Soft-feeling hot melt adhesive composition in laminates, method for using same, and articles made therewith - Patents.com

The hot melt adhesive composition, utilizing specific polypropylene-based polymers and styrene block copolymers, addresses thermal degradation and hardness issues, providing strong, stable, and soft-touch laminates for bonding heat-sensitive substrates.

JP2024543282AInactive Publication Date: 2024-11-21BOSTIK SA(FR)

Patent Information

Application Number
JP2023551703
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2021-02-24
Filing Date
2022-02-24
Publication Date
2024-11-21
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Existing hot melt adhesives suffer from thermal degradation, crosslinking issues, and lack of soft feel in laminates, particularly when bonding delicate and heat-sensitive substrates, leading to equipment damage and performance deterioration.

Method used

A hot melt adhesive composition using semi-crystalline, low molecular weight, single-site catalyzed polypropylene-based polymers and essentially amorphous, high molecular weight, single-site catalyzed polypropylene-based polymers, combined with waxes and hydrogenated styrene block copolymers, to provide high bond strength, cohesive strength, thermal stability, and a soft touch.

Benefits of technology

The adhesive composition offers high bond strength, cohesive strength, thermal stability, wide application temperature range, and a soft feel, while maintaining compatibility with various coating methods, reducing thermal degradation, and enhancing performance in laminates.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024543282000001
    Figure 2024543282000001
  • Figure 2024543282000002
    Figure 2024543282000002
  • Figure 2024543282000003
    Figure 2024543282000003
Patent Text Reader

Abstract

The hot melt adhesive composition comprises a combination of polymers including a low molecular weight, semi-crystalline propylene-based polymer and a high molecular weight, essentially amorphous propylene-based polymer, both of which are prepared by using a single-site catalyst, along with wax, a hydrogenated styrene block copolymer, a tackifier, and a plasticizer. The composition has a suitable viscosity in the range of 500 cP to 40,000 cP at 177°C and is useful in a variety of industrial applications that find bonding between low surface energy substrates and elastic substrates, including disposable nonwoven hygienic articles. The cooled adhesive in the laminate does not feel hard, but instead feels soft, even though the adhesive demonstrates a relatively high Shore A hardness.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a novel hot melt adhesive composition based on a polymer blend containing a polypropylene polymer, prepared using a single-site catalyst, that is soft to the touch in laminates. The adhesive composition is particularly useful for bonding elastic and low surface energy substrates that are often found in the manufacture of various disposable nonwoven hygiene products, such as baby diapers, adult incontinence articles, and feminine hygiene pads. [Background technology]

[0002] Hot melt adhesives typically exist as solid materials at ambient temperatures, but can be converted to a flowable liquid upon the application of heat. These adhesives are particularly useful in the manufacture of various disposable goods where it is often necessary to bond various substrates together. Specific applications include disposable diapers, hospital pads, feminine sanitary napkins, panty shields, surgical drapes, and adult incontinence briefs (collectively referred to as disposable nonwoven sanitary products). Other miscellaneous applications include paper products, packaging materials, automobile headliners, home appliances, tapes, and labels. In most of these applications, the hot melt adhesive is heated to its molten state and then applied to a substrate (often named the primary substrate). A second substrate (often named the secondary substrate) is then immediately brought into contact with and pressed against the first substrate. The adhesive solidifies upon cooling, forming a strong bond. A major advantage of hot melt adhesives is the absence of a liquid carrier, as is the case with water-based or solvent-based adhesives, thereby eliminating the costly process associated with removing the solvent.

[0003] In many applications, hot melt adhesives are often extruded directly onto a substrate in the form of a thin film or beads by using piston or gear pump equipment. In this case, the substrate is placed in intimate contact with a heated die under pressure. The temperature of the die must be maintained well above the melting point of the adhesive to allow the molten hot melt material to flow smoothly out of the discharge nozzle. Most applications, especially those encountered in the manufacture of food packaging and disposable nonwoven hygienic articles, often involve bonding delicate and heat-sensitive substrates, such as plastic films of thin dimensions. This defines the upper coating temperature limit for hot melt adhesive applications. Today's commercially available hot melts are typically formulated to have a coating temperature below 200°C, preferably below 150°C, to avoid burning or deformation of the substrate. In addition to direct coating, several indirect or non-contact coating methods have also been developed, whereby hot melt adhesives can also be spray-coated onto substrates from a distance using compressed air. These non-contact coating techniques include conventional spiral spray, Omega™, Surewrap™, and various forms of melt-blowing. Indirect methods, however, often require that the viscosity of the adhesive must be low enough at the application temperature to obtain an acceptable coating pattern, typically in the range of 2,000-30,000 cP, preferably in the range of 2,000-15,000 cP. Many other physical factors, especially the rheological properties of the adhesive, play a role in determining the sprayability of a hot melt. The majority of commercially available hot melt products are not suited for spray application. There are no accepted theoretical models or guidelines for predicting sprayability, which must be determined experimentally using application equipment.

[0004] Hot melt adhesives are typically organic materials consisting of a package of polymers, plasticizers, tackifying resins, and antioxidants. Other ingredients, such as waxes, fillers, colorants, and UV absorbers, can also be used to modify the adhesion or impart special properties. These organic ingredients are susceptible to thermal decomposition under the coating conditions of the adhesive. For example, a widely used commercial hot melt adhesive based on styrene-isoprene-styrene (SIS) triblock copolymer can experience a viscosity drop of about 50 percent from its original value after 24 hours at 175°C. Styrene-butadiene-styrene (SBS) based hot melts can experience crosslinking problems under similar conditions. Crosslinking can result in a dramatic increase in viscosity and ultimately render the adhesive unable to flow due to the formation of a three-dimensional polymer network. The change in viscosity is often accompanied by charring, gelation, and the formation of a skin on top of the molten material. Decomposition will inevitably result in the deterioration of the adhesive's properties and performance. In addition, they can also result in equipment damage. The rate of decomposition is temperature dependent, with higher temperatures resulting in faster decomposition. Therefore, decomposition can be slowed down by lowering the adhesive coating temperature.

[0005] US Patent No. 10,011,744 describes a hot melt adhesive composition comprising a low molecular weight semi-crystalline propylene-based polymer and a high molecular weight essentially amorphous propylene-based polymer, a tackifier, and a plasticizer. The adhesive according to this patent has been found to provide a unique combination of properties that previous hot melt adhesives have not been successful in providing, including providing high bond strength to a variety of low surface energy substrates, high cohesive strength to hold elastic materials under constant tension, excellent thermal stability, good wetting properties, a wide application temperature range, long open time, good green bond strength, and compatibility with essentially all known hot melt coating methods. However, the particular adhesive formulation disclosed in this patent has a hard feel after cooling in the laminate. Summary of the Invention

[0006] It would therefore be advantageous to provide a hot melt adhesive that would overcome the shortcomings of the prior art adhesives discussed above. In the present invention, it is found that polyolefin polymer blends including semi-crystalline, low molecular weight, single-site catalyzed polypropylene-based (LMW SSC-PP) polymers and essentially amorphous, high molecular weight, single-site catalyzed polypropylene-based (HMW SSC-PP) polymers, along with wax and hydrogenated styrene block copolymers, provide adhesives that are soft to the touch when cooled and in laminated form. The adhesives further provide the unique combination of properties provided by the '744 patent, including providing high bond strength to a variety of low surface energy substrates, high cohesive strength to hold elastic materials under constant tension, excellent thermal stability, good wetting properties, a wide application temperature range, long open time, good green bond strength, and compatibility with essentially all known hot melt coating methods.

[0007] According to an embodiment of the present invention, a hot melt adhesive composition includes a first polymer comprising a single-site catalyzed polypropylene copolymer having a weight average molecular weight of about 10,000 g / mole to about 90,000 g / mole and a melting enthalpy of about 30 J / g to about 100 J / g, a second polymer comprising a single-site catalyzed polypropylene copolymer having a weight average molecular weight greater than 100,000 g / mole and a melting enthalpy of about 0 J / g to about 30 J / g, a wax, a hydrogenated styrene block copolymer, a tackifier, and a plasticizer.

[0008] According to another embodiment of the invention, a method of making a laminate includes applying a hot melt adhesive composition of any of the embodiments of the invention in a molten state to a primary substrate, and laminating a secondary substrate to a first substrate by contacting the secondary substrate with the adhesive composition, where at least one of the first substrate or the second substrate is elastic. Upon cooling, the adhesive bonds the first substrate and the second substrate together. An embodiment of the invention also includes a laminate made by a method according to an embodiment of the invention. Such a laminate may include elastic leg cuffs, standing leg cuffs, elastic side panels, or stretchable ears for use in disposable articles. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0009] As used herein, SSC refers to a single-site catalyst for the polymerization of α-olefins.

[0010] As used herein, Mw refers to the weight average molecular weight of a polymer. Unless otherwise specified, weight average molecular weights herein are characterized using size exclusion chromatography (SEC) at elevated temperatures using polystyrene standards.

[0011] For purposes of this invention, the term essentially amorphous is used to refer to the state in which a polypropylene-based polymer exhibits an enthalpy of fusion of from 0 J / g to about 30 J / g.

[0012] For purposes of this invention, the term semi-crystalline is used to refer to the state in which a polypropylene-based polymer exhibits an enthalpy of fusion greater than 30 J / g.

[0013] As used herein, HMW SSC-PP refers to a class of high molecular weight, essentially amorphous, propylene homopolymers or copolymers produced by using single-site catalysts and having a Mw of greater than about 100,000 g / mol. The polymers may be completely amorphous, exhibiting no melting peaks on the DSC curve, but they may also have a small percentage of crystallinity that produces one or more small but discernible melting peaks on the DSC curve with enthalpies of fusion of 30 Joules per gram of material (J / g) or less, i.e., 0 J / g to about 30 J / g.

[0014] As used herein, a DSC curve refers to a plot of heat flow or heat capacity versus temperature obtained by using a Differential Scanning Calorimetry (DSC) instrument. The test method used to determine the enthalpy of fusion is ASTM E793-01 "Standard Test Method for Enthalpies of Fusion and Crystallization by Differential Scanning Calorimetry", as described in more detail in the Examples below.

[0015] As used herein, LMW SSC-PP refers to a class of low molecular weight, semi-crystalline propylene homopolymers or copolymers having a weight average molecular weight (Mw) of about 100,000 g / mole or less and a distinct melting peak or peaks on the DSC curve with a melting enthalpy of 30 Joules per gram of material (J / g) or more, i.e., typically about 30 J / g to about 100 J / g, more preferably about 30 J / g to about 90 J / g, and most preferably about 35 J / g to about 80 J / g. "Enthalpy of melting", "enthalpy of fusion", "heat of fusion", and "heat of melting" are used interchangeably.

[0016] According to the present invention, a hot melt adhesive composition is produced that includes as a base polymer component a first polymer comprising a single-site catalyzed polypropylene copolymer having a weight average molecular weight of about 10,000 g / mol to about 90,000 g / mol and a melting enthalpy of about 30 J / g to about 100 J / g, and a second polymer comprising a single-site catalyzed polypropylene copolymer having a weight average molecular weight of more than 100,000 g / mol and a melting enthalpy of about 0 J / g to about 30 J / g. Thus, the first polymer is an LMW SSC-PP and the second polymer is an HMW SSC-PP. Both polymers are prepared by using a single-site catalyst system that can be distinguished from conventional Ziegler-Natta catalyst systems in several ways. Ziegler-Natta catalyst systems typically consist of a catalyst and cocatalyst pair, the most common such pairs being TiCl3 and Al(C2H5)2Cl, or TiCl4 and Al(C2H5)3. Conventional ZN catalyst systems are typically supported on inert supports and have several active catalytic sites on the support particles, each of which has a different activity. In the homopolymerization of α-olefins, more active sites incorporate more monomer molecules into the polymer backbone, thereby producing polymer molecules with relatively longer chain lengths, i.e., higher molecular weights. Conversely, fewer active sites result in polymer molecules with shorter chain lengths. Polymers produced by ZN catalysts have very broad molecular weight distributions with polydispersity index (PDI) up to 10, while polymers prepared by SSC catalysts typically have narrow molecular weight distributions with PDIs of about 1 (i.e., 1.1) to about 4. PDI is defined as the ratio of weight average molecular weight (Mw) / number average molecular weight (Mn). With ZN catalysts, the polymerization reaction is highly stereospecific. α-olefin molecules add to the polymer chain only in certain orientations, depending on the chemical and crystalline structure of the catalyst, resulting in a regular, three-dimensional repeating configuration of the polymer chain.

[0017] Single-site catalyst systems (SSC) differ from conventional ZN catalysts in at least one important respect. They have only a single active transition metal site in each catalyst molecule, and therefore the activity at this metal site is the same for all catalyst molecules. One type of SSC catalyst currently widely used on an industrial scale is a metallocene catalyst system consisting of a catalyst and a cocatalyst or activator. The catalyst is a transition metal complex with the metal atom located between two cyclic organic ligands, the ligands being the same or different cyclopentadiene derivatives. The cocatalyst can be any compound capable of activating the metallocene catalyst by converting the metallocene complex into a catalytically active species; one example of such a compound is an alumoxane, preferably a methylalumoxane with an average degree of oligomerization of 4 to 30. For purposes of the present invention, other neutral or ionic activators may be used, including, but not limited to, various organoboron compounds, such as tri(n-butyl)ammonium tetrakis(pentafluorophenylborate, dimethylanilinium tetrakis(pentafluorophenylborate, or trityl tetrakis(pentafluorophenylborate). Another type of SSC catalyst is the constrained geometry catalyst (CGC).

[0018] As used herein, CGC refers to a subclass of SSC catalyst systems known as constrained geometry catalysts. Unlike metallocenes, constrained geometry catalysts (CGCs) are characterized by having only one cyclic ligand bonded to one of the other ligands on the same metal center such that the angle at this metal between the center of mass of the π system and the additional ligand is smaller than in the comparable non-bridged complex. More specifically, the term CGC is used for ansa-bridged cyclopentadienyl amide complexes, but the definition goes far beyond this class of compounds. Thus, the term CGC is used broadly to refer to other more or less related ligand systems, which may or may not be isolobal and / or isoelectronic with the ansa-bridged cyclopentadienyl amide ligand system. In addition, the term is often used for related complexes with long ansa bridges that do not induce distortion.

[0019] Similar to metallocenes, suitable CGCs can be activated methylaluminoxane (MAO), perfluorinated borane, and trityl borate cocatalysts. However, CGC-based catalyst systems show much higher incorporation of higher alpha-olefins than the corresponding metallocene-based systems. Nonmetallocene-based SSC (also called post-metallocene) single-site catalysts for olefin polymerization are also known. Typical post-metallocene catalysts are characterized by bulky, neutral alpha-diimine ligands. These post-metallocene catalysts, however, are much more commonly used in the polymerization of ethylene to produce plastomers and elastomers. They are rarely used in the polymerization of α-olefins such as propylene. Single-site catalyst systems for olefin polymerization are well known to those skilled in the art and have been extensively discussed in two symposiums: Stereoselective Polymerization with Single-Site Catalysts (edited by Lisa S. Baugh and Jo Ann M. Canich, published by CRC Press (2008)) and Polyolefins: 50 Years after Ziegler and Natta II: Polyolefins by Metallocenes and Other Single-Site Catalysts (edited by Walter Kaminsky, published by Springer Heidelberg (2013)).

[0020] The compositions of the invention may include a first polymer and a second polymer in a weight ratio of about 9:1 to about 1:9, preferably about 7:1 to about 2:3, and most preferably about 5:1 to about 3:1. When multiple ranges of ingredients or properties are provided herein, the invention contemplates additional ranges between any of the limits of the ranges. For example, the weight ratio of the first polymer to the second polymer may be about 9:1 to about 2:3 and about 7:1 to about 3:1. The total amount of polymer in the compositions of the invention may vary over a wide range, for example, about 20% to about 80% by weight, preferably about 25% to about 60% by weight, and most preferably about 30% to about 45% by weight.

[0021] The first polymer in the hot melt adhesive composition of the present invention comprises either a homopolymer of propylene or a copolymer of propylene and at least one comonomer selected from the group consisting of ethylene and alpha-olefins having a carbon chain length of 4 to 8, having from about 70% to about 99% by weight propylene, preferably from about 80% to about 98% by weight, and most preferably from about 85% to about 98% by weight. The first polymer has a weight average molecular weight of about 10,000 g / mol to about 100,000 g / mol, preferably about 10,000 g / mol to about 80,000 g / mol, and most preferably about 10,000 g / mol to about 60,000 g / mol, a melting point measured using DSC of about 20° C. to about 150° C., preferably about 30° C. to about 110° C., and most preferably about 40° C. to about 100° C., and a melting enthalpy measured using DSC of about 30 J / g to about 100 J / g, preferably about 35 J / g to about 80 J / g, and most preferably about 35 J / g to about 60 J / g. These fusion enthalpies correspond to a crystallinity of about 18% to about 53% by weight, preferably about 18% to about 42% by weight, and most preferably about 18% to about 32% by weight, calculated from the fusion enthalpy of 190 J / g for 100% crystalline isotactic PP. Furthermore, the first polymer has a Brookfield viscosity at 190° C. preferably in the range of about 800 cP to about 100,000 cP, and most preferably about 1,000 cP to about 20,000 cP. In some embodiments, the first polymer has a weight average molecular weight of about 10,000 g / mol to about 30,000 g / mol, preferably about 12,000 g / mol to about 29,000 g / mol, and most preferably about 15,000 g / mol to about 27,500 g / mol. An exemplary first polymer according to the present invention includes Vistamaxx 8880, available from Exxonmobil Chemical Company.

[0022] The second polymer in the hot melt composition of the present invention is either a propylene homopolymer or a propylene-based copolymer with at least one comonomer selected from the group consisting of ethylene and alpha-olefins having a carbon chain length of 4 to 8, having about 70% to about 99% by weight, preferably about 80% to about 98% by weight, and most preferably about 80% to about 90% by weight of propylene. The second polymer has a weight average molecular weight of greater than 100,000 g / mol, preferably about 100,000 g / mol to about 1,000,000 g / mol, and most preferably about 100,000 g / mol to about 600,000 g / mol. Further, the second polymer is either a primarily amorphous material, exhibiting no DSC melting peak or with only slight residual crystallinity, exhibiting a DSC melting peak at about 20° C. to about 120° C., preferably about 30° C. to about 100° C., and most preferably about 40° C. to about 80° C., and having a melting enthalpy measured using DSC of about 0 J / g to about 30 J / g, preferably about 5 J / g to about 25 J / g, and most preferably about 5 J / g to about 20 J / g. These melting enthalpies correspond to a crystallinity of about 0% to about 18% by weight, preferably about 2.6% to about 15.8% by weight, and most preferably about 2.6% to about 13.2% by weight, calculated from the melting enthalpy of 190 J / g for 100% crystalline isotactic PP. The second polymer has a melt flow rate (MFR) of about 1 g / 10 min to about 200 g / 10 min, preferably about 10 g / 10 min to about 100 g / 10 min, and most preferably about 20 g / 10 min to about 60 g / 10 min, as measured at 230° C. / 2.16 Kg according to ASTM D1238. Exemplary second polymers according to the present invention include Vistamaxx 6502, available from Exxonmobil Chemical Company.

[0023] According to an embodiment of the present invention, the molecular weight of the second polymer (M w) is at least twice the molecular weight of the first polymer. Preferably, the molecular weight of the second polymer is at least three times greater than the molecular weight of the first polymer. More preferably, the molecular weight of the second polymer is at least five times greater than the molecular weight of the first polymer. The molecular weight of the second polymer may even be at least eight or ten times greater than the molecular weight of the first polymer. It has been found that by utilizing two polymer components with such a molecular weight offset for any adhesive disclosed herein, the object of the present invention can be more easily achieved. In another embodiment, the melting enthalpy of the first polymer is at least 20 J / g, preferably at least 35 J / g, and most preferably at least 50 J / g greater than the melting enthalpy of the second polymer.

[0024] The hot melt adhesive composition of the present invention also comprises a wax. Preferably, the wax comprises a Fischer-Tropsch wax. Synthetic Fischer-Tropsch wax is obtained by Fischer-Tropsch synthesis and comprises the hydrocarbons resulting from the cobalt or iron catalyzed Fischer-Tropsch synthesis of synthesis gas (CO and H2) into alkanes. The crude products of this synthesis are separated into liquid and different solid fractions by distillation. The hydrocarbons contain mainly n-alkanes, a few branched alkanes and essentially no cycloalkanes or impurities. Fischer-Tropsch waxes consist of methylene units and their carbon chain length distribution is characterized according to one embodiment by an even increase or decrease in the number of molecules for the particular carbon atom chain length involved.

[0025] The Fischer-Tropsch wax preferably has a branched hydrocarbon content of 10-25 wt%. The branched molecules of the Fischer-Tropsch wax preferably contain more than 10 wt%, most preferably more than 25 wt%, of molecules with methyl branches. Furthermore, the branched molecules of the Fischer-Tropsch wax preferably do not contain quaternary carbon atoms.

[0026] In a preferred embodiment of the present invention, the hydrocarbon wax has a molecular weight (number average) of 500 to 1200 grams per mole, more preferably 575 to 950 grams per mole. The molecular weight (number average) and isoalkane content of the hydrocarbon wax are provided using gas chromatography according to the European Wax Federation EWF method 001 / 03. In a preferred embodiment, the hydrocarbon wax further has one or more of the following properties, independent of each other: · Brookfield viscosity less than 20 mPa·s at 135 °C; a penetration at 25°C of less than 10 1 / 10 mm, preferably less than 8 1 / 10 mm; The hydrocarbon wax is hydrotreated; and Less than 1wt% oil content.

[0027] Needle penetration values ​​at 25° C. are provided according to ASTM D1321 and oil content of the wax is provided according to ASTM D721.

[0028] In an embodiment of the invention, the wax has one or more of the following characteristics: A freezing point according to ASTM D938 of about 60° C. to about 105° C., preferably about 64° C. to about 102° C., more preferably about 80° C. to about 102° C., and most preferably about 80° C. to about 86° C.; a percentage of isoalkanes of about 2.5% to 20%, preferably about 5% to 15%, and most preferably about 10% to 15%; and A heat of fusion provided in accordance with ASTM E793 of about 180 J / g to about 230 J / g, preferably about 205 J / g to about 230 J / g, and most preferably about 215 J / g to about 225 J / g.

[0029] A preferred wax for use herein is the SERATION line of Fischer-Tropsch waxes, particularly SERATION 1830, available from Sasol Ltd.

[0030] The hot melt adhesive composition of the present invention also comprises a hydrogenated styrenic block copolymer (SBC). The hydrogenated SBC may be selected from the group comprising styrene-ethylene-butylene-styrene (SEBS), styrene-ethylene-butylene (SEB), styrene-ethylene-propylene-styrene (SEPS), styrene-ethylene-propylene (SEP), and styrene-ethylene-ethylene-propylene-styrene (SEEPS). Preferably, the hydrogenated styrenic block copolymer comprises or is a SEBS, SEPS, or SEEPS polymer. Most preferably, the hydrogenated styrenic block copolymer comprises or is SEBS. In an embodiment, the SEBS has a diblock content of about 50 to about 85%, preferably about 60 to about 80%, a styrene content of about 15 to about 50%, preferably about 20 to about 40%, a melt flow rate of about 1 to about 100, preferably about 20 to about 90, more preferably about 40 to about 80 g / 10 min, tested at 200° C. using a 5 kg weight, and a Shore A hardness of about 40 to about 100, preferably about 50 to about 90, most preferably about 55 to about 85. One suitable SBC polymer for use in the present invention is commercially available under the trademark KRATON® G1726 by Kraton Corporation.

[0031] The hot melt adhesive compositions of the present invention also include a compatible tackifying resin or tackifier that enhances adhesion and improves specific adhesion. As used herein, the term "tackifier" or "tackifying resin" includes: (a) aliphatic and cycloaliphatic petroleum-based hydrocarbon resins having a Ring and Ball (R&B) softening point of 10° C. to 150° C. as determined by ASTM method E28-58T, the latter resins being obtained from the polymerization of monomers consisting mainly of aliphatic and / or cycloaliphatic olefins and diolefins; hydrogenated aliphatic and cycloaliphatic petroleum-based hydrocarbon resins are also included; examples of such resins available commercially based on C5 olefin fractions of this type are Piccotac 95 tackifying resin sold by Eastman Chemicals and Escorez 1310LC sold by ExxonMobil Chemical Company, examples of hydrogenated cycloaliphatic petroleum-based hydrocarbon resins based on cyclopentadiene are Escorez 5400 from Exxonmobil and Resinall R1095S from Resinall Corporation; (b) aromatic petroleum-based hydrocarbon resins and their hydrogenated derivatives; an example of a hydrogenated aromatic hydrocarbon resin is Arkon P-115 from Arakawa Chemicals; (c) Aliphatic / aromatic petroleum derived hydrocarbon resins and their hydrogenated derivatives; (d) Aromatically modified cycloaliphatic resins and their hydrogenated derivatives; (e) polyterpene resins having a softening point of about 10° C. to about 140° C., the latter polyterpene resins being generally obtained from the polymerization of terpene hydrocarbons, such as the monoterpene known as pinene, in the presence of Friedel-Crafts catalysts at moderately low temperatures; hydrogenated polyterpene resins are also included; (f) Copolymers and terpolymers of natural terpenes, such as styrene / terpene, -ethylstyrene / terpene, and vinyltoluene / terpene; (g) natural and modified rosins, such as gum rosin, wood rosin, tall oil rosin, distilled rosin, hydrogenated rosin, dimerized rosin, and polymerized rosin; (h) glycerol and pentaerythritol esters of natural and modified rosins, such as the glycerol ester of pale wood rosin, the glycerol ester of hydrogenated rosin, the glycerol ester of polymerized rosin, the pentaerythritol ester of pale wood rosin, the pentaerythritol ester of hydrogenated rosin, the pentaerythritol ester of tall oil rosin, and the phenolic modified pentaerythritol ester of rosin; and (i) Phenol-modified terpene resins, such as resin products obtained from the condensation of terpenes and phenols in an acidic medium.

[0032] In some formulations, a mixture of two or more of the above tackifying resins may be required. The tackifying resins useful in the present invention may possibly include polar tackifying resins. However, the selection of available polar tackifying resins is limited by the fact that many of the polar resins appear to be only partially compatible with polyolefins. Preferably, the tackifying resins may be selected from any of the non-polar types, which are commercially available. The preferred resins for use herein are thermoplastic resins obtained from the copolymerization and hydrogenation of C5 aliphatic olefins and diolefins generated in the naphtha pyrolysis process. Examples of such resins include the SUKOREZ® line of resins available from Kolon Industries.

[0033] The hot melt adhesive composition of the present invention also includes a plasticizer. The plasticizer serves to provide the desired viscosity control and impart flexibility. Suitable plasticizers may be selected from the group including not only conventional plasticizing oils such as mineral oils, but also olefin oligomers and low molecular weight polymers, as well as vegetable and animal oils and their derivatives. The petroleum-based oils that may be employed are relatively high boiling materials that contain only a small proportion of aromatic hydrocarbons. In this regard, aromatic hydrocarbons should preferably be less than 30%, more preferably less than 15%, of the oil, as measured by the proportion of aromatic carbon atoms. More preferably, the oil may be essentially non-aromatic. The oligomers may be polypropylene, polybutene, hydrogenated polyisoprene, hydrogenated polybutadiene, and the like, having an average molecular weight of about 350 g / mole to about 10,000 g / mole. Suitable vegetable and animal oils include glycerol esters of conventional fatty acids and their polymerization products. Other useful plasticizers may be found in the groups of conventional dibenzoates, phosphates, phthalate esters, and esters of mono- or polyglycols. Examples of such plasticizers include, but are not limited to, dipropylene glycol dibenzoate, pentaerythritol tetrabenzoate, 2-ethylhexyl diphenyl phosphate, polyethylene glycol 400-di-2-ethylhexoate; butyl benzyl phthalate, dibutyl phthalate, and dioctyl phthalate. The plasticizers that find utility in the present invention can be any number of different plasticizers, but the inventors have found that mineral oils and liquid polybutenes having an average molecular weight of less than 5,000 g / mol are particularly advantageous. As will be appreciated, plasticizers have typically been used to reduce the viscosity of the overall adhesive composition without substantially reducing the adhesive strength and / or the use temperature of the adhesive, as well as to extend the open time and improve the flexibility of the adhesive. Suitable plasticizers for use herein include the CALSOL line of plasticizers available from Calumet Specialty Products.

[0034] The relative amounts of the components of the hot melt adhesive composition of the present invention can vary over a wide range depending on the particular end use and desired properties, such as adhesion, application temperature, viscosity at application temperature, Shore A hardness, and perceived softness. In an embodiment of the present invention, the first polymer, second polymer, wax, hydrogenated styrenic block copolymer, tackifier, and plasticizer are present in amounts effective to provide a hot melt adhesive composition having one or both of the following: a creep resistance of at least 80 initially, after 1 week aging, and after 2 weeks aging, and at least 60 after 4 weeks aging; and A Shore A hardness of at least 80, preferably at least 87.

[0035] As used herein, creep resistance has the meaning as illustrated in the Examples below.

[0036] In an embodiment of the invention, the first polymer, the second polymer, the wax, the hydrogenated styrenic block copolymer, the tackifier, and the plasticizer are present in amounts effective to provide a hot melt adhesive composition having one or both of the following: Softness up to about 4, preferably up to about 3.5; A sprayability of at least about 1.5, preferably at least about 2; and A blocking value of up to about 3, preferably up to about 2.5.

[0037] As used herein, softness and sprayability have the meanings and are determined as explained in the examples below. Blocking value is a measure of the extent to which a peeled spool of laminate sticks to itself due to adhesive flowing from the substrate. A value of 1 means that none of the peeled spools stuck to themselves, while a value of 5 means that a large area of ​​the laminate stuck to itself. As the amount of wax increases, the Shore A hardness value increases, but it has also been found that the perceived softness of the cooled adhesive in the laminate increases with increasing amounts of wax. The increase in Shore A hardness accompanied by an improvement in perceived softness is counterintuitive and surprising.

[0038] According to another embodiment of the present invention, the main components of the hot melt adhesive composition, individually or collectively, are present in the following amounts: (a) the first polymer is present in an amount of about 0.1 to about 20 wt %; (b) the second polymer is present in an amount of about 8 to about 40 wt %; (c) the wax is present in an amount of about 2 to about 24 wt %; (d) the hydrogenated styrenic block copolymer is present in an amount of about 0.25 to about 30 wt %; (e) the tackifier is present in an amount of about 35 to about 65 wt %; (f) The plasticizer is present in an amount of about 2 to about 12 wt %.

[0039] According to another embodiment of the present invention (herein referred to as the “low SBC formulation”), the major components of the hot melt adhesive composition, individually or collectively, are present in the following amounts: (a) the first polymer is present in an amount of from about 4 to about 20 wt %, preferably from about 5 to about 15 wt %, and most preferably from about 6 to about 10 wt %; (b) the second polymer is present in an amount of from about 12 to about 40 wt %, preferably from about 15 to about 35 wt %, and most preferably from about 20 to about 30 wt %; (c) the wax is present in an amount of from about 4 to about 24 wt %, preferably from about 5 to about 20 wt %, and most preferably from about 7 to about 15 wt %; (d) the hydrogenated styrenic block copolymer is present in an amount of from about 0.25 to about 10 wt %, preferably from about 0.5 to about 5 wt %, and most preferably from about 0.5 to about 2 wt %; (e) the tackifier is present in an amount of from about 35 to about 65 wt %, preferably from about 40 to about 60 wt %, and most preferably from about 45 to about 55 wt %; (f) The plasticizer is present in an amount of from about 2 to about 12 wt %, preferably from about 3 to about 10 wt %, and most preferably from about 4 to about 7 wt %.

[0040] According to yet another embodiment of the present invention (herein referred to as the “high SBC formulation”), the major components of the hot melt adhesive composition, individually or collectively, are present in the following amounts: (a) the first polymer is present in an amount of from about 0.1 to about 10 wt %, preferably from about 0.2 to about 5 wt %, and most preferably from about 0.25 to about 3 wt %; (b) the second polymer is present in an amount of from about 8 to about 40 wt %, preferably from about 12 to about 30 wt %, and most preferably from about 15 to about 25 wt %; (c) the wax is present in an amount of from about 2 to about 20 wt %, preferably from about 3 to about 15 wt %, and most preferably from about 4 to about 10 wt %; (d) the hydrogenated styrenic block copolymer is present in an amount of from about 10 to about 30 wt %, preferably from about 12 to about 27 wt %, and most preferably from about 15 to about 25 wt %; (e) the tackifier is present in an amount of from about 35 to about 65 wt %, preferably from about 40 to about 60 wt %, and most preferably from about 45 to about 55 wt %; (f) The plasticizer is present in an amount of from about 2 to about 12 wt %, preferably from about 3 to about 10 wt %, and most preferably from about 4 to about 7 wt %.

[0041] The amounts of the components mentioned herein are based on the total weight of the hot melt adhesive composition. The composition may consist only of (i.e., consist essentially of or consist of) the six major components mentioned above. Alternatively, the hot melt adhesive composition may include one or more additional optional components. One such optional component is a stabilizer. The stabilizer, when present, may be included in an amount of about 0.1% to about 3% by weight. Preferably, about 0.2% to 1% of the stabilizer is incorporated into the composition. The stabilizers useful in the hot melt adhesive composition of the present invention are incorporated to help protect the above-mentioned polymers, and thus the entire adhesive system, from the effects of thermal and oxidative degradation, which typically occur during the manufacture and application of the adhesive, as well as during normal exposure of the final product to the ambient environment. Among the applicable stabilizers are high molecular weight hindered phenols and multifunctional phenols, such as sulfur and phosphorus-containing phenols. Hindered phenols are well known to those skilled in the art and may be characterized as phenolic compounds that also contain sterically bulky groups in close proximity to their phenolic hydroxyl groups. In particular, tertiary butyl groups are generally substituted on the benzene ring in at least one of the ortho positions relative to the phenolic hydroxyl group. The presence of these sterically bulky substituents near the hydroxyl group serves to suppress its stretching frequency and, accordingly, its reactivity; this steric hindrance therefore provides the phenolic compound with its stabilizing properties.

[0042] The performance of these stabilizers can be further improved by utilizing in combination with: (1) synergists, such as thiodipropionate esters and phosphites; and (2) chelating agents and metal deactivators, such as ethylenediaminetetraacetic acid, its salts, and disalicylalpropylenediimine.

[0043] It should be understood that other optional additives may be incorporated into the hot melt adhesive composition of the present invention to modify certain physical properties. These may include, for example, such materials as inert colorants, such as titanium dioxide, fillers, fluorescent agents, UV absorbers, surfactants, other types of polymers, etc. Typical fillers include talc, calcium carbonate, clay, silica, mica, wollastonite, feldspar, aluminum silicate, alumina, hydrated alumina, glass microspheres, ceramic microspheres, thermoplastic microspheres, barite, and wood flour. Surfactants are particularly important in disposable nonwovens for hygiene, because they can dramatically reduce the surface tension of the adhesive applied to, for example, the core of the diaper, thereby allowing for more rapid transfer and subsequent absorption of urine by the core.

[0044] The hot melt compositions of the present invention are further characterized in that they have a low viscosity at 177°C of at most about 40,000 cP, preferably at most about 20,000 cP, and most preferably at most about 10,000 cP, as measured using a Brookfield viscometer at 177°C according to ASTM-D3236.

[0045] The hot melt adhesive composition of the present invention may be compounded by using any of the mixing techniques known in the art. A representative example of a prior art mixing procedure involves placing all ingredients other than the polymer used in the present invention into a jacketed mixing kettle equipped with a rotor, and then raising the temperature of the mixture to a range of 150°C to 200°C to melt the contents. It should be understood that the exact temperature used in this step will depend on the melting points of the particular ingredients. The first and second polymers can then be subsequently introduced into the kettle under stirring, and mixing is continued until a consistent homogenous mixture is formed. The contents of the kettle are protected throughout the mixing process with an inert gas such as carbon dioxide or nitrogen. Various additions and modifications can be made to this procedure to produce the hot melt composition without departing from the spirit of the present invention, such as applying a vacuum to facilitate removal of entrapped air. Other equipment useful for compounding the compositions of the present invention include, but is not limited to, single or twin screw extruders or other types of extruders, kneaders, intensive mixers, Ross™ mixers, and the like.

[0046] The adhesive composition of the present invention can be used as a general purpose hot melt adhesive in many applications, such as disposable nonwoven hygiene articles, paper converting, flexible packaging, woodworking, carton and case sealing, labeling, and other assembly applications. Particularly preferred applications include nonwoven disposable diaper and feminine sanitary napkin constructions, elastic attachments in diapers and adult incontinence briefs, diaper and napkin core stabilization, diaper backsheet laminates, industrial filter material processing, surgical gown and drape assembly, etc.

[0047] The resulting hot melt adhesive can then be applied to a substrate using a variety of application techniques. Examples include hot melt glue gun, hot melt slot die coating, hot melt wheel coating, hot melt roller coating, melt blow coating, spiral spray, contact or non-contact strand coating (commercially available as Omega™, Surewrap™, V-slot™, and Allegro™). In a preferred embodiment, the hot melt adhesive is applied directly onto the elastic strands using a strand coating technique, which is the preferred technique for elastic accessories in the manufacture of diapers and adult incontinence articles. In one example, the hot melt composition of the present invention is coated using an Allegro™ nozzle to form a continuous adhesive bond line on the elastic strands used for the elastic legs, leg cuffs, and waistbands of baby diapers, training pants, and adult incontinence articles. It is not the intent of the present invention to provide a complete description of the various techniques, and details can be found in the literature or on the nozzle manufacturers' websites (www.nordson.com or www.itw.com).

[0048] In an embodiment of the present invention, the method of making a laminate includes the steps of: (1) applying the hot melt adhesive composition of the present invention in a molten state to a primary substrate; and (2) laminating the secondary substrate to a first substrate by contacting the secondary substrate with the adhesive composition, where at least one of the first substrate or the second substrate is elastic. The primary substrate can be an elastic portion of a diaper, such as an elastic strand used as part of a leg cuff of the diaper, or an elastic band used as a back-ear laminate of the diaper. Such elastic strands (or bands) and their use as part of a leg cuff of a diaper are shown in U.S. Pat. No. 5,190,606, which is incorporated herein by reference. The secondary substrate can include a nonwoven material, a woven fabric, or a film, such as a spunbond / meltblown / spunbond (SMS) nonwoven or a polyethylene film, and the method can include folding the secondary substrate around the elastic strands or wrapping the elastic strands with the secondary substrate. In this way, the secondary substrate may function solely as a substrate to encase one or more strands of the leg cuff.

[0049] In an alternative embodiment, a tertiary substrate may be used, with the secondary and tertiary substrates laminated to the elastic strands on opposite sides of the elastic strands. In such an embodiment, the secondary substrate may be a polyethylene film and the tertiary substrate may be a film of a nonwoven material, or vice versa. Additionally, a composite diaper backsheet consisting of a polyolefin film combined with a nonwoven may also be used as the secondary and tertiary substrates described above.

[0050] In other embodiments where the primary substrate is an elastic strand, the secondary substrate can be a polyethylene film and a tertiary substrate such as a nonwoven fabric can be adhered to the film. In embodiments where the primary substrate is a nonwoven fabric, the secondary substrate can be an elastic film. As shown in the examples below, the compositions of the present invention, when applied to elastic strands, provide outstanding results in creep tests that simulate industry performance requirements.

[0051] Laminates made by any of the methods described herein can be used as elastic leg cuffs, standing leg cuffs, elastic side panels, or elasticated ears in disposable articles. Such laminates have an elastic substrate and at least one other substrate.

[0052] Aspects of the invention Aspect 1. (a) a first polymer comprising a single-site catalyzed polypropylene copolymer having a weight average molecular weight of about 10,000 g / mole to about 90,000 g / mole and a fusion enthalpy of about 30 J / g to about 100 J / g; (b) a second polymer comprising a single-site catalyzed polypropylene copolymer having a weight average molecular weight greater than 100,000 g / mole and an enthalpy of fusion of from about 0 J / g to about 30 J / g; (c) wax; (d) hydrogenated styrene block copolymers; (e) tackifiers; and (f) Plasticizers 1. A hot melt adhesive composition comprising:

[0053] Aspect 2. 2. The composition of embodiment 1, wherein the hydrogenated styrenic block copolymer is selected from the group consisting of at least one of SEBS, SEPS, and SEEPS.

[0054] Aspect 3. 2. The composition of embodiment 1, wherein the hydrogenated styrenic block copolymer comprises SEBS.

[0055] Aspect 4. The composition according to embodiment 3, wherein the SEBS has a diblock content of about 50 to about 85%, preferably about 60 to about 80%, about 15 to about 50%, preferably about 20 to about 40%, of styrene, a melt flow rate of about 1 to about 60, preferably about 2 to about 50, more preferably about 5 to about 40 g / 10 min in a test at 200° C. using a 5 kg weight, and a Shore A hardness of about 40 to about 100, preferably about 50 to about 90, most preferably about 55 to about 85.

[0056] Aspect 5. (a) the first polymer is present in an amount of about 0.1 to about 20 wt %; (b) the second polymer is present in an amount of about 8 to about 40 wt %; (c) the wax is present in an amount of about 2 to about 24 wt %; (d) the hydrogenated styrenic block copolymer is present in an amount of about 0.25 to about 30 wt %; (e) the tackifier is present in an amount of about 35 to about 65 wt %; (f) the plasticizer is present in an amount of about 2 to about 12 wt %; The composition according to any one of aspects 1 to 4.

[0057] Aspect 6. (a) the first polymer is present in an amount of from about 4 to about 20 wt %, preferably from about 5 to about 15 wt %, and most preferably from about 6 to about 10 wt %; (b) the second polymer is present in an amount of from about 12 to about 40 wt %, preferably from about 15 to about 35 wt %, and most preferably from about 20 to about 30 wt %; (c) the wax is present in an amount of from about 4 to about 24 wt %, preferably from about 5 to about 20 wt %, and most preferably from about 7 to about 15 wt %; (d) the hydrogenated styrenic block copolymer is present in an amount of from about 0.25 to about 10 wt %, preferably from about 0.5 to about 5 wt %, more preferably from about 0.5 to about 3 wt %, and most preferably from about 0.5 to about 2 wt %; (e) the tackifier is present in an amount of from about 35 to about 65 wt %, preferably from about 40 to about 60 wt %, and most preferably from about 45 to about 55 wt %; (f) the plasticizer is present in an amount of from about 2 to about 12 wt %, preferably from about 3 to about 10 wt %, and most preferably from about 4 to about 7 wt %; The composition according to any one of aspects 1 to 4.

[0058] Aspect 7. (a) the first polymer is present in an amount of from about 0.1 to about 10 wt %, preferably from about 0.2 to about 5 wt %, and most preferably from about 0.25 to about 3 wt %; (b) the second polymer is present in an amount of from about 8 to about 40 wt %, preferably from about 12 to about 30 wt %, and most preferably from about 15 to about 25 wt %; (c) the wax is present in an amount of from about 2 to about 20 wt %, preferably from about 3 to about 15 wt %, and most preferably from about 4 to about 10 wt %; (d) the hydrogenated styrenic block copolymer is present in an amount of from about 10 to about 30 wt %, preferably from about 12 to about 27 wt %, and most preferably from about 15 to about 25 wt %; (e) the tackifier is present in an amount of from about 35 to about 65 wt %, preferably from about 40 to about 60 wt %, and most preferably from about 45 to about 55 wt %; (f) the plasticizer is present in an amount of from about 2 to about 12 wt %, preferably from about 3 to about 10 wt %, and most preferably from about 4 to about 7 wt %; The composition according to any one of aspects 1 to 4.

[0059] Aspect 8. 8. The composition of any one of the preceding aspects, wherein the wax comprises a Fischer-Tropsch wax.

[0060] Aspect 9. The wax has the following characteristics: (a) a freezing point according to ASTM D938 of about 60° C. to about 105° C., preferably about 64° C. to about 102° C., more preferably about 80° C. to about 102° C., and most preferably about 80° C. to about 86° C.; (b) a percentage of isoalkanes between about 2.5% and 20%, preferably between about 5% and 15%, and most preferably between about 10% and 15%; (c) Brookfield viscosity less than 20 mPa·s at 135°C; (d) a penetration at 25° C. of less than 10 1 / 10 mm, preferably less than 8 1 / 10 mm; (e) a heat of fusion, provided in accordance with ASTM E793, of from about 180 J / g to about 230 J / g, preferably from about 205 J / g to about 230 J / g, and most preferably from about 215 J / g to about 225 J / g; (f) less than 1% by weight oil; and (g) a molecular weight (number average) of 500 to 1200 grams per mole, more preferably 575 to 950 grams per mole; The composition of embodiment 8, comprising one or more of the following:

[0061] Aspect 10. 10. The composition of any of the preceding aspects, wherein the weight average molecular weight of the second polymer is at least two times, and preferably at least three times, the weight average molecular weight of the first polymer, and the enthalpy of fusion of the first polymer is at least 20 J / g, preferably at least 35 J / g, and most preferably at least 50 J / g greater than the enthalpy of fusion of the second polymer.

[0062] Aspect 11. The first polymer, the second polymer, the wax, the hydrogenated styrene block copolymer, the tackifier, and the plasticizer may be any of the following: a creep resistance of at least 80 initially, after 1 week aging, and after 2 weeks aging, and at least 60 after 4 weeks aging; and Shore A hardness of at least 80, preferably at least 87 11. The composition of any of the preceding embodiments, wherein the composition is present in an amount effective to provide a hot melt adhesive composition having

[0063] Aspect 12. The first polymer, the second polymer, the wax, the hydrogenated styrene block copolymer, the tackifier, and the plasticizer may be any of the following: Softness up to about 4, preferably up to about 3.5; A sprayability of at least about 1.5, preferably at least about 2; and Blocking value of up to about 3, preferably up to about 2.5 12. The composition of any of embodiments 1-11, wherein the composition is present in an amount effective to provide.

[0064] Aspect 13. 13. The composition of any of the preceding claims, wherein the hot melt adhesive has a viscosity at 177°C of at most about 40,000 cP, preferably at most about 20,000 cP, and most preferably at most about 10,000 cP, as measured by ASTM D3236-88.

[0065] Aspect 14. applying the hot melt adhesive composition according to any one of embodiments 1 to 13 in a molten state to a primary substrate; and laminating a secondary substrate to a first substrate by contacting the secondary substrate with an adhesive composition, where at least one of the first substrate or the second substrate is elastic. A method of making a laminate comprising:

[0066] Aspect 15. The method of embodiment 14, wherein the primary substrate is an elastic strand.

[0067] Aspect 16. 15. The method of embodiment 14, wherein the primary substrate is a nonwoven fabric.

[0068] Aspect 17. The method of embodiment 15, wherein the secondary substrate is a nonwoven fabric that encases the elastic strands.

[0069] Aspect 18. 16. The method of embodiment 15, wherein the secondary substrate is a polyethylene film and the tertiary substrate is a nonwoven fabric.

[0070] Aspect 19. 19. A laminate made by the method of any of aspects 14-18 for use as an elastic leg cuff, a standing leg cuff, an elastic side panel, or an elasticated ear of a disposable article.

[0071] Working Example The present invention is further illustrated by the following examples.

[0072] Brookfield viscosity is provided herein according to ASTM D-3236 method at 163°C (325°F).

[0073] Differential scanning calorimetry (DSC) tests were performed on a TA Instrument DSC Model Q1000 using a heat-cool-heat program. Samples, preferably about 10 mg in size, were sealed in aluminum DSC sample pans. The pans were placed in the instrument's sample chamber and heated from ambient temperature to 200°C at a heating rate of 20°C / min, from which the samples were quenched to -110°C. The temperature was then increased to 200°C at a heating rate of 20°C / min and data was collected. The enthalpy of fusion (ΔH), measured in Joules / gram (J / g), was calculated from the area of ​​the melting peak of the DSC curve using an application software package built into the Model Q1000 DSC. For the purposes of this invention, unless otherwise specified, the melting point is defined as the temperature corresponding to the maximum of the melting peak, i.e., the highest point of the melting peak.

[0074] Specimens for creep testing were prepared using a custom-built coater / laminator equipped with a Nordson™ Zero-Cavity hot melt coating module designed to accommodate Surewrap™, Allegro™, and slot die tips. For the present invention, the Allegro™ tip is used to apply the composition of the present invention directly to an Invista™ elastic strand having a fineness of 680 decitex (dtex). The tip has three separate adhesive nozzles or orifices spaced 5 mm apart, allowing three elastic strands to be coated simultaneously. Specimens for creep retention testing were prepared by using the Allegro™ single strand coating technique on a custom-built hot melt coater equipped with a Nordson Zero Cavity™ coating module fitted with an Allegro™ nozzle. Three elastic strands (Investa 680) stretched to 300% elongation were each coated at a coating temperature of approximately 150°C. In these coating tests, the entrance angle of the elastic strand to the nozzle guide (i.e., the angle between a line perpendicular to the applicator axis and the elastic strand extending between the nozzle and the guide or roller closest to the nozzle on the entrance side) was maintained at 2.5°. (Note that the above parameters are described using the convention adopted by the nozzle manufacturer, "Universal Allegro Elastic Coating Nozzles Customer Product Manual, Part 1120705_01" (published 2 / 15).) The adhesive was applied at a line speed of about 300 meters / min, a loading of 25 milligrams / strand / meter (mg / s / m), an open time of 0.5 seconds, and a nip roll pressure of 40 psi. The coated strand was then laminated between a polyethylene film (Clopay DH284 PE) and a polypropylene spunbond nonwoven (NW FQN 12 gsm) to form an elastic laminate.

[0075] Creep resistance tests were performed using the laminate specimens described in Examples 1 and 2. The laminate specimens include elastic strands and a non-elastic substrate. A segment of the laminate specimen of approximately 350 mm is fully stretched and securely attached to a piece of rigid Polyglass board. While the non-elastic substrate is maintained in the stretched configuration, a mark is made at 300 mm in length and the elastic strands are cut at the mark. The specimens are then placed in an air-circulating oven at 37.8° C. (100° F.). Under these conditions, the elastic strands in tension may retract to some distance. After 4 hours, the distance between the ends of the elastic strands is measured. The ratio of the final length to the initial length, defined as creep retention and expressed as a percentage (%), is a measure of the adhesive's ability to retain the elastic strands.

[0076] material Calsol 5550 is a naphthenic process oil available from Calumet Specialty Products.

[0077] Sukorez SU-500, available from Kolon USA Inc, is a hydrogenated DCPD tackifier with an R&B softening point of about 100°C.

[0078] Irganox 1010 is a hindered phenolic antioxidant commercially available from BASF Corporation.

[0079] Seration 1830 is a Fischer-Tropsch wax having a freezing point of about 83°C, commercially available from Sasol Ltd.

[0080] Licocene PP2502, commercially available from Clariant, is a polypropylene copolymer having a weight average molecular weight (Mw) of about 18,000 g / mol and a heat of fusion of about 37 J / g.

[0081] Vistamaxx 6502, commercially available from Exxonmobil Chemical Company, is a polypropylene copolymer having a weight average molecular weight (Mw) of about 119,000 g / mol and a heat of fusion of about 9 J / g.

[0082] Kraton G1726M, commercially available from Kraton Corporation, is a SEBS copolymer having a styrene content of 30 wt% and a diblock content of 70 wt%.

[0083] The hot melt adhesives of Examples 1 and 2, shown in weight percent in Table 1, were prepared using the ingredients and mixing procedure described herein above. Mixing was performed in a laboratory type mixer consisting of a motor-driven propeller, a heating mantle, a temperature control unit, and a vessel of approximately 1 gallon size under nitrogen at 177°C. The appropriate amount of each ingredient, calculated according to the ratios shown in the table, except for the polymer, was added to the vessel. The temperature of the vessel was then increased to melt the contents. Once the ingredients in the vessel were completely melted, the motor was started and stirring commenced. The polymeric ingredient was then introduced. Mixing was continued until the polymer was completely dissolved and a homogenous mixture was formed.

[0084] [Table 1]

[0085] Ring and Ball Softening Point ("SP" in Table 1) was measured in glycerol using an automated Herzog unit according to ASTM E28.

[0086] The following tests were performed on Examples 1 and 2, and on a commercially available PO-based adhesive H9696U from Bostik, Inc., and are reported in Tables 2 and 3 below: Creep Retention, Softness Test, and Sprayability Test.

[0087] The softness test averages five different parameters: hand friction, roughness, fuzziness, even weight hand feel, and asymmetric hand feel, with each parameter rated on a scale of 1 to 5, with 1 being softest and 5 being least soft. Hand friction is the force required to move the hand over the adhesive-deposited laminate surface, with no drag contributing to a lower number and high resistance (or drag) contributing to a higher number. Roughness is the overall presence of rough, grainy, or uneven particles on the adhesive-deposited laminate surface, with no such particles contributing to a lower number and more of such particles contributing to a higher number. Fuzziness is the amount of pile, fiber, or fuzz on the adhesive-deposited laminate surface, with no such pile, fiber, or fuzz contributing to a lower number and more of such contributing to a higher number. Hand feel is simply an overall subjective measure of how soft the laminate feels to the person touching the adhesive deposited laminate, and is counted twice in arriving at the overall average softness: once as the mean (called "evenly weighted" in Table 3) and once as the median (called "asymmetric" in Table 3).

[0088] The sprayability test was based on the observation of a non-spiral spray nozzle. Two criteria were observed: (1) the uniformity of each interval of the adhesive deposited on the strand, and (2) the amount of adhesive deposited on the strand relative to the total amount of adhesive sprayed. For the former, a small deviation in the length or width of the interval between adjacent adhesive deposits contributed to good sprayability, meaning a higher number on a scale of 1 to 5. Conversely, a large deviation in the length or width of the interval between adjacent adhesive deposits contributed to poor sprayability, meaning a lower number on a scale of 1 to 5. For the second criterion, a larger amount of adhesive deposited on the strand relative to the total amount of adhesive sprayed resulted in better sprayability (and better creep retention), and therefore a higher sprayability number, and vice versa.

[0089] [Table 2]

[0090] Example 1 demonstrated sprayability and creep retention comparable to the control.

[0091] [Table 3]

[0092] Both Examples 1 and 2 demonstrated better softness than the control.

[0093] Where a range of values ​​is provided, it is understood that each intermediate value between the upper and lower limits of that range, and any combination or subcombination of intermediate values, as well as any other stated or intermediate value in that stated range, is encompassed within the stated range of values. In addition, the invention includes a range of a component that is the lower limit of a first range and the upper limit of a second range for that component.

[0094] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as commonly understood by one of ordinary skill in the art to which this invention belongs. All publications and patents specifically mentioned herein are incorporated by reference in their entirety for all purposes, including describing and disclosing the chemicals, instruments, statistical analyses and methodologies described therein that may be used in connection with the present invention. All references cited herein should be taken as indicative of the level of skill in the art. Nothing herein should be taken as an admission that the present invention is not entitled to backdate such disclosure by virtue of prior invention.

[0095] Although illustrated and described herein with reference to certain specific embodiments, it is nevertheless not intended to limit the invention to the details shown, but rather various modifications may be made in the details within the scope and range of equivalents of the claims and without departing from the spirit of the invention.

Claims

1. (a) a first polymer comprising a single-site catalyzed polypropylene copolymer having a weight average molecular weight of about 10,000 g / mole to about 90,000 g / mole and an enthalpy of fusion of about 30 J / g to about 100 J / g; (b) a second polymer comprising a single-site catalyzed polypropylene copolymer having a weight average molecular weight greater than 100,000 g / mole and an enthalpy of fusion from about 0 J / g to about 30 J / g; (c) wax; (d) hydrogenated styrene block copolymer; (e) a tackifier; and (f) Plasticizer 1. A hot melt adhesive composition comprising:

2. 2. The composition of claim 1, wherein the hydrogenated styrenic block copolymer is selected from the group consisting of at least one of SEBS, SEPS, and SEEPS.

3. 2. The composition of claim 1, wherein the hydrogenated styrenic block copolymer comprises SEBS.

4. 4. The composition of claim 3, wherein the SEBS has a diblock of about 50 to about 85%, preferably about 60 to about 80%, about 15 to about 50%, preferably about 20 to about 40%, styrene, a melt flow rate of about 1 to about 60, preferably about 2 to about 50, more preferably about 5 to about 40 g / 10 min when tested at 200° C. using a 5 kg weight, and a Shore A hardness of about 40 to about 100, preferably about 50 to about 90, most preferably about 55 to about 85.

5. (a) the first polymer is present in an amount of about 4 to about 20 wt %, preferably about 5 to about 15 wt %, and most preferably about 6 to about 10 wt %; (b) said second polymer is present in an amount of about 12 to about 40 wt %, preferably about 15 to about 35 wt %, and most preferably about 20 to about 30 wt %; (c) the wax is present in an amount of from about 4 to about 24 wt %, preferably from about 5 to about 20 wt %, and most preferably from about 7 to about 15 wt %; (d) the hydrogenated styrenic block copolymer is present in an amount of from about 0.25 to about 10 wt %, preferably from about 0.5 to about 5 wt %, more preferably from about 0.5 to about 3 wt %, and most preferably from about 0.5 to about 2 wt %; (e) the tackifier is present in an amount of from about 35 to about 65 wt %, preferably from about 40 to about 60 wt %, and most preferably from about 45 to about 55 wt %; (f) the plasticizer is present in an amount of about 2 to about 12 wt %, preferably about 3 to about 10 wt %, and most preferably about 4 to about 7 wt %; The composition of claim 1.

6. The composition of claim 1 , wherein the wax comprises a Fischer-Tropsch wax.

7. 2. The composition of claim 1, wherein the weight average molecular weight of the second polymer is at least two times, preferably at least three times, the weight average molecular weight of the first polymer and the enthalpy of fusion of the first polymer is at least 20 J / g, preferably at least 35 J / g, and most preferably at least 50 J / g, greater than the enthalpy of fusion of the second polymer.

8. The first polymer, the second polymer, the wax, the hydrogenated styrene block copolymer, the tackifier, and the plasticizer are selected from the group consisting of the following: a creep resistance of at least 80 initially, after 1 week aging, and after 2 weeks aging, and at least 60 after 4 weeks aging; and Shore A hardness of at least 80, preferably at least 87 13. The composition of claim 1, present in an amount effective to provide a hot melt adhesive composition having

9. The first polymer, the second polymer, the wax, the hydrogenated styrene block copolymer, the tackifier, and the plasticizer are selected from the following: Softness up to about 4, preferably up to about 3.5; A sprayability of at least about 1.5, preferably at least about 2; and A blocking value of up to about 3, preferably up to about 2.5 The composition of claim 1 , present in an amount effective to provide.

10. 10. The composition of claim 1, wherein the hot melt adhesive has a viscosity of at most about 40,000 cP, preferably at most about 20,000 cP, and most preferably at most about 10,000 cP at 177°C as measured by ASTM D3236-88.

11. applying the hot melt adhesive composition of claim 1 in a molten state to a primary substrate; and laminating a secondary substrate to the first substrate by contacting the secondary substrate with the adhesive composition, wherein at least one of the first substrate or the second substrate is elastic. A method of making a laminate comprising:

12. The method of claim 11 , wherein the primary substrate is an elastic strand.

13. The method of claim 11 , wherein the primary substrate is a nonwoven fabric.

14. The method of claim 12 , wherein the secondary substrate is a nonwoven fabric that encases the elastic strands.

15. The method of claim 12, wherein the secondary substrate is a polyethylene film and the tertiary substrate is a nonwoven fabric.

16. 12. A laminate made by the method of claim 11 used as an elastic leg cuff, a standing leg cuff, an elastic side panel, or an elasticated ear of a disposable article.

Citation Information

Patent Citations

  • Polyolefin-based hot melt adhesive with improved properties

    JP2017516888A

  • Hot melt adhesive compositions and methods based on blends of propylene copolymers prepared using single-site catalysts

    JP2019508521A

  • Disposable absorbent article and a method for making the same

    US20140358100A1

  • Polypropylene impact copolymer based hot melt adhesive

    US20150024649A1

  • Hot melt adhesive compositions including polyolefin and styrene block copolymers, and articles including the same

    US20190382631A1

Cited By

  • Method for producing adhesive layer composition for producing cooling sheet, method for producing cooling sheet, and cooling sheet

    US12297380B2

  • Method for producing adhesive layer composition for producing cooling sheet, method for producing cooling sheet, and cooling sheet

    US20230093050A1