A6xxx alloys for extrusion with improved properties and method for producing extruded products

A 6xxx aluminum alloy with controlled cooling and specific element composition addresses ductility and thermal stability issues in vehicle collision components, ensuring improved crushing and corrosion resistance without shape distortions.

JP2024543100AActive Publication Date: 2024-11-19NORSK HYDRO ASA
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
JP2024529751
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2022-11-23
Publication Date
2024-11-19
Estimated Expiration
2042-11-23

AI Technical Summary

Technical Problem

Existing Al-Mg-Si alloys used in structural components for vehicle collisions face issues with ductility, crushing properties, and thermal stability, particularly when exposed to high temperatures, and rapid quenching methods lead to shape distortions in complex profiles.

Method used

A 6xxx aluminum alloy composition with specific ranges of Mg, Si, Ti, V, and other elements, combined with a controlled cooling rate after extrusion, to enhance ductility, crushing properties, and thermal stability, avoiding rapid quenching distortions.

Benefits of technology

The alloy achieves improved ductility, crushing performance, and thermal stability without shape distortions, suitable for complex profiles, with enhanced corrosion resistance and recrystallized grain structure.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024543100000004
    Figure 2024543100000004
  • Figure 2024543100000005
    Figure 2024543100000005
  • Figure 2024543100000006
    Figure 2024543100000006
Patent Text Reader

Abstract

The present invention includes, by weight percent, Mg: 0.45 to 1.2, Si: 0.40 to 1.0, Ti: 0.05 to 0.20, V: 0.05 to 0.15, Cu: less than 0.30, Mn: less than 0.30, Cr: less than 0.15, Zr: less than 0.15, Fe: less than 0.50, Zn: less than 0.50, and the balance being aluminum and unavoidable impurities, the content of Ti+V being 0.10 to 0.30, and Si eff The present invention relates to an Al-Mg-Si aluminum alloy having an Al / Mg ratio of less than 1.0, which has improved ductility and crush properties, good energy absorption, corrosion resistance and temperature stability, and is particularly useful for structural components in areas exposed during vehicle collisions.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to an Al-Mg-Si aluminum alloy and its extrusion product, which has excellent ductility and crushing properties, good energy absorption and temperature stability, and is particularly useful for structural parts exposed during vehicle collisions. The extrusion product according to the present invention also has high corrosion resistance. [Background technology]

[0002] WO 2007 / 094686 discloses Al-Mg-Si alloys with 0-0.4 wt. Ti additions to improve the alloy's ductility. The range of Mg and Si is broad, with a preferred range of Si / Mg ratio of 1.4. The patent application also teaches that the best temperature stability is found at high Si / Mg ratios.

[0003] EP 0936278 claims that the addition of 0.05-0.20 wt% V in combination with 0.15-0.4 wt% Mn to Al-Mg-Si alloys improves ductility. According to this patent application, the preferred Mn / Fe ratio is 0.45-1.0, more preferably 0.67-1.0. The role of Ti in EP 0936278 is clearly stated as a grain refiner during casting or welding. The preferred range of Ti is 0.1 wt% or less.

[0004] In the prior art, the profiles are water quenched after extrusion, however, water quenching can lead to distortion of the shape of the extruded part, the risk of distortion increasing as the complexity of the profile increases. Summary of the Invention

[0005] Extrusion profiles of Al-Mg-Si (6xxx) alloys are used as structural components in parts exposed to automobile crashes. Such parts are required to absorb large energies during a crash and must therefore deform without fracture. One of the means of controlling that the extrusion profiles have the required properties is to test them by crushing. In this test, a specimen of a thin-walled extruded hollow profile with one or more chambers of predefined length is axially crushed at a controlled rate, reducing the length of the specimen, typically to one-third of its original length. Good deformation behavior is characterized by regular folding of the specimen walls, few or no cracks in the specimen, and a smooth surface of the deformed part. Poor deformation behavior is characterized by limited folding of the specimen walls, extensive cracking or fracture of the specimen, and a rough and uneven surface of the deformed part.

[0006] An alternative to the crush test is to test how far one of the walls in the profile can be bent before the first crack appears on the outside of the bend.

[0007] Some structural components in crash-exposed sections may also be exposed to high temperatures. Such exposure may affect the mechanical properties of the alloy. For such applications, it is important to select an alloy that is less susceptible to thermal exposure. The term "thermal stability" refers to the ability of an alloy to retain its mechanical properties after exposure to high temperatures. The present invention provides an alloy with high temperature stability that can be manufactured using lower cooling rates after extrusion while maintaining corrosion and crush properties.

[0008] The invention is characterized by the features defined in the independent claims 1, 13 and 25 and in the dependent claims 2 to 12, 14 to 24 and 26.

[0009] According to a first aspect, in weight percent: Mg: 0.45 to 1.2 Si: 0.40 to 1.0 Ti: 0.05~0.20 V: 0.05~0.15 Cu: Less than 0.30 Mn: Less than 0.30 Cr: Less than 0.15 Zr: Less than 0.15 Fe: Less than 0.50 Zn: Less than 0.50 The balance is aluminum and unavoidable impurities, the Ti+V content is 0.10 to 0.30 wt%, and Si eff A 6xxx aluminum alloy is provided in which the aluminum / Mg ratio is less than 1.0.

[0010] S eff =Si-(Fe+Mn+Cr) / 3[wt%]. If Zr is included in the alloy, Si eff =Si-(Fe+Mn+Cr+Zr) / 3[weight%].

[0011] In some embodiments, the Ti content is 0.05 to 0.15 wt % or 0.07 to 0.12 wt %.

[0012] In some embodiments, the V content is 0.07 to 0.12 wt %.

[0013] In some embodiments, the content of Ti+V is 0.14 to 0.24 wt % or 0.15 to 0.20 wt %.

[0014] In some embodiments, Si eff The / Mg ratio is 0.50 to 0.96.

[0015] In some embodiments, Si eff The / Mg ratio is 0.60 to 0.85 or 0.65 to 0.75.

[0016] In some embodiments, Si eff The / Mg ratio is 0.80 to 0.96.

[0017] In some embodiments, the Si content is 0.45 to 0.65 wt % and the Mg content is 0.55 to 0.75 wt %.

[0018] In some embodiments, the Si content is 0.45 to 0.55 wt % and the Mg content is 0.55 to 0.65 wt %.

[0019] In some embodiments, the Mn content is 0.10 to 0.20 wt %.

[0020] In some embodiments, the Cu content is less than 0.20 or between 0.08 and 0.15 wt %.

[0021] In some embodiments, the Cr content is less than 0.08 wt.% or less than 0.05 wt.%.

[0022] In some embodiments, the Fe content is less than 0.35 wt.%.

[0023] In some embodiments, the 6xxx aluminum alloy is an extrusion alloy.

[0024] According to a second aspect, there is provided a method for producing an extruded product from an alloy according to the first aspect or any embodiment thereof, comprising the steps of: a. by weight percent Mg: 0.45 to 1.2 Si: 0.40 to 1.0 Ti: 0.05~0.20 V: 0.05~0.15 Cu: Less than 0.30 Mn: Less than 0.30 Cr: Less than 0.15 Zr: Less than 0.15 Fe: Less than 0.50 Zn: Less than 0.50 The balance is aluminum and unavoidable impurities, the Ti+V content is 0.10 to 0.30, and Si effcasting a billet from a 6xxx aluminum alloy, wherein the aluminum / Mg ratio is less than 1.0; b. homogenizing the cast billet at a temperature of 480°C to 600°C for 1 hour to 24 hours; c. cooling the homogenized billet; d. extruding the homogenized billet to form an extruded product; e. cooling the extruded product to room temperature using a cooling rate of less than 80° C. / sec. f. Optionally, stretching the profile; g. ageing the extruded product; A method is provided that includes:

[0025] S eff =Si-(Fe+Mn+Cr) / 3[wt%]. If Zr is included in the alloy, Si eff =Si-(Fe+Mn+Cr+Zr) / 3[weight%].

[0026] In some embodiments, the stretching in step f is 1.5 to 4% or 1.5 to 3%.

[0027] In some embodiments, the cooling rate in step e is less than 40° C. / sec or less than 20° C. / sec.

[0028] In some embodiments, the cooling rate in step e is greater than 5° C. / sec or greater than 7° C. / sec.

[0029] In some embodiments, the content of Ti+V is 0.14 to 0.24 wt % or 0.15 to 0.20 wt %.

[0030] In some embodiments, Si eff The / Mg ratio is 0.50 to 0.96.

[0031] In some embodiments, Si eff The / Mg ratio is 0.60 to 0.85 or 0.65 to 0.75.

[0032] In some embodiments, Si eff The / Mg ratio is 0.80 to 0.96.

[0033] According to a third aspect, there is provided an extruded product comprising an alloy according to the first aspect or any embodiment thereof and produced by the method of the second aspect or any embodiment thereof, wherein the material of the final extruded product has a recrystallized grain structure.

[0034] In some embodiments, the extruded product is a structural component of a vehicle that is exposed during a crash.

[0035] Unless otherwise specified, the AA6xxx series alloys referred to herein refer to AlMgSi alloys listed in "International Alloy Designations and Chemical Composition Limits for Wrought Aluminum and Wrought Aluminum Alloys" published by the Aluminum Association.

[0036] Unless otherwise stated, all alloy compositions are expressed as weight percent based on the total weight of the alloy. [Brief description of the drawings]

[0037] [Figure 1a] FIG. 1a shows the yield strength values ​​Rp0.2 of the seven alloys in Table 1 stretched by 0.5%, 2% and 4% before ageing to T6. [Figure 1b] FIG. 1b shows the local elongation of seven alloys in Table 1 stretched by 0.5%, 2% and 4% before aging to T6. [Diagram 2] FIG. 2 shows how the sample bend test is performed. [Diagram 3] FIG. 3 shows how to manually measure the bend angle at which the sample first cracks. [Figure 4] FIG. 4 shows the bend angle of extrusions made according to the present disclosure from Alloys 1, 3, 5 and 7 in Table 1 and oil quenched after SHT at a cooling rate of 50-60° C. / s. [Diagram 5] FIG. 5 shows the bend angle of extrusions produced as disclosed from Alloys 1, 3, 5 and 7 in Table 1 and air-cooled after SHT at a cooling rate of 6-7° C. / s. [Figure 6(a)] FIG. 6(a) shows the yield strength Rp0.2 of water quenched (WQ), oil quenched (OQ) and air cooled (AC) samples for alloy variants 1, 3, 5 and 7 of Table 1 stretched by 0.5%. [Figure 6(b)] FIG. 6(b) shows the local elongation (A25mm-Ag) of water quenched (WQ), oil quenched (OQ) and air cooled (AC) samples for alloy variants 1, 3, 5 and 7 of Table 1 stretched by 0.5%. [Figure 7(a)] FIG. 7(a) shows the average of the three deepest IGC attacks for the seven alloys in Table 1 tested after stretching of 0.5%, 2% and 4%. [Figure 7(b)] FIG. 7(b) shows an optical microscope image of a typical site measured for the IGC values ​​shown in FIG. 7(a). [Figure 8] FIG. 8 shows the yield strength (Rp0.2) and ultimate tensile strength (Rm) of age hardened extrusion profiles made from Alloy 3 in Table 1 after thermal exposure at 150° C. for 500 hours and 1000 hours. [Figure 9] FIG. 9 shows typical quenching rates along a 10 cm long profile during air quenching (AQ). [Figure 10] FIG. 10 shows the yield strength (a) and ultimate tensile strength (b) of the sample described in Example 5 after aging to T6. [Figure 11] FIG. 11 shows crush specimens from the three alloys of Example 5, with two parallel columns from left to right (vertical rows) showing alloys 21-031, 21-032, and 21-033. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0038] The present invention will now be further described by way of examples with reference to the drawings. The invention according to the present disclosure relates to an aluminum alloy containing Mg and Si as the major alloying elements with the addition of Ti and V. The alloy contains an amount of Ti in excess of the amount of Ti normally added as a grain refiner. The excess Ti contributes to improved ductility and improved corrosion resistance of the alloy. The aluminum alloy is a 6xxx aluminum alloy. The aluminum alloy may in particular be a 6xxx aluminum extrusion alloy.

[0039] The present disclosure provides, in weight percent: Mg: 0.45 to 1.2 Si: 0.40 to 1.0 Ti: 0.05~0.20 V: 0.05~0.15 Cu: Less than 0.30 Mn: Less than 0.30 Cr: Less than 0.15 Zr: Less than 0.15 Fe: Less than 0.50 Zn: Less than 0.50 The balance is aluminum and unavoidable impurities, the Ti+V content is 0.10 to 0.30, and Si eff For 6xxx aluminum alloys, the / Mg ratio is less than 1.0.

[0040] S eff =Si-(Fe+Mn+Cr) / 3[wt%]. If Zr is included in the alloy, Si eff =Si-(Fe+Mn+Cr+Zr) / 3[weight%].

[0041] The alloy may contain Cu for additional strength and temperature stability. The Cu content should be less than 0.30 wt.%. In some embodiments, the Cu content can be less than 0.20 wt.%. A Cu content of 0.08-0.15 wt.% has shown good strength and temperature stability in some embodiments.

[0042] The alloy may contain up to 0.50 wt% Fe. Iron is an impurity element that typically originates from sources such as aluminum oxide, manufacturing processes, and scrap metal. Too high a content of Fe can reduce the corrosion properties of the alloy. It also reduces the strength of the material by binding the Si in the AlFeSi-containing primary particles. However, increasing the maximum Fe content or having a relatively high Fe content allows for more use of post-consumer scrap, which is important for reducing the carbon footprint of aluminum.

[0043] The number density of dispersoids formed per weight percent of the added element is significantly higher for Cr than for Mn (O. Lohne and AL Dons: Scand. J. Metall. vol. 12 (1983) pp. 34-36), which means that to achieve a certain dispersoid number density, a lower Cr addition is needed than an Mn addition. Dispersoids have three negative effects on the extrusion process. The first is that the hot deformation resistance of the material increases, leading to a decrease in productivity. The second is that an increase in the number density of dispersoids increases the requirements for the cooling rate after extrusion to avoid a loss of the hardening potential of the alloy. The reason is that the dispersoids act as nucleation sites for non-hardening Mg-Si precipitates. The third negative effect is related to the grain size of the extrusion profile. With a slightly lower number of dispersoids than is required to prevent recrystallization, a situation is obtained in which only a few grains can grow, resulting in a very coarse grain structure during the extrusion profile. The subsequent formation of the extrusion profile can result in extensive orange peeling. In the final product, coarse grains have a negative effect on the crushing and bending behavior. Therefore, we try to avoid adding Mn and Cr in excess of the amount required to benefit from improved ductility. The optimum Mn and Cr content strongly depends on the processing conditions and the profile shape.

[0044] The final extrusion product produced according to the method disclosed herein is preferably recrystallized and therefore has a recrystallized grain structure. Materials with a large number of dispersoid particles sufficient to prevent recrystallization after extrusion will have a higher deformation resistance and therefore be more difficult to extrude than materials with fewer dispersoid particles. Furthermore, a high number of dispersoid particles may increase the quench sensitivity of the material, forcing it to be quenched to meet the strength requirements of the product. In such cases, dimensional tolerance requirements may be difficult to meet due to distortion of the extrusion profile during quenching.

[0045] Thus, alloys according to the present disclosure may contain up to 0.30 wt% Mn. In some embodiments, the amount of Mn may be 0.10-0.20 wt%. Cr may be added up to 0.15 wt%. In some embodiments, the amount of Cr is less than 0.08 wt% or even less than 0.05 wt%. Alloys according to the present disclosure may contain 0.10-0.20 wt% Mn and up to 0.15 wt% Cr. When combining two elements, Mn and Cr, the amount of each element may have to be reduced to keep the total number of dispersoids at an acceptable level. Too much Mn and / or Cr can result in a mixed grain structure (recrystallized and non-recrystallized) that results in unfavorable mechanical properties.

[0046] Zr additions are less common in the 6xxx alloys, but they do form dispersoid particles similar to the addition of Mn or Cr. Zr may be added up to 0.15 wt.%, but the same considerations as for Mn and Cr additions are required to keep the total number of dispersoids at acceptable levels.

[0047] The alloy may contain up to 0.50 wt.% Zn to allow for more post-consumer scrap to be added to the melt. In one embodiment, the alloy contains up to 0.20 wt.% Zn. Some Zn does not significantly affect the extrudability, mechanical properties, or corrosion properties of the aluminum alloy. At higher Zn concentrations, extrudability and corrosion properties decrease slightly, so the upper limit for Zn is 0.50 wt.%.

[0048] This alloy was developed for extrusion products where good crush behavior is required. It is optimized for productivity and high ductility without the need to rapidly quench the extrusion profile in the extrusion press. The alloy according to the present disclosure is therefore particularly suitable for extrusions with complex profiles. However, it can also be used for other products such as forgings where improved ductility or corrosion resistance is required.

[0049] To find the optimum Si / Mg ratio for the alloy, one must take into account that some of the Si is tied up in the Fe-containing primary particles and other non-hardening particles formed during casting and homogenization of the alloy, and this Si can be considered as "lost" or ineffective with respect to age hardening. S eff =Si-(Fe+Mn+Cr) / 3[wt%], for alloys containing Zr, Si eff "Available Si content" defined as Si-(Fe+Mn+Cr+Zr) / 3 [weight%] eff The term can be introduced.

[0050] The alloy according to the present disclosure has Mg in an amount of 0.45-0.2 wt.% and Si in an amount of 0.40-1.0 wt.%. To optimize the crush resistance of extruded products made from the alloy according to the present disclosure, Si eff The Si / Mg ratio should be less than 1.0. eff The Si / Mg ratio is preferably maintained within the range of 0.50 to 0.96. The optimum Si / Mg ratio is within the range of 0.60 to 0.85 or 0.65 to 0.75. eff The Si / Mg ratio has been found to be advantageous, as demonstrated by the examples. However, in some embodiments, eff The / Mg ratio may be 0.80 to 0.96.

[0051] According to some embodiments, the optimum composition of Mg and Si for ductility and temperature stability is 0.45-0.65 wt.% Si and 0.55-0.75 wt.% Mg, or more narrowly defined compositions of 0.45-0.55 wt.% Si and 0.55-0.65 wt.% Mg.

[0052] Titanium (Ti) is usually added to Al alloys together with boron (B) or carbon (C) for the purpose of refining the grain size of the alloy during casting. The extra Ti in the melt enhances the grain refining effect of TiB2 particles. The Ti content required for grain refinement of Al-Mg-Si alloys is typically in the range of 0.005-0.03 wt%. The amount of Ti in the alloy according to the present disclosure is in the range of 0.05-0.20 wt%, for example, in the range of 0.05-0.15 wt% or 0.07-0.12 wt%. Furthermore, the amount of V in the alloy according to the present disclosure is in the range of 0.05-0.15 wt% or 0.07-0.12 wt%. Both Ti and V are peritectic elements that usually segregate towards the center of the grain during solidification. During extrusion, the Ti- and V-rich regions in the grain are elongated into fine bands. Without wishing to be bound by theory, it is believed that these Ti- / V-bands reduce the diffusion rate of Mg and Si towards the grain boundaries at high temperatures, thus allowing for a reduced cooling rate after extrusion without compromising material properties such as bend angle, strength and crushability. Addition of both Ti and V in a total of 0.10 wt% or more, e.g., a total of 0.14 wt% or more, improves the crush resistance and corrosion resistance of Al-Mg-Si alloys according to the present disclosure. This requires a Ti content above that typically used for grain refinement. Thus, according to the present disclosure, the total amount of Ti and V (Ti+V) should be 0.10-0.30 wt%. In some embodiments, the Ti+V content may be 0.14-0.24 wt%, e.g., 0.15-0.20 wt%. The total amount of Ti+V should not be too high, as this would result in undesirable precipitation of primary particles. Since Ti and V in solid solution increase the deformation resistance and decrease the extrudability, the total amount of Ti and V should also be kept within the indicated limits. The improvement in crushing performance obtained by the addition of Ti and V to Al-Mg-Si alloys is demonstrated by the examples of the present invention.

[0053] The present disclosure further relates to a method for producing an extruded product. The method includes the following steps. Step a. weight percent Mg: 0.45 to 1.2 Si: 0.40 to 1.0 Ti: 0.05~0.20 V: 0.05~0.15 Cu: Less than 0.30 Mn: Less than 0.30 Cr: Less than 0.15 Zr: Less than 0.15 Fe: Less than 0.50 Zn: Less than 0.50 The balance is aluminum and unavoidable impurities, the Ti+V content is 0.10 to 0.30, and Si eff A billet is cast from a 6xxx aluminum alloy, the alloy having a Fe / Mg ratio of less than 1.0, which may have a composition according to the above disclosure, or any of the above disclosed embodiments of the alloy further specifying alternative amounts of alloying elements. S eff =Si-(Fe+Mn+Cr) / 3[wt%]. In the case of alloys containing Zr, Si eff =Si-(Fe+Mn+Cr+Zr) / 3[weight%].

[0054] Step b. Homogenize the cast billet at a temperature of 480-600°C for 1-24 hours. The homogenization step homogenizes the microstructure of the cast billet. Typical homogenization temperatures are above the solvus temperature of the alloys involved in order to dissolve the Mg and Si contained in the alloy.

[0055] Step c. Cooling the homogenized billet from the homogenization temperature to room temperature. The cooling rate from the homogenization temperature may be greater than 100° C. per hour. Typically, the cooling rate from the homogenization temperature can be greater than 200° C. per hour or greater than 300° C. per hour.

[0056] Step d. extruding the billet to form an extruded product. Prior to extrusion, the extruded billet should be reheated to an appropriate extrusion temperature, typically 450-510°C. According to the present disclosure, the billet may be superheated before being cooled to the desired extrusion temperature.

[0057] Step e. Cool the extruded product to room temperature. The cooling of the extruded product should use a cooling rate of less than 80°C / s. The cooling rate may be less than 40°C / s or even less than 20°C / s. However, the cooling rate should be greater than 5°C / s, and in some embodiments, greater than 7°C / s. If the cooling rate is too low, the potential strength of the final product may be reduced because the Mg and Si contained in the alloy may precipitate as large Mg2Si that do not contribute to strengthening during aging. This results in less Mg and Si being available for precipitation of strengthening nano-sized precipitate phases formed during artificial aging. The use of low cooling rates for extrusion allows the production of complex extruded sharps with the desired strength and crush properties without introducing geometric distortions to the profile. The advantages of using lower cooling rates for cooling the extruded product are demonstrated by the examples.

[0058] Step f. Optionally, stretch the profile. Optional stretching step f may include stretching the cooled profile up to 4%. Stretching between 1.5-4%, for example 1.5-3%, has been shown to be beneficial to the ductility of the material, as demonstrated by the examples. Stretching is typically performed shortly after extrusion, for example within 10-30 minutes after extrusion, although the times shown are not critical and stretching may occur later.

[0059] Step g. Aging the extruded product. The aging step g involves artificially aging the product to a desired strength level. It should be understood that the aging step can also include natural aging, since natural aging is practically unavoidable in industrial production. To achieve the desired crush performance, the extruded product may be aged to a T6 temper. Profiles stretched according to step f may be designated as T8 temper (aged after cold working), although in this disclosure the T6 designation is used for all aged profiles. Aging temperatures are typically within the range of 160-210°C for 1-24 hours, with typical aging temperatures being within the range of 175-205°C. Artificial aging may be performed in one step or in stages.

[0060] The extruded product produced according to the method disclosed above has the following composition (by weight): Mg: 0.45 to 1.2 Si: 0.40 to 1.0 Ti: 0.05~0.15 V: 0.05~0.15 Cu: Less than 0.30 Mn: Less than 0.30 Cr: Less than 0.15 Zr: Less than 0.15 Fe: Less than 0.50 Zn: Less than 0.50 The balance is aluminum and unavoidable impurities. The Ti+V content is 0.10 to 0.30. Si eff / Mg ratio is less than 1.0, The alloys include those having the formula:

[0061] The alloy composition of the extruded product may have any composition as described in the above disclosure.

[0062] S eff =Si-(Fe+Mn+Cr) / 3[wt%]. In the case of alloys containing Zr, Si eff =Si-(Fe+Mn+Cr+Zr) / 3[weight%].

[0063] The extrusion products produced by the methods of the present disclosure should have a recrystallized grain structure. In some embodiments, the extrusion products have a recrystallized grain structure and a yield strength Rp0.2 of at least 240 MPa (C24 alloy requirement). Furthermore, the extrusion products of the alloys of the present disclosure produced by the methods of the present disclosure exhibit excellent bend angle properties and have a combination of excellent crushability and corrosion resistance. As is evident from the examples below, the extrusion products also have good temperature stability. EXAMPLES

[0064] <Example 1> Seven alloys having the compositions shown in Table 1 were cast into billets with a diameter of 95 mm by DC casting.

[0065] [Table 1]

[0066] Homogenization was carried out at a temperature of 575° C. for 2 hours and 15 minutes, followed by cooling at a rate of about 350° C. / hour.

[0067] The billet was heated to about 550°C for 8-10 minutes and then cooled to about 490-500°C just before extrusion. Hollow rectangular profiles with external dimensions of 29 x 37 mm and wall thickness of 2.8 mm were extruded from different alloys. The profiles were quenched in water at a distance of about 50 cm behind the die exit with a quenching rate estimated to be more than 300°C / s. After extrusion, the profiles were stretched either 0.5%, 2% or 4%. About 24 hours after extrusion, the profiles were heated to 150°C at a rate of 200°C / h, held at 150°C for 1.5 hours, heated to 195°C at a rate of 15°C / h and aged to T6 at 195°C for 2 hours for the 0.5% stretched profile, 195°C for 1 hour 40 minutes for the 2% stretched profile and 195°C for 1 hour 20 minutes for the 4% stretched profile. Figure 1(a) shows the yield strength values ​​Rp0.2 of the seven alloys in Table 1 stretched by 0.5%, 2% and 4% before ageing to T6. The strength levels of the different variants are very similar. This is expected since both vanadium and titanium have little effect on the strength in the T6 condition. There is a slight decrease in strength for the profiles stretched by 2% and 4% compared to the profiles stretched by 0.5% before ageing to T6. Tensile tests were performed according to ISO 6892-1-Metallic materials-Tensile tests-Part 1: Method of tests at room temperature.

[0068] Uniform or total elongation is not a good measure of the ductility of a material subjected to deformation by crushing. 25mm ) and uniform elongation (A g) is known as the local elongation and is a better measure of the ductility of a material. Figure 1(b) shows the local elongation for the seven alloys tested. In the water quench profile, the addition of either vanadium or titanium has a small positive effect. Increasing the elongation from 0.5% to 2% or 4% before T6 ageing appears to have a positive effect on the local elongation.

[0069] <Example 2> The bending test was carried out according to standard VDA 238-100, with the exception that a load drop of 1% was used as the stopping criterion instead of 60 N. The bending angle measured based on this criterion typically corresponds to the angle at which the first crack is observed in the sample. The test sample was taken from the widest side wall of the profile of Example 1. The sample was 30 mm wide, 60 mm long and 2.8 mm thick. The sample is bent along an axis at 90° to the extrusion direction (i.e. perpendicular to the extrusion direction) (see Figure 2). Figure 3 shows how to manually measure the bending angle at which the first crack occurs in the sample.

[0070] To investigate the effect of different cooling rates from extrusion on the flexural properties, extruded samples stretched by 0.5% after extrusion were subjected to separate solution heat treatment (SHT) at 530 °C for 20 min (time measured after the temperature reached 525 °C) and then quenched in air, oil or water.

[0071] One set of specimens (set 1) was quenched in water maintaining a temperature of about 25° C. The cooling rate in the temperature interval between 450° C. and 250° C. is estimated to be greater than 300° C. / sec. After quenching, the specimens were stretched by 0.5% and 2% and then aged to T6 in the same manner as in Example 1.

[0072] Another set of samples (set 2) were quenched in oil maintaining a temperature in the range of 26-28° C. The cooling rate in the temperature interval between 450° C. and 250° C. is measured to be in the range of 50-60° C. / s. After quenching, the samples were stretched by 0.5% and 2% and then aged to T6 in the same manner as described in Example 1.

[0073] The third set of specimens was cooled in forced air. In order to obtain a higher cooling rate than that obtained for all hollow profile specimens, blanks for bending specimens were prepared before SHT, with a width of 30 mm, a length of 150 mm and a thickness of 2.8 mm. The cooling rates in the temperature interval between 450°C and 250°C were measured to be in the range of 6-7°C / s. After cooling to room temperature, the specimens were stretched by 0.5% and 2% and then aged to T6 in the same manner as described in Example 1.

[0074] The bend angles of the water-quenched samples all exceeded the limits of the equipment, so the results presented here are not representative.

[0075] Figure 4 shows the bend angle measured as described in Example 2 for extrusions made according to the invention from alloys 1, 3, 5 and 7 and oil quenched after SHT with a cooling rate of 50-60 °C / s. In this case a clear effect of adding Ti or V is seen, but according to the invention the best effect is obtained by adding Ti and V together. There is also a very clear effect of stretching by 2% compared to 0.5% before ageing to T6.

[0076] Figure 5 shows the bend angle of extrusions made according to the invention from alloys 1, 3, 5 and 7 in Table 1 and air cooled after SHT at a cooling rate of 6-7°C / s. Air cooling reduces the bend angle for all alloys, but again there is a clear effect of adding Ti or V, but according to the invention the best effect is obtained by adding Ti and V together. Also a very clear effect of 2% elongation compared to 0.5% before ageing to T6.

[0077] Although the bendability of the water-quenched and oil-quenched samples is better than that obtained with the air-cooled samples, the very high cooling rates impose limitations on the profile shapes and geometric tolerances that can be provided. Using the compositions according to the invention, it is possible to obtain bend angles with samples that are air-cooled after extrusion that approach those of the more rapidly quenched samples of the prior art.

[0078] In Fig. 6(a), the yield stress Rp of alloy variants cooled at different cooling rates after SHT is 0.2 The values ​​of Rp are shown in Fig. 1. Rp values ​​are shown in Fig. 1 for the air-cooled samples compared to the water-cooled samples. 0.2 The minimum Rp of all variants was 240MPa. 0.2 This meets the typical requirements.

[0079] In Fig. 6(b), the total elongation A 25mm and uniform elongation A g The difference between (referred to as local elongation) and (referred to as local elongation) is plotted for the same alloy variants as in Figure 6(a). Local elongation is best for the highest cooling rate. The addition of Ti or V (variants 3 and 5) increases local elongation compared to the low Ti and V alloy variant (variant 1). However, the greatest increase in local elongation is found according to the invention when both elements are added together (variant 7).

[0080] <Example 3> Intergranular corrosion (IGC) tests were performed according to standard ISO 11846 method B. Three parallel specimens from each sample were immersed in the same beaker. The IGC results of the seven alloys are shown in Figure 7. Four areas were examined for each sample and the three deepest IGC erosions were measured.

[0081] Figure 7(a) shows the average of the three deepest IGC attacks for the seven alloys tested after stretching by 0.5%, 2% and 4%. The alloys were water quenched after extrusion and stretched before ageing to T6. The alloy containing neither Ti nor V (Alloy 1) experienced the deepest corrosion attack, with the maximum average depth measured ranging from 350 to 410 μm.

[0082] FIG. 7(b) shows a light microscope image of a typical site measured for the mean IGC values ​​shown in FIG. 7(a).

[0083] From the images in Figures 7(a) and 7(b), it is clear that increasing Ti and V in these alloys significantly reduces the IGC depth. Alloy 7, which has high Ti and V, clearly showed the least IGC attack, followed by alloys 6 and 3. Stretching by 2% and 4% before aging appears to reduce the maximum IGC depth compared to 0.5% stretching.

[0084] <Example 4> Figure 8 shows the decrease in yield strength (YS) and ultimate tensile strength (UTS) after thermal exposure at 150°C for 500 and 1000 hours for age hardened extrusion profiles made from alloy 3 of Table 1. The results indicate that the Mg and Si contents selected according to the present invention result in high thermal stability. Since the thermal stability does not seem to depend on the Ti and V contents, the obtained results should be valid for all alloys in this study.

[0085] <Example 5> Three alloys with different Mg / Si ratios were cast. The nominal chemical compositions of the three alloys are shown in Table 2. The blanks were GC cast with a diameter of 95 mm.

[0086] [Table 2]

[0087] Homogenization was carried out at a temperature of 575° C. for 2 hours and cooled to room temperature at a rate of about 350° C. / hour.

[0088] One chamber crash box profiles of dimensions 28mm x 37mm x 2.8mm with a seam weld in the centre of the profile wall were extruded. The billet was heated to 560°C and held at the same temperature in an air circulating furnace, then the billet was water quenched to 500°C before extrusion. The extrusion tool / container was held at 430°C. The profile was water quenched at a distance of about 50cm behind the die exit.

[0089] Before each cooling test, a separate solution heat treatment (SHT) was performed. Each sample was solution heat treated (SHT) at 530°C for 20 minutes (starting when the temperature reached 525°C). Then, different quenching rates were applied: water quenching (WQ), oil quenching (OQ) and air quenching (AQ). The following sections describe the three different quenching lines. All profiles were stretched by 0.5% or 2% immediately after quenching, naturally aged for about 24 hours and then artificially aged to T6. The aging to T6 used the temperature profile shown in Table 3. Results shown here are after the final AA step to T6 unless otherwise stated.

[0090] [Table 3]

[0091] Water quenching after SHT Profile specimens of 35 cm length were subjected to SHT as described above. The profiles were immediately quenched in water held at approximately 25°C. The water was not agitated. The average quenching rate was greater than 300°C / sec. The profiles were stretched immediately after quenching and then naturally aged (NA) from AA to T6 for approximately 24 hours at room temperature.

[0092] Oil quenching after SHT Profiles of 35 cm length were subjected to SHT as described above. The profiles were quenched in oil held at 26-28°C. The oil was stirred during quenching. The average quenching rate was about 55°C / sec. The profiles were stretched immediately after quenching. The profiles were then naturally aged (NA) at room temperature for about 24 hours from AA to T6.

[0093] Air cooling after SHT The samples were subjected to SHT at 530°C for 20 minutes (the time after the temperature reached 525°C). The profiles were then air-cooled by keeping them on the fan for 1 minute before quenching in water. The average quenching rate was about 7°C / sec. The profiles were stretched immediately after quenching and then kept at room temperature for about 24 hours from AA to T6. The experimental setup and sample geometry used during AQ are shown in Figure 9 along with the corresponding temperature traces, where T1 is the lower curve and T2 is the upper curve in the figure.

[0094] The mechanical properties of the profiles were tested. For tensile testing, standard flat 12 cm long tensile specimens were machined from the narrowest profile wall of each alloy variant. Two parallel pieces were tested for each condition. Tensile tests were performed according to ISO 6892-1-Metallic materials-Tensile tests-Part 1: Method of tests at room temperature.

[0095] The results of the tensile test are shown in Figure 10a) and b). The quenching rates are as mentioned above. The yield strength and ultimate tensile strength in Figure 10a) and b) are both Si. eff It increases slightly with increasing / Mg ratio. From Fig. 10b), Rm increases with increasing stretch from 0.5% to 2% for all quenching rates. Regarding the yield strength in Fig. 10a), the effect of stretching after SHT seems less pronounced. However, for the slowest quenching rate (AQ), Rp0.2 increases by 4–8 MPa with stretching from 0.5% to 2%.

[0096] For the crush test, two parallel specimens were cut for crush testing of each alloy after WQ and 0.5% elongation. All the crush boxes were crushed to 1 / 3 of their original height. The crush specimens are shown in Figure 11. The lowest Si eff The 21-031 alloy having a Cr / Mg ratio performed best, with reference to FIG. 11(a), obtaining a perfect crush score of 10, which means that the specimen did not show any signs of cracking. Referring to FIG. 11(b), the higher Si effThe 21-032 alloy, which has the highest Si / Mg ratio, also performed well, but had a slightly lower crush rating. eff The 21-033 alloy with a Cr / Mg ratio performed the worst, exhibiting at least one deep corner crack.

Claims

1. In weight percent, Mg: 0.45-1.2 Si:0.40~1.0 Ti: 0.05-0.20 V:0.05~0.15 Cu: less than 0.30 Mn: less than 0.30 Cr: less than 0.15 Zr: less than 0.15 Fe: less than 0.50 Zn: less than 0.50 The balance is aluminum and unavoidable impurities, the Ti+V content is 0.10 to 0.30, and Si eff A 6xxx aluminum alloy having a Zr / Mg ratio of less than 1.

0.

2. The 6xxx aluminum alloy of claim 1, wherein the Ti content is 0.07 to 0.12 wt.%.

3. The 6xxx aluminum alloy according to claim 1 or 2, wherein the V content is 0.07 to 0.12 wt.%.

4. 4. The 6xxx alloy of any one of claims 1 to 3, wherein the Ti+V content is 0.14 to 0.24 wt.% or 0.15 to 0.20 wt.%.

5. S eff The 6xxx aluminum alloy of any one of claims 1 to 4, wherein the Si / Mg ratio is 0.50 to 0.

96.

6. S eff 6xxx aluminum alloy as claimed in claim 5, wherein the Si / Mg ratio is 0.60 to 0.85 or 0.65 to 0.

75.

7. S eff The 6xxx aluminum alloy of claim 5, wherein the Si / Mg ratio is 0.80 to 0.

96.

8. The 6xxx aluminum alloy according to any one of the preceding claims, wherein the Si content is 0.45 to 0.65 wt.% and the Mg content is 0.55 to 0.75 wt.%.

9. The 6xxx aluminum alloy of claim 8, wherein the Si content is 0.45 to 0.55 wt.% and the Mg content is 0.55 to 0.65 wt.%.

10. 6xxx aluminum alloy according to any one of claims 1 to 9, wherein the Mn content is 0.10 to 0.20 wt.%.

11. The 6xxx aluminum alloy of any one of the preceding claims, wherein the Cu content is less than 0.20 or 0.08 to 0.15 wt.%.

12. The 6xxx aluminum alloy according to any one of the preceding claims, having a Cr content of less than 0.08 wt.% or less than 0.05 wt.%.

13. A method for producing an extrusion product from an alloy according to any one of claims 1 to 12, comprising the steps of: a. in weight percent Mg: 0.45-1.2 Si:0.40~1.0 Ti:0.05~0.15 V:0.05~0.15 Cu: less than 0.30 Mn: less than 0.30 Cr: less than 0.15 Zr: less than 0.15 Fe: less than 0.50 Zn: less than 0.50 The balance is aluminum and unavoidable impurities, the content of Ti+V is 0.10 to 0.30, and Si eff casting a billet from a 6xxx aluminum alloy, wherein the Al / Mg ratio is less than 1.0; b. homogenizing the cast billet at a temperature of 480°C to 600°C for 1 hour to 24 hours; c. cooling the homogenized billet; d. extruding the billet to form an extruded product; e. cooling the extruded product to room temperature using a cooling rate of less than 80° C. / sec; f. Optionally, stretching the profile; g. Aging the extruded product. A method for producing an extruded product comprising:

14. The method for producing an extruded product according to claim 13, wherein the stretching in step f is 1.5 to 4%.

15. The method for producing an extruded product according to claim 14, wherein the stretching in step f is 1.5 to 3%.

16. Method for producing an extruded product according to any one of claims 13 to 15, wherein the cooling rate in step e) is less than 40°C / s or less than 20°C / s.

17. Method for producing an extruded product according to any one of claims 13 to 16, wherein the cooling rate in step e) is greater than 5°C / s or greater than 7°C / s.

18. A method for producing an extruded product according to any one of claims 13 to 17, wherein the Ti+V content is between 0.14 and 0.24 or between 0.15 and 0.

20.

19. S eff A method for producing an extruded product according to any one of claims 13 to 18, wherein the / Mg ratio is between 0.50 and 0.

96.

20. S eff 20. A method for producing an extruded product according to claim 19, wherein the Mo / Mg ratio is from 0.60 to 0.85, or from 0.65 to 0.75, or from 0.80 to 0.

96.

21. The method for producing an extrusion product according to any one of claims 13 to 20, wherein the Si content is 0.45 to 0.65 wt.% and the Mg content is 0.55 to 0.75 wt.%.

22. The method for producing an extrusion product according to claim 21, wherein the Si content is 0.45-0.55 wt.% and the Mg content is 0.55-0.65 wt.%.

23. The method for producing an extruded product according to any one of claims 13 to 22, wherein the Cu content is less than 0.20 or between 0.08 and 0.15 wt.%.

24. The method for producing an extruded product according to any one of claims 13 to 23, wherein the Cr content is less than 0.08 wt.% or less than 0.05 wt.%.

25. An extruded product produced according to any one of claims 13 to 24, comprising, in weight percent: Mg: 0.45-1.2 Si:0.40~1.0 Ti:0.05~0.15 V:0.05~0.15 Cu: less than 0.30 Mn: less than 0.30 Cr: less than 0.15 Zr: less than 0.15 Fe: less than 0.50 Zn: less than 0.50 The balance is aluminum and unavoidable impurities, the Ti+V content is 0.10 to 0.30, and Si eff 6xxx aluminum alloys, in which the Al / Mg ratio is less than 1.0; The final material has a recrystallized grain structure.

26. 26. The extrusion product of claim 25, wherein the extrusion product is a structural component of a vehicle that is exposed during a crash.

Citation Information

Patent Citations

  • Energy absorption aluminum profile for railway vehicle body and manufacturing method thereof

    CN104988366A

  • Aluminum alloy material for automobile energy absorption box

    CN108193093A

  • High strength aluminum alloy excellent in intergranular corrosion resistance, and its production

    JP1998219381A

  • Aluminum alloy with improved crush properties

    JP2009526913A

  • Component of an automobile body structure having an excellent compromise between mechanical strength and crash behavior

    JP2018534434A