Polyethylene yarn with improved weaving properties and functional fabric containing the same

A polyethylene yarn with controlled PDI, strength, and elongation rate addresses the poor weaving and fuzzing issues of conventional fibers, providing improved thermal conductivity and comfort in fabrics.

JP2024541731AActive Publication Date: 2024-11-11KOLON INDUSTRIES INC
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
JP2024530503
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2021-12-02
Filing Date
2022-12-01
Publication Date
2024-11-11
Estimated Expiration
2042-12-01

AI Technical Summary

Technical Problem

Conventional high molecular weight polyethylene fibers exhibit low elongation rates and poor weaving properties due to high crystallinity and orientation, resulting in fabrics with low flexibility and wearing comfort, and high frequency of fuzzing.

Method used

A polyethylene yarn with a polydispersity index (PDI) of 5 to 20, strength of 1.5 to 10 g/d, and elongation rate of 10 to 50% is developed, with specific molecular weight distribution and crystallinity, enabling improved thermal conductivity, weavability, and reduced fuzzing.

Benefits of technology

The yarn achieves excellent thermal conductivity, improved weavability, and reduced fuzzing, allowing for fabrics with enhanced cooling sensation and wearing comfort.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024541731000001_ABST
    Figure 2024541731000001_ABST
Patent Text Reader

Abstract

The present invention relates to a polyethylene yarn having improved weaving properties and a functional fabric containing the same, and more particularly to a polyethylene yarn having improved weaving properties that can provide a user with an appropriate cool feeling and excellent wearing comfort and enable the production of a fabric with an extremely low incidence of fuzz, and a functional fabric containing the same.The polyethylene yarn according to the present invention has a polydispersity index (PDI) of 5 to 20, a tenacity of 1.5 to 10 g / d as measured according to ASTM D2256, and an elongation at maximum strength of 10 to 50%.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a polyethylene raw yarn having improved weaving properties and a functional fabric containing the same, and more particularly to a polyethylene raw yarn having improved weaving properties that can provide a user with an appropriate cool feeling and excellent wearing comfort and can produce a fabric with an extremely low frequency of fuzzing, and a functional fabric and a cool feeling product containing the same. [Background technology]

[0002] Recently, due to the improvement of living standards and population growth, the demand for textiles has been shifting from general-purpose yarns for general clothing and industrial fibers to advanced textile materials with high functionality and performance and various functions. In particular, the development of textile materials with a cooling sensation that gives users a comfortable feeling in summer and in high-temperature working environments is actively underway.

[0003] Cool-sensation fiber materials are imparted with a cool sensation by using the thermal conductivity of the fiber itself, or by adjusting the thermal conductivity of the surface of the fiber material through coating with a metal component having high thermal conductivity, etc. In particular, cool-sensation fiber materials that utilize the thermal conductivity of the fiber itself can be manufactured only through the weaving process of the fabric, and can maintain a cool sensation even after washing, so they are currently being produced in a variety of industrial fields.

[0004] Conventionally, as disclosed in Japanese Patent Publication JP2010-236130A and Korean Patent Publication No. 10-2017-0135342, there have been various attempts to apply the excellent thermal conductivity of high molecular weight polyethylene (HMWPE) fibers to fashion clothing and technical textile fields that require a high cooling sensation, such as sportswear, mountain climbing clothing, and workwear.

[0005] However, conventional high molecular weight polyethylene fibers have high strength because they are manufactured as raw yarns with maximized crystallinity and orientation to exhibit a cool feeling, and therefore have the disadvantages of low elongation of the raw yarns, which reduces weaving properties, and low flexibility, which makes the manufactured fabrics relatively uncomfortable to wear. Summary of the Invention [Problem to be solved by the invention]

[0006] An object of the present invention is to provide a polyethylene raw yarn with improved weaving properties that can provide a user with an appropriate cool feeling and excellent wearing comfort and that enables the production of a fabric with an extremely low frequency of fuzzing, a functional fabric containing the same, and a cool feeling product. [Means for solving the problem]

[0007] The polyethylene raw yarn according to the present invention has a polydispersity index (PDI) of 5 or more and 20 or less, a strength measured according to ASTM D2256 of 1.5 to 10 g / d, and an elongation at maximum strength of 10 to 50%.

[0008] In the polyethylene raw yarn according to one embodiment of the present invention, the polyethylene raw yarn satisfies the following Formula 1 in a weight distribution graph obtained by gel permeation chromatography (GPC) analysis in which the log scale of molecular weight (Mw) is on the x-axis and the weight distribution ratio (dw / dLogM) is on the y-axis, and the weight distribution graph may be unimodal.

[0009] [Formula 1] (M max -Mw aver )<(Mw aver -Mw min )

[0010] (In the above formula, Mw aver is the molecular weight having the maximum weight distribution in the weight distribution graph, and Mw max and Mw min , Mw averFor the weight distribution value Q in the weight distribution graph, the two molecular weights corresponding to 0.25Q are referred to as Mw maw The maximum of the two molecular weights is Mw min means the minimum value.)

[0011] In the polyethylene yarn according to one embodiment of the present invention, the yarn may have an initial modulus of 30 to 80 d / g as measured by ASTM2256.

[0012] In the polyethylene yarn according to one embodiment of the present invention, the yarn may have a crystallinity of 65 to 85%.

[0013] In the polyethylene yarn according to one embodiment of the present invention, the yarn has a density of 0.93 to 0.97 g / cm 3 It is possible.

[0014] In the polyethylene yarn according to an embodiment of the present invention, the yarn may have a weight average molecular weight of 90,000 to 400,000 g / mol.

[0015] The polyethylene fabric according to the present invention comprises the polyethylene yarn described above.

[0016] In the polyethylene fabric according to an embodiment of the present invention, the fabric has a cool touch sensation of 0.18 to 0.30 W / cm, measured at 20±2°C and 65±2% RH by contacting a 30±2°C hot plate (T-box) with the fabric at 20±2°C. 2 It is possible.

[0017] In the polyethylene fabric according to an embodiment of the present invention, the fabric may have a thermal conductivity of 0.05 to 0.20 W / mK in the thickness direction, measured at 20±2° C. and 65±2% RH by contacting a heat source plate (BT-box) of 30±2° C. with the fabric of 20±2° C.

[0018] In a polyethylene fabric according to an embodiment of the present invention, the fabric has a length of 100,000 m 2 The number of fluff particles generated per hit may be 10 or less.

[0019] In one embodiment of the present invention, the polyethylene fabric has an areal density of 150 to 800 g / m 2 It is possible.

[0020] The cooling sensation product according to the present invention is produced from the above-mentioned fabric. Effect of the Invention

[0021] The polyethylene yarn according to the present invention has excellent thermal conductivity, and at the same time, it has improved weaving properties, and can be used to produce fabrics with appropriate cool feeling properties and very low incidence of fluff.

[0022] In addition, the functional fabric according to the present invention contains polyethylene yarn having excellent thermal conductivity and high weaving property, so that the fabric has a cool feeling property and has excellent quality with few defects such as fuzz.

[0023] In addition, the functional fabric according to the present invention has not only a cooling sensation but also excellent drapeability, so that when a user wears a product made from such a fabric, the contact area between the user and the product is large, thereby providing a substantially more excellent cooling sensation effect. [Brief description of the drawings]

[0024] [Figure 1] 1 is a schematic diagram showing a polyethylene yarn production apparatus according to one embodiment of the present invention. [Diagram 2] FIG. 1 is a schematic diagram showing an apparatus for measuring the cool touch feeling of fabric. [Diagram 3] FIG. 1 is a schematic diagram showing an apparatus for measuring thermal conductivity in the thickness direction of a fabric. [Figure 4] 1 is a weight distribution graph through GPC analysis of raw yarn according to Example 3. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0025] Unless otherwise defined, technical and scientific terms used in this specification have the meanings that are commonly understood by those having ordinary knowledge in the technical field to which this invention belongs, and in the following description and attached drawings, descriptions of known functions and configurations that may unnecessarily blur the gist of the present invention will be omitted.

[0026] Additionally, as used herein, the singular forms "a," "an," and "the" are intended to include the plural forms as well, unless the context clearly indicates otherwise.

[0027] Furthermore, units used in this specification, unless otherwise specified, are based on weight. For example, the unit of % or ratio means % by weight or weight ratio, and % by weight means the weight % of any one component in a total composition unless otherwise defined.

[0028] In addition, the numerical ranges used herein include lower and upper limits and all values ​​within the range, increments logically derived from the form and width of the ranges defined, all values ​​that are doubly limited, and all possible combinations of upper and lower limits of numerical ranges that are limited in different forms. Unless otherwise specified in the specification of the present invention, values ​​outside the numerical ranges that may occur due to experimental error or rounding of values ​​are also included in the defined numerical ranges.

[0029] As used herein, the term 'comprising' is an open-ended term having the same meaning as terms such as 'comprising,' 'containing,' 'having,' or 'characterized by,' and does not exclude additional, unrecited elements, materials, or steps.

[0030] Conventional high molecular weight polyethylene fibers are manufactured into yarns by maximizing the degree of crystallinity and orientation to produce a cooling sensation, which results in high strength and low elongation, resulting in poor weaving properties. In addition, the degree of twist of the manufactured yarns is poor, which not only reduces weaving properties, but also results in poor drapeability and wearability of fabrics manufactured from the yarns. Therefore, when actually worn by a user, the contact area between the user and the fabric is not high, resulting in a poor actual cooling sensation felt by the user.

[0031] Therefore, the applicant conducted extensive research for a long period of time to develop a polyethylene fiber having excellent weaving properties while maintaining a cooling sensation property. As a result, the applicant discovered that a polyethylene fiber having a specific polydispersity index, strength, and elongation has appropriate thermal conductivity, excellent weaving properties, and can be manufactured into a fabric having excellent physical properties. As a result of further in-depth research into this, the applicant has completed the present invention.

[0032] In this specification, polyethylene raw yarn refers to monofilament or multifilament manufactured by using polyethylene chips as raw material through processes such as spinning and drawing. As an example, the polyethylene fiber may include 40 to 500 filaments each having a fineness of 1 to 3 denier, and may have a total fineness of 100 to 1,000 denier.

[0033] The polyethylene raw yarn of the present invention has a polydispersity index (PDI) of 5 or more and 20 or less, a strength of 1.5 to 10 g / d as measured by ASTM D2256, and an elongation at maximum strength of 10 to 50%, and at the same time has excellent thermal conductivity and improved weaving properties, and can be manufactured into a fabric having appropriate cool feeling properties and an extremely low frequency of pilling.

[0034] The cool sensation of the fabric containing the polyethylene yarn according to the present invention is a characteristic that the user wearing the fabric can feel an appropriate cool sensation, i.e., a cooling feeling, due to the high thermal conductivity of the yarn. Specifically, in the case of polymers, heat is transferred within the polymer (especially in the direction of molecular chains connected through covalent bonds) mainly through lattice vibrations called phonons. In other words, the thermal conductivity of the yarn can be adjusted to be different depending on the structural characteristics of the polymer itself, such as the degree of crystallinity and the degree of orientation, even if the yarn is made from the same resin.

[0035] As described above, a raw yarn having a polydispersity index (PDI) of 5 to 20, a strength of 1.5 to 10 g / d as measured by ASTM D2256, and an elongation at maximum strength of 10 to 50% has excellent thermal conductivity, high flexibility, and can be excellently woven, and can be manufactured into a fabric having excellent cooling properties and low pilling frequency.

[0036] Specifically, the polydispersity index may be 7 to 20, or 11 to 16, more specifically 12 to 15. Here, the strength measured by ASTM D2256 may be 5 to 10 g / d, or 6 to 9 g / d, more specifically 7 to 8 g / d, and the elongation at maximum strength may be 10 to 30%, or 15 to 25%, more specifically 17 to 23%, but is not limited thereto. However, within the above range, the fiber can have high thermal conductivity and at the same time an appropriate high twist degree that is advantageous for weaving.

[0037] In particular, when the polyethylene raw yarn satisfies the following formula 1 in a weight distribution graph obtained by gel permeation chromatography (GPC) analysis in which the log scale of molecular weight (Mw) is on the x-axis and the weight distribution (dw / dlogM) is on the y-axis, the polyethylene raw yarn can be manufactured into a fabric having excellent thermal conductivity and a very low incidence of fluffing. Here, the weight distribution graph is unimodal.

[0038] [Formula 1] (M max -Mw aver )<(Mw aver -Mw min )

[0039] (In the above formula, Mw aver is the molecular weight having the maximum weight distribution in the weight distribution graph, and Mw max and Mw min , Mw aver For the weight distribution value Q in the weight distribution graph, the two molecular weights corresponding to 0.25Q are referred to as Mw maw The maximum of the two molecular weights is Mw min means the minimum value.)

[0040] The polyethylene raw yarn satisfying the above formula 1 has a relatively low molecular weight and a wide weight distribution. Such polyethylene raw yarn has excellent thermal conductivity due to phonons, and can have high flexibility and strength, so that it has better weaving properties and can be manufactured into a cool-feeling fabric with an extremely low incidence of fuzzing.

[0041] In addition, by satisfying the above formula 1, (Mw max -Mw aver )-(Mw aver -Mw min The value of (a) may be a negative number. As an example, but not limited to, it may be greater than 0 and less than -3, specifically greater than 0 and less than -1, and more specifically greater than 0 and less than -0.5.

[0042] Gel permeation chromatography analysis was performed using the following analytical equipment after completely dissolving the polyethylene yarn in the following solvent.

[0043] -Analytical equipment: Tosoh HLC-8321 GPC / HT -Column: PLgel guard (7.5 x 50 mm) + 2 x PLgel mixed-B (7.5 x 300 mm) -Column temperature: 160°C -Solvent: Trichlorobenzene (TCB) + 0.04 wt.% dibutylhydroxytoluene (BHT) (after drying with 0.1% CaCl2) -Injector and detector temperature: 160℃ -Detector: RI Detector -Flow rate: 1.0ml / min -Injection volume: 300mL -Sample concentration: 1.5mg / mL -Standard sample: polystyrene

[0044] In addition, the polyethylene yarn has a lower initial modulus than that of ordinary polyethylene yarn for cooling, i.e., the initial modulus measured by ASTM D2256 may be 50 to 100 g / d, specifically 30 to 80 g / d. If the initial modulus of the polyethylene yarn is higher than the above range, the elasticity is good but the stiffness may be poor, and if the initial modulus of the polyethylene yarn is lower than the above range, the stiffness is good but the elastic recovery force is low and the toughness of the fabric may be poor. That is, by having appropriate stiffness and toughness within the above range, it is possible to have better weaving properties and therefore to manufacture a fabric with excellent drapeability.

[0045] In one embodiment, the polyethylene raw yarn may have a weight average molecular weight of 20,000 to 200,000 g / mol, preferably 30,000 to 150,000 g / mol. Within this range, the flowability of the molten material during melt extrusion of the raw yarn is good, thermal decomposition is prevented, and processability such as no yarn breakage during drawing is ensured, so that raw yarn with uniform physical properties can be produced, and a fabric with excellent durability can be provided.

[0046] In addition, the density of polyethylene yarn is 0.93 to 0.97 g / cm 3The crystallinity of the polyethylene raw yarn may be 50-90%, specifically 60-85%. The crystallinity of the polyethylene raw yarn may be determined together with the size of the crystallites when analyzing the crystallinity using an X-ray diffraction analyzer. As described above, when the crystallinity is within the above range, heat is rapidly diffused and dissipated in the direction of the molecular chains connected through covalent bonds of the high density polyethylene (HDPE) through lattice vibrations called 'phonons', and the function of discharging moisture such as sweat and breath is improved, providing a fabric with excellent wearability.

[0047] A method for producing a polyethylene raw yarn according to one embodiment of the present invention will be described in detail below with reference to Fig. 1. The polyethylene raw yarn of the present invention is not limited to this production method as long as it satisfies the above-mentioned ranges of physical properties such as PDI, strength, and elongation at maximum strength, and the following describes one embodiment.

[0048] First, polyethylene in the form of chips is fed into an extruder 100 and melted to obtain a polyethylene melt.

[0049] Molten polyethylene is transported through a die 200 by a screw (not shown) in the extruder 100, and is extruded through a number of holes formed in the die 200. The number of holes in the die 200 can be determined according to the DPF (Denier Per Filament) and fineness of the raw yarn to be produced. For example, when a raw yarn having a total fineness of 75 denier is produced, the die 200 can have 20 to 75 holes, and when a raw yarn having a total fineness of 450 denier is produced, the die 200 can have 90 to 450 holes, preferably 100 to 400 holes.

[0050] The melting process in the extruder 100 and the extrusion process through the die 200 can be changed and applied depending on the melt index of the polyethylene chips, but specifically, for example, they are preferably performed at 150 to 315°C, preferably 250 to 315°C, and more preferably 265 to 310°C. That is, it is preferable that the extruder 100 and the die 200 are maintained at 150 to 315°C, preferably 250 to 315°C, and more preferably 265 to 310°C.

[0051] If the spinning temperature is less than 150° C., the polyethylene may not be uniformly melted due to the low spinning temperature, making spinning difficult, whereas if the spinning temperature exceeds 315° C., the polyethylene may be thermally decomposed, making it difficult to achieve the desired strength.

[0052] The ratio L / D, which is the ratio of the hole length L to the hole diameter D of the spinneret 200, may be 3 to 40. If L / D is less than 3, a die swell phenomenon may occur during melt extrusion, making it difficult to control the elastic behavior of the polyethylene, resulting in poor spinnability, and if L / D exceeds 40, thread breakage may occur due to necking of the molten polyethylene passing through the spinneret 200, as well as non-uniform extrusion due to pressure drop.

[0053] As the molten polyethylene is discharged from the holes of the spinneret 200, the polyethylene begins to solidify due to the difference between the spinning temperature and room temperature, forming semi-solidified filaments 11. In this specification, not only semi-solidified filaments but also completely solidified filaments are collectively referred to as "filaments".

[0054] The filaments 11 are completely solidified by being cooled in a cooling section (or "quenching zone") 300. The filaments 11 can be cooled by air cooling.

[0055] It is preferable that the filaments 11 are cooled in the cooling unit 300 to 15 to 40° C. using cooling air at a speed of 0.2 to 1 m / sec. If the cooling temperature is less than 15° C., the filaments 11 may be overcooled, resulting in insufficient elongation and yarn breakage during drawing, whereas if the cooling temperature exceeds 40° C., the filaments 11 may be solidified non-uniformly, resulting in large deviation in fineness and yarn breakage during drawing.

[0056] In addition, by performing multi-stage cooling during cooling in the cooling section, crystallization can be performed more uniformly, which allows for smoother discharge of moisture and sweat and allows for the production of raw yarn with excellent coolness. More specifically, the cooling section can be divided into three or more sections. For example, when it is composed of three cooling sections, it is preferable that the temperature is designed to be gradually lower from the first cooling section to the second cooling section. Specifically, for example, the first cooling section can be set to 50 to 80°C, the second cooling section can be set to 30 to 50°C, and the third cooling section can be set to 15 to 30°C.

[0057] Also, by setting the wind speed at the first cooling section to the highest, it is possible to produce fibers with a smoother surface. Specifically, the first cooling section may use cooling wind with a wind speed of 1.0-1.5 m / sec to cool to 50-80°C, the second cooling section may use cooling wind with a wind speed of 0.6-1.0 m / sec to cool to 30-50°C, and the third cooling section may use cooling wind with a wind speed of 0.3-0.6 m / sec to cool to 15-30°C. By adjusting the conditions in this way, it is possible to produce raw yarn with a higher crystallinity and a smoother surface.

[0058] The cooled and fully solidified filaments 11 are then bundled by a bundler 400 to form a multifilament 10.

[0059] As illustrated in Fig. 1, the polyethylene raw yarn of the present invention can be produced through a direct spin-draw (DSD) process. That is, the multifilament 10 is directly transferred to a multi-stage drawing section 500 including a plurality of godet roller sections GR1...GRn, and is multi-stage drawn at a total draw ratio of 2 to 20 times, preferably 3 to 15 times, and then wound up by a winder 600. In addition, in the multi-stage drawing, a shrinkage draw (relaxation) of 1 to 5% is imparted in the final drawing section, thereby providing a raw yarn with better durability.

[0060] Alternatively, the polyethylene raw yarn of the present invention can be produced by once winding the multifilament 10 as an undrawn yarn and then drawing the undrawn yarn. That is, the polyethylene raw yarn of the present invention can be produced through a two-stage process in which polyethylene is melt-spun to once produce an undrawn yarn, and then the undrawn yarn is drawn.

[0061] If the total draw ratio applied in the drawing process is less than 2, the final polyethylene raw yarn cannot have a crystallinity of 60% or more, and there is a risk of fuzz (filling) being induced on the fabric produced from the raw yarn.

[0062] On the other hand, if the total draw ratio exceeds 15 times, yarn breakage may occur, the strength of the finally obtained polyethylene raw yarn may not be adequate, and the weavability of the polyethylene raw yarn may be poor, and the fabric manufactured using the same may be too stiff, causing inconvenience to users.

[0063] Once the linear speed of the first godet roller section GR1, which determines the spinning speed of the melt spinning of the present invention, is determined, the linear speeds of the remaining godet roller sections are appropriately determined so that a total draw ratio of 2 to 20, preferably 3 to 15, is applied to the multifilament 10 in the multi-stage drawing section 500.

[0064] According to an embodiment of the present invention, the heat-setting of the polyethylene raw yarn is performed through the multistage drawing section 500 by appropriately setting the temperature of the godet roller units GR1...GRn of the multistage drawing section 500 in the range of 40 to 140°C. Specifically, for example, the multistage drawing section may be composed of three or more, specifically, three to five, drawing sections. Also, each drawing section may be composed of a plurality of godet roller units.

[0065] Specifically, for example, the multi-stage drawing section may be composed of four drawing sections, in which the fiber is drawn to a total draw ratio of 2 to 15 times in the first to fourth drawing sections, and then contracted and drawn (relaxed) by 1 to 3% in the fifth drawing section. The total draw ratio refers to the final draw ratio of the fiber after the first to third drawing sections, compared to the fiber before drawing.

[0066] More specifically, the first stretching section may be performed at 40 to 80°C, and the stretch ratio of the first stretching section may be 1.5 to 3 times. The second stretching section may be performed at a higher temperature than the first stretching section, specifically 80 to 130°C, and stretching may be performed so that the stretch ratio of the second stretching section is 1.05 to 3 times. The third stretching section may be performed at 100 to 150°C, and stretching may be performed so that the stretch ratio is 1.05 to 3 times. The fourth stretching section may be performed at the same or lower temperature as the second stretching section, specifically 80 to 140°C, and may be performed with 1 to 3% shrinkage / stretching (relaxation).

[0067] The multistage drawing section 500 simultaneously performs multistage drawing and heat setting of the multifilament 10, and the multistage drawn multifilament 10 is wound by a winder 600 to complete the polyethylene raw yarn of the present invention.

[0068] The functional fabric according to the present invention contains the polyethylene yarn described above, which has excellent thermal conductivity and high weavability, and thus has a cooling sensation characteristic and excellent quality with few defects such as fluff. In addition, the functional fabric contains the polyethylene yarn described above, and thus has not only a cooling sensation but also excellent drapeability, so that when a user wears a product made from such a fabric, the contact area between the user and the product is large, and a substantially better cooling sensation effect can be achieved.

[0069] The functional fabric according to the present invention may be one that uses the polyethylene yarn described above alone, or may further include a different type of yarn in order to impart other functionality. However, from the viewpoint of simultaneously having a cool sensation and weaving properties, it is preferable to use the polyethylene yarn alone.

[0070] Specifically, the functional fabric has a cooling sensation of 0.15 to 0.45 W / cm2 when measured by contacting a 30±2°C hot plate (T-box) with a 20±2°C fabric at 20±2°C and 65±2% RH. 2 When a heat source plate (BT-box) of 30±2°C is in contact with a fabric of 20±2°C, the thermal conductivity in the thickness direction at 20°C can be 0.01~0.30W / mK. More specifically, the cool feeling to the touch can be 0.18~0.30W / cm 2 The thermal conductivity in the thickness direction may be 0.05~0.2W / mK. When the functional fabric having such a cooling sensation is later manufactured or processed into a product and worn by a user, it can provide an appropriate cooling sensation that allows the user to feel comfortable in a high temperature environment.

[0071] In addition, functional fabrics are available in 100,000m 2 The number of fluffs generated per unit may be 10 or less, specifically, 8 or less. That is, the functional fabric can be manufactured with high quality by including the polyethylene raw yarn with improved weaving properties.

[0072] Functional fabrics are 150-800g / m 2 The fabric may be a woven or knitted fabric having a weight per unit area (i.e., areal density) of 150 g / m 2 If the surface density of the fabric is less than 800 g / m, the fabric will not be dense enough and many voids will exist in the fabric, which will reduce the cooling sensation of the fabric. 2 If it exceeds this value, the fabric will be too dense in structure, causing problems with the feel felt by the user, and the high weight will cause problems in use.

[0073] Such fabrics can be processed into cooling products that require appropriate cooling sensation. The products can be any conventional textile products, but preferably can be summer clothes, sportswear, masks, and work clothes for imparting cooling sensation to the human body.

[0074] The cooling sensation product of the present invention is manufactured from the above-mentioned fabric, and has a low twist of 5 gf or less, more preferably 2 to 5 gf, and thus has excellent drapeability and excellent wearing comfort. Furthermore, by exhibiting excellent drapeability, the contact area with the user's body is large when worn by the user, and the cooling sensation effect can be substantially improved.

[0075] Hereinafter, the present invention will be described in more detail with reference to the following examples. However, the following examples are merely a reference for explaining the present invention in detail, and the present invention is not limited thereto, and may be realized in various forms.

[0076] In addition, unless otherwise defined, all technical and scientific terms have the same meaning as commonly understood by one of ordinary skill in the art to which the present invention belongs. The terms used in the description of this application are merely for the purpose of effectively describing a particular embodiment and are not intended to limit the present invention. In addition, the unit of additives not specifically described in the specification may be weight percent. EXAMPLES

[0077] The physical properties were measured as follows.

[0078] [Measurement of yarn physical properties] <1. Weight distribution graph, weight average molecular weight (Mw) (g / mol), and polydispersity index (PDI)> The polyethylene raw yarn was completely dissolved in the following solvent, and then the weight distribution graph, weight average molecular weight (Mw) and polydispersity index (Mw / Mn: PDI) of the polyethylene raw yarn were obtained using the following gel permeation chromatography (GPC).

[0079] -Analytical equipment: Tosoh HLC-8321 GPC / HT -Column: PLgel guard (7.5 x 50 mm) + 2 x PLgel mixed-B (7.5 x 300 mm) -Column temperature: 160°C -Solvent: Trichlorobenzene (TCB) + 0.04 wt.% dibutylhydroxytoluene (BHT) (after drying with 0.1% CaCl2) -Injector and detector temperature: 160℃ -Detector: RI Detector -Flow rate: 1.0ml / min -Injection volume: 300mL -Sample concentration: 1.5mg / mL -Standard sample: polystyrene

[0080] <2. Strength (g / d), initial modulus (g / d), and elongation (%)> The deformation-stress curves of polyethylene raw yarns were obtained using a universal tensile tester (Instron Engineering Corp, Canton, Mass.) according to the method of ASTM D2256. The sample length was 250 mm, the tensile speed was 300 mm / min, and the initial load was set to 0.05 g / d. The strength (g / d) and the elongation rate (%) at the maximum strength were calculated from the stress and elongation at the break point, and the initial modulus (g / d) was calculated from the tangent line that gave the maximum slope near the origin of the curve. Five measurements were taken for each raw yarn, and the average value was calculated.

[0081] <3. Crystallinity> The crystallinity of the polyethylene yarn was measured using an XRD (X-ray Diffractometer) manufactured by PANalytical, model name: EMPYREAN. Specifically, the polyethylene yarn was cut to prepare a sample having a length of 2.5 cm, and the sample was fixed to a sample holder, and then the measurement was performed under the following conditions.

[0082] -Light source (X-ray Source): Cu-K α radiation -Power: 45KV x 25mA - Mode: Continuous scan mode -Scan angle range: 10~40° -Scan speed: 0.1° / sec

[0083] [Fabric property measurement] <1. Cool sensation to the touch> The measurements were conducted at the Korea Clothing Testing and Research Institute using a KES-F7 (Thermo Labo II) device at a test environment of 20±2°C and 65±2% RH.

[0084] Specifically, a fabric sample with a size of 20cm x 20cm was prepared and left for 24 hours under conditions of 20±2°C temperature and 65±2% RH. Then, in a test environment of 20±2°C temperature and 65±2% RH, the contact coolness (Qmax) of the fabric was measured using a KES-F7 THERMO LABO II (Kato Tech Co., LTD.) device. Specifically, as illustrated in FIG. 2, the fabric sample 23 was placed on a base plate (also called a 'Water-Box') 21 maintained at 20°C, and a hot plate (T-Box) 22a (contact area: 3cm x 3cm) heated to 30°C was placed on the fabric sample 23 for only 1 second. That is, the other side of the fabric sample 23, one side of which is in contact with the base plate 21, was instantaneously brought into contact with the T-Box 22a. The contact pressure applied to the fabric sample 23 by the T-Box 22a was 6gf / cm. 2 Then, the Qmax value displayed on a monitor (not shown) connected to the device was recorded. This test was repeated 10 times, and the arithmetic mean of the Qmax values ​​was calculated.

[0085] <2. Thermal conductivity> After preparing a dough sample of 20 cm x 20 cm size, it was left for 24 hours under the conditions of 20 ± 2 ° C temperature and 65 ± 2% RH. Then, in the test environment of 20 ± 2 ° C temperature and 65 ± 2% RH, the thermal conductivity and heat transfer coefficient of the dough were measured using a KES-F7 THERMO LABO II (Kato Tech Co., LTD.) device. Specifically, as illustrated in FIG. 3, the dough sample 23 was placed on a base plate 21 maintained at 20 ° C, and a heat source plate (BT-Box) 22b (contact area: 5 cm x 5 cm) of 30 ± 2 ° C was placed on the dough sample 23 for 1 minute. While the BT-Box 22b was in contact with the dough sample 23, heat was continuously supplied to the BT-Box 22b so that the temperature was maintained at 30 ° C. The amount of heat supplied to maintain the temperature of the BT-Box 22b (i.e., heat flow loss) was displayed on a monitor (not shown) connected to the device. This test was repeated five times, and the arithmetic average of the heat flow loss was calculated. Then, the thermal conductivity and heat transfer coefficient of the fabric were calculated using the following Equations 2 and 3.

[0086] Equation 2: K = (W D) / (A ΔT) Equation 3: k=K / D

[0087] Here, K is the thermal conductivity (W / cm °C), D is the thickness (cm) of the fabric sample 23, and A is the contact area of ​​the BT-Box 22b (= 25 cm 2 ), ΔT is the temperature difference between the two sides of the fabric sample 23 (=10°C), W is the heat flow loss (Watt), and k is the heat transfer coefficient (W / cm 2 ·℃).

[0088] <3. Stiffness (gf)> After taking fabric samples (width: 60 mm, length: 60 mm), the bending resistance of the specimens was measured according to ASTM D885 / D885M-10a(2014) section 38. The measuring device was as follows.

[0089] (i) CRE-type Tensile Testing Machine (model: INSTRON3343) (ii) Loading Cell, 2 KN (200 kgf) (iii) Specimen Holder: A specimen holder as defined in section 38.4.3. (iv) Specimen Depressor: Specimen depressor as defined in section 38.4.4.

[0090] Specifically, the sample was placed in the center of the specimen holder so that the sample was directly supported by the specimen holder. The sample was kept flat without bending. At this time, the distance between the specimen supporting part of the specimen holder and the depressing part of the specimen depressor was 5 mm. Next, the specimen holder was raised to 15 mm while the specimen depressor was left as it was without moving, and the maximum strength was measured.

[0091] [Example 1] <Production of polyethylene yarn> Using the apparatus illustrated in FIG. 1, a polyethylene yarn containing 200 filaments and having a total denier of 150 was produced.

[0092] Specifically, polyethylene chips were put into an extruder 100 and melted. The molten polyethylene was extruded through a die 200 having 200 holes. The ratio of hole length L to hole diameter D of the die 200, L / D, was 6. The die temperature was 270°C.

[0093] The filaments 11 formed while being discharged from the nozzle holes of the spinneret 200 were sequentially cooled in the cooling section 300 consisting of three sections. In the first cooling section, the filaments were cooled to 70° C. by cooling air with a wind speed of 1.2 m / sec, in the second cooling section, the filaments were cooled to 40° C. by cooling air with a wind speed of 0.8 m / sec, and in the third cooling section, the filaments were finally cooled to 20° C. by cooling air with a wind speed of 0.4 m / sec. After being cooled, the filaments were bundled into a multifilament yarn 10 by a bundler 400.

[0094] Next, the multifilament yarn was transferred to the drawing section 500. The drawing section was a multi-stage drawing section consisting of four sections, and specifically, in the first drawing section, the yarn was drawn at a total draw ratio of 1.5 times at a maximum draw temperature of 70°C, in the second drawing section, the yarn was drawn at a total draw ratio of 2.0 times at a maximum draw temperature of 100°C, in the third drawing section, the yarn was drawn at a total draw ratio of 1.5 times at a maximum draw temperature of 120°C, and in the fourth drawing section, the yarn was drawn and heat-set at a maximum draw temperature of 125°C such that the yarn was shrunk and drawn (relaxed) by 2% compared to the third drawing section.

[0095] The drawn multifilament yarn was then wound on a winder 600. The winding tension was 0.8 g / d.

[0096] The physical properties of the produced yarn were measured and are shown in Table 1 below.

[0097] <Manufacturing of functional fabrics> The polyethylene yarn thus produced was woven to a surface density of 500 g / m 2 The physical properties of the functional fabric thus produced were measured and are shown in Table 3 below.

[0098] [Examples 2 to 7] A fabric was manufactured in the same manner as in Example 1, except that the raw yarn conditions were changed as shown in Table 1 below. In addition, the physical properties of the fabric manufactured in the same manner as in Example 1 were measured and are shown in Table 3 below.

[0099] [Comparative Examples 1 to 4] A fabric was manufactured in the same manner as in Example 1, except that the raw yarn conditions were changed as shown in Table 2 below. In addition, the physical properties of the fabric manufactured in the same manner as in Example 1 were measured and are shown in Table 4 below.

[0100] [Table 1]

[0101] [Table 2]

[0102] [Table 3]

[0103] [Table 4]

[0104] Referring to Tables 1 to 4, it can be seen that the fabrics according to the examples have an appropriate cool feeling, excellent stiffness and drapeability, and that the frequency of fuzz generation during the manufacture of the fabric is extremely low, making it excellent in weaving properties. In particular, referring to FIG. 4 showing the weight distribution graph through the GPC analysis of Example 3, in the examples that satisfy the above formula 1, that is, (Mw max -Mw aver )-(Mw aver -Mw min It was confirmed that the examples in which the value of .DELTA..times ...

[0105] As described above, the present invention has been described using specific and limited embodiments and drawings. However, this is merely provided to aid in a more general understanding of the present invention. The present invention is not limited to the above embodiments. Those skilled in the art will appreciate that various modifications and variations can be made from such descriptions.

[0106] Therefore, the concept of the present invention should not be limited to the described embodiments, and all things that are equivalent to the scope of the claims or have equivalent variations should be considered to fall within the scope of the concept of the present invention, not just the scope of the claims described below. [Explanation of symbols]

[0107] 100: Extruder 200: Base 300: Cooling section 400:Focusing part 500: Stretching part 600: Winder

Claims

1. A polyethylene raw yarn having a polydispersity index (PDI) of 5 to 20, a strength of 1.5 to 10 g / d as measured by ASTM D2256, and an elongation at maximum strength of 10 to 50%.

2. The polyethylene yarn is 2. The polyethylene raw yarn according to claim 1, wherein a weight distribution graph obtained by gel permeation chromatography (GPC) analysis, in which the log scale of molecular weight (Mw) is on the x-axis and the weight distribution rate (dw / dLogM) is on the y-axis, satisfies the following formula 1, and the weight distribution graph is unimodal. [Formula 1] (Mw max -Mw aver ) < (M aver -Mw min ) (In the above formula, Mw aver is the molecular weight having the maximum weight distribution in the weight distribution graph, and Mw max and Mw min , Mw aver For the weight distribution value Q at 0.25Q in the weight distribution graph, Mw maw The maximum of the two molecular weights is Mw min means the minimum value.)

3. The polyethylene raw yarn according to claim 1, wherein the raw yarn has an initial modulus of 30 to 80 d / g as measured by ASTM 2256.

4. The polyethylene yarn according to claim 1, wherein the yarn has a crystallinity of 65 to 85%.

5. The raw yarn has a density of 0.93 to 0.97 g / cm 3 The polyethylene raw yarn according to claim 1,

6. The polyethylene raw yarn according to claim 1, wherein the raw yarn has a weight average molecular weight of 90,000 to 400,000 g / mol.

7. A functional fabric comprising the polyethylene yarn according to any one of claims 1 to 6.

8. The fabric has a cool touch of 0.18 to 0.30 W / cm2 when measured at 20±2°C and 65±2% RH by contacting a 30±2°C hot plate (T-box) with the fabric at 20±2°C. 2 The functional fabric according to claim 7 .

9. The functional fabric according to claim 7, wherein the thermal conductivity in the thickness direction of the fabric is 0.05 to 0.20 W / mK when measured at 20±2°C and 65±2% RH by contacting a heat source plate (BT-box) at 30±2°C with the fabric at 20±2°C.

10. The fabric is 100,000 m 2 The functional fabric according to claim 7, wherein the number of fuzz particles generated per unit is 10 or less.

11. The fabric has a surface density of 150 to 800 g / m 2 The functional fabric according to claim 7 .

12. A cooling product produced from the fabric of claim 7.

Citation Information

Patent Citations

  • Comfortable cloth

    JP2010236130A

  • Polyethylene fibers and their manufacturing method

    JP2012510570A

  • Functional original reaction

    JP2023548825A

  • Semiconductor device, power diode, and rectifier

    KR1020200040724A

  • Apparatus for sensing

    KR1020210088974A