High strength self-lubricating polyurethane piston seal body and method for making same
A high-strength, self-lubricating polyurethane piston composition, enhanced with treated ultra-high molecular weight polyethylene and alumina powders, addresses the mechanical weaknesses of existing pistons, offering improved wear resistance and extended service life.
Patent Information
- Application Number
- JP2023557264
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2021-11-30
- Publication Date
- 2024-11-21
- Estimated Expiration
- 2041-11-30
AI Technical Summary
Existing piston seal bodies for concrete pumps, made from rubber or polyurethane materials, suffer from low mechanical strength, wear resistance, and high replacement frequency, leading to high operating costs.
A high-strength, self-lubricating polyurethane piston composition is developed by incorporating specially treated ultra-high molecular weight polyethylene powder, alumina powder, and molybdenum disulfide or sodium polytetrafluoroethylene powder into a polyurethane prepolymer system, enhancing mechanical strength and reducing friction.
The new composition achieves a tensile strength of ≧60MPa, elongation at break of ≧550%, tear strength of ≧115kN/m, Shore hardness of 96~98HA, and a service life exceeding 550 hours, significantly improving wear resistance and reducing friction.
Smart Images

Figure 2024543283000003 
Figure 2024543283000004 
Figure 2024543283000001
Abstract
Description
[Technical field]
[0001] The present invention relates to the field of polymeric materials, in particular to a composition for making a piston seal, a piston seal made from the composition, and a method for making a piston seal, which can be used as a concrete piston seal for a concrete pumping device. [Background technology]
[0002] The piston is an important core component of concrete pumping equipment (e.g., pump trucks, drag pumps, and truck-mounted pumps), which plays the role of sealing voids and pushing concrete during concrete delivery. The concrete delivered has a hard medium, complex components, high pump pressure, and high requirements for sealing performance, so the piston needs to have good mechanical strength and wear resistance. At present, the piston has a short service life, frequent replacement, and high operating costs.
[0003] Existing piston seals mainly include two materials: rubber material or polyurethane material. Rubber pistons are made of nitrile rubber as the main part by adding reinforcing agents, anti-aging agents, vulcanizing agents, etc., mixing them, and compressing them at high temperature. Patent Document 1 uses nitrile rubber as the main material to make pistons for concrete pump vehicles, where the main raw materials include nitrile rubber, ethyl acetate, polyisocyanate, etc., and fiber reinforcement is added during the making process, but the pump still has low strength and low hardness with a maximum hardness of 85A and a maximum tensile strength of 36MPa, so it cannot meet market demand.
[0004] Patent Document 2 relates to a portable pump mechanism for pumping construction materials or water, and Patent Document 3 relates to a vehicle structure for a concrete pump truck, but neither relates to a method for making a piston material. Patent Document 4 relates to a method for making a foamed polyurethane material, but the tensile strength is low at about 2 MPa, so it is not suitable for making a polyurethane material for a piston head. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] Chinese Patent Application No. CN201310234970.3 [Patent Document 2] U.S. Patent No. 10,415,556 [Patent Document 3] US Patent Application Publication No. 2010 / 0264635 [Patent Document 4] German Patent Application Publication No. 102005008242 Summary of the Invention [Means for solving the problem]
[0006] One of the objectives of the present invention is to provide a high strength, self-lubricating polyurethane piston that overcomes the problems of existing polyurethane pistons, which have low strength and high wear.By adding specially treated fillers to the polymerization system, the strength and wear resistance of the piston are improved, thereby extending its service life and reducing the frequency of replacement.
[0007] In one aspect, the present application provides a composition for making a piston seal, comprising the following components: 100 parts by weight of a polyurethane prepolymer, 10 to 20 parts by weight of a chain extender, 5 to 10 parts by weight of a surface silyated ultra-high molecular weight polyethylene powder, 1 to 1.5 parts by weight of an antioxidant, 1 to 2 parts by weight of a surface silyated alumina powder, and 1 to 3 parts by weight of molybdenum disulfide or sodium polytetrafluoroethylene powder.
[0008] In the present invention, "prepolymer" refers to a material formed by prepolymerization of monomers, which can be used when it is difficult to completely polymerize the monomers into a polymer at one time, or when voids and cracks should be avoided in processing and molding the polymer. The present invention uses polyurethane prepolymer as the main material for making the piston seal body.
[0009] "Polyurethane" is a general name for polymers that contain a certain amount of carbamate groups in the molecule. Polyurethanes can be prepared by the interaction of mono- or poly-organic isocyanates (e.g., toluene diisocyanate (TDI) or diphenylmethane diisocyanate (MDI)) with polyol compounds (e.g., polyether polyols or polyester polyols), and the polymer backbone formed contains multiple repeating carbamate groups. Polyurethane prepolymers are reactive semi-finished products obtained by reacting polyorganic isocyanates with polyols in a controlled ratio.
[0010] In certain embodiments, the polyurethane prepolymer is of the polyether type.
[0011] In certain embodiments, the polyurethane prepolymer is selected from one or both of the LF M2050 and LF M2032 models.
[0012] In certain embodiments, the polyurethane prepolymer has the following characteristics: Free MDI content: less than 0.1 wt%, for example, 0.01 wt% to 0.02 wt%, 0.02 wt% to 0.03 wt%, 0.03 wt% to 0.04 wt%, 0.04 wt% to 0.05 wt%, 0.05 wt% to 0.06 wt%, 0.06 wt% to 0.07 wt%, 0.07 wt% to 0.08 wt%, or 0.08 wt% to 0.09 wt%; Isocyanate (-NCO) content: 3.0% to 5.0%, for example, 3.0% to 3.5%, 3.5% to 4.0%, 4.0% to 4.5%, or 4.5% to 5.0%; Viscosity: 120 to 500 cps, for example, 120 to 150 cps, 150 to 200 cps, 200 to 300 cps, 300 to 400 cps, or 400 to 500 cps has one or more of the following.
[0013] In the present invention, the term "chain extender" refers to a substance that can react with a functional group on a linear polymer chain to extend the molecular chain and increase the molecular weight, which is commonly used to improve the mechanical properties and processing properties of polyurethane, polyester products, etc. In certain embodiments, the chain extender used is an alcohol chain extender, for example, an aromatic alcohol chain extender such as 1,4-bis(2-hydroxyethoxy)benzene (HQEE). In certain embodiments, the chain extender used is an amine chain extender, for example, a diamine chain extender such as 3,3'-dichloro-4,4'-diaminodiphenylmethane.
[0014] The present invention adds fillers such as specially modified ultra-high molecular weight polyethylene powder and alumina powder to the polyurethane base material to increase the mechanical strength of the polyurethane, and adds molybdenum disulfide or specially treated polytetrafluoroethylene as self-lubricating particles to the inside of the piston to reduce the coefficient of friction.
[0015] In a specific embodiment, the ultra-high molecular weight polyethylene powder used in the present invention has a particle size of 30 to 50 μm, for example, 30 to 35 μm, 35 to 40 μm, 40 to 45 μm, or 45 to 50 μm.
[0016] In certain embodiments, the ultra high molecular weight polyethylene powder used in the present invention has a molecular weight (e.g., viscosity average molecular weight) of from 4,000,000 to 5,000,000, e.g., from 4,000,000 to 4,500,000 or from 4,500,000 to 5,000,000.
[0017] In certain embodiments, the alumina powder used in the present invention has a particle size of from 3000 to 5000 mesh, such as from 3000 to 4000 mesh or from 4000 to 5000 mesh.
[0018] In certain embodiments, the antioxidant used in the present invention is a hindered phenol antioxidant, such as Antioxidant 1010.
[0019] In a particular embodiment, the sodium polytetrafluoroethylene powder is sodium naphthalene treated polytetrafluoroethylene powder.
[0020] In some embodiments, the sodium polytetrafluoroethylene powder has a particle size of from 3 to 20 μm, e.g., from 3 to 5 μm, from 5 to 10 μm, from 10 to 15 μm, or from 15 to 20 μm.
[0021] In certain embodiments, the composition comprises 10 to 11, 11 to 12, 12 to 13, 13 to 14, 14 to 15, 15 to 16, 16 to 17, 17 to 18, 18 to 19, or 19 to 20 parts by weight of a chain extender.
[0022] In some embodiments, the composition comprises 5 to 6, 6 to 7, 7 to 8, 8 to 9, or 9 to 10 parts by weight of the surface silylated ultra high molecular weight polyethylene powder.
[0023] In some embodiments, the composition comprises 1 to 1.2, 1.2 to 1.3, 1.3 to 1.4, or 1.4 to 1.5 parts by weight of an antioxidant.
[0024] In some embodiments, the composition comprises 1 to 1.2, 1.2 to 1.5, or 1.5 to 2 parts by weight of the surface silylated alumina powder.
[0025] In some embodiments, the composition comprises 1 to 2 or 2 to 3 parts by weight of molybdenum disulfide or sodium polytetrafluoroethylene powder.
[0026] The surface silylated ultra-high molecular weight polyethylene powder used in the present invention is Step 1: oxidizing ultra-high molecular weight polyethylene powder; Step 2: reacting the oxidized ultra-high molecular weight polyethylene powder with a silane coupling agent; The composition may be prepared by a method comprising:
[0027] The oxidation treatment in step 1 may be carried out in a solution containing potassium permanganate and nitric acid. In a specific embodiment, the solution is a mixed solution of saturated potassium permanganate aqueous solution and nitric acid aqueous solution (e.g., 50% to 60% nitric acid aqueous solution). In a specific embodiment, the oxidation treatment includes the steps of putting the ultra-high molecular weight polyethylene powder into a solution containing potassium permanganate and nitric acid (e.g., a mixed solution of saturated potassium permanganate aqueous solution and 50% nitric acid aqueous solution), heating (e.g., heating to 80 to 90°C) and stirring (e.g., stirring for 30 to 40 minutes), and then filtering it to obtain a powder, and then repeatedly washing the powder with deionized water, filtering it, and oven-drying it.
[0028] In step 2, a common silane coupling agent may be used in the silylation reaction, such as silane coupling agent KH540, silane coupling agent KH550, silane coupling agent KH560, and silane coupling agent KH570. In a specific embodiment, the silane coupling agent used is silane coupling agent KH550. The weight of the silane coupling agent used may be 0.1% to 1% (e.g., 0.3% or 0.6%) of the weight of the ultra-high molecular weight polyethylene powder.
[0029] The silylation reaction may be carried out under conditions of stirring (e.g., at a speed of 1500 to 2000 rpm) and heating (e.g., at 70 to 80° C.). In certain embodiments, the silylation process is carried out in a high speed mixer.
[0030] In a particular embodiment, the silylation reaction includes the steps of feeding the oxidized ultra-high molecular weight polyethylene powder into a high-speed mixer adjusted to a speed of 1500 rpm and a temperature of 70° C., and then adding dropwise the silane coupling agent KH550 in an amount of 0.3% or 0.6% by weight of the powder to carry out the coupling process.
[0031] According to the present invention, the sodium naphthalene treatment may include the steps of adding polytetrafluoroethylene powder to the sodium naphthalene treatment solution in which the powder is completely immersed, stirring it for 10 to 15 minutes, filtering it, and washing it several times with tetrahydrofuran and deionized water until the sodium naphthalene treatment solution has no odor. In certain embodiments, the sodium naphthalene treatment further includes putting the sodium polytetrafluoroethylene powder in an oven to dry (e.g., dry at 100-110°C for 100-150 hours), grinding it, and dispersing it.
[0032] In the present invention, the sodium naphthalene treatment solution is a solution obtained by dissolving or complexing equimolar amounts of sodium and naphthalene in an active ether, such as tetrahydrofuran.
[0033] In certain embodiments, the sodium naphthalene treatment solution is made by the following method: under the protection of nitrogen atmosphere, naphthalene is weighed and charged into active ether (e.g., tetrahydrofuran), and when naphthalene is completely dissolved, sodium is added thereto, and the mixture is thoroughly stirred, so that sodium dissolves to produce sodium naphthalene treatment solution. In certain embodiments, the weight of naphthalene is 120 to 150 g (e.g., 128 g). In certain embodiments, the weight of sodium is 20 to 25 g (e.g., 23 g). In certain embodiments, the volume of active ether (e.g., tetrahydrofuran) is 1 L.
[0034] The surface silylated alumina powder used in the present invention may be prepared by a method including a step of reacting alumina powder with a silane coupling agent under conditions of stirring (e.g., at a speed of 2000 to 3000 rpm) and heating (e.g., at 70 to 80° C.). In a particular embodiment, the step is carried out in a high-speed mixer. The silylation reaction may use a common silane coupling agent, such as silane coupling agent KH540, silane coupling agent KH550, silane coupling agent KH560, and silane coupling agent KH570. In a particular embodiment, the silane coupling agent used is silane coupling agent KH550. The weight of the silane coupling agent used may be 1% to 5%, for example 2%, of the weight of the alumina powder.
[0035] In a particular embodiment, the steps include feeding the alumina powder into a high-speed mixer adjusted to a speed of 2000 rpm and a temperature of 70° C., and adding a coupling agent KH550 in an amount of 2% by weight of the powder dropwise to perform the coupling process.
[0036] In one aspect, the present application provides a use of any of the compositions described above for making a piston seal body. In certain embodiments, the piston seal body is a concrete piston seal body.
[0037] In one aspect, the present application provides a piston seal body made by casting any of the compositions described above. In certain embodiments, the piston seal body is a concrete piston seal body.
[0038] The present application further provides a method of making the piston seal body of the present invention, comprising casting any of the compositions described above.
[0039] In certain embodiments, the method comprises: a) weighing out a polyurethane prepolymer, a chain extender, a surface-silylated ultra-high molecular weight polyethylene powder, a molybdenum disulfide or sodium polytetrafluoroethylene powder, a surface-silylated alumina powder, and an antioxidant, each in parts by weight; b) putting polyurethane prepolymer, surface silylated ultra-high molecular weight polyethylene powder, molybdenum disulfide or sodium polytetrafluoroethylene powder, and surface silylated alumina powder into tank A of the injection molding machine, mixing it uniformly, and stirring it at a low speed of 650 rpm to 950 rpm (e.g., 700 rpm) by controlling the temperature at 80 to 100°C (e.g., 90°C); c) adding the chain extender to tank B of the injection molding machine, and controlling the temperature to 110 to 120°C (e.g., 115°C) until the chain extender is completely dissolved; and adding the antioxidant while stirring at a high speed of 1500 to 2500 rpm (e.g., 1600 rpm); d) cleaning the mold cavity, spraying the mold with a release agent and preheating it in an oven at 110 to 130° C. (e.g., 120° C.); e) mixing the liquids in tank A and tank B at a controlled ratio by an injection molding machine under reduced pressure, stirring at a high speed of 2000 to 3500 rpm by maintaining the temperature at 100 to 120°C, and then injecting it into a mold; f) placing the mold in an oven for heating at 100-120°C for 16-20 hours, and demolding after the mold is removed; g) machining the demolded blank to obtain the piston seal body of the present invention; Includes.
[0040] In certain embodiments, the surface-silylated ultra-high molecular weight polyethylene powder, sodium polytetrafluoroethylene powder, and / or surface-silylated alumina powder are made by the methods described above.
[0041] The piston seal of the present invention has excellent wear resistance and a small coefficient of friction, and at the same time, can be used as a high-strength self-lubricating piston seal having high mechanical strength, and can greatly extend the service life of the piston. In a specific embodiment, the piston seal has the following characteristics: Tensile strength: ≥60MPa; Elongation at break: ≥ 550%; Tear strength: ≧115kN / m; Shore hardness: 96~98HA; Akron wear: ≦0.025cm 3 ; Service life: over 550 hours (over 50% improvement over the service life of pure polyurethane concrete pistons) has one or more of the following.
[0042] Methods commonly used in the art are used to test the performance of piston seals. Typical test criteria are as follows:
[0043] [Table 1]
[0044] The present application further provides a piston comprising the piston seal body of the present invention.In a particular embodiment, the piston is a concrete piston.
[0045] Furthermore, the present application also provides a delivery cylinder comprising a piston seal body or a piston of the present invention.
[0046] Furthermore, the present application also provides a concrete pumping apparatus (e.g., pump truck, drag pump, truck-mounted pump) comprising the piston seal body, piston, or delivery cylinder of the present invention.
[0047] 1 and 2 show an example of the structure of the concrete piston seal body of the present invention, in which Fig. 1 is a cross-sectional view, and Fig. 2 is a partial schematic view of the cross-section of Fig. 1.
[0048] In the drawings, the numbers refer to the following: 1 - the angle of the inner ring of the lip opening of the concrete piston relative to the horizontal plane, 2 - the angle of the lip opening of the concrete piston relative to the horizontal plane, 3 - the angle of inclination of the outer lip opening of the concrete piston relative to the vertical, 4- Side friction surface of the concrete piston, 5 - lubricating oil receiving groove of concrete piston, 6-Schematic diagram of ultra-high molecular weight polyethylene powder, and 7-Schematic diagram of alumina powder.
[0049] In a particular embodiment, the concrete piston seal body of the present invention has the following main dimensions: Angle of the inner ring of the lip opening to the horizontal plane: 40~45°, Lip opening angle to horizontal plane: 3~10°, Angle of inclination of the outer lip opening relative to the vertical: 15-25°; Width of side friction surface: 10~15mm, Lubricant groove depth: 3~5mm.
[0050] The piston seal is provided with a special oil-receiving groove for improved lubrication. Effect of the Invention
[0051] The piston seal of the present invention has the following advantageous effects: 1. The piston seal body of the present invention provides a simple production process with low cost and stable quality; 2. For the piston seal body of the present invention, a special filler treatment process is adopted, so that the ultra-high molecular weight polyethylene powder, polytetrafluoroethylene powder and alumina powder are tightly bonded and uniformly dispersed in the polyurethane substrate; 3. The particles that enhance the anti-friction of the piston seal body of the present invention are uniformly dispersed, which can improve the wear resistance; 4. The piston seal body of the present invention has excellent mechanical properties and can meet the operating conditions of concrete extrusion under high pressure; 5. The piston seal of the present invention can realize self-lubrication at the sealing lip opening, the contact surface with the cylinder, and the contact surface with the concrete, so as to reduce the friction coefficient and wear loss; 6. The self-lubricating particles inside the piston seal body of the present invention are uniformly dispersed and continue to achieve the self-lubricating effect on the new friction surface. has one or more of the following. [Brief description of the drawings]
[0052] [Figure 1] A cross-sectional view of the piston seal body of the present invention. The numbers in the drawing refer to: 1 - the angle of the inner ring of the lip opening of the piston relative to the horizontal plane, 2 - the angle of the lip opening of the piston relative to the horizontal plane, 3 - the angle of the outer inclination of the lip opening of the piston relative to the vertical direction, 4 - the side friction surface of the concrete piston, 5 - the lubricating oil receiving groove of the piston. [Diagram 2]FIG. 2 is a partial schematic diagram of the cross section of FIG. 1. The numbers in the drawing refer to: 6 - schematic diagram of ultra-high molecular weight polyethylene powder, 7 - schematic diagram of polytetrafluoroethylene powder, 8 - schematic diagram of alumina powder. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0053] The embodiments of the present invention are described in detail below with reference to examples. However, those skilled in the art will understand that the following examples are merely illustrative of the present invention and should not be considered as limiting the scope of the present invention. The examples without detailed conditions are carried out according to conventional conditions or conditions recommended by the manufacturer. All reagents or equipment used that are not indicated with the manufacturer are conventional products available on the market. EXAMPLES
[0054] Example 1 (1) 2500g of ultra-high molecular weight polyethylene powder was put into a mixed solution of saturated potassium permanganate solution and 50% nitric acid, heated to 80℃ and stirred for 30 minutes, and then filtered to obtain a powder. The powder was then repeatedly washed with deionized water, filtered, and oven-dried. The powder was then put into a high-speed mixer adjusted to a speed of 1500 rpm and a temperature of 70℃, and 7.5g of coupling agent KH550 was added dropwise to carry out coupling treatment; (2) 750g of polytetrafluoroethylene powder was put into the sodium naphthalene solution to be completely soaked, then stirred, the powder was repeatedly washed with tetrahydrofuran, filtered, and put into an oven to dry for 150 hours, after which it was crushed and dispersed; (3) 250g of alumina powder was put into a high-speed mixer adjusted to a speed of 2000 rpm and a temperature of 70°C, and 5g of coupling agent KH550 was added dropwise to carry out coupling treatment; (4) 25,000 g of prepolymer was added to tank A of the injection molding machine, the temperature was controlled at 90°C, and the above surface-treated ultra-high molecular weight polyethylene powder, polytetrafluoroethylene powder and alumina powder were uniformly mixed to form a prepolymer, and stirred at a low speed of 700 rpm; (5) 3750g of chain extender was put into tank B of the injection molding machine, and the temperature was controlled at 115°C. When the chain extender was completely dissolved, 250g of antioxidant was added thereto and stirred at a speed of 1600 rpm; (6) The mold cavity was cleaned, the mold was sprayed with a release agent, and the mold was preheated in an oven at 120°C; (7) The liquids in tank A and tank B were mixed, decompressed, the temperature was controlled at 120°C, and the liquid was stirred at a high speed of 2500 rpm, and then injected into the cavity of the mold; (8) The mold was placed in a 120°C oven for 16 hours, and then demolded; (9) The resulting demolded blank was machined to produce a high strength, self-lubricating polyurethane piston.
[0055] Example 2 (1) 1250g of ultra-high molecular weight polyethylene powder was put into a mixed solution of saturated potassium permanganate solution and 50% nitric acid, heated to 80℃ and stirred for 30 minutes, and then filtered to obtain a powder. The powder was then repeatedly washed with deionized water, filtered, and oven-dried. The powder was then put into a high-speed mixer adjusted to a speed of 1500 rpm and a temperature of 70℃, and 7.5g of coupling agent KH550 was added dropwise to carry out coupling treatment; (2) 500g of polytetrafluoroethylene powder was put into the sodium naphthalene solution to be completely soaked, then stirred, the powder was repeatedly washed with tetrahydrofuran, filtered, and put into an oven to dry for 150 hours, after which it was crushed and dispersed; (3) 250g of alumina powder was put into a high-speed mixer adjusted to a speed of 2000 rpm and a temperature of 70°C, and 5g of coupling agent KH550 was added dropwise to carry out coupling treatment; (4) 25,000 g of prepolymer was added to tank A of the injection molding machine, the temperature was controlled at 90°C, and the above surface-treated ultra-high molecular weight polyethylene powder, polytetrafluoroethylene powder and alumina powder were uniformly mixed to form a prepolymer, and stirred at a low speed of 700 rpm; (5) 3750g of chain extender was put into tank B of the injection molding machine, and the temperature was controlled at 115°C. When the chain extender was completely dissolved, 250g of antioxidant was added thereto, and stirred at a high speed of 1600 rpm; (6) The mold cavity was cleaned, the mold was sprayed with a release agent, and the mold was preheated in an oven at 120°C; (7) The liquids in tank A and tank B were mixed, decompressed, the temperature was controlled at 120°C, and the liquid was stirred at a high speed of 2500 rpm, and then injected into the cavity of the mold; (8) The mold was placed in a 120°C oven for 16 hours, and then demolded; (9) The resulting demolded blank was machined to produce a high strength, self-lubricating polyurethane piston.
[0056] Comparative Example 1 (1) 25,000 g of prepolymer was added into tank A of the injection molding machine, stirred at a low speed of 700 rpm, and the temperature was controlled at 90°C; (2) 3750g of chain extender was charged into tank B of the injection molding machine, the temperature was controlled at 115℃, and when the chain extender was completely dissolved, it was stirred at a high speed of 1600 rpm; (3) The cavity of the mold was cleaned, the mold was evenly sprayed with a release agent, and the mold was preheated in an oven at 120°C; (4) The liquids in tank A and tank B were mixed, decompressed, the temperature was controlled at 120°C, and the liquid was stirred at a high speed of 2500 rpm, and then injected into the cavity of the mold; (5) The mold was placed in a 120°C oven for 16 hours, and then demolded; (6) The demolded blanks were machined to produce high strength, self-lubricating polyurethane pistons.
[0057] The concrete piston seal bodies prepared in Example 1, Example 2 and Comparative Example 1 were tested for mechanical performance, wear resistance and service life. The results are shown in Table 1.
[0058] [Table 2]
[0059] Although specific embodiments of the present invention have been described in detail, those skilled in the art will understand that many modifications and variations can be made in detail in light of the entire teachings disclosed herein, and each of such modifications and variations falls within the scope of protection of the present invention. The full scope of the present invention is provided by the appended claims and any equivalents thereof.
Claims
1. A composition for making a piston seal body, comprising the following components: 100 parts by weight of a polyurethane prepolymer, 10 to 20 parts by weight of a chain extender, 5 to 10 parts by weight of a surface silylated ultra-high molecular weight polyethylene powder, 1 to 1.5 parts by weight of an antioxidant, 1 to 2 parts by weight of a surface silylated alumina powder, and 1 to 3 parts by weight of molybdenum disulfide or sodium polytetrafluoroethylene powder.
2. The polyurethane prepolymer is of the polyether type, Preferably, the polyurethane prepolymer is selected from one or both of the LF M2050 and LF M2032 models; Preferably, the polyurethane prepolymer has the following characteristics: (1) Free MDI content: less than 0.1 wt%; (2) Isocyanate (-NCO) content: 3.0% to 5.0%; (3) Viscosity: 120 to 500 cps The composition of claim 1 having one or more of the following:
3. The surface silylated ultra-high molecular weight polyethylene powder is Step 1: oxidizing ultra-high molecular weight polyethylene powder; Step 2: reacting the oxidized ultra-high molecular weight polyethylene powder with a silane coupling agent; The method comprises the steps of: Preferably, the oxidation treatment in step 1 is carried out in a solution containing potassium permanganate and nitric acid; Preferably, the solution is a mixture of a saturated potassium permanganate aqueous solution and a nitric acid aqueous solution (e.g., a 50% to 60% nitric acid aqueous solution); Preferably, step 1 includes: putting the ultra-high molecular weight polyethylene powder into the solution containing potassium permanganate and nitric acid; heating and stirring the solution, and then filtering the solution to obtain a powder; and then repeatedly washing the powder with deionized water, filtering the powder, and oven-drying the powder. Including, Preferably, the silane coupling agent is selected from the group consisting of silane coupling agent KH540, silane coupling agent KH550, silane coupling agent KH560, and silane coupling agent KH570; 3. The composition according to claim 1 or 2, wherein the weight of the silane coupling agent is preferably from 0.1% to 1% of the weight of the ultra-high molecular weight polyethylene powder.
4. The sodium polytetrafluoroethylene powder is a sodium naphthalene-treated polytetrafluoroethylene powder, Preferably, the polytetrafluoroethylene powder is treated by adding the polytetrafluoroethylene powder to a sodium naphthalene treatment solution in which it is completely immersed, stirring for 10 to 15 minutes, filtering, and washing the powder several times with tetrahydrofuran and deionized water until the sodium naphthalene treatment solution is odorless; 4. The composition of claim 1, wherein the sodium naphthalene treatment further comprises grinding and dispersing the sodium polytetrafluoroethylene powder after placing it in an oven for drying.
5. The surface-silylated alumina powder is prepared by a method comprising the steps of reacting an alumina powder with a silane coupling agent under the conditions of stirring and heating; Preferably, the silane coupling agent is selected from the group consisting of silane coupling agent KH540, silane coupling agent KH550, silane coupling agent KH560, and silane coupling agent KH570; 5. The composition according to claim 1, wherein the weight of the silane coupling agent is from 1% to 5% of the weight of the alumina powder.
6. Features: (1) The chain extender is an alcohol chain extender or an amine chain extender, for example, an aromatic alcohol chain extender or a diamine chain extender such as 1,4-bis(2-hydroxyethoxy)benzene or 3,3′-dichloro-4,4′-diaminodiphenylmethane; (2) the ultra-high molecular weight polyethylene powder has a particle size of 30 to 50 μm; (3) the ultra-high molecular weight polyethylene powder has a molecular weight of 4,000,000 to 5,000,000; (4) the alumina powder has a particle size of 3000 to 5000 mesh; (5) The antioxidant is a hindered phenol antioxidant, such as Antioxidant 1010; (6) The sodium polytetrafluoroethylene powder has a particle size of 3 to 20 μm. The composition of claim 1 , wherein the at least one of the following is a hydroxyl group:
7. Use of a composition according to any one of claims 1 to 6 for making a piston seal, comprising Preferably, the piston seal body is a concrete piston seal body.
8. A piston seal body made by injection molding a composition according to any one of claims 1 to 7, Preferably, the piston seal is a concrete piston seal; Preferably, the piston seal body has the following characteristics: Tensile strength: ≧60 MPa; Breaking elongation: ≧550%; Tear strength: ≧115kN / m; Shore hardness: 96-98HA; Akron wear: ≦0.025 cm 3 ; Service life: over 550 hours The piston seal body has one or more of the following:
9. 7. A method of making a piston seal body comprising casting a composition according to any one of claims 1 to 6, comprising the steps of: Preferably, the method comprises the steps of: a) weighing out a polyurethane prepolymer, a chain extender, a surface-silylated ultra-high molecular weight polyethylene powder, a molybdenum disulfide or sodium polytetrafluoroethylene powder, a surface-silylated alumina powder, and an antioxidant, each in parts by weight; b) putting the polyurethane prepolymer, the surface-silylated ultra-high molecular weight polyethylene powder, the molybdenum disulfide or the sodium polytetrafluoroethylene powder, and the surface-silylated alumina powder into tank A of an injection molding machine, mixing it uniformly, and stirring it at a low speed of 650 rpm to 950 rpm by controlling the temperature at 80 to 100°C; c) adding the chain extender into tank B of the injection molding machine, controlling the temperature at 110-120°C, and adding the antioxidant when the chain extender is completely dissolved while stirring at a high speed of 1500-2500 rpm; d) cleaning the mold cavity, spraying the mold with a release agent and preheating it in an oven at 110-130° C.; e) mixing the liquids in tank A and tank B in a controlled ratio by the injection molding machine under reduced pressure, stirring at a high speed of 2000 to 3500 rpm while maintaining the temperature at 100 to 120° C., and then injecting the liquid into the mold; f) placing the mold in an oven for heating at 100-120° C. for 16-20 hours, and demolding after it is removed; g) machining the demolded blank to obtain the piston seal body; Including, Preferably, the surface-silylated ultra-high molecular weight polyethylene powder, the sodium polytetrafluoroethylene powder, and / or the surface-silylated alumina powder are made by the method according to claims 3, 4, and / or 5.
10. A piston comprising the piston seal body according to claim 8, Preferably, the piston is a concrete piston.
11. A delivery cylinder comprising a piston seal body according to claim 8 or a piston according to claim 10.
12. 12. A concrete pumping apparatus (e.g. a pump car, a drag pump or a truck mounted pump) comprising a piston seal body as claimed in claim 8, a piston as claimed in claim 10 or a delivery cylinder as claimed in claim 11.
Citation Information
Patent Citations
Self-lubricating high-wear-resistance piston sealing body and preparation method thereof
CN113527864A
Biaxially oriented polyester film for capacitor
JP1998315416A
Polyurethane elastomer seal for hydraulic pumps
JP2016535149A
Thermoplastic polyurethane elastomer composition, thermoplastic polyurethane elastomer, packing and method for producing thermoplastic polyurethane elastomer
JP2019019255A
Adhesive of short fiber rubber used for concrete delivery pump piston and method for manufacturing short fiber rubber
CN103319754A