Process for recovering dialkyl terephthalates from polyester compositions - Patents.com

The method addresses the high resource and energy demands of conventional polyester recycling by using controlled depolymerization and alcoholysis to recover dialkyl terephthalates efficiently and effectively.

JP2024541916AInactive Publication Date: 2024-11-13EASTMAN CHEM CO
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
JP2024524622
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2021-10-25
Filing Date
2022-10-25
Publication Date
2024-11-13
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Conventional glycolysis and methanolysis processes for recycling polyester compositions require substantial amounts of resources and energy.

Method used

A method involving depolymerization of polyester compositions with glycols and methanol under controlled conditions, followed by alcoholysis, to recover dialkyl terephthalates, utilizing reduced temperatures and pressures to minimize energy and resource consumption.

Benefits of technology

The method achieves high yields and high purity of dialkyl terephthalates with reduced energy and resource requirements, enabling efficient recycling of polyester materials.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024541916000008
    Figure 2024541916000008
  • Figure 2024541916000009
    Figure 2024541916000009
  • Figure 2024541916000010
    Figure 2024541916000010
Patent Text Reader

Abstract

A method for recovering dialkyl terephthalate. The method may include exposing a polyester composition to a first composition comprising one or more glycols and methanol under depolymerization conditions, thereby providing one or more depolymerization products. The one or more depolymerization products may be exposed to an alcoholysis process to recover the dialkyl terephthalate. Optionally, the one or more glycols and / or methanol may be recovered at the end of the alcoholysis process and reused in a subsequent process for recovering the dialkyl terephthalate.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present disclosure relates to methods for recycling polyester compositions. More particularly, the present disclosure relates to recovering dialkyl terephthalates from polyester compositions. [Background technology]

[0002] Certain conventional systems may utilize glycolysis and / or methanolysis processes in an attempt to recycle polyesters, however, certain conventional glycolysis and / or methanolysis processes may require substantial amounts of resources and energy to arrive at a product suitable for use in a subsequent production process, such as a production process to make recycled polyester or other compositions. Summary of the Invention

[0003] In one aspect, a method for recovering one or more dialkyl terephthalates from a polyester composition is provided. The method includes exposing a first polyester composition to a first composition comprising one or more glycols and methanol under depolymerization conditions in a first reaction vessel to provide a first mixture, the first mixture comprising one or more first depolymerization products. The depolymerization conditions include a temperature of 150°C to 260°C and a pressure of 10 atm to 70 atm. The method also includes cooling at least a portion of the first mixture to a temperature of 150°C or less; and exposing at least a portion of the first mixture to an alcohol composition and an alcoholysis catalyst under conditions including a temperature of 23°C to 90°C and a pressure of 1 atm to 2 atm for 0.5 hours to 5 hours to provide a second mixture. The second mixture comprises one or more dialkyl terephthalates. The method may also include separating at least a portion of the one or more dialkyl terephthalates by solid-liquid separation to provide a dialkyl terephthalate solid component and a filtrate. [Brief description of the drawings]

[0004] [Figure 1] 1 is an exemplary system for recovering one or more dialkyl terephthalates from a polyester composition according to an embodiment of the present disclosure. [Diagram 2] 1 is a graph of the ratio of methyl esters to ethylene glycol plotted against the ratio of methanol and ethylene glycol in the feed based on the data provided in the examples. [Diagram 3] 1 is a gas chromatography graph of the dimethyl terephthalate (DMT) product of Example 1. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0005] overview The present disclosure may be more readily understood by reference to the following detailed description of certain aspects and examples of the disclosure. In accordance with the purposes of this disclosure, certain aspects of the disclosure are described in the Summary of the Invention and further described herein below. Other aspects of the disclosure are also described herein.

[0006] Aspects herein relate to methods for recovering one or more dialkyl terephthalates from a polyester composition. As described herein, an exemplary method may include exposing a polyester composition to one or more glycols and methanol under depolymerization conditions to produce one or more depolymerization products, which are then exposed to an alcoholysis process to recover the dialkyl terephthalates.

[0007] As discussed above, certain conventional glycolysis and / or methanolysis processes may require substantial amounts of resources and energy to arrive at a product suitable for use in a downstream production process, such as a production process for making recycled polyester or other compositions.

[0008] The methods and systems disclosed herein can alleviate one or more of the above problems. For example, in certain embodiments, the methods disclosed herein can include exposing a polyester composition to depolymerization conditions with one or more glycols and methanol to provide one or more depolymerization products. In various embodiments, the one or more depolymerization products can include monomers, oligomers, or combinations thereof. In embodiments, the one or more depolymerization products can be exposed to alcoholysis conditions to obtain high yields and high purity dialkyl terephthalate products. As discussed herein, the alcoholysis conditions include reduced temperatures compared to certain conventional systems, which reduces the overall energy and resources required.

[0009] Polyester Composition As discussed above, the methods described herein relate to recovering one or more dialkyl terephthalates from a polyester composition. The term "polyester" may refer to a synthetic polymer prepared by the reaction of one or more difunctional carboxylic acids and / or polyfunctional carboxylic acids with one or more difunctional hydroxyl compounds and / or polyfunctional hydroxyl compounds. The difunctional carboxylic acids may be dicarboxylic acids and the difunctional hydroxyl compounds may be dihydric alcohols such as glycols. Additionally, as used herein, the term "diacid" or "dicarboxylic acid" includes polyfunctional acids such as branching agents. As used herein, the term "glycol" or "diol" includes, but is not limited to, diols, glycols, and / or polyfunctional hydroxyl compounds. The dicarboxylic acid residues may be derived from dicarboxylic acid monomers or their associated acid halides, esters, salts, anhydrides, or mixtures thereof. Thus, as used herein, the term dicarboxylic acid is intended to include dicarboxylic acids and any derivatives thereof, including their associated acid halides, esters, half esters, salts, half salts, anhydrides, mixed anhydrides, or mixtures thereof, that are useful in the reaction process with diols to make polyesters. As used herein, the term "polyester" should be understood to also refer to copolyesters.

[0010] As used herein, the term "residue" refers to a monomeric or repeating unit in a polymer, oligomer, or dimer. For example, a polymer may be made from the condensation of the following monomers: terephthalic acid ("TPA") and cyclohexyl-1,4-dimethanol ("CHDM"). The condensation reaction results in the loss of a water molecule. The residue in the resulting polymer comes from either terephthalic acid or cyclohexyl-1,4-dimethanol. Formula (I) below illustrates a non-limiting example of a polyester.

[0011] [ka]

[0012] In an embodiment, the polyester composition exhibits an intrinsic viscosity of from about 0.1 dL / g to about 1.2 dL / g, as determined in accordance with ASTM D2857-70, from about 0.2 dL / g to about 1.2 dL / g, as determined in accordance with ASTM D2857-70, from about 0.3 dL / g to about 1.2 dL / g, as determined in accordance with ASTM D2857-70, or from about 0.4 dL / g to about 1.2 dL / g, as determined in accordance with ASTM D2857-70.

[0013] In embodiments, the polyester composition may include one or more polyesters. In various embodiments, the one or more polyesters may include terephthalate polyesters. Terephthalate polyesters are polyesters that include residues of terephthalic acid or any derivative of terephthalic acid, including its associated acid halides, esters, half esters, salts, half salts, anhydrides, mixed anhydrides, and / or mixtures thereof or residues thereof, that are useful in the reaction process with diols to make copolyesters. In various embodiments, the polyester composition may include polyethylene terephthalate (PET). In one or more embodiments, the polyester composition may include glycol modified PET. In certain embodiments, the polyester composition may comprise polyethylene terephthalate (PET), 1,4-cyclohexanedimethanol (CHDM) modified PET, isophthalic acid (IPA) modified PET, diethylene glycol (DEG) modified PET, glycol modified PET, neopentyl glycol (NPG) modified PET, propanediol (PDO) modified PET, butanediol (BDO) modified PET, heaxanediol (HDO) modified PET, 2-methyl-2,4-pentanediol (MP diol) modified PET, isosorbide modified PET, polycyclohexylene dimethylene terephthalate (PCT), cyclohexanedimethanol (CHDM) containing copolyesters, isosorbide containing copolyesters, or combinations thereof.

[0014] In various embodiments, the polyester composition may include CHDM. In one embodiment, the polyester composition may include about 0 mol% to about 100 mol% CHDM, about 1 mol% to about 100 mol% CHDM, about 1 mol% to about 90 mol% CHDM, about 1 mol% to about 80 mol% CHDM, about 1 mol% to about 70% CHDM, about 1 mol% to about 60 mol% CHDM, about 1 mol% to about 50 mol% CHDM, about 1 mol% to about 40 mol% CHDM, about 1 mol% to about 35 mol% CHDM, about 1 mol% to about 30 mol% CHDM, about 1 mol% to about 25 mol% CHDM, about 1 mol% to about 20 mol% CHDM, about 1 mol% to about 10 mol% CHDM, or about 1 mol% to about 5 mol% CHDM. In an embodiment, the mol% of CHDM refers to the mol% of CHDM relative to all diol equivalents in the polyester composition. In various embodiments, the polyester composition may include DEG. In embodiments, the polyester composition may include about 0 mol% to about 100 mol% DEG, about 1 mol% to about 100 mol% DEG, about 1 mol% to about 90 mol% DEG, about 1 mol% to about 80 mol% DEG, about 1 mol% to about 70 mol% DEG, about 1 mol% to about 60 mol% DEG, about 1 mol% to about 50 mol% DEG, about 1 mol% to about 40 mol% DEG, about 1 mol% to about 35 mol% DEG, about 1 mol% to about 30 mol% DEG, about 1 mol% to about 20 mol% DEG, about 1 mol% to about 10 mol% DEG, about 1 mol% to about 5 mol% DEG, or about 1 mol% to about 3 mol% DEG. In embodiments, the mol% of DEG refers to the mol% of DEG relative to all diol equivalents in the polyester composition. In an embodiment, the polyester composition may include isophthalic acid.In an embodiment, the polyester composition may comprise from about 0 mol% to about 30 mol% isophthalic acid, from about 1 mol% to about 30 mol% isophthalic acid, from about 1 mol% to about 25 mol% isophthalic acid, from about 1 mol% to about 20 mol% isophthalic acid, from about 1 mol% to about 15 mol% isophthalic acid, from about 1 mol% to about 10 mol% isophthalic acid, from about 1 mol% to about 7.5 mol% isophthalic acid, from about 1 mol% to about 5 mol% isophthalic acid, from about 1 mol% to about 3 mol% isophthalic acid, up to about 10 mol% isophthalic acid, up to about 7.5 mol% isophthalic acid, up to about 5 mol% isophthalic acid, or up to about 3 mol% isophthalic acid. In an embodiment, the mol% of isophthalic acid refers to the mol% of isophthalic acid relative to the total diacid equivalents in the polyester composition. In certain embodiments, the polyester composition may comprise about 0 mol% to about 100 mol% CHDM, about 0 mol% to about 100 mol% DEG, about 0 mol% to about 30 mol% isophthalic acid, or a combination thereof. In certain embodiments, the polyester composition may comprise about 1 mol% to about 100 mol% CHDM, about 1 mol% to about 100 mol% DEG, about 1 mol% to about 30 mol% isophthalic acid, or a combination thereof. In various embodiments, the polyester composition may comprise other glycols, such as those listed above. For example, in embodiments, the polyester composition may comprise, but is not limited to, neopentyl glycol (NPG), 2-methyl-2,4-pentanediol (MP diol), butanediol (BDO), propanediol (PDO), hexanediol (HDO), isosorbide, poly(tetramethylene ether) glycol (PTMG), poly(ethylene) glycol (PEG), or a combination thereof.In certain embodiments, each of NPG, MP diol, BDO, PDO, HDO, isosorbide, PTMG and PEG may be present in the polyester composition in an amount of 0 mol % to about 100 mol %, about 1 mol % to about 100 mol %, about 1 mol % to about 90 mol %, about 1 mol % to about 80 mol %, about 1 mol % to about 70 mol %, about 1 mol % to about 60 mol %, about 1 mol % to about 50 mol %, about 1 mol % to about 40 mol %, about 1 mol % to about 35 mol %, about 1 mol % to about 30 mol %, about 1 mol % to about 25 mol %, about 1 mol % to about 20 mol %, about 1 mol % to about 10 mol %, or about 1 mol % to about 5 mol %. In embodiments, the mole % of each of NPG, MP diol, BDO, PDO, HDO, isosorbide, PTMG, and PEG refers to the mole % of each of NPG, MP diol, BDO, PDO, HDO, isosorbide, PTMG, and PEG, respectively, relative to the total diol equivalents in the polyester composition. In various embodiments, the polyester composition may include CHDM, DEG, NPG, MP diol, BDO, PDO, HDO, isosorbide, PTMG, PEG, isophthalic acid, or combinations thereof, each component being present in any of the amounts for such components described in this paragraph.

[0015] In embodiments, the polyester composition or one or more polyesters present in the polyester composition may be recycled polyester. In various embodiments, recycled polyester may include materials recovered as manufacturing scrap, post-industrial waste, post-consumer waste, or combinations thereof. In embodiments, recycled polyester may be used and / or discarded post-consumer products. In embodiments, the polyester composition and / or recycled polyester may be obtained from various sources and / or in various forms, including, but not limited to, textiles, carpets, thermoforming materials, bottles, pellets, and films. In one or more embodiments, the polyester composition may include recycled polyester, e.g., polyester formed from DMT recovered from a prior DMT recovery process, such as the processes described herein.

[0016] In various embodiments, the polyester composition may include one or more foreign materials. In embodiments, the one or more foreign materials may include, but are not limited to, polyesters other than polyethylene terephthalate, polyvinyl chloride (PVC), polyvinyl acetal, polyvinyl butyral (PVB), polyvinyl alcohol (PVOH), ethylene vinyl alcohol (EVOH), cotton, polyolefins, polyethylene, polypropylene, polystyrene, polycarbonate, spandex, natural fibers, cellulose esters, polyacrylates, polymethacrylates, polyamides, nylons, poly(lactic acid), polydimethylsiloxanes, polysilanes, calcium carbonate, titanium dioxide, inorganic fillers, dyes, pigments, color toners, colorants, plasticizers, adhesives, flame retardants, metals, aluminum and iron, or combinations thereof. In various embodiments, the one or more foreign matter may be present in the polyester composition in an amount of from about 0.01 wt.% to about 50 wt.%, from about 0.01 wt.% to about 40 wt.%, from about 0.01 wt.% to about 30 wt.%, from about 0.01 wt.% to about 20 wt.%, from about 0.01 wt.% to about 15 wt.%, from about 0.01 wt.% to about 10 wt.%, from about 0.01 wt.% to about 7.5 wt.%, from about 0.01 wt.% to about 5 wt.%, from about 0.01 wt.% to about 2.5 wt.%, or from about 0.01 wt.% to about 1.0 wt.%, based on the weight of the one or more polyesters in the polyester composition.

[0017] In embodiments, the polyester composition may be in a solid form, liquid form, melt form, or solution. In certain embodiments, the solution may include the polyester composition pre-dissolved in a solvent, such as DMT, EG, DEG, TEG, or combinations thereof.

[0018] Optional Pretreatment of the Polyester Composition In certain embodiments, optional treatment of the polyester composition may be performed prior to glycolysis and / or methanolysis. In various embodiments, the optional pretreatment may include any type of treatment that aids in removing a portion of any contaminants from the polyester composition and / or aids in recovering one or more polyesters from a mixed feedstock, such as a feedstock containing the contaminants discussed above. For example, in one embodiment, the optional pretreatment may include exposing the polyester composition to one or more solvents to selectively dissolve the polyesters in the polyester composition (or at least a portion of the contaminants in the polyester composition) to allow separation between at least a portion of the contaminants and one or more polyesters in the polyester composition. In one example embodiment, the optional pretreatment may include exposing the polyester composition to one or more solvents, such as one or more solvents that can cause dissolution of the polyesters in the polyester composition. For example, the one or more solvents may include, but are not limited to, 4-methylcyclohexanemethanol (MCHM), ethylene glycol (EG), diethylene glycol (DEG), triethylene glycol (TEG), 1,4-cyclohexanedimethanol (CHDM), poly(ethylene glycol) (PEG), neopentyl glycol (NPG), propanediol (PDO), butanediol (BDO), 2-methyl-2,4-pentanediol (MP diol), poly(tetramethylene ether) glycol (PTMG), dibutyl terephthalate (DBT), dioctyl terephthalate (DOTP), ethylene carbonate (EC), dimethyl carbonate (DMC), dimethyl sulfoxide (DMSO), dimethylformamide (DMF), or combinations thereof. In the same or alternative embodiment, the polyester composition may be exposed to one or more solvents at a particular temperature to effect dissolution of one or more components. In various embodiments, the pretreatment process may include one or more dissolution and separation steps using various solvents and / or temperatures to achieve a desired level of contaminant removal and / or purity level of PET.For example, in one embodiment, dissolution and separation can be utilized using one solvent at a particular temperature, e.g., to remove one or more contaminants, followed by subsequent dissolution and separation of the polyester fraction using another solvent at a particular temperature, e.g., to remove one or more other contaminants. The dissolution and / or separation in this optional pretreatment step can utilize any suitable system, reactor, vessel, and / or separation technique to achieve the desired pretreated polyester composition.

[0019] Glycolysis and / or depolymerization of polyester compositions As discussed above, in various aspects, the methods disclosed herein may include exposing a polyester composition to depolymerization conditions to depolymerize at least a portion of the one or more polyesters into one or more depolymerized products. In various aspects, the one or more depolymerized products may include monomers, oligomers, or combinations thereof. In certain aspects, the oligomers may exhibit a degree of polymerization of 2-10, 2-8, 2-6, or 2-4. In aspects, the one or more polyesters may be depolymerized into one or more depolymerized products that may include monomers and terephthalate oligomers having a degree of polymerization of 2-10, 2-8, 2-6, or 2-4. In aspects, liquid chromatography may be performed to identify the degree of polymerization of the oligomers, and / or gel permeation chromatography may be utilized to identify the molecular weight of the oligomers.

[0020] In an embodiment, the term degree of polymerization (DP) may refer to the number of residues in an oligomer. As used herein, degree of polymerization (DP) refers to the number of difunctional carboxylic acid residues and / or polyfunctional carboxylic acid residues in an oligomer. For example, in one exemplary embodiment, a DP of 1 refers to a residue that includes one terephthalic acid residue or one isophthalic acid residue. In such an exemplary embodiment, a DP of 1 may also be referred to as a monomer. A non-limiting example of a DP of 1 is shown in the following formula (II):

[0021] [ka]

[0022]

[0028] Formulas (III)-(V) below show non-limiting examples of oligomers having DPs of 2, 3, and n, respectively, in embodiments.

[0023] [ka]

[0024] In an embodiment, this depolymerization may be carried out by a glycolysis process. In general, in an embodiment, the glycolysis process disclosed herein may include exposing the polyester composition to one or more glycols and methanol, which react with the polyester, optionally in the presence of a transesterification catalyst, to form a mixture of bis(hydroxyethyl) terephthalate (BHET) or other terephthalate residues (e.g., bis(2-hydroxydiethylene terephthalate) (BHDET) when DEG is utilized) and low molecular weight terephthalate oligomers, depending on the glycol used. Some representative examples of glycolysis processes are disclosed in U.S. Patent Nos. 3,257,335; 3,907,868; 6,706,843; and 7,462,649, which are incorporated herein by reference.

[0025] In one embodiment of the glycolysis process, one or more polyesters, such as one or more recycled polyesters, and one or more glycols and methanol can be fed to a glycolysis reactor, where the one or more recycled polyesters are dissolved and depolymerized under depolymerization conditions.

[0026] In embodiments, any amount of one or more glycols suitable for use in a glycolysis process can be utilized. In various embodiments, the weight ratio of one or more glycols to the amount of polyester composition can be 9:1 to 1:9, 8:1 to 1:9, 7:1 to 1:9, 6:1 to 1:9, 5:1 to 1:9, 4:1 to 1:9, 3:1 to 1:9, 2:9 to 1:9, 9:1 to 1:8, 9:1 to 1:7, 9:1 to 1:6, 9:1 to 1:5, 9:1 to 1:4, 9:1 to 1:3, or 9:1 to 1:2. In the same or alternative embodiments, any amount of methanol suitable for use in a depolymerization or glycolysis process can be utilized. In certain embodiments, the weight ratio of the amount of one or more glycols to the amount of methanol may be 1:20 to 100:1, 1:10 to 100:1, 1:5 to 100:1, 1:1 to 100:1, 1:20 to 80:1, 1:20 to 60:1, 1:20 to 50:1, 1:20 to 40:1, 1:20 to 30:1, 1:20 to 20:1, or 1:20 to 10:1.

[0027] In certain embodiments, the one or more glycols may include any glycol suitable for use in the glycolysis process. As used herein, the term "glycol" refers to aliphatic, cycloaliphatic, and aralkyl glycols. Exemplary glycols include ethylene glycol, 1,2-propanediol (also known as propylene glycol), 1,3-propanediol, 1,4-butanediol, 1,5-pentanediol, 1,6-hexanediol, 2,2-dimethyl-1,3-propanediol, 1,2-cyclohexanedimethanol, 1,3-cyclohexanedimethanol, 1,4-cyclohexanedimethanol, 2,2,4,4-tetramethyl-1,3-cyclobutanediol, isosorbide, p-xylylenediol, and the like. These glycols may also include ether linkages, such as in the case of diethylene glycol, triethylene glycol, and tetraethylene glycol. Additional glycol embodiments include the higher molecular weight homologs known as polyethylene glycols, such as those produced by Dow Chemical Company under the trade name Carbowax™. In one embodiment, the polyethylene glycol (PEG) has a molecular weight of greater than 200 to about 10,000 Daltons (M n ) These glycols also include higher alkyl analogs such as dipropylene glycol, dibutylene glycol, etc. Similarly, additional glycols have molecular weights of about 200 to about 10,000 Daltons (M n) (also referred to as g / mole) range, and higher polyalkylene ether diols such as polypropylene glycol and polytetramethylene glycol. In one aspect, the glycol can be selected from aliphatic, cycloaliphatic and aralkyl glycols. In various aspects, the glycol can be selected from polyalkylene ether diols selected from ethylene glycol; 1,2-propanediol; 1,3-propanediol; 1,4-butanediol; 1,5-pentanediol; 1,6-hexanediol; 2,2-dimethyl-1,3-propanediol; 1,2-cyclohexanedimethanol; 1,3-cyclohexanedimethanol; 1,4-cyclohexanedimethanol; 2,2,4,4-tetramethyl-1,3-cyclobutanediol; isosorbide; p-xylylenediol; diethylene glycol; triethylene glycol; tetraethylene glycol; polyethylene glycol; dipropylene glycol; dibutylene glycol; polypropylene glycol and polytetramethylene glycol.

[0028] In certain embodiments, the one or more glycols may include diethylene glycol (DEG), triethylene glycol (TEG), 1,4-cyclohexanedimethanol (CHDM), poly(ethylene glycol) (PEG), neopentyl glycol (NPG), propanediol (PDO), butanediol (BDO), 2-methyl-2,4-pentanediol (MP diol), poly(tetramethylene ether) glycol (PTMG), or combinations thereof, and optionally, ii) ethylene glycol (EG). In such embodiments, the weight ratio of glycols in group i) to EG may be 100:0 to 1:99. In certain embodiments, the one or more glycols may include about 0 wt.% to about 100 wt.% DEG, or about 1 wt.% to about 100 wt.% DEG, based on the total weight of the one or more glycols. In certain embodiments, the one or more glycols may comprise about 0 wt.% to about 100 wt.% TEG, or about 1 wt.% to about 100 wt.% TEG, based on the total weight of the one or more glycols. In embodiments, the one or more glycols may comprise about 0 wt.% to about 50 wt.% CHDM, or about 1 wt.% to about 50 wt.% CHDM, based on the total weight of the one or more glycols. In various embodiments, the one or more glycols may comprise 0 wt.% to about 100 wt.% PEG, or about 1 wt.% to about 100 wt.% PEG, based on the total weight of the one or more glycols. In various embodiments, the one or more glycols may comprise 0 wt.% to about 100 wt.% NPG, or about 1 wt.% to about 100 wt.% NPG, based on the total weight of the one or more glycols. In various embodiments, the one or more glycols may comprise 0 wt.% to about 100 wt.% PDO, or about 1 wt.% to about 100 wt.% PDO, based on the total weight of the one or more glycols. In various embodiments, the one or more glycols may comprise 0 wt.% to about 100 wt.% BDO, or about 1 wt.% to about 100 wt.% BDO, based on the total weight of the one or more glycols. In various embodiments, the one or more glycols may comprise 0 wt.% to about 100 wt.% MP diol, or about 1 wt.% to about 100 wt.% MP diol, based on the total weight of the one or more glycols.In various embodiments, the one or more glycols may comprise 0 wt.% to about 100 wt.% PTMG, or about 1 wt.% to about 100 wt.% PTMG, based on the total weight of the one or more glycols. In certain embodiments, the one or more glycols may comprise about 0 wt.% to about 100 wt.% EG, or about 1 wt.% to about 100 wt.% EG, based on the total weight of the one or more glycols. In one embodiment, the one or more glycols may include 0 wt.% to about 100 wt.% EG, 0 wt.% to about 100 wt.% DEG, 0 wt.% to about 100 wt.% TEG, 0 wt.% to about 100 wt.% PEG, 0 wt.% to about 100 wt.% NPG, 0 wt.% to about 100 wt.% PDO, 0 wt.% to about 100 wt.% BDO, 0 wt.% to about 100 wt.% MP diol, 0 wt.% to about 100 wt.% PTMG, and 0 wt.% to about 50 wt.% CHDM, based on the total weight of the one or more glycols. In certain embodiments, as discussed in detail below, the one or more glycols may be recycled glycols recovered from a prior glycolysis and / or methanolysis process to recover one or more dialkyl terephthalates, as disclosed herein.

[0029] In various embodiments, as discussed above, the glycolysis process may include one or more catalysts, such as a transesterification catalyst. In certain embodiments, the catalyst may be present in an amount of 0.1 wt.% to 10 wt.% based on the weight of the polyester composition. In embodiments, any suitable catalyst may be utilized. In one embodiment, the catalyst is a carbonate catalyst, such as, but not limited to, Li 2 CO 3 , K 2 CO 3 , Na 2 CO 3 , Cs 2 CO 3 , ZrCO 3, or combinations thereof. In one embodiment, the catalyst may include a hydroxide catalyst, such as, but not limited to, LiOH, NaOH, KOH, tetrabutylammonium hydroxide (TBAH), or combinations thereof. In one embodiment, the catalyst may include an alkoxide catalyst, such as, but not limited to, sodium methoxide (NaOMe), lithium methoxide (LiOMe), magnesium methoxide, potassium t-butoxide, ethylene glycol monosodium salt, ethylene glycol disodium salt, or combinations thereof. In one embodiment, the catalyst may include tetraisopropyl titanate (TIPT), butyltin tris-2-ethylhexanoate (FASCAT 4102), 1,8-diazabicyclo[5.4.0]undec-7-ene (DBU), zinc acetylacetonate hydrate (Zn(acac) 2 ), zinc acetate (Zn(OAc) 2 ), and manganese(II) acetate (Mn(OAc) 2 )), or combinations thereof. In certain embodiments, the catalyst may include LiOH, NaOH, KOH, tetraisopropyl titanate (TIPT), butyltin tris-2-ethylhexanoate (FASCAT 4102), ZrCO 3 , 1,8-diazabicyclo[5.4.0]undec-7-ene (DBU), sodium methoxide (NaOMe), lithium methoxide (LiOMe), and zinc acetylacetonate hydrate (Zn(acac) 2 ), or combinations thereof. In one embodiment, the catalyst may include LiOH, NaOH, KOH, sodium methoxide (NaOMe), and lithium methoxide (LiOMe). In a particular embodiment, the catalyst may include Li 2 CO 3 , K 2 CO 3 , CaCO 3 , Na 2 CO 3 , Cs 2 CO 3, ZrCO3, LiOH, NaOH, KOH, Tetrabutylammonium hydroxide (TBAH), Sodium methoxide (NaOMe), Lithium methoxide (LiOMe), Magnesium methoxide (Mg(OMe) 2 , potassium t-butoxide, ethylene glycol monosodium salt, ethylene glycol disodium salt, tetraisopropyl titanate (TIPT), butyltin tris-2-ethylhexanoate (FASCAT 4102), 1,8-diazabicyclo[5.4.0]undec-7-ene (DBU), zinc acetylacetonate hydrate (Zn(acac) 2 ), zinc acetate (Zn(OAc) 2 ), manganese(II) acetate (Mn(OAc) 2 ), hydrotalcite, zeolite, lithium chloride, or combinations thereof.

[0030] The depolymerization conditions may include temperatures of 120° C. to 260° C. and absolute pressures of 10 atmospheres (atm) (147 psig) to 70 atm (1029 psig) for 0.5 to 10 hours in an agitated reactor. In an embodiment, the increased pressure may help to prevent methanol from vaporizing at the temperatures utilized in the depolymerization conditions. One or more reactors may be used to react the polyester with one or more glycols and methanol. For example, the reaction mixture may be continuously withdrawn from a first stage and introduced, along with additional glycol and / or methanol, to a second stage maintained under the aforementioned pressure ranges, with the depolymerization continuing to the desired degree of completion. In various embodiments, any type of vessel, reactor, and / or reactor system may be utilized for the depolymerization or glycolysis of the polyester composition. In an embodiment, a continuous stirred tank reactor or vessel, a fixed bed reactor, or a melt extruder may be utilized. In the same or alternative embodiments, the depolymerization or glycolysis of the polyester composition may be a batch or continuous process.

[0031] After exposure to the depolymerization conditions detailed above, the resulting mixture can be optionally cooled to a temperature below about 150° C., or between about 50° C. and about 150° C. In embodiments, the resulting mixture can be cooled to a desired temperature in the glycolysis reactor or transferred to a different vessel to reduce the temperature. The resulting mixture can include a solid component and a liquid component. In embodiments, the liquid component can include one or more depolymerization products, such as monomers and / or oligomers having a degree of polymerization of 2 to 10, along with one or more glycols, and can further include any additional soluble components from the polyester composition, one or more glycols, catalyst, or combinations thereof. In various embodiments, the solid component can be residual foreign matter and any other insoluble components of the polyester composition and can be considered waste to be disposed of.

[0032] As further discussed below, the liquid component is further subjected to at least a methanolysis and / or alcoholysis process to recover one or more dialkyl terephthalates. In various embodiments, the liquid component can be separated from the solid component prior to the methanolysis process. In embodiments, the liquid component may be separated from the solid component using any system. In one embodiment, the liquid component can be separated from the solid component while the resulting mixture is at a temperature of about 50° C. to about 150° C. In such an embodiment, separating the liquid component from the solid component at a temperature of about 150° C. or less, e.g., about 50° C. to about 150° C., can provide a more efficient and / or less resource intensive process than current conventional processes. In the same or alternative embodiment, separating the liquid component from the solid component at a temperature of about 150° C. or less, e.g., about 50° C. to about 150° C., can be beneficial because some impurities may be unstable at higher temperatures, e.g., temperatures above 150° C., thereby adversely affecting the process described herein, product yield, and / or product purity.

[0033] In various embodiments, the separation of the liquid component from the solid component may include a filtration process. In such embodiments, any suitable filtration process capable of withstanding elevated filtration temperatures of about 50° C. to about 150° C. may be utilized. In certain embodiments, the solid components may be removed by centrifugation. In certain embodiments, the solids may be removed by settling or sedimentation. In certain embodiments, the solid components may settle to the bottom of the vessel, and the liquid components may be removed through vessel conduits or valves appropriately positioned within the vessel. In one embodiment, such conduits and / or valves may include filtration devices to minimize inclusion of the solid components in downstream processes.

[0034] Alcoholysis of one or more of the depolymerization products As discussed above, in embodiments, one or more of the depolymerized products produced in the glycolysis process described above may be subjected to an alcoholysis process.

[0035] Generally, in a typical alcoholysis process, a polyester is reacted with an alcohol, such as methanol, to produce a depolymerized mixture that includes oligomers, terephthalate monomers, such as dimethyl terephthalate (DMT), and one or more glycols. In other embodiments, depending on the composition of the polyester, other monomers may also be produced, such as, for example, CHDM, DEG, and dimethyl isophthalate (DMI). In one embodiment, during the alcoholysis process, terephthalate oligomers are reacted with methanol to produce a depolymerized polyester mixture that includes polyester oligomers, DMT, CHDM, and / or EG.

[0036] Some representative examples of the methanolysis of PET are described in U.S. Patent Nos. 3,321,510; 3,776,945; 5,051,528; 5,298,530; 5,414,022; 5,432,203; 5,576,456; and 6,262,294, which are incorporated herein by reference.

[0037] In an embodiment, the alcoholysis process may include exposing the liquid component and / or one or more depolymerized products obtained from the glycolysis process to an alcohol composition under conditions that result in one or more dialkyl terephthalates. As discussed above, in an embodiment, the one or more depolymerized products may be present in the liquid component obtained from the glycolysis process. In various embodiments, as discussed above, before subjecting the one or more depolymerized products and / or liquid component obtained from the glycolysis process to the alcoholysis process, the liquid component may be separated from the resulting mixture of the glycolysis process and / or from the resulting solid component. In certain embodiments, after separating the liquid component from the solid component of the glycolysis process, the liquid component may be directly utilized in the alcoholysis process. In the same or alternative embodiments, after separating the liquid component from the solid component of the glycolysis process, the liquid component is not subjected to further processing, such as distillation and / or other separation processes, before being utilized in the alcoholysis process. Without being bound to any particular theory, it is believed that because the glycolysis process is carried out using a smaller amount of glycol (or a weight ratio of glycol to amount of polyester composition of from 3:1 to 1:9) compared to certain conventional processes, the liquid components resulting from the glycolysis process can be utilized directly in the alcoholysis process without the need for further processing, for example, to concentrate the resulting depolymerization product(s) and / or remove a portion of the glycol.

[0038] The alcohol composition may comprise any suitable alcohol known in the art for use in an alcoholysis process to obtain a particular dialkyl terephthalate. In one embodiment, the alcohol composition may be and / or comprise methanol. In an embodiment, when methanol is utilized as the alcohol composition, it may be the methanolysis product that results in DMT.

[0039] In certain embodiments, the amount of the alcohol composition may be any amount that is in excess by weight relative to the amount or weight of the polyester composition. In certain embodiments, the weight ratio of the amount of the alcohol composition to the amount of the polyester composition may be from about 2:1 to about 10:1. In various embodiments, the weight ratio of the amount of the alcohol composition to the amount of the polyester composition may be from about 2:1 to about 9:1, from about 2:1 to about 8:1, from about 2:1 to about 7:1, from about 2:1 to about 6:1, or from about 2:1 to about 5:1. In embodiments, the amount of the polyester composition refers to the amount or weight of the polyester composition utilized in the glycolysis process described above.

[0040] In embodiments, the alcoholysis reaction may be carried out at a temperature of about 90° C. or less, about 80° C. or less, about 70° C. or less, about 60° C. or less, about 50° C. or less, about 40° C. or less, or about 30° C. or less. In the same or alternative embodiments, the alcoholysis reaction may be carried out at a temperature of about 20° C. to about 90° C., about 20° C. to about 80° C., about 20° C. to about 70° C., about 20° C. to about 60° C., about 20° C. to about 50° C., about 20° C. to about 40° C., or about 20° C. to about 30° C. In certain embodiments, the alcoholysis reaction may be carried out at a temperature of about 25° C. to about 90° C., about 25° C. to about 80° C., about 25° C. to about 70° C., about 25° C. to about 60° C., about 25° C. to about 50° C., about 25° C. to about 40° C., or about 25° C. to about 30° C. In various aspects, without being bound to any particular theory, it is believed that in the methods disclosed herein, the polyester in the polyester composition has already undergone at least a partial depolymerization process, e.g., in the glycolysis step discussed above, so that the methanolysis process can be carried out at the relatively reduced temperatures described above compared to certain other conventional processes. Additionally or alternatively, without being bound to any particular theory, it is believed that the alcoholysis process can be carried out at the reduced temperatures described above because one or more depolymerization products produced in the glycolysis process are separated from waste or insoluble materials prior to the alcoholysis process.

[0041] In embodiments, the alcoholysis process may be carried out in any suitable reactor and / or vessel. In embodiments, the alcoholysis reactor may be in fluid communication with the reactor utilized in the glycolysis process described above. In certain embodiments, the alcoholysis reactor is a different reactor than the vessel used for glycolysis. Alternatively, in various embodiments, the alcoholysis process may be carried out in the same vessel as the glycolysis process and / or filtration process described above. In certain embodiments, the alcoholysis process may be carried out at ambient pressure, e.g., at a pressure of about 1 atm, or from about 1 atm to about 5 atm, or from about 1 atm to about 3 atm, or from about 1 atm to about 2 atm. In various embodiments, the alcoholysis reaction may be carried out at pressures above ambient pressure, e.g., greater than 1 atm, or less than about 5 atm, less than about 3 atm, less than about 2 atm, when the alcoholysis reaction temperature is high relative to the process conditions disclosed herein, e.g., greater than about 50° C., greater than about 60° C., greater than about 70° C., greater than about 80° C., or greater than about 90° C.

[0042] In various embodiments, an alcoholysis catalyst can be utilized in the alcoholysis process. In embodiments, the alcoholysis catalyst may be present in an amount of about 0.1 wt.% to about 20 wt.% based on the weight of the polyester composition, or about 0.1 wt.% to about 10 wt.% based on the weight of the polyester composition, or about 0.1 wt.% to about 5 wt.% based on the weight of the polyester composition, or about 0.1 wt.% to about 2 wt.% based on the weight of the polyester composition, or about 0.1 wt.% to about 1 wt.% based on the weight of the polyester composition, or about 0.1 wt.% to about 0.5 wt.% based on the weight of the polyester composition. In such embodiments, the amount of polyester composition refers to the amount or weight of the polyester composition utilized in the above-mentioned alcoholysis process. In various embodiments, the amount of alcoholysis catalyst disclosed in this paragraph refers to the amount of alcoholysis catalyst present in the alcoholysis reaction. In various embodiments, the amount of alcoholysis catalyst disclosed in this paragraph refers to the amount of alcoholysis catalyst added to one or more depolymerization products and one or more alcohols to promote the alcoholysis reaction. In certain embodiments, a reduced or smaller amount of alcoholysis catalyst can be added to one or more depolymerization products and one or more alcohols to promote the alcoholysis reaction, for example, about 0.1 wt.% to about 10 wt.% by weight of the polyester composition, or about 0.1 wt.% to about 5 wt.% by weight of the polyester composition, or about 0.1 wt.% to about 2 wt.% by weight of the polyester composition, or about 0.1 wt.% to about 1 wt.% by weight of the polyester composition, or about 0.1 wt.% to about 0.5 wt.% by weight of the polyester composition. In embodiments, such a smaller amount of alcoholysis catalyst can be added, at least in part, because the alcoholysis catalyst is already present in one or more depolymerization products and / or one or more alcohols. In such embodiments, as discussed below, the alcohol and / or glycol may be recycled and reused in subsequent glycolysis and alcoholysis processes disclosed herein, which may include at least a portion of the alcoholysis catalyst from the preceding alcoholysis and / or glycolysis process.

[0043] In various embodiments, the alcoholysis catalyst is a carbonate catalyst, such as, but not limited to, K 2 CO 3 , Na 2 CO 3 , Li 2 CO 3 , Cs 2 CO 3 hydroxide catalysts, such as, but not limited to, KOH, LiOH, NaOH; alkoxide catalysts, such as, but not limited to, NaOMe, Mg(OMe) 2 , KOMe, KOt-Bu, ethylene glycol monosodium salt, ethylene glycol disodium salt, or combinations thereof. In certain embodiments, the alcoholysis catalyst may include KOH, NaOH, LiOH, or combinations thereof. In certain embodiments, the alcoholysis catalyst may include NaOMe, KOMe, Mg(OMe) 2 , KOt-Bu, ethylene glycol monosodium salt, ethylene glycol disodium salt, or combinations thereof. In various embodiments, the alcoholysis catalyst may be in solid form, in solution form in water, methanol, or ethylene glycol, or combinations thereof. In certain embodiments, the alcoholysis catalyst may be added to the one or more depolymerization products and the alcohol composition once the alcohol composition and the one or more depolymerization products reach the desired reaction temperature or temperature range disclosed above.

[0044] The one or more depolymerization products may be exposed to the alcohol composition and optionally the alcoholysis catalyst under the above-mentioned temperature and pressure conditions for a time to achieve a desired yield of the resulting dialkyl terephthalate. In certain embodiments, the one or more depolymerization products may be exposed to the alcohol composition and optionally the alcoholysis catalyst under the above-mentioned temperature and pressure conditions for a time of about 5 minutes to about 5 hours, or about 5 minutes to about 2 hours, or about 5 minutes to about 1 hour, or about 5 minutes to about 30 minutes, or about 5 minutes to about 15 minutes, or about 5 minutes to about 10 minutes.

[0045] In an embodiment, the alcoholysis process results in a mixture comprising one or more dialkyl terephthalates. In various embodiments, the alcoholysis process results in a mixture in which the dialkyl terephthalates are insoluble and / or solid components. In an embodiment, the liquid components of the mixture may comprise one or more glycols, methanol, alcohol compositions, or combinations thereof. In an embodiment, at least a portion of the glycols and / or methanol may be glycols and / or methanol utilized in the glycolysis process that were present with the one or more depolymerization products at the start of the alcoholysis process. In various embodiments, the dialkyl terephthalates may be isolated from the mixture using any known separation technique, such as filtration, centrifugation, precipitation, sedimentation, or a combination of one or more separation techniques. In an embodiment, the filtration may include washing the solid components with additional alcohol compositions or other solvents. The resulting liquid components may include filtrates and washes. The resulting solid component may comprise about 90 wt.% or more of a dialkyl terephthalate, e.g., DMT, about 93 wt.% or more of a dialkyl terephthalate, e.g., DMT, or about 95 wt.% or more of a dialkyl terephthalate, e.g., DMT, based on the weight of the solid component. In the same or alternative embodiments, the dialkyl terephthalate, e.g., DMT, in the resulting solid component may be about 90% or more pure, about 93% or more pure, or about 95% or more pure. In various embodiments, the solid component may also comprise dimethyl isophthalate (DMI). In such embodiments, the DMI may be present in an amount of about 1000 ppm or less, or about 500 ppm or less, or about 1 ppm to about 1000 ppm, or about 1 ppm to about 500 ppm. In one or more embodiments, the solid component may also comprise bisphenol A (BPA). In such embodiments, BPA may be present in an amount of about 1000 ppm or less, or about 500 ppm or less, or from about 1 ppm to about 1000 ppm, or from about 1 ppm to about 500 ppm.

[0046] The processes described herein, e.g., glycolysis and / or alcoholysis processes, are substantially milder than certain conventional processes, e.g., high temperature one-step glycolysis or methanolysis processes. For example, certain conventional one-step processes use Lewis acid catalysts, e.g., Zn(OAc) 2or KOAc, the glycolysis process may be utilized at temperatures of 240° C. or higher. Such harsh conditions may result in reduced EG yield from the depolymerization due to the conversion of EG in various side reactions to various impurity compounds, including, but not limited to, diethylene glycol (DEG), triethylene glycol (TEG), acetaldehyde, 1,1-dimethoxyethane, 1,2-dimethoxyethane, dioxane, 2-methoxyethanol, 1-methoxyethanol, and dimethyl ether. In an embodiment, the process described herein is substantially milder than such conventional processes, and further results in less EG yield loss, for example, due to fewer side reactions that convert EG to various impurities. In an embodiment, the process described herein results in about 5% or less EG yield loss, about 2% or less EG yield loss, or about 1% or less EG yield loss, or about 0.5% or less EG yield loss. In such an embodiment, the EG yield loss is the percentage of EG formed into impurities, e.g., DEG, relative to the combined amount of EG from the polyester composition feed and EG added in the glycolysis process. In the same or alternative embodiment, the process described herein produces minimal glycol impurities.For example, in one embodiment, the process described herein can result in a net production of about 5 wt.% or less DEG, about 2 wt.% or less DEG, or about 1 wt.% or less DEG, or about 0.5 wt.% or less DEG, or about 0.01 wt.% to about 5 wt.% DEG, about 0.01 wt.% to about 2 wt.% DEG, or about 0.01 wt.% to about 1 wt.% DEG, or about 0.01 wt.% to about 0.5 wt.% DEG, or about 0.01 wt.% to about 0.2 wt.% DEG when EG is used as one or more glycols in the glycolysis process.In an embodiment, the processes described herein can result in a net generation of about 5 wt.% or less DEG and / or other impurities, about 2 wt.% or less DEG and / or other impurities, or about 1 wt.% or less DEG and / or other impurities, or about 0.5 wt.% or less DEG and / or other impurities, or about 0.01 wt.% to about 5 wt.% DEG and / or other impurities, about 0.01 wt.% to about 2 wt.% DEG and / or other impurities, or about 0.01 wt.% to about 1 wt.% DEG and / or other impurities, or about 0.01 wt.% to about 0.5 wt.% DEG and / or other impurities, or about 0.01 wt.% to about 0.2 wt.% DEG and / or other impurities when EG is used as one or more glycols in the glycolysis process. In an embodiment, the net generation of DEG (or other impurities) is the weight percent of the amount of DEG or other impurities present relative to the amount of DEG or other impurities present in the polyester composition feed. In an embodiment, the DEG produced may be produced in a glycolysis process described herein and / or an alcoholysis process described herein. In certain embodiments, when EG is used as one or more glycols in the glycolysis process, EG such as DEG and / or any glycol impurities may be present in the liquid component resulting from the alcoholysis step. In certain embodiments, the utilization of a Lewis base catalyst, e.g., a hydroxide-based or carbonate-based catalyst, in the glycolysis process may also facilitate or contribute to the reduction of EG decomposition and / or the reduction of glycol impurities.

[0047] Recycling of glycol, methanol, and alcohol compositions As discussed above, in various embodiments, the glycol and / or methanol utilized in the glycolysis process can be reused in a subsequent process sequence to recover one or more dialkyl terephthalates disclosed herein. In embodiments, at a high level, the liquid component obtained from the alcoholysis process can be processed for reuse, for example, for reuse in a subsequent glycolysis and / or methanolysis sequence of a subsequent polyester composition to recover one or more dialkyl terephthalates. In the same or alternative embodiments, methanol can be recovered from the liquid component obtained from the alcoholysis process, for example, reused in a subsequent alcoholysis process or used in the glycolysis or depolymerization process described above. In such embodiments, methanol can be recovered by exposing the liquid component to distillation conditions.

[0048] In embodiments, as discussed above, the liquid component resulting from the alcoholysis process may include glycols and / or methanol used in the glycolysis process, alcohol compositions, glycols generated in the glycolysis process, e.g., EG, DEG, and / or CHDM. In various embodiments, this liquid component may be subjected to a separation process, e.g., to remove or separate at least a portion of the alcohol composition, e.g., methanol, or a mixture of methanol and ethylene glycol. In certain embodiments, the liquid component may be exposed to distillation or short path distillation to remove at least a portion of the alcohol composition. In exemplary non-limiting embodiments, the distillation conditions may include exposing the liquid component to a temperature of about 260° C. or less, about 220° C. or less, about 200° C. or less, about 180° C. or less, about 160° C. or less, about 150° C. or less, about 130° C. or less, about 60° C. or more, about 70° C. or more, about 60° C. to about 220° C., about 70° C. to about 220° C., about 60° C. to about 180° C., or about 60° C. to about 160° C. In the same or alternative embodiments, the distillation conditions may include a pressure of about 1 Torr (133.3 Pa) to about 800 Torr (106,657 Pa), or about 30 Torr (3999 Pa) to about 500 Torr (66,661 Pa). In embodiments, the liquid component may be exposed to the distillation conditions until all or a substantial portion of the alcoholic composition is removed from the liquid component, e.g., vaporized. In certain embodiments, at least a portion of the alcohol composition, e.g., methanol, if present with the recycle glycol, may be utilized during a subsequent glycolysis process. In certain embodiments, the alcohol, e.g., methanol, recovered from the liquid component may be returned to the alcoholysis reactor for use in a subsequent alcoholysis process and / or may be returned to the glycolysis reactor for use in the glycolysis process described above.

[0049] In embodiments, distillation of the liquid components may be carried out in any vessel or distillation system suitable for use in the methods and systems described herein. In one embodiment, the distillation vessel can be in fluid communication with the alcoholysis reaction vessel and / or any component of the filtration process utilized subsequent to alcoholysis, for example, to isolate the dialkyl terephthalate solid or insoluble components. In the same or alternative embodiments, the distillation vessel can be in fluid communication with the glycolysis vessel.

[0050] In various embodiments, distillation of the liquid component can vaporize the alcohol composition and leave a pot residue. In various embodiments, the pot residue includes glycols and any other heavies present in the liquid component, such as non-vaporizable compounds. In embodiments, the glycols in the pot residue can be referred to as recycled glycols, and / or the glycols from the non-vaporizable portion of the continuous distillation process using the distillation conditions described herein can be referred to as recycled glycols. In an embodiment, the recycled glycols can include ethylene glycol (EG), diethylene glycol (DEG), triethylene glycol (TEG), 1,4-cyclohexanedimethanol (CHDM), poly(ethylene glycol) (PEG), neopentyl glycol (NPG), propanediol (PDO), butanediol (BDO), 2-methyl-2,4-pentanediol (MP diol), poly(tetramethylene ether) glycol (PTMG), or combinations thereof.

[0051] In an embodiment, as discussed above, the recycled glycol may be utilized in a subsequent process sequence described herein to recover one or more dialkyl terephthalates from the polyester composition. Furthermore, in an embodiment, the recycled glycol may be recycled again using the process described herein after this subsequent dialkyl terephthalate recovery sequence. In an embodiment, the recycled glycol may be recovered and reused at least two times, at least three times, at least four times, or at least five times. In certain embodiments, when the recycled glycol is used in a subsequent dialkyl terephthalate recovery sequence, the addition of a catalyst in the subsequent glycolysis step may be omitted since the recycled glycol may contain a used catalyst.

[0052] In embodiments, it has been unexpectedly discovered that when recycled glycol is recovered and reused, the resulting recovered dialkyl terephthalate exhibits a purity comparable to that of dialkyl terephthalate recovered using glycol that was not recovered and reused. In embodiments, this comparable purity of dialkyl terephthalate exists after reusing recycled glycol at least two, at least three, at least four, or at least five times, resulting in the recovery of dialkyl terephthalate having a purity of at least about 90%, at least about 93%, or at least about 95%.

[0053] Exemplary System FIG. 1 illustrates generally one exemplary system and / or method for recovering one or more dialkyl terephthalates from a polyester composition. System 100 includes a source 110 of a polyester composition, such as the polyester composition described above. In one exemplary embodiment, the polyester composition can undergo an optional pretreatment process, as discussed in detail above. In such an embodiment, this optional pretreatment can occur prior to exposing the polyester composition to depolymerization conditions in vessel 120. Vessel 120 represents a glycolysis vessel, in which the polyester composition is received and exposed to one or more glycols and methanol under depolymerization conditions, as discussed in detail above. In an embodiment, vessel 120 can be in fluid communication with source 110. In various embodiments, as discussed above, the polyester composition is converted to one or more depolymerization products after being exposed to depolymerization conditions in vessel 120. In various embodiments, as discussed above, the one or more depolymerization products may include monomers and / or oligomers having a degree of polymerization of 2-10, 2-8, 2-6, or 2-4. In embodiments, the one or more depolymerization products are present in a mixture including a liquid component and a solid component, with the one or more depolymerization products in the liquid component. In embodiments, as discussed above, the mixture is exposed to a solid-liquid separation device 130, e.g., a filtration system, where the liquid component including the one or more depolymerization products is separated from the solid component. In various embodiments, the solid-liquid separation device 130 may be in fluid communication with vessel 120 and / or vessel 140, as discussed herein. In the embodiment shown in FIG. 1, the one or more depolymerization products and / or liquid components may be exposed to alcoholysis conditions in vessel 140. In embodiments, the one or more depolymerization products and / or liquid components may be directly utilized in the alcoholysis process. In such embodiments, the one or more depolymerization products and / or liquid components may not be subjected to any further processing, such as distillation and / or other separation processes, before being utilized in the alcoholysis process. Alcohololysis conditions are discussed in detail above.In embodiments, as discussed above, alcoholysis of one or more depolymerization products and / or liquid components may result in a mixture including an insoluble or solid component including dialkyl terephthalate, and a liquid component including alcohol compositions, glycols, methanol, and potentially other soluble components as described herein. As discussed above, the resulting alcoholysis reaction mixture may be exposed to a solid-liquid separation device 150, e.g., a filtration system, to separate the solid component including recovered dialkyl terephthalate 160. In embodiments, solid-liquid separation device 150 may be in fluid communication with vessel 140. In various embodiments, the liquid component resulting from solid-liquid separation in solid-liquid separation device 150 may include one or more alcohols, e.g., methanol, and / or one or more glycols. In such embodiments, the liquid component may be exposed to one or more distillation or other separation processes in system 170. In system 170, one or more alcohols, e.g., methanol, may be separated from the liquid component as discussed above and optionally returned to vessel 140 for use in a subsequent alcoholysis process and / or returned to vessel 120 for use in a subsequent glycolysis process. In the same or alternative embodiment, in system 170, one or more glycols may be recovered as discussed above and returned to vessel 120 alone or together with recovered methanol for a subsequent depolymerization process. Additionally, in various embodiments, system 170 may selectively remove EG from the liquid component for purposes other than storage or return to vessel 120. System 170 may be any type of separation or distillation system suitable for selectively recovering one or more alcohols and / or one or more glycols from the liquid component. In certain embodiments, the methods described herein relating to system 100 may be implemented as continuous, batch, or semi-continuous methods. It is understood that system 100 is merely an example system and other configurations of system components are contemplated by the disclosure herein. For example, one or more components of the system 100 may not be physically separate or distinct from one or more other components of the system 100 .It is further understood that system 100 is depicted merely diagrammatically to highlight aspects of the methods disclosed herein.

[0054] Use of Recovered Dialkyl Terephthalates to Form Polyesters or Other Products As discussed above, the methods disclosed herein can result in high purity dialkyl terephthalates such as DMT. For example, in certain embodiments, the recovered DMT may be utilized to form one or more polyesters, including, but not limited to, PET and TMCD-containing polyesters. In certain embodiments, the polyesters formed using the recovered DMT may be referred to as recycled polyesters. In various embodiments, the products formed using the recovered DMT may be indistinguishable from similar products formed from virgin DMT. In such embodiments, any suitable process for forming PET and TMCD-containing polyesters may be utilized, since the DMT is of sufficient purity.

[0055] In the same or alternative embodiments, the recovered DMT may be utilized to form CHDM. In various embodiments, the CHDM formed using the recovered DMT may be indistinguishable from CHDM formed from virgin DMT due to the high purity of the recovered DMT. In such embodiments, the CHDM may be formed from the recovered DMT using any suitable process.

[0056] In various embodiments, the recovered DMT may be utilized to form one or more plasticizers. In certain embodiments, the plasticizers formed using the recovered DMT may include dibutyl terephthalate (DBT) and / or dioctyl terephthalate (DOTP). In various embodiments, the DBT and / or DOTP formed using the recovered DMT may be indistinguishable from the DBT and / or DOTP, respectively, formed from virgin DMT due to the high purity of the recovered DMT. In such embodiments, the DBT and / or DOTP may be formed from the recovered DMT using any suitable process. EXAMPLES

[0057] material FDST-5 contains 100 mol % TPA, 93.0 mol % EG, 4.1 mol % CHDM, and 2.9 mol % DEG and is available from Eastman. IV: 0.751 dL / g.

[0058] Ethylene glycol (EG), methanol, potassium carbonate, and 50% aqueous sodium hydroxide were obtained from commercial suppliers. All chemicals and reagents were used as received unless otherwise noted.

[0059] Analytical procedures Gas Chromatography (GC) Analysis. GC analysis was performed on an Agilent Model 7890B Gas Chromatograph equipped with a 7693A autosampler and two G4513A towers. The GC was equipped with two columns, a 60m x 0.32mm x 1.0 micron DB-1701™ (J&W123-0763) and a 60m x 0.32 x 1 micron DB-1™ (J&W123-1063), and samples were injected simultaneously onto both columns. A common oven temperature program was used and sample components were detected by flame ionization detection (FID). A five-point calibration was performed for components of interest. The gas chromatograph was interfaced to an EZChrom Elite Chromatography Data System.

[0060] Methanolysis product samples were prepared by adding a known volume of pyridine-based internal standard solution to a known mass of sample, followed by derivatization with N,O-bis(trimethylsilyl)trifluoroacetamide (BSTFA). The GC wt.% of BHET (bis(hydroxyethyl)terephthalate), GC wt.% of MHT (4-(methoxycarbonyl)benzoic acid), and GC wt.% of MHET (methyl-2-hydroxyethyl terephthalate) are provided as readouts from the GC process software.

[0061] The % yield of DMT (dimethyl terephthalate) was calculated as follows: (weight of final DMT) / (weight of theoretical DMT). * 100%. DMT GC purity % was calculated as follows: (wt.% DMT in final product by GC) / (total wt.% by GC). * 100%. Major impurities as shown by GC include MeOH, water, and EG. DMT purity in almost all examples is greater than 99% excluding MeOH, water, and EG.

[0062] Measurement of Intrinsic Viscosity. The intrinsic viscosity (IV) of certain polymeric materials useful herein is determined according to the ASTM D2857-70 procedure on a LabGlass Wagner Viscometer with a 1 / 2 mL capillary valve using a polymer concentration of about 0.5 wt % in 60 / 40 phenol / tetrachloroethane by weight. The procedure is performed by heating the polymer / solvent system at 120° C. for 15 minutes, cooling the solution to 25° C., and measuring the flow time at 25° C. The IV is calculated from the following formula:

[0063]

number

[0064] (wherein η is the intrinsic viscosity at 25° C. at a polymer concentration of 0.5 g / 100 mL of solvent, tS is the sample flow time, t0 is the solvent blank flow time, and C is the polymer concentration in grams per 100 mL of solvent). The unit of intrinsic viscosity in this application is deciliter / gram.

[0065] Viscosity is measured in tetrachloroethane / phenol (50 / 50, by weight) at 30° C. and can be calculated by the following formula:

[0066]

number

[0067] (In the formula, η sp is the specific viscosity and C is the concentration).

[0068] Example 1: PET depolymerization with EG and methanol in a 1:1 wt. ratio at 195° C. followed by methanolysis In this Example 1, for depolymerization, a 100 mL autoclave was equipped with a mechanical stirrer, thermocouple, gas inlet, and vent. Ground FDST-5 (15.18 g), ethylene glycol (15.57 g), methanol (15.14 g), and potassium carbonate (0.1533 g) were charged to the reactor. The vessel was pressurized to 150 psig (10.20 atm) using nitrogen, and the mixture was heated to 195° C. When the internal temperature reached 195° C., the pressure was adjusted to 750 psig (51.03 atm). This condition was held for 3 hours. The crude mixture was cooled to 25° C., and the pressure was released. GC analysis showed that the crude mixture contained 5.2% BHET, 14.4% MHET, and 17.4% DMT.

[0069] For methanolysis, the crude product was diluted with MeOH (45.0 g) and heated to 50° C. NaOH (50 wt%, 93 uL) was added. The resulting mixture was held at 50° C. for 30 min, then cooled to ambient temperature and held for an additional 2 h. After filtration and MeOH washing, the product was isolated as a white solid (85.0% yield, 99% purity).

[0070] Example 2: PET depolymerization with EG and methanol in a 1:1 wt. ratio at 215°C A 100 mL autoclave was equipped with a mechanical stirrer, thermocouple, gas inlet, and vent. Ground FDST-5 (15.06 g), ethylene glycol (15.22 g), methanol (15.07 g), and potassium carbonate (0.1554 g) were charged to the reactor. The vessel was pressurized to 150 psig (10.20 atm) using nitrogen, and the mixture was heated to 215 °C. When the internal temperature reached 215 °C, the pressure was adjusted to 750 psig (51.03 atm). This condition was held for 3 hours. The crude mixture was cooled to 25 °C, and the pressure was released. GC analysis showed that the crude mixture contained 5.2% BHET, 14.9% MHET, and 15.1% DMT.

[0071] Example 3: PET depolymerization with EG and methanol at 4:1 wt. ratio at 195°C A 100 mL autoclave was equipped with a mechanical stirrer, thermocouple, gas inlet, and vent. Ground FDST-5 (15.01 g), ethylene glycol (24.48 g), methanol (6.07 g), and potassium carbonate (0.1504 g) were charged to the reactor. The vessel was pressurized to 150 psig (10.20 atm) using nitrogen, and the mixture was heated to 195 °C. When the internal temperature reached 195 °C, the pressure was adjusted to 750 psig (51.03 atm). This condition was held for 3 hours. The crude mixture was cooled to 25 °C, and the pressure was released. GC analysis showed that the crude mixture contained 16.2% BHET, 15.7% MHET, and 3.8% DMT.

[0072] Example 4: PET depolymerization with EG and methanol at 1:0 wt. ratio at 195°C A 500 mL RB (round bottom) flask was equipped with a mechanical stirrer, thermocouple, gas inlet and vent. Ground FDST-5 (30 g), ethylene glycol (70 g) and potassium carbonate (1 wt.%) were charged to the reactor. The mixture was heated to 195° C. at ambient pressure. These conditions were maintained for 3 hours. The crude mixture was cooled to 25° C. GC analysis showed that the crude mixture contained 33.1% BHET and no DMT.

[0073] Example 5: PET depolymerization with EG and methanol at 0:1 wt. ratio at 195°C A 100 mL autoclave was equipped with a mechanical stirrer, thermocouple, gas inlet and vent. Ground FDST-5 (15.01 g), methanol (approximately 30 g), and potassium carbonate (0.1504 g) were charged to the reactor. The vessel was pressurized to 150 psig (10.20 atm) using nitrogen and the mixture was heated to 195°C. Once the internal temperature reached 195°C, the pressure was adjusted to 750 psig (51.03 atm). This condition was held for 3 hours. The crude mixture was cooled to 25°C and the pressure was released. GC analysis showed that the crude mixture contained 1.2 wt.% 0.1 wt.% BHET, 3.7 wt.% MHET, and 39.9 wt.% DMT.

[0074] Tables 1 and 2 below summarize the results of the above examples.

[0075] [Table 1]

[0076] [Table 2]

[0077] As shown in Table 1, the BHET% and DMT% in the depolymerized products are strongly correlated with the MeOH / EG ratio. Furthermore, when different ratios of MeOH / EG were used, the MHET% remained around 15%, whereas the MHET level dropped significantly when pure EG or MeOH was used. As shown in Table 2 and Figure 2, the ratio of methyl esters / EG esters was plotted against the ratio of MeOH / EG in the feed. The plot has a slope of 1.02 and an R of 0.99. 2 This suggested that methanol has a similar reactivity to EG, as shown by

[0078] Example 6: GC and NMR analysis of DMT products Additionally, the crude depolymerized product of Example 1 was subjected to methanolysis conditions at 50° C. The DMT product was isolated in 85% yield in two steps. Both NMR and GC showed that the purity of the product was 99%. Figure 3 shows a graph of the GC data.

[0079] The present disclosure may also be described according to the following numbered sections: Item 1. A method for recovering one or more dialkyl terephthalates from a polyester composition, comprising: exposing a first polyester composition to a first composition comprising one or more glycols and methanol under depolymerization conditions in a first reaction vessel to prepare a first mixture, the first mixture comprising one or more first depolymerization products, the depolymerization conditions comprising a temperature of 150°C to 260°C and a pressure of 10 atm to 70 atm; cooling at least a portion of the first mixture to a temperature of 150°C or less; exposing at least a portion of the first mixture to an alcohol composition and an alcoholysis catalyst under conditions comprising a temperature of 23°C to 90°C and a pressure of 1 atm to 2 atm for 0.5 hours to 5 hours to prepare a second mixture, the second mixture comprising one or more dialkyl terephthalates; and separating at least a portion of the one or more dialkyl terephthalates by solid-liquid separation to prepare a dialkyl terephthalate solid component and a filtrate.

[0080] Item 2. The method of item 1, wherein at least a portion of the methanol is recovered from a prior process for recovering dialkyl terephthalate from a prior polyester composition. Item 3. The method of item 1, wherein the filtrate comprises one or more of glycol and methanol.

[0081] Item 4. The method of item 3, further comprising exposing a second polyester composition to at least a portion of the filtrate in the first reaction vessel under depolymerization conditions to produce one or more second depolymerized products.

[0082] Item 5. The method according to any one of Items 1 to 4, wherein the weight ratio of the amount of the one or more glycols to the amount of methanol in the first reaction vessel is 1:20 to 100:1. Item 6. The method according to any one of items 1 to 5, wherein the step of cooling at least a portion of the first mixture to a temperature of 150°C or less includes cooling at least a portion of the first mixture to a temperature of 50°C to 150°C.

[0083] Item 7. The method according to any one of Items 1 to 6, further comprising a step of separating at least a portion of the one or more first depolymerization products in the first mixture from an insoluble component in the first mixture, the separation being carried out at a temperature of 50° C. to 150° C.

[0084] Item 8. The method according to any one of items 1 to 7, wherein the weight ratio of the one or more glycols to the first polyester composition is in the range of about 1:9 to about 9:1 during exposing the first polyester composition to the first composition comprising one or more glycols and methanol under depolymerization conditions in the first reaction vessel.

[0085] Item 9. The method of any one of items 1 to 8, wherein the one or more glycols include ethylene glycol (EG), diethylene glycol (DEG), triethylene glycol (TEG), 1,4-cyclohexanedimethanol (CHDM), poly(ethylene glycol) (PEG), neopentyl glycol (NPG), propanediol (PDO), butanediol (BDO), 2-methyl-2,4-pentanediol (MP diol), poly(tetramethylene ether) glycol (PTMG), or a combination thereof.

[0086] Item 10. The method according to any one of Items 1 to 9, wherein the weight ratio of the alcohol composition to the first polyester composition can be in the range of about 2:1 to about 10:1. Item 11. The method according to any one of items 1 to 10, wherein the first polyester composition comprises polyethylene terephthalate (PET), 1,4-cyclohexanedimethanol (CHDM) modified PET, isophthalic acid (IPA) modified PET, diethylene glycol (DEG) modified PET, neopentyl glycol (NPG) modified PET, propanediol (PDO) modified PET, butanediol (BDO) modified PET, hexanediol (HDO) modified PET, 2-methyl-2,4-pentanediol (MP diol) modified PET, isosorbide modified PET, poly(tetramethylene ether) glycol (PTMG) modified PET, poly(ethylene glycol) (PEG) modified PET, polycyclohexylene dimethylene terephthalate (PCT), cyclohexanedimethanol (CHDM)-containing copolyester, isosorbide-containing copolyester, or a combination thereof.

[0087] Item 12. The method according to any one of items 1 to 11, wherein the first polyester composition comprises 0 mol% to 100 mol% CHDM, 0 mol% to 100 mol% DEG, 0 mol% to 100 mol% NPG, 0 mol% to 100 mol% PDO, 0 mol% to 100 mol% BDO, 0 mol% to 100 mol% HDO, 0 mol% to 100 mol% MP diol, 0 mol% to 100 mol% isosorbide, 0 mol% to 100 mol% PTMG, 0 mol% to 100 mol% PEG, and 0 mol% to 30 mol% isophthalic acid, wherein the total of the diol equivalents in the one or more polyesters is about 100 mol%, and the total of the diacid equivalents in the first polyester composition is about 100 mol%.

[0088] Item 13. The method according to any one of items 1 to 12, wherein the polyester composition has an intrinsic viscosity of about 0.1 dL / g to about 1.2 dL / g as determined according to ASTM D2857-70. Item 14. The method according to any one of items 1 to 13, wherein one or more polyesters present in the first polyester composition are recycled polyesters.

[0089] Item 15. The method according to any one of items 1 to 14, wherein the first polyester composition contains one or more foreign substances, and the one or more foreign substances contain at least one member selected from the group consisting of polyesters other than polyethylene terephthalate, polyvinyl chloride (PVC), polyvinyl acetal, polyvinyl butyral (PVB), polyvinyl alcohol (PVOH), ethylene vinyl alcohol (EVOH), cotton, polyolefins, polyethylene, polypropylene, polystyrene, polycarbonate, spandex, natural fibers, cellulose esters, polyacrylates, polymethacrylates, polyamides, nylons, poly(lactic acid), polydimethylsiloxanes, polysilanes, calcium carbonate, titanium dioxide, inorganic fillers, dyes, pigments, color toners, colorants, plasticizers, adhesives, flame retardants, metals, aluminum, and iron.

[0090] Item 16. The method according to item 15, wherein the one or more foreign substances are present in the polyester composition in an amount of 0.01 wt.% to 50 wt.% based on the weight of the one or more polyesters in the polyester composition.

[0091] Item 17. The method according to any one of Items 1 to 16, wherein the dialkyl terephthalate solid component comprises dimethyl terephthalate (DMT), and the DMT has a purity of at least 90%. Item 18. The method according to any one of items 1 to 17, wherein the dialkyl terephthalate solid component further comprises dimethyl isophthalate (DMI) in an amount of 1000 ppm or less, or 500 ppm or less; bisphenol A (BPA) in an amount of 1000 ppm or less, or 500 ppm or less; or both.

[0092] Item 19. The step of exposing the first polyester composition to a first composition comprising one or more glycols and methanol under depolymerization conditions in a first reaction vessel further comprises exposing the first polyester composition to one or more glycolysis catalysts, wherein the one or more glycolysis catalysts are selected from the group consisting of Li 2 CO 3 , K 2 CO 3 , CaCO 3 , Na 2 CO 3 , Cs 2 CO 3 , ZrCO3, LiOH, NaOH, KOH, Tetrabutylammonium hydroxide (TBAH), Sodium methoxide (NaOMe), Lithium methoxide (LiOMe), Magnesium methoxide (Mg(OMe) 2 , potassium t-butoxide, ethylene glycol monosodium salt, ethylene glycol disodium salt, tetraisopropyl titanate (TIPT), butyltin tris-2-ethylhexanoate (FASCAT 4102), 1,8-diazabicyclo[5.4.0]undec-7-ene (DBU), zinc acetylacetonate hydrate (Zn(acac) 2 ), zinc acetate (Zn(OAc) 2 ), manganese(II) acetate (Mn(OAc) 219. The method according to any one of items 1 to 18, comprising a member selected from the group consisting of hydrotalcite, zeolite and lithium chloride.

[0093] Item 20. One or more glycolysis catalysts are selected from the group consisting of LiOH, NaOH, KOH, tetraisopropyl titanate (TIPT), butyltin tris-2-ethylhexanoate (FASCAT 4102), ZrCO 3 , 1,8-diazabicyclo[5.4.0]undec-7-ene (DBU), sodium methoxide (NaOMe), lithium methoxide (LiOMe), zinc acetylacetonate hydrate (Zn(acac) 2 ), Cs 2 CO 3 , ethylene glycol sodium salt, and manganese(II) acetate (Mn(OAc) 2 20. The method of claim 19, comprising a member selected from the group consisting of:

[0094] Item 21. One or more glycolysis catalysts are LiOH, NaOH, KOH, sodium methoxide (NaOMe), Cs 2 CO 3 20. The method of claim 19, comprising a member selected from the group consisting of ethylene glycol sodium salt and lithium methoxide (LiOMe).

[0095] Item 22. The method according to any one of Items 15 to 21, further comprising a step of separating insoluble components in the first mixture before exposing at least a portion of the first mixture to the alcohol composition and the alcoholysis catalyst, the insoluble components including one or more foreign substances.

[0096] Item 23. The method of item 22, wherein the separating comprises filtration, centrifugation, sedimentation, settling, or a combination thereof. Item 24. The method according to items 1 to 23, wherein the alcohol composition contains methanol.

[0097] Item 25. The method according to any one of items 1 to 24, wherein the alcoholysis catalyst is present in an amount of 0.1 wt.% to 20 wt.% based on the weight of the first polyester composition. Item 26. The alcoholysis catalyst is K 2 CO 3 , Na 2 CO 3 , Li 2 CO 3 , Cs 2 CO 3 ;KOH, LiOH, NaOH;NaOMe, Mg(OMe) 2 26. The method according to any one of claims 1 to 25, comprising: KOMe, KOt-Bu, ethylene glycol monosodium salt, ethylene glycol disodium salt, or a combination thereof.

[0098] Item 27. The method of item 26, wherein the alcoholysis catalyst comprises KOH, NaOH, NaOMe, or a combination thereof. Item 28. The method of items 1 to 27, carried out as a batch process, a semi-continuous process, or a continuous process.

[0099] Item 29. The method of any one of items 1 to 28, wherein the one or more depolymerization products include monomers, oligomers, or combinations thereof. Item 30. The method according to item 29, wherein the one or more oligomers have a degree of polymerization of 2 to 10.

[0100] The present disclosure has been described in detail with particular reference to certain embodiments thereof, but it will be understood that variations and modifications can be made within the spirit and scope of the disclosure.

Claims

1. 1. A method for recovering one or more dialkyl terephthalates from a polyester composition, the method comprising: exposing a first polyester composition to a first composition comprising one or more glycols and methanol under depolymerization conditions in a first reaction vessel to provide a first mixture, the first mixture comprising one or more first depolymerization products, the depolymerization conditions comprising a temperature of 150° C. to 260° C. and a pressure of 10 atm to 70 atm; cooling at least a portion of the first mixture to a temperature of 150° C. or less; exposing at least a portion of the first mixture to an alcohol composition and an alcoholysis catalyst under conditions comprising a temperature of 23° C. to 90° C. and a pressure of 1 atm to 2 atm for 0.5 hours to 5 hours to provide a second mixture, the second mixture comprising one or more dialkyl terephthalates; and separating at least a portion of the one or more dialkyl terephthalates by solid-liquid separation to provide a dialkyl terephthalate solid component and a filtrate.

2. 10. The method of claim 1, wherein at least a portion of the methanol is recovered from a prior process for recovering dialkyl terephthalate from a prior polyester composition.

3. 10. The method of claim 1 , wherein the filtrate comprises one or more of glycol and methanol.

4. 4. The method of claim 3, further comprising exposing a second polyester composition to at least a portion of the filtrate in the first reaction vessel under depolymerization conditions to produce one or more second depolymerized products.

5. 2. The process of claim 1, wherein the weight ratio of the amount of one or more glycols to the amount of methanol in the first reaction vessel is from 1:20 to 100:

1.

6. 10. The method of claim 1 , wherein the step of cooling at least a portion of the first mixture to a temperature of 150° C. or less comprises cooling at least a portion of the first mixture to a temperature of from 50° C. to 150° C.

7. 10. The method of claim 1, further comprising separating at least a portion of the one or more first depolymerization products in the first mixture from insoluble components in the first mixture, wherein the separation is conducted at a temperature from 50° C. to 150° C.

8. 10. The method of claim 1, wherein during the exposure of the first polyester composition to a first composition comprising one or more glycols and methanol under depolymerization conditions in the first reaction vessel, the weight ratio of the one or more glycols to the first polyester composition ranges from about 1:9 to about 9:

1.

9. 2. The method of claim 1, wherein the one or more glycols comprise ethylene glycol (EG), diethylene glycol (DEG), triethylene glycol (TEG), 1,4-cyclohexanedimethanol (CHDM), poly(ethylene glycol) (PEG), neopentyl glycol (NPG), propanediol (PDO), butanediol (BDO), 2-methyl-2,4-pentanediol (MP diol), poly(tetramethylene ether) glycol (PTMG), or combinations thereof.

10. The method of claim 1, wherein the weight ratio of the alcohol composition to the first polyester composition can range from about 2:1 to about 10:

1.

11. 2. The method of claim 1, wherein the first polyester composition comprises polyethylene terephthalate (PET), 1,4-cyclohexanedimethanol (CHDM) modified PET, isophthalic acid (IPA) modified PET, diethylene glycol (DEG) modified PET, neopentyl glycol (NPG) modified PET, propanediol (PDO) modified PET, butanediol (BDO) modified PET, hexanediol (HDO) modified PET, 2-methyl-2,4-pentanediol (MP diol) modified PET, isosorbide modified PET, poly(tetramethylene ether) glycol (PTMG) modified PET, poly(ethylene glycol) (PEG) modified PET, polycyclohexylene dimethylene terephthalate (PCT), cyclohexanedimethanol (CHDM)-containing copolyester, isosorbide-containing copolyester, or combinations thereof.

12. 2. The method of claim 1, wherein the first polyester composition comprises 0 mol% to 100 mol% CHDM, 0 mol% to 100 mol% DEG, 0 mol% to 100 mol% NPG, 0 mol% to 100 mol% PDO, 0 mol% to 100 mol% BDO, 0 mol% to 100 mol% HDO, 0 mol% to 100 mol% MP diol, 0 mol% to 100 mol% isosorbide, 0 mol% to 100 mol% PTMG, 0 mol% to 100 mol% PEG, and 0 mol% to 30 mol% isophthalic acid, the total of the diol equivalents in the one or more polyesters being about 100 mol% and the total of the diacid equivalents in the first polyester composition being about 100 mol%.

13. The method of claim 1, wherein the polyester composition has an intrinsic viscosity of from about 0.1 dL / g to about 1.2 dL / g, as determined according to ASTM D2857-70.

14. 10. The method of claim 1, wherein the first polyester composition comprises one or more contaminants, the one or more contaminants being present in the polyester composition in an amount of 0.01 wt. % to 50 wt. %, based on the weight of the one or more polyesters in the polyester composition, and the one or more contaminants comprises at least one member selected from the group consisting of polyesters other than polyethylene terephthalate, polyvinyl chloride (PVC), polyvinyl acetal, polyvinyl butyral (PVB), polyvinyl alcohol (PVOH), ethylene vinyl alcohol (EVOH), cotton, polyolefins, polyethylene, polypropylene, polystyrene, polycarbonate, spandex, natural fibers, cellulose esters, polyacrylates, polymethacrylates, polyamides, nylons, poly(lactic acid), polydimethylsiloxanes, polysilanes, calcium carbonate, titanium dioxide, inorganic fillers, dyes, pigments, color toners, colorants, plasticizers, adhesives, flame retardants, metals, aluminum, and iron.

15. 2. The method of claim 1, wherein the dialkyl terephthalate solids component comprises dimethyl terephthalate (DMT), the DMT being at least 90% pure.

16. The step of exposing the first polyester composition to a first composition comprising one or more glycols and methanol under depolymerization conditions in a first reactor further comprises exposing the first polyester composition to one or more glycolysis catalysts, the one or more glycolysis catalysts being selected from the group consisting of Li, 2 CO 3 , K 2 CO 3 , CaCO 3 , Na 2 CO 3 , Cs 2 CO 3 , ZrCO3, LiOH, NaOH, KOH, tetrabutylammonium hydroxide (TBAH), sodium methoxide (NaOMe), lithium methoxide (LiOMe), magnesium methoxide (Mg(OMe) 2 , potassium t-butoxide, ethylene glycol monosodium salt, ethylene glycol disodium salt, tetraisopropyl titanate (TIPT), butyltin tris-2-ethylhexanoate (FASCAT 4102), 1,8-diazabicyclo[5.4.0]undec-7-ene (DBU), zinc acetylacetonate hydrate (Zn(acac) 2 ), zinc acetate (Zn(OAc) 2 ), Manganese(II) acetate (Mn(OAc) 2 ), a member selected from the group consisting of hydrotalcite, zeolite and lithium chloride.

17. 15. The method of claim 14, further comprising the step of separating insoluble components in the first mixture prior to exposing at least a portion of the first mixture to the alcohol composition and the alcoholysis catalyst, the insoluble components including one or more foreign objects.

18. The method of claim 1 , wherein the alcohol composition comprises methanol.

19. The alcoholysis catalyst is present in an amount of 0.1 wt. % to 20 wt. % based on the weight of the first polyester composition, and the alcoholysis catalyst is 2 CO 3 , Na 2 CO 3 , Li 2 CO 3 , Cs 2 CO 3 ;KOH, LiOH, NaOH; NaOMe, Mg(OMe) 2 , KOMe, KOt-Bu, ethylene glycol monosodium salt, ethylene glycol disodium salt, or combinations thereof.

20. 10. The method of claim 1 , wherein the one or more depolymerization products comprise monomers, oligomers, or combinations thereof, and the oligomers exhibit a degree of polymerization of 2 to 10.