Fluorocarbon / palladium / magnesium-scandium hydrogen gaschromic color changing film and its manufacturing method
The fluorocarbon/palladium/magnesium-scandium hydrogen gaschromic color conversion film addresses the limitations of conventional sensors by enhancing hydrogen storage and release rates and durability, ensuring efficient and safe hydrogen detection.
Patent Information
- Application Number
- JP2024533136
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2021-04-29
- Filing Date
- 2022-04-27
- Publication Date
- 2024-11-28
AI Technical Summary
Conventional hydrogen gas sensors based on palladium/magnesium composite materials face issues with hydrogen storage and release rates, cycle durability, and water corrosion, limiting their effectiveness in detecting hydrogen gas safely and efficiently.
A fluorocarbon/palladium/magnesium-scandium hydrogen gaschromic color conversion film is developed, comprising a magnesium-scandium composite film layer, a palladium catalyst layer, and a fluorocarbon film layer, synthesized using magnetron co-sputtering and plasma vapor deposition methods, to enhance hydrogen absorption and release rates and improve cycle durability.
The film achieves fast hydrogen storage and release reactions, high cycle durability, and resistance to water corrosion, making it suitable for reliable hydrogen gas detection without electrical leads.
Smart Images

Figure 2024544206000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to the technical field of hydrogen gaschromic color conversion film, and more particularly to a fluorocarbon / palladium / magnesium-scandium gaschromic light-control film and its manufacturing method. [Background technology]
[0002] Hydrogen gas plays an important role in the future sustainable society as a clean energy carrier. However, when the hydrogen gas content in the air is 4% to 75%, it will explode when exposed to an open flame. At the same time, hydrogen gas has a low ignition energy and hydrogen molecules are very easy to diffuse. Therefore, problems such as hydrogen gas leakage should be avoided during the storage, transportation and use of hydrogen gas. On the other hand, hydrogen gas is colorless, odorless and undetectable by humans, so it is essential to have a sensitive and reliable hydrogen gas detection device, i.e., a hydrogen gas sensor.
[0003] Traditional hydrogen gas sensing work is mainly realized by catalytic resistance detectors or electrochemical devices, and at present, such devices still have shortcomings that need to be improved, for example, they all need to use electrical leads, which may cause sparks at the detection point and cause safety problems, and at the same time, the space occupied by these detection systems is too large, the consumables are expensive, and the application range is limited. Therefore, some research groups have turned to optical sensors based on hydrogen gas chromic color conversion films. At present, the most representative hydrogen gas chromic color conversion film structure is palladium / magnesium-based composite material / quartz glass, in which palladium has high adsorption to gas and can be used as a catalytic layer, magnesium-based material has strong hydrogen storage ability and can be used as a dimming layer, and conventional composite materials include transition metals, rare earth metals, alkaline earth metals and transition metal oxides, etc. However, the conventional magnesium-based hydrogen gas chromic color conversion film needs to further improve the hydrogen absorption and release rate and cycle durability to meet the response requirements and durability requirements of hydrogen gas sensors. In addition, because palladium has low hydrophobicity, water molecules generated by dehydrogenation and water vapor in the air tend to gather on the surface of the palladium layer and corrode the photochromic film. Therefore, it is necessary to develop a new hydrogen gas chromic photochromic film layer system that has excellent optical conversion characteristics of hydrogen absorption and release and excellent cycle durability.
[0004] Scandium, as a rare earth element, is known as an important "green energy science and technology metal", "important" or "strategic" mineral resource in the 21st century, and is widely used in the fields of structural materials, catalysts and so on.
[0005] The inventor's previous patent application CN109136841A describes a fluorocarbon / palladium / magnesium-niobium pentoxide gas chromic light control film and its manufacturing method, which includes a magnesium-niobium pentoxide composite film layer, a palladium catalyst layer and a fluorocarbon hydrophobic layer sequentially provided on a substrate. Patent document CN112596279A describes a fluorocarbon / palladium / magnesium-ruthenium gas chromic light control film and its manufacturing method, which includes a substrate, a magnesium-ruthenium composite light control film layer, a palladium catalyst layer and a carbon fluorine protective film layer sequentially provided on a substrate. However, the hydrogen absorption / desorption speed (hydrogen absorption reaction time is 80s and 50s, respectively, and hydrogen desorption reaction time is 800s and 900s, respectively) and cycle durability (fluorocarbon / palladium / magnesium-niobium pentoxide composite film layer is cycled 50 times, and the dimming range decreases by 1.5%) of the fluorocarbon / palladium / magnesium-niobium pentoxide composite film layer and the fluorocarbon / palladium / magnesium-ruthenium system need to be further improved. Summary of the Invention [Problem to be solved by the invention]
[0006] The object of the present invention is to make up for the shortcomings in the field of conventional light-control films by providing a fluorocarbon / palladium / magnesium-scandium hydrogen gas chromic color conversion film and its manufacturing method, which can change from a reflective state to a transparent state by reacting with hydrogen gas at room temperature, and can change from a transparent state to a reflective state by reacting with air. The fluorocarbon / palladium / magnesium-scandium system of the present invention has a higher hydrogen absorption / release rate and better cycle durability than the fluorocarbon / palladium / magnesium-niobium pentoxide composite film layer and the fluorocarbon / palladium / magnesium-ruthenium system, and has higher application value. [Means for solving the problem]
[0007] The object of the present invention is achieved by the following technical means.
[0008] According to the present invention, there is provided a fluorocarbon / palladium / magnesium-scandium hydrogen gas chromic color conversion membrane, which comprises a magnesium-scandium composite membrane layer, a palladium catalyst layer and a fluorocarbon membrane layer sequentially disposed on a substrate.
[0009] Preferably, the molar percentage of scandium in the magnesium-scandium composite film layer is 5-75%, more preferably, the molar percentage of scandium is 13-55%, and most preferably, the molar percentage of scandium is 31%. If the magnesium content in the magnesium-scandium composite film layer is too high and the scandium content is too low, the hydrogen absorption and desorption time is too long, the reaction is slow, the conversion speed is reduced, the cycle performance is poor, and conversely, the dimming range is shortened.
[0010] Preferably, the thickness of the magnesium-scandium composite film layer is 10-80 nm. If the composite film layer is too thick, the hydrogen absorption / release response time will be long, and the cycle performance will be reduced. If the composite film layer is too thin, the transmittance of the film in the dehydrogenated state will be high, and the dimming range will be small. The thickness of the palladium catalyst layer is 3-7 nm. If the palladium layer is too thick, it will block light and reduce the transmittance in the hydrogen storage state. If the palladium layer is too thin, it will be easily destroyed by the volume change caused by the hydrogen storage / release cycle, reducing the catalytic efficiency. The fluorocarbon film layer has a thickness of 30 to 150 nm.
[0011] Preferably, the substrate comprises any one of quartz glass, optical fiber, conductive glass, organic glass, and flexible glass.
[0012] According to the present invention, the method includes the steps of growing the magnesium-scandium composite film layer on the substrate by magnetron co-sputtering, then fabricating the palladium catalyst layer on the magnesium-scandium composite film layer by magnetron sputtering, and finally fabricating a fluorocarbon film on the surface of the palladium catalyst layer by plasma vapor deposition; in particular, A step S1 of immersing the substrate in a cleaning solution and then cleaning the substrate; Step S2: placing the cleaned substrate in a magnetron sputtering reaction chamber and turning on a vacuum system to perform vacuuming; Step S3: heating the substrate, introducing working gas A, and maintaining the pressure. After the gas pressure is stabilized, turn on the power of the palladium target, the magnesium target, and the scandium target, close the baffle in front of the target material, and perform pre-sputtering cleaning on the target material; Step S4: after the pre-sputtering is completed, open the baffles of the magnesium target and the scandium target, load a co-sputtering process program, and deposit the magnesium-scandium composite film layer; After the deposition is completed in step S4, the baffle of the palladium target is opened while maintaining the vacuum level constant, and a sputtering process program for the palladium catalyst layer is loaded to deposit the palladium catalyst layer in step S5. After deposition is completed in step S5, power off all the targets and subsequently purge the sample with the working gas A, then stop the introduction of the working gas A and remove the sample in step S6; and step S7: placing the sample taken out into a reaction chamber of a reactive ion vapor deposition machine, introducing working gas B, loading a plasma vapor deposition process program, depositing the fluorocarbon film on the surface of the palladium catalyst layer, and after the deposition is completed, taking out the sample to obtain a fluorocarbon / palladium / magnesium-scandium hydrogen gaschromic color conversion film.
[0013] Preferably, the scandium target material in the scandium target is produced by producing a scandium target material from scandium with a purity (mass fraction) of 99.99% and adding a copper backing plate to the scandium target material, which improves electrical conductivity, uniformly dissipates heat from the target material, and protects the target material.
[0014] Preferably, in step S1, the cleaning solution is a mixed solution of concentrated sulfuric acid and hydrogen peroxide solution, with a volume ratio of 3:1, which can effectively remove impurities and contaminants on the substrate surface, without affecting the components of the substrate, and improve the film formation quality of the substrate.
[0015] Preferably, in step S3, the working gas A is argon gas, and the argon ions generated after the gas is ionized can collide with the target material to excite the target ions without reacting with the target ions, without affecting the components of the film, and the background vacuum degree is less than 8×10 -4 ~9×10 -5 Pull the vacuum until the pressure reaches 1 Pa. In step S3, the substrate is heated to a temperature of 20 to 25° C., the pressure is maintained at 0.4 to 0.6 Pa, and the pre-sputtering time is set to 5 to 20 minutes.
[0016] Preferably, in step S4, the sputtering powers of the magnesium target and the scandium target used in the simultaneous sputtering process program are set to 20 to 100 W and 20 to 300 W, respectively, and the simultaneous sputtering time is set to 30 to 100 s.
[0017] Preferably, in step S5, the sputtering process program uses a sputtering power of the palladium target of 30 to 80 W and a sputtering time of 10 to 60 s.
[0018] Preferably, in steps S4 and S5, the baffle in front of the target material is opened when sputtering, and the baffle is closed when not sputtering, both of which are controlled by a set sputtering process program.
[0019] Preferably, in step S7, the working gas B is C4F8 gas, and in the plasma vapor deposition process program, the working gas pressure used is 2-6 Pa, the flow rate of gas B is 20-50 sccm, the gas excitation power is 400 W-800 W, and the deposition time is 10-100 s. The gas excitation power affects not only the compounding method of fluorocarbons, but also the density of the film layer. If the power is too high, the film layer becomes too dense, hindering the passage of gas and reducing the hydrogen absorption and release efficiency, and if the power is too low, the film layer becomes too sparse, weakening the hydrophobic effect and reducing the protective effect on the inner layer film.
[0020] The opening and closing of the baffle of the target material, the sputtering power, the sputtering time and the deposition parameters of the fluorocarbon film can all be precisely controlled by writing and implementing a process program, and the degree of automation is high.
[0021] In the present invention, first, a magnesium-scandium composite film layer is grown on a substrate by co-sputtering, then a palladium catalyst layer is grown on the film layer by magnetron sputtering, and finally, a fluorocarbon protective layer is deposited on the outer periphery of the film layer by plasma vapor deposition. In the present invention, the catalytic effect of the palladium film is utilized to decompose hydrogen gas into hydrogen atoms in the hydrogen absorption stage, which are then combined with the magnesium substrate to generate hydrides, and scandium is added to accelerate the diffusion of hydrogen atoms in the magnesium substrate, promoting the formation of hydrides, so that the film changes from a reflective state to a transparent state; in the hydrogen release stage, scandium can accelerate the decomposition of hydrides, and the hydrogen atoms obtained in this process diffuse to the surface of the palladium film, so that the film returns to a reflective state. At the same time, the addition of scandium can effectively improve the hydrogen absorption and release cycle performance of the film, that is, the fast reaction speed and dimming range can be maintained even after multiple hydrogen absorption and release reactions. The fluorocarbon film can disperse the generated water and effectively prevent the corrosion of the inner layer film caused by the external environment. The entire reaction process does not require heating or pressurization, and the reversible transformation between the two forms of the film can be achieved at room temperature. The light-control film has a short response and recovery time, a simple process, and has important applications in the field of hydrogen gas sensing. Effect of the Invention
[0022] Compared with the prior art, the present invention has the following beneficial effects:
[0023] 1) Magnesium-scandium composite film was synthesized by magnetron co-sputtering method. The whole process was controlled by a preset program, which is simple to operate, has high stability, and produces a uniform film layer.
[0024] 2) Taking advantage of the feature that scandium improves the adsorption and hydrogen release kinetics of magnesium, scandium is compounded with a magnesium substrate to improve the microstructure and composition of the magnesium-based membrane, accelerate the diffusion rate of hydrogen atoms, improve the hydrogen storage and release efficiency of the membrane, and improve the cycle performance of the membrane.
[0025] 3) The palladium film has strong oxidation resistance. Through the in situ growth method, palladium can more completely protect the magnesium substrate, and palladium can realize reversible catalytic activity for hydrogen gas at room temperature, with low requirements for experimental conditions.
[0026] 4) Fluorocarbon films have high permeability to gas molecules and strong hydrophobicity, which allows gas molecules to be distributed uniformly on the surface of the film, which not only helps to accelerate the gaschromic reaction but also improves the corrosion resistance of the film. Plasma vapor deposition can produce solid films at low temperatures, with high film bonding strength and fast reaction speed.
[0027] 5) The film has a large dimming range, a fast optical conversion speed for hydrogen absorption and desorption, and high cycle durability for hydrogen absorption and desorption, and has important applications. [Brief description of the drawings]
[0028] Other characteristics, objects and advantages of the invention will appear more clearly on reading the detailed description given by way of non-limiting examples with reference to the following drawings, in which:
[0029] [Figure 1] FIG. 1 shows a membrane structure of CF / Pd / Mg-31% mol Sc prepared in Example 1 of the present invention and a transmittance curve during the hydrogen absorption process obtained by testing. FIG. 1a shows the membrane structure, and FIG. 1b shows the transmittance curve during the hydrogen absorption process. [Diagram 2] FIG. 2 is a transmittance curve diagram of a hydrogen release process of a film having a composition of CF / Pd / Mg-31% mol Sc obtained by testing in Example 1 of the present invention. [Diagram 3] FIG. 2 is a transmittance curve obtained after a film having a composition of CF / Pd / Mg-31% mol Sc obtained by testing in Example 1 of the present invention was subjected to 50 cycles of hydrogen absorption / desorption reaction. [Figure 4] 1 shows the cross-sectional EDS analysis results of a film of CF / Pd / Mg-9% mol Sc, the composition of which was obtained by the test in Example 2 of the present invention. [Diagram 5] FIG. 2 is a cross-sectional view of a CF / Pd / Mg-31% mol Sc film layer obtained by transmission electron microscope analysis in Example 1 of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0030] The present invention will be described in detail below with reference to specific examples. The following examples are useful for those skilled in the art to further understand the present invention, but are not intended to limit the present invention. However, those skilled in the art may make some modifications and improvements without departing from the concept of the present invention. All of these are within the scope of protection of the present invention.
[0031] Example 1 According to this embodiment, there is provided a method for producing a fluorocarbon / palladium / magnesium-scandium hydrogen gasochromic color changing film, which comprises the following steps (1) to (5).
[0032] In step (1), a scandium target material is manufactured using scandium powder with a purity (mass fraction) of 99.99%, and a copper backing plate is added. In the following Examples 2 to 6, the same scandium target material is used in all cases. In step (2), the quartz glass plate is immersed in the prepared cleaning solution for 15 minutes, and then washed with deionized water for 1 minute. The cleaning solution is a mixed solution of concentrated sulfuric acid and hydrogen peroxide in a ratio of 3:1. The washed quartz glass substrate is placed in a magnetron sputtering reaction chamber, and the vacuum system is turned on to ensure that the background vacuum is 3×10 -4 Pull the vacuum until the pressure reaches 1 Pa. In step (3), the substrate is heated to a temperature of 20 to 25°C, working gas A (argon gas) is introduced, and the pressure is maintained at 0.4 to 0.6 Pa. After the gas pressure is stabilized, the power of the palladium target, magnesium target, and scandium target is turned on, the baffle in front of each target material is closed, and the target material is pre-sputtered for 10 min. Next, a simultaneous sputtering process program is set, the sputtering power of the magnesium target and the scandium target are set to 40 W and 200 W, respectively, the simultaneous sputtering time is set to 60 s, and the deposition of the magnesium-scandium film is started, and the thickness of the film layer is set to 50 nm. In step (4), after the deposition is completed, the vacuum level is kept at 0.5 Pa, and the sputtering process program for the palladium catalyst layer is loaded. The sputtering power of the palladium target is adjusted to 80 W, the sputtering time to 14 s, and the thickness of the film layer to 5 nm. After the growth of the palladium film is completed, all the targets are turned off, and the sample is purged with working gas A (argon gas) for 1 min. Then, the sample is taken out to obtain a film with the composition Pd / Mg-31% mol Sc. The transmission electron microscope image of the obtained Pd / Mg-31% mol Sc film is shown in Figure 5. In step (5), the Pd / Mg-31% mol Sc film is placed in a reactive ion vapor deposition machine, and the process parameters of the fluorocarbon film are set as follows: working gas pressure is 4 Pa, gas B flow rate is 40 sccm, gas excitation power is 600 W, and deposition time is 60 s. Working gas B (C4F8) is introduced, the process program is loaded, and the fluorocarbon film is deposited to a thickness of 100 nm. After completion, the sample is taken out to obtain a film with the composition CF / Pd / Mg-31% mol Sc. The structure of the obtained film includes a magnesium-scandium composite film layer (Mg-Sc layer), a palladium catalyst layer (Pd layer), and a fluorocarbon film layer (FC layer) sequentially provided on the substrate, as shown in Figure 1.
[0033] The schematic diagram of the transmittance curve of the hydrogen absorption process of the CF / Pd / Mg-31% mol Sc film obtained by the test is shown in Fig. 1b. As can be seen from Fig. 1b, the hydrogen absorption reaction time of the CF / Pd / Mg-31% mol Sc film is about 5 s.
[0034] A schematic diagram of the transmittance curve of the hydrogen release process of the CF / Pd / Mg-31% mol Sc film obtained by the test is shown in Figure 2. As can be seen from Figure 2, the hydrogen release reaction time of the CF / Pd / Mg-31% mol Sc film is about 70 s.
[0035] The schematic diagram of the transmittance curve of the CF / Pd / Mg-31% mol Sc film obtained by the test after 50 cycles of hydrogen release process is shown in Figure 3. As can be seen from Figure 3, the CF / Pd / Mg-31% mol Sc film has good cycle performance.
[0036] Example 2 According to this embodiment, there is provided a method for producing a fluorocarbon / palladium / magnesium-scandium hydrogen gasochromic color changing film, which comprises the following steps (1) to (4).
[0037] In step (1), the quartz glass plate is immersed in the prepared cleaning solution for 15 minutes, and then washed with deionized water for 1 minute. The cleaning solution is a mixed solution of concentrated sulfuric acid and hydrogen peroxide in a ratio of 3:1. The cleaned quartz glass substrate is placed in a magnetron sputtering reaction chamber, and the vacuum system is turned on to ensure that the background vacuum is 3×10 -4 Pull the vacuum until the pressure reaches 1 Pa. In step (2), the substrate is heated to a temperature of 20 to 25°C, working gas A (argon gas) is introduced, and the pressure is maintained at 0.4 to 0.6 Pa. After the gas pressure is stabilized, the power of the palladium target, magnesium target, and scandium target is turned on, the baffle in front of each target material is closed, and the target material is pre-sputtered for 10 minutes. Next, a simultaneous sputtering process program is set, the sputtering power of the magnesium target and the scandium target are set to 40 W and 40 W, respectively, the simultaneous sputtering time is set to 60 s, and the deposition of the magnesium-scandium film is started, and the film layer thickness is set to 40 nm. In step (3), after the deposition is completed, while maintaining the vacuum at 0.5 Pa, load the sputtering process program for the palladium catalyst layer, adjust the sputtering power of the palladium target to 80 W, the sputtering time to 14 s, and the thickness of the film layer to 5 nm. After the growth of the palladium film is completed, turn off all the targets, and then purge the sample with working gas A for 1 min, and then take out the sample to obtain a film with the composition Pd / Mg-9% mol Sc. In step (4), the Pd / Mg-9% mol Sc film is placed in the reactive ion vapor deposition machine, and the process parameters for the fluorocarbon film are set as follows: working gas pressure 3 Pa, gas B flow rate 30 sccm, gas excitation power 400 W, and deposition time 30 s. Introduce working gas B (C4F8), load the process program, and deposit the fluorocarbon film to a thickness of 20 nm. After completion, take out the sample to obtain a film with the composition CF / Pd / Mg-9% mol Sc.
[0038] The cross-sectional EDS analysis result of the CF / Pd / Mg-9% mol Sc film is shown in Fig. 4, from which the presence of Sc element can be confirmed.
[0039] The hydrogen absorption reaction time of the CF / Pd / Mg-9% mol Sc film obtained by the test is about 38 s, and the hydrogen desorption reaction time is about 600 s.
[0040] Example 3 According to this embodiment, there is provided a method for producing a fluorocarbon / palladium / magnesium-scandium hydrogen gasochromic color changing film, which comprises the following steps (1) to (4).
[0041] In step (1), the quartz glass plate is immersed in the prepared cleaning solution for 15 minutes, and then washed with deionized water for 1 minute. The cleaning solution is a mixed solution of concentrated sulfuric acid and hydrogen peroxide in a ratio of 3:1. The cleaned quartz glass substrate is placed in a magnetron sputtering reaction chamber, and the vacuum system is turned on to ensure that the background vacuum is 9×10 -5 Pull the vacuum until the pressure reaches 1 Pa. In step (2), the substrate is heated to a temperature of 20 to 25°C, working gas A (argon gas) is introduced, and the pressure is maintained at 0.4 to 0.6 Pa. After the gas pressure is stabilized, the power of the palladium target, magnesium target, and scandium target is turned on, the baffle in front of each target material is closed, and the target material is pre-sputtered for 10 minutes. Next, a simultaneous sputtering process program is set, the sputtering power of the magnesium target and the scandium target are set to 40 W and 60 W, respectively, and the simultaneous sputtering time is set to 60 s, and the deposition of the magnesium-scandium film is started, with the film layer thickness being set to 25 nm. In step (3), after the deposition is completed, while maintaining the vacuum at 0.5 Pa, load the sputtering process program for the palladium catalyst layer, adjust the sputtering power of the palladium target to 60 W, the sputtering time to 20 s, and the thickness of the film layer to 4 nm. After the growth of the palladium film is completed, turn off the power of all the targets, and then purge the sample with working gas A for 1 min, and then take out the sample to obtain a film with the composition Pd / Mg-13% mol Sc. In step (4), the Pd / Mg-13% mol Sc film is placed in a reactive ion vapor deposition machine, and the process parameters for the fluorocarbon film are set as follows: working gas pressure 3.5 Pa, gas B flow rate 35 sccm, gas excitation power 450 W, and deposition time 40 s. Introduce working gas B (C4F8), load the process program, and deposit the fluorocarbon film to a thickness of 70 nm. After completion, take out the sample to obtain a film with the composition CF / Pd / Mg-13% mol Sc.
[0042] The hydrogen absorption reaction time of the CF / Pd / Mg-13% mol Sc film obtained by the test is about 45 s, and the hydrogen desorption reaction time is about 500 s.
[0043] Example 4 According to this embodiment, there is provided a method for producing a fluorocarbon / palladium / magnesium-scandium hydrogen gasochromic color changing film, which comprises the following steps (1) to (4).
[0044] In step (1), the quartz glass plate is immersed in the prepared cleaning solution for 15 minutes, and then washed with deionized water for 1 minute. The cleaning solution is a mixed solution of concentrated sulfuric acid and hydrogen peroxide in a ratio of 3:1. The cleaned quartz glass substrate is placed in a magnetron sputtering reaction chamber, and the vacuum system is turned on to ensure that the background vacuum is 3×10 -4 Pull the vacuum until the pressure reaches 1 Pa. In step (2), the substrate is heated to a temperature of 20 to 25°C, working gas A (argon gas) is introduced, and the pressure is maintained at 0.4 to 0.6 Pa. After the gas pressure is stabilized, the power of the palladium target, magnesium target, and scandium target is turned on, the baffle in front of each target material is closed, and the target material is pre-sputtered for 25 minutes. Next, a simultaneous sputtering process program is set, the sputtering power of the magnesium target and the scandium target are set to 20 W and 80 W, respectively, and the simultaneous sputtering time is set to 60 s, and the deposition of the magnesium-scandium film is started, with the film layer thickness being 30 nm. In step (3), after the deposition is completed, while maintaining the vacuum at 0.5 Pa, load the sputtering process program for the palladium catalyst layer, adjust the sputtering power of the palladium target to 80 W, the sputtering time to 25 s, and the thickness of the film layer to 7 nm. After the growth of the palladium film is completed, turn off all the targets, and then purge the sample with working gas A for 1 min, and then take out the sample to obtain a film with the composition Pd / Mg-28% mol Sc. In step (4), the Pd / Mg-28% mol Sc film is placed in the reactive ion vapor deposition machine, and the process parameters for the fluorocarbon film are set as follows: working gas pressure 5 Pa, gas B flow rate 40 sccm, gas excitation power 700 W, and deposition time 80 s. Introduce working gas B (C4F8), load the process program, and deposit the fluorocarbon film to a thickness of 120 nm. After completion, take out the sample to obtain a film with the composition CF / Pd / Mg-28% mol Sc.
[0045] The hydrogen absorption reaction time of the CF / Pd / Mg-28% mol Sc film obtained by the test is about 26 s, and the hydrogen desorption reaction time is about 320 s.
[0046] Example 5 According to this embodiment, there is provided a method for producing a fluorocarbon / palladium / magnesium-scandium hydrogen gasochromic color changing film, which comprises the following steps (1) to (4).
[0047] In step (1), the quartz glass plate is immersed in the prepared cleaning solution for 15 minutes, and then washed with deionized water for 1 minute. The cleaning solution is a mixed solution of concentrated sulfuric acid and hydrogen peroxide in a ratio of 3:1. The cleaned quartz glass substrate is placed in a magnetron sputtering reaction chamber, and the vacuum system is turned on to ensure that the background vacuum is 3×10 -4 Pull the vacuum until the pressure reaches 1 Pa. In step (2), the substrate is heated to a temperature of 20 to 25°C, working gas A (argon gas) is introduced, and the pressure is maintained at 0.4 to 0.6 Pa. After the gas pressure is stabilized, the power of the palladium target, magnesium target, and scandium target is turned on, the baffle in front of each target material is closed, and the target material is pre-sputtered for 25 minutes. Next, a simultaneous sputtering process program is set, the sputtering power of the magnesium target and the scandium target are set to 40 W and 20 W, respectively, and the simultaneous sputtering time is set to 100 s, and the deposition of the magnesium-scandium film is started, with the film layer thickness being 40 nm. In step (3), after the deposition is completed, while maintaining the vacuum at 0.5 Pa, load the sputtering process program for the palladium catalyst layer, adjust the sputtering power of the palladium target to 80 W, the sputtering time to 25 s, and the thickness of the film layer to 7 nm. After the growth of the palladium film is completed, turn off all the target materials, and then purge the sample with working gas A for 1 min, and then take out the sample to obtain a film with the composition Pd / Mg-5% mol Sc. In step (4), the Pd / Mg-5% mol Sc film is placed in the reactive ion vapor deposition machine, and the process parameters for the fluorocarbon film are set as follows: working gas pressure 5 Pa, gas B flow rate 40 sccm, gas excitation power 700 W, and deposition time 80 s. Introduce working gas B (C4F8), load the process program, and deposit the fluorocarbon film to a thickness of 120 nm. After completion, take out the sample to obtain a film with the composition CF / Pd / Mg-5% mol Sc.
[0048] The hydrogen absorption reaction time of the CF / Pd / Mg-5% mol Sc film obtained by the test is about 16 s, and the hydrogen desorption reaction time is about 750 s.
[0049] Example 6 According to this embodiment, there is provided a method for producing a fluorocarbon / palladium / magnesium-scandium hydrogen gasochromic color changing film, which comprises the following steps (1) to (4).
[0050] In step (1), the quartz glass plate is immersed in the prepared cleaning solution for 15 minutes, and then washed with deionized water for 1 minute. The cleaning solution is a mixed solution of concentrated sulfuric acid and hydrogen peroxide in a ratio of 3:1. The cleaned quartz glass substrate is placed in a magnetron sputtering reaction chamber, and the vacuum system is turned on to ensure that the background vacuum is 3×10 -4 Pull the vacuum until the pressure reaches 1 Pa. In step (2), the substrate is heated to a temperature of 20 to 25°C, working gas A (argon gas) is introduced, and the pressure is maintained at 0.4 to 0.6 Pa. After the gas pressure is stabilized, the power of the palladium target, magnesium target, and scandium target is turned on, the baffle in front of each target material is closed, and the target material is pre-sputtered for 25 minutes. Next, a simultaneous sputtering process program is set, the sputtering power of the magnesium target and the scandium target are set to 40 W and 300 W, respectively, and the simultaneous sputtering time is set to 30 s, and the deposition of the magnesium-scandium film is started, with the film layer thickness set to 40 nm. In step (3), after the deposition is completed, while maintaining the vacuum at 0.5 Pa, load the sputtering process program for the palladium catalyst layer, adjust the sputtering power of the palladium target to 80 W, the sputtering time to 25 s, and the thickness of the film layer to 7 nm. After the growth of the palladium film is completed, turn off the power of all the targets, and then purge the sample with working gas A for 1 min, and then take out the sample to obtain a film with the composition Pd / Mg-55% mol Sc. In step (4), the Pd / Mg-55% mol Sc film is placed in the reactive ion vapor deposition machine, and the process parameters for the fluorocarbon film are set as follows: working gas pressure 5 Pa, gas B flow rate 40 sccm, gas excitation power 700 W, and deposition time 80 s. Introduce working gas B (C4F8), load the process program, and deposit the fluorocarbon film to a thickness of 120 nm. After completion, take out the sample to obtain a film with the composition CF / Pd / Mg-55% mol Sc.
[0051] The hydrogen absorption reaction time of the CF / Pd / Mg-55% mol Sc film obtained by the test is about 11 s, and the hydrogen desorption reaction time is about 105 s.
[0052] Example 7 According to this embodiment, there is provided a method for producing a fluorocarbon / palladium / magnesium-scandium hydrogen gasochromic color changing film, which comprises the following steps (1) to (4).
[0053] In step (1), the quartz glass plate is immersed in the prepared cleaning solution for 15 minutes, and then washed with deionized water for 1 minute. The cleaning solution is a mixed solution of concentrated sulfuric acid and hydrogen peroxide in a ratio of 3:1. The cleaned quartz glass substrate is placed in a magnetron sputtering reaction chamber, and the vacuum system is turned on to ensure that the background vacuum is 3×10 -4 Pull the vacuum until the pressure reaches 1 Pa. In step (2), the substrate is heated to a temperature of 20 to 25°C, working gas A (argon gas) is introduced, and the pressure is maintained at 0.4 to 0.6 Pa. After the gas pressure is stabilized, the power of the palladium target, magnesium target, and scandium target is turned on, the baffle in front of each target material is closed, and the target material is pre-sputtered for 25 minutes. Next, a simultaneous sputtering process program is set, the sputtering power of the magnesium target and the scandium target are set to 20 W and 300 W, respectively, and the simultaneous sputtering time is set to 30 s, and the deposition of the magnesium-scandium film is started, with the film layer thickness set to 40 nm. In step (3), after the deposition is completed, while maintaining the vacuum at 0.5 Pa, load the sputtering process program for the palladium catalyst layer, adjust the sputtering power of the palladium target to 80 W, the sputtering time to 25 s, and the thickness of the film layer to 7 nm. After the growth of the palladium film is completed, turn off the power of all the targets, and then purge the sample with working gas A for 1 min, and then take out the sample to obtain a film with the composition Pd / Mg-75% mol Sc. In step (4), the Pd / Mg-75% mol Sc film is placed in a reactive ion vapor deposition machine, and the process parameters for the fluorocarbon film are set as follows: working gas pressure 5 Pa, gas B flow rate 40 sccm, gas excitation power 700 W, and deposition time 80 s. Introduce working gas B (C4F8), load the process program, and deposit the fluorocarbon film to a thickness of 120 nm. After completion, take out the sample to obtain a film with the composition CF / Pd / Mg-75% mol Sc.
[0054] The hydrogen absorption reaction time of the CF / Pd / Mg-75% mol Sc film obtained by the test is about 10 s, and the hydrogen desorption reaction time is about 95 s.
[0055] (Comparative Example) According to this comparative example, there is provided a method for producing a fluorocarbon / palladium / magnesium hydrogen gasochromic color changing film, which includes the following steps (1) to (4).
[0056] In step (1), the quartz glass plate is immersed in the prepared cleaning solution for 15 minutes, and then washed with deionized water for 1 minute. The cleaning solution is a mixed solution of concentrated sulfuric acid and hydrogen peroxide in a ratio of 3:1. The cleaned quartz glass substrate is placed in a magnetron sputtering reaction chamber, and the vacuum system is turned on to ensure that the background vacuum is 3×10 -4 Pull the vacuum until the pressure reaches 1 Pa. In step (2), the substrate is heated to a temperature of 20 to 25°C, working gas A (argon gas) is introduced, and the pressure is maintained at 0.4 to 0.6 Pa. After the gas pressure is stabilized, the power of the palladium target and the magnesium target are turned on, the baffle in front of each target material is closed, and the target material is pre-sputtered for 25 min. Next, a simultaneous sputtering process program is set, the sputtering power of the magnesium target is set to 40 W, the sputtering time is set to 60 s, and the deposition of the magnesium film is started, with the thickness of the film layer being 25 nm. In step (3), after the deposition is completed, while maintaining the vacuum at 0.5 Pa, load the sputtering process program for the palladium catalyst layer, adjust the sputtering power of the palladium target to 80 W, the sputtering time to 25 s, and the thickness of the film layer to 7 nm. After the growth of the palladium film is completed, turn off all the target materials, and then purge the sample with working gas A for 1 min, and then take out the sample to obtain a film with a composition of Pd / Mg. In step (4), the Pd / Mg film is placed in the reactive ion vapor deposition machine, and the process parameters for the fluorocarbon film are set as follows: working gas pressure 5 Pa, gas B flow rate 40 sccm, gas excitation power 700 W, and deposition time 80 s. Introduce working gas B (C4F8), load the process program, and deposit the fluorocarbon film to a thickness of 120 nm. After completion, take out the sample to obtain a film with the composition CF / Pd / Mg.
[0057] The hydrogen absorption reaction time of the CF / Pd / Mg thin film obtained by the test was about 20 s, and the hydrogen desorption reaction time was more than 900 s, and the cycle performance was much lower than that of the fluorocarbon / palladium / magnesium-scandium system.
[0058] The present invention has many specific application approaches, and the above are only preferred embodiments of the present invention. It should be noted that the above examples are only for illustrating the present invention, and do not limit the scope of protection of the present invention. Those skilled in the art can make some improvements without departing from the principle of the present invention, and these improvements are also included in the scope of protection of the present invention.
Claims
1. a magnesium-scandium composite membrane layer, a palladium catalyst layer and a fluorocarbon membrane layer disposed in sequence on a substrate; A hydrogen gas chromic color changing film of fluorocarbon / palladium / magnesium-scandium, characterized in that
2. In the magnesium-scandium composite membrane layer, the mole percentage of scandium is 5 to 75%; 2. The fluorocarbon / palladium / magnesium-scandium hydrogen gas chromic color changing film according to claim 1.
3. The magnesium-scandium composite membrane layer has a thickness of 10-80 nm, the palladium catalyst layer has a thickness of 3-7 nm, and the fluorocarbon membrane layer has a thickness of 30-150 nm; 2. The fluorocarbon / palladium / magnesium-scandium hydrogen gas chromic color changing film according to claim 1.
4. The substrate includes any one of quartz glass, optical fiber, conductive glass, organic glass, and flexible glass; 2. The fluorocarbon / palladium / magnesium-scandium hydrogen gas chromic color changing film according to claim 1.
5. growing the magnesium-scandium composite film layer on the substrate using a magnetron co-sputtering method, then fabricating the palladium catalyst layer on the magnesium-scandium composite film layer using a magnetron sputtering method, and finally fabricating a fluorocarbon film on the surface of the palladium catalyst layer using a plasma vapor deposition method; in particular, A step S1 of immersing the substrate in a cleaning solution and then cleaning the substrate; Step S2: placing the cleaned substrate in a magnetron sputtering reaction chamber and turning on a vacuum system to perform vacuum evacuation; Step S3: heating the substrate, introducing working gas A, and maintaining the pressure. After the gas pressure is stabilized, the power supply of the palladium target, the magnesium target, and the scandium target is turned on, the baffle in front of the target material is closed, and the target material is pre-sputtered and cleaned; Step S4: after the pre-sputtering is completed, open the baffles of the magnesium target and the scandium target, load a co-sputtering process program, and deposit the magnesium-scandium composite film layer; After the deposition is completed in step S4, open the baffle of the palladium target while maintaining the vacuum level constant, load a sputtering process program for the palladium catalyst layer, and deposit the palladium catalyst layer in step S5. After the deposition is completed in step S5, power off all the targets and continue purging the sample with the working gas A, then stop the introduction of the working gas A and remove the sample in step S6; Step S7: insert the sample into a reaction chamber of a reactive ion vapor deposition machine, introduce working gas B, load a plasma vapor deposition process program, deposit the fluorocarbon film on the surface of the palladium catalyst layer, and after the deposition is completed, remove the sample to obtain a fluorocarbon / palladium / magnesium-scandium hydrogen gas chromic color conversion film.
5. A method for producing the fluorocarbon / palladium / magnesium-scandium hydrogen gas chromic color changing film according to claim 1.
6. In step S1, the cleaning solution is a mixed solution of concentrated sulfuric acid and hydrogen peroxide solution, and the volume ratio is 3:
1.
6. The method for producing a fluorocarbon / palladium / magnesium-scandium hydrogen gas chromic color changing film according to claim 5.
7. In step S3, the working gas A is argon gas, and the background vacuum is 8×10 4 ~9×10 -5 The vacuum is drawn until the pressure reaches Pa. In step S3, the substrate is heated to a temperature of 20 to 25° C., the pressure is maintained at 0.4 to 0.6 Pa, and the pre-sputtering time is 5 to 20 min.
6. The method for producing a fluorocarbon / palladium / magnesium-scandium hydrogen gas chromic color changing film according to claim 5.
8. In step S4, in the simultaneous sputtering process program, the sputtering powers of the magnesium target and the scandium target used are set to 20 to 100 W and 20 to 300 W, respectively, and the simultaneous sputtering time is set to 30 to 100 s.
6. The method for producing a fluorocarbon / palladium / magnesium-scandium hydrogen gas chromic color changing film according to claim 5.
9. In step S5, in the sputtering process program, the sputtering power of the palladium target used is set to 30 to 80 W, and the sputtering time is set to 10 to 60 s.
6. The method for producing a fluorocarbon / palladium / magnesium-scandium hydrogen gas chromic color changing film according to claim 5.
10. In step S7, the working gas B is C 4 F 8 In the plasma vapor deposition process program, the working gas pressure used is 2 to 6 Pa, the flow rate of Gas B is 20 to 50 sccm, the gas excitation power is 400 W to 800 W, and the deposition time is 10 to 100 s.
6. The method for producing a fluorocarbon / palladium / magnesium-scandium hydrogen gas chromic color changing film according to claim 5.
Citation Information
Patent Citations
Fluorocarbon / palladium / magnesium-ruthenium gas-induced dimming film and preparation method thereof
CN112596279A
optical switching device
JP2004514933A
Reflection type dimming element
JP2014026262A