Method for preparing a laminated article comprising a silicone pressure sensitive adhesive bonded to a silicone rubber

JP2024541939APending Publication Date: 2024-11-13DOW SILICONES CORP
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
JP2024525023
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2022-04-28
Filing Date
2022-10-25
Publication Date
2024-11-13

AI Technical Summary

Technical Problem

Current silicone pressure sensitive adhesives exhibit relatively low adhesion strength to silicone rubber substrates, which is inadequate for applications such as electronics and automotive uses.

Method used

A method involving specific ratios and molecular weights of bis-hydroxyl terminated polydiorganosiloxanes and hydroxyl-functional polyorganosilicate resins, combined with a condensation reaction catalyst and solvent, followed by curing and coating, to form a silicone pressure sensitive adhesive with enhanced adhesion to silicone rubber.

Benefits of technology

The method produces a silicone pressure sensitive adhesive with peel adhesion strengths greater than 1,000 gf/in, effectively adhering to silicone rubber articles, suitable for various applications including electronics and automotive uses.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024541939000010
    Figure 2024541939000010
  • Figure 2024541939000011
    Figure 2024541939000011
  • Figure 2024541939000001
    Figure 2024541939000001
Patent Text Reader

Abstract

The laminate article includes a silicone pressure sensitive adhesive adhered to a silicone rubber article.A method of making a laminate article is provided.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] (CROSS REFERENCE TO RELATED APPLICATIONS) This application claims the benefit under 35 U.S.C. §119(e) of U.S. Provisional Patent Application No. 63 / 335734, filed April 28, 2022, and U.S. Provisional Patent Application No. 63 / 274131, filed November 1, 2021. U.S. Provisional Patent Application Nos. 63 / 335734 and 63 / 274131 are incorporated herein by reference.

[0002] FIELD OF THEINVENTION The present invention relates to a method for preparing a silicone pressure sensitive adhesive composition that can be cured to form a silicone pressure sensitive adhesive having good adhesion to silicone rubber. More specifically, the present invention relates to a method for preparing a peroxide curable silicone pressure sensitive adhesive composition that can be cured to form a silicone pressure sensitive adhesive. A laminate article comprises a silicone pressure sensitive adhesive adhered to an article comprising silicone rubber. [Background technology]

[0003] Introduction Currently available silicone pressure sensitive adhesives can suffer from the problem of having relatively poor adhesion strength to silicone rubber substrates, which may not meet the needs of applications in which they are used to adhere to silicone rubber, such as electronics, automotive, and masking tape applications. Summary of the Invention

[0004] A method of making a laminate article is provided, the method comprising: (a) under conditions for carrying out a condensation reaction; (P) a bis-hydroxyl terminated polydiorganosiloxane having a weight average molecular weight of from 10,000 g / mol to less than 200,000 g / mol as measured by GPC; (R) a hydroxyl-functional polyorganosilicate resin having a weight average molecular weight of 15,000 g / mol to 30,000 g / mol as measured by GPC; (wherein the starting materials (P) and (R) are present in a weight ratio (R) / (P) of from 0.65 / 1 to less than 3.0 / 1), (S) combining starting materials with a solvent to form a reaction mixture; (b) adding to the reaction mixture (C) a condensation reaction catalyst to form a catalyzed reaction mixture; (c) mixing the catalyzed reaction mixture at a temperature between 20° C. and 150° C. and removing water; (d)(R') adding additional polyorganosiloxane resin to form a silicone pressure sensitive adhesive composition; (e) coating a silicone pressure sensitive adhesive composition onto the surface of the backing; (f) drying the silicone pressure sensitive adhesive composition; and (g) curing the silicone pressure sensitive adhesive composition to form a silicone pressure sensitive adhesive layer having a surface adhered to the surface of the backing, the silicone pressure sensitive adhesive layer further including an opposing surface opposite the surface of the backing; (h) adhering an opposing surface of the silicone pressure sensitive adhesive to a surface of the silicone rubber article; A laminate article comprising a silicone pressure sensitive adhesive that adheres to a silicone rubber article can be prepared by this method. [Brief description of the drawings]

[0005] [Figure 1] FIG. 1 is a partial cross-sectional view of laminate article 100. [Diagram 2] FIG. 2 is a partial cross-sectional view of laminate article 200.

[0006] Reference number 100 Partial cross section of laminated article 101 Backing 101b Surface of backing material 101 102 Silicone pressure sensitive adhesive 102a Surface of silicone pressure sensitive adhesive 102 102b: the opposite surface of the silicone pressure sensitive adhesive 102 103 Silicone rubber articles 103a Surface of silicone rubber article 103 200 Partial cross section of laminated article 201 Backing material containing silicone rubber 201b Surface of backing material 201 202 Silicone pressure sensitive adhesives 202a Surface of silicone pressure sensitive adhesive 202 202b: the opposite surface of the silicone pressure sensitive adhesive 202 DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0007] The method of making a laminate article comprises: (1) under conditions for carrying out a condensation reaction, (P) a starting material (P), which is a bis-hydroxyl terminated polydiorganosiloxane having a weight average molecular weight of from 10,000 g / mol to less than 200,000 g / mol as measured by GPC, and which is present in an amount of greater than 20.5 weight percent based on the combined weight of starting materials (P) and (R); (R) a hydroxyl-functional polyorganosiloxane resin having a weight average molecular weight of 15,000 g / mol to 30,000 g / mol as measured by GPC, the starting material (R) being present in an amount of less than 79.5% by weight, based on the combined weight of the starting materials (P) and (R); (S) a solvent, and optionally, (N) a neutralizing agent, wherein the starting materials (P) and (R) are present in a weight ratio (R) / (P) of from 0.65 / 1 to less than 3.0 / 1; combining starting materials comprising: (2) adding to the reaction mixture (C) a condensation reaction catalyst to form a catalyzed reaction mixture; (3) mixing the catalyzed reaction mixture at a temperature between 20° C. and 150° C. and removing water to form a reaction product comprising a condensation reaction product of (P) and (R); Optionally, (4) recovering the condensation reaction product of (P) and (R); and (5) The condensation reaction product is mixed with (R') an additional polyorganosilicate resin having a weight average molecular weight of 5,500 g / mol to 30,000 g / mol as measured by GPC, and (R') is less than 2.27 / 1 to 3.88 / 1. tot ) / (P) ratio (where R tot represents the sum of the amount of (R') and the amount of (R) from step (1), where (R tot (R) / (P)>(R) / (P); optionally, (6) adding up to 4 weight percent, based on the combined weight of (R), (R'), and (P), of (X) a peroxide crosslinker to form a silicone pressure sensitive adhesive composition; Optionally, (7) treating the surface of the backing; and (8) coating a silicone pressure sensitive adhesive composition onto a surface of a backing; (9) drying the silicone pressure sensitive adhesive composition; and (10) curing the silicone pressure sensitive adhesive composition to form a silicone pressure sensitive adhesive layer having a surface adhered to a surface of a backing, the silicone pressure sensitive adhesive layer further including an opposing surface opposite the surface of the backing; Optionally, (11) treating the surface of the silicone rubber article; and (12) adhering an opposing surface of the silicone pressure sensitive adhesive to a surface of a silicone rubber article; Includes.

[0008] Step (1) of the above process may be carried out by any convenient means, such as by mixing the starting materials, including (P), (R), (S), and optionally (N), as introduced above and described in detail below, in a batch reactor, optionally equipped with a stirrer and jacket. The condensation reaction may be carried out at a temperature of at least 20° C., alternatively at least room temperature, while the condensation reaction may be carried out at a temperature of up to 145° C., alternatively up to 150° C. Alternatively, the temperature may be from 20° C. to 150° C., alternatively from 20° C. to 145° C., alternatively from room temperature to the reflux temperature of the starting material (S) solvent. The reaction time will depend on various factors, including the choice of starting materials and the temperature, but the condensation reaction in step (1) may be carried out for, for example, 0.5 hours to 20 hours, alternatively from 1 hour to 10 hours. The condensation reaction may be carried out, for example, as described in U.S. Pat. No. 5,916,981 to Cifuentes et al., by changing the appropriate starting materials to those described below.

[0009] (P) Bis-hydroxyl terminated polydiorganosiloxane The starting material (P) is the bis-hydroxyl terminated polydiorganosiloxane (polymer) used in step (1). This polymer has the following formula:

[0010] [ka] (In the formula, each R 1are independently selected alkyl groups of 1 to 6 carbon atoms, and the subscript a represents the average number of difunctional siloxane units per molecule, where 250≦a≦3000, alternatively 270≦a≦2000. Alternatively, the subscript a may be at least 250, alternatively at least 270, alternatively at least 300, alternatively at least 350, alternatively at least 400, alternatively at least 450, alternatively at least 500, while the subscript a may be up to 3,000, alternatively up to 2,500, alternatively up to 2,100, alternatively up to 2,000, alternatively up to 1,900, alternatively up to 1,800. Alternatively, subscript a may have a value sufficient to impart to the polymer a Mw of at least 20,000 g / mol, alternatively at least 40,000 g / mol, while subscript a may be sufficient to impart to the polymer a Mw of less than 200,000 g / mol, alternatively at most 150,000 g / mol, alternatively at most 135,000 g / mol. 1 Examples of alkyl groups include methyl, ethyl, propyl (including n-propyl and isopropyl), butyl (including n-butyl, tert-butyl, sec-butyl, and isobutyl), pentyl (including n-pentyl, cyclopentyl, and branched isomers having 5 carbon atoms), and hexyl (including n-hexyl, cyclohexyl, and branched isomers having 6 carbon atoms). 1 may be methyl or ethyl, or may be methyl.

[0011] Suitable polymers for starting material (A) are known in the art and commercially available from a variety of sources, such as Gelest Inc. (Morrisville, Pennsylvania, USA) and DSC. Examples of suitable polymers include bis-hydroxyl terminated polydimethylsiloxanes having a Mw of 20,000 g / mol to 150,000 g / mol, alternatively 40,000 g / mol to 135,000 g / mol, where Mw can be measured by GPC.

[0012] (R) Polyorganosilicate resin The starting material (R) is the hydroxyl-functional polyorganosilicate resin (resin) used in step (1). The resin has the formula R 1 3SiO 1 / 2 and a monofunctional unit of formula SiO 4 / 2 wherein R 1 is as above). Alternatively, the monofunctional unit may be of the formula (MeSiO 1 / 2 The polyorganosilicate resin is soluble in solvents such as those described below as starting materials (S), exemplified by aliphatic and / or aromatic hydrocarbons such as benzene, toluene, xylene, ethylbenzene, heptane, and combinations thereof.

[0013] When prepared, the resin contains the monofunctional and tetrafunctional units described above, the resin further contains units having silicon-bonded hydroxyl groups and has the formula Si(OSiR 1 3)4 (in the formula, R 1 The polyorganosilicate resin may include a neopentamer of the formula (I) (wherein m is as defined above), for example, the neopentamer may be tetrakis(trimethylsiloxy)silane. The concentration of silanol groups present in the resin may be determined using FTIR spectroscopy according to ASTM standard E-168-16. The molar ratio of mono- to tetrafunctional units, excluding mono- and tetrafunctional units from the neopentamer, is expressed as {M(resin)} / {Q(resin)}, or M:Q. The M:Q ratio represents the molar ratio of the total number of triorganosiloxy groups (monofunctional units) in the resinous portion of the polyorganosilicate resin to the total number of silicate groups (Q units) in the resinous portion. The M:Q ratio may be from 0.5:1 to 1.5:1.

[0014] The Mn of the polyorganosilicate resin is determined by the R 1The Mn of the polyorganosilicate resins depends on various factors including the type of alkyl group represented by the formula: Mn=Mw / Mw / Mw / Mw / Mw. The Mn of the polyorganosilicate resins refers to the number average molecular weight measured using GPC when the peak representing the neopentamer is excluded from the measurement. The Mn of the polyorganosilicate resins may be greater than 3,000 g / mol, alternatively greater than 3,000 g / mol to 8,000 g / mol. Alternatively, the Mn of the polyorganosilicate resins may be 3,500 g / mol to 8,000 g / mol. The Mw of the polyorganosilicate resins refers to the weight average molecular weight measured using GPC. The Mw of the polyorganosilicate resins may be 15,000 g / mol to 30,000 g / mol, alternatively 20,000 g / mol to 30,000 g / mol, alternatively 21,000 g / mol to 29,500 g / mol.

[0015] The polyorganosilicate resins can be prepared by any suitable method, such as cohydrolysis of the corresponding silanes or by silica hydrosol capping methods. The polyorganosilicate resins can be prepared by silica hydrosol capping methods, such as those disclosed in U.S. Patent No. 2,676,182 to Daudt et al., U.S. Patent No. 4,611,042 to Rivers-Farrell et al., and U.S. Patent No. 4,774,310 to Butler et al. The method of Daudt et al. described above involves reacting a silica hydrosol with a hydrolyzable triorganosilane, such as trimethylchlorosilane, a siloxane, such as hexamethyldisiloxane, or a mixture thereof, under acidic conditions, and recovering a copolymer having monofunctional units and Q units. The resulting copolymer generally contains 2 to 5 weight percent hydroxyl groups.

[0016] The intermediates used to prepare the polyorganosilicate resins can be triorganosilanes and silanes or alkali metal silicates containing four hydrolyzable substituents. The triorganosilanes are represented by the formula R 1 3SiX 1 (In the formula, R 1 is as above, and X 1represents a hydrolyzable substituent such as hydroxyl. A silane having four hydrolyzable substituents can have the formula SiX 2 4, wherein each X 2 is halogen, alkoxy, or hydroxyl. Suitable alkali metal silicates include sodium silicate.

[0017] The resin selected for the starting material (R) has the unit formula (R 1 3SiO 1 / 2 ) b (SiO 4 / 2 ) c (HO 1 / 2 ) d (In the formula, each R 1 are independently selected alkyl groups of 1 to 6 carbon atoms as described above, subscripts b and c represent the mole fractions of mono- and tetrafunctional units, respectively, with subscripts b and c having values ​​such that 0.4≦b≦0.5, 0.5≦c≦0.6, and the amount (b+c)=1, and subscript d represents the amount of hydroxyl groups in the resin, with subscript d having a value sufficient to provide the resin with a hydroxyl content of 2% to 5% by weight. The resin may have a Mw of 15,000 g / mol to 30,000 g / mol as measured by GPC. Alternatively, the resin may have a Mw of from 20,000 g / mol to 30,000 g / mol, alternatively from 21,000 g / mol to 30,000 g / mol, alternatively from 21,000 g / mol to 29,500 g / mol, alternatively from 21,000 g / mol to 29,100 g / mol. Suitable resins are known in the art and commercially available, for example, from DSC.

[0018] The resin (R) and polymer (P) are present in a weight ratio (R) / (P) of 0.65 / 1 to less than 3.0 / 1. Alternatively, (R) / (P) may be 0.65 / 1 to 1.82 / 1, alternatively 1 / 1 to 1.82 / 1, alternatively (R) / (P) may be 1 / 1 to 1.46 / 1. Alternatively, (R) / (P) may be 0.65 / 1 to less than 2.27 / 1.

[0019] (S) Solvent The starting material (S) is a solvent. To facilitate the introduction of certain starting materials, such as (R) resin, a solvent may be added during step (1) and optionally subsequent steps, such as step (2). Solvents that can be used herein are those that aid in fluidizing the starting materials but do not essentially react with the starting materials. The solvent may be selected based on the solubility of the starting materials and the volatility of the solvent. Solubility refers to the solvent being sufficient to dissolve and / or disperse the starting materials. Volatility refers to the vapor pressure of the solvent. Without wishing to be bound by theory, it is believed that if the solvent is too volatile (has too high a vapor pressure), the solvent may evaporate too quickly from the reaction mixture during step (3). However, if the solvent is not volatile enough (has too low a vapor pressure), too much solvent may remain in the condensation reaction product prepared in step (3) and / or water produced as a by-product of the condensation reaction may not be sufficiently removed during step (3) and, if present, step (4).

[0020] Suitable solvents include polyorganosiloxanes having suitable vapor pressures, such as hexamethyldisiloxane, octamethyltrisiloxane, hexamethylcyclotrisiloxane, and other low molecular weight polyorganosiloxanes, such as DOWSIL™ 200 Fluids and DOWSIL™ OS FLUIDS, 0.5-1.5 cSt, commercially available from DSC.

[0021] Alternatively, the solvent may comprise an organic solvent. The organic solvent may be a ketone such as acetone, methyl ethyl ketone, or methyl isobutyl ketone; an aromatic hydrocarbon such as benzene, toluene, ethylbenzene, or xylene; an aliphatic hydrocarbon such as heptane, hexane, or octane; a glycol ether such as propylene glycol methyl ether, dipropylene glycol methyl ether, propylene glycol n-butyl ether, propylene glycol n-propyl ether, or ethylene glycol n-butyl ether, a halogenated hydrocarbon, for example, dichloromethane, 1,1,1-trichloroethane, or methylene chloride; chloroform; dimethyl sulfoxide; dimethylformamide, acetonitrile; tetrahydrofuran, white spirit; mineral spirit, naphtha, n-methylpyrrolidone; or a combination thereof.

[0022] The amount of solvent depends on various factors, such as the type of solvent selected and the amount and type of other starting materials selected for use in the process. However, the amount of solvent may range from 1% to 99%, alternatively 2% to 90%, based on the weight of all starting materials in step (1). All or a portion of the solvent may be optionally removed during and / or after step (3). For example, water may be formed as a by-product of the condensation reaction in steps (2) and (3). To drive the reaction forward, some or all of the water may be removed, for example, by azeotropic distillation with the solvent.

[0023] (N) Neutralizer The starting material (N), the neutralizing agent, is optional. The neutralizing agent may include silyl phosphate. Without being bound by theory, it is believed that the neutralizing agent may be added to scavenge impurities in the above-mentioned (R) resin and / or (P) polymer before the condensation reaction. The neutralizing agent may be, for example, silyl phosphate. Silyl phosphates, such as bis(trimethylsilyl) hydrogen phosphate, are commercially available from DSC.

[0024] The amount of neutralizing agent will depend on a variety of factors, including the type of (P) polymer and (R) resin selected, but the amount of neutralizing agent may be from 0.005% to 0.02% based on the combined weight of the starting materials (P), (R), (C), and (N).

[0025] (C) Condensation reaction catalyst The starting material (C) added in step (2) is a condensation reaction catalyst capable of catalyzing the condensation reaction of the hydroxyl groups of the above-mentioned (P) polymer and (R) resin. The condensation reaction catalyst is not particularly limited and may include an acid or a base condensation reaction catalyst. For example, suitable base catalysts include metal hydroxides such as lithium hydroxide, sodium hydroxide, potassium hydroxide, and calcium hydroxide, carbonates such as sodium carbonate and potassium carbonate, bicarbonates such as sodium bicarbonate and potassium bicarbonate, metal alkoxides such as sodium methoxide and potassium butoxide, organometallic compounds such as butyl lithium, potassium silanolate, ammonia gas, aqueous ammonia, nitrogen compounds such as methylamine, trimethylamine, and triethylamine, and the like. Alternatively, the condensation reaction catalyst may be an acid, for example, organic acids such as acetic acid, benzoic acid, octanoic acid, and citric acid, and mineral acids such as hydrochloric acid, sulfuric acid, and phosphoric acid are suitable. Alternatively, the condensation reaction catalyst may be an acid catalyst, for example, an organic acid such as benzoic acid.

[0026] Suitable condensation reaction solvents are commercially available from a variety of sources, including Sigma Aldrich, Inc. (St. Louis, Missouri, USA) and Acros. The amount of catalyst will depend on a variety of factors, including the type of catalyst selected and the temperature of step (1), but the amount of catalyst may be 0.1% to 0.5% based on the combined weight of the starting materials (P), (R), (C), and (N).

[0027] Step (4) in the above method is optional. After the condensation reaction product of the (P) polymer and the (R) resin is formed, the condensation reaction product may further include unreacted starting materials, solvent, and water as a by-product. In step (4), the condensation reaction product may be recovered, for example, by removing the solvent, water, and unreacted starting materials, for example, by distillation and / or stripping, optionally with heating and / or under reduced pressure. The condensation reaction product may also be called a bodied resin.

[0028] In step (5) of the above method, (R') additional polyorganosilicate resin is combined with the condensation reaction product (i.e., thickening resin). Step (5) may be performed after step (3). Alternatively, step (5) may be performed after step (4), if present. Step (5) may be performed by any convenient means, such as mixing under ambient conditions. For example, (R') additional polyorganosilicate resin may be (optionally) dissolved in a solvent, which may be a solvent as described above for starting material (S). The additional polyorganosilicate resin and the condensation reaction product may then be mixed at room temperature or at an elevated temperature. Starting material (R') additional polyorganosilicate resin may be added to the same vessel used for steps (1)-(3) and, if present, (4), as described above. In step (5), a resin / polymer blend is produced.

[0029] (R') Additional polyorganosilicate resin The additional polyorganosilicate resin added in step (5) can be prepared by the method described above for the starting material (R) by varying the appropriate starting materials so that the Mw of the (R') additional polyorganosilicate resin can be from 5,500 g / mol to 30,000 g / mol. The additional polyorganosilicate resin may be selected from the group consisting of (R'-1) capped resin, (R'-2) uncapped resin, and (R'-3) a combination of both (R'-1) capped resin and (R'-2) uncapped resin. Alternatively, the (R') additional polyorganosilicate resin may be (R'-2) uncapped resin, or (R'-3) a combination of both (R'-1) capped resin and (R'-2) uncapped resin. Alternatively, the (R') additional resin may be (R'-2) uncapped resin. The additional polyorganosilicate resin may be of the formula R 1 3SiO 1 / 2 and a monofunctional unit of formula SiO 4 / 2 wherein R 1 is as above). Alternatively, the monofunctional unit may be of the formula R M 3SiO 1 / 2 (In the formula, each R M are independently selected alkyl groups (e.g., R 1 R may be a monovalent hydrocarbon group such as those described above for R, an alkenyl group (e.g., vinyl, allyl, or hexenyl), or an aryl group (e.g., phenyl, tolyl, or xylyl). M At least 1 / 3, or at least 2 / 3, of the groups are alkyl groups (e.g., methyl groups). Alternatively, the monofunctional units are (MeSiO 1 / 2 ) and (Me2PhSiO 1 / 2 )

[0030] When prepared, the additional polyorganosilicate resin contains the monofunctional units and Q units described above, and units having silicon-bonded hydroxyl groups. The additional polyorganosilicate resin has the formula Si(OSiR M 3)4 (In the formula, R M is as defined above), for example, the neopentamer can be tetrakis(trimethylsiloxy)silane. 29 Si NMR spectroscopy can be used to measure the hydroxyl content and molar ratio of monofunctional and Q units, expressed as {M(resin)} / {Q(resin)}, excluding the monofunctional and Q units from the neopentamer. The M:Q ratio represents the molar ratio of the total number of triorganosiloxy groups (monofunctional units) in the resinous portion of the polyorganosilicate resin to the total number of silicate groups (Q units) in the resinous portion. The M:Q ratio may be from 0.5:1 to 1.5:1.

[0031] The Mn of the additional polyorganosilicate resin is determined by the R M The Mn of the additional polyorganosilicate resin refers to the number average molecular weight measured using GPC when the peak representing the neopentamer is excluded from the measurement. The Mw of the additional polyorganosilicate resin refers to the weight average molecular weight measured using GPC and can be from 5,500 g / mol to 30,000 g / mol, alternatively from 15,000 g / mol to 30,000 g / mol, alternatively from 21,000 g / mol to 29,500 g / mol. The additional polyorganosilicate resin can have a silanol content of from 0.5% to 5% by weight, alternatively from 3% to 5% by weight.

[0032] U.S. Patent No. 8,580,073, column 3, line 5 to column 4, line 31, and U.S. Patent Application Publication No. 2016 / 0376482, paragraphs

[0023] to

[0026] , are incorporated herein by reference to disclose MQ resins, which are additional polyorganosilicate resins suitable for use herein. The additional polyorganosilicate resins can be prepared by any suitable method, such as cohydrolysis of the corresponding silanes or a silica hydrosol capping method. The additional polyorganosilicate resins can be prepared by a silica hydrosol capping method, such as those disclosed in U.S. Patent No. 2,676,182 to Daudt et al., U.S. Patent No. 4,611,042 to Rivers-Farrell et al., and U.S. Patent No. 4,774,310 to Butler et al. The method of Daudt et al., supra, involves reacting a silica hydrosol with a hydrolyzable triorganosilane, such as trimethylchlorosilane, a siloxane, such as hexamethyldisiloxane, or a mixture thereof, under acidic conditions, and recovering a copolymer having monofunctional units and Q units. The resulting copolymer generally contains 2-5 weight percent hydroxyl groups.

[0033] The intermediates used to prepare the additional polyorganosilicate resins may be triorganosilanes and silanes or alkali metal silicates containing four hydrolyzable substituents. The triorganosilanes are represented by the formula R M3 Six 1 (In the formula, R M is as above, and X 1 may have hydrolyzable substituents such as halogen, alkoxy, acyloxy, hydroxyl, oximo, or ketoximo, alternatively halogen, alkoxy, or hydroxyl. Silanes having four hydrolyzable substituents have the formula SiX 2 4, wherein each X 2 is halogen, alkoxy, or hydroxyl. Suitable alkali metal silicates include sodium silicate.

[0034] The additional polyorganosilicate resin prepared as described above is an uncapped resin and typically contains silicon-bonded hydroxyl (silanol) groups. The additional polyorganosilicate resin may contain 3% to 10% by weight, alternatively 3% to 5% by weight, of silicon-bonded hydroxyl groups as measured by NMR spectroscopy, as described above. In certain applications, it may be desirable for the amount of silicon-bonded hydroxyl groups to be 2% or less, alternatively less than 0.7% by weight, alternatively 0.5% by weight, alternatively less than 1% by weight, alternatively 0.5% to 5% by weight. The silicon-bonded hydroxyl groups formed during the preparation of the additional polyorganosilicate resin can be converted to trihydrocarbonsiloxane groups or different hydrolyzable groups by reacting the silicone resin with a silane, disiloxane, or disilazane containing the appropriate end group, in a process called capping. The silane containing the hydrolyzable group may be added in molar excess over the amount required to react with the silicon-bonded hydroxyl groups in the polyorganosilicate resin.

[0035] When the additional polyorganosilicate resin is an (R'-1)-capped resin, the capped resin may contain 2% or less by weight of silanol groups, alternatively 0.7% or less by weight, alternatively 0.5% or less by weight, alternatively 0.5% to 0.8% by weight. The concentration of silanol groups present in the polyorganosiloxane can be measured using NMR spectroscopy as described above.

[0036] Thus, the additional polyorganosilicate resin (R') has the unit formula (R 1 3SiO 1 / 2 ) b’ (SiO 4 / 2 ) c’ (HO 1 / 2 ) d’ (In the formula, each R 1are independently selected alkyl groups of 1 to 6 carbon atoms, subscripts b' and c' represent the mole fractions of monofunctional and tetrafunctional units, respectively, with subscripts b' and c' having values ​​such that 0.4≦b≦0.5, 0.5≦c≦0.6, and the amount (b'+c')=1, and subscript d' represents the amount of hydroxyl groups in the resin, with subscript d' having a value sufficient to provide the resin with a silanol content and Mw as described above. Alternatively, when (R') additional polyorganosilicate resin includes or is (R2') uncapped resin, the Mw may be from 15,000 g / mol to 30,000 g / mol, and the silanol content may be from 3 wt% to 5 wt%.

[0037] The amount of additional polyorganosilicate resin (R') added in step (5) is in a weight ratio (R') of from 2.27 / 1 to less than 3.88 / 1, alternatively from 2.27 / 1 to 3.0 / 1, alternatively from 2.9 / 1 to 3.0 / 1. tot ) / (P). In this ratio, (R tot ) means the sum of the amount of the above (R) resin before the condensation reaction in step (1) and the amount of the (R') additional polyorganosilicate resin added in step (5). The amount of the (R') additional polyorganosilicate resin is tot (R) / (P)>(R) / (P), where (P) represents the amount of the polymer prior to the condensation reaction in step (1). Without wishing to be bound by theory, it is believed that (R) is less than 2.27 / 1. tot ) / (P) may result in a silicone pressure sensitive adhesive with insufficient adhesion to silicone rubber, whereas an (R tot It is believed that a mixture of (A) / (P) may result in a silicone pressure sensitive adhesive that is glassy and does not even have sufficient adhesion to silicone rubber.

[0038] The resin / polymer blend produced in step (5) can be used to form a silicone pressure sensitive adhesive composition. Step (6) in the above method is optional. If step (6) is present, then (X) a peroxide crosslinker is added in step (6) to form a silicone pressure sensitive adhesive composition, which can cure faster than in the absence of the peroxide crosslinker, as long as other conditions, such as temperature, are kept constant.

[0039] (X) Peroxide crosslinking agent The starting material (X) added when step (6) is present is a peroxide crosslinker. The peroxide crosslinking agent may be an organic peroxide or hydroperoxide, such as benzoyl peroxide; 4-monochlorobenzoyl peroxide; t-butyl peroctoate; t-butyl peroxybenzoate, tert-butyl peroxybenzoate, tert-butylcumyl peroxide, tert-butyl oxide 2,5-dimethyl-2,5-di-tert-butylperoxyhexane; 2,4-dichlorobenzoyl peroxide; di-tertbutylperoxy-diisopropylbenzene; 1,1-bis(tert-butylperoxy)-3,3,5-trimethylcyclohexane; 2,5-di-tert-butylperoxyhexane-3,2,5-dimethyl-2,5-bis(tert-butylperoxy)hexane; cumyl-tert-butyl peroxide; dicumyl peroxide; di-t-butyl peroxide; t-butyl hydroperoxide; cumene hydroperoxide; di-t-amyl peroxide, and combinations of two or more thereof. Furthermore, the diperoxide crosslinking agent may be used alone or in combination with other diperoxide crosslinking agents. Such diperoxide crosslinking agents include, but are not limited to, 1,4-bis-(t-butylperoxycarbo)cyclohexane; 1,2-di(t-butylperoxy)cyclohexane, and 2,5-di(t-butylperoxy)-3-hexyne. Peroxide crosslinking agents suitable for use as starting material (X) are known in the art and are commercially available from various sources, such as Sigma-Aldrich, Inc. (St. Louis, Missouri, USA).

[0040] Starting material (X) may include one peroxide crosslinking agent or may include a combination of two or more peroxide crosslinking agents. The amount of starting material (X) added in step (5) will depend on various factors, including the type and amount of peroxide crosslinking agent selected, and the selection of the (P) polymer, (R) resin, and (R') additional polyorganosilicate resin, but the amount of peroxide crosslinking agent, if present, may be from 0.1% to 4% by weight, alternatively from 1% to 4% by weight, alternatively from 2% to 3% by weight, based on the combined weight of starting materials (P), (R), (R'), (C), and (S).

[0041] Step (7) in the method described herein is optional. However, step (7) may be included in the method to improve adhesion of the silicone pressure sensitive adhesive to the backing. Thus, the method of forming an adhesive article may optionally further comprise (7) treating the surface of the backing before applying the silicone pressure sensitive adhesive composition. Treating the surface may be carried out by any convenient means, such as applying a primer or subjecting the surface to a corona discharge treatment, etching, or plasma treatment before applying the silicone pressure sensitive adhesive composition to the surface. Alternatively, treating the surface may comprise applying a primer to the surface of the backing.

[0042] The step (8) of coating the silicone pressure-sensitive adhesive composition onto the surface of the backing may be carried out by any convenient means, for example, the silicone pressure-sensitive adhesive composition may be applied by a gravure coater, a comma coater, an offset coater, an offset gravure coater, a roller coater, a reverse roller coater, an air knife coater, a slot die, or a curtain coater.

[0043] In the methods described herein, steps (8)-(10) may be carried out via wet casting or dry casting. In wet casting, the silicone pressure sensitive adhesive layer may be durably adhered to a backing, such as a polymeric film and / or foam, as described below.

[0044] The backing may be any material that can withstand the curing conditions used in step (10) to cure the silicone pressure sensitive adhesive composition to form a silicone pressure sensitive adhesive on the surface of the backing. For example, any backing that can withstand heat treatment at a temperature of 120°C or higher, or even 150°C or higher, is suitable. Examples of suitable materials for such backings include polymer films and / or foams, which may be composed of polyimide (PI), polyetheretherketone (PEEK), polyethylenenaphthalate (PEN), liquid crystal polyarylate, polyamideimide (PAI), polyethersulfide (PES), polyethyleneterephthalate, polyester (PET), polycarbonate (PC), polymethylmethacrylate (PMMA), thermoplastic polyurethane (TPU), thermoplastic elastomer (TPE), polyethylene (PE), or polypropylene (PP). Alternatively, the backing may be glass. Alternatively, the backing may be a release liner, for example when the silicone pressure sensitive adhesive is used in a dry casting process. The thickness of the substrate is not critical. However, the thickness may be from 5 μm to 300 μm, alternatively from 10 μm to 200 μm. Alternatively, the backing used in step (8) may be selected from the group consisting of PE, PU, ​​TPE, and TPU.

[0045] Step (9) of the method involves drying the silicone pressure sensitive adhesive composition. Drying may be accomplished by any convenient means, such as heating at a temperature and for a time sufficient to evaporate all or a portion of the solvent, but insufficient to completely cure the silicone pressure sensitive adhesive composition. For example, drying may be accomplished by heating at a temperature of from 50° C. to 120° C., alternatively from 70° C. to 100° C., alternatively from 70° C. to 80° C., for a time sufficient to remove all or a portion of the solvent (e.g., from 30 seconds to 1 hour, alternatively from 1 minute to 5 minutes).

[0046] After drying, the method further includes the step (10) of curing the silicone pressure sensitive adhesive composition to form a laminate article comprising a silicone pressure sensitive adhesive layer having a surface adhered to a surface of a backing, the silicone pressure sensitive adhesive layer further comprising an opposing surface opposite the surface of the backing.

[0047] Curing of the pressure sensitive adhesive composition in step (10) may be carried out by heating at a temperature of 80°C to 200°C, alternatively 90°C to 210°C, alternatively 150°C to 205°C, alternatively 180°C to 205°C for a time sufficient to cure the pressure sensitive adhesive composition (e.g., 30 seconds to 1 hour, alternatively 1 to 5 minutes). If a faster cure rate or a lower process oven temperature is required, the amount of (X) peroxide crosslinker may be increased. This results in a silicone pressure sensitive adhesive on the surface of the backing. Curing may be carried out by placing the coated backing in an oven. The amount of silicone pressure sensitive adhesive composition coated on the backing will depend on the particular application, but the amount may be sufficient to provide a silicone pressure sensitive adhesive having a thickness of 5 micrometers to 100 micrometers after curing.

[0048] The methods described herein may optionally further include additional steps after step (10), such as applying a removable release liner to the opposing surface of the silicone pressure-sensitive adhesive layer opposite the backing to protect the silicone pressure-sensitive adhesive prior to use (e.g., when the backing is a polymeric film and / or foam, or glass). The release liner can be applied before, during, or after curing the silicone pressure-sensitive adhesive composition, or after curing.

[0049] The silicone pressure sensitive adhesive prepared in step (10) adheres to a silicone rubber article. Without being bound by theory, it is believed that the silicone pressure sensitive adhesive prepared in step (10) may have an adhesion to silicone rubber of greater than 1,000 gf / in, alternatively greater than 1,200 gf / in, alternatively greater than 1,300 gf / in, or alternatively greater than 1,500 gf / in, when tested according to the Peel Adhesion Test Method described in the Examples below, while the adhesion may be up to 2,500 gf / in, alternatively up to 2,200 gf / in, alternatively up to 2,000 gf / in, or alternatively up to 1,800 gf / in.

[0050] Although treatment of the silicone rubber article is not required for this adhesion, the method may optionally further comprise a step (11) of treating the surface of the silicone rubber article, which may promote and / or improve adhesion of the silicone pressure sensitive adhesive to the surface of the silicone rubber article. Treating the surface of the silicone rubber article may be by any convenient means, such as, for example, cleaning the silicone rubber surface with an alcohol, such as isopropanol, or any of the surface treatments described above in step (7).

[0051] The silicone rubber article is not particularly limited. The silicone rubber article may have a durometer Shore A of 30 to 75, alternatively 30 to 50, as measured by ASTM D2240. Liquid silicone rubber (LSR) and high viscosity rubber (HCR) may be used in the silicone rubber article. Alternatively, the silicone rubber article may be LSR. LSR is known in the art and can be made by known methods, such as those disclosed in U.S. Patent No. 5,777,002 to Conway et al. or U.S. Patent No. 8,198,357 to Jeram et al. Alternatively, the silicone rubber article may be selected based on the desired end use of the laminate article prepared herein.

[0052] For example, optical silicone elastomers (optical LSRs) are known in the art and are described, for example, in U.S. Patent No. 8,859,693 to Hasegawa et al. and U.S. Patent No. 8,853,332 to Akitomo et al. Optical LSRs are commercially available. For example, optical LSRs include moldable optical silicone elastomers SILASTIC™ MS-1001, MS-1002, MS-1003, MS-4001, MS-4002, and MS-4007, and SYLGARD™ 182, 184, and 186 are other optical silicone elastomers, all of which are commercially available from DSC.

[0053] Alternatively, LSRs such as XIAMETER™ RBL-2004-30, XIAMETER™ RBL-2004-50 SILASTIC™ 9202-50 LSR, SILASTIC™ LCF 3760, and SILASTIC™ LCF 3600, or Varox™ DBPH-50 manufactured by TDCC, or SILASTIC™ RBC 7600-50, XIAMETER™ RBB 2000-35, XIAMETER™ RBB 2001-65, XIAMETER™ RBB-2030-40EN, XIAMETER™ RBB-6660-60EN, XIAMETER™ RBB-2002-30, respectively manufactured by DSC. An HCR such as Base, XIAMETER™ RBB-2004-60, or XIAMETER™ RBB-2220-70 may be used.

[0054] The method described herein further comprises a step (12) of adhering the opposite surface of the silicone pressure sensitive adhesive described in step (10) to a surface of a silicone rubber article. Step (12) may be performed by any convenient means, such as contacting the surface of the silicone rubber article with the opposite surface of the silicone pressure sensitive adhesive and applying pressure. If a release liner is used to protect the opposite surface of the silicone pressure sensitive adhesive, the release liner is removed before contacting the surface of the silicone rubber article with the opposite surface of the silicone pressure sensitive adhesive. The resulting product prepared in step (12) is a laminated article. In the method comprising wet casting described above, the laminated article may comprise a backing selected from a polymeric film, a polymeric foam, or glass, the silicone pressure sensitive adhesive described above, and a silicone rubber article.

[0055] Alternatively, if dry casting is used in steps (8)-(10) above, the backing includes a release liner. The release liner may be removed after step (10) to form the silicone pressure sensitive adhesive layer as a free-standing film. Alternatively, the release liner may be removed after step (12). When dry casting is performed, the method includes: Optionally, (13) treating a surface of the second silicone rubber article; and (14) adhering the surface of the silicone pressure sensitive adhesive layer (exposed by removal of the release liner) to the surface of a second silicone rubber article.

[0056] The second silicone rubber article is as described above for use in step (12). The second silicone rubber article may be the same as the silicone rubber article used in step (12). Alternatively, the second silicone rubber article may be different from the silicone rubber article used in step (12). In this case, the laminated article formed by the method has a silicone pressure sensitive adhesive layer sandwiched between the silicone rubber article and the second silicone rubber article.

[0057] FIG. 1 shows a partial cross-sectional view of a laminate article (100) prepared by the method described above. The laminate article (100) comprises a silicone pressure sensitive adhesive (102) having a surface (102a) and an opposing surface (102b). The opposing surface (102b) of the silicone pressure sensitive adhesive (102) adheres to a surface (103a) of a silicone rubber article (103) with a peel adhesion of greater than 1,000 gf / in as measured by the test method described in the Examples below. The silicone pressure sensitive adhesive (102) may have a thickness of 10 μm to 200 μm. The silicone pressure sensitive adhesive (102) adheres to a backing (101) having a surface (101b). The surface (102a) of the silicone pressure sensitive adhesive (102) is in contact with the surface (101b) of the backing (101). The backing (101) is a polymer film that may be selected from the group consisting of PE, PU, ​​TPU, and TPE and may have a thickness of 10 μm to 200 μm. The silicone rubber article (103) may be an LSR as described above.

[0058] The silicone pressure sensitive adhesive composition may be used in the fabrication of a laminate article (100) by wet casting. For example, the silicone pressure sensitive adhesive composition may be applied to the surface (101b) of a backing (101) and cured to form a silicone pressure sensitive adhesive (102). Alternatively, the silicone pressure sensitive adhesive composition may be applied to the surface (103a) of a silicone rubber article (103) and cured to form a silicone pressure sensitive adhesive (102). Alternatively, the silicone pressure sensitive adhesive composition may be applied to the surface of a release liner and cured to form a silicone pressure sensitive adhesive (102). The silicone rubber article (103) may then be contacted with the opposite surface (102b) of the silicone pressure sensitive adhesive (102), and the surface (101b) of the backing (101) may be contacted with the surface (102a) of the silicone pressure sensitive adhesive (102). Pressure may be applied to adhere the layers of backing (101), silicone pressure sensitive adhesive (102), and silicone rubber article (103) together.

[0059] Alternatively, wet casting may be used to prepare a laminate article comprising a backing comprising silicone rubber and the silicone pressure sensitive adhesive described above, and optionally a (second) silicone rubber article. In this method, the backing may be the same or a different silicone rubber article as the (second) silicone rubber article used in step (12) below. Alternatively, the backing may comprise more than one component material, such as a mesh (which may be fabricated from a polymeric material as described above) impregnated with silicone rubber. This method for fabricating a laminate article includes: (1) under conditions for carrying out a condensation reaction, (P) a starting material (P), which is a bis-hydroxyl terminated polydiorganosiloxane having a weight average molecular weight of from 10,000 g / mol to less than 200,000 g / mol as measured by GPC, and which is present in an amount of greater than 20.5 weight percent based on the combined weight of starting materials (P) and (R); (R) a hydroxyl-functional polyorganosiloxane resin having a weight average molecular weight of 15,000 g / mol to 30,000 g / mol as measured by GPC, the starting material (R) being present in an amount of less than 79.5% by weight, based on the combined weight of the starting materials (P) and (R); (S) a solvent, and optionally, (N) a neutralizing agent, wherein the starting materials (P) and (R) are present in a weight ratio (R) / (P) of from 0.65 / 1 to less than 3.0 / 1; combining starting materials comprising: (2) adding to the reaction mixture (C) a condensation reaction catalyst to form a catalyzed reaction mixture; (3) mixing the catalyzed reaction mixture at a temperature between 20° C. and 150° C. and removing water to form a reaction product comprising a condensation reaction product of (P) and (R); Optionally, (4) recovering the condensation reaction product of (P) and (R); and (5) The condensation reaction product is mixed with (R') an additional polyorganosilicate resin having a weight average molecular weight of 5,500 g / mol to 30,000 g / mol as measured by GPC, and (R') is less than 2.27 / 1 to 3.88 / 1. tot) / (P) ratio (where R tot represents the sum of the amount of (R') and the amount of (R) from step (1), where (R tot (R) / (P)>(R) / (P); optionally, (6) adding up to 4 weight percent, based on the combined weight of (R) and (P), of (X) a peroxide crosslinker to form a silicone pressure sensitive adhesive composition; Optionally, (7) treating the surface of the backing with silicone rubber; and (8) coating a silicone pressure sensitive adhesive composition onto a surface of a backing; (9) drying the silicone pressure sensitive adhesive composition; and (10) curing the silicone pressure sensitive adhesive composition to form a silicone pressure sensitive adhesive layer having a surface adhered to a surface of a backing, the silicone pressure sensitive adhesive layer further including an opposing surface opposite the surface of the backing; The method optionally includes: Optionally, (11) treating the surface of the silicone rubber article; and (12) adhering an opposing surface of the silicone pressure sensitive adhesive to a surface of a silicone rubber article; It may further include.

[0060] FIG. 2 shows a partial cross-sectional view of a laminated article (200) prepared by the method described above. The laminated article (200) comprises a silicone pressure sensitive (202) having a surface (202a) and an opposing surface (202b). The silicone pressure sensitive agent (202) may have a thickness of 10 μm to 200 μm. The silicone pressure sensitive agent (202) comprises a silicone rubber (201) and is adhered to a backing having a surface (201b), the peel adhesion being greater than 1,000 gf / in, as measured by the test method described in the Examples below. The surface (202a) of the silicone pressure sensitive agent (202) is in contact with the surface (201b) of the backing (201). The backing (201) may be a silicone rubber article, such as an LSR or HCR, as described above. Alternatively, the backing (201) may comprise a mesh impregnated with silicone rubber.

[0061] The silicone pressure sensitive adhesive composition may be used in the fabrication of a laminate article (200) by wet casting. For example, the silicone pressure sensitive adhesive composition may be applied to a surface (201b) of a backing (201) and cured to form a silicone pressure sensitive adhesive (202). EXAMPLES

[0062] The following examples are provided to illustrate the invention to one of ordinary skill in the art and should not be construed as limiting the scope of the invention as set forth in the claims. The starting materials used in these examples are listed in Table 1.

[0063] [Table 1]

[0064] TDCC means The Dow Chemical Company, Midland, Michigan, USA. DSC means Dow Silicones Corporation, Midland, Michigan, USA.

[0065] In this Reference Example 1, the condensation reaction product (thickened resin) was prepared as follows: PDMS polymer, MQ resin, solvent, and neutralizer were combined in a three-neck flask at room temperature. The contents of the flask were stirred at 250 rpm for 20 minutes with a stainless steel stirring paddle in the center neck. The condensation catalyst was then added while stirring. Another neck was connected to a Dean-Stark trap, which was then connected to a condenser with tap water cooling capability. The last neck contained a thermometer and a nitrogen sweep adapter to close the system. Finally, the three-neck flask with the mixture inside was attached to a heating mantle with temperature control and heated to a reaction temperature of 145°C. The reaction was allowed to continue for 3 hours starting from the start of reflux. Thickened resins A-E were prepared according to this procedure and are summarized in Table 2 below, with the selection and amount of each starting material as defined in Table 1.

[0066] [Table 2]

[0067] Table 2 shows the synthesis of thickening resins with different resin to polymer ratios while keeping the polymer and resin selection constant.

[0068] In this Reference Example 2, the starting materials in the amounts summarized in Tables 3 and 4 below were added to a dental mixer cup and mixed at 3500 rpm for 30 seconds at room temperature until homogenous. Peroxide crosslinker (in toluene) and Solvent 1 were added to each sample prepared as above in the dental mixer cup to reach a solids level of 50% by weight and a peroxide crosslinker level of 2% by weight. The resulting samples were mixed at 3500 rpm for 30 minutes until homogenous. Each sample was prepared for application testing by coating onto a 2 mil thick polyester (PET) sheet using a 3 mil coating bar. Each sheet was then cured in an oven at 80°C for 2 minutes, followed by 180°C for 2 minutes. Comparative Examples CE1-CE6 and Examples IE1-IE12 were prepared according to this Reference Example 2.

[0069] In this Reference Example 3, a commercially available peroxide curable silicone pressure sensitive adhesive supplied in CE7 was evaluated, and additional MQ resin was cold blended into it (in CE8 and CE9) by mixing in a dental mixer cup at 3500 rpm for 30 seconds under ambient conditions. Peroxide crosslinker (in toluene) and solvent 1 were added to each sample prepared as above in a dental mixer cup to reach a solids level of 50% by weight and a peroxide crosslinker level of 2% by weight. The resulting samples were mixed at 3500 rpm for 30 minutes until homogenous. Each sample was prepared for application testing by coating onto a 2 mil thick polyester (PET) sheet using a 3 mil coating bar. Each sheet was then cured in an oven at 80°C for 2 minutes, followed by 180°C for 2 minutes.

[0070] In this Example 4, the liquid silicone rubber (LSR) substrates were XIAMETER® RBL-2004-30 LSR and XIAMETER® RBL-2004-50 LSR samples from DSC. To mix Part A and Part B, 100g of Part A and 100g of Part B were added to a dental mixer cup and mixed for 3 cycles, each cycle for 20 seconds at 1800 rpm. To ensure that the material did not stick to the bottom and corners of the dental cup, the cup was scraped and mixed by hand between cycles. The mixture was transferred to a polished book mold or Teflon lined chase and cured at 350°F for 5 minutes.

[0071] In this Reference Example 5, Peel Adhesion Strengthwas measured as follows: peel adhesion (180°) was tested according to PSTC-101 standard. Each silicone pressure sensitive adhesive coated on 2 mil polyester film (tape) prepared as described in Reference Examples 2 and 3 was laminated onto a silicone rubber surface, typically after 1 day of curing. The silicone rubber surface was wiped with isopropyl alcohol to clean the surface and allowed to dry for 5 minutes under ambient conditions before the silicone pressure sensitive adhesive was laminated to it. After lamination, a 2 kg rubber-coated roller was applied to the resulting article (5 times each before and after), and the article was allowed to rest at room temperature for 20 minutes of dwell time before peel adhesion testing. A 1 inch wide tape from the silicone rubber substrate was pulled at 12 inches / minute using a TMI peel and adhesion tester. The results are shown in Tables 3 and 4 below.

[0072] [Table 3]

[0073] Examples IE1-IE5 show that combining additional polyorganosilicate resin (resin 2, Mw 21,350 g / mol, OH content 3.07 wt%) with thickening resin at (R) / (P) ratios of 0.65 / 1 to 2.27 / 1 increased adhesion of each sample to both 30 and 50 durometer LSR to over 1,000 g / in under the conditions tested. The higher (R) / (P) ratio in the thickening resin of IE5 resulted in higher adhesion after the additional resin was added. In samples CE2-CE5 and sample CE6, different additional resins (with various Mw and OH levels) were added to the same thickening resin. Adding resins with lower Mw or lower levels of OH content did not result in strong adhesion to LSR. For the thickened resin with an (R) / (P) ratio of 1 / 1, the addition of resins with low Mw (CE2) or low OH levels (as shown in samples CE3-CE5) did not provide strong adhesion to LSR (less than 1,000 g / in). For the thickened resin with an (R) / (P) ratio of 1.46 / 1, the addition of additional resins with low Mw and low OH levels (as shown in sample CE6) did not provide strong adhesion to LSR (less than 1,000 g / in).

[0074] [Table 4]

[0075] In each of samples IE6 and IE7 and samples IE8-IE12, different additional resins (with various Mw and OH levels) were added to the same thickened resin. Adding resins with higher Mw or higher levels of OH content resulted in high adhesion to LSR. For thickened resins with an (R) / (P) ratio of 1 / 1, adding resins with high Mw and high OH levels (as shown in samples IE2, IE6, and IE7) resulted in strong adhesion to LSR (greater than 1,000 g / in). For thickened resins with an (R) / (P) ratio of 1.46 / 1, adding additional resins with high Mw (as shown in samples IE3, IE9, IE10, IE11, and IE12) or high OH levels (as shown in sample IE8) resulted in strong adhesion to LSR (greater than 1,000 g / in).

[0076] Comparative Examples CE8 and CE9 showed that when additional resin was added to a commercial peroxide-curable silicone pressure sensitive adhesive composition (CE7), the adhesion of the silicone pressure sensitive adhesive prepared by curing the composition to silicone rubber was still less than 1,000 gf / in on at least one substrate.

[0077] In this Example 6, samples of laminate articles were prepared by a method involving wet casting (Method 2) as follows: 1. Samples of silicone pressure sensitive adhesive compositions were prepared by mixing peroxide crosslinker (in toluene) and solvent 1 with each of composition IE10 and commercial PSA (7406-VLO, CE7) (prepared as described above) in a dental mixer cup to reach a solids level of 50% by weight and a peroxide crosslinker level of 2% by weight. Each resulting sample was mixed at 3500 rpm for 30 seconds until homogenous. 2. Two sheets of silicone rubber substrate (50 durometer LSR) were prepared as described above in Reference Example 4. The surface of each silicone rubber substrate was cleaned by wiping with isopropyl alcohol and allowing to dry under ambient conditions for 5 minutes. 3. Each sample of the silicone pressure-sensitive adhesive composition was coated onto the cleaned surface of a silicone rubber substrate using a 3 mil coating bar. Each coated substrate was then placed in an oven at 80° C. for 2 minutes, followed by 180° C. for 2 minutes to prepare a laminate of a (cured) silicone pressure-sensitive adhesive layer on each silicone rubber sheet. 4. Two additional sheets of silicone rubber substrate (50 durometer LSR) were prepared as described above in Reference Example 4. The surface of each silicone rubber substrate was cleaned by wiping with isopropyl alcohol and allowing to dry under ambient conditions for 5 minutes. 5. One day after step 3, the surface of each silicone pressure sensitive adhesive layer was contacted with the cleaned surface of each silicone rubber substrate from step 4. A rubber-coated 2 kg roller was applied to the resulting articles (five times back and forth), the articles were allowed to rest at room temperature for 20 minutes dwell time, and then peel adhesion testing was performed according to the PSTC-101 standard, as described above, except that a silicone rubber substrate was used as the backing (instead of polyester film). A TMI peel and adhesion tester was used to pull a 1 inch wide tape from the silicone rubber substrate at 12 inches / minute. The peel adhesion test results are shown in Table 5 below.

[0078] [Table 5]

[0079] The results in Table 5 show that when the silicone pressure sensitive adhesive is adhered via wet casting (Method 2) to a silicone rubber article used as a backing, the silicone pressure sensitive adhesive has a higher peel adhesion than a commercial PSA (CE7).

[0080] In this Example 7, samples of laminate articles were prepared by a method involving dry casting (Method 3) as follows: 1. Two samples of silicone pressure sensitive adhesive compositions were prepared by mixing peroxide crosslinker (in toluene) and solvent 1 with each of composition IE10 and commercial PSA (7406-VLO, CE7) (prepared as described above) in a dental mixer cup to reach a solids level of 50% by weight and a peroxide crosslinker level of 2% by weight. Each resulting sample was mixed at 3500 rpm for 30 seconds until homogenous. 2. Each sample of the silicone pressure sensitive adhesive composition was coated onto a fluorosilicone release liner using a 3 mil coating bar. Each coated liner was then placed in an oven at 80° C. for 2 minutes, followed by 180° C. for 2 minutes to prepare a laminate of a (cured) silicone pressure sensitive adhesive layer on each fluorosilicone release liner. Each laminate was aged at room temperature for 1 day. 3. Two sheets of silicone rubber substrate (50 durometer LSR) were prepared as described above in Reference Example 4. The surface of each silicone rubber substrate was cleaned by wiping with isopropyl alcohol and allowing to dry under ambient conditions for 5 minutes. 4. The surface of each silicone pressure sensitive adhesive layer from Step 2 was contacted with the cleaned surface of each silicone rubber substrate from Step 3. 5. Two sheets of silicone rubber substrate (50 durometer LSR) were prepared as described above in Reference Example 4. The surface of each silicone rubber substrate was cleaned by wiping with isopropyl alcohol and allowing to dry under ambient conditions for 5 minutes. 6. One day after step 4, the fluorosilicone release liner was removed from each laminate and the exposed surface of each resulting silicone pressure sensitive adhesive layer was contacted with the cleaned surface of the silicone rubber substrate from step 5. A rubber coated 2 kg roller was applied to the resulting article (five times back and forth) and the article was allowed to sit at room temperature for 20 minutes dwell time before peel adhesion testing according to the PSTC-101 standard, as described above except that a silicone rubber substrate was used (instead of polyester film). A TMI peel and adhesion tester was used to pull a 1 inch wide tape from the silicone rubber substrate at 12 inches / minute. The peel adhesion test results are shown in Table 6 below.

[0081] [Table 6]

[0082] The results in Table 6 show that when the silicone pressure sensitive adhesive is adhered to a silicone rubber article via dry casting (Method 3), the silicone pressure sensitive adhesive has a higher peel adhesion than a commercial PSA (CE7).

[0083] Definitions and Use of Terms All amounts, ratios and percentages are by weight unless otherwise indicated. The amounts of all starting materials in the composition total 100% by weight. The Summary and Abstract of the Invention are incorporated herein by reference. The articles "a", "an" and "the" each refer to one or more, unless otherwise indicated by the context of the specification. The singular includes the plural unless otherwise indicated. The terms "comprising" and its derivatives, such as "comprise" and "comprises", are used herein in their broadest sense to mean and include the notions "including", "include", "consist(ing) essentially of" and "consist(ing) of". The use of "for example", "eg", "such as" and "including" to list examples is not limited to only the examples listed. Thus, "for example" or "such as" means "for example, but not limited to" or "such as, but not limited to," and includes other similar or equivalent examples.

[0084] It is to be understood that the appended claims are not limited to the specific compounds, compositions, or methods described therein for purposes of describing the "Description of the Invention" and may vary among specific embodiments within the scope of the appended claims. With respect to any Markush group relied upon in this specification to describe particular features or aspects of various embodiments, different, special, and / or unexpected results may result from each element of the respective Markush group independent of all other Markush elements. Each element of the Markush group may be relied upon individually and / or in combination to provide sufficient support for specific embodiments within the scope of the appended claims.

[0085] Abbreviations used herein are defined in Table 7.

[0086] [Table 7]

[0087] The Mn, Mw, and molecular weight distribution of the polymer and condensation reaction product can be determined by GPC using an Agilent Technologies 1260 Infinity chromatograph and toluene as the solvent. The instrument is equipped with two PLgel Mixed C columns. Calibration was performed using polystyrene standards. Samples were prepared by dissolving the polymer in toluene (approximately 10 mg / mL) and then immediately analyzing the material by GPC (flow rate 1 mL / min and column temperature 45° C.).

[0088] The Mn, Mw, and molecular weight distribution of the resin can be determined by GPC using an Agilent Technologies 1260 Infinity chromatograph and ethyl acetate as the solvent. The instrument is equipped with two columns, an Agilent PLgel Mixed-D and a PLgel Mixed-E column. Calibration was performed using polystyrene standards. Samples were prepared by dissolving the polymer in toluene (approximately 20 mg / mL) and then immediately analyzing the material by GPC (flow rate 1 mL / min and column temperature 35° C.).

Claims

1. 1. A method of making a laminate article, comprising: (1) under conditions for carrying out a condensation reaction, (P) a bis-hydroxyl terminated polydiorganosiloxane having a weight average molecular weight of from 10,000 g / mol to less than 200,000 g / mol as measured by GPC, said starting material (P) being present in an amount of greater than 20.5 weight percent based on the combined weight of starting materials (P) and (R); (R) a hydroxyl-functional polyorganosiloxane resin having a weight average molecular weight of 15,000 g / mol to 30,000 g / mol as measured by GPC, said starting material (R) being present in an amount of less than 79.5 wt.%, based on the combined weight of starting materials (P) and (R); (S) a solvent, and optionally, (N) a neutralizing agent, wherein the starting materials (P) and (R) are present in a weight ratio (R) / (P) of from 0.65 / 1 to less than 3.0 / 1; combining starting materials comprising: (2) adding (C) a condensation reaction catalyst to the reaction mixture to form a catalyzed reaction mixture; (3) mixing the catalyzed reaction mixture at a temperature between 20° C. and 150° C. and removing water to form a reaction product comprising the condensation reaction product of (P) and (R); Optionally, (4) recovering the condensation reaction product of (P) and (R); and (5) The condensation reaction product is added with (R') an additional polyorganosilicate resin having a weight average molecular weight of 5,500 g / mol to 30,000 g / mol as measured by GPC, and (R tot ) / (P) ratio (where R tot represents the sum of the amount of (R′) and the amount of (R) from step (1), where (R tot (R) / (P)>(R) / (P); optionally, (6) adding up to 4 weight percent, based on the combined weight of (R), (R'), and (P), of (X) a peroxide crosslinker to form a silicone pressure sensitive adhesive composition; Optionally, (7) treating the surface of the backing; and (8) coating the silicone pressure sensitive adhesive composition onto the surface of the backing; and (9) drying the silicone pressure sensitive adhesive composition; and (10) curing the silicone pressure sensitive adhesive composition to form a silicone pressure sensitive adhesive layer having a surface adhered to the surface of the backing, the silicone pressure sensitive adhesive layer further comprising an opposing surface opposite the surface of the backing; Optionally, (11) treating the surface of the silicone rubber article; and (12) adhering the opposing surface of the silicone pressure sensitive adhesive to the surface of the silicone rubber article; and A method comprising:

2. The starting material (P), said bis-hydroxyl terminated polydiorganosiloxane, has the formula 【Chemistry 1】 (In the formula, each R 1 10. The method of claim 1, wherein: R is an independently selected alkyl group of 1 to 6 carbon atoms, and the subscript a represents the average number of difunctional siloxane units per molecule, where 250≦a≦3,000.

3. The hydroxyl-functional polyorganosilicate resin starting material (R) has the unit formula (R 1 3 SiO 1/2 ) b (SiO 4/2 ) c (HO 1/2 ) d (In the formula, each R 1 13. The method of claim 1, wherein: x is an independently selected alkyl group of 1 to 6 carbon atoms; subscripts b and c represent the mole fractions of mono- and tetrafunctional units, respectively, with subscripts b and c having values ​​such that 0.4≦b≦0.5, 0.5≦c≦0.6, and the amount (b+c)=1; and subscript d represents the amount of hydroxyl groups in the resin, with subscript d having a value sufficient to provide the resin with a hydroxyl content of 2% to 5% by weight.

4. 2. The method of claim 1, wherein (R) / (P) is from 0.65 / 1 to 1.82 / 1.

5. 2. The method of claim 1, wherein (N) the neutralizing agent is present and the neutralizing agent comprises a silyl phosphate.

6. The method of claim 1 , wherein (C) the condensation reaction catalyst is an acid.

7. (R′) the additional polyorganosilicate resin has the unit formula (R 1 3 SiO 1/2 ) b’ (SiO 4/2 ) c’ (HO 1/2 ) d’ (In the formula, each R 1 5. The method of claim 1, wherein: a is an independently selected alkyl group of 1 to 6 carbon atoms; subscripts b' and c' represent the mole fractions of monofunctional and tetrafunctional units, respectively, with subscripts b' and c' having values ​​such that 0.4≦b≦0.5, 0.5≦c≦0.6, and the amount (b'+c')=1; subscript d' represents the amount of hydroxyl groups in the resin, with subscript d' having a value sufficient to provide the resin with a hydroxyl content of 0.5% to 5% by weight; and wherein the additional polyorganosilicate resin has a weight average molecular weight of 5,500 g / mol to 30,000 g / mol as measured by GPC.

8. (R tot 8. The method of claim 7, wherein the ratio of (A) / (P) is 3 / 1.

9. 2. The method of claim 1, wherein step (6) is present and (X) the peroxide crosslinking agent comprises benzoyl peroxide.

10. The method of claim 1 , wherein there is a step (7), step (7) comprising applying a primer to the surface of the backing.

11. 2. The method of claim 1, wherein step (11) is present and step (11) comprises cleaning the surface of the silicone rubber with alcohol.

12. The method of claim 1, wherein in step (12), the silicone rubber has a durometer of 30-50.

13. A laminated article prepared by the method of any one of claims 1 to 12.

14. the backing comprises a release liner; removing the release liner after step (10); and Optionally, (13) treating the surface of the silicone rubber article; and (14) adhering said surface of said silicone pressure sensitive adhesive layer to said surface of said silicone rubber article; The method of claim 1 further comprising:

15. 1. A method of making a laminate article, comprising: (1) under conditions for carrying out a condensation reaction, (P) a bis-hydroxyl terminated polydiorganosiloxane having a weight average molecular weight of from 10,000 g / mol to less than 200,000 g / mol as measured by GPC, said starting material (P) being present in an amount of greater than 20.5 weight percent based on the combined weight of starting materials (P) and (R); (R) a hydroxyl-functional polyorganosiloxane resin having a weight average molecular weight of 15,000 g / mol to 30,000 g / mol as measured by GPC, said starting material (R) being present in an amount of less than 79.5 wt.%, based on the combined weight of starting materials (P) and (R); (S) a solvent, and optionally, (N) a neutralizing agent, wherein the starting materials (P) and (R) are present in a weight ratio (R) / (P) of from 0.65 / 1 to less than 3.0 / 1; combining starting materials comprising: (2) adding (C) a condensation reaction catalyst to the reaction mixture to form a catalyzed reaction mixture; (3) mixing the catalyzed reaction mixture at a temperature between 20° C. and 150° C. and removing water to form a reaction product comprising the condensation reaction product of (P) and (R); Optionally, (4) recovering the condensation reaction product of (P) and (R); and (5) The condensation reaction product is added with (R') an additional polyorganosilicate resin having a weight average molecular weight of 5,500 g / mol to 30,000 g / mol as measured by GPC, and (R tot ) / (P) ratio (where R tot represents the sum of the amount of (R′) and the amount of (R) from step (1), where (R tot (R) / (P)>(R) / (P); optionally, (6) adding up to 4 weight percent, based on the combined weight of (R) and (P), of (X) a peroxide crosslinker to form a silicone pressure sensitive adhesive composition; Optionally, (7) treating the surface of the backing with silicone rubber; and (8) coating the silicone pressure sensitive adhesive composition onto the surface of the backing; and (9) drying the silicone pressure sensitive adhesive composition; and (10) curing the silicone pressure sensitive adhesive composition to form a silicone pressure sensitive adhesive layer having a surface adhered to the surface of the backing, the silicone pressure sensitive adhesive layer further comprising an opposing surface opposite the surface of the backing; Optionally, (10) treating a surface of the silicone rubber article; and Optionally, (11) adhering the opposing surface of a silicone pressure sensitive adhesive to the surface of the silicone rubber article; and A method comprising:

Citation Information

Patent Citations

  • Production of pressure-sensitive silicone adhesive

    JP1998130617A

  • Silicone-based pressure-sensitive adhesive composition, pressure-sensitive adhesive sheet, and silicone rubber laminate

    JP2009155515A

  • Polyorganosiloxane hybrid pressure-sensitive adhesives and methods for preparing and using same

    JP2023521567A

  • Pressure sensitive adhesives and methods for their preparation

    US20090294023A1