collector and drying it.

23. 23. A lithium ion battery comprising the electrode of claim 22.

24. 13. An article comprising the polyvinylidene fluoride polymer of claim 1.

25. A method for manufacturing a battery electrode, comprising the steps of: i) providing the polyvinylidene fluoride polymer of claim 1, wherein the polyvinylidene fluoride polymer is in the form of precipitated particles having an average particle size of from 50 μm to 2500 μm; ii) combining the polyvinylidene fluoride polymer of step i) with a solvent and an electrode material to provide an electrode-forming composition, wherein the polyvinylidene fluoride polymer is dissolved in a solvent; iii) applying the electrode-forming composition onto at least one surface of a conductive substrate; and iv) evaporating the solvent in the electrode-forming composition to form a composite electrode layer on the conductive substrate.

Citation Information

Patent Citations

  • Polyvinylidene fluoride synthesis process

    CN112521537A

  • A continuous process for producing polymers in carbon dioxide

    JP2003514083A

  • Method of thin film formation

    JP2005200623A

  • Aqueous polyvinylidene fluoride composition

    JP2012528466A

  • High dielectric film

    JP2014156599A