Shrinkable label film with excellent transparency and printability
A shrinkable label film with a specific gravity of less than 1, using cyclic olefin resin and polyolefin materials, addresses recycling challenges and enhances transparency and printability while maintaining seaming characteristics.
Patent Information
- Application Number
- JP2024529396
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2021-11-24
- Filing Date
- 2022-10-04
- Publication Date
- 2024-11-21
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Conventional shrink label films made from materials like polystyrene and polyvinyl chloride have high specific gravity, making them difficult to recycle, and exhibit low tensile strength and high haze, which affects printability and clarity.
A shrinkable label film composed of a skin layer, core layer, and sealing layer, using cyclic olefin resin, propylene terpolymer, petroleum resin, and polyolefin elastomer, with specific compositions to achieve a specific gravity of less than 1, improved transparency, and enhanced printability and seaming properties.
The film achieves a shrinkage rate of 40% or more, stiffness of 4.5 gf/50 μm or more, haze of less than 8%, and tensile strength of 250 to 500 kgf/cm², ensuring effective recycling and improved aesthetic quality.
Smart Images

Figure 2024543524000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a shrink label film, and more particularly to a shrink label film having excellent transparency and printability.
[0002] This application claims priority to and the benefit of Korean Patent Application No. 10-2021-0163638, filed on November 24, 2021, the entire text of which is incorporated herein by reference. [Background technology]
[0003] Generally, labels with a printed layer are attached to various plastic containers such as PET bottles. These labels are classified into adhesive labels and non-adhesive labels, which are categorized according to whether or not an adhesive is used between the container and the label.
[0004] Adhesive labels are usually made using polypropylene materials, while non-adhesive labels are mainly made using polystyrene, polyester, polyvinyl chloride, etc. Containers made of polyethylene terephthalate (PET), polystyrene (PS), etc. with labels attached are crushed and pelletized after use, and then recycled as containers through a recycling process. In this case, the pelletized containers are put into water and sorted according to their specific gravity.
[0005] Meanwhile, the Ministry of Environment has implemented grading standards for the ease of recycling of packaging materials (Ministry of Environment Notification No. 2019-255, effective December 30, 2019), which classifies non-adhesive labels with a specific gravity of less than 1 as having the highest recyclability grade, calling for the development of non-adhesive labels with a specific gravity of less than 1.
[0006] In terms of the physical properties of non-adhesive labels, conventional materials such as PS, PET, and polyvinyl chloride (PVC) have a high specific gravity, so it is possible to consider using polyolefin materials with a specific gravity of less than 1. However, it is difficult to give polyolefin material films shrinkability and seaming properties, so cyclic olefin copolymer (COC) is added to form the film.
[0007] Meanwhile, in the case of labels, gravure printing is performed on the produced film, and if the tensile strength of the film in the machine direction (MD) is low, the tension applied to the roll is low, which reduces productivity during printing. Also, if the film has high haze during printing, the clarity and aesthetic quality of the printed product will be reduced.
[0008] Japanese Patent Publication No. 6268136 discloses a heat-shrinkable multilayer film composed of front and back layers containing a cyclic olefin resin and an ethylene resin, and an intermediate layer containing an olefin resin and a plastic resin. However, the film has high haze and low tensile strength in the machine direction (MD), making it difficult to adjust the tension during printing. Summary of the Invention [Problem to be solved by the invention]
[0009] The present invention provides a shrink label film using a polyolefin-based material, which has improved transparency and printability while maintaining improved seaming properties, rigidity, and shrinkability as a non-adhesive label with a specific gravity of less than 1. [Means for solving the problem]
[0010] In order to solve the above problems, the present invention provides a shrink label film comprising a skin layer, a core layer, and a seal layer, wherein the skin layer and the seal layer comprise a cyclic olefin resin, and the core layer comprises 40 to 90 parts by weight of a terpolymer of propylene and two olefins selected from ethylene and α-olefin, 5 to 30 parts by weight of a petroleum resin having a softening point of 120 to 140°C, and 5 to 30 parts by weight of a polyolefin elastomer.
[0011] The present invention also provides a shrink label film, characterized in that the cyclic olefin resin has a glass transition temperature (Tg) of 60 to 75°C.
[0012] The terpolymer has a melting point (Tm) of 123 to 138°C and a melt index (230°C, 2.16 kg load) of 2 to 10 g / 10 min, and the two olefins are ethylene and 1-butene.
[0013] The present invention also provides a shrink label film, wherein the ethylene and 1-butene are each contained in the terpolymer in an amount of 1 to 5% by weight.
[0014] The polyolefin elastomer has a density of 0.85 to 0.9 g / cm 3 and a propylene-ethylene rubber (PER) or propylene-butene rubber (PBR) having a melt index (230° C., 2.16 kg load) of 0.5 to 10 g / 10 min.
[0015] The present invention also provides a film for shrink labels, wherein the core layer further comprises 0.1 to 20 parts by weight of a propylene homopolymer.
[0016] The propylene homopolymer has a melt index (230° C., 2.16 kg load) of 1 to 10 g / 10 min.
[0017] The film has a density of 1 g / cm 3 The present invention provides a shrink label film having a shrinkage ratio of 40% or more and a stiffness of 4.5 gf / 50 μm or more when measured by the following method. [Method of measuring shrinkage rate] The film stretched in the transverse direction (TD) was cut into pieces of 50 mm x 50 mm size, and immersed in a 100°C hot water bath for 10 seconds each, after which the dimensions were measured and the transverse direction (TD) shrinkage rate was calculated according to the following formula (1) and shown as the average shrinkage rate.
number
[0018] The film has a haze (ASTM D1003, thickness 50 μm) of less than 8% and a tensile strength in the machine direction (MD) of 250 to 500 kgf / cm as measured by the following method. 2 The present invention provides a shrink label film having a transverse direction (TD) elongation rate of 30% or more. [Measurement method] The tensile strength in the machine direction (MD) of the produced paper pieces (ASTM D638 Type IV standard) is measured at 50 mm / min using a universal testing machine in accordance with ASTM D638, and the elongation in the transverse direction (TD) until the film breaks is measured under the same conditions as the tensile strength measurement. Effect of the Invention
[0019] According to the present invention, in a shrink label film comprising a skin layer, a core layer, and a seal layer, conventional linear low density polyethylene is not used for the skin layer and the seal layer, and the core layer is composed of a propylene terpolymer, a petroleum resin, and a polyolefin elastomer, and further contains a polypropylene homopolymer, thereby providing a shrink label film having improved transparency and printability while maintaining improved seaming properties, rigidity, and shrinkability as a non-adhesive label with a specific gravity of less than 1. [Brief description of the drawings]
[0020] [Figure 1] FIG. 2 is a schematic diagram illustrating a labeling process (shooting and shrinking) using a shrink label film and a sleeve manufacturing process. [Diagram 2] FIG. 2 is a diagram illustrating a site for checking whether a film is adhered or not in a test example of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0021] The present invention will be described in detail below through preferred embodiments. Prior to this, the terms and words used in this specification and claims should not be interpreted in their ordinary or dictionary sense, but should be interpreted in their meaning and concept consistent with the technical idea of the present invention, based on the principle that the inventor can appropriately define the concept of the term to best describe his / her invention. Therefore, the configuration of the embodiment described in this specification is merely one of the most preferred embodiments of the present invention, and does not fully represent the technical idea of the present invention, so it should be understood that there may be various equivalents and modifications that can replace them at the time of this application.
[0022] The present invention discloses a shrink label film comprising a skin layer, a core layer, and a seal layer, wherein the skin layer and the seal layer comprise a cyclic olefin resin, and the core layer comprises 40 to 90 parts by weight of a terpolymer of propylene and two kinds of olefins selected from ethylene and an α-olefin, 5 to 30 parts by weight of a petroleum resin having a softening point of 120 to 140°C, and 5 to 30 parts by weight of a polyolefin elastomer.
[0023] The present invention provides a shrink label film that has improved transparency and printability while maintaining improved seaming properties, stiffness, and shrinkability as a non-adhesive label with a specific gravity of less than 1.
[0024] Fig. 1 is a schematic diagram for explaining the labeling process (shooting and shrinking) using a shrink label film and the sleeve manufacturing process. As shown in Fig. 1, the seaming property is a necessary physical property for bonding between films when manufacturing a sleeve, the stiffness is a certain value (about 4.5gf) or more of the film (loop stiffness) required for the process of inserting the label into the bottle (shooting process) to be performed smoothly, the transparency affects the appearance of the film when printing on the film, and the shrinkage (TD direction) is a physical property required for the film to adhere to the bottle container when passing through a heat shrink tunnel after label shooting.
[0025] In the present invention, the cyclic olefin resin used in each of the skin layer and the seal layer is a component used to basically impart shrinkage and seaming properties to a polypropylene material, and may have a glass transition temperature (Tg) of 60 to 75° C., preferably 62 to 68° C. If the glass transition temperature is less than 60° C., low-temperature shrinkage occurs, and the dimensional stability of the shrink label film may decrease when the atmospheric temperature rises in summer, while if it exceeds 75° C., the heat shrinkability of the film may decrease because the stretching temperature in the stretching process in the stretching process in the manufacturing process of the shrink label film must be high in the stretching direction.
[0026] The cyclic olefin resin contains a cyclic olefin component as a copolymer component, and is not particularly limited as long as it is a polyolefin containing a cyclic olefin component in the main chain, but for example, the cyclic olefin resin may be a polymer of a cyclic olefin or a hydrogenated product thereof, a copolymer of a cyclic olefin and an α-olefin or a hydrogenated product thereof, etc. Also, it may be a polymer obtained by grafting and / or copolymerizing an unsaturated compound having a hydrophilic group onto these polymers. These cyclic olefin resins may be used alone or in combination of two or more kinds.
[0027] Conventionally, linear low density polyethylene was mixed into the skin layer and seal layer to lower the specific gravity of the film, but in order to prevent a decrease in transparency due to linear low density polyethylene, the present invention excludes linear low density polyethylene from the skin layer and seal layer and changes the composition of the core layer to satisfy the specific gravity of the film being less than 1. In other words, conventional shrink label films showed a haze of 10% or more when they contained linear low density polyethylene in the skin layer and seal layer, but by eliminating it, transparency can be improved to a haze level of 4.5% or less.
[0028] In the present invention, it has been confirmed that the core layer is most suitable for containing a terpolymer of propylene and two olefins selected from ethylene and α-olefin, a petroleum resin, and a polyolefin elastomer, in order to reduce the specific gravity of the film without compromising the improved physical properties achieved by using the cyclic olefin resin in the skin layer and the seal layer, and to maintain the excellent rigidity, shrinkability, and seaming properties of the film.
[0029] The terpolymer may be preferably an ethylene-propylene-α-olefin terpolymer, and the α-olefin may have 4 to 10 carbon atoms, such as 1-butene, 1-pentene, 1-hexene, 4-methyl 1-pentene, 1-heptene, 1-octene, 1-nonene, 1-decene, etc., and preferably 1-butene. In the case of the ethylene-propylene-α-olefin terpolymer, the contents of ethylene and α-olefin may each be 1 to 5 wt %.
[0030] The terpolymer preferably has a melting point (Tm) of 123 to 138°C and a melt index (230°C, 2.16 kg load) of 2 to 10 g / 10 min, more preferably a melting point (Tm) of 126 to 135°C and a melt index (230°C, 2.16 kg load) of 4 to 8 g / 10 min.
[0031] In the present invention, the petroleum resin constituting the core layer is a modifier mixed to improve the transparency of the film and to increase its rigidity. The petroleum resin is a pale yellow or dark brown thermoplastic resin with a molecular weight of 2,000 g / mol or less, obtained by polymerizing higher unsaturated hydrocarbons found in high-temperature pyrolysis oil such as naphtha as a raw material with an acid catalyst. In the present invention, a petroleum resin with a softening point of 120 to 140°C, preferably 120 to 130°C, can be used from the viewpoint of improving rigidity.
[0032] In the case of aromatic petroleum resin, the main component may be a copolymer of styrene vinyl toluene, α-methyl styrene, and indene, and in the case of aliphatic petroleum resin, the main component may be a copolymer of isoprene, piperylene-2-methylbutene-1, etc., which is a resin produced from C5 oil produced in the olefin process of the naphtha cracking process. In addition, aliphatic petroleum resin may include petroleum resin produced from dicyclopentadiene. In addition, hydrogenated petroleum resin is a resin formed by adding hydrogen to the aromatic petroleum resin and the aliphatic petroleum resin, and may include petroleum resin produced from dicyclopentadiene and added with hydrogen.
[0033] In the present invention, the core layer contains polyolefin elastomer (POE) to improve dispersion and fluidity by increasing the compatibility between the components, and to increase the elongation in the transverse direction (TD), in particular. In other words, if the elongation in the transverse direction (TD) of a shrink film is low, the label may tear when applied to a label for a product such as a carbonated drink, but in the present invention, by mixing polyolefin elastomer into the core layer, the elongation in the transverse direction (TD) can be improved to a level of 50% or more compared to the conventional method.
[0034] In consideration of this purpose, the polyolefin elastomer has a density of 0.85 to 0.9 g / cm 3 , and the melt index (230°C, 2.16 kg load) may be 0.5 to 10 g / 10 min, but preferably the density is 0.86 to 0.89 g / cm 3 , and the melt index (230° C., 2.16 kg load) may be 2 to 8 g / 10 min.
[0035] The polyolefin elastomer may be a copolymer of propylene and ethylene or an olefin selected from α-olefins, preferably an ethylene-propylene rubber in which propylene and 5 to 20% by weight of ethylene are copolymerized, or an ethylene-butene rubber in which propylene and 10 to 30% by weight of butene are copolymerized, and more preferably an ethylene-propylene rubber in which propylene and 10 to 20% by weight of ethylene are copolymerized.
[0036] In the present invention, the core layer further contains propylene homopolymer to improve the tensile strength in the machine direction (MD). In other words, when printing a film for shrink labels, if the tensile strength in the machine direction (MD) is low, it is difficult to adjust the roll tension, which reduces the printing speed. However, by mixing 0.1 to 20 parts by weight, preferably 1 to 10 parts by weight, of propylene homopolymer into the composition of the core layer, the tensile strength in the machine direction (MD) of the film is improved, which increases the printing speed.
[0037] In addition, in consideration of the purpose of improving the tensile strength in the machine direction (MD), the propylene homopolymer may have a melt index (230°C, 2.16 kg load) of 1 to 10 g / 10 min, preferably 2 to 5 g / 10 min.
[0038] In the present invention, the combination of the above components in each layer has a certain range of component content ratio, which allows the film for shrink labels to maintain improved seaming properties, rigidity, and shrinkability while improving transparency and printability. To this end, the core layer contains 40 to 90 parts by weight of the terpolymer, 5 to 30 parts by weight of the petroleum resin, and 5 to 30 parts by weight of the polyolefin elastomer. Preferably, the core layer contains 50 to 80 parts by weight of the terpolymer, 5 to 25 parts by weight of the petroleum resin, and 10 to 25 parts by weight of the polyolefin elastomer.
[0039] If the content of the terpolymer in the core layer is less than 40 parts by weight, the transparency during stretching decreases, and if it exceeds 90 parts by weight, the shrinkage of the film decreases. If the content of the petroleum resin exceeds 30 parts by weight, the shrinkage of the film decreases. If the content of the polyolefin elastomer is less than 10 parts by weight, the shrinkage and elongation of the film decrease, and if it exceeds 30 parts by weight, the stiffness, transparency, and tensile strength of the film decrease.
[0040] Meanwhile, in the present invention, uneven flow may occur due to the difference in viscosity between the cyclic olefin resin and the polyolefin, but in order to solve such a problem, the skin layer, the core layer, and the seal layer may each be made of a melt blended composition, and the respective compositions may be laminated to produce a film. As a result, the melt blending before film stretching due to the difference in fluidity of the raw materials of each layer can improve dispersibility and allow a smooth stretching process to be performed after film formation.
[0041] The resin composition of each layer constituting the shrink label film according to the present invention may further contain one or more additives, such as antioxidants, catalyst neutralizers, pigments, dispersants, weatherproofing agents, antistatic agents, UV stabilizers, talc, etc., if necessary, so long as the object of the present invention is not impaired. The amount of such additives used may be adjusted taking into consideration the total production amount and production process, within the ranges known to be usable for producing the shrink label film according to the present invention without affecting its properties.
[0042] In the present invention, the film using the above components can be manufactured by a conventional method known in the art. For example, the components constituting each layer are mixed in a mixer in the required amount, and then pelletized at 180 to 240°C using an extruder, and melt-molded into a film using a multi-layer film molding machine to manufacture a shrink label film.
[0043] In this case, a multi-layer film molding machine is used to form a sheet having a thickness of 175 to 200 μm by configuring the thickness ratio of the skin layer:core layer:seal layer to, for example, 1:5 to 10:0.5 to 1.5, and then stretched at a stretch ratio of 3.5 to 5 times under conditions of a stretching section of 80 to 85° C., a preheating section of 95 to 100° C., and a heat setting section of 75 to 80° C. to produce a film having a final thickness of about 50 μm.
[0044] The shrink label film according to the present invention can provide a shrink label film having improved transparency and printability while maintaining improved seaming properties, rigidity, and shrinkability as a non-adhesive label having a specific gravity of less than 1. More specifically, the shrink label film according to the present invention has a density of 1 g / cm 3 The shrinkage rate measured by the method described below may be 40% or more, preferably 45% or more, the stiffness may be 4.5 gf / 50 μm or more, preferably 5 gf / 50 μm or more, the haze (ASTM D1003, thickness 50 μm) may be less than 8%, preferably 4.5 or less, and the tensile strength in the machine direction (MD) measured by the method described below may be 250 to 500 kgf / cm 2 , preferably 260 to 400 kgf / cm2 The transverse direction (TD) elongation may be 30% or more, preferably 35% or more. [Method of measuring shrinkage rate] The film stretched in the transverse direction (TD) was cut into pieces of 50 mm x 50 mm size, and immersed in a 100°C hot water bath for 10 seconds each, after which the dimensions were measured and the transverse direction (TD) shrinkage rate was calculated according to the following formula (1) and shown as the average shrinkage rate.
number
[0045] The present invention will be described in more detail with reference to the following specific examples and comparative examples. The specifications of the components used in the examples and comparative examples are summarized in Table 1 below, and the methods for measuring physical properties are as follows. [Measurement method] - Density: Measured by the density gradient tube method of ASTM D1505. Melt index: Measured according to ASTM D1238 at 190°C or 230°C under a load of 2.16 kg. - Melting point (Tm): Measured according to the standard of ASTM D3418. Using a differential scanning calorimeter (DSC, manufactured by TA Instruments), 10 mg of a specimen was pre-melted at 220°C for 5 minutes under nitrogen gas atmosphere, and then the temperature was lowered to 40°C at a rate of 10°C / min. Then, the temperature was increased at a rate of 10°C / min, and the peak temperature of the maximum peak of the obtained melting endothermic curve was defined as the melting point (Tm). - Glass transition temperature (Tg): Measured according to the standard of ASTM D3418. Using a differential scanning calorimeter (DSC, manufactured by TA Instruments), 10 mg of a specimen was pre-melted at 220°C for 5 minutes under nitrogen gas atmosphere, and then the temperature was lowered to -80°C at a rate of 10°C / min. Then, the temperature was increased at a rate of 10°C / min, and the midpoint between the heights of the start and end points of the glass transition was calculated and defined as the glass transition temperature (Tg). -Softening point (VICAT): Measured according to the ASTM D1525 standard (ASTM E28 standard for petroleum resins). In the penetration test, a load of 1 kg or 5 kg was applied to a 3 mm thick specimen, and the temperature was raised uniformly at a rate of 50°C / hr. 2 The softening point was defined as the temperature at which a standard needle penetrated 1 mm into the paper piece. [Table 1]
[0046] <Examples and Comparative Examples> The molten mixture (using a twin screw extruder) was prepared for each layer with the composition shown in Table 2 below, and then the mixture for each layer was molded into a sheet having a thickness of 175 to 200 μm using a multi-layer film molding machine with a skin layer, core layer, and seal layer thickness ratio of 1:8:1 or 1.5:7.1:5. After molding, the sheet was stretched at a stretching ratio of 3.8 to 4.8 times under conditions of a stretching section of 80 to 85° C., a preheating section of 98° C., and a heat setting section of 78° C. to produce a film with a final thickness of 50 μm.
[0047] <Test Example> The physical properties of the prepared film were measured by the following methods, and the results are shown in Table 2 below. [Method of measuring physical properties] -Shrinkage rate: The film stretched in the transverse direction (TD) was cut into pieces of 50 mm x 50 mm size, and immersed in a hot water bath at 100°C for 10 seconds each, after which the dimensions were measured, and the transverse direction (TD) shrinkage rate was calculated according to the following formula (1) and shown as the average shrinkage rate.
number
[0048] Referring to Table 2, when a cyclic olefin resin is applied to the skin layer and the seal layer according to the present invention and the core layer is composed of a propylene terpolymer, a petroleum resin, and a polyolefin elastomer, the transparency and tensile strength are improved while maintaining generally good shrinkage properties, seaming properties, and rigidity. However, when PER is used as the polyolefin elastomer in the core layer (Examples 5 to 9) or when propylene homopolymer is further mixed (Examples 2 to 6, 8, and 9), it can be seen that these effects are significantly improved.
[0049] In contrast, when linear low density polyethylene was mixed into the skin layer and the seal layer (Comparative Examples 1 and 2), the transparency was significantly reduced and the elongation rate was also somewhat reduced.
[0050] The preferred embodiments of the present invention have been described in detail above. The description of the present invention is for illustrative purposes only, and those skilled in the art will understand that the present invention can be easily modified into other specific forms without changing the technical concept or essential features of the present invention.
[0051] Therefore, the scope of the present invention is defined by the claims set forth below rather than the above detailed description, and all modifications and variations that fall within the meaning, scope and equivalent concept of the claims should be interpreted as being included within the scope of the present invention.
Claims
1. A shrink label film comprising a skin layer, a core layer, and a seal layer, The skin layer and the seal layer contain a cyclic olefin resin, The core layer is a shrink label film comprising 40 to 90 parts by weight of a terpolymer of propylene and two olefins selected from ethylene and α-olefin, 5 to 30 parts by weight of a petroleum resin having a softening point of 120 to 140°C, and 5 to 30 parts by weight of a polyolefin elastomer.
2. 2. The shrink label film according to claim 1, wherein the cyclic olefin resin has a glass transition temperature (Tg) of 60 to 75[deg.] C.
3. 10. The shrink label film of claim 1, wherein the skin and seal layers are free of linear low density polyethylene.
4. The shrink label film according to claim 1, wherein the terpolymer has a melting point (Tm) of 123 to 138°C and a melt index (230°C, 2.16 kg load) of 2 to 10 g / 10 min, and the two olefins are ethylene and 1-butene.
5. 2. The shrink label film of claim 1, wherein the ethylene and 1-butene are each contained in the terpolymer in an amount of 1 to 5% by weight.
6. The polyolefin elastomer has a density of 0.85 to 0.9 g / cm 3 2. The shrink label film according to claim 1, which is made of propylene-ethylene rubber (PER) or propylene-butene rubber (PBR) having a melt index (230° C., 2.16 kg load) of 0.5 to 10 g / 10 min.
7. 2. The shrink label film of claim 1, wherein the core layer further comprises 0.1 to 20 parts by weight of a propylene homopolymer.
8. 8. The shrink label film according to claim 7, wherein the propylene homopolymer has a melt index (230[deg.] C., 2.16 kg load) of 1 to 10 g / 10 min.
9. The film has a density of 1 g / cm 3 The shrink label film according to claim 1, characterized in that the shrinkage rate measured by the following method is 40% or more and the stiffness is 4.5 gf / 50 μm or more. [Method of measuring shrinkage rate] The film stretched in the transverse direction (TD) was cut into a size of 50 mm x 50 mm, and each cut was immersed in a hot water bath at 100°C for 10 seconds. The dimensions were then measured, and the transverse direction (TD) shrinkage rate was calculated using the following formula (1), and is shown as the average shrinkage rate. [0010] [Method of measuring stiffness] Using a LOOP STIFFNESS TESTER (manufactured by TOYOSEIKI CORPORATION), the stretched film was cut into a size of 25 mm x 150 mm, and the left and right clamps (film fixing device) of the tester were fixed with a distance of 50 mm. The parts protruding outside the clamps were cut off, and the film was bent so that the distance between the clamps disappeared. The load (gf) applied to the end of the loop-shaped test piece formed by bending the film so that the clamp distance disappeared was measured by pressing the end of the test piece with a Recorder (loading device) at a speed of 60 mm / min.
10. The film has a haze (ASTM D1003, thickness 50 μm) of less than 8% and a tensile strength in the machine direction (MD) of 250 to 500 kgf / cm as measured by the following method. 2 The shrink label film according to claim 9, characterized in that the elongation in the transverse direction (TD) is 30% or more. [Measurement method] The tensile strength in the machine direction (MD) of the produced paper piece (ASTM D638 Type IV standard) is measured at 50 mm / min using a universal testing machine in accordance with ASTM D638, and the elongation in the transverse direction (TD) until the film breaks is measured under the same conditions as those for measuring the tensile strength.
Citation Information
Patent Citations
Heat-shrinkable polyolefinic film
JP2001162725A
Heat-shrinkable multi-layer film
WO2017061308A1