A method for producing oxidation-resistant base metals and alloys by using high-temperature sintering under air
By using base metal conductors and alloys with added aluminum powder to sinter under air, the method addresses high costs and oxidation issues, ensuring excellent electrical properties and preventing shrinkage mismatch in ceramic elements.
Patent Information
- Application Number
- JP2023568174
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2022-08-11
- Publication Date
- 2024-11-19
- Estimated Expiration
- 2042-08-11
AI Technical Summary
Existing thick film printed conductor technologies face high costs due to the need for precious metals or require reducing atmospheres for base metals, leading to oxidation and property loss, and mismatched shrinkage during co-firing of ceramic embryos and electrodes.
Use of base metal conductors and alloys with added aluminum powder to sinter under air, leveraging aluminum's oxidizing and reducing properties to prevent oxidation and maintain electrical properties, and employ a sintering technique that avoids shrinkage mismatch.
Achieves cost-effective production of base metal electrodes and alloys with excellent electrical properties, reducing material costs and eliminating the need for additional equipment, while maintaining conductivity and preventing shrinkage mismatch.
Smart Images

Figure 2024542902000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for producing oxidation-resistant base metals and alloys by utilizing high-temperature sintering under air, and in particular to a base metal thick-film printed conductor or alloy technology that uses high-temperature sintering under air, and more particularly to a base metal or alloy that not only does not oxidize but also maintains excellent electrical properties even when sintered under air. [Background technology]
[0002] Existing thick film printed conductor paste technology has the following problems.
[0003] 1. Thick Film Printing The precious metals silver and silver-palladium alloys can be subjected to high-temperature heat treatment in air, but precious metals and alloy materials that can be sintered at high temperatures in air and are resistant to oxidation are very expensive.
[0004] 2. When using nickel or copper-nickel alloys instead of the base metal copper or the precious metal silver or silver-palladium alloys in thick film printing, if heat treatment is not performed by high-temperature sintering under a reducing atmosphere (nitrogen or nitrogen-hydrogen mixture), the base metals copper and nickel or copper-nickel alloys will oxidize and lose their properties. Therefore, the material can be changed from a precious metal to a base metal to reduce costs, but in the heat treatment process, the atmosphere must be changed from air sintering to a reducing atmosphere for sintering, which increases the cost of the sintering process.
[0005] 3. There are some base metal materials that cannot be subjected to high temperature heat treatment even in a reducing atmosphere. For example, when resistance alloy materials are used as chip resistors, or when they are used as electrodes in ceramic thermistors or induction magnetometers, manganese copper alloys and nickel-chromium alloys are used. When the original ceramic elements are sintered in a reducing atmosphere, their properties change, so when these parts are manufactured, they must be sintered by heat treatment in air.
[0006] In order to overcome the above drawbacks, the inventors have conducted careful research and, by utilizing scientific theory, have proposed the present invention, which can effectively overcome the above drawbacks and has a rational design. DISCLOSURE OF THEINVENTION [Problem to be solved by the invention]
[0007] The existing prior art has the following drawbacks:
[0008] 1. In the existing technology, the conductive paste film of base metals, such as copper, nickel, and copper-nickel alloys, must be sintered by heat treatment under a reducing atmosphere, such as nitrogen or nitrogen-hydrogen mixture, which causes the base metals copper and nickel or copper-nickel alloys to lose their effectiveness due to oxidation. Although base metals and alloys are inexpensive, the process cost is significantly increased when sintering by heat treatment under a reducing atmosphere.
[0009] 2. Existing multilayer ceramic devices have a shrinkage mismatch problem when ceramic embryos and electrodes are co-fired, and existing technologies use sintering technology that can suppress shrinkage in both X and Y axes when co-firing by covering a non-shrink ceramic embryo with a higher temperature than the co-fired ceramic embryo or by inserting another ceramic embryo with a lower temperature than the co-fired ceramic embryo to reduce the mismatch problem when ceramic embryos and electrodes are co-fired. However, this extra step increases the manufacturing cost.
[0010] 3. In the case of existing ceramic elements, when external electrodes are made on the sintered ceramic body, the properties of the sintered ceramic body change when the external electrodes are sintered in a reducing atmosphere. For example, the properties of chip resistors, negative temperature coefficient (NTC) thermistors, positive temperature coefficient (PTC) thermistors, voltage dependent resistors (VDR) and piezoelectrics (PZT) change. Therefore, it is not possible to use nitrogen sintering of copper electrodes.
[0011] 4. Existing chip alloy resistors have a very low temperature coefficient of resistance, and their manufacturing method is mainly to first print a positive electrode paste on both ends of a substrate 61, then print a resistance alloy paste, and then fabricate precious metal silver electrodes 62, 63 and a silver-palladium resistance alloy layer 64 by air sintering (e.g., 850°C), as shown in Fig. 18, or fabricate by sintering base metal copper electrodes and a copper-nickel resistance alloy layer in a reducing atmosphere using nitrogen (or nitrogen and hydrogen). However, although the precious metal silver-palladium is expensive and the base metal copper-nickel alloy is inexpensive, the sintering heat treatment in a reducing atmosphere prevents oxidation, and the process cost is significantly increased.
[0012] As the price of precious metal raw materials increases, it is possible to use base metal raw materials, which are abundant in ore reserves, instead, but the existing method of sintering base metals and alloys in a reducing atmosphere to produce conductive paste films for thick film printing does not meet the technical and market needs. Therefore, an invention is needed that can improve the shortcomings of the existing technology and avoid the high cost of precious metal materials. [Means for solving the problem]
[0013] The main object of the present invention is to provide a method that can solve the above-mentioned problems of the conventional technology, can change existing thick-film printed electrode materials from precious metals to base metals, and can utilize base metals and alloys, which are very inexpensive materials, and can sinter base metal electrodes and alloys at high temperatures under air using a low-cost process that not only does not oxidize but also maintains excellent electrical properties even when sintered at high temperatures under air, thereby significantly reducing material costs, and does not require any additional equipment.
[0014] In order to achieve the above object, the present invention provides a method for sintering base metal electrodes or alloys at high temperatures under air, by adding 10 to 90 wt % of metallic aluminum powder to a thick-film printed base metal conductor paste or base metal alloy paste, and carrying out a heat treatment at 500 to 1400°C under air, utilizing the highly aerobic nature of the metallic aluminum powder to avoid oxidation of the base metal conductor paste or base metal alloy paste due to sintering under high-temperature air, or after the base metal conductor paste or base metal alloy paste is sintered and oxidized under high-temperature air, the strong reducing properties of the metallic aluminum powder are used to reduce the oxidized base metal conductor paste or base metal alloy paste to a metal or alloy, thereby obtaining a thick-film base metal electrode film or alloy film.
[0015] According to an embodiment of the present invention, the base metal conductor paste is one of metallic copper powder and nickel powder.
[0016] According to an embodiment of the present invention, the base metal alloy paste is one of copper-nickel alloy powder, manganese-copper powder, or nickel-chromium powder.
[0017] According to an embodiment of the present invention, the thick base metal electrode film or alloy film is applied to external electrodes of bulk ceramic elements, internal electrodes of multilayer ceramic elements, chip resistor electrodes, and alloy chip resistors.
[0018] According to an embodiment of the present invention, the bulk ceramic element is a GPS ceramic antenna, a Negative Temperature Coefficient (NTC) thermistor, a Positive Temperature Coefficient (PTC) thermistor, a Voltage Dependent Resistor (VDR), or a safety capacitor.
[0019] According to an embodiment of the present invention, the multilayer ceramic element is a Low Temperature Co-fired Ceramic (LTCC), a multilayer ceramic capacitor (MLCC), a multilayer NTC component, a multilayer VDR component, or a multilayer piezoelectric component.
[0020] At the same time, the present invention also provides another method, in which a single layer of thick-film aluminum conductor paste film is printed on the upper surface of a base metal conductor paste film or a base metal alloy paste film produced by thick-film printing, and then heat-treated under air at 500 to 1400°C, and the highly aerobic nature of the aluminum conductor paste film is utilized to protect the base metal conductor paste film or the base metal alloy paste film from oxidation when sintered under high-temperature air, or the base metal conductor paste film or the base metal alloy paste film is sintered and oxidized under high-temperature air, and then the strongly reducing property of the aluminum conductor paste film is utilized to reduce the oxidized base metal conductor paste film or the base metal alloy paste film to a metal or alloy, thereby obtaining a thick-film base metal electrode film or alloy film.
[0021] According to an embodiment of the present invention, the base metal conductor paste film is one of a metallic copper film and a nickel film.
[0022] According to an embodiment of the present invention, the base metal alloy paste film is one of an alloy copper-nickel film, a manganese-copper film, or a nickel-chromium film.
[0023] According to an embodiment of the present invention, the thick base metal electrode film or alloy film is applied to external electrodes of bulk ceramic elements, internal electrodes of multilayer ceramic elements, chip resistor electrodes, and alloy chip resistors.
[0024] According to an embodiment of the present invention, the thick base metal electrode film or alloy film can be applied to a new alloy chip resistor process, in which the aluminum layer located in the middle for protection is removed by laser engraving to expose the resistive alloy layer, and the aluminum layer at both ends that is not removed by laser engraving is used as the terminal electrodes of the alloy chip resistor.
[0025] According to an embodiment of the present invention, the bulk ceramic element is a GPS ceramic antenna, an NTC thermistor, a PTC thermistor, a VDR, or a safety capacitor.
[0026] According to an embodiment of the present invention, the multilayer ceramic element is a LTCC or MLCC, a multilayer NTC component, a multilayer VDR component, or a multilayer piezoelectric component.
[0027] Hereinafter, the features and technical contents of the present invention will be described in detail with reference to the drawings. However, these drawings are for reference and explanation only, and the present invention is not limited thereto. BEST MODE FOR CARRYING OUT THEINVENTION
[0028] 1 to 14 are respectively a graph showing the change in weight with increasing temperature in thermal analysis when copper is added to the aluminum of the present invention, a graph showing the change in weight with increasing temperature in thermal analysis when nickel is added to the aluminum of the present invention, a sintered microstructure diagram when copper is added to the aluminum of the present invention, a sintered microstructure diagram when nickel is added to the aluminum of the present invention, a sintered aluminum alloy microstructure diagram when nickel is added to the aluminum of the present invention, a sintered microstructure diagram when a copper film is coated on the aluminum film of the present invention, a sintered microstructure diagram when a nickel film is coated on the aluminum film of the present invention, and an aluminum alloy of the present invention. a microstructural diagram of sintering when a copper-nickel film is coated on an aluminum film of the present invention, a microstructural diagram of sintering when a manganese-copper film is coated on an aluminum film of the present invention, a structural conceptual diagram of an external electrode of a bulk ceramic element produced by the new process of the present invention, a structural conceptual diagram of a non-shrinking internal electrode of a multilayer ceramic element produced by the new process of the present invention, a structural conceptual diagram of a non-shrinking laminated internal electrode of a multilayer ceramic element produced by the new process of the present invention, a structural conceptual diagram of a chip resistor electrode produced by the new process of the present invention, and a structural conceptual diagram of a chip resistor alloy produced by the new process of the present invention.As shown in the figure, the method of the present invention for producing oxidation-resistant base metals and alloys by using high-temperature sintering under air is to add 10 to 90 wt% of metallic aluminum powder to a thick-film printing base metal conductor paste or base metal alloy paste, or to print a single layer of thick-film aluminum conductor paste film on the top surface of a thick-film printing base metal conductor paste film or base metal alloy paste film, and then heat-treat at 500 to 1400°C under air, utilizing the highly aerobic and strongly reducing properties of the aluminum used, and the highly aerobic and strongly reducing properties of the metallic aluminum powder are used to produce base metal conductors and alloys. By avoiding oxidation of base metal alloys by sintering under high-temperature air, or by utilizing the strong reducing properties of the metallic aluminum powder after sintering and oxidizing the base metal conductors or base metal alloys under high-temperature air, the oxidized base metal conductors or base metal alloys are reduced to metals or alloys to obtain thick base metal electrode films or alloy films, thereby allowing the base metal conductors (e.g., copper and nickel) and base metal alloys (e.g., copper-nickel alloys), which are easily oxidized by high-temperature sintering under the original air, to maintain their metal conductivity and alloy properties.
[0029] The present invention will be described below with reference to examples, but the present invention is not limited thereto.
[0030] In the following Tables 1, 2 and 3, metallic aluminum powder is added to metallic copper powder, metallic nickel powder or copper-nickel alloy powder to prepare a thick film paste, and a thick film is formed by screen printing. This results in the resistance value and resistance characteristics when sintered by heat treatment at 500 to 900°C under air.
[0031] [Table 1]
[0032] As can be seen from Table 1, the antioxidant ability of the metallic copper powder during heat treatment increases with the amount of metallic aluminum powder added. When 40 wt% metallic aluminum powder is added to 60 wt% metallic copper powder, the copper-aluminum mixed conductor paste can maintain high conductivity even when sintered at 900°C under air.
[0033] [Table 2]
[0034] As can be seen from Table 2, the heat treatment resistance of the metallic nickel powder increases with the amount of metallic aluminum powder added. When 50 wt% metallic aluminum powder is added to 50 wt% metallic nickel powder, the nickel-aluminum mixed conductor paste can maintain high conductivity even when sintered at 900°C under air.
[0035] [Table 3]
[0036] As can be seen from Table 3, the copper-nickel alloy powder has stronger oxidation resistance during heat treatment as the amount of metallic aluminum powder added increases. Among them, when 40wt% metallic aluminum powder is added to 60wt% copper-nickel alloy powder, or when 30wt% metallic aluminum powder is added to 70wt% copper-nickel alloy powder, the copper-nickel alloy aluminum mixed resistor paste can maintain excellent resistance properties even when sintered at 500-900℃ under air, and can also achieve a low temperature coefficient of resistance (TCR), i.e., TCR<±100ppm.
[0037] [Table 4]
[0038] As can be seen from Table 4, electrical properties are obtained when a thick-film printed metallic aluminum film is coated on a thick-film printed metallic copper film, metallic nickel film, copper-nickel alloy, manganese copper, or nickel-chromium film, and then heat-treated and sintered under air at 700 to 900°C. The metallic copper film or metallic nickel film coated with the metallic aluminum film maintains an extremely low resistance value, and the copper-nickel alloy film coated with the metallic aluminum film has an extremely low resistance temperature characteristic (TCR<±100ppm), i.e., very excellent resistance characteristics. The resistance value is equivalent to that of an existing, general, thick-film printed metallic copper film, metallic nickel film, or copper-nickel alloy film sintered under a reducing atmosphere (nitrogen or nitrogen-hydrogen mixture), and the resistance characteristics include a low temperature coefficient of resistance.
[0039] As can be seen from the thermogravimetric analysis (TGA) of the 50wt% copper plus 50wt% aluminum mixed paste as a function of temperature in Figure 1, the weight of the sample hardly changes up to 1000°C, which means that the copper can be sintered under air, protected by the highly aerobic aluminum powder.
[0040] As can be seen from the thermogravimetric analysis of 50wt% nickel plus 50wt% aluminum mixed paste with temperature change in Figure 2, the weight of the sample hardly changes until the temperature reaches 1000°C, which means that the nickel can be sintered under air, protected by the highly aerobic aluminum powder.
[0041] Figure 3 shows the microstructure when metallic aluminum powder is added to metallic copper powder and sintered under air at a temperature of 850°C / min. Due to the presence of highly aerobic aluminum metal powder, copper can maintain its high metallic conductivity even when sintered at high temperature under air.
[0042] Figure 4 shows the microstructures of the nickel metal powder sintered at 850℃ / min under air after adding aluminum metal powder in different ratios. Due to the presence of highly aerobic aluminum metal powder, the nickel aluminum alloy or nickel metal formed can maintain the high conductive properties of the metal even after high temperature sintering under air.
[0043] Figure 5 shows the microstructure when metallic aluminum powder is added to copper-nickel alloy powder and sintered under air at a temperature of 850°C / min. Due to the presence of highly aerobic aluminum metal powder, the copper-nickel alloy can maintain its high electrical conductivity even when sintered at high temperature under air.
[0044] Figure 6 shows the microstructure of a printed copper metal film coated with an aluminum film and sintered at 850°C under air. Because of the presence of the aluminum metal film with high aerobic and strong reducing properties, the lower copper metal film can maintain its high metal conductivity even when sintered at high temperature under air.
[0045] Figure 7 shows the microstructure after an aluminum film is printed on top of the printed metallic nickel film and sintered at 850°C under air. Because the aluminum metal film has high aerobic and strong reducing properties, the metallic nickel film can maintain its high conductive properties even when sintered at high temperatures under air.
[0046] FIG. 8 shows the microstructure of the printed copper-nickel metal film after an aluminum film is printed on top of it and sintered at 850°C under air. Due to the presence of the aluminum metal film with high aerobic and strong reducing properties, the copper-nickel alloy film can maintain the excellent resistance properties of the alloy even after high-temperature sintering under air.
[0047] FIG. 9 shows the microstructure of a printed manganese copper alloy film coated with an aluminum film and sintered at 850°C under air. Due to the presence of the aluminum metal film with high aerobic and strong reducing properties, the manganese copper alloy film can maintain the excellent resistance properties of the alloy even when sintered at high temperature under air.
[0048] [Example 1] According to the present invention, the novel process can be applied to the external electrodes of bulk ceramic elements, such as GPS ceramic antennas, Negative Temperature Coefficient (NTC) thermistors, Positive Temperature Coefficient (PTC) thermistors, Voltage Dependent Resistors (VDR), or safety capacitors, as shown in FIG. 10.
[0049] In the present invention, copper aluminum (or nickel aluminum) is mixed to prepare a conductive paste, which is then printed on both sides of a bulk ceramic element 11 to form copper aluminum (or nickel aluminum) electrodes 12 as external electrodes, so that a heat treatment at 500 to 1000°C can be performed under air, as shown in FIG. 10(a).
[0050] Furthermore, according to the present invention, a copper (or nickel) electrode 13 is printed on each side of the bulk ceramic element 11, and an aluminum electrode 14 is printed on the copper (or nickel) electrode 13. Then, a heat treatment is performed at 500 to 1000°C under air, so that the copper (or nickel) electrode 13 on the lower side is protected by the aluminum electrode 14 on the upper side, thereby preventing oxidation, as shown in Figure 10(b).
[0051] [Example 2] According to the present invention, the novel process can be applied to the internal electrodes of multilayer ceramic elements, such as low temperature co-fired ceramics (LTCC), multilayer ceramic capacitors (MLCC), multilayer NTC components, multilayer VDR components, or multilayer piezoelectric components, as shown in Figs. 11 and 12.
[0052] 1. In the case of multilayer ceramic co-firing parts, if the sintering temperature is less than 1050°C, a copper thick film conductor paste mixed with 10 to 90 wt% aluminum powder can be used to print a copper aluminum electrode 22 as an internal electrode, and the product can be co-fired with the ceramic embryo 21 under air, resulting in an LTCC like that shown in Figure 11(a); if the sintering temperature is between 1050°C and 1450°C, a nickel or nickel copper thick film conductor paste mixed with 10 to 90 wt% aluminum powder can be used to print a nickel aluminum electrode 23 as an internal electrode, and the product can be co-fired with the ceramic embryo 21 under air, resulting in an MLCCD like that shown in Figure 11(b).
[0053] 2. The laminated ceramic co-fired part is produced by first printing a layer of copper thick-film conductor paste film at a sintering temperature of <1050°C, then printing a layer of thick-film aluminum conductor paste film, and co-firing the copper electrode 24 and aluminum electrode 25 layers as internal electrodes with the ceramic embryo 21 under air to produce an LTCC as shown in Figure 12(a). If the sintering temperature is between 1050 and 1450°C, first forming a layer of nickel (or copper-nickel) thick-film conductor paste film, then printing a layer of thick-film aluminum conductor paste film, and then co-firing the nickel (or copper-nickel) electrode 26 and aluminum electrode 27 layers as internal electrodes with the ceramic embryo 21 under air to produce an MLCC as shown in Figure 12(b).
[0054] 3. The laminated ceramic co-fired part is produced by first printing a layer of copper thick film conductor paste film at a sintering temperature of less than 1050°C, and then co-firing the three layers of copper electrode 24, aluminum electrode 25, and copper electrode 24 as internal electrodes with ceramic embryo 21 under air to produce an LTCC as shown in FIG. 12(c). If the sintering temperature is between 1050 and 1450°C, first forming a layer of nickel (or copper-nickel) thick film conductor paste film, printing a layer of thick film aluminum conductor paste film, and finally printing a layer of nickel (or copper-nickel) thick film conductor paste film, and then co-firing the three layers of nickel (or copper-nickel) electrode 26, aluminum electrode 27, and nickel (or copper-nickel) electrode 26 as internal electrodes with ceramic embryo 21 under air to produce an MLCC as shown in FIG. 12(d).
[0055] 4. When the above internal electrodes are co-fired, since they have aluminum electrodes, they do not shrink in the X and Y axes when co-fired with the ceramic embryo, and the effect of sintering is limited to the Z axis. Therefore, there is almost no change in the electrode pattern after printing and after sintering. In addition, since the shrinkage after sintering is concentrated in the thickness direction of the Z axis, it is twice as effective in reducing the thickness of the dielectric layer and improving the capacitance value as in multilayer ceramic capacitors.
[0056] [Example 3] Chip resistor
[0057] 1. The present invention applies a new process to the electrodes of chip resistors, as shown in FIG. 13, in which (a) and (b) are the lower electrode structures, and (c) and (d) are the upper electrode structures.
[0058] When a chip resistor is to produce a positive electrode connected to the resistive layer 31, a positive electrode conductor paste made of copper (or copper-nickel) with 10 to 90 wt % aluminum powder is printed on the upper surface of the substrate 35 (for example, an alumina substrate) and connected to the resistive film, followed by a heat treatment at 500 to 1000°C; alternatively, a single layer of copper or copper-aluminum conductor paste film is printed and connected to the resistive film, followed by a single layer of aluminum conductor paste film for protecting the copper or copper-aluminum conductor paste film is printed on the upper surface, followed by a heat treatment at 500 to 1000°C. In this way, a highly conductive aluminum copper electrode 32 (e.g., as shown in Fig. 13(b) and (d)) can be obtained by sintering under air, or a resistive layer 31 can be connected to an aluminum electrode 33 by using a copper (or copper aluminum) electrode 34 (e.g., as shown in Fig. 13(a) and (c)) coated on the aluminum electrode 33. Also, a resistive layer 31 can be printed on the copper aluminum electrode 34, and then an aluminum electrode 33 can be printed as a protective layer and sintered at high temperature. The result is as shown in Fig. 14, and the stability of the resistor characteristics can be ensured, which is equivalent to the high conductivity of the existing positive silver electrode sintered under air.
[0059] 2. The present invention applies the new process to alloy chip resistors, as shown in Figure 15.
[0060] Method 1: Alloy powder + aluminum powder
[0061] For example, a suitable amount of aluminum powder is added to copper-nickel alloy, manganese-copper alloy, or nickel-chromium alloy powder to obtain a resistive paste, which is then printed with a resistive film and sintered at 500-1400°C. By adding the aluminum powder, the oxidation of the alloy powder can be avoided and the highly effective resistive properties of the alloy film can be maintained.
[0062] Method 2: Coating the aluminum film with a mixture of copper, nickel, manganese and chromium
[0063] On the upper surface of an (alumina) substrate 43 having an aluminum copper electrode 44, a resistive alloy paste is printed, such as an alloy film such as a copper nickel film, a manganese copper film, or a nickel-chromium (silicon) film. Then, a thick aluminum film is printed on the upper surface of the alloy film, and a heat treatment is performed at 500 to 1400°C to form a copper-nickel (or manganese copper or nickel-chromium) resistive alloy layer 41 covered with an aluminum (or aluminum nickel) layer 42. The printed aluminum conductor paste film protects the alloy film during the heat treatment to prevent oxidation, and maintains the highly effective resistive properties of the alloy film, as shown in Figure 15(a).
[0064] Wherein, the copper-nickel film can be obtained by mixing metallic copper powder 411 and metallic nickel powder 412 in a specific ratio according to need, or can be made of copper-nickel alloy powder 413, as shown in FIG. 15(b).
[0065] Wherein, the manganese copper film can be obtained by mixing metallic copper powder 411 with metallic manganese powder 414 or copper-coated manganese powder 415 in a specific ratio according to need, or can be made with manganese copper alloy powder 416, as shown in FIG. 15(c).
[0066] Wherein, the nickel-chromium film can be obtained by mixing metallic nickel powder 412 with metallic chromium powder 417 or nickel-coated chromium powder 418 in a certain ratio according to need, or can be made with nickel-chromium alloy powder 419, as shown in FIG. 15(d).
[0067] In addition, the present invention proposes a process for a novel base metal alloy chip resistor as shown in FIG. 16, in which a base metal resistance alloy paste, such as an alloy film such as copper-nickel film, manganese copper film or nickel-chromium (silicon) film, is printed on a substrate 51, and then an anti-oxidation aluminum film is printed. Then, high-temperature sintering (for example: 850°C) is carried out under air to form aluminum layers 52, 53 and a copper-nickel (or manganese copper or nickel-chromium) resistance alloy layer 54 covered by the aluminum layer 52. Then, the aluminum layer located in the upper middle of the copper-nickel (or manganese copper or nickel-chromium) resistance alloy layer 54 is removed by laser engraving. The electronic image of the structure is shown in FIG. 17(a) and (b), so that the aluminum layers 52 located at both ends that are not removed by laser engraving can be used as terminal electrodes of the alloy chip resistor.
[0068] Therefore, the method according to the present invention has the following technical features:
[0069] 1. By adding 10 to 90 wt% of metallic aluminum powder to thick-film printing base metal powder (e.g., nickel or copper) or base metal alloy powder (e.g., copper-nickel, manganese-copper, and nickel-chromium), and then carrying out a heat treatment at 500 to 1400°C under air, it is possible to avoid oxidation of the base metal or alloy, and obtain a thick-film base metal electrode film or alloy film with high performance characteristics.
[0070] 2. For example, a layer of base metal nickel or copper conductor paste film or a paste film of copper-nickel, manganese-copper or nickel-chromium (silicon) base metal alloy is thick-film printed on the upper surface of a substrate, and then a layer of thick-film printed aluminum conductor paste film is printed on the upper surface of the base metal conductor paste film or the base metal alloy paste film. Heat treatment is performed at 500 to 1400°C under air, and the aluminum layer can protect the base metal or alloy from oxidation, resulting in a thick-film base metal electrode film or alloy film with high efficacy properties. The aluminum layer for intermediate protection is then removed by laser engraving, and the aluminum layers remaining at both ends without being removed by laser engraving can be used as terminal electrodes of an alloy chip resistor.
[0071] 3. For laminated ceramic co-firing parts, if the sintering temperature is less than 1050℃, 10~90wt% aluminum powder mixed with copper thick film conductor paste can be used as the internal electrode, and the ceramic embryo can be co-fired under air, like LTCC; if the sintering temperature is between 1050℃~1450℃, 10~90wt% aluminum powder mixed with nickel or nickel copper thick film conductor paste can be used as the internal electrode, and the ceramic embryo can be co-fired under air, like MLCC.
[0072] 4. The multilayer ceramic co-firing parts can be manufactured by first printing a single layer of copper thick-film conductor paste film at a sintering temperature <1050°C, and then printing a single layer of thick-film aluminum conductor paste film on the top surface of the film, and then co-firing the ceramic embryo under air with both layers of the multilayer electrode concept as internal electrodes, like LTCC; if the sintering temperature is between 1050-1450°C, first printing a single layer of nickel or nickel-copper thick-film conductor paste film, and then printing a single layer of thick-film aluminum conductor paste film, and then co-firing the ceramic embryo under air with both layers of the multilayer electrode concept as internal electrodes, like MLCC.
[0073] 5. The multilayer ceramic co-firing parts can be manufactured at a sintering temperature <1050°C by first printing a layer of copper thick film conductor paste film, then printing a layer of thick film aluminum conductor paste film, and finally printing another layer of copper thick film conductor paste film, and then co-firing the three layers of the multilayer electrode concept as the internal electrode under air to form a ceramic embryo, like LTCC; if the sintering temperature is between 1050-1450°C, first printing a layer of nickel or copper-nickel thick film conductor paste film, then printing a layer of thick film aluminum conductor paste film, and finally printing another layer of nickel or nickel-copper thick film conductor paste film, and then co-firing the three layers of the multilayer electrode concept as the internal electrode under air to form a ceramic embryo, like MLCC.
[0074] 6. When preparing a positive electrode that connects a chip resistor and a resistance layer, first, a positive electrode conductor paste made of copper or copper-nickel with 10-90 wt% aluminum powder added is printed to connect the resistance film, and then a heat treatment is performed at 500-1000°C; alternatively, a single layer of copper or copper-nickel conductive film is printed to connect the resistance film, and then a single layer of aluminum conductor paste film is printed on the upper surface to protect the copper or copper-nickel conductive film and prevent high-temperature oxidation, and then a heat treatment is performed at 500-1000°C.
[0075] 7. Semiconductor ceramic PTC thermistor electrodes not only require high conductivity but also need to form ohmic contact with the semiconductive ceramic formation, so by adjusting the proportion of aluminum (10-90wt%) added to copper or nickel, ohmic contact can be formed with thick film electrodes of different work functions.
[0076] 8. Print the resistance alloy paste to make an alloy film, such as a copper-nickel film, a manganese-copper film, or a nickel-chromium (silicon) film, and then print a thick aluminum film on the alloy film to protect the alloy film from oxidation during heat treatment (500-1400°C) and maintain the high-performance resistance properties of the alloy film.
[0077] The present invention differs from the existing techniques in the following respects.
[0078] 1. According to existing technology, when a base metal is heat-treated to thick-print conductive copper, nickel, or copper-nickel alloy paste film, the base metal is sintered by heat-treating in a reducing atmosphere, for example, nitrogen or a nitrogen-hydrogen mixture, to prevent the base metals copper, nickel, or alloys from being oxidized and losing their effectiveness.
[0079] The new technology of the present invention protects base metals such as copper, nickel, and alloys by adding or covering them with aluminum powder or aluminum film that has highly aerobic and strong reducing properties, and does not oxidize or lose its efficacy even when sintered by high-temperature heat treatment in air.
[0080] 2. Existing multilayer ceramic elements have a problem of shrinkage mismatch when ceramic embryos and electrodes are co-fired. Existing technologies use a sintering technology that does not shrink in both the X and Y axes when co-firing by covering a non-shrink ceramic embryo with a higher temperature than the ceramic embryo being co-fired, or by inserting another ceramic embryo with a lower temperature than the ceramic embryo being co-fired, thereby reducing the problem of mismatch between ceramic embryos and electrodes when co-firing.
[0081] The new technology of the present invention utilizes the property that metal electrodes do not shrink when co-firing with ceramic matrix, and uses a sintering technology that does not shrink in both the X and Y axes when co-firing, which can reduce the problem of mismatch between ceramic matrix and electrodes when co-firing.
[0082] 3. Many existing ceramic elements, such as chip resistors, NTC, PTC, VDR and piezoelectric PZT, have a problem that the properties of the ceramic body after sintering change when the external electrodes are sintered in a reducing atmosphere, so copper electrodes cannot be sintered in nitrogen.
[0083] The new technology of the present invention can protect a thick copper electrode film with a thick aluminum film and perform a heat treatment under air, thereby making it possible to fabricate copper electrodes for ceramic elements such as chip resistors, NTC, PTC, VDR, and piezoelectric PZT.
[0084] 4. Existing alloy resistors have a very low temperature coefficient of resistance. They are mainly manufactured by using a precious metal silver-palladium alloy sintered in air, or by sintering a base metal copper-nickel alloy in a reducing atmosphere of nitrogen (or nitrogen and hydrogen).
[0085] The new technology of the present invention can sinter in an air atmosphere when making a base metal alloy (such as copper-nickel, manganese-copper, nickel-chromium) resistor, and it corresponds to the characteristics of sintering in a reducing atmosphere (such as copper-nickel, manganese-copper, nickel-chromium). In addition, the new air sintering chip-type base metal resistance alloy manufacturing method is different from the existing chip alloy resistor manufacturing method, for example, as in the background art, the conventional process is to first print the positive electrode paste on both ends, then print the resistance alloy paste, and sinter the precious metal silver electrodes 62, 63 and the silver-palladium resistance alloy layer 64 under air, as shown in Figure 18, or to use the base metal copper electrodes and the copper-nickel resistance alloy layer sintered under a nitrogen reducing atmosphere.
[0086] The novel process of the present invention involves printing a base metal resistance alloy paste, then printing an anti-oxidation aluminum film, then sintering at high temperature under air, and then removing the intermediate protective aluminum layer by laser engraving, so that the aluminum that is not removed by laser engraving at both ends becomes the two terminal electrodes of the chip resistor.
[0087] Therefore, the method of the present invention for producing oxidation-resistant base metals and alloys by high-temperature sintering under air can completely change the electrode materials of existing thick-film printing from precious metals to base metals, but when using base metals instead of precious metals, high-temperature sintering must be performed under a reducing atmosphere to prevent metal oxidation. The method of the present invention can firstly sinter very cheap base metals or alloys at high temperatures under air using a cheap process without oxidation, and can also maintain excellent electrical properties. Related industries can use the existing equipment to sinter under air, i.e., base metal materials can be used instead of precious metal materials, so there is no need to purchase new equipment and the material costs are greatly reduced.
[0088] The present invention is a method for producing oxidation-resistant base metals and alloys by using high-temperature sintering under air, which can effectively eliminate the various shortcomings of the past and completely change the electrode material of existing thick-film printing from precious metals to base metals. In addition, very cheap base metals or alloys can be sintered at high temperatures under air using a cheap process without oxidation and while maintaining excellent electrical properties. Therefore, the present invention is more advanced and more practical, and therefore patent claims are filed in accordance with the law.
[0089] The above is merely a better embodiment of the present invention, and the present invention is not limited thereby. All equivalent changes and modifications made based on the claims and the contents of the specification related to the present invention are included in the scope of the claims of the present invention. [Brief description of the drawings]
[0090] [Figure 1] FIG. 2 is a graph showing the change in weight with increasing temperature in thermal analysis when copper is added to the aluminum of the present invention. [Diagram 2] FIG. 2 is a graph showing the change in weight with increasing temperature in a thermal analysis when nickel is added to the aluminum of the present invention. [Diagram 3] FIG. 2 is a sintered microstructure diagram when copper is added to the aluminum of the present invention. [Figure 4]FIG. 2 is a sintered microstructure diagram when nickel is added to the aluminum of the present invention. [Diagram 5] FIG. 2 is a microstructure diagram of the sintered aluminum alloy when nickel is added to the aluminum of the present invention. [Figure 6] FIG. 2 is a microstructure diagram of sintering when a copper film is coated on an aluminum film of the present invention. [Figure 7] FIG. 2 is a microstructure diagram of sintering when a nickel film is coated on an aluminum film of the present invention. [Figure 8] FIG. 2 is a microstructure diagram of sintering when a copper-nickel film is coated on an aluminum film of the present invention. [Figure 9] FIG. 2 is a microstructure diagram of sintering when coating a manganese copper film on an aluminum film of the present invention. [Figure 10] FIG. 10 is a structural conceptual diagram of an external electrode of a bulk ceramic element manufactured by a new process according to the present invention. [Figure 11] FIG. 2 is a structural conceptual diagram of a non-shrinking internal electrode of a multilayer ceramic element manufactured by a new process according to the present invention. [Figure 12] FIG. 2 is a structural conceptual diagram of a non-shrinking laminated internal electrode of a multilayer ceramic element manufactured by a new process according to the present invention. [Figure 13] 1 is a structural conceptual diagram of a chip resistor electrode manufactured by a new process according to the present invention. [Figure 14] FIG. 2 is a schematic diagram of the structure of a chip resistor alloy produced by the novel process of the present invention. [Figure 15] FIG. 2 is a schematic diagram of the structure of a chip resistor alloy produced by the novel process of the present invention. [Figure 16] 1 is a schematic diagram of a novel base metal alloy chip resistor process according to the present invention. [Figure 17] 1 is a schematic diagram of a chip resistor alloy structure produced by the novel process of the present invention. [Figure 18] FIG. 1 is a conceptual diagram of a process for manufacturing existing precious metal alloy chip resistors. [Explanation of symbols]
[0091] (The present invention) 11 Ceramic elements 12 Copper aluminum (or nickel aluminum) electrode 13 Copper (or nickel) electrode 14 Aluminum Electrode 21 Ceramic Embryogenesis 22 Copper aluminum electrode 23 Nickel-aluminum electrode 24 copper electrode 25 Aluminum Electrode 26 Nickel (or nickel-copper) electrodes 27 Aluminum Electrode 31 Resistance layer 32 Aluminum copper electrode 33 Aluminum Electrode 34 Copper (or copper-nickel) electrode 35 Substrate 41 Copper-nickel (or manganese-copper, nickel-chromium) resistance alloy layer 411 Metallic copper powder 412 Metallic Nickel Powder 413 Copper-nickel alloy powder 414 Metallic manganese powder 415 Copper-coated manganese powder 416 Manganese copper alloy powder 417 Metallic Chromium Powder 418 Nickel-coated Chromium Powder 419 Nickel-chromium alloy powder 42 Aluminum (or Aluminum Nickel) Layer 43 Substrate 51 Substrate 52, 53 Aluminum layer 54 Copper-nickel (or manganese-copper, nickel-chromium) resistance alloy layer (Previously) 61 Substrate 62, 63 Noble metal silver electrodes 64 Silver-palladium resistance alloy layer
Claims
1. This method is characterized in that 10 to 90 wt % of metallic aluminum powder is added to a base metal conductor paste or base metal alloy paste for thick film printing, and heat treatment is performed under air at 500 to 1400°C, and the highly aerobic nature of the metallic aluminum powder is utilized to protect the base metal conductor paste or base metal alloy paste and prevent oxidation when sintered under high-temperature air, or the base metal conductor paste or base metal alloy paste is sintered under high-temperature air and oxidized, and then the strongly reducing nature of the metallic aluminum powder is utilized to reduce the oxidized base metal conductor paste or base metal alloy paste to a metal or alloy, thereby obtaining a thick-film base metal electrode film or alloy film.
2. The method for producing oxidation-resistant base metals and alloys by high temperature sintering under air as described in claim 1, characterized in that the base metal conductor paste is one of metallic copper powder or nickel powder, and the base metal alloy paste is one of copper-nickel alloy powder, manganese-copper powder, or nickel-chromium powder.
3. The thick base metal electrode film or alloy film is applied to external electrodes of bulk ceramic elements, internal electrodes of multilayer ceramic elements, chip resistor electrodes, and alloy chip resistors, as described in claim 1, and is a method for producing oxidation-resistant base metals and alloys by using high-temperature sintering in air.
4. The bulk ceramic element is a GPS ceramic antenna, a Negative Temperature Coefficient (NTC) thermistor, a Positive Temperature Coefficient (PTC) thermistor, a Voltage Dependent Resistor (VDR) or a safety capacitor. The method of producing oxidation-resistant base metals and alloys by high temperature sintering under air is described in claim 3.
5. The multilayer ceramic element is a low temperature co-fired ceramic (LTCC), a multilayer ceramic capacitor (MLCC), a multilayer NTC component, a multilayer VDR component, or a multilayer piezoelectric component, as described in claim 3. The method is capable of producing oxidation-resistant base metals and alloys by using high temperature sintering in air.
6. This method is characterized in that a single layer of thick-film aluminum conductor paste film is printed on the top surface of a base metal conductor paste film or a base metal alloy paste film produced by thick film printing, and then heat-treated at 500 to 1400°C under air, and the highly aerobic nature of the aluminum conductor paste film is utilized to protect the base metal conductor paste film or the base metal alloy paste film from oxidation when sintered under high-temperature air, or, after the base metal conductor paste film or the base metal alloy paste film is sintered and oxidized under high-temperature air, the strongly reducing nature of the aluminum conductor paste film is utilized to reduce the oxidized base metal conductor paste film or the base metal alloy paste film to a metal or alloy, thereby obtaining a thick-film base metal electrode film or alloy film.
7. The method for producing oxidation-resistant base metals and alloys by high-temperature sintering under air as described in claim 6, characterized in that the base metal conductor paste film is one of metallic copper film and nickel film, and the base metal alloy paste film is one of alloy copper-nickel film, manganese copper film, and nickel-chromium film.
8. The thick base metal electrode film or alloy film is applied to external electrodes of bulk ceramic elements, internal electrodes of multilayer ceramic elements, chip resistor electrodes, and alloy chip resistors, as described in claim 6. This method is capable of producing oxidation-resistant base metals and alloys by using high-temperature sintering under air.
9. The thick base metal electrode film or alloy film can be applied to the process of alloy chip resistors, and the aluminum layer located in the middle for protection is removed by laser engraving to expose the resistance alloy layer, and the aluminum layer at both ends that has not been removed by laser engraving is used as the terminal electrodes of the alloy chip resistor, as described in claim 6. This is a method for producing oxidation-resistant base metals or alloys by high-temperature sintering under air.
10. The method for producing oxidation-resistant base metals and alloys by high temperature sintering under air as described in claim 8, characterized in that the bulk ceramic components are GPS ceramic antennas, NTC thermistors, PTC thermistors, VDRs or safety capacitors, and the multilayer ceramic components are LTCCs, MLCCs, multilayer NTC components, multilayer VDR components or multilayer piezoelectric components.
Citation Information
Patent Citations
Base metal electrode structure and preparing method thereof
CN103578607A
Production method of high-conductivity base metal electrode or alloy low-ohm chip resistor
CN108735408A
Preparation method of high-conductivity base metal thick-film conductive paste
CN109786027A
Ceramic dielectric material, preparation method, and lamination ceramic capacitor of low metal
CN1917105A
Electrode, electrode paste, and electronic component using same
JP2010161331A