Method for manufacturing a dual layer heat exchange wall
The method forms a ductile iron interface between metal sheets in double-layer walls, improving thermal conductivity and fatigue resistance, addressing the balance of liquid tightness and pressure resistance in heat exchange walls.
Patent Information
- Application Number
- JP2024532911
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2021-12-02
- Filing Date
- 2022-11-30
- Publication Date
- 2024-11-26
AI Technical Summary
Existing methods for manufacturing double-layer heat exchange walls do not adequately balance the dual functions of liquid tightness and pressure resistance while maintaining high thermal conductivity, and fail to effectively prevent the propagation of fatigue defects.
A manufacturing method involving the use of pure iron leaves or coatings between two metal sheets, followed by mechanical pressing, welding, and hot isostatic pressing to create a ductile and dense interface, ensuring uniform bonding and preventing relative movement of the layers, thereby enhancing thermal conductivity and fatigue resistance.
The method achieves thermal conductivities of up to 95% of the reference, with a 30% increase in service life under fatigue and prevention of fluid propagation, while maintaining mechanical integrity and reducing production complexity.
Smart Images

Figure 2024544004000001 
Figure 2024544004000002 
Figure 2024544004000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for manufacturing a double-layer heat exchange wall, which is intended in particular to equip a device of the heat exchanger type.
[0002] Such heat exchangers find application in the chemical industry or in the energy sector. [Background technology]
[0003] A heat exchanger is a device for transferring thermal energy from a first fluid to a second fluid without mixing the fluids.
[0004] There are various types of dual-fluid heat exchangers, including those with so-called "double-layer" heat exchange walls consisting of two layers of different or the same thickness, each intended to be in contact with one of the heat-transfer fluids.
[0005] This particular construction of a double-layered wall has the advantage that each layer redundantly performs a double function, namely, a liquid-tight function to avoid contact between the two heat transfer fluids and a function to withstand the pressure of these heat transfer fluids, thereby improving the safety of the heat exchanger to which it is attached.
[0006] This dual function is particularly important when the heat exchanger is equipped to plants, such as chemical reactors, where a heat exchange between a first fluid, such as a reactive molten metal or metal salt (based on sodium, lithium or potassium, for example), and a second fluid, such as water, must be realized safely and effectively, since any failure of the heat exchange wall equipped to such plants can have serious consequences for the operation due to the chemical reactivity of the heat transfer medium with the medium to be cooled. In this particular case, strains during use, as well as static pressures and surface corrosion of the fluid, arise as a result of stresses of thermal origin and fatigue strains imposed by vibrations caused by the operating cycle or by thermo-hydraulic actions.
[0007] In most dual layer heat exchange walls, it is expected that a mechanical clearance or gap will be left between the two layers.
[0008] By connecting this gap to a detection system, the presence of fluid caused by the puncture of one of the two layers can be detected before the integrity of the second layer is compromised.
[0009] However, the presence of this gap is particularly detrimental in terms of the thermal conductivity characteristics of the heat exchange wall, and furthermore, if perforations occur simultaneously in the first and second layers forming the heat exchange wall, it is not possible to effectively deal with this.
[0010] In order to improve the thermal conductivity of a double-layer heat exchange wall, it has been proposed to at least partially fill the gap that exists between the first and second layers.
[0011] Thus, US Patent Application Publication No. 2013 / 0205861, the document referred to in the remainder of this specification as [1], proposes a method for manufacturing a heat exchange wall formed by a double-layered tube, in which, after a step of polishing the inner surface of the outer tube and the outer surface of the inner tube, a braided wire is interposed in the gap formed by the outer tube and the inner tube, followed by drawing and heat treatment.
[0012] Document CN203928838, referenced as [2], proposes a method for manufacturing a heat exchange wall, also formed by a double-walled tube, which method includes a step consisting of filling the gap between the inner and outer tube with a metal powder, which gives the double-walled tube good thermal conductivity by radially distributing the temperature, and also allows the attenuation of the degradation risks associated with sudden thermal transitions.
[0013] The document US 2013 / 070889, referenced as [3], proposes a method for manufacturing a double-walled tube, which comprises a step of cold cutting an assembly formed by inserting an inner tube inside an outer tube. The method is either: - an outer tube made of a ferritic steel containing at least 2% by weight of chromium, provided on its inner surface with an oxide scale layer containing chromium having a thickness between 10 μm and 30 μm, and an inner tube made of a steel or alloy containing at least 2% by weight of chromium, provided with a scale layer on its outer surface which is machined and / or polished over a thickness of at least 0.1 mm; or - an inner tube made of a ferritic steel containing at least 2% by weight of chromium, provided on its outer surface with an oxide scale layer containing chromium having a thickness between 10 μm and 30 μm, and an outer tube made of a steel or alloy containing at least 2% by weight of chromium, provided with a scale layer on its inner surface which has been machined and / or polished over a thickness of at least 0.1 mm.
[0014] The cold cutting step performed in the method of document [3] is carried out to achieve a reduction in the outer thickness of 5% to 30%.
[0015] Furthermore, document GB2241339, referenced as [4], proposes a method for manufacturing a heat exchange wall comprising three concentric metal tubes, which are in intimate contact at their interfaces to ensure good thermal contact between the three tubes. This intimate contact can be achieved by brazing or welding. In document [4], the middle tube can be made of iron or steel based material, and the inner and outer tubes can be made of copper or copper alloy.
[0016] Although the manufacturing methods described in references [1]-[4] improve the thermal conduction properties of the double-walled tube, these manufacturing methods have thermal conductivities that are too detrimental to the intended operation. [Prior art documents] [Patent documents]
[0017] [Patent Document 1] US Patent Application Publication No. 2013 / 0205861 [Patent Document 2] CN203928838 [Patent Document 3] US Patent Application Publication No. 2013 / 070889 [Patent Document 4] GB2241339 Summary of the Invention [Problem to be solved by the invention]
[0018] The object of the present invention is therefore to propose a method for producing a double-layer heat exchange wall having the dual function of being liquid-tight and resistant to the pressure of a heat transfer fluid, in particular by preventing the propagation of fatigue defects, while maximally guaranteeing its integrity in use, with a minimum sacrifice of thermal conductivity. [Means for solving the problem]
[0019] The foregoing and other objects are achieved by a method for manufacturing a dual layer heat exchange wall comprising a first layer and a second layer that are metallic.
[0020] According to the present invention, the method comprises the following sequence of steps (i) to (v) and, optionally, step (vi): (i) a first metal sheet intended to form a first layer and having a thickness e1, a second metal sheet intended to form the second layer and having a thickness e2, and Iron Fe with a thickness e3 between 10 μm and 100 μm, advantageously between 50 μm and 100 μm 0 Reef and (ii) a first metal sheet and a second metal sheet and iron Fe 0 assembling the leaf of the first metal sheet and the second metal sheet, the leaf being interposed between the first metal sheet and the second metal sheet; (iii) mechanical pressing of the assembly obtained at the end of step (ii) at a minimum pressure of 1 MPa; (iv) perimeter welding the pressed assembly obtained at the end of step (iii); (v) heat treating the welded assembly obtained at the end of step (iv), said heat treatment being carried out at a temperature between 800° C. and 1200° C. for 10 8 Pa~2.10 8 and optionally a hot isostatic pressing step, the step being carried out at a pressure of between 100 and 200 Pa for a period of between 1 hour and 3 hours. (vi) performing a supplemental treatment such as carving, bending, quenching, normalizing aging, or annealing; Includes.
[0021] The method according to the invention makes it possible to form a metallic interface made of pure iron between the first and second layers. This interface is therefore ductile and dense, filling the entire initial volume of the gap between the first and second metal sheets, ensuring a uniform mechanical joint between the first and second layers. The absence of clearance between the first and second layers makes it possible to prevent the two layers from moving relative to each other; they then form a single layer, which deforms during subsequent mechanical stress or forming in the same way as a monolithic wall. The manufacturing method according to the invention makes it possible to obtain a double-layer wall with a geometric quality that does not require calibration after the heat treatment step by hot isostatic pressing.
[0022] Moreover, the metallic interface made of pure iron makes it possible to provide the double-layer wall with excellent heat conduction properties by ensuring very good heat transfer between the first and second layers, which has the effect of increasing the efficiency of a heat exchanger comprising such a double-layer wall. 0 This ductile dense interface, made from Fe, is 80% or more dense than a comparable solid wall. 0 The inventors have realised that in certain cases using leaves of this type, the thermal conductivity can be greater than 95%.
[0023] Furthermore, the ductility of this metal-iron interface makes it possible to deflect and / or stop the propagation of any fatigue cracks that may form and propagate in one of the two layers, especially after a large number of cycles, thus preserving the integrity of the other layer. In particular, when fatigue cracks are deflected, they propagate in the ductile metal interface, which extends the service life at room temperature by 30%.
[0024] Moreover, this iron interface is characterized by an impermeability that may prevent capillary propagation of fluids arising from cracks between the two layers.
[0025] By the method according to the invention, the thickness e tot It is possible to produce a double layer wall having
[0026] The method according to the invention comprises steps (i) to (v) and optionally step (vi) as set out above and detailed hereinafter.
[0027] During step (i) of the manufacturing method according to the invention, two metal sheets are provided: a first metal sheet intended to form a first layer of a double-layer wall, and a second metal sheet intended to form a second layer of this same double-layer wall.
[0028] The first metal sheet has a thickness denoted as e1 and the second metal sheet has a thickness denoted as e2.
[0029] According to one embodiment, the thickness e1 of the first metal sheet and the thickness e2 of the second metal sheet are each between 1 mm and 30 mm, advantageously between 1 mm and 5 mm, preferentially between 1 mm and 2 mm. However, the thickness e1 of the first metal sheet and the thickness e2 of the second metal sheet are not necessarily identical, although they are within the same numerical interval.
[0030] The expression "between ..." used above, and further on in the present description, to define an interval should be understood as defining not only the numerical value of the interval, but also the range limit values of this interval.
[0031] During step (i) of the method according to the invention, iron having an oxidation state of 0, i.e. pure iron Fe 0 A leaf consisting of:
[0032] This iron Fe 0 The leaves have a thickness between 10 μm and 100 μm, advantageously between 50 μm and 100 μm, this thickness being denoted as e3.
[0033] The manufacturing method according to the invention further comprises, after step (i), the step of: 0 (ii) assembling the leaf of said first metal sheet and said second metal sheet, said leaf being interposed between said first metal sheet and said second metal sheet.
[0034] In other words, at the end of step (ii), iron Fe 0 The result is an assembly in which the leaf is sandwiched between a first metal sheet and a second metal sheet.
[0035] In one variant of the manufacturing method according to the invention, the above-described steps (i) and (ii) are respectively further divided into the following steps (i') and (ii'): (i') a first metal sheet intended to form a first layer and having a thickness e1, and A second metal sheet, intended to form a second layer and having a thickness e2, is provided with iron Fe on one of its surfaces. 0 a second metal sheet having a coating of and (ii') assembling a first metal sheet and a coated second metal sheet, 0 a coating of said metal is disposed between a first metal sheet and a second metal sheet; may be replaced by
[0036] During step (i') of this variant of the manufacturing method according to the invention, two metal sheets are provided, namely a first metal sheet intended to form the first layer of the double-layer wall and a second metal sheet intended to form the second layer of this same double-layer wall.
[0037] As previously mentioned, the first metal sheet has a thickness designated as e1 and the second metal sheet has a thickness designated as e2.
[0038] According to one embodiment, the thickness e1 of the first metal sheet and the thickness e2 of the second metal sheet are each between 1 mm and 30 mm, advantageously between 1 mm and 5 mm and preferentially between 1 mm and 2 mm. As already mentioned before, the thickness e1 of the first metal sheet and the thickness e2 of the second metal sheet are in the same numerical interval, but do not necessarily have to be identical.
[0039] In this variant, the second metal sheet has on one of its surfaces iron with oxidation state 0, i.e. pure iron Fe 0 The coating is provided.
[0040] This iron Fe 0The coating has a thickness between 10 μm and 100 μm, advantageously between 50 μm and 100 μm, this thickness being denoted as e3.
[0041] In other words, the coated second sheet is 2' where e 2' =e2+e3.
[0042] According to one embodiment of this variant of the manufacturing method according to the invention, iron powder Fe is applied to one of the surfaces of the second metal sheet. 0 This is obtained by cold spraying.
[0043] In this variant, the manufacturing method according to the invention comprises, after step (i'), a step (ii') of assembling a first metal sheet and a second metal sheet, the first metal sheet being made of iron Fe 0 the coating is disposed between the first metal sheet and the coated second metal sheet.
[0044] In other words, at the end of step (ii'), iron Fe 0 The result is an assembly in which the leaf is positioned between the first metal sheet and the second metal sheet.
[0045] Iron Fe with a thickness of 10μm to 100μm 0 The choice of using a leaf of iron Fe with a thickness of 10 μm to 100 μm by cold spraying 0 As well as the choice to produce a coating of Fe between the first and second layers, 0 This makes it possible to create a ductile interface of Fe 0 The ductile interface makes it possible to significantly slow down and deflect the propagation rate of any fatigue cracks that may form in one of these two layers, thereby making it possible to extend the service life under fatigue of the other (undamaged) layer, and thus of the bilayer wall produced by the method according to the invention, by up to 30%.
[0046] As can be seen from the following example, this choice is 0 This makes the interface advantageously suited to the creation of an iron interface using the interposition of iron powder Fe 0 It is possible to obtain a bilayer wall having better mechanical and thermal conductivity properties than a bilayer wall in which an iron interface is obtained by cold spraying of .
[0047] In one advantageous variant, the method according to the invention further comprises a step of cleaning the surface of the first metal sheet and the surface of the second metal sheet or the coated second metal sheet, this cleaning step being carried out before the assembling step (ii) or (ii').
[0048] In another advantageous variant, the method according to the invention further comprises a step of polishing the first metal sheet and the second metal sheet (optionally coated), this polishing step being carried out before the assembling step (ii) or (ii').
[0049] The manufacturing method according to the invention comprises, after the assembling step (ii) or (ii'), a step (iii) of mechanical pressing of the assembly obtained at the end of step (ii) or (ii'), said mechanical pressing being carried out at a minimum pressure of 1 MPa.
[0050] The choice of such mechanical pressing step (iii) has the advantage that the volume of the gap existing between the first metal sheet and the second (optionally coated) metal sheet is further reduced, so that the amount of gas contained between these two metal sheets is negligible.
[0051] The manufacturing method according to the invention comprises, after the mechanical pressing step (iii), a step (iv) of circumferential welding of the assembly obtained at the end of step (iii), thereby achieving a peripheral weld of the first metal sheet and the second metal sheet.
[0052] This welding step (iv) may be carried out by any welding technique capable of achieving a gas-tight weld, with the iron Fe interposed between the first metal sheet and the second metal sheet. 0 This makes it possible to isolate the interfaces.
[0053] This welding step (iv) can in particular be carried out by laser, rod, electron beam or, preferably, arc welding methods using a non-molten electrode in the presence of a filler metal, this latter type of welding in particular being carried out by TIG welding (TIG being the acronym for "Tungsten Inert Gas") without a filler metal.
[0054] Iron 0 The presence of the interface does not affect the composition of the weld joint, nor the composition of the first and second metal sheets, and therefore allows them to retain their mechanical properties. 0 By choosing the interface, it is possible to provide, by reliable welding, the assembly of the double-layered walls produced by the method according to the invention with the structure of the device they are intended to comprise, for example with the structure of a heat exchanger. The reason for this is that the iron Fe at the interface 0 This is because the interface only slightly changes the composition of the circumferential weld and, as a result, does not change the mechanical properties of the circumferential weld so produced.
[0055] The manufacturing method according to the invention comprises, at the end of the welding step (iv), a step (v) of heat treating the welded assembly as obtained at the end of step (iv).
[0056] The heat treatment step (v) is carried out at a temperature of 800°C to 1200°C for 10 8 Pa~2.10 8 This is carried out by hot isostatic pressing (HIP) at a pressure of 100 MPa for a period of 1 to 3 hours.
[0057] This hot isostatic pressing step (v) makes it possible to weld the first metal sheet and the second metal sheet (optionally coated) by diffusion, thereby making it possible to obtain a homogeneous mechanical joint between said first and second metal sheets, which is formed by an iron Fe interface at the end of the hot isostatic pressing step (v).
[0058] In one advantageous variant, the method according to the invention further comprises at least one step of grinding the assembly, this or these grinding steps being carried out before the welding step (iv) and / or before the heat treatment step (v).
[0059] In one particularly advantageous variant, the method according to the invention does not include a degassing step between the mechanical pressing step (iii) and the welding step (iv) and / or does not include a degassing step between the welding step (iv) and the heat treatment step (v).
[0060] The elimination of one or two degassing steps, which are particularly complicated to implement on an industrial scale in the context of double-wall manufacturing, contributes to a significant reduction in cycle times, costs and manufacturing times.
[0061] The method according to the invention makes it possible to produce double-layer walls of variable length and shape.
[0062] The materials of the first tube and the second tube (without coating) may be the same or different. These materials may in particular include iron.
[0063] In one advantageous variant, the first metal sheet and the second metal sheet are made of a material containing iron, which material is advantageously iron Fe 0and steels, for example martensitic steels such as Eurofer-97.
[0064] In one preferred variant, the material of the first metal sheet and the second metal sheet is identical.
[0065] In one variant, the method according to the invention further comprises a step (vi) of carrying out at least one supplementary treatment, the purpose of such supplementary treatment (vi) being to give a particular shape and / or particular mechanical properties to the bilayer wall produced in particular by the method according to the invention.
[0066] This supplementary treatment (vi) can be chosen, for example, from carving, bending, quenching, normalizing ageing or annealing, or it can be a combination of supplementary treatments (quenching followed by normalizing ageing).
[0067] By such a complementary treatment (vi), the double layer wall can be formed, for example, as a tube having a circular, square or rectangular cross section.
[0068] The present invention will be better understood in light of the following additional description, which refers to the accompanying Figures 1 and 2.
[0069] This additional description is presented only to illustrate the purpose of the present invention and should not be construed as limiting this purpose in any way. [Brief description of the drawings]
[0070] [Figure 1] FIG. 1 shows the variation in fatigue crack (shown as a, expressed in mm) progression at ambient temperature versus number of cycles (shown as N) for two double-layered walls according to the invention (shown as RS and CS) and a similar reference solid wall (shown as Massive). [Diagram 2]FIG. 1 shows the variation of equivalent thermal conductivity (denoted as λ and expressed in W / mK) versus temperature (denoted as T and expressed in K) for two double-layer walls according to the invention (denoted as RS and CS) and a similar reference solid wall (denoted as Massive). DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0071] 1. Production of double-layer walls and reference walls by the method according to the invention A first bilayer wall, designated 1.1.RS, was prepared by the method according to the present invention.
[0072] Two metal sheets made from Eurofer-97 were rolled such that the first metal sheet was 6.00mm (+0.0 / -0.1mm) thick and the second metal sheet was 4mm (+0.0 / -0.1mm) thick.
[0073] Metallic iron (Fe) 0 The sheet was rolled to finally obtain a leaf having a thickness of 100 μm.
[0074] After the surfaces of the two metal sheets were polished and then cleaned, the two metal sheets and the leaf were assembled in a sandwich by interposing the metallic iron leaf between the first and second metal sheets.
[0075] Next, this assembly was mechanically pressed by applying a pressure of 1 MPa using a press, and then peripheral welding was performed by TIG around the entire circumference of the assembly.
[0076] The thus welded assembly is then subjected to a tensile test at a temperature of 1100° C. and a pressure of 1200 bar (1.2×10 8 The alloys were heat treated by performing a hot isostatic pressing (HIP) cycle at a pressure of 1000 psi (1 Pa) for 1 hour, followed by a complementary heat treatment at 980°C for 30 minutes followed by quenching and ageing at 760°C for 90 minutes.
[0077] At the end of these heat treatments, a double-layer wall RS is obtained.
[0078] A second bilayer wall, designated 1.2.CS, was prepared by the method according to the present invention.
[0079] Two metal sheets made from Eurofer-97 were rolled such that the first metal sheet was 6.00mm (+0.0 / -0.1mm) thick and the second metal sheet was 4mm (+0.0 / -0.1mm) thick.
[0080] Metallic iron powder was then applied by cold spray to one of the surfaces of a second metal sheet to form an iron coating greater than 100 μm thick.
[0081] The deposit was polished to a thickness of 100 μm and then the surfaces of the two metal sheets were cleaned before assembling the first metal sheet with the coated second metal sheet, with the metallic iron coating positioned between the first and second metal sheets.
[0082] The assembly thus obtained was then subjected to the steps of mechanical pressing, welding, heat treatment by HIC and supplementary heat treatment as described in section 1.1 above.
[0083] At the end of these heat treatments, a double-layer wall CS is obtained.
[0084] 1.3. Additionally, a reference wall designated as Massive was fabricated.
[0085] Metal sheets made from Eurofer-97 were rolled to a thickness of 10.00 mm (+0.0 / -0.1 mm).
[0086] The metal sheet was then subjected to heat treatment by HIC and the supplemental heat treatment described in section 1.1 above.
[0087] At the end of these heat treatments, a reference wall Massive is obtained.
[0088] 2. Characteristics of double-layered walls RS and CS and reference wall Massive 2.1. Bending specimens of 10 × 10 × 55 mm were taken from each wall RS, CS, and Massive. A 2 mm notch, marked by point A in Figure 1, was formed in each specimen, shown as RS, CS, and Massive, respectively, to initiate fatigue cracks during fatigue loading.
[0089] The propagation of this notch was then investigated by subjecting the specimen to a three-point bending stress cycle with a constant maximum force of 60% of the yield strength of the metal sheet material. A minimum force of 150 N is maintained to prevent the tool from dislodging from the specimen. The crack path is tracked in situ by image correlation.
[0090] With reference to the zone marked as B in FIG. 1, it can be seen that the specimens RS and CS according to the invention are characterized by a retardation of crack propagation when compared to the reference specimen Massive.
[0091] Furthermore, referring to the zone marked as C in Fig. 1, it can be seen that the specimens RS and CS according to the invention show a stagnation in the length of the crack at the interface (propagation distance 6 mm), which increases the service life of the double-layer walls RS and CS when compared to the reference wall Massive.
[0092] These results suggest that Fe 0 It is clearly shown that by selecting a ductile interface, it is possible to significantly change the crack propagation rate and significantly extend the fatigue life of the intact layer at ambient temperature.
[0093] 2.2. The thermal conductivity of each test piece (RS, CS, and Massive) was measured.
[0094] With reference to the results shown in FIG. 2, it can be seen that the test pieces RS and CS manufactured by the method according to the invention have a thermal conductivity λ very close to that of the reference test piece Massive, the thermal conductivity coefficient corresponding to at least 80% of the thermal conductivity of the reference wall Massive for the double-layer wall CS and close to 95% for the double-layer wall RS.
Claims
1. A method for manufacturing a double-layer heat exchange wall comprising a first layer and a second layer which are metal, the method comprising the following sequence of steps (i) to (v) and, optionally, step (vi): (i) The first layer is intended to form a 1 a first metal sheet having The second layer is intended to form a 2 a second metal sheet having A thickness e between 10 μm and 100 μm, advantageously between 50 μm and 100 μm 3 Fe 0 Reef and (ii) the first metal sheet and the second metal sheet and iron Fe 0 wherein the leaf is interposed between the first metal sheet and the second metal sheet; and (iii) mechanical pressing of the assembly obtained at the end of the preceding step (ii) at a minimum pressure of 1 MPa; (iv) periphery welding the pressed assembly obtained at the end of step (iii); (v) heat treating the welded assembly obtained at the end of step (iv), said heat treatment being carried out at a temperature between 800° C. and 1200° C. for 10 8 Pa~2.10 8 and optionally a hot isostatic pressing step carried out at a pressure of between 100 and 200 Pa for a period of between 1 hour and 3 hours. (vi) performing a supplemental treatment such as carving, bending, quenching, normalizing aging, or annealing; A method comprising:
2. The steps (i) and (ii) are respectively the following steps (i') and (ii'): (i') The first layer is intended to form a 1 a first metal sheet having The second layer is intended to form a 2 A second metal sheet having iron Fe on one of the surfaces of the second metal sheet. 0 said coating having a thickness e between 10 μm and 100 μm, advantageously between 50 μm and 100 μm. 3 and the coated second metal sheet has a thickness e 2' where e 2' =e 2 +e 3 A second metal sheet and (ii') assembling the first metal sheet and the coated second metal sheet, 0 the coating being disposed between the first metal sheet and the second metal sheet; The method of claim 1, wherein
3. Iron 0 The coating of iron powder Fe on one of the surfaces of the second metal sheet. 0 The method according to claim 2, wherein the composition is obtained by cold spraying.
4. 4. The method according to claim 1, wherein the welding step (iv) is carried out by an arc welding process with a non-molten electrode, if appropriate in the presence of a filler metal.
5. 5. The method of claim 1, further comprising the step of cleaning the surface of the first metal sheet and the surface of the coated second metal sheet, the cleaning step being carried out prior to the assembling step (ii) or (ii').
6. 6. The method of claim 1, further comprising a step of polishing the first metal sheet and the second metal sheet, the polishing step being carried out prior to the assembling step (ii) or (ii').
7. 7. The method according to claim 1, further comprising at least one step of polishing the assembly, the polishing step being carried out before the welding step (iv) and / or before the heat treatment step (v).
8. 8. The method according to claim 1, wherein the method does not include a degassing step between the mechanical pressing step (iii) and the welding step (iv) and / or between the welding step (iv) and the heat treatment step (v).
9. The first metal sheet and the second metal sheet are made of a material containing iron, advantageously the material being iron Fe 0 and steel.
10. 10. The method according to claim 1, wherein the material of the first metal sheet and the second metal sheet is the same.
11. The thickness e of the first metal sheet 1 and the thickness e of the second metal sheet 2 The method according to any one of claims 1 to 10, wherein the thickness of the membrane is between 1 mm and 30 mm, advantageously between 1 mm and 5 mm and preferentially between 1 mm and 2 mm.
Citation Information
Patent Citations
Tungsten and heat sink material connecting head and manufacturing method thereof
CN111347146A
Leak detection in a heat exchanger
GB2241339A
Manufacture of high corrosion resistant double metal pipe
JP1989197081A
Double-wall heat exchange tube comprising metal powder interlayer in molten salt heat exchanger
CN203928838U
Double-walled tube with interface gap and production method therefor
US20130070889A1