Platinum-carbon catalyst, its preparation and use, and hydrogen fuel cell
A platinum-carbon catalyst with strong support interactions is produced through ultrasonic dispersion and reduction, addressing scalability and stability issues, resulting in improved electrochemical performance for fuel cells.
Patent Information
- Application Number
- JP2024525640
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2021-10-29
- Filing Date
- 2022-10-31
- Publication Date
- 2024-11-19
Smart Images

Figure 2024543017000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a platinum-carbon catalyst and its manufacturing method and use. The present invention also relates to a hydrogen fuel cell using the platinum-carbon catalyst. [Background technology]
[0002] Catalysts are key materials in fuel cell technology. During fuel cell operation, there are biases in activity, concentration, permeability, and resistance. Among these, the most significant bias in activity is the one that causes a low exchange current density for the oxygen reduction reaction (ORR) at the cathode.
[0003] So far, the most efficient oxygen reduction catalyst is a platinum-carbon catalyst. The main methods for synthesizing platinum-carbon catalysts that have been reported include the immersion method, high-temperature calcination method, vacuum sputtering method, ion exchange method, electrochemical deposition method, sol-gel method, gas-liquid phase reduction method, glow discharge plasma method, displacement method, and microwave-promoted reduction method. Each of these methods has its own advantages and disadvantages, but all of them have some problems in terms of industrial expansion.
[0004] The support is a very important element in fuel cell catalysts. The synergistic effect between the support and the metal catalyst can improve catalytic performance. In principle, platinum-carbon catalysts are unstable due to the weak interaction between the metallic platinum particles and the carbon support. Strengthening the interaction between the metallic platinum and the carbon support is one of the keys to improving the stability of the catalyst.
[0005] Therefore, there is an urgent need in the art to develop a manufacturing method for batch production of platinum-carbon catalysts that can not only improve the stability of platinum-carbon catalysts by increasing the interaction between metallic platinum and the carbon support, but also produce platinum-carbon catalysts with high uniformity and batch stability in batches. Summary of the Invention
[0006] The object of the present invention is to provide a platinum-carbon catalyst and a method for producing the same. The platinum-carbon catalyst of the present invention has a strong interaction with the support, and has improved oxygen reduction activity and stability. The platinum-carbon catalyst obtained by the production method of the present invention has high uniformity and batch stability, and has a strong interaction between metallic platinum and the support, and has improved oxygen reduction activity and stability.
[0007] According to a first aspect of the present invention, there is provided a platinum-carbon catalyst comprising a carbonaceous support and metallic platinum particles supported on the carbonaceous support, wherein at least 50% of the metallic platinum particles have a contact angle with the carbonaceous support of 70° or less.
[0008] According to a second aspect of the present invention, there is provided a method for preparing a platinum-carbon catalyst, the method comprising the steps of: Step S1: The carbonaceous material, the platinum precursor, the complexing agent, and the dispersion medium are dispersed by ultrasonic waves to obtain a first dispersion. The complexing agent is a carboxylate. The dispersion medium is a C2-C4 dihydric alcohol and water. The volume ratio of the dihydric alcohol to water is (0.1-10):1. The molar ratio of the platinum precursor to the complexing agent is 1:(0.1-10). In S1, C1 / C0<0.5 is satisfied. Here, C0 is the molar concentration of the platinum precursor relative to the dispersion medium. C1 is the molar concentration of platinum contained in the liquid phase of the first dispersion obtained in step S1. Step S2: The pH value of the first dispersion is adjusted to 8 to 14 to obtain a second dispersion. Step S3: A reducing agent is added to the second dispersion, and the reducing agent and the platinum precursor are brought into contact with each other in the second dispersion to cause a reduction reaction. The reducing agent is an acidic organic reducing agent. The molar ratio of the reducing agent to the platinum precursor as elemental platinum is generally (5 to 1000):1.
[0009] According to a third aspect of the present invention, there is provided a platinum-carbon catalyst obtainable by the process according to the second aspect of the present invention.
[0010] According to a fourth aspect of the invention, there is provided the use of a platinum-carbon catalyst according to the first or third aspect of the invention in a fuel cell.
[0011] According to a fifth aspect of the invention, there is provided a hydrogen fuel cell, the anode and / or cathode of which comprises a platinum-carbon catalyst according to the first or third aspect of the invention.
[0012] Specifically, the present disclosure provides the following technical solutions: <Technical solution 1> A platinum-carbon catalyst comprising a carbonaceous support and metallic platinum particles supported on the carbonaceous support, At least 50% of the metallic platinum particles have a contact angle of 70° or less with respect to the carbonaceous support; Preferably, 55% or more of the metallic platinum particles have a contact angle of 70° or less with respect to the carbonaceous support (e.g., 55-70% or 60-70% of the metallic platinum particles have a contact angle of 70° or less with respect to the support), More preferably, the contact angle of the metallic platinum particles with respect to the carbonaceous support is 40° to 70°; Based on the total amount of the platinum-carbon catalyst, The content of the metallic platinum is 20 to 70% by weight, The content of the carbonaceous support is 30 to 80% by weight; Preferably, based on the total amount of the platinum-carbon catalyst, The content of the metallic platinum is 50 to 70% by weight, The content of the carbonaceous support is 30 to 50% by weight; Platinum-carbon catalyst <Technical solution 2> The average particle size of the metallic platinum particles contained in the platinum-carbon catalyst is 3 to 6 nm. The platinum-carbon catalyst according to technical solution 1. <Technical solution 3> The platinum-carbon catalyst essentially consists of the carbonaceous support and metallic platinum particles supported on the carbonaceous support. The platinum-carbon catalyst according to technical solution 1 or 2. <Technical solution 4> The platinum-carbon catalyst comprises the carbonaceous support and metallic platinum particles supported on the carbonaceous support. The platinum-carbon catalyst according to any one of technical solutions 1 to 3. In the present invention, the phrase "the platinum-carbon catalyst is (substantially) composed of a carbonaceous support and metallic platinum particles supported on the carbonaceous support" means the following: based on the weight of the platinum-carbon catalyst, the total weight of the carbonaceous support and metallic platinum particles can be 90% by weight or more, 95% by weight or more, 96% by weight or more, 97% by weight or more, 98% by weight or more, or 99% by weight or more. <Technical solution 5> The carbonaceous support is conductive carbon black, Preferably, the specific surface area of the conductive carbon black is 200 to 2000 m 2 / g (preferably 250 to 1500m 2 / g), The platinum-carbon catalyst according to any one of technical solutions 1 to 4. <Technical solution 6> A platinum-carbon catalyst according to any one of technical solutions 1 to 5, which satisfies the following (i) and / or (ii): (i) The electrochemically active surface area of the platinum-carbon catalyst is 70 to 120 m 2 ·g -1 -Pt; (ii) The mass specific activity of the platinum-carbon catalyst is 0.2 A mg -1 -Pt or more (preferably 0.2 to 0.25 A mg -1 -Pt). <Technical solution 7> A method for producing a platinum-carbon catalyst, comprising the steps of: Step S1: Dispersing a carbonaceous material, a platinum precursor, a complexing agent, and a dispersion medium (optionally, ultrasonically dispersing) to obtain a first dispersion, The complexing agent is a carboxylate, The dispersion medium is a C2-C4 dihydric alcohol and water, the volume ratio of the dihydric alcohol to the water is (0.1 to 10:1); the molar ratio of the platinum precursor to the complexing agent is 1:(0.1-10); In an optional configuration, a pH value of the dispersion obtained in step S1 is 1 to 4; Step S2: adjusting the pH value of the first dispersion to 8 to 14 to obtain a second dispersion; Step S3: A step of adding a reducing agent to the second dispersion, contacting the reducing agent with the platinum precursor in the second dispersion, and causing a reduction reaction, The reducing agent is an acidic organic reducing agent, The molar ratio of the reducing agent to the platinum precursor as elemental platinum is generally (5-1000):1. <Technical solution 8> The manufacturing method according to technical solution 7, which satisfies the following relationships: C1 / C0<0.5 (C1 / C0 is, for example, 0.15 to 0.49, preferably 0.15 to 0.45, and more preferably 0.2 to 0.4) During the ceremony, C0: Molar concentration of the platinum precursor relative to the dispersion medium in step S1 C1: Molar concentration of platinum contained in the liquid phase of the first dispersion obtained in step S1 <Technical solution 9> The manufacturing method according to technical solution 7 or 8, which satisfies one or more of the following (i) to (iii): (i) in step S1, the complexing agent is an alkali metal salt of a monocarboxylic acid and / or an ammonium salt of a monocarboxylic acid; Preferably, the complexing agent is one or more compounds of formula I: R-COOM (Formula I) In formula I, R is hydrogen, C1-C6 alkyl or C1-C6 haloalkyl; M is an alkali metal ion or an ammonium ion; (ii) preferably, the complexing agent is one or more of sodium formate, sodium acetate, sodium monochloroacetate, sodium dichloroacetate and sodium trichloroacetate; (iii) The molar ratio of the platinum precursor to the complexing agent is 1:(0.5 to 5) (preferably 1:(1 to 3)). <Technical solution 10> In the step S1, the carbonaceous material, the platinum precursor, the complexing agent, and the dispersion medium are dispersed by ultrasonic waves; The ultrasonic output for 1 L of the dispersion medium is 1 to 20 W (preferably 2 to 12 W). The dispersion time by ultrasonic waves is 0.1 to 5 hours (for example, 0.2 to 1 hour). The manufacturing method according to any one of technical solutions 7 to 9. <Technical solution 11> The manufacturing method according to any of technical solutions 7-10, which satisfies the following (i) and / or (ii): (i) in the step S1, the volume ratio of the dihydric alcohol to the water is (0.5-5):1, 1:(0.5-5), (0.67-3):1 or 1:(1-3); (ii) The dihydric alcohol is ethylene glycol, 1,2-propylene glycol, or 1,3-propylene glycol, and preferably the dihydric alcohol is ethylene glycol. <Technical solution 12> In the step S1, the mass ratio of the platinum precursor to the dispersion medium is 1:(100 to 5000) (preferably 1:(120 to 1000), more preferably 1:(160 to 300)). The manufacturing method according to any one of technical solutions 7 to 11. <Technical solution 13> The preparation method according to any one of technical solutions 7 to 12, further comprising the steps of: Step S0: pre-treating the carbonaceous material of step S1, in which the carbonaceous material is successively treated with a solvent treatment, a first oxidation treatment, a second oxidation treatment and a high temperature treatment to obtain a pre-treated carbonaceous material; Where: In the solvent treatment, the carbonaceous material is immersed in an organic solvent to obtain a carbonaceous material immersed in an organic solvent; Preferably, the organic solvent is one or more of a ketone solvent; In the first oxidation treatment, the carbonaceous material immersed in the organic solvent is contacted with a first oxidizing agent to obtain a carbonaceous material subjected to a first oxidation treatment; the first oxidizing agent is one or more of hydrogen peroxide and an organic peroxide represented by formula II; [ka] In formula II, R1 and R2 are H, C4-C 12 Alkyl, C6-C 12 Aryl, C7-C 12 aralkyl and the following structure: [ka] R1 and R2 are not H at the same time, R3 is C4~C 12 Straight or branched alkyl of C6 to C 12 is aryl; In the second oxidation treatment, the carbonaceous material subjected to the first oxidation treatment is contacted with a second oxidizing agent to obtain a carbonaceous material subjected to a second oxidation treatment; the second oxidant being one or more of HNO3 and / or H2SO4; In the high-temperature treatment, the carbonaceous material subjected to the second oxidation treatment is fired in an inert atmosphere at 300 to 700°C (for example, 300 to 600°C, as one example, 400°C, 500°C, 600°C, or 700°C) to obtain the pre-treated carbonaceous material. <Technical solution 14> The manufacturing method according to technical solution 13, which satisfies one or more of the following (i) to (iii): (i) In the solvent treatment in step S0, The immersion time is 5 to 24 hours (e.g., 8 hours), The mass ratio of the solvent to the carbonaceous material is (5 to 100):1 (e.g., 20:1 or 18:1); (ii) the temperature of the organic solvent in the solvent treatment is 20 to 70°C (preferably 25 to 40°C, for example, 25°C or 35°C); (iii) The organic solvent in the above solvent treatment is acetone. <Technical solution 15> The manufacturing method according to technical solution 13 or 14, which satisfies one or more of the following (i) to (iv): In the first oxidation treatment in step S0, The contact time is 5 to 24 hours (e.g., 12 hours or 10 hours), a mass ratio of the first oxidant to the carbonaceous material immersed in the organic solvent is (5 to 30:1) (e.g., 25:1 or 20:1); (ii) the contact temperature in the first oxidation treatment is 20 to 70°C (preferably 25 to 40°C, for example 25°C); (iii) the first oxidizing agent in the first oxidation treatment is provided as an aqueous solution, and the content of the first oxidizing agent in the aqueous solution is 5 to 30% by weight (e.g., 15% by weight or 10% by weight); (iv) The first oxidizing agent in the first oxidation treatment is hydrogen peroxide. <Technical solution 16> The manufacturing method according to any one of technical solutions 13 to 15, which satisfies one or more of the following (i) to (iii): In the second oxidation treatment in step S0, The contact time is 5 to 24 hours (e.g., 12 hours), The mass ratio of the second oxidizing agent to the carbonaceous material that has been subjected to the first oxidation treatment is (5 to 50):1 (preferably (10 to 30):1, more preferably (12 to 20):1, for example, 15:1 or 12:1); (ii) the contact temperature in the second oxidation treatment is 50 to 90°C (e.g., 70°C or 65°C); (iii) the second oxidizing agent in the second oxidation treatment is nitric acid; Preferably, the concentration of the nitric acid is 25 to 68% by weight (preferably 30 to 40% by weight, for example, 30% by weight or 35% by weight). <Technical solution 17> The manufacturing method according to any of technical solutions 13-16, which satisfies the following (i) and / or (ii): (i) In the high-temperature treatment in the step S0, the firing temperature is 500 to 600° C. (for example, 600° C.); (ii) The firing time in the high-temperature treatment is 2 to 8 hours (preferably 3 to 6 hours, for example 4 hours). <Technical solution 18> The manufacturing method according to technical solution 7, which meets the following (i) and / or (ii): (i) in step S1, the water-soluble platinum precursor is one or more of sodium chloroplatinate, ammonium hexachloroplatinate, potassium hexachloroplatinate, sodium hexachloroplatinate, platinum tetrachloride, tetraammineplatinum nitrate, platinum nitrate, chloroplatinic acid, potassium chloroplatinate, and sodium chloroplatinate; (ii) in step S1, the carbonaceous material is conductive carbon black; The specific surface area of the conductive carbon black is preferably 200 to 2000 m 2 / g, more preferably 250 to 1500m 2 / g. <Technical solution 19> In the step S2, the pH value of the first dispersion obtained in the step S1 is adjusted to 8 to 12; Adjusting the pH value, for example by adding sodium carbonate, potassium carbonate or sodium hydroxide, The manufacturing method according to any one of technical solutions 7 to 18. <Technical solution 20> The manufacturing method according to any of technical solutions 7-19, which satisfies the following (i) and / or (ii): (i) in step S3, the reducing agent is one or more of formic acid, citric acid, and tartaric acid; The reducing agent preferably comprises, and more preferably is, formic acid; (ii) in step S3, the molar ratio of the reducing agent to the water-soluble platinum precursor is (50-600):1, (80-400):1, or (100-200):1 (e.g., 200:1); In this case, the water-soluble platinum precursor is calculated as metallic platinum; <Technical solution 21> The manufacturing method according to any of technical solutions 7-20, which satisfies the following (i) and / or (ii): (i) In the above step S3, the reduction temperature is 50 to 140°C, 55 to 90°C, or 60 to 80°C (e.g., 75°C); (ii) In the above step S3, the reduction time is 2 to 12 hours (for example, 6 hours). <Technical solution 22> A platinum-carbon catalyst obtained by any one of the production methods of technical solutions 7 to 21. <Technical solution 23> Use of the platinum-carbon catalyst according to any of technical solutions 1-6, 22 in a fuel cell. <Technical solution 23> The electrochemical cell is provided with an anode and / or a cathode containing a platinum-carbon catalyst according to any one of technical solutions 1 to 6 and 22. Hydrogen fuel cell.
[0013] The platinum-carbon catalyst and the manufacturing method thereof according to the present invention can provide the following technical effects.
[0014] (1) The platinum-carbon catalyst of the present invention has excellent dispersion of metallic platinum particles on the carbonaceous support, forming very uniform cluster particles, and the interaction between the metallic platinum and the carbonaceous support is strong, so that the metallic platinum particles are fixed to the carbonaceous support. Therefore, the platinum-carbon catalyst of the present invention has an improved electrochemically active surface area and excellent electrochemical stability. (2) The method for producing a platinum-carbon catalyst according to the present invention has batch reproducibility and is easily scaled up to an industrial scale, allowing the above-mentioned platinum-carbon catalyst to be produced in batches. [Brief description of the drawings]
[0015] [Figure 1] FIG. 2 is a schematic diagram for explaining the contact angle between metallic platinum and a carbonaceous support in a platinum-carbon catalyst. [Diagram 2] 1 is a TEM image showing the contact angle between metallic platinum and a carbonaceous support in the platinum-carbon catalyst prepared in Example 1. [Diagram 3] 1 is a TEM image showing the contact angle between metallic platinum and a carbonaceous support in the platinum-carbon catalyst prepared in Comparative Example 1. [Figure 4] 1 is a TEM image of the platinum-carbon catalyst prepared in Example 1. Based on the total weight of the platinum-carbon catalyst, the content of metallic platinum is 55% by weight. [Diagram 5] 1 is a TEM image of the platinum-carbon catalyst prepared in Comparative Example 1. Based on the total amount of the platinum-carbon catalyst, the content of metallic platinum is 55% by weight. [Figure 6] 1 shows statistical results of particle sizes of metallic platinum particles included in the field of view in a transmission electron microscope image of the platinum-carbon catalyst prepared in Example 1. [Figure 7] This is a TEM image of the commercially available catalyst, JM70%. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0016] The endpoints of the ranges and any numerical values disclosed herein do not necessarily correspond exactly to the ranges or numerical values. Instead, these ranges or numerical values should be understood to include the values close to the ranges or numerical values. In addition, when referring to ranges, one or more new ranges can be obtained by combining two endpoints of the ranges, combining endpoints of the ranges with a specific numerical value, or combining any two specific numerical values. These ranges should also be understood to be specifically disclosed herein.
[0017] According to a first aspect, the present invention provides a platinum-carbon catalyst comprising a carbonaceous support and metallic platinum particles supported on the carbonaceous support.
[0018] The platinum-carbon catalyst of the present invention has excellent dispersion of metallic platinum particles on the carbonaceous support, forming very uniform metallic platinum cluster particles, and has a strong interaction between the metallic platinum and the carbonaceous support.
[0019] In the platinum-carbon catalyst of the present invention, 50% or more of the metallic platinum particles have a contact angle of 70° or less with the support. For example, 50 to 75% of the metallic platinum particles have a contact angle of 70° or less with the support. Preferably, 55% or more of the metallic platinum particles have a contact angle of 70° or less with the support. For example, 55 to 70% of the metallic platinum particles have a contact angle of 70° or less with the support. More preferably, 60% or more (for example, 60 to 70%) of the metallic platinum particles have a contact angle of 70° or less with the support. In the platinum-carbon catalyst of the present invention, the contact angle of the metallic platinum particles with the carbonaceous support is generally 40 to 70°.
[0020] In the present invention, the specific definition of the contact angle of the metallic platinum particles with the carbonaceous support is shown in Figure 1. The contact angle (θ) is obtained from a straight line forming the plane of the carbon layer and a tangent line drawn to the contact arc of the Pt particles and the carbon support surface. In the present invention, the contact angle between the metallic platinum particles and the carbonaceous support is measured by a profile imaging method based on an electron microscope. The range of the contact angle θ is 0°≦θ<180°.
[0021] In the platinum-carbon catalyst of the present invention, the metallic platinum particles contained in the platinum-carbon catalyst have an average particle size of 3 to 6 nm. In the present invention, the average particle size of the metallic platinum particles contained in the platinum-carbon catalyst is determined by observation with a transmission electron microscope.
[0022] In the platinum-carbon catalyst of the present invention, the content of metallic platinum may be 20 to 70% by weight, preferably 30 to 70% by weight, and more preferably 35 to 70% by weight, based on the total amount of the platinum-carbon catalyst. The content of the carbonaceous support may be 30 to 80% by weight, preferably 30 to 70% by weight, and more preferably 30 to 65% by weight. In a preferred embodiment, the content of metallic platinum is 50 to 70% by weight or 60 to 70% by weight, based on the total amount of the platinum-carbon catalyst. The content of the carbonaceous support is 30 to 50% by weight or 30 to 40% by weight.
[0023] In the present invention, the contents of platinum element and carbonaceous support contained in the platinum-carbon catalyst are determined by inductively coupled plasma spectroscopy (ICP spectroscopy).
[0024] In the platinum-carbon catalyst of the present invention, the carbonaceous support is conductive carbon black. The conductive carbon black may be one or more of normal conductive carbon black, high conductive carbon black, and ultra-high conductive carbon black. Examples of preferred conductive carbon black include, but are not limited to, one or more of Vulcan XC72, Ketjen EC300J, Ketjen EC600J, Blackpearls 2000, and Blackpearls 3000. The specific surface area of the conductive carbon black is preferably 200 to 2000 m. 2 / g, more preferably 250 to 1500m 2 In the present invention, the specific surface area is measured by the BET method.
[0025] The platinum-carbon catalyst of the present invention has an increased electrochemically active surface area. The electrochemically active surface area (ECSA) of the platinum-carbon catalyst of the present invention is 70 m 2 ·g -1 -Pt or more, preferably 70 to 120 m 2 ·g -1 -Pt, more preferably 80 to 120 m 2 ·g -1 The mass specific activity of the platinum-carbon catalyst according to the present invention is 0.2 A mg -1 -Pt or more, preferably 0.2 to 0.25 A mg -1 -Pt.
[0026] According to a second aspect of the present invention, there is provided a method for preparing a platinum-carbon catalyst, the method comprising the steps of: Step S1: A carbonaceous material, a platinum precursor, a complexing agent, and a dispersion medium are dispersed by ultrasonic waves to obtain a first dispersion. Step S2: The pH value of the first dispersion is adjusted to 8 to 14 to obtain a second dispersion. Step S3: A reducing agent is added to the second dispersion, and the reducing agent and the platinum precursor are brought into contact with each other in the second dispersion to cause a reduction reaction.
[0027] In step S1, the platinum precursor may be a platinum compound that can be reduced to metallic platinum by a reducing agent under reduction reaction conditions. In the manufacturing method of the present invention, the platinum precursor may be one or more of sodium chloroplatinate, ammonium hexachloroplatinate, potassium hexachloroplatinate, sodium hexachloroplatinate, platinum tetrachloride, tetraammine platinum nitrate, platinum nitrate, chloroplatinic acid, potassium chloroplatinate, and sodium chloroplatinate. Preferably, the platinum precursor is chloroplatinic acid.
[0028] In step S1, the complexing agent is a carboxylate. A carboxylate is a water-soluble salt of a carboxylic acid. Preferably, the complexing agent is one or more monocarboxylates. For example, the complexing agent may be an alkali metal salt of a monocarboxylate and / or an ammonium salt of a monocarboxylate. A monocarboxylate is a water-soluble salt of a monocarboxylate.
[0029] In the present invention, the complexing agent may be one or more of the compounds of formula I. R-COOM (Formula I)
[0030] In formula I, R can be hydrogen, C1-C6 alkyl, or C1-C6 haloalkyl. M is an alkali metal ion or an ammonium ion (-NH4 + ) may be possible.
[0031] In the present invention, C1-C6 alkyl includes C1-C6 linear alkyl and C3-C6 branched alkyl, specific examples of which include, but are not limited to, methyl, ethyl, n-propyl, isopropyl, n-butyl, sec-butyl, isobutyl, tertiary butyl, n-pentyl, 2-methylbutyl, 3-methylbutyl, 2,2-dimethylpropyl, n-hexyl, 2-methylpentyl, 3-methylpentyl, 4-methylpentyl, 2,3-dimethylbutyl, 2,2-dimethylbutyl, 3,3-dimethylbutyl, and 2-ethylbutyl.
[0032] In the present invention, the halogen atom contained in the haloalkyl may be fluorine, chlorine or bromine, and is preferably chlorine.
[0033] Specific examples of complexing agents include, but are not limited to, one or more of sodium formate, sodium acetate, ammonium acetate, sodium propionate, ammonium propionate, sodium butyrate, sodium valerate, sodium hexanoate, sodium monochloroacetate, sodium dichloroacetate, and sodium trichloroacetate.
[0034] Preferably, the complexing agent is one or more of sodium formate, sodium acetate, sodium monochloroacetate, sodium dichloroacetate and sodium trichloroacetate, more preferably, the complexing agent is sodium formate and / or sodium acetate.
[0035] In step S1, the molar ratio of the platinum precursor to the complexing agent is preferably 1:(0.1 to 10), more preferably 1:(0.5 to 5), and further preferably 1:(1 to 3).
[0036] In step S1, the dispersion medium is a C2-C4 dihydric alcohol and water. Preferably, the dihydric alcohol is ethylene glycol. In step S1, the volume ratio of the dihydric alcohol to water may be 1:(0.1-10), preferably 1:(0.5-5), and more preferably 1:(1-3).
[0037] In step S1, the amount of the dispersion medium used may be selected depending on the amount of the platinum precursor and the carbonaceous support used. Suitably, in step S1, the mass ratio of the platinum precursor to the dispersion medium may be 1:(100-5000), preferably 1:(120-1000), more preferably 1:(150-500), and further preferably 1:(160-300).
[0038] In step S1, the carbonaceous support is conductive carbon black. The conductive carbon black may be one or more of normal conductive carbon black, high conductive carbon black, and ultra-high conductive carbon black. Examples of preferred conductive carbon black include, but are not limited to, one or more of Vulcan XC72, Ketjen EC300J, Ketjen EC600J, Blackpearls 2000, and Blackpearls 3000. The specific surface area of the conductive carbon black is preferably 200 to 2000 m. 2 / g, more preferably 250 to 1500m 2 / g.
[0039] The amounts of the carbonaceous support and the platinum precursor used may be selected according to the target content of platinum to be introduced into the carbonaceous support. In the production method of the present invention, the amounts of the carbonaceous support and the platinum precursor used are amounts such that the content of metallic platinum is 20 to 70% by weight (preferably 30 to 70% by weight, more preferably 35 to 70% by weight) and the content of the carbonaceous support is 30 to 80% by weight (preferably 30 to 70% by weight, more preferably 30 to 65% by weight) based on the total amount of the platinum-carbon catalyst. In a preferred embodiment, the amounts of the carbonaceous support and the platinum precursor used are amounts such that the content of metallic platinum is 50 to 70% by weight (preferably 60 to 70% by weight) and the content of the carbonaceous support is 30 to 50% by weight (preferably 30 to 40% by weight) based on the total amount of the platinum-carbon catalyst.
[0040] From the viewpoint of further improving the activity and stability of the resulting platinum-carbon catalyst, the production method according to the present invention preferably includes step S0. In step S0, the carbonaceous material in step S1 is pretreated. In step S0, the carbonaceous material is successively treated by a solvent treatment, a first oxidation treatment, a second oxidation treatment, and a high-temperature treatment to obtain a pretreated carbonaceous material. The pretreated carbonaceous material is used in step S1.
[0041] In the solvent treatment, the carbonaceous material is immersed in an organic solvent to obtain a carbonaceous material immersed in the organic solvent. The organic solvent is one or more ketone solvents (e.g., C3-C6 ketones). Preferably, the organic solvent is acetone. The immersion may be performed at room temperature or at elevated temperature. Suitably, the temperature of the organic solvent is 20-70°C, preferably 20-50°C, and more preferably 25-40°C. The immersion time may be selected according to the immersion temperature. In general, the immersion time is 5-24 hours, and preferably 8-12 hours. The amount of the organic solvent used must be sufficient to submerge the carbonaceous material. In general, the volume ratio of the solvent to the carbonaceous material may be (5-100):1, preferably (8-50):1, and more preferably (10-30):1.
[0042] After the immersion in the solvent treatment is completed, the solid and liquid phases may be separated by a conventional method (such as filtration). The obtained solid phase may be dried to obtain a carbonaceous material immersed in an organic solvent. The drying temperature may be 50 to 120°C, and preferably 60 to 80°C. The drying time may be 5 to 24 hours, and preferably 8 to 12 hours. The drying may be performed under normal pressure conditions or under reduced pressure conditions.
[0043] In the first oxidation treatment, the carbonaceous material immersed in the organic solvent is contacted with a first oxidizing agent to obtain a carbonaceous material subjected to the first oxidation treatment. The first oxidizing agent is one or more of hydrogen peroxide and an organic peroxide represented by formula II. [ka]
[0044] In formula II, R1 and R2 are each H, C4-C 12 Alkyl, C6-C 12 Aryl, C7-C 12 R1 and R2 are not H at the same time. R3 is C4-C 12 Straight or branched alkyl of C6 to C 12It is aryl. [ka]
[0045] In the present invention, C4 to C 12 Examples of alkyl include, but are not limited to, n-butyl, sec-butyl, isobutyl, tert-butyl, n-pentyl, neopentyl, isopentyl, tert-pentyl, hexyl (including the various isomers of hexyl), cyclohexyl, octyl (including the various isomers of octyl), nonyl (including the various isomers of nonyl), decyl (including the various isomers of decyl), undecyl (including the various isomers of undecyl), and dodecyl (including the various isomers of dodecyl).
[0046] In the present invention, C6 to C 12 Examples of aryl include, but are not limited to, phenyl, naphthyl, methylphenyl, and ethylphenyl.
[0047] In the present invention, C7 to C 12 Examples of aralkyl include, but are not limited to, phenylmethyl, phenylethyl, phenyl-n-propyl, phenyl-n-butyl, phenyl-tert-butyl, phenyl-isopropyl, phenyl-n-pentyl, and phenyl-n-butyl.
[0048] Specific examples of organic peroxides include, but are not limited to, tert-butyl hydroperoxide, cumene hydroperoxide, ethylbenzene hydroperoxide, cyclohexyl hydroperoxide, diisopropylbenzene peroxide, dibenzoyl peroxide, di-tert-butyl peroxide, and lauroyl peroxide.
[0049] Preferably, the first oxidizing agent is hydrogen peroxide.
[0050] In the first oxidation treatment, the carbonaceous material immersed in an organic solvent is contacted with the first oxidizing agent in a liquid phase in the presence of a liquid dispersion medium. The liquid dispersion medium may be water and / or a C1-C4 alcohol, and is preferably water. In a preferred embodiment, the first oxidizing agent is dissolved in the liquid dispersion medium to form a first oxidizing agent solution, and the first oxidizing agent solution is contacted with the carbonaceous material immersed in an organic solvent. In this preferred embodiment, a hydrogen peroxide solution is preferably used as the first oxidizing agent solution. The hydrogen peroxide solution may have a concentration of 8 to 30% by weight, and is preferably 10 to 20% by weight.
[0051] In the first oxidation treatment, the contact temperature is suitably 20 to 70°C, preferably 25 to 50°C, and more preferably 25 to 40°C. The contact time may be selected according to the contact temperature. The contact time is preferably 5 to 24 hours, and more preferably 8 to 12 hours. The amount of the first oxidizing agent used may be selected according to the amount of the carbonaceous material immersed in the organic solvent. The mass ratio of the first oxidizing agent to the carbonaceous material immersed in the organic solvent may be (5 to 30):1, and preferably (10 to 25):1.
[0052] After the treatment with the first oxidizing agent in the first oxidation treatment is completed, the solid and liquid phases may be separated by a conventional method (such as filtration). The obtained solid phase may be dried to obtain the carbonaceous material subjected to the first oxidation treatment. The drying temperature may be 80 to 120°C, and preferably 90 to 110°C. The drying time may be 5 to 24 hours, and preferably 8 to 24 hours. The drying may be performed under normal pressure conditions or under reduced pressure conditions.
[0053] In the second oxidation treatment, the carbonaceous material subjected to the first oxidation treatment is contacted with a second oxidizing agent to obtain a carbonaceous material subjected to the second oxidation treatment. The second oxidizing agent is HNO3 and / or H2SO4. Preferably, the second oxidizing agent is HNO3. The mass ratio of the second oxidizing agent to the carbonaceous material subjected to the second oxidation treatment is (5-50):1, preferably (10-30):1, and more preferably (12-20):1.
[0054] In the second oxidation treatment, the carbonaceous material subjected to the first oxidation treatment is contacted with a second oxidizing agent in the presence of a liquid dispersion medium. The liquid dispersion medium may be water and / or a C1-C4 alcohol, and is preferably water. In a preferred embodiment, the second oxidizing agent is dissolved in the liquid dispersion medium to form a second oxidizing agent solution, and the second oxidizing agent solution is contacted with the carbonaceous material subjected to the first oxidation treatment. In this preferred embodiment, preferably, nitric acid is used as the second oxidizing agent solution. The concentration of nitric acid may be 25-68% by weight, and is preferably 30-40% by weight.
[0055] In the second oxidation treatment, the contact temperature is preferably 50 to 90° C., more preferably 55 to 80° C., and further preferably 60 to 75° C. In the second oxidation treatment, the contact time may be selected depending on the contact temperature. Suitably, the contact time may be 5 to 24 hours, and preferably 5 to 12 hours.
[0056] After the treatment with the second oxidizing agent in the second oxidation treatment is completed, the solid and liquid phases may be separated by a conventional method (such as filtration). The obtained solid phase may be dried to obtain a carbonaceous material subjected to the second oxidation treatment. The drying temperature may be 80 to 120° C. The drying time may be 5 to 15 hours, and preferably 8 to 12 hours. The drying may be performed under normal pressure conditions or under reduced pressure conditions.
[0057] In the high-temperature treatment, the carbonaceous material that has been subjected to the second oxidation treatment is calcined in an inert atmosphere to obtain a pre-treated carbonaceous material. The calcination temperature is 300 to 700°C, preferably 500 to 600°C. The inert atmosphere may be an atmosphere formed by nitrogen gas and / or a Group 0 gas. An example is an atmosphere formed by one or more gases selected from nitrogen gas, argon gas, and helium gas. The calcination time may be selected depending on the calcination temperature. The calcination time is preferably 2 to 8 hours, more preferably 3 to 6 hours.
[0058] In the manufacturing method of the present invention, in step S1, the carbonaceous material, the platinum precursor, the complexing agent, and the dispersion medium are dispersed by ultrasonic waves. This allows the carbonaceous material and the platinum precursor to be completely mixed. Preferably, the ultrasonic output per 1 L of the dispersion medium is 1 to 20 W, and more preferably 2 to 12 W. The dispersion time by ultrasonic waves can be 0.2 to 1 hour. A normal ultrasonic dispersion device may be used to disperse the carbonaceous material, the platinum precursor, the complexing agent, and the dispersion medium.
[0059] In the production method of the present invention, in the dispersion obtained in step S1, the platinum content in the liquid phase of the first dispersion is relatively low, and the ratio of platinum precursor attached to the carbonaceous material is high. In the production method of the present invention, C1 / C0<0.5. C1 / C0 is preferably 0.15 to 0.49, more preferably 0.15 to 0.45, and further preferably 0.2 to 0.4. Here, the definitions of each symbol are as follows. C0: Molar concentration of platinum precursor in the dispersion medium (C0=m Pt / V 分散媒 ) m Pt : Molar amount of platinum precursor (mol) ·V 分散媒 : Volume of dispersion medium (L) C1: Molar concentration of platinum contained in the liquid phase of the first dispersion obtained in step S1
[0060] In the present invention, the molar concentration C1 of platinum contained in the liquid phase of the first dispersion is measured by inductively coupled plasma emission spectroscopy (ICP method). The specific test method is as follows. 1. Measure the mass and volume of the first dispersion. 2. Take a certain volume of the dispersion from the first dispersion and measure it. This volume is called V1. 3. Filter the dispersion with volume V1 through a mobile phase filter (pore size of the filter membrane: 0.22 μm). Wash the solid phase with deionized water. The filtered liquid and washing liquid are collected to form the liquid phase. The total volume of the liquid phase is V2. Take a sample from the liquid phase and measure the molar concentration of platinum contained in the liquid phase by ICP. This molar concentration is C2. Calculate the molar concentration of platinum contained in the first dispersion by C1 = C2 × V2 / V1.
[0061] In the production method of the present invention, in step S2, the pH value of the first dispersion obtained from step S1 is adjusted to 8 to 14, preferably 8 to 12. A pH adjuster may be added to the first dispersion to adjust the pH value to 8 to 14 (preferably 8 to 12). Preferably, the pH adjuster is one or more of sodium carbonate, potassium carbonate, ammonia, potassium hydroxide, and sodium hydroxide. Preferably, the pH adjuster is added as an aqueous solution. The concentration of the aqueous solution may be selected as in the conventional manner and is not particularly limited.
[0062] In the production method of the present invention, in step S3, the reducing agent is an acidic organic reducing agent. Preferably, the reducing agent is one or more of formic acid, citric acid, and tartaric acid. More preferably, the reducing agent contains formic acid. Even more preferably, the reducing agent is formic acid.
[0063] In the production method of the present invention, in step S3, the amount of the reducing agent used is greater than the stoichiometric ratio. The molar ratio of the reducing agent to the platinum precursor as platinum element is generally 5 to 1000:1, preferably (50 to 600):1, more preferably (80 to 400):1, and further preferably (100 to 200):1.
[0064] In the production method of the present invention, in step S3, the reducing agent is brought into contact with the second dispersion at 50 to 140°C. In a preferred embodiment, in step S3, the reducing agent is brought into contact with the second dispersion at 55 to 90°C to cause a reduction reaction. According to this preferred embodiment, in the finally obtained platinum-carbon catalyst, the metallic platinum particles are more uniformly dispersed on the carbonaceous support. The particle size of the metallic platinum particles also becomes more uniform. In this preferred embodiment, more preferably, in step S3, the reducing agent is brought into contact with the second dispersion at 60 to 80°C to cause a reduction reaction.
[0065] In step S3, the reduction reaction time may be selected depending on the temperature of the reduction reaction. In general, the reduction reaction time in step S3 may be 2 to 12 hours, preferably 4 to 10 hours, and more preferably 6 to 8 hours. In step S3, the reduction reaction is carried out in an inert atmosphere. Examples of the inert atmosphere include an atmosphere formed by nitrogen gas and / or a Group 0 gas (such as argon gas and / or helium gas).
[0066] In a preferred embodiment, the reduction reaction temperature is 60 to 80° C., and the reduction reaction time is 6 to 8 hours. According to this preferred embodiment, the activity and stability of the finally obtained platinum-carbon catalyst can be further improved.
[0067] In the production method of the present invention, a solid content may be separated from the reduction mixture obtained in step S3 by a conventional separation method. The separated solid content is then washed with water and dried to obtain a platinum-carbon catalyst. In general, the reduction mixture obtained in step S3 may be separated into solid and liquid by a combination of one or more of filtration, centrifugation, and sedimentation to obtain a solid content. The drying may be thermal drying or freeze-drying. The temperature of the thermal drying may be 55 to 85°C, preferably 60 to 70°C. The temperature of the freeze-drying may be -30°C to 5°C. The drying time may be selected depending on the drying method and drying temperature. The drying time may generally be 4 to 24 hours, preferably 5 to 15 hours.
[0068] According to a third aspect of the present invention, there is provided a platinum-carbon catalyst obtainable by the process according to the second aspect of the present invention.
[0069] In the platinum-carbon catalyst produced by the production method according to the second aspect of the present invention, 50% or more of the metallic platinum particles have a contact angle of 70° or less with the support. For example, 50 to 75% of the metallic platinum particles have a contact angle of 70° or less with the support. Preferably, 55% or more of the metallic platinum particles have a contact angle of 70° or less with the support. For example, 55 to 70% of the metallic platinum particles have a contact angle of 70° or less with the support. More preferably, 60% or more of the metallic platinum particles have a contact angle of 70° or less with the support. In the platinum-carbon catalyst produced by the production method according to the second aspect of the present invention, the contact angle of the metallic platinum particles with the carbonaceous support is generally 40 to 70°.
[0070] In the platinum-carbon catalyst produced by the production method according to the second embodiment of the present invention, the average particle size of the metallic platinum particles contained in the platinum-carbon catalyst is 3 to 6 nm.
[0071] The platinum-carbon catalyst produced by the method according to the second aspect of the present invention has an increased electrochemically active surface area. The electrochemically active surface area (ECSA) of the platinum-carbon catalyst produced by the method according to the second aspect of the present invention is 70 m 2 ·g -1 -Pt or more, preferably 70 to 120 m 2 ·g -1 -Pt, more preferably 80 to 120 m 2 ·g -1 The mass specific activity of the platinum-carbon catalyst according to the present invention is 0.2 A mg -1 -Pt or more, preferably 0.2 to 0.25 A mg -1 -Pt.
[0072] The platinum-carbon catalyst according to the invention is particularly suitable for use in fuel cells. According to a fourth aspect of the invention, the invention provides the use of a platinum-carbon catalyst according to the first or third aspect of the invention in a fuel cell.
[0073] According to a fifth aspect of the invention, there is provided a hydrogen fuel cell, the anode and / or cathode of which comprises a platinum-carbon catalyst according to the first or third aspect of the invention. EXAMPLES
[0074] The present invention will be described in detail below with reference to examples. However, the scope of the present invention is not limited to these examples.
[0075] In the following Examples and Comparative Examples, a Tecnai G2 F20 (FEI Company) was used for the transmission electron microscope analysis. The sample preparation method is as follows. 1. Approximately 1 mg of sample was taken and dispersed in 60-80% by weight of ethanol aqueous solution. Dispersed by ultrasonic for 10 minutes. 2. A small amount of the dispersion was pipetted onto a copper grid for electron microscopy. The copper grids used were either microgrids or ultrathin microgrids, and neither ultrathin carbon films nor carbon support films were used.
[0076] A specific method for measuring the contact angle of metallic platinum particles with respect to a support in a platinum-carbon catalyst is as follows. 1. Single-layer particles (particles with no overlapping Pt / C layers) were selected. 2. The transmission electron microscope was adjusted to bright field mode and a field of view was selected in which the hemispherical surface (approximately spherical surface) of the Pt particles was visible. 3. As shown in Figure 1, the contact angle (θ) between the straight line of the carbon layer and the tangent line drawn to the contact arc between the Pt particle and the carbon support surface was determined. 4. Eight different fields of view were selected, and the contact angle of the platinum particles in each field of view was measured and recorded.
[0077] A specific method for measuring the particle size of metallic platinum particles in a platinum-carbon catalyst is as follows. 1. The samples were analyzed under a transmission electron microscope, and eight fields of view were randomly selected where the catalyst particles were not overlapping and were widely dispersed (magnification: 40,000–200,000 times). 2. 50 metallic platinum particles were randomly selected for each field (total: 400). 3. The particle size of the particles was measured and recorded. The average particle size was taken as the average particle size of the metallic platinum particles.
[0078] In the following examples and comparative examples, the molar concentration C1 of platinum contained in the liquid phase of the first dispersion obtained by ultrasonic treatment was determined by inductively coupled plasma emission spectroscopy (ICP method). The specific measurement method is as follows. 1. Measure the mass and volume of the first dispersion. 2. Take a certain volume of the dispersion from the first dispersion and measure it. This volume is called V1. 3. Filter the dispersion with volume V1 through a mobile phase filter (pore size of the filter membrane: 0.22 μm). Wash the solid phase with deionized water. The filtered liquid and washing liquid are collected to form the liquid phase. The total volume of the liquid phase is V2. Take a sample from the liquid phase and measure the molar concentration of platinum contained in the liquid phase by ICP. This molar concentration is C2. Calculate the molar concentration of platinum contained in the first dispersion by C1 = C2 × V2 / V1.
[0079] In the following Examples and Comparative Examples, the composition of the platinum-carbon catalyst was measured by inductively coupled plasma emission spectroscopy (ICP method).
[0080] In the following examples and comparative examples, the electrochemical activity of platinum-carbon catalysts may be measured according to GB / T0042.4-2009 (Proton exchange membrane fuel cells-Part 4: Test methods for electrode catalysts). Specifically, the test method may be a rotating disk. In this test method, a slurry is prepared from the catalyst, drop-coated onto a glassy carbon electrode (diameter: 5 mm), and then dried for testing (at this time, the amount of Pt on the electrode is 18-22 μg / cm). 2The test conditions for the catalytic polarization curve were 0.1M HCOO4 solution (saturated with oxygen gas), voltage sweep range: 0-1.0V (vs. reversible hydrogen electrode (RHE)), sweep rate: 10mV / s, and rotation speed of the rotating disk electrode: 1600r / min. The test method for the electrochemically active surface area (ECSA) was the hydrogen underpotential deposition method (HUPD method) based on the adsorption and desorption of hydrogen atoms on a metal surface. The test conditions were 0.1M HCLO4 solution (saturated with nitrogen gas), voltage sweep range: 0-1.0 (vs. RHE), and sweep rate: 50mV / s. For example, if a monolayer of hydrogen atoms is adsorbed on the Pt surface of the cathode and desorbed from the anode, a CV peak appears in the range of about 0.05 to about 0.4V (vs. RHE).
[0081] A specific method for integrating the CV peaks is as follows. 1. The baseline of the peak is determined by extending to the left the horizontal tangent at the lowest point of the upper curve in the vicinity of 0.4 to 0.6 V of the CV curve. 2. Subtract the double layer current. 3. The areas of desorption and adsorption of hydrogen atoms on the baseline are integrated. This area is called S H Let us assume that. 4. Calculate the electrochemically active surface area (ECSA) of the platinum-carbon catalyst using the following formula:
number
[0082] Mass specific activity of platinum-carbon catalyst (A / mg Pt The formula for calculating ) is as follows:
number
number
[0083] In the following examples and comparative examples, the following conductive carbon blacks were used:
[0084] (1) Product name: Ketjen EC300J (purchased from Lion of Japan), particle size: 50-100 nm, specific surface area: 1200 m 2 / g (2) Product name: Ketjen EC600J (purchased from Lion of Japan), particle size: 50-100 nm, specific surface area: 1500 m 2 / g (3) Product name: Vulcan XC72 (purchased from Carbter), particle size: 50-100 nm, specific surface area: 260 m 2 / g
[0085] Examples 1 to 11 of the present invention will be described below.
[0086] Example 1 (1) Pretreatment of conductive carbon black (Step S0) Conductive carbon black Ketjen EC600J (hereinafter, conductive carbon black may be referred to as "carbon black") was immersed in analytical grade acetone at 25°C for 8 hours. The mass ratio of acetone to conductive carbon black was 20:1. After completion of immersion, solids were obtained by suction filtration. The solids were dried at 65°C for 12 hours to obtain conductive carbon black immersed in acetone.
[0087] The conductive carbon black immersed in acetone was mixed with a hydrogen peroxide solution (mass concentration: 15%) and reacted at 25°C for 12 hours. The mass ratio of hydrogen peroxide to carbon black was 25:1. After the reaction was completed, the reaction mixture was suction filtered. The filter cake was washed three times with distilled water and then vacuum dried. The obtained solid content was dried at 110°C for 24 hours to obtain conductive carbon black that had been subjected to a first oxidation treatment.
[0088] The carbon black subjected to the first oxidation treatment and an aqueous nitric acid solution (mass concentration: 30%) were mixed and reacted at 70°C for 12 hours. The mass ratio of HNO3 to carbon black was 15:1. After the reaction was completed, the reaction mixture was suction filtered. The obtained solid was dried at 110°C for 12 hours to obtain conductive carbon black subjected to the second oxidation treatment.
[0089] The carbon black that had been subjected to the second oxidation treatment was calcined at 600° C. for 4 hours in a nitrogen gas atmosphere to obtain pre-treated conductive carbon black.
[0090] (2) Preparation of Dispersion (Steps S1 and S2) (Process S1) 819g of pretreated conductive carbon black was added to a mixture of 175L of deionized water and 262L of ethylene glycol. After uniform mixing, 700g of sodium acetate was added. Next, an aqueous solution of chloroplatinic acid (containing 5.7mol of chloroplatinic acid) was added. The resulting mixture was ultrasonically dispersed to obtain a dispersion. The mass ratio of the materials was carbon black:chloroplatinic acid:water:ethylene glycol:complexing agent=1.17:3.33:250:416.7:1. The ultrasonic output was 1000W. The ultrasonic dispersion time was 0.5 hours. A sample taken from the dispersion was analyzed, and the molar concentration of platinum contained in the liquid phase of the dispersion was C1, and the molar concentration of the platinum precursor relative to the dispersion medium was C0 (determined from the blending ratio. The same applies below), C1 / C0=0.23. The pH of the dispersion obtained after ultrasonic treatment was 2.
[0091] (Process S2) Sodium carbonate was added to the dispersion obtained after ultrasonic treatment to adjust the pH value of the dispersion to 12.
[0092] (3) Reduction reaction (step S3) The pH-adjusted dispersion was heated to 75°C using a heater. The reducing agent, formic acid, was added and stirred to carry out the reduction reaction. The molar ratio of the reducing agent to chloroplatinic acid was 200:1. After the addition of the reducing agent was completed, the heating conditions of the heater were maintained to continue the reaction for 6 hours.
[0093] After the reaction was completed, the reduction reaction mixture was filtered to recover the solids. -The solid was washed with deionized water until the mass concentration of was less than 50 ppm. The washed solid was dried in vacuum at 60° C. for 12 hours. The dried solid was pulverized to obtain 1000 g of platinum-carbon catalyst. Measurements showed that the platinum mass content in the platinum-carbon catalyst was 54.5% (this is denoted as Pt / C-55%). Analysis of a sample taken from the platinum-carbon catalyst showed that 69% of the metallic platinum contained in the platinum-carbon catalyst had a contact angle of 70° or less with respect to the support (see FIG. 2). Measurements showed that the average particle size of the platinum particles contained in the platinum-carbon catalyst was 3.6 nm (see FIG. 3). The electrochemical properties of the prepared platinum-carbon catalyst were measured, and the experimental results are summarized in Table 1.
[0094] Example 2 A platinum-carbon catalyst was prepared in the same manner as in Example 1, except for the following points: In step S0, the temperature at which the conductive carbon black subjected to the second oxidation treatment was baked under a nitrogen gas atmosphere was changed to 400°C, 500°C, or 700°C to obtain a pre-treated conductive carbon black. The obtained platinum-carbon catalysts are referred to as Pt / C-55%-400, Pt / C-55%-500, and Pt / C-55%-700, respectively.
[0095] In step S1, a sample taken from the dispersion was analyzed. The concentration of platinum in the liquid phase of the dispersion was C1, and the molar concentration of the platinum precursor relative to the dispersion medium was C0. C1 / C0 was 0.39 (400°C), 0.28 (500°C), and 0.31 (700°C).
[0096] In Pt / C-55%-400, the metallic platinum had a contact angle of 70° or less with respect to the support, which was 64%. In Pt / C-55%-500, the metallic platinum had a contact angle of 70° or less with respect to the support, which was 67%. In Pt / C-55%-700, the metallic platinum had a contact angle of 70° or less with respect to the support, which was 66%. The average particle size of the metallic platinum particles in all of the obtained platinum-carbon catalysts was 3 to 6 nm. The electrochemical properties of the prepared platinum-carbon catalysts were measured, and the experimental results are summarized in Table 1.
[0097] Example 3 The platinum-carbon catalysts were prepared in the same manner as in Example 1, except that in step S2, potassium carbonate or sodium hydroxide was added to the dispersion obtained after ultrasonic treatment to adjust the pH of the dispersion to 12. The resulting platinum-carbon catalysts are designated as Pt / C-55%-K2CO3 and Pt / C-55%-NaOH, respectively.
[0098] In Pt / C-55%-K2CO3, the metallic platinum had a contact angle of 70° or less with the support of 56%. In Pt / C-55%-NaOH, the metallic platinum had a contact angle of 70° or less with the support of 58%. The average particle size of the metallic platinum particles in all of the obtained platinum-carbon catalysts was 3 to 6 nm. The electrochemical properties of the prepared platinum-carbon catalysts were measured, and the experimental results are summarized in Table 1.
[0099] Example 4 A platinum-carbon catalyst was prepared in the same manner as in Example 1, except that in step S2, sodium carbonate was added to the dispersion obtained after ultrasonic treatment to adjust the pH of the dispersion to 8 or 10. The resulting platinum-carbon catalysts are designated as Pt / C-55%-pH8 and Pt / C-55%-pH10, respectively.
[0100] In Pt / C-55%-pH8, the metallic platinum had a contact angle of 70° or less with the support of 52%. In Pt / C-55%-pH10, the metallic platinum had a contact angle of 70° or less with the support of 65%. The average particle size of the metallic platinum particles in all of the obtained platinum-carbon catalysts was 3 to 6 nm. The electrochemical properties of the prepared platinum-carbon catalysts were measured, and the experimental results are summarized in Table 1.
[0101] Comparative Example 1 A platinum-carbon catalyst was prepared in the same manner as in Example 1, except for the following points. That is, in step S1, a sodium salt of an organic acid and ethylene glycol were not used. In step S1, a sample taken from the dispersion was analyzed, and C1 / C0 was 0.79, where C1 is the concentration of platinum contained in the liquid phase of the dispersion and C0 is the molar concentration of the platinum precursor relative to the dispersion medium. In the prepared platinum-carbon catalyst, 35% of the metallic platinum had a contact angle of 70° or less with respect to the support (see FIG. 4). The electrochemical properties of the prepared platinum-carbon catalyst were measured, and the experimental results are summarized in Table 1.
[0102] Comparative Example 2 A platinum-carbon catalyst was prepared in the same manner as in Example 2, except for the following points. That is, in step S1, a sodium salt of an organic acid and ethylene glycol were not used. In step S1, a sample taken from the dispersion was analyzed, and the concentration of platinum contained in the liquid phase of the dispersion was C1, and the molar concentration of the platinum precursor relative to the dispersion medium was C0. C1 / C0 was 0.73 (400°C), 0.76 (500°C), and 0.74 (700°C), respectively. In the prepared platinum-carbon catalyst, the metallic platinum having a contact angle of 70° or less with respect to the support was 30% (400°C), 33% (500°C), and 34% (700°C), respectively. The electrochemical properties of the prepared platinum-carbon catalyst were measured, and the experimental results are summarized in Table 1.
[0103] Comparative Example 3 A platinum-carbon catalyst was prepared in the same manner as in Example 3, except for the following points. That is, in step S1, a sodium salt of an organic acid and ethylene glycol were not used. In the prepared platinum-carbon catalyst, the metallic platinum having a contact angle of 70° or less with the support was 29% (potassium carbonate) and 31% (sodium hydroxide), respectively. The electrochemical properties of the prepared platinum-carbon catalyst were measured, and the experimental results are summarized in Table 1.
[0104] Comparative Example 4 A platinum-carbon catalyst was prepared in the same manner as in Example 4, except for the following points. That is, in step S1, a sodium salt of an organic acid and ethylene glycol were not used. In the prepared platinum-carbon catalyst, the metallic platinum having a contact angle of 70° or less with respect to the support was 26% (pH=8) and 30% (pH=10), respectively. The electrochemical properties of the prepared platinum-carbon catalyst were measured, and the experimental results are summarized in Table 1.
[0105] Comparative Example 5 A platinum-carbon catalyst was prepared in the same manner as in Example 1, except for the following points. That is, in step S1, no sodium salt of an organic acid was used. In step S1, a sample taken from the dispersion was analyzed, and C1 / C0 was 0.65, where C1 is the concentration of platinum contained in the liquid phase of the dispersion and C0 is the molar concentration of the platinum precursor relative to the dispersion medium. In the prepared platinum-carbon catalyst, the metallic platinum having a contact angle of 70° or less with respect to the support was 46%. The electrochemical properties of the prepared platinum-carbon catalyst were measured, and the experimental results are summarized in Table 1.
[0106] Comparative Example 6 A platinum-carbon catalyst was prepared in the same manner as in Example 1, except for the following points. That is, in step S3, the reducing agent formic acid was changed to glucose. The amount of glucose used was the same as the amount of formic acid used in step S3 of Example 1. In the platinum-carbon catalyst prepared from step S3, the metallic platinum having a contact angle of 70° or less with respect to the support was 24%. The electrochemical properties of the prepared platinum-carbon catalyst were measured, and the experimental results are summarized in Table 1.
[0107] Comparative Example 7 A platinum-carbon catalyst was prepared in the same manner as in Example 1, except for the following points. That is, in step S3, the amount of formic acid used as the reducing agent was changed so that the molar ratio of the reducing agent to chloroplatinic acid was 2:1. In the platinum-carbon catalyst prepared in step S3, the metallic platinum having a contact angle of 70° or less with respect to the support was 43%. The electrochemical properties of the prepared platinum-carbon catalyst were measured, and the experimental results are summarized in Table 1.
[0108] Example 5 A platinum-carbon catalyst was prepared in the same manner as in Example 1, except for the following points. That is, step S0 was omitted, and conductive carbon black Ketjen EC600J was directly used in step S1 to obtain a dispersion. That is, a platinum-carbon catalyst was prepared from conductive carbon black that was not pretreated. In step S1, a sample taken from the dispersion was analyzed, and the concentration of platinum contained in the liquid phase of the dispersion was C1, and the molar concentration of the platinum precursor relative to the dispersion medium was C0, and C1 / C0 was 0.43. In the platinum-carbon catalyst prepared from step S3, the metallic platinum with a contact angle of 70° or less with respect to the support was 51%. The electrochemical properties of the prepared platinum-carbon catalyst were measured, and the experimental results are summarized in Table 1.
[0109] Example 6 A platinum-carbon catalyst was prepared in the same manner as in Example 1, except for the following points. That is, in step S1, the mass ratio of materials was changed to conductive carbon black: chloroplatinic acid: water: ethylene glycol: complexing agent = 1.17: 3.33: 300: 300: 1. In step S1, a sample taken from the dispersion was analyzed, and the concentration of platinum contained in the liquid phase of the dispersion was C1, and the molar concentration of the platinum precursor relative to the dispersion medium was C0, and C1 / C0 was 0.31. In the platinum-carbon catalyst prepared from step S3, the metallic platinum having a contact angle of 70° or less with respect to the support was 58%. The electrochemical properties of the prepared platinum-carbon catalyst were measured, and the experimental results are summarized in Table 1.
[0110] Comparative Example 8 A platinum-carbon catalyst was prepared in the same manner as in Example 1, except for the following points. That is, in step S1, the mass ratio of materials was changed to conductive carbon black: chloroplatinic acid: water: ethylene glycol: complexing agent = 1.17: 3.33: 30: 550: 1. In step S1, a sample taken from the dispersion was analyzed, and the concentration of platinum contained in the liquid phase of the dispersion was C1, and the molar concentration of the platinum precursor relative to the dispersion medium was C0, and C1 / C0 was 0.59. In the platinum-carbon catalyst prepared from step S3, the metallic platinum having a contact angle of 70° or less with respect to the support was 48%. The electrochemical properties of the prepared platinum-carbon catalyst were measured, and the experimental results are summarized in Table 1.
[0111] Example 7 A platinum-carbon catalyst was prepared in the same manner as in Example 1, except for the following points. That is, in step S1, the ultrasonic dispersion time was changed to 0.25 hours. In step S1, a sample taken from the dispersion was analyzed, and C1 / C0 was 0.37, where C1 is the concentration of platinum contained in the liquid phase of the dispersion and C0 is the molar concentration of the platinum precursor relative to the dispersion medium. In the platinum-carbon catalyst prepared from step S3, 54% of the metallic platinum had a contact angle of 70° or less with respect to the support. The electrochemical properties of the prepared platinum-carbon catalyst were measured, and the experimental results are summarized in Table 1.
[0112] Example 8 A platinum-carbon catalyst was prepared in the same manner as in Example 1, except for the following: In step S3, the molar ratio of the reducing agent to the platinum precursor was changed to 400:1. In the platinum-carbon catalyst prepared in step S3, the metallic platinum having a contact angle of 70° or less with respect to the support was 58%. The electrochemical properties of the prepared platinum-carbon catalyst were measured, and the experimental results are summarized in Table 1.
[0113] Example 9 (1) Pretreatment of conductive carbon black (Step S0) Conductive carbon black, Ketjen EC300J, was immersed in acetone (analytical grade) at 35° C. for 8 hours. The mass ratio of acetone to conductive carbon black was 18:1. After immersion was completed, the solids were obtained by suction filtration. The solids were dried at 65° C. for 8 hours to obtain conductive carbon black immersed in acetone.
[0114] The conductive carbon black immersed in acetone was mixed with a hydrogen peroxide solution (mass concentration: 10%) and reacted at 25°C for 10 hours. The mass ratio of hydrogen peroxide to carbon black was 20:1. After completion of the reaction, the reaction mixture was suction filtered. The obtained solid content was dried at 105°C for 8 hours to obtain conductive carbon black that had been subjected to a first oxidation treatment.
[0115] The conductive carbon black subjected to the first oxidation treatment was mixed with an aqueous nitric acid solution (mass concentration: 35%) and reacted at 65°C for 12 hours. The mass ratio of HNO3 to the conductive carbon black was 12:1. After the reaction was completed, the reaction mixture was suction filtered. The obtained solid was dried at 86°C for 10 hours to obtain the conductive carbon black subjected to the second oxidation treatment.
[0116] The carbon black that had been subjected to the second oxidation treatment was calcined at 600° C. in a nitrogen gas atmosphere for 4 hours to obtain pre-treated conductive carbon black.
[0117] (2) Preparation of Dispersion (Steps S1 and S2) (Process S1) The pretreated conductive carbon black was added to a mixture of 7.5 L of deionized water and 11.3 L of ethylene glycol. After uniform mixing, 30 g of sodium formate was added. Then, an aqueous solution of chloroplatinic acid was added. The resulting mixture was ultrasonically dispersed to obtain a dispersion. The mass ratio of the materials was carbon black:chloroplatinic acid:water:ethylene glycol:complexing agent=1.17:3.33:250:416.7:1. The ultrasonic output was 300 W. The ultrasonic dispersion time was 0.5 hours. A sample taken from the dispersion was analyzed, and the concentration of platinum contained in the liquid phase of the dispersion was C1, and the molar concentration of the platinum precursor relative to the dispersion medium was C0, and C1 / C0 was 0.35. The pH of the dispersion obtained after ultrasonic treatment was 3.
[0118] (Process S2) Sodium carbonate was added to the dispersion obtained after ultrasonic treatment to adjust the pH value of the dispersion to 12.
[0119] (3) Reduction reaction (step S3) The pH-adjusted dispersion was heated to 65°C using a heater. The reducing agent, formic acid, was added and stirred to cause a reduction reaction. The molar ratio of the reducing agent to chloroplatinic acid was 100:1. After the addition of the reducing agent was completed, the heating conditions of the heater were maintained to allow the reaction to continue for 6 hours.
[0120] After the reaction was completed, the reduction reaction mixture was filtered to recover the solids. -The solid was washed with deionized water until the mass concentration of was less than 50 ppm. The washed solid was dried in vacuum at 60°C for 6 hours. The solid was pulverized to obtain a platinum-carbon catalyst. The particle size of platinum in the catalyst was 4.7 nm. Measurements showed that the mass content of platinum in the platinum-carbon catalyst was 68%. Analysis of a sample taken from the platinum-carbon catalyst showed that 52% of the metallic platinum contained in the platinum-carbon catalyst had a contact angle of 70° or less with respect to the support. Measurements showed that the average particle size of platinum particles contained in the platinum-carbon catalyst was 4.7 nm. The electrochemical properties of the prepared platinum-carbon catalyst were measured, and the experimental results are summarized in Table 1.
[0121] Example 10 (1) Pretreatment of conductive carbon black (Step S0) Conductive carbon black, Vulcan XC72, was pretreated in the same manner as in Example 9 to obtain a pretreated conductive carbon black.
[0122] (2) Preparation of Dispersion (Steps S1 and S2) (Process S1) The pretreated conductive carbon black was added to a mixture of 15 L of deionized water and 22.5 L of ethylene glycol. After uniform mixing, 60 g of sodium acetate was added. Then, an aqueous solution of chloroplatinic acid was added. The resulting mixture was ultrasonically dispersed to obtain a dispersion. The mass ratio of the materials was carbon black: chloroplatinic acid: water: ethylene glycol: complexing agent = 4.0: 3.33: 250: 416.7: 1. The ultrasonic output was 300 W. The dispersion time by ultrasonic was 0.6 hours. A sample taken from the dispersion was analyzed, and the concentration of platinum contained in the liquid phase of the dispersion was C1, and the molar concentration of the platinum precursor relative to the dispersion medium was C0, and C1 / C0 was 0.4. The pH of the dispersion obtained after ultrasonic treatment was 12.
[0123] (Process S2) Sodium carbonate was added to the dispersion obtained after ultrasonic treatment to adjust the pH value of the dispersion to 9.
[0124] (3) Reduction reaction (step S3) The dispersion prepared in Example 10 was used to carry out a reduction reaction in the same manner as in Example 9. After completion of the reaction, the reduction reaction mixture was filtered to recover the solid content. The Cl content in the filtrate was 0.01%. - The solid was washed with deionized water until the mass concentration of was less than 50 ppm. The washed solid was dried in vacuum at 60°C for 8 hours to obtain a dried solid. The dried solid was pulverized to obtain a platinum-carbon catalyst. Measurement revealed that the mass content of platinum in the platinum-carbon catalyst was 39%. Analysis of a sample taken from the platinum-carbon catalyst revealed that 67% of the metallic platinum contained in the platinum-carbon catalyst had a contact angle of 70° or less with respect to the support. Measurement revealed that the average particle size of the platinum particles contained in the platinum-carbon catalyst was 3.5 to 4.2 nm. The electrochemical properties of the prepared platinum-carbon catalyst were measured, and the experimental results are summarized in Table 1.
[0125] Example 11 A platinum-carbon catalyst was prepared in the same manner as in Example 10, except for the following points. That is, step S0 was omitted, and carbon black was directly used in step S1 to obtain a dispersion. That is, a platinum-carbon catalyst was prepared from carbon black that was not pretreated. In step S1, a sample taken from the dispersion was analyzed, and the concentration of platinum contained in the liquid phase of the dispersion was C1, and the molar concentration of the platinum precursor relative to the dispersion medium was C0, and C1 / C0 was 0.49. When the sample was analyzed in step S3, the metallic platinum with a contact angle of 70° or less with respect to the support was 51%. The electrochemical properties of the prepared platinum-carbon catalyst were measured, and the experimental results are summarized in Table 1.
[0126] Comparative Example 9 A platinum-carbon catalyst was prepared in the same manner as in Example 10, except for the following points. That is, in step S1, a sodium salt of an organic acid and ethylene glycol were not used. In step S1, a sample taken from the dispersion was analyzed, and C1 was the concentration of platinum contained in the liquid phase of the dispersion, and C0 was the molar concentration of the platinum precursor relative to the dispersion medium, and C1 / C0 was 0.74. When the sample was analyzed in step S3, the metallic platinum having a contact angle of 70° or less with respect to the support was 34%. The electrochemical properties of the prepared platinum-carbon catalyst were measured, and the experimental results are summarized in Table 1.
[0127] Comparative Example 10 A platinum-carbon catalyst was prepared in the same manner as in Example 10, except for the following points. That is, in step S3, the reducing agent formic acid was changed to hydrazine hydrate. The amount of hydrazine hydrate used was the same as the amount of formic acid used in step S3 of Example 1. When the sample was analyzed in step S3, the metallic platinum having a contact angle of 70° or less with respect to the support was 21%. The electrochemical properties of the prepared platinum-carbon catalyst were measured, and the experimental results are summarized in Table 1.
[0128] Comparative Example 11 A platinum-carbon catalyst was prepared in the same manner as in Example 10, except for the following points. That is, in step S3, the amount of formic acid used as the reducing agent was changed so that the molar ratio of the reducing agent to chloroplatinic acid was 2:1. When the sample was analyzed in step S3, the metallic platinum having a contact angle of 70° or less with respect to the support was 45%. The electrochemical properties of the prepared platinum-carbon catalyst were measured, and the experimental results are summarized in Table 1.
[0129] Example 12 A platinum-carbon catalyst was prepared in the same manner as in Example 1, except for the following: in step S1, 1,2-propylene glycol was used instead of ethylene glycol. The electrochemical properties of the prepared platinum-carbon catalyst were measured, and the experimental results are summarized in Table 1.
[0130] Example 13 A platinum-carbon catalyst was prepared in the same manner as in Example 1, except for the following: in step S1, 1,3-propylene glycol was used instead of ethylene glycol. The electrochemical properties of the prepared platinum-carbon catalyst were measured, and the experimental results are summarized in Table 1.
[0131] 2 and 3 are transmission electron microscope images (TEM images) of the platinum-carbon catalysts prepared in Example 1 and Comparative Example 1, respectively. As can be seen from Figs. 2 and 3, in the platinum-carbon catalyst prepared in Example 1, most of the metallic platinum particles had a contact angle with the support of less than 70°. On the other hand, in the platinum-carbon catalyst prepared in Comparative Example 1, most of the metallic platinum particles had a contact angle with the support of more than 70°.
[0132] 4 and 5 are transmission electron microscope images of the platinum-carbon catalyst prepared in Example 1 or Comparative Example 1, respectively. FIG. 7 is a transmission electron microscope image of a commercially available catalyst (JM HiSPEC 13100, Pt / C: 70 wt%, abbreviated as "JM-70%"). As can be seen from a comparison of FIG. 4 with FIG. 5 and FIG. 7, in the platinum-carbon catalyst prepared in Example 1, the dispersion of metallic platinum particles on the support was good, the metallic platinum formed very uniform cluster particles, and the particle size was relatively uniform. On the other hand, in the platinum-carbon catalyst prepared in Comparative Example 1, the dispersion of metallic platinum on the support was relatively low, and the size of the metallic platinum particles was not sufficiently uniform. FIG. 6 is a statistical result of the particle size of metallic platinum particles included in the field of view of the transmission electron microscope image of the platinum-carbon catalyst prepared in Example 1. As can be seen from FIG. 6, the particle size of metallic platinum particles included in the platinum-carbon catalyst prepared in Example 1 was relatively uniform.
[0133] The test results of the electrochemical properties of the platinum-carbon catalysts prepared in Examples 1 to 11 and Comparative Examples 1 to 11 are summarized in Table 1. As can be seen from Table 1, the platinum-carbon catalysts according to the present invention had improved stability of electrochemical activity. Furthermore, the amounts of the platinum-carbon catalysts prepared in Examples 1 to 11 were all on the order of kilograms. This shows that the production method according to the present invention is suitable for batch production of platinum-carbon catalysts.
[0134] [Table 1]
[0135] The preferred embodiments of the present invention have been described in detail above. However, the present invention is not limited to these. Various simple modifications can be made to the technical solutions of the present invention within the scope of the technical idea of the present invention, including combinations of various technical features with any other suitable means. Such simple modifications and combinations are also included in the contents disclosed by the present invention and should be considered to be within the protection scope of the present invention.
Claims
1. A platinum-carbon catalyst comprising a carbonaceous support and metallic platinum particles supported on the carbonaceous support, 50% or more of the metallic platinum particles have a contact angle of 70° or less with respect to the carbonaceous support; Preferably, 55% or more of the metallic platinum particles have a contact angle of 70° or less with respect to the carbonaceous support (e.g., 55-70% or 60-70% of the metallic platinum particles have a contact angle of 70° or less with respect to the support), More preferably, the contact angle of the metallic platinum particles with respect to the carbonaceous support is between 40° and 70°; Based on the total amount of the platinum-carbon catalyst, The content of the metallic platinum is 20 to 70% by weight, The content of the carbonaceous support is 30 to 80% by weight; Preferably, based on the total amount of the platinum-carbon catalyst, The content of the metallic platinum is 50 to 70% by weight, The content of the carbonaceous support is 30 to 50% by weight; Platinum-carbon catalyst.
2. The average particle size of the metallic platinum particles contained in the platinum-carbon catalyst is 3 to 6 nm. The platinum-carbon catalyst of claim 1.
3. The platinum-carbon catalyst essentially consists of the carbonaceous support and metallic platinum particles supported on the carbonaceous support. The platinum-carbon catalyst of claim 1.
4. The platinum-carbon catalyst comprises the carbonaceous support and metallic platinum particles supported on the carbonaceous support. The platinum-carbon catalyst of claim 1.
5. The carbonaceous support is conductive carbon black, Preferably, the specific surface area of the conductive carbon black is 200 to 2000 m 2 / g (preferably 250 to 1500 m 2 / g), The platinum-carbon catalyst of claim 1.
6. The electrochemically active surface area of the platinum-carbon catalyst is 70 to 120 m 2 ・g -1 -Pt, Preferably, the mass specific activity of the platinum-carbon catalyst is 0.2 A mg -1 -Pt or more (preferably 0.2 to 0.25 A mg -1 -Pt), The platinum-carbon catalyst of claim 1.
7. A method for producing a platinum-carbon catalyst, comprising the steps of: Step S1: A step of dispersing a carbonaceous material, a platinum precursor, a complexing agent, and a dispersion medium to obtain a first dispersion, The complexing agent is a carboxylate, The dispersion medium is C 2 ~C 4 and water, the volume ratio of the dihydric alcohol to the water is (0.1-10):1; the molar ratio of said platinum precursor to said complexing agent is 1:(0.1-10); Step S2: adjusting the pH value of the first dispersion to 8 to 14 to obtain a second dispersion; Step S3: A step of adding a reducing agent to the second dispersion, contacting the reducing agent with the platinum precursor in the second dispersion, and causing a reduction reaction, The reducing agent is an acidic organic reducing agent, The molar ratio of the reducing agent to the platinum precursor, as elemental platinum, is generally (5-1000):
1.
8. The method according to claim 7, wherein the following relationship is satisfied: C 1 / C 0 <0.5(C 1 / C 0 is, for example, 0.15 to 0.49, preferably 0.15 to 0.45, and more preferably 0.2 to 0.
4. During the ceremony, C 0 : Molar concentration of the platinum precursor relative to the dispersion medium in the step S1 C 1 : Molar concentration of platinum contained in the liquid phase of the first dispersion obtained in step S1
9. In the step S1, the complexing agent is an alkali metal salt of a monocarboxylic acid and / or an ammonium salt of a monocarboxylic acid; Preferably, the complexing agent is one or more compounds of formula I: R-COOM (Formula I) In formula I, R is hydrogen, C 1 ~C 6 Alkyl or C 1 ~C 6 is haloalkyl, M is an alkali metal ion or an ammonium ion; Preferably, the complexing agent is one or more of sodium formate, sodium acetate, sodium monochloroacetate, sodium dichloroacetate and sodium trichloroacetate; Preferably, the molar ratio of said platinum precursor to said complexing agent is 1:(0.5-5) (preferably 1:(1-3)); The method of claim 7.
10. In the step S1, the carbonaceous material, the platinum precursor, the complexing agent, and the dispersion medium are dispersed by ultrasonic waves, The ultrasonic output for 1 L of the dispersion medium is 1 to 20 W (preferably 2 to 12 W); The ultrasonic dispersion time is 0.1 to 5 hours (for example, 0.2 to 1 hour). The method of claim 7.
11. In the step S1, the volume ratio of the dihydric alcohol to the water is (0.5 to 5):1 (preferably (0.67 to 3):1), Preferably, the dihydric alcohol is ethylene glycol, 1,2-propylene glycol, or 1,3-propylene glycol; More preferably, the dihydric alcohol is ethylene glycol. The method of claim 7.
12. In the step S1, the mass ratio of the platinum precursor to the dispersion medium is 1:(100 to 5000) (preferably 1:(120 to 1000), more preferably 1:(160 to 300)); The method of claim 7.
13. The method of claim 7 further comprising the steps of: Step S0: pre-treating the carbonaceous material of step S1, in which the carbonaceous material is successively treated with a solvent treatment, a first oxidation treatment, a second oxidation treatment and a high temperature treatment to obtain a pre-treated carbonaceous material; Where: In the solvent treatment, the carbonaceous material is immersed in an organic solvent to obtain a carbonaceous material immersed in an organic solvent; Preferably, the organic solvent is one or more of a ketone solvent; In the first oxidation treatment, the carbonaceous material immersed in the organic solvent is contacted with a first oxidizing agent to obtain a carbonaceous material subjected to a first oxidation treatment; The first oxidizing agent is one or more of hydrogen peroxide and an organic peroxide represented by formula II, 【Chemistry 1】 In formula II, R 1 and R 2 are H and C, respectively. 4 ~C 12 Alkyl, C 6 ~C 12 Aryl, C 7 ~C 12 aralkyl and the following structure: 【Chemistry 2】 R 1 and R 2 At the same time, it is not H. R 3 is C 4 ~C 12 or C 6 ~C 12 is aryl; In the second oxidation treatment, the carbonaceous material subjected to the first oxidation treatment is contacted with a second oxidizing agent to obtain a carbonaceous material subjected to a second oxidation treatment; The second oxidant is HNO 3 and / or H 2 SO 4 one or more of: In the high-temperature treatment, the carbonaceous material that has been subjected to the second oxidation treatment is fired in an inert atmosphere at 300 to 700° C. (eg, 300 to 600° C.) to obtain the pre-treated carbonaceous material.
14. In the solvent treatment in step S0, The immersion time is 5 to 24 hours. a mass ratio of the solvent to the carbonaceous material is (5 to 100):1; Preferably, the temperature of the organic solvent in the solvent treatment is 20 to 70° C. (preferably 25 to 40° C.); Preferably, the organic solvent in the solvent treatment is acetone. The method of claim 13.
15. In the first oxidation treatment in step S0, The contact time is from 5 to 24 hours. a mass ratio of the first oxidant to the carbonaceous material immersed in the organic solvent is (5 to 30):1; Preferably, the contact temperature in the first oxidation treatment is 20 to 70° C. (preferably 25 to 40° C.); Preferably, in the first oxidation treatment, the first oxidizing agent is provided as an aqueous solution, and the content of the first oxidizing agent in the aqueous solution is 5 to 30 wt %; Preferably, the first oxidizing agent in the first oxidation treatment is hydrogen peroxide. The method of claim 13.
16. In the second oxidation treatment in step S0, The contact time is from 5 to 24 hours. the mass ratio of the second oxidizing agent to the carbonaceous material subjected to the first oxidation treatment is (5 to 50):1 (preferably (10 to 30):1, more preferably (12 to 20):1); Preferably, the contact temperature in the second oxidation treatment is 50 to 90° C. Preferably, the second oxidizing agent in the second oxidation treatment is nitric acid; Preferably, the concentration of the nitric acid is 25 to 68% by weight (preferably 30 to 40% by weight); The method of claim 13.
17. In the high-temperature treatment in step S0, the firing temperature is 500 to 600° C., Preferably, the firing time in the high-temperature treatment is 2 to 8 hours (preferably 3 to 6 hours); The method of claim 13.
18. In the step S1, the water-soluble platinum precursor is one or more of sodium chloroplatinate, ammonium hexachloroplatinate, potassium hexachloroplatinate, sodium hexachloroplatinate, platinum tetrachloride, tetraammine platinum nitrate, platinum nitrate, chloroplatinic acid, potassium chloroplatinate, and sodium chloroplatinate; Preferably, in step S1, the carbonaceous material is conductive carbon black, The specific surface area of the conductive carbon black is preferably 200 to 2000 m 2 / g, more preferably 250 to 1500m 2 / g, The method of claim 7.
19. In the step S2, the pH value of the first dispersion obtained from the step S1 is adjusted to 8 to 12; Adjusting the pH value, for example by adding sodium carbonate, potassium carbonate or sodium hydroxide; The method of claim 7.
20. In the step S3, the reducing agent is one or more of formic acid, citric acid, and tartaric acid; The reducing agent preferably comprises, and more preferably is, formic acid; Preferably, in step S3, the molar ratio of the reducing agent to the water-soluble platinum precursor is (50-600):1 (preferably (80-400):1, more preferably (100-200):1); In this case, the water-soluble platinum precursor is calculated as metallic platinum; The method of claim 7.
21. In the above step S3, the reduction temperature is 50 to 140° C. (preferably 55 to 90° C., more preferably 60 to 80° C.), Preferably, in step S3, the reduction time is 2 to 12 hours. The method of claim 7.
22. Use of the platinum-carbon catalyst according to any one of claims 1 to 6 in a fuel cell.
23. The present invention is provided with an anode and / or a cathode comprising the platinum-carbon catalyst according to any one of claims 1 to 6. Hydrogen fuel cell.
Citation Information
Patent Citations
Method for preparing Pt / C catalysts for fuel batter with proton exchanging film
CN101096016A
Platinum-carbon catalyst and preparation method and application thereof
CN111146448A
Carbon material supported platinum catalyst, and preparation method and application thereof
CN113363515A
Electrode catalyst
JP2008047472A