Printed packaging material with improved recyclability and its manufacturing method

The packaging material with thermally stable inks and adhesives, composed of laminated plastic films, addresses the limited recyclability of plastic packaging by producing high-quality recycled granules with minimal impurities and improved processing properties.

JP2024543328APending Publication Date: 2024-11-21KONSTANTIA PIRK GMBH BESCHLENKTEL HAFTSUNG & KOMPANY KOMMANDI TOGESELLSCHAFT
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
JP2024525416
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2021-11-03
Filing Date
2022-11-03
Publication Date
2024-11-21

AI Technical Summary

Technical Problem

Existing plastic packaging materials have limited recyclability, leading to low-quality recycled products and limited applications due to impurities and decomposition products during recycling.

Method used

A recyclable plastic-containing packaging material composed of laminated plastic films with at least 70% of a single type of monomer or polymer, featuring thermally stable printing inks and adhesives with controlled weight loss at specific temperature ranges, and optionally including additives to minimize gaseous decomposition products.

Benefits of technology

The solution enhances recyclability, producing high-quality recycled plastic granules with reduced impurities and improved mechanical properties, suitable for further processing without gas bubbles or viscosity issues.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024543328000001
    Figure 2024543328000001
  • Figure 2024543328000002
    Figure 2024543328000002
  • Figure 2024543328000003
    Figure 2024543328000003
Patent Text Reader

Abstract

The present invention relates to a recyclable plastic-containing packaging material comprising a carrier material consisting of at least two plastic films laminated with an adhesive, the films comprising at least 70% by weight of a single type of monomer and / or polymer, and an optically perceptible element formed by a printing ink, wherein the printing ink and / or adhesive are thermally stable and have a weight loss of less than 20% when exposed to temperatures in the range of ≥ 30° C. and ≤ 320° C. Furthermore, the present invention relates to a method for predicting the recyclability of a plastic-containing packaging material comprising the printing ink and / or adhesive.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a printed and / or adhesive-containing packaging material. The present invention further relates to a package made of such a packaging material, a recycle product obtained from a recycling process of this packaging material, and a method for producing such a packaging material. The present invention further relates to a method for predicting the recyclability of such a packaging material. [Background technology]

[0002] A variety of plastic materials and composites are known in the art for packaging purposes, e.g., food packaging. To meet the requirements regarding protection of the packaged goods, these plastic packages often include a barrier layer. Composites and / or laminates of different materials are often used to provide a barrier against multiple substances or classes of substances. Packaging is often printed to allow the packaged goods to be labelled and / or assigned to a particular company and / or manufacturer.

[0003] Such packaging materials are often constructed from multiple layers, not necessarily all of which are made of plastic - for example, packaging materials are known that include layers of metal and paper.

[0004] The recyclability of packaging has become very important in recent years. There is an increasing demand for packaging that provides sufficient safety for the packaged goods and is as completely recyclable as possible.

[0005] While cellulose fibers obtained from paper and metal are already recycled to a high extent and can be used to manufacture high-quality products, the recyclability of plastics is still limited and the materials obtained during recycling are often only capable of thermal recycling due to impurities or are further processed into lower-value products with lower purity requirements for the materials used.

[0006] In order to increase the recyclability of plastics, attempts have been made in the past to produce packaging materials from as few as possible one type of plastic. However, to meet the requirements of mechanical strength, barrier properties, printability, processability, etc., laminates using different polymers of a single monomer and its associated comonomers (e.g. α-olefins to synthesize LLDPE) are often used. For example, starting from ethylene as the only monomer, it is possible to obtain polymers that can be assigned to the groups HDPE (high density polyethylene), LDPE (low density polyethylene), LLDPE (linear low density polyethylene), PE-HMW (high molecular weight polyethylene), PE-UHMW (ultra-high molecular weight HDPE) and PE-X (post-crosslinked PE). Furthermore, any type of polyethylene can be considered as a polyolefin material and is preferred for some embodiments. In particular, ethylene copolymers selected from the group consisting of ethylene-vinyl acetate copolymer (EVA), methacrylic acid ethyl ester (EMA), ethylene / acrylic acid copolymer (EAA) and ethylene-butyl acrylate copolymer (EBA) are preferred. Preferably, these copolymers have an ethylene by weight and / or particle content of ≧70%.

[0007] Starting from propylene, the addition of methyl groups compared to ethylene allows for even more variations. For example, the properties of polypropylene can be differentiated into isotactic polypropylene (iPP), syndiotactic polypropylene (sPP) and atactic polypropylene (aPP) depending on the arrangement of the additional groups in the chain. Furthermore, any combination of polypropylene with ethylene as a comonomer is considered as a polyolefin material and is preferred for some applications. Preferably, the polypropylene copolymer is selected from the group consisting of polypropylene random copolymers with ethylene as a comonomer and polypropylene-ethylene block copolymers. Preferably, these copolymers have a propylene content of 70% by weight or more.

[0008] Propylene-based foams (polypropylene foams (EPP)) are also known. Mechanical (post)treatment of polypropylene (films) can also change the properties by favouring the orientation of the polymer chains. For example, unoriented polypropylene films (CPP) and unoriented polypropylene films (OPP and BOPP) are known. In the case of oriented polypropylene films, a distinction can also be made between unidirectionally oriented polypropylene films (OPP) and bidirectionally oriented polypropylene films (BOPP (biaxially oriented polypropylene)). Summary of the Invention [Problem to be solved by the invention]

[0009] However, it has become clear that only a small proportion of single-plastic-based packaging materials, when recycled, can provide raw materials that meet the quality requirements for manufacturing high-quality plastic products, which has led to significant customer concerns about recycled plastics and their potential applications remaining limited.

[0010] Therefore, there is a demand for plastic products (especially plastic packaging materials) that are easier to recycle and contain fewer impurities than those currently on the market. Furthermore, if a plastic product contains additional components in addition to plastic, it is necessary to be able to predict the recyclability of that product. [Means for solving the problem]

[0011] This problem is solved by the object of the independent patent claims. One solution to the above problem lies in a recyclable plastic-containing packaging material consisting of a carrier material consisting of at least two plastic films laminated with an adhesive. These films consist of at least 70% by weight of a single type of monomer and / or polymer. Furthermore, such packaging material comprises an optically perceptible element formed by a printing ink, and is characterized in particular in that the printing ink and / or the adhesive are thermally stable and have a weight loss of less than 20% when exposed to temperatures in the range of ≧30° C., preferably ≧100° C., more preferably ≧125° C., even more preferably ≧130° C., particularly preferably ≧140° C., most preferably ≧150° C., and ≦320° C., preferably ≦300° C. This weight loss can be caused, for example, by decomposition of the printing ink or the adhesive. It is conceivable that decomposition products - for example H2O, CO, CO2, NOx - pass into the gas phase and thus lead to a weight loss of the sample. Preferably, the adhesive is a PU adhesive. Alternatively or additionally, EVA adhesives can also be used and are preferred depending on the application.

[0012] In a preferred embodiment, at least one of the films comprises at least one additive, which is preferably selected from the group consisting of catalysts, plasticizers, dyes, pigments, antiblocking agents, bactericides, disinfectants, light stabilizers, in particular UV absorbers and / or hindered amine light stabilizers (HALS), mold release agents, lubricants, flame retardants, antioxidants, heat stabilizers, crosslinking additives, light stabilizers, in particular UV absorbers and / or hindered amine light stabilizers (HALS), mold release agents, lubricants, flame retardants, antioxidants, heat stabilizers, crosslinking additives, emulsifiers, fillers and antistatic agents, and combinations thereof.

[0013] The values ​​given above for the weight loss due to exposure to temperature preferably refer to dried or (partially) cured samples of the respective substances and / or mixtures. For example, printing inks are often applied in liquid form to a substrate. For this purpose, colorants are dissolved in the liquid or are present as an emulsion or suspension in the liquid. Adhesives (also called adhesives for short) also often solidify and / or harden, which can cause a change in the viscosity of the adhesive. This change in viscosity can be related to outgassing of the substance and / or evaporation of the liquid. Similar reactions can also occur with other additives, which in a preferred embodiment can be included in the packaging material as mentioned above.

[0014] Preferably, the plastic of the plastic film comprises at least 70% by weight, preferably more than 90% by weight, particularly preferably more than 95% by weight, of a polymerization product of propylene or ethylene or butadiene or ethenylbenzene or propenoic acid esters or butane or hexane or octane. In particular, it is preferred that in each case only one of the above-mentioned monomers is used in the polymerization to form the plastic, so that the plastic is a reaction product of a single monomer and / or a single type of polymer. However, the monomers often contain small amounts of impurities, which are suitable for producing high-quality plastics. Such impurities are also acceptable within the scope of the present invention. The above weight percentages preferably refer only to the proportion of substances that are polymerizable under the selected polymerization conditions. Non-polymerizable substances such as catalysts, solvents present, (radical) initiators, quenchers and other additives that affect the polymerization are not taken into account when calculating the above weight percentages.

[0015] It has been found to be particularly disadvantageous if the decomposition of the printing ink and / or adhesive and / or additive leads to the generation of large amounts of gaseous decomposition products. These are responsible for the generation of (gas) bubbles in the plastic and in the recycled goods during recycling. These are often difficult to remove and can be harmful during further processing of the recycled goods. Therefore, packaging materials are preferred in which the printing ink and / or adhesive and / or additive do not form ≦15% by weight, preferably ≦10% by weight, more preferably ≦5% by weight, particularly preferably ≦3% by weight, most preferably no gaseous decomposition products when exposed to temperature. These figures, as well as all other percentage figures within the scope of the invention, refer to weight percentages based on the total weight of the sample of the printing ink and / or adhesive and / or additive (or mixtures thereof) before the application of temperature, unless otherwise stated.

[0016] Preference is given to packaging materials which exhibit such weight losses when the printing ink and / or adhesive and / or additives are exposed to temperatures in the range of ≧30° C. and ≦320° C., preferably in the range of ≧200° C. and ≦310° C., more preferably in the range of ≧250° C. and ≦300° C., particularly preferably in the range of ≧150° C. and ≦320° C. Additionally or alternatively, preference is given to packaging materials which have a weight loss of less than 15%, preferably ≦10%, more preferably ≦5%, more preferably ≦3%, when the printing ink and / or adhesive and / or additives are exposed to a temperature in one of the ranges mentioned above (possibly also having one of the lower limit temperatures defined above). An overview of exemplary weight losses of various printing inks when exposed to temperature can be found in Table 1 below.

[0017] [Table 1]

[0018] The weight losses of the respective printing inks due to the formation of decomposition products shown in Table 1 were determined by thermogravimetric analysis of the respective samples of the printing inks to be analyzed. The respective measurements were carried out over a temperature range that included at least the temperature range ≧30 ° C and ≦ 320 ° C, preferably ≧ 30 ° C and ≦ 260 ° C. The values ​​shown in Table 1 show excerpts from thermogravimetric analyses carried out in the temperature range from 30 to 900 ° C. However, only the volume losses of the printing inks or laminating adhesives occurring in the temperature ranges ≧ 30 ° C and ≦ 260 ° C are shown. The weight losses are determined by the mass difference of the samples at 30 ° C and 260 ° C. The course of the curves (temperature-dependent weight loss) determined during the thermogravimetric analysis of the various printing inks can provide information about the temperature range in which the decomposition of the printing ink leads to particularly strong weight losses. Even if for the printing inks and / or adhesives contained in the packaging material according to the invention there is a weight loss of ≦20 wt. % when exposed to temperatures in the ranges of ≧30° C. and ≦320° C., the range of ≧130 to ≦260° C. nevertheless forms the range for many of these printing inks and / or laminating adhesives over which a large (negative) gradient occurs in the thermogravimetric analysis. In particular, printing inks based on polyurethane, polyvinyl chloride, polyvinyl acetal, especially polyvinyl butyral or combinations thereof have been shown to meet this requirement.Packaging materials having printing inks with components selected from the group consisting of polyurethane, polyvinyl chloride, polyvinyl acetal, especially polyvinyl butyral are therefore preferred.

[0019] As can be seen from Table 1, not all printing inks meet the requirements of the present invention. For example, printing inks based on cellulose nitrate or containing large amounts of cellulose nitrate show amounts of decomposition products of more than 18%, and in some cases more than 28% and even close to 30%, which are clearly outside the acceptable range. Such printing inks are not suitable in the context of the present invention and can be understood as non-heat-resistant printing inks.

[0020] Preferably, the packaging material is a packaging film and / or a packaging container. Both flexible films and containers of predefined shapes are used for packaging purposes in a wide variety of designs. The combination of a film and a dimensionally stable container is also known, for example in the case of plastic salad cups sealed with a film of the same plastic.

[0021] The plastic can be part of a packaging composite, e.g. a paper-plastic composite, preferably a film composite. The individual (material) layers can preferably be separated (non-destructively) from one another so that each material / layer can be fed, preferably by type, to a respective recycling process.

[0022] In a preferred embodiment, the printing ink is a color, in particular an ink. The printing ink can be applied to the packaging material, for example, by gravure printing, flexographic printing, UV flexographic printing, offset printing or digital printing. Preferably, the applied print is covered with a protective layer.

[0023] Preferably, the plastic is selected from the group consisting of HDPE (high density polyethylene), LDPE (low density polyethylene), LLDPE (linear low density polyethylene), PE-HMW (high molecular weight polyethylene), PE-UHMW (ultra-high molecular weight HDPE), ethylene copolymers, preferably (each independently) ethylene-vinyl acetate copolymer (EVA), methacrylic acid ethyl ester (EMA), ethylene / acrylic acid copolymer (EAA), ethylene-butyl acrylate copolymer (EBA) or mixtures thereof, isotactic polypropylene (iPP), syndiotactic polypropylene (sPP) and atactic polypropylene (aPP), polypropylene foam (EPP), unoriented polypropylene film (CPP), (unidirectionally or bidirectionally) oriented polypropylene film (OPP and BOPP) or mixtures thereof, combinations of polypropylenes with ethylene as a comonomer, preferably polypropylene copolymers, polypropylene random copolymers with ethylene as a comonomer, preferably polypropylene-ethylene block copolymers.

[0024] Furthermore, the present invention relates to a recycled plastic product comprising the above-mentioned packaging material, which preferably comprises a weight percentage of the above-mentioned packaging material of ≧25%, preferably ≧70%, more preferably ≧75%, particularly preferably ≧90%.

[0025] As mentioned above with respect to packaging materials, this is particularly easy to recycle. Mixtures with other plastic materials (preferably based on the same type of monomers and / or polymers) have also been shown to be higher quality recyclates compared to known recyclates. This can in particular be explained by the fact that fewer decomposition products are produced during the thermal treatment of the (preferably separated, particularly preferably unmixed) plastic waste to form plastic or recycled granules. A lower proportion of decomposition products, in particular gaseous decomposition products, means that fewer low molecular weight impurities are formed in the recyclate and fewer gaseous inclusions are formed in the pellets in particular. These impurities subject the material to high mechanical stresses, especially at the high pressures and pressure differences that occur during the extrusion of plastics, which can adversely affect the chemical and physical properties of the polymer.

[0026] In particular, it is preferred that the recycled plastic is in the form of granules, which have proven to be particularly suitable in the plastics processing industry as they are easy to handle and in particular easy to extrude.

[0027] Preferably, the granules have an average particle size (d 50 Granules of this average particle size are particularly easy to handle, do not tend to form dust and can be easily and homogeneously shaped in an extruder.

[0028] Such plastic recycles can be particularly advantageously obtained by a process comprising the following steps: a) providing plastic waste consisting of packaging material as described above, preferably in a proportion of ≧25% by weight, more preferably ≧70% by weight, even more preferably ≧75% by weight, particularly preferably ≧90% by weight; b) washing the plastic waste; c) optionally sorting and / or crushing and / or mixing the plastic waste: d) feeding the plastic waste into an extruder to produce an extrudate from the plastic waste; and e) chopping the extrudate into granules.

[0029] This process makes it particularly easy to recycle such packaging materials: the resulting granules have a high degree of purity and their physical and / or chemical properties closely correspond to those of the plastics obtained from the primary raw materials.

[0030] It has been found that even relatively small amounts of the abovementioned packaging materials are sufficient to favorably affect the properties of the recycled product. However, a high proportion of such packaging materials is preferred, since it allows a reduction in the amount of decomposition products generated during the thermal treatment of the plastics mixture. In particular, it allows a favorable reduction in the amount of gases evolved during the thermal treatment.

[0031] Gas generation is particularly detrimental during the extrusion of plastics into plastic strands, which are then further processed into pellets. Typically, crushed plastic waste is fed into an extruder and conveyed towards a die at elevated temperature and pressure. At these temperatures and pressures, the plastic particles soften and become flowable. However, decomposition products resulting from this process can have a negative effect on the flowability. For example, they have a different softening point than the plastic and therefore can exist as a solid in the melt, which can have a negative effect on the viscosity. Another problem with gaseous decomposition products is that their behavior also depends on the current pressure. Since the pressure conditions change many times during the extrusion of plastics, there is a risk of gas bubbles forming in the melt. The gas bubbles also have a negative effect on the viscosity of the melt. Furthermore, the gas trapped in these bubbles has the disadvantage that if the pressure conditions change suddenly after leaving the extruder through the die, the gas can suddenly escape from the extruded strand, which results in cracks in the extrudate. The formation of a homogeneous extrudate or pellets with a defined particle size is therefore not possible.

[0032] In step b) the plastic waste is washed to avoid contamination that would lead to the drawbacks mentioned above. The timing of this step does not have a significant impact on the process, so the order of the steps can basically be chosen freely, for example to suit local conditions. However, it is essential that the washing takes place before feeding into the extruder.

[0033] Step c) can also be carried out depending on the prevailing conditions. However, steps such as sorting, crushing and / or mixing of the plastic waste may not be necessary. For example, if a pure mixture of plastic waste is already available, further sorting can be omitted. The size of the packaging waste available for further processing may also depend on the respective conditions. If the extruder is suitable for processing large packaging waste, further crushing may not be necessary. Mixing different plastic wastes may also be advantageous or not depending on the available plastic waste and / or the requirements of the pellets to be produced. Preferably, only packaging wastes obtained from a single type of monomer and / or polymer are mixed, whereby minor impurities may be tolerated, as mentioned above.

[0034] The present invention is further directed to a method for predicting the recyclability of a plastic material containing printing inks and / or adhesives and / or additives, said method being characterized by the following steps: Providing samples of the ink and / or adhesive and / or additive; performing a thermogravimetric analysis of the sample, the thermogravimetric analysis comprising at least one measurement of mass change in the temperature range ≧30° C. to ≦320° C.; determining a critical temperature value in this temperature range; Determining the mass loss of the sample at the critical temperature; Classifying the recyclability of the ink and / or adhesive and / or additive based on the mass loss of the sample at a critical temperature.

[0035] It has been shown that this method can be used to make good predictions regarding the recyclability of plastics with the material being subjected to thermogravimetric analysis.

[0036] Preferably, the recyclability is classified based on the weight loss of the sample, whereby for good recyclability a limit value of weight loss of less than 20%, preferably ≦15%, preferably ≦10%, more preferably ≦5%, particularly preferably ≦3% is set.

[0037] Preferably, the printing ink and / or adhesive and / or additives are dried and / or cured before the thermogravimetric analysis is carried out.

[0038] In the case of printing inks, it is particularly preferred that the drying is carried out at a temperature of ≧20° C. and ≦100° C., preferably ≧30° C. and ≦50° C., particularly preferably 40° C.±3° C. Additionally or alternatively, it is preferred that the drying is carried out over a period of ≧2 days and ≦14 days, preferably ≧3 days and ≦10 days, more preferably ≧4 days and ≦7 days, particularly preferably 5 days±12 hours.

[0039] For drying or curing the adhesive, a temperature range of ≧50° C. and ≦150° C., preferably 80° C.-120° C., particularly preferably ≧90° C.-110° C., has proven suitable. Additionally or alternatively, the drying and / or curing period is preferably about 5 days (possibly ±24 hours). Typically, after this period, the isocyanate and / or solvent content is ≦5% by weight. However, preferably, at least one of these two values ​​is checked. If one or both of these values ​​exceeds a predefined limit value, which is preferably set to ≦5% by weight, the drying and / or curing period at the abovementioned temperature is preferably extended. The additional drying and / or curing period is preferably ≧1 day and ≦5 days, preferably ≧2 days and ≦4 days, particularly preferably 3 days ±12 hours. The solvent content is preferably tested by headspace GC and, separately from this, the isocyanate content is preferably tested by ATR-FTIR analysis.

[0040] Drying and / or curing is preferably carried out on a solid support. In particular, it is preferred that the solid support has high thermal conductivity. In particular, it is preferred that the support is made of metal or is made of metal. In particular, aluminum supports have been shown to be advantageous, since such supports are also resistant to corrosion by various materials.

[0041] Preferably, less than 500 mg of sample is used in thermogravimetric analysis. Small sample amounts have proven to be advantageous, since they react particularly quickly to temperature changes and allow the applied temperature to be uniformed quickly throughout the sample. Preferably, a sample amount of ≦200 mg, preferably ≦100 mg, more preferably ≦50 mg, even more preferably ≦20 mg, particularly preferably 10 mg, and possibly ±5 mg is used in thermogravimetric analysis.

[0042] Due to the drying and / or hardening of the sample, the printing inks and / or adhesives and / or additives are present in a relatively short time in the form in which they will be present in the packaging material when it is sent for recycling, so the prediction of recyclability is particularly reliable.

[0043] In a preferred variant, it is envisaged that the thermogravimetric analysis in the method is carried out with a temperature rise of ≧10° C. / min and ≦100° C. / min, preferably ≧20° C. / min and ≦50° C. / min, more preferably ≧25° C. / min and ≦40° C. / min, particularly preferably 30° C. / min ±3° C. / min. This temperature rise has been shown to provide a manageable decomposition time for commonly used substances, and allows sufficient time for the samples to homogeneously reach the decomposition temperature of the respective substances. In this way, the reproducibility of the results can be increased.

[0044] In a preferred variant, the thermogravimetric analysis is followed by the analysis of the decomposition products obtained. In particular, it is preferred to analyze the decomposition products by gas chromatography. Preferably, the gas chromatography analysis is carried out at a trigger temperature of 260°C. Preferably, the trigger temperature is adapted to the melting temperature of the plastic during regranulation (e.g., the melting temperature of PE).

Claims

1. A recyclable packaging material comprising plastic, A carrier material consisting of at least two plastic films laminated with an adhesive, the films comprising at least 70% by weight of a single type of monomer and / or polymer; an optically perceptible element formed by printing inks; A packaging material, wherein the printing ink and / or adhesive is thermally stable and exhibits less than 20% weight loss when exposed to temperatures in the range of ≧30° C. and ≦320° C.

2. 2. Packaging material (1) according to claim 1, wherein the plastic of the plastic film comprises at least 70% by weight, preferably more than 90% by weight, particularly preferably more than 95% by weight, of a polymerization product of propylene or ethylene or butadiene or butane or hexane or octane or ethenylbenzene or a propanoic acid ester.

3. 3. The packaging material (1) according to claim 1 or 2, which does not form ≦15% by weight, preferably ≦10% by weight, more preferably ≦5% by weight, particularly preferably ≦3% by weight, and most preferably does not form gaseous decomposition products when exposed to temperature.

4. Packaging material (1) according to any one of claims 1 to 3, containing a printing ink comprising a component selected from the group consisting of polyurethane, polyvinyl chloride, polyvinyl acetal, in particular polyvinyl butyral, or combinations thereof.

5. 5. Packaging material (1) according to any one of claims 1 to 4, wherein the plastic is an ethylene-based copolymer selected from the group consisting of HDPE (high density polyethylene), LDPE (low density polyethylene), LLDPE (linear low density polyethylene), PE-HMW (high molecular weight polyethylene), PE-UHMW (ultra-high molecular weight HDPE), preferably (each independently of the other) ethylene-vinyl acetate copolymer (EVA), methacrylic acid ethyl ester (EMA), ethylene / acrylic acid copolymer (EAA) and ethylene-butyl acrylate copolymer (EBA), or mixtures thereof, isotactic polypropylene (iPP), syndiotactic polypropylene (sPP) and atactic polypropylene (aPP), polypropylene foam (EPP), unoriented polypropylene film (CPP), (unidirectionally or bidirectionally) oriented polypropylene film (OPP and BOPP) or mixtures thereof, combinations of polypropylene with ethylene as comonomer, preferably polypropylene copolymers, preferably polypropylene random copolymers with ethylene as comonomer, preferably polypropylene-ethylene block copolymers.

6. 6. A plastic recycled product comprising a weight percentage of the packaging material according to any one of claims 1 to 5, preferably ≧25%, preferably ≧70%, more preferably ≧75%, particularly preferably ≧90%.

7. The granules preferably have an average particle size (d 50 7. The plastic recycled product according to claim 6, having a sieve analysis.

8. A method for producing recycled plastic according to claim 6 or 7, comprising the following steps: a) providing plastic waste consisting of packaging material according to any one of claims 1 to 5, preferably in a weight proportion of at least 25%, more preferably at least 70%, even more preferably at least 75%, particularly preferably at least 90%; b) washing the plastic waste; c) if necessary, crushing and / or blending the plastic waste; d) feeding the plastic waste into an extruder to produce an extrusion product from the plastic waste; e) grinding the extrudate into granules

9. The method according to claim 8, wherein step b) is carried out before step d), and preferably steps a) to e) are carried out in the above order.

10. 1. A method for predicting the recyclability of plastic-containing packaging materials, including printing inks and / or adhesives, comprising the steps of: - providing a sample of the printing ink and / or adhesive; performing a thermogravimetric analysis of the sample, the thermogravimetric analysis comprising at least one measurement of mass change in the temperature range ≧30° C. to ≦320° C.; - specifying a critical temperature for this temperature range; - determining the mass loss of the sample at the critical temperature; Classifying the recyclability of the inks and / or adhesives based on the mass loss of the sample at a critical temperature.

11. 11. The method according to claim 10, characterized in that the printing ink is dried before the thermogravimetric analysis is carried out, the drying being preferably carried out at a temperature of ≧20° C. and ≦100° C., preferably ≧30° C. and ≦50° C., particularly preferably 40° C.±3° C., and / or the drying is carried out over a period of ≧2 days and ≦14 days, preferably ≧3 days and ≦10 days, further preferably ≧4 days and ≦7 days, particularly preferably 5 days±12 hours.

12. characterised in that the adhesive is dried and / or cured before the thermogravimetric analysis is carried out, the drying and / or curing being preferably carried out at a temperature between 50°C and 150°C, preferably between 80°C and 120°C, more preferably between 90°C and 110°C, and / or for a period of 5 days ±24 hours, 12. The method according to claim 10 or 11, wherein if the isocyanate and / or solvent content, preferably measured after this period, exceeds a specified limit value, preferably set at ≦5 wt.-%, the drying and / or curing period at said temperature is extended by an additional drying and / or curing period, preferably being ≧1 day≦5 days, preferably ≧2 days≦4 days, more preferably 3 days±12 hours.

13. 13. The method according to any one of claims 10 to 12, wherein the thermogravimetric analysis is carried out with a temperature increase of ≧10° C. / min and ≦100° C. / min, preferably ≧20° C. / min and ≦50° C. / min, more preferably ≧25° C. / min and ≦40° C. / min, particularly preferably 30° C. / min ±3° C. / min.

14. 14. The method according to any one of claims 10 to 13, characterized in that less than 500 mg of sample are used for the thermogravimetric analysis, preferably with a sample amount ≦200 mg, preferably ≦100 mg, more preferably ≦50 mg, even more preferably ≦20 mg, particularly preferably 10 mg, optionally ±5 mg.

15. 15. The method according to claim 10, characterized in that the thermogravimetric analysis is followed by an analysis of the formed decomposition products, which are preferably analyzed by gas chromatography, the gas chromatography analysis being preferably carried out at a trigger temperature which corresponds to the melting temperature of the plastic during regranulation.