Cold-rolled steel sheet and its manufacturing method

A cold-rolled steel sheet with optimized alloying and controlled manufacturing process achieves ultra-high strength and formability, addressing the challenges of weight and structural integrity in vehicle components.

JP2024542211AActive Publication Date: 2024-11-13POHANG IRON & STEEL CO LTD
View PDF 15 Cites 0 Cited by

Patent Information

Application Number
JP2024529592
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2021-11-19
Filing Date
2022-11-07
Publication Date
2024-11-13
Estimated Expiration
2042-11-07

AI Technical Summary

Technical Problem

Existing cold-rolled steel sheets face challenges in achieving ultra-high tensile strength of 1180 MPa or more, while maintaining high ductility and formability, due to issues such as poor shape quality, reduced elongation, and increased weight, which are exacerbated by the need for high-strength materials in vehicle structures.

Method used

A cold-rolled steel sheet composition comprising specific alloying elements (C, Si, Al, Mn, Cr, Mo, B, Nb, Ti) within defined ranges, combined with a controlled manufacturing process involving continuous annealing, multi-stage cooling, and reheating, to achieve a microstructure of fresh and tempered martensite, bainite, and retained austenite, ensuring strength and formability.

Benefits of technology

The solution results in a steel sheet with yield strength of 800-1200 MPa, tensile strength of 1180-1400 MPa, and excellent formability, including high elongation and resistance to Liquid Metal Embrittlement (LME) cracks, suitable for vehicle body components.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024542211000001_ABST
    Figure 2024542211000001_ABST
Patent Text Reader

Abstract

The present invention relates to a cold-rolled steel sheet and a manufacturing method thereof, and more particularly to a cold-rolled steel sheet having excellent strength and formability that can be suitably applied to structural members such as vehicle body members, seat rails, and pillars, and a manufacturing method thereof.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a cold-rolled steel sheet and a manufacturing method thereof, and more particularly to a cold-rolled steel sheet having excellent strength and formability that can be suitably applied to structural members such as vehicle body members, seat rails, and pillars, and a manufacturing method thereof. [Background technology]

[0002] Recently, as the construction of safety devices is mandatory due to the strengthening of safety regulations for automobile passengers and pedestrians, the weight of the vehicle body increases, which is the opposite of the weight reduction required to improve the fuel efficiency of automobiles. Consumers are increasingly interested in hybrid and electric vehicles, which are environmentally friendly and highly fuel efficient. In order to produce such environmentally friendly and safe vehicles, the weight of the vehicle body structure and the stability of the vehicle body materials must be ensured. However, hybrid vehicles are equipped with various devices such as electric engines, electric batteries, and secondary fuel storage tanks in addition to the existing gasoline engine. In addition, the weight of the vehicle body increases as the driver's convenience facilities are continuously added. Therefore, in order to realize the weight reduction of the vehicle body, it is essential to develop a material that is thin and has excellent strength, ductility, and bending properties. Therefore, in order to solve this problem, it is necessary to develop a giga-class steel plate that can ensure high strength and high ductility with a tensile strength of 1180 MPa or more.

[0003] Meanwhile, in recent years, with the expansion of regulations on the impact stability of automobiles, high-strength steels with excellent yield strength are being used for structural members such as members, seat rails, and pillars to improve the impact resistance of the vehicle body. The higher the yield strength relative to the tensile strength, i.e., the higher the yield ratio (yield strength / tensile strength), the more advantageous it is for structural members to absorb impact energy. However, in general, as the strength of steel plate increases, the elongation decreases, which causes a problem of reduced formability. Therefore, there is a demand for the development of materials that simultaneously have improved high yield ratios, formability, and bending properties, which are important physical properties when processing parts.

[0004] A typical manufacturing method for increasing the yield strength is a method using water cooling during continuous annealing. For example, after soaking in water in the annealing process, a steel sheet can be manufactured in which the microstructure is transformed from martensite to tempered martensite by tempering. A typical prior art of such a method is Patent Document 1. Patent Document 1 relates to a technique for manufacturing a steel material having a volume fraction of martensite of 80 to 97% and the remainder of ferrite by water cooling to room temperature after continuous annealing, and then performing overaging treatment at a temperature of 120 to 300°C for 1 to 15 minutes. In this way, when ultra-high strength steel is manufactured by the water cooling and tempering method, although the yield ratio is extremely high, there is a problem that the shape quality of the coil deteriorates due to temperature variations in the width direction and length direction. This also causes problems such as poor material quality and reduced workability depending on the part during roll forming processing.

[0005] Patent Document 2 is a conventional technique for improving the workability of the high-tensile steel sheet. Patent Document 2 relates to a steel sheet made of a composite structure mainly composed of tempered martensite, and is characterized in that fine precipitated Cu particles with a particle size of 1 to 100 nm are dispersed inside the structure in order to improve the workability. However, Patent Document 2 has the problem that the Cu content is excessively increased to 2 to 5% in order to precipitate good fine Cu particles, which may cause red brittleness due to Cu, and also excessively increases the manufacturing cost.

[0006] Patent Document 3 presents a steel sheet having a fine structure containing 2-10% by area of ​​pearlite in a ferrite matrix, and improved in strength by precipitation strengthening and grain refinement through the addition of carbonitride-forming elements such as Ti. Patent Document 3 has the advantage of being able to easily obtain high strength at low manufacturing costs, but has the disadvantage of requiring high-temperature annealing to cause sufficient recrystallization and ensure ductility, since the recrystallization temperature rises sharply due to fine precipitates. In addition, the existing precipitation strengthened steel, which is strengthened by precipitating carbonitrides in a ferrite matrix, has the problem that it is difficult to obtain high-strength steel of 600 MPa class or more.

[0007] Another method is the Quenching & Partitioning (Q&P) method, which can secure strength and elongation at the same time by quenching austenite to a temperature between Ms, the martensite transformation start temperature, and Mf, the transformation completion temperature, during the heat treatment process to secure martensite, and at the same time diffusing austenite stabilizing elements such as C and Mn into the residual austenite phase at an appropriate temperature. In the Q&P method, the heat treatment process in which steel is heated to a temperature of A3 or higher, quenched to a temperature below Ms, and maintained between Ms and Mf temperatures is called 1-step Q&P, and the process in which steel is reheated to a temperature above Ms after quenching and then heat treated is called 2-step Q&P. For example, Patent Document 4 describes a method for retaining austenite by Q&P heat treatment. However, although precise control of the annealing temperature, cooling temperature, and reheating temperature is important in the Q&P process, Patent Document 4 merely describes the concept of Q&P heat treatment, and does not provide a detailed description of a specific control method, so that there are limitations in practical application.

[0008] Therefore, there is a demand for the development of an ultra-high strength steel material having a tensile strength of 1180 MPa or more that can solve the above-mentioned problems, does not crack even in a 180° fully crimped bending test, and has a high yield ratio that allows cold forming. [Prior art documents] [Patent documents]

[0009] [Patent Document 1] Japanese Patent Registration No. 2528387 [Patent Document 2] Japanese Patent Publication No. 2005-264176 [Patent Document 3] Korean Patent Publication No. 2015-0073844 [Patent Document 4] U.S. Patent Publication No. 2006-0011274 Summary of the Invention [Problem to be solved by the invention]

[0010] One aspect of the present invention is to provide a cold-rolled steel sheet having excellent strength and formability, and a method for producing the same. [Means for solving the problem]

[0011] One embodiment of the present invention contains, by weight, 0.10 to 0.20% C, 0.05 to 0.495% Si, 0.01 to 0.18% Al, 2.4 to 3.5% Mn, 0.05 to 0.8% Cr, 0.05 to 0.8% Mo, 0.0001 to 0.003%, 0.005 to 0.07% Nb, 0.005 to 0.07% Ti, the balance being Fe and other unavoidable impurities, and satisfies the following relational expressions 1 to 3. The microstructure is composed of, by area%, 1-11% fresh martensite, 80-97% one or two of tempered martensite and bainite, 1-9% retained austenite, and 7% or less (including 0%) ferrite, and contains 50 particles / μm of one or more of MC, M (C, N) and their composite precipitates (M = Nb, Ti, Si, Cr, Mo, Fe) with an average size of 20 nm or less. 2 The present invention provides a cold-rolled steel sheet comprising the above. [Relationship 1] 1120≦X=2301×C+287×Mn+1533×Nb+228×Cr-71×Si-84.1×Al≦1380 [Relationship 2] 0.25≦Y=C+Si / 30+Mn / 20≦0.36 [Relationship 3] 3420≦X / Y≦4360 (However, in the above relational expressions 1 to 3, the content of each alloy element is in weight percent.)

[0012] Another embodiment of the present invention includes the steps of: heating a slab containing, by weight, 0.10-0.20% C, 0.05-0.495% Si, 0.01-0.18% Al, 2.4-3.5% Mn, 0.05-0.8% Cr, 0.05-0.8% Mo, 0.0001-0.003%, 0.005-0.07% Nb, 0.005-0.07% Ti, the balance being Fe and other inevitable impurities, and satisfying the following relations 1-3; finish rolling the heated slab so that the finish rolling delivery temperature is A3+50°C to A3+160°C to obtain a hot-rolled steel sheet; cooling the hot-rolled steel sheet to Ms+100°C to Ms+300°C, and then coiling the steel sheet; and winding the coil. The present invention provides a method for producing a cold-rolled steel sheet, the method including: cold-rolling the removed hot-rolled steel sheet to obtain a cold-rolled steel sheet; continuously annealing the cold-rolled steel sheet at a continuous annealing temperature (SS) range of 800 to 860°C; primarily cooling the continuously annealed cold-rolled steel sheet to a primary cooling finish temperature (SCS) of 450 to 650°C at an average cooling rate of less than 10°C / s; secondarily cooling the primarily cooled cold-rolled steel sheet to a secondary cooling finish temperature (RCS) of 300 to 390°C at an average cooling rate of 10°C / s or more; and reheating the secondarily cooled cold-rolled steel sheet at a reheating temperature (RHS) range of 400 to 540°C, wherein the continuous annealing, secondary cooling and reheating satisfy the following Relational Formulas 4 to 6. [Relationship 1] 1120≦X=2301×C+287×Mn+1533×Nb+228×Cr-71×Si-84.1×Al≦1380 [Relationship 2] 0.25≦Y=C+Si / 30+Mn / 20≦0.36 [Relationship 3] 3420≦X / Y≦4360 [Equation 4] SS-A3≧5℃ [Equation 5] -30℃≧Ms-RCS≧110℃ [Equation 6] -30℃≧RHS-RCS≧250℃ (However, in the above relational expressions 1 to 3, the content of each alloy element is in weight percent.) Effect of the Invention

[0013] According to one aspect of the present invention, it is possible to provide a cold-rolled steel sheet having excellent strength and formability, and a method for producing the same. [Brief description of the drawings]

[0014] [Figure 1] FIG. 2 is a schematic diagram of a welding method performed to measure the average length of LME cracks according to one embodiment of the present invention. [Diagram 2] 1 is a photograph of Example 1 according to an embodiment of the present invention, observed by SEM. [Diagram 3] 1 is a TEM photograph of Example 1 according to an embodiment of the present invention. [Figure 4] 13 is a photograph showing a cross section of a welded portion after LME evaluation for Example 3 according to an embodiment of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0015] Hereinafter, a cold rolled steel sheet according to an embodiment of the present invention will be described. First, the alloy composition of the present invention will be described. The content of the alloy composition described below is expressed in weight percent.

[0016] C: 0.10-0.20% Carbon (C) is an extremely important element added for solid solution strengthening. In addition, C contributes to improving strength by combining with precipitation strengthening elements to form fine carbides. When the C content is less than 0.10%, it is extremely difficult to ensure the desired strength. On the other hand, when the C content exceeds 0.20%, the strength increases rapidly as martensite is excessively formed during cooling due to an increase in hardening ability, and bending workability may deteriorate. In addition, weldability deteriorates, and there is a high possibility that welding defects will occur during part processing at a customer company. Therefore, the C content is preferably in the range of 0.10 to 0.20%. The lower limit of the C content is more preferably 0.11%, and even more preferably 0.12%. The upper limit of the C content is more preferably 0.19%, and even more preferably 0.18%.

[0017] Silicon: 0.05 to 0.495% Silicon (Si) is an element that is advantageous in securing elongation because it not only contributes to increasing strength, but also inhibits carbide formation, and carbon is distributed and accumulated in the retained austenite without being formed as carbides during annealing soaking and cooling, so that the retained austenite exists as an austenite phase at room temperature. If the Si content is less than 0.05%, it may be difficult to sufficiently secure the above-mentioned effects. On the other hand, if the Si content exceeds 0.495%, it becomes impossible to prevent deterioration of the physical properties of the welded part due to the formation of LME cracks, and surface defects such as red scale are induced, resulting in deterioration of the surface characteristics and platability of the steel material. The lower limit of the Si content is more preferably 0.10%, and even more preferably 0.15%. The upper limit of the Si content is more preferably 0.490%, and even more preferably 0.485%.

[0018] Al: 0.01 to 0.18% Aluminum (Al) is not only an element contained for deoxidizing the steel material, but also an element that is effective in suppressing the precipitation of cementite and stabilizing the retained austenite. If the Al content is less than 0.01%, it may be difficult to sufficiently ensure the above-mentioned effects. On the other hand, if the Al content exceeds 0.18%, the castability of the steel material is impaired. The lower limit of the Al content is more preferably 0.02%, and even more preferably 0.03%. The upper limit of the Si content is more preferably 0.17%, and even more preferably 0.16%.

[0019] Mn: 2.4-3.5% Manganese (Mn) is an element added to ensure strength. If the Mn content is less than 2.4%, it is difficult to ensure strength. On the other hand, if the Mn content exceeds 3.5%, the bainite transformation rate slows down and excessive fresh martensite is formed, making it difficult to obtain high hole expandability. In addition, band structures are formed due to the segregation of Mn, which impairs the material uniformity and formability of the material. The lower limit of the Mn content is more preferably 2.5%, and even more preferably 2.6%. The upper limit of the Mn content is more preferably 3.4%, and even more preferably 3.2%.

[0020] Cr: 0.05~0.8% Chromium (Cr) is an element added to ensure strength and hardenability. When Mn is added alone, an extremely large amount of Mn must be added beyond the range of the Mn content of the present invention in order to ensure strength and hardenability, but this problem can be solved by adding 0.05% or more of Cr. On the other hand, if the Cr content exceeds 0.8%, local corrosion resistance is deteriorated and oxides are formed on the surface, impairing phosphating ability. The lower limit of the Cr content is more preferably 0.06%, and even more preferably 0.07%. The upper limit of the Cr content is more preferably 0.7%, and even more preferably 0.6%.

[0021] Mo: 0.05-0.8% Molybdenum (Mo) is an element added to ensure strength and hardenability. When Mn is added alone, an extremely large amount of Mn must be added, exceeding the range of the Mn content of the present invention. However, by adding Mo at 0.05% or more, such problems can be solved. On the other hand, when the Mo content exceeds 0.8%, phase transformation is suppressed, making it difficult to obtain a bainite structure, and since Mo is an expensive element, the economic efficiency of the steel sheet is poor. The lower limit of the Mo content is more preferably 0.06%, and even more preferably 0.07%. The upper limit of the Mo content is more preferably 0.7%, and even more preferably 0.6%.

[0022] B: 0.0001 to 0.003% Boron (B) is an element added to ensure hardenability. When Mn is added alone, an extremely large amount of Mn must be added, exceeding the range of the Mn content of the present invention, but this problem can be solved by adding 0.0001% or more of the above B. On the other hand, when the content of B exceeds 0.0030%, B accumulates excessively on the surface, impairing the plating adhesion. The lower limit of the above B content is more preferably 0.0002%, and even more preferably 0.0003%. The upper limit of the above B content is more preferably 0.0025%, and even more preferably 0.0020%.

[0023] Nb: 0.005 to 0.07% Niobium (Nb) is an element added to ensure strength and refine the microstructure. If the Nb content is less than 0.005%, it is difficult to obtain the effects of improving strength and refining the microstructure. On the other hand, if the Nb content exceeds 0.07%, recrystallization is delayed due to localized grain fixation, and the uniformity of the microstructure is impaired. The lower limit of the Nb content is more preferably 0.010%, and even more preferably 0.015%. The upper limit of the Nb content is more preferably 0.06%, and even more preferably 0.05%.

[0024] Ti: 0.005 to 0.07% Titanium (Ti) is an element added to ensure strength and refine the microstructure. If the Ti content is less than 0.005%, it is difficult to obtain the effects of improving strength and refining the microstructure. On the other hand, if the Ti content exceeds 0.07%, castability is impaired due to excessive formation of TiN, and recrystallization is delayed due to localized grain fixation, resulting in impaired uniformity of the microstructure. The lower limit of the Ti content is more preferably 0.010%, and even more preferably 0.015%. The upper limit of the Ti content is more preferably 0.06%, and even more preferably 0.05%.

[0025] On the other hand, the cold-rolled steel sheet of the present invention preferably satisfies the above-mentioned alloy composition and at the same time satisfies the following relations 1 to 3. In the following relations 1 to 3, the content of each alloy element is expressed in weight %.

[0026] [Relationship 1] 1120≦X=2301×C+287×Mn+1533×Nb+228×Cr-71×Si-84.1×Al≦1380 The above-mentioned relational formula 1 is a component relational formula for ensuring the excellent strength and moldability targeted by the present invention. If the value of X is less than 1120, it is difficult to ensure the strength targeted by the present invention due to insufficient hardening ability, and if it exceeds 1380, the tensile strength may become too high, resulting in deterioration of hole expandability and bending properties. Therefore, the value of X is preferably in the range of 1120 to 1380. The lower limit of the value of X is more preferably 1130, and even more preferably 1140. The upper limit of the value of X is more preferably 1370, and even more preferably 1360.

[0027] [Relationship 2] 0.25≦Y=C+Si / 30+Mn / 20≦0.36 The above-mentioned relational expression 2 is a component relational expression for ensuring weldability and fusion zone hardness. If the value of Y is less than 0.25, the weld carbon equivalent is low and it is difficult to ensure the target fusion zone hardness, and if it exceeds 0.36, the fusion zone hardness is too high and brittle fracture may occur. Therefore, the value of Y is preferably in the range of 0.25 to 0.36. The lower limit of the value of the above-mentioned relational expression 2 is more preferably 0.26, and even more preferably 0.27. The upper limit of the value of the above-mentioned relational expression 2 is more preferably 0.35, and even more preferably 0.34.

[0028] [Relationship 3] 3420≦X / Y≦4360 The above-mentioned relational formula 3 is a component relational formula for simultaneously and stably securing the strength, weldability and fusion zone hardness targeted by the present invention. When the value of the above-mentioned X / Y is less than 3420, it is difficult to secure the strength targeted by the present invention due to insufficient hardening ability, and the weld carbon equivalent is high, so that brittle fracture of the weld zone may occur. On the other hand, when it exceeds 4360, the hardening ability is excessively high, and the hole expandability and bending properties are deteriorated due to a sudden increase in tensile strength, and the weld carbon equivalent is low, so that it is difficult to secure the targeted fusion zone hardness. Therefore, it is preferable that the value of the above-mentioned X / Y is in the range of 3420 to 4360. The lower limit of the value of the above-mentioned X / Y is more preferably 3440, and more preferably 3460. The upper limit of the value of the above-mentioned X / Y is more preferably 4340, and more preferably 4320.

[0029] The remaining component of the present invention is iron (Fe). However, in normal manufacturing processes, unintended impurities may be inevitably mixed in from raw materials or the surrounding environment, and this cannot be excluded. Since these impurities are known to anyone skilled in normal manufacturing processes, the contents of all of them are not specifically mentioned in this specification.

[0030] On the other hand, the above impurities may include one or more of P, S, Sb, N, Mg, Sn, Sb, Zn, and Pb as tramp elements, and the total amount of the tramp elements may be 0.1% by weight or less. The tramp elements are impurity elements derived from scraps and the like used as raw materials in the steelmaking process, and if the total amount of the tramp elements exceeds 0.1%, it may cause surface cracks in the slab and deteriorate the surface quality of the steel plate.

[0031] The cold rolled steel sheet according to an embodiment of the present invention preferably has a microstructure consisting of, in area %, 1 to 11% fresh martensite (hereinafter also referred to as "FM"), 80 to 97% of one or two of tempered martensite (hereinafter also referred to as "TM") and bainite (hereinafter also referred to as "B"), 1 to 9% of retained austenite (hereinafter also referred to as "RA"), and 7% or less (including 0%) of ferrite (hereinafter also referred to as "F"). If the FM fraction is less than 1% or the fraction of one or two of TM and B is less than 80%, it is difficult to ensure the strength targeted by the present invention. On the other hand, if the FM fraction exceeds 11% or the fraction of one or two of TM and B exceeds 97%, the elongation and bending properties may deteriorate. The RA must be 1.0% or more because it is advantageous in terms of ensuring elongation, but if it is less than 9%, it may be difficult to ensure strength. If the F fraction exceeds 7%, it may be difficult to ensure the strength targeted by the present invention.

[0032] The cold rolled steel sheet according to an embodiment of the present invention is characterized in that it contains at least one of MC, M (C, N) and their composite precipitates (M = Nb, Ti, Si, Cr, Mo, Fe) having an average size of 20 nm or less at a concentration of 50 particles / μm 2 The precipitates preferably have an average size of more than 20 nm or a fraction of 50 particles / μm 2If the average particle size is less than 15 nm, it is disadvantageous in terms of ensuring strength and bending properties. The size of the precipitates is more preferably 15 nm or less, and even more preferably 10 nm or less. The fraction of the precipitates is 75 particles / μm 2 More preferably, it is 100 particles / μm or more. 2 More preferably, it is equal to or greater than this.

[0033] The cold rolled steel sheet according to the embodiment of the present invention provided as described above has a yield strength (YS): 800 to 1200 MPa, a tensile strength (TS): 1180 to 1400 MPa, a total elongation (T-EL): 5% or more, a uniform elongation (U-EL): 3% or more, a yield ratio (YS / TS): 0.60 or more, and a hole expansion ratio (HER): 20% or more, and thus has excellent strength and formability. The yield strength (YS) is more preferably 850 to 1150 MPa, and even more preferably 850 to 950 MPa. The tensile strength (TS) is more preferably 1185 to 1380 MPa, and even more preferably 1190 to 1350 MPa. The total elongation (T-EL) is more preferably 6% or more, and even more preferably 7% or more. The uniform elongation (U-EL) is more preferably 4% or more, and even more preferably 5% or more. The yield ratio (YR, YS / TS) is more preferably 0.65 or more, and even more preferably 0.70% or more. The hole expansion ratio (HER, Hole Expansion Ratio) is more preferably 22% or more, and even more preferably 25% or more.

[0034] Meanwhile, the cold-rolled steel sheet of the present invention may have a plating layer formed on at least one surface. In the present invention, the type of the plating layer is not particularly limited, but may be, for example, a Zn-based plating layer. In order to use the cold-rolled steel sheet having the plating layer formed thereon as an automobile part, spot welding is generally performed. At this time, the alloying suppression layer formed on the GI steel sheet melts due to welding heat and generates liquid zinc. More specifically, during the spot welding, the welded part rises to about 1500°C or more within about 1 second, so that the base steel and the plating layer melt and are welded. At this time, the temperature of the plating layer rises to 600 to 800°C in the welding heat-affected zone (HAZ), which causes Fe to diffuse into the plating layer, so that a part of the plating layer is alloyed with an Fe-Zn alloy layer, and the rest becomes liquid zinc. The liquid zinc penetrates into the grain boundaries on the surface of the base steel sheet, and when tensile stress is applied to the HAZ at this time, cracks having a size of about tens to hundreds of μm are generated, causing brittle fracture. This is called liquid metal embrittlement (hereinafter, also referred to as "LME"). In the present invention, the average length of the LME cracks is 170 μm or less, and excellent LME resistance can be obtained. The average length of the LME cracks is more preferably 160 μm or less, and even more preferably 150 μm or less.

[0035] In addition, the cold-rolled steel sheet of the present invention may have a hardness (HvFZ) of 400 to 650Hv in the fusion zone. If the hardness of the fusion zone is less than 400Hv, sufficient hardness of the fusion zone cannot be ensured, and the strength of the welded zone may be reduced. On the other hand, if the hardness exceeds 650Hv, the hardness of the fusion zone is too high, and the sensitivity to crack generation increases, so that the strength of the welded zone and especially the impact absorption energy may be reduced. The hardness of the fusion zone is more preferably 420 to 630Hv, and even more preferably 450 to 600Hv.

[0036] Hereinafter, a method for producing a cold-rolled steel sheet according to one embodiment of the present invention will be described.

[0037] First, a slab satisfying the above-mentioned alloy composition and relational expressions 1 to 3 is heated. In the present invention, the slab heating temperature is not particularly limited, but for example, the slab can be heated at 1100 to 1300°C. If the slab heating temperature is less than 1100°C, there is a drawback such as rolling load during rough rolling, and if it exceeds 1300°C, there is a drawback such as coarsening of the microstructure and increased power costs. The lower limit of the slab heating temperature is more preferably 1125°C, and even more preferably 1150°C. The upper limit of the slab heating temperature is more preferably 1275°C, and even more preferably 1250°C. Meanwhile, the slab can have a thickness of 230 to 270 mm.

[0038] Thereafter, the heated slab is finish-rolled so that the finish rolling exit temperature (hereinafter also referred to as "FDT") is A3+50°C to A3+160°C to obtain a hot-rolled steel sheet. If the finish rolling exit temperature is less than A3+50°C, there is a high possibility that the hot deformation resistance will increase rapidly. If the finish rolling exit temperature exceeds A3+160°C, there is a high possibility that not only an excessively thick oxide scale will be generated but also the microstructure of the steel sheet will become coarse. Therefore, the finish rolling exit temperature is preferably in the range of A3+50°C to A3+160°C. The lower limit of the finish rolling exit temperature is more preferably A3+60°C, and even more preferably A3+70°C. The upper limit of the finish rolling exit temperature is more preferably A3+150°C, and even more preferably A3+140°C. Meanwhile, the A3 temperature can be calculated by the following formula 1.

[0039] [Formula 1] A3=910-203×C 1 / 2 +44.7×Si+31.5×Mo-30×Mn-11×Cr+400×Al+400×Ti

[0040] Thereafter, the hot-rolled steel sheet is cooled to Ms+100°C to Ms+300°C, and then coiled. If the coiling temperature (hereinafter also referred to as "CT") is less than Ms+100°C, martensite or bainite is excessively generated, which leads to an excessive increase in the strength of the hot-rolled steel sheet, and problems such as defective shape due to load during cold rolling may occur. On the other hand, if it exceeds Ms+300°C, the pickling property may deteriorate due to an increase in surface scale. Therefore, the coiling temperature is preferably in the range of Ms+100°C to Ms+300°C. The lower limit of the coiling temperature is more preferably Ms+120°C, and even more preferably Ms+150°C. The upper limit of the coiling temperature is more preferably Ms+280°C, and even more preferably Ms+260°C. On the other hand, in the present invention, the cooling step after the coiling is not particularly limited, but for example, the coiled hot-rolled steel sheet can be cooled to room temperature at a cooling rate of 0.1°C / s or less. On the other hand, the Ms temperature can be calculated by the following formula 2.

[0041] [Formula 2] Ms=539-423×C-30.4×Mn-7.5×Si+30×Al

[0042] Thereafter, the coiled hot-rolled steel sheet is cold-rolled to obtain a cold-rolled steel sheet. In the present invention, the reduction ratio during the cold rolling is not particularly limited, but for example, the cold rolling can be performed at a reduction ratio of 30 to 70%. If the cold rolling reduction ratio is less than 30%, the driving force for recrystallization is weak, and there is a high possibility that problems will occur in obtaining good recrystallized grains, and shape correction is extremely difficult. On the other hand, if it exceeds 70%, there is a high possibility that cracks will occur at the edge of the steel sheet, and the rolling load may increase rapidly. Therefore, it is preferable to perform the cold rolling at a reduction ratio of 30 to 70%. On the other hand, before the cold rolling, pickling can be performed to remove scale and impurities attached to the surface.

[0043] Thereafter, the cold-rolled steel sheet is subjected to continuous annealing at a continuous annealing temperature (hereinafter also referred to as "SS") in the range of 800 to 860°C. The continuous annealing is performed to form nearly 100% austenite by heating the steel sheet to the austenite single phase region, and to use it in the subsequent phase transformation. If the continuous annealing temperature is less than 800°C, sufficient recrystallization and austenite transformation are not performed, and therefore the martensite and bainite fractions that the present invention aims to obtain after annealing cannot be secured. On the other hand, if the continuous annealing temperature exceeds 860°C, the productivity decreases, coarse austenite is formed, and the material may deteriorate, and the surface quality such as peeling of the plated material is deteriorated. The lower limit of the continuous annealing temperature is more preferably 805°C, and more preferably 810°C. The upper limit of the continuous annealing temperature is more preferably 855°C, and more preferably 850°C.

[0044] On the other hand, the continuous annealing temperature is an extremely important factor in securing the strength targeted by the present invention, and precise control is required. Therefore, in the present invention, it is preferable to satisfy the following relational expression 4. If the SS-A3 value is 5°C or less, excessive ferrite transformation occurs and sufficient austenite transformation cannot be secured, and it is difficult to secure the targeted fractions of FM and T.M+B in the final microstructure, and therefore the targeted strength cannot be obtained. The following SS-A3 value is more preferably 10°C or more, even more preferably 15°C or more, and most preferably 30°C or more.

[0045] [Equation 4] SS-A3≧5℃

[0046] In the present invention, the atmosphere during the continuous annealing is not particularly limited, but for example, the continuous annealing can be performed in a gas atmosphere consisting of, by volume, 95% or more nitrogen and the remainder hydrogen. If the nitrogen fraction is less than 95%, and the hydrogen fraction is not increased accordingly, an oxidizing atmosphere is formed in the furnace, and oxides are formed on the steel sheet surface, which may deteriorate the surface quality, and if the hydrogen fraction is high, process difficulties such as explosion prevention may increase.

[0047] Then, the continuously annealed cold-rolled steel sheet is primarily cooled to a primary cooling finish temperature (SCS) of 450 to 650°C at an average cooling rate of less than 10°C / s. The primary cooling finish temperature can be defined as the point at which secondary cooling (quenching) is started by further applying a quenching equipment not applied in the primary cooling. In the present invention, the cooling process is divided into primary and secondary cooling and is performed stepwise, so that the temperature distribution of the steel sheet can be uniform in the slow cooling stage, and the final temperature and material variations can be reduced, and a desired phase can be obtained. If the primary cooling finish temperature exceeds 650°C, the cooling amount to the secondary cooling finish temperature becomes large, the steel sheet shape becomes poor, and the bainite fraction may be lower than the target level. Meanwhile, considering the length of the actual equipment, it is difficult to cool to less than 450°C at a cooling rate of less than 10°C / s, so the lower limit of the primary cooling finish temperature is preferably 450°C. If the cooling rate is 10° C. / s or more, the amount of cooling in the secondary cooling becomes large, and the final temperature variation and material variation increase.

[0048] Thereafter, the cold-rolled steel sheet subjected to the primary cooling is secondarily cooled to a secondary cooling finish temperature (RCS) of 300 to 390°C at an average cooling rate of 10°C / sec or more. The secondary cooling finish temperature is set so that the steel sheet is at or below the Ms temperature so that martensite transformation occurs during cooling, and this martensite finally becomes tempered martensite and bainite phase through a subsequent reheating step. Since the Ms temperature of most 1180 MPa class ultra-high strength steel sheets is at a level of 400°C or less, in the present invention, the secondary cooling finish temperature is controlled to a range of 300 to 390°C. If the secondary cooling finish temperature is less than 300°C, the amount of martensite transformation is too large, resulting in high strength, insufficient elongation, and too high yield strength, resulting in poor formability. On the other hand, if it exceeds 390°C, sufficient martensite transformation does not occur, making it difficult to obtain the target strength. If the secondary cooling rate is less than 10°C / s, even if the target secondary cooling end temperature is reached, high temperature phase transformation occurs during cooling, and the target martensite fraction and high strength cannot be obtained. The lower limit of the secondary cooling end temperature is more preferably 305°C, and even more preferably 310°C. The upper limit of the secondary cooling end temperature is more preferably 385°C, and even more preferably 380°C. The secondary cooling rate is more preferably 15°C / s or more, and even more preferably 20°C / s or more.

[0049] On the other hand, the secondary cooling end temperature is an extremely important factor in securing the strength targeted by the present invention, and precise control is required. Therefore, in the present invention, it is preferable to satisfy the following relational expression 5. If the Ms-RCS value is less than -30°C, sufficient martensite transformation does not occur, and bainite transformation increases, making it difficult to secure the targeted strength. On the other hand, if the Ms-RCS value exceeds 110°C, martensite is transformed excessively, which increases TM transformation during reheating, making it difficult to obtain the targeted yield strength. The lower limit of the Ms-RCS value below is more preferably -20°C, and even more preferably -10°C. The upper limit of the Ms-RCS value below is more preferably 105°C, and even more preferably 100°C.

[0050] [Equation 5] -30℃≧Ms-RCS≧110℃

[0051] As described above, the secondary cooling can further apply a quenching equipment that is not applied in the primary cooling, and the present invention does not particularly limit the type of the quenching equipment, but a preferred example is a hydrogen quenching equipment. More specifically, the hydrogen quenching equipment may be a gas atmosphere consisting of 50 to 80% hydrogen by volume and the remainder nitrogen. If the hydrogen fraction exceeds 80%, there is a drawback that it becomes difficult to manage the explosion control of the equipment, and if it is less than 50%, there is a drawback that it becomes difficult to utilize the efficient heat transfer characteristics of hydrogen, which is a light element.

[0052] Then, the second-cooled cold-rolled steel sheet is reheated at a reheating temperature (RHS) range of 400 to 540°C. Through the above process, interphase carbon partitioning and additional bainite phase transformation necessary for stabilizing the retained austenite are obtained. In the present invention, the end temperature of the heating section is conveniently referred to as the reheating temperature (hereinafter also referred to as "RHS"). If the reheating temperature is less than 400°C, the martensite generated during the primary cooling is not tempered, and the strength becomes too high, resulting in poor elongation. On the other hand, if the reheating temperature exceeds 540°C, excessive tempering or bainite transformation occurs during reheating, which may make it difficult to ensure the target strength. The lower limit of the reheating temperature is more preferably 410°C, and more preferably 420°C. The upper limit of the cooling end temperature is more preferably 530°C, and more preferably 520°C.

[0053] On the other hand, the reheating temperature is an extremely important factor in ensuring the strength targeted by the present invention, and precise control is required. Therefore, in the present invention, it is preferable to satisfy the following relational expression 6. When the value of the following RHS-RCS is less than -30 ° C, excessive martensitic transformation occurs, and the strength increases significantly, resulting in deterioration of hole expandability and bending properties. On the other hand, when the value of the RHS-RCS exceeds 250 ° C, excessive tempering may make it difficult to ensure the target tensile strength. The lower limit of the following RHS-RCS value is more preferably -25 ° C, and even more preferably -20 ° C. The upper limit of the following RHS-RCS value is more preferably 240 ° C, and even more preferably 230 ° C.

[0054] [Equation 6] -30℃≧RHS-RCS≧250℃

[0055] Meanwhile, in the present invention, after the reheating step, the cold-rolled steel sheet may further include a step of hot-dipping the cold-rolled steel sheet in a coating bath at 430 to 490 ° C. If the hot-dipping temperature is less than 430 ° C, it is difficult to ensure uniform coating quality due to the low coating temperature, and if it exceeds 490 ° C, the coating amount becomes excessive, which deteriorates weldability during resistance spot welding, and in particular increases the risk of LME (Liquid Metal Embrittlement) occurring. The lower limit of the hot-dipping temperature is more preferably 435 ° C, and more preferably 440 ° C. The upper limit of the hot-dipping temperature is more preferably 485 ° C, and more preferably 470 ° C. In the present invention, the type of the hot-dipping is not particularly limited, but for example, the hot-dipping may be hot-dipping galvanizing. In addition, in the present invention, after the reheating, the cold-rolled steel sheet may be hot-dipped as it is, or may be cooled to room temperature and then reheated to be hot-dipped.

[0056] In addition, the present invention may further include a step of temper rolling the cold-rolled steel sheet at a rolling reduction of less than 2% after the hot-dip coating. The temper rolling is for correcting the shape of the steel sheet and adjusting the yield strength. The temper rolling can be performed after cooling to room temperature after the hot-dip coating. EXAMPLES

[0057] The present invention will be described in more detail with reference to the following examples. However, it should be noted that the following examples are intended to illustrate and embody the present invention, and are not intended to limit the scope of the present invention, since the scope of the present invention is determined by the matters described in the claims and matters reasonably inferred therefrom.

[0058] Example 1 Molten steel having the alloy composition shown in Table 1 below was prepared, and then continuously cast to produce a slab with a thickness of 250 mm. The slab was heated at 1200°C for 12 hours, and then hot-rolled and coiled under the conditions shown in Table 2 below to obtain a hot-rolled steel sheet with a thickness of 3.0 mm. The hot-rolled steel sheet was then pickled and cold-rolled at a cold reduction of 50% to obtain a cold-rolled steel sheet with a thickness of 1.5 mm. The cold-rolled steel sheet was then subjected to continuous annealing, primary cooling, secondary cooling, and reheating under the conditions shown in Tables 2 and 3 below. At this time, the gas used during the continuous annealing was 95% by volume N-5% by volume H, and the gas used during the secondary cooling was 75% by volume H-25% by volume N. The microstructure, precipitates, and mechanical properties of the cold-rolled steel sheet produced in this manner were measured, and the results are shown in Tables 4 and 5 below. Additionally, the cold rolled steel sheets were hot-dip galvanized at the hot-dip galvanizing bath temperatures shown in Table 3 below to form a coating layer, and then welded. The hardness of the molten zone and the average length of LME cracks were measured, and the results are shown in Table 5 below. At this time, the welding method used in the above welding was BOP (Bead On Plate) welding under the conditions of 6 kW-3 min using a CO2 laser welder.

[0059] Tensile strength (TS), yield strength (YS), yield ratio (YR), total elongation (T-EL) and uniform elongation (U-EL) were measured through tensile tests in the horizontal rolling direction, with a gauge length of 50 mm and a tensile specimen width of 15 mm. Hole expansion was measured according to the ISO 16330 standard, and the holes were sheared using a 10 mm diameter punch with a clearance of 12%.

[0060] The fraction of the microstructure was measured using electron backscatter diffraction (EBSD) and XRD. Samples of the precipitates were prepared by the replica method and observed with a transmission electron microscope (TEM). In the present invention, however, since it is difficult to distinguish between TM and B, the fraction was shown as the sum of their fractions.

[0061] The hardness of the fusion zone was calculated as the average value after five measurements were made at 1 / 4t (t = steel plate thickness) under a load of 500 gf using a Vickers hardness tester.

[0062] The average length of the LME cracks was measured using an optical microscope after stacking two sheets of steel material (applicable material) corresponding to the invention example or comparative example and mild steel plated material (thickness: 2 mm) in sequence, tilting by 5°, and then performing resistance spot welding under ISO18278-2 (2016) conditions (Force: 4.5KN, Welding time: 380ms, Welding Current: Explosion current -0.2kA, Holding time: 260ms). The length of the LME cracks was calculated by measuring 10 welded test pieces and taking the average value.

[0063] [Table 1]

[0064] [Table 2]

[0065] [Table 3]

[0066] [Table 4]

[0067] [Table 5]

[0068] As shown in Tables 1 to 5 above, in the case of Examples 1 to 5 which satisfy the alloy compositions, Relational Formulas 1 to 3, and manufacturing conditions proposed by the present invention, it can be seen that the microstructure, precipitates, average length of LME cracks, and mechanical properties that the present invention aims to obtain are secured.

[0069] In contrast, in the case of Comparative Examples 1 to 5, which do not satisfy the alloy compositions or Relational Formulas 1 to 3 proposed by the present invention, it is found that the microstructure, precipitates, average length of LME cracks, and mechanical properties that the present invention aims to obtain are not secured.

[0070] Figure 2 is a SEM photograph of Example 1, and Figure 3 is a TEM photograph of Example 1. As shown in Figures 2 and 3, Example 1 not only has the composite structure that the present invention aims to obtain, but also has fine precipitates having an average size of several nm that are uniformly distributed.

[0071] Figure 4 is a photograph of the cross section of the weld after LME evaluation for Example 3. As shown in Figure 4, in the case of Example 3, it can be seen that the average length of the LME cracks is about 45 µm.

[0072] Example 2 In Example 1, molten steel having the alloy composition of Invention Steels 1 and 3 was prepared, and then continuous casting was performed to produce a slab having a thickness of 250 mm. The slab was heated at 1200°C for 12 hours, and then hot-rolled and coiled under the conditions shown in Table 2 below to obtain a hot-rolled steel sheet having a thickness of 3.0 mm. The hot-rolled steel sheet was then pickled and cold-rolled at a cold reduction rate of 50% to obtain a cold-rolled steel sheet having a thickness of 1.5 mm. The cold-rolled steel sheet was then subjected to continuous annealing, primary cooling, secondary cooling, and reheating under the conditions shown in Tables 6 and 7 below. At this time, the gas used during the continuous annealing was 95% by volume N-5% by volume H, and the gas used during the secondary cooling was 75% by volume H-25% by volume N. The microstructure, precipitates, and mechanical properties of the cold-rolled steel sheet produced in this manner were measured, and the results are shown in Tables 8 and 9 below. Additionally, the cold rolled steel sheets were hot-dip galvanized at the hot-dip galvanizing bath temperatures shown in Table 3 below to form a coating layer, and then welded. The hardness of the molten zone and the average length of LME cracks were measured, and the results are shown in Table 9 below. At this time, the welding method used in the above welding was BOP (Bead On Plate) welding under the conditions of 6 kW-3 min using a CO2 laser welder.

[0073] The microstructure, precipitates, average LME crack length and mechanical properties were measured under the conditions described in Example 1.

[0074] [Table 6]

[0075] [Table 7]

[0076] [Table 8]

[0077] [Table 9]

[0078] As shown in Tables 6 to 9 above, in the case of Examples 6 to 10, which satisfy the alloy compositions, Relational Formulas 1 to 3, and manufacturing conditions proposed by the present invention, it can be seen that the microstructure, precipitates, average length of LME cracks, and mechanical properties that the present invention aims to obtain are secured.

[0079] In contrast, in the case of Comparative Examples 6 to 14, which satisfy the alloy composition and Relational Formulas 1 to 3 proposed by the present invention but do not satisfy the manufacturing conditions, it is found that the microstructure and mechanical properties that the present invention aims to obtain are not secured.

Claims

1. The composition is expressed by weight as follows: C: 0.10-0.20%, Si: 0.05-0.495%, Al: 0.01-0.18%, Mn: 2.4-3.5%, Cr: 0.05-0.8%, Mo: 0.05-0.8%, B: 0.0001-0.003%, Nb: 0.005-0.07%, Ti: 0.005-0.07%, the balance being Fe and other unavoidable impurities; The following relations 1 to 3 are satisfied, A microstructure having, in area percentages, 1 to 11% fresh martensite, 80 to 97% of one or two of tempered martensite and bainite, 1 to 9% retained austenite, and 7% or less (including 0%) ferrite, 50 particles / μm of one or more of MC, M(C, N) and their composite precipitates (M=Nb, Ti, Si, Cr, Mo, Fe) with an average size of 20 nm or less 2 Cold rolled steel sheet including above. [Relationship 1] 1120≦X=2301×C+287×Mn+1533×Nb+228×Cr−71×Si−84.1×Al≦1380 [Relationship 2] 0.25≦Y=C+Si / 30+Mn / 20≦0.36 [Relationship 3] 3420≦X / Y≦4360 (However, in the above Relational Formulas 1 to 3, the content of each alloy element is expressed in weight percent.)

2. The cold-rolled steel sheet according to claim 1, wherein the impurities include one or more of P, S, Sb, N, Mg, Sn, Sb, Zn, and Pb as tramp elements, and the total amount thereof is 0.1 wt% or less.

3. The cold-rolled steel sheet has a yield strength (YS): 800 to 1200 MPa, a tensile strength (TS): 1180 to 1400 MPa, a total elongation (T-EL): 5% or more, a uniform elongation (U-EL): 3% or more, a yield ratio (YS / TS): 0.60 or more, and a hole expansion ratio (HER): 20% or more. The cold-rolled steel sheet according to claim 1.

4. The cold-rolled steel sheet according to claim 1 , wherein the cold-rolled steel sheet has a plating layer formed on at least one surface thereof.

5. The cold-rolled steel sheet according to claim 4, wherein the cold-rolled steel sheet has an average length of LME cracks of 170 μm or less.

6. The cold-rolled steel sheet according to claim 4, wherein the cold-rolled steel sheet has a hardness (HvFZ) of a fusion zone of 400 to 650 Hv.

7. a step of heating a slab containing, in weight percent, 0.10-0.20% C, 0.05-0.495% Si, 0.01-0.18% Al, 2.4-3.5% Mn, 0.05-0.8% Cr, 0.05-0.8% Mo, 0.0001-0.003% B, 0.005-0.07% Nb, 0.005-0.07% Ti, the balance being Fe and other inevitable impurities, and satisfying the following relations 1 to 3; The heated slab is subjected to finishing rolling at a temperature of A 3 +50℃~A 3 A step of finish rolling to obtain a hot-rolled steel sheet at +160°C; cooling the hot-rolled steel sheet to Ms+100°C to Ms+300°C and then coiling it; cold rolling the coiled hot-rolled steel sheet to obtain a cold-rolled steel sheet; Continuously annealing the cold-rolled steel sheet at a continuous annealing temperature (SS) range of 800 to 860°C; subjecting the continuously annealed cold-rolled steel sheet to a primary cooling finish temperature (SCS) of 450 to 650° C. at an average cooling rate of less than 10° C. / s; Secondarily cooling the primarily cooled cold-rolled steel sheet to a secondary cooling finish temperature (RCS) of 300 to 390° C. at an average cooling rate of 10° C. / sec or more; and reheating the second-cooled cold-rolled steel sheet at a reheating temperature (RHS) range of 400 to 540° C.; The method for producing a cold-rolled steel sheet satisfies the following Relational Formulas 4 to 6 during the continuous annealing, secondary cooling, and reheating. [Relationship 1] 1120≦X=2301×C+287×Mn+1533×Nb+228×Cr−71×Si−84.1×Al≦1380 [Relationship 2] 0.25≦Y=C+Si / 30+Mn / 20≦0.36 [Relationship 3] 3420≦X / Y≦4360 [Relationship 4] SS-A 3 ≧5℃ [Relationship 5] -30°C ≧ Ms-RCS ≧ 110°C [Relationship 6] -30°C ≧ RHS - RCS ≧ 250°C (However, in the above Relational Formulas 1 to 3, the content of each alloy element is expressed in weight percent.)

8. The method for producing a cold-rolled steel sheet according to claim 7, wherein the slab contains one or more of P, S, Sb, N, Mg, Sn, Sb, Zn and Pb as tramp elements, and the total amount thereof is 0.1 wt% or less.

9. The method for producing a cold rolled steel sheet according to claim 7, wherein the slab is heated at 1100 to 1300°C.

10. The method for producing a cold-rolled steel sheet according to claim 7, wherein the cold rolling is performed at a rolling reduction of 30 to 70%.

11. The method for producing a cold-rolled steel sheet according to claim 7, wherein the continuous annealing is performed in a gas atmosphere containing, by volume%, 95% or more of nitrogen and the remainder hydrogen.

12. The method for producing a cold-rolled steel sheet according to claim 7, wherein the secondary cooling is performed in a hydrogen quenching facility in a gas atmosphere containing, by volume, 50 to 80% hydrogen and the remainder nitrogen.

13. The method for producing a cold-rolled steel sheet according to claim 7, further comprising the step of hot-dip galvanizing the cold-rolled steel sheet in a galvanizing bath at 430 to 490°C after the reheating step.

14. The method for producing a cold rolled steel sheet according to claim 13, further comprising the step of temper rolling the cold rolled steel sheet at a reduction of less than 2% after the hot dip coating.

Citation Information

Patent Citations

  • 1300 Mpa-grade complex-phase steel, and preparation method and application thereof

    CN111647732A

  • High strength thin steel sheet excellent in hydrogen embitterment resistance and its manufacturing method

    JP2005068548A

  • High strength steel sheet excellent in formability and production method therefor

    JP2016216808A

  • High-strength hot-dip galvanized steel sheet with excellent surface quality and spot weldability, and its manufacturing method

    JP2019504196A

  • High-strength thin steel sheet and method for manufacturing the same

    JP2021025094A