Structurally enhanced roughening mechanism for improved thermal spray equipment and method of use to produce uniform coating properties - Patents.com

Structurally enhanced roughening features on thermal spray components address the issue of scale buildup and overheating in HVOF torches, ensuring consistent coating properties and extended component life by improving heat transfer.

JP2024544213AActive Publication Date: 2024-11-28PRAXAIR ST TECHNOLOGY INC
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
JP2024533856
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2021-12-17
Publication Date
2024-11-28
Estimated Expiration
2041-12-17

AI Technical Summary

Technical Problem

Conventional thermal spray equipment, such as HVOF torches, suffer from ineffective heat transfer and thermal failure due to scale deposits on internal components, leading to overheating and potential damage.

Method used

Incorporating structurally enhanced roughening features on the external surfaces of thermal spray components, such as ribbed, grit-blasted, or knurled textures, to prevent scale buildup and enhance heat transfer by maintaining consistent contact with cooling media.

Benefits of technology

The structurally enhanced roughening features significantly reduce scale deposits, ensuring consistent coating properties and extended component life by maintaining efficient heat transfer and preventing thermal failure.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024544213000001_ABST
    Figure 2024544213000001_ABST
Patent Text Reader

Abstract

A new and improved thermal spray component is provided having structurally enhanced roughening features on the wetted surface that facilitates reduced scale deposit buildup and improves coating property performance during operation of a thermal spray torch.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to novel structurally enhanced roughening features on one or more thermal spray components incorporated into a thermal spray device. The modified thermal spray components contribute to improved performance of the thermal spray device. [Background technology]

[0002] High Velocity Oxygen Flame Spraying (HVOF) is a combustion flame spraying process that produces molten particles that are deposited on a substrate. The spray torch uses a fuel, such as propylene or kerosene, that burns in the presence of oxygen under relatively high pressure in the internal combustion chamber of the spray torch. Combustion gases are produced. In particular, a combustion flame is produced along the inside of the combustion chamber. The temperature of the combustion flame can reach approximately 2000°F or higher. The combustion gases are discharged through a throat portion of the combustion chamber and then flow downstream into an extended barrel, which is an elongated nozzle-like structure. Feedstock in the form of powder or wire of metal or ceramic material can be fed into the barrel or into an interconnect portion located between the combustion chamber and the barrel. As the feedstock is injected, it is trapped by the combustion gas flow. The feedstock particles exit the barrel in molten form as a high velocity jet stream and are directed towards the substrate where they are deposited to form a coating.

[0003] The relatively high temperatures generated from the energy source in the HVOF apparatus can be problematic. The interior surfaces of the barrel and combustion chamber can become hotter and be at risk of overheating, leading to thermal failure. To control the temperature and reduce the risk of overheating the interior surfaces of the HVOF torch, cooling water is circulated along the various surfaces of the spray components of the HVOF torch, including the exterior surface of the barrel and the combustion chamber, to allow heat to be extracted from within their respective interior surfaces.

[0004] Despite efforts to control the operating temperature of the HVOF torch during its operation, ineffective heat transfer to the cooling water persists. There remains an unmet need for improved thermal spray equipment that can operate at high power levels without thermal damage. Summary of the Invention

[0005] In one aspect, an improved thermal spray apparatus for use in producing a thermal spray coating is provided, the improved thermal spray apparatus comprising: a high velocity fuel (HVOF) torch for spraying, the torch including a combustion chamber having an internal volume defined by an inner surface, the combustion chamber configured to receive oxygen and fuel and generate a heated flow therefrom to allow combustion reaction products to be produced in contact with the inner surface, the combustion chamber including a first outer surface in contact with a cooling medium; and a barrel operatively connected downstream of the combustion chamber, the barrel having an internal volume defined by an inner surface configured to contact the heated flow of combustion reaction products and including a second outer surface in contact with the cooling medium, at least one of the first outer surface of the combustion chamber and the second outer surface of the barrel featuring structurally enhanced roughening features, the structurally enhanced roughening features configured to reduce accumulation of scale deposits on the first and / or second outer surfaces when the first and / or second outer surfaces are exposed to the cooling medium during operation of the HVOF torch.

[0006] In a second aspect, an improved thermal spray apparatus is provided for use in producing thermal spray coatings, the improved thermal spray apparatus comprising: a plasma torch for spraying, the torch including a cathode arrangement and an anode, the anode having an exterior surface and an interior portion, the interior portion of the anode operatively connected to the cathode arrangement, the exterior surface of the anode being in fluid communication with a cooling medium, and an exterior surface of the anode featuring structurally enhanced roughening features, the structurally enhanced roughening features configured to reduce the accumulation of scale deposits on the exterior surface of the anode when exposed to the cooling medium during operation of the plasma torch.

[0007] In a third aspect, an improved thermal spray component is provided for use in a thermal spray device to form a thermal spray coating, the improved thermal spray component comprising: a body having a substantially tubular geometry, the substantially tubular geometry having a first end and a second end, a central longitudinal axis traversing the body from the first end to the second end, the body having a first surface adapted to contact a plasma arc or combustion reaction products when the thermal spray component is operably connected within the thermal spray device, the body further having a second surface extending from the first end to the second end, the second surface configured to contact a cooling medium during operation of the thermal spray device, and structurally enhanced roughening features along at least a portion of the second surface, the structurally enhanced roughening features oriented substantially parallel to the central longitudinal axis, the structurally enhanced roughening features configured to reduce accumulation of scale deposits on the second surface when the second surface is exposed to a cooling medium during operation of the thermal spray device.

[0008] In a fourth aspect, an improved thermal spray component is provided for use in a thermal spray apparatus to form a thermal spray coating. The improved thermal spray component comprises a body having a substantially tubular geometry, the substantially tubular geometry having a first end and a second end, a central longitudinal axis traversing the body from the first end to the second end, the body having a first surface adapted to contact a plasma arc or combustion reaction products when the thermal spray component is operably connected within the thermal spray apparatus, the body further having a second wetting surface extending from the first end to the second end, at least a portion of the second wetting surface including a structurally enhanced roughened feature configured to contact a cooling medium during operation of the thermal spray apparatus.

[0009] In a fifth aspect, a method of producing consistent coating properties during operation of an improved thermal spray apparatus, the method including: generating a high temperature energy source with an improved thermal spray apparatus including at least one thermal spray component having a wetting surface, the wetting surface having structurally enhanced roughening features therealong; introducing a powder or wire feedstock to an inlet of the improved thermal spray apparatus; heating the powder or wire feedstock to produce substantially molten particles; introducing a cooling medium into the improved thermal spray apparatus such that the powder or wire feedstock contacts the wetting surface along the structurally enhanced roughening features; and directing the substantially molten particles onto a substrate to produce a coating, the coating including at least one coating property that exhibits less variation during operation of the improved thermal spray apparatus than a coating property produced using a thermal spray apparatus that does not include the at least one thermal spray component, the at least one coating property being selected from the group consisting of porosity, deposition thickness, microhardness, and residual stress. [Brief description of the drawings]

[0010] [Figure 1] FIG 1a is a representative cross-sectional schematic diagram of an improved HVOF apparatus in accordance with the principles of the present invention. FIG 1b is an enlarged view of FIG 1a to show in greater detail the cooling passages through which cooling water flows to cool the exterior surface of a barrel having structurally reinforced roughness features. FIG 1c is an enlarged view of FIG 1a to show in greater detail the cooling passages through which cooling water flows to cool the exterior surface of a combustion chamber having structurally reinforced roughness features. [Diagram 2] 1 is a representative schematic diagram of a structurally enhanced roughening mechanism in accordance with the principles of the present invention; [Diagram 3] Photographs of a standard production barrel (i.e., smooth barrel) and a standard production combustion tube (i.e., smooth chamber) along with a structurally reinforced roughened barrel of the present invention (e.g., ribbed barrel) and a structurally reinforced roughened combustion tube of the present invention (e.g., ribbed chamber), each in a pre-operational state. [Figure 4] 1 shows photographs of a new smooth barrel and a new smooth combustion tube after undergoing the HVOF baseline test described in Comparative Example 1a. [Diagram 5] 1 shows photographs of a new ribbed barrel according to the principles of the present invention and a smooth chamber used in Comparative Example 1 after being subjected to HVOF testing as described in Example 1a. [Figure 6] 1 shows a photograph of a new ribbed chamber and a new smooth barrel according to the principles of the present invention after being subjected to HVOF testing as described in Example 2a. [Figure 7] 13 shows a photograph of the new ribbed barrel and ribbed chamber used in Example 2 in accordance with the principles of the present invention after being subjected to HVOF testing as described in Example 3a. [Figure 8] Photographs of a standard manufactured plasma anode (i.e., a smooth anode) after being subjected to plasma testing as described in Comparative Example 2 and of a new inventive structurally reinforced roughened plasma anode (e.g., a ribbed plasma anode) according to the principles of the present invention after being subjected to plasma testing as described in Example 4 are shown. [Figure 9] 1 shows photographs of a new inventive structurally reinforced roughened barrel (e.g., grit blasted barrel) and a new inventive structurally reinforced roughened combustion tube (e.g., grit blasted chamber) according to the principles of the present invention after being subjected to HVOF testing as described in Example 5. [Figure 10] 13 shows a photograph of the new smooth chamber and new ribbed barrel according to the principles of the present invention after being subjected to 40 hours of long-term HVOF testing as described in Example 6. [Figure 11] Photographs are shown of a smooth as-machined barrel subjected to previous testing and a new inventive structurally reinforced roughened combustion tube (e.g., knurled tube) according to the principles of the present invention after being subjected to HVOF testing as described in Example 7. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0011] Applicants have surprisingly discovered that modifications to existing exterior surfaces of one or more thermal spray components can result in a significant reduction in the buildup of scaled deposits and further improve the consistency of coating properties produced during operation of the modified thermal spray torch.

[0012] As used herein and throughout, "wet surface" means a surface that comes into direct or indirect contact with a cooling medium.

[0013] As used herein and throughout, "cooling medium" means any type of coolant suitable for circulation through a thermal spray apparatus, including, but not limited to, water-based coolants (eg, water).

[0014] As used herein and throughout, "smooth surface" refers to as-machined components, including standard OEM manufactured combustion tubes and standard OEM manufactured barrels, each of which has an outside diameter (OD) with an as-machined surface that is less than a surface finish of 84Ra.

[0015] "Ra" is a roughness parameter that refers to the average surface roughness, calculated as the arithmetic mean of the absolute values ​​of the profile heights over a mean line or evaluation length, and indicates the arithmetic mean profile height deviation from the mean line or evaluation length. In this specification and throughout, units are expressed in microinches unless otherwise indicated.

[0016] "Rz" is a roughness parameter that refers to the average absolute value of the heights of the five highest profile peaks and the depths of the five deepest arrays within a mean line or evaluation length, and typically represents a numerical value greater than Ra. In this specification and throughout, units are expressed in micrometers unless otherwise indicated.

[0017] "Gun" and "torch" have the same meaning as used herein and throughout, and may be used interchangeably to refer to a thermal spray device, including, but not limited to, an HVOF device, a plasma device, or a detonation gun (D-gun) device.

[0018] The present invention recognizes the shortcomings of existing thermal spraying devices, such as high velocity flame (HVOF) torches and plasma spray arc guns. For example, with respect to HVOF torches, applicants have observed that water fouling buildup (i.e., accumulation of scale deposits) on the exterior surfaces of the combustion chamber and barrel tends to occur when the exterior surfaces come into contact with cooling water during operation of the HVOF torch. In particular, minerals or other contaminants inherently present in the cooling water can be extracted from the cooling water and then deposited on the hot exterior surfaces as the cooling water flows directly or indirectly along such surfaces. Such scale deposit buildup acts as an insulating layer that can increase the heat generated in the combustion chamber and nozzle during operation of the thermal spray torch. As a result, the increased heat can no longer be adequately dissipated through the combustion chamber and barrel. Ultimately, the combustion chamber, barrel, and potentially other components of the HVOF torch operate at temperatures that exceed their respective maximum allowable design operating temperatures, thereby resulting in thermal failure of the torch. An example of a common thermal failure is surface melting. In the case of the barrel of an HVOF torch, the powder particles can become overheated and begin to accumulate on the interior surfaces they come into contact with, resulting in what is known as undesirable "barrel loading." Thermal damage can be exacerbated and can also cause harmful slag to build up on the coating workpiece.

[0019] Applicants have recognized the shortcomings of conventional HVOF torches and devised a solution to overcome them. The present invention emerged from the shortcomings of conventional HVOF torches. Figures 1a, 1b and 1c show an improved HVOF apparatus 100 according to the principles of the present invention. The improved HVOF apparatus 100 includes a combustion chamber 110 and a barrel 120. Figure 1b shows an enlarged view of an exterior surface 121 of the barrel 120 having structurally reinforced roughening features 140 therealong. Figure 1c shows an enlarged view of an exterior surface 109 of the combustion chamber 110 having structurally reinforced roughening features 141 therealong. The structurally reinforced features 140 and 141 are in direct or indirect contact with a cooling passage 160 through which cooling water or other suitable cooling medium flows. Applicants have discovered that structurally strengthened features 140 and 141 reduce the accumulation of water fouling buildup (i.e., scale deposits) along the barrel exterior surface 121 and chamber exterior surface 109, respectively, during operation of the improved HVOF apparatus 100.

[0020] Referring to FIG. 1a, during operation, a predetermined flow rate of fuel (e.g., a hydrocarbon fuel such as kerosene) is introduced into the fuel inlet 111 and a predetermined amount of oxygen is introduced into the oxygen inlet 112. An electric current is sent to an electrode of a spark plug 199, which causes the fuel to ignite and burn in the presence of oxygen in the combustion chamber 110. Combustion of the fuel occurs in the combustion chamber 110, generating combustion reaction products 113 (i.e., a flame). The heated flow of the combustion reaction products 113 is directed downstream of the barrel 120. Powder is injected at a radial location 130 shown in FIG. 1a. The powder particles contact the combustion reaction products 113 as they flow from the combustion chamber 110 toward the barrel 120. The molten particles with the combustion reaction products 113 exit the tip of the barrel 120. The powder particles melt as they move toward the surface of the substrate.

[0021] The large amount of heat generated during the combustion process requires sufficient cooling of the internal components of the HVOF device 100. Applicants have observed that the combustion reaction products 113 can accelerate the rate of scale deposition on the outer surface 121 of the barrel and the outer surface 109 of the combustion chamber 110. A cooling medium inlet 180 receives a cooling medium, such as cooling water. The cooling water flows through the HVOF device 100 as shown by the arrows. The cooling water enters the cooling passages 160 as shown in Figures 1b and 1c. The cooling passages 160 are located between the housing 170 and the outer surface 121 of the barrel 120 and between the housing 170 and the outer surface 109 of the combustion chamber 110. As the cooling water flows through the cooling passages 160, the cooling water extracts heat from the outer surface 121 of the barrel 120 and the outer surface 109 of the combustion chamber 110. At least a portion of the exterior surface 121 of the barrel 120 has a structurally reinforced roughened surface 140, and at least a portion of the exterior surface 109 of the combustion chamber 110 has a structurally reinforced roughened surface 141. The structurally reinforced roughened surfaces 140 and 141 are configured to reduce, eliminate, and / or inhibit the formation of fouling associated with mineral deposits in the cooling water that tend to accumulate on the corresponding exterior surfaces 121 and 109. The cooling water continues to flow through the HVOF device 100 and eventually exits the HVOF device 100 through the cooling medium outlet 181. Additional cooling water is reintroduced to continue cooling. The continuous flow of cooling water over the structurally reinforced roughened surfaces 140 and 141 allows for the effective transfer of heat from the barrel 120 and the combustion chamber 110, thereby preventing the melting of the surfaces or the occurrence of internal failures such as barrel loading.

[0022] It should be understood that while both outer surfaces 121 and 109 are shown having structurally reinforcing roughening features 140 and 141, the present invention also contemplates that only one of outer surfaces 121 or 109 has structurally reinforcing roughening features 140 or 141 provided along the outer surface 121 or 109.

[0023] The design of the present invention may be applicable to any thermal spray component that requires sufficient cooling during operation of the thermal spray device. Thus, while Figures 1a, 1b, and 1c show an HVOF device 100, it should be understood that other thermal spray devices may include one or more thermal spray components with structurally enhanced roughening features. By way of example, Figure 8 shows a photograph of a plasma torch 300 having an anode 310 with an outer surface 311 that includes a ribbed feature 320 having structural features similar to those shown in Figure 2. As will be described below in connection with Figure 2, the ribbed feature 320 prevents the buildup of scale from minerals in the cooling water on the outer surface 311 during operation of the plasma torch, whereas the as-machined surface of the plasma anode 312 is a relatively smooth, non-textured surface that is susceptible to scale buildup, as evidenced by the black scale in the photograph of Figure 8.

[0024] An exemplary structurally reinforced roughened surface is shown in FIG. 2. FIG. 2 shows a close-up view of an exterior surface 203 of a thermal sprayed component having a structurally reinforced roughened surface, characterized by a ribbed feature 200. The ribbed feature 200 can extend along a portion or the entirety of the exterior surface 203. The ribbed feature 200 is characterized by a predetermined depth 201, a predetermined number of helical threads per inch 203, and a groove angle 202. The predetermined depth 201 can be any suitable value required for a particular thermal spray application. By way of example, and not intended to be limiting, the depth 201 shown in FIG. 2 ranges from about 0.015 inches to about 0.025 inches. The helical threads 203 define the ribbed feature 200. In the example of FIG. 2, a total of 21 helical threads per inch define the pitch. Other threads per inch are contemplated to produce the required Ra and Rz values ​​in accordance with the present invention. The ribbed feature 200 further includes a groove angle 202, which is the angle measured between adjacent helical threads 203. The groove angle 202 in FIG. 2 is 55 degrees. Other suitable groove angles can be used to create the desired surface texture profile. The ribbed feature 200 shown in FIG. 2 is a design used by the applicant in the examples for both the HVOF and plasma devices described below. The ribbed feature 200 successfully prevents scale buildup during operation of the HVOF and plasma devices. The ribbed feature can have Ra values ​​ranging from greater than 84 up to 1000 or more as measured by a commercially available profilometer.

[0025] Other types of structurally enhanced roughening features 200 other than the ribbed features 200 are contemplated by the present invention. In one example, the exterior surface 121 of the barrel 120 and / or the exterior surface 109 of the combustion chamber 110 are grit blasted and textured profiles created using suitable commercially available abrasives. The grit blasted surface profile can have a predetermined roughness greater than that produced by an as-machined surface, which is generally smoother and characterized by the absence of a textured profile. The grit blasted profile can have an Ra value ranging from 100 to 500 or more as measured by a commercially available profilometer. FIG. 9 shows an example of an exterior surface of a chamber and an exterior surface of a barrel, both of which have grit blasted rough surfaces. The chamber has a portion of its exterior surface grit blasted, and the barrel has substantially the entirety of its exterior surface grit blasted. The outer diameter surface of the barrel was grit blasted and measured to have an Ra of 303 microinches (0.0003 inches) and an Rz of 1804 micrometers (0.0018 inches). Other Ra and Rz values ​​of the grit blasted profile can be used. Applicants have successfully demonstrated that HVOF equipment having chambers and barrels with grit blasted surface textures can withstand scale buildup. The grit blasted design can include any type of exterior surface that is appropriately surface roughened to impart a structurally enhanced roughening mechanism that can withstand scale buildup during operation of the HVOF equipment.

[0026] The exterior surfaces of the combustion chamber and barrel of conventional HVOF torches are "as-machined" components that are characterized by the absence of the required surface texture profile required by the principles of the present invention. Such finishes can be characterized as having an Ra of about 60 microinches or less.

[0027] In another example, the exterior surface 121 of the barrel 120 and / or the exterior surface 109 of the combustion chamber 110 are knurled rough. FIG. 11 shows an example of a photograph of a chamber having a portion of its exterior surface formed with a knurled rough texture having a raised profile. The knurled raised profile of FIG. 11 has a cut depth along its exterior surface ranging from about 0.012 inches to 0.015 inches. As described below, applicants have successfully demonstrated that an HVOF device having a chamber with a knurled surface texture can withstand scale buildup. Other knurled raised profiles can be used in accordance with the present invention. The knurling design can include any type of projection extending from the exterior surface to form a structurally reinforced roughened texture that can withstand scale buildup during operation of the HVOF device.

[0028] The above figures demonstrate that the present invention contemplates various structurally enhanced roughening features on the exterior surface of a thermal spray component that comes into direct or indirect contact with a cooling medium during operation of a thermal spray torch. The structurally enhanced roughening features of the present invention have an average surface roughness, referred to as Ra, of 84 or more, preferably 150 or more, and most preferably 250 or more.

[0029] Unexpected advantages of the present invention include the ability to produce coatings with more consistent properties compared to those produced using conventional thermal spray torches. The following examples demonstrate that certain coating properties, such as % porosity, deposition thickness, microhardness and residual stress, can be maintained relatively constant during a thermal spray operation using the improved and modified thermal spray apparatus of the present invention. In one embodiment, a method is provided for producing consistent coating properties during operation of the improved thermal spray apparatus. A high temperature energy source or plume is produced using an improved thermal spray apparatus including at least one thermal spray component having a wetting surface. The wetting surface has structurally enhanced roughening features therealong, which contacts a cooling medium directly or indirectly during operation of the improved thermal spray apparatus. A powder or wire feedstock is introduced into an inlet of the improved thermal spray apparatus. The powder or wire feedstock enters the thermal spray apparatus where it contacts the plume, thereby at least substantially melting the powder feedstock. A cooling medium is introduced into the improved thermal spray apparatus such that it contacts the wetting surface having structurally enhanced roughening features therealong. In a preferred embodiment, the cooling medium is water. The water cooling circuit can be supplied from a plant closed loop chilled water system. The substantially molten particles are directed onto a substrate to produce a coating. The coating includes at least one coating characteristic that exhibits less variation during operation of the improved thermal spray apparatus than that produced in a thermal spray apparatus that does not include the at least one thermal spray component having the structurally enhanced roughening feature. The at least one coating characteristic can include porosity, deposition thickness, microhardness, and residual stress.

[0030] Without being bound by any theory, applicants have determined that structurally roughened and enhanced features along the outer wetted surface prevent or substantially inhibit or reduce the formation of scaled deposits thereon. In the absence of fouling, the coating properties do not decay, but instead remain relatively constant during the coating process. Furthermore, the structurally enhanced features can maintain the same amount of heat within the powder particles, which means that the amount of heat transfer across the outer wetted surface is relatively constant. Conversely, without being bound by any theory, when fouling occurs along the outer wetted surface that remains machined and does not have a textured profile, the same coating properties decay as a result of the accumulation of scale and minerals extracted from the cooling medium. These findings are verified by applicants in the examples provided below.

[0031] Further unexpected advantages of the present invention include extended source life of thermal spray components having structurally reinforced roughening features, in which one of the examples described below demonstrates the ability of the structurally reinforced roughening features to withstand a total burn time of 40 hours without fouling along the exterior wetted surfaces having the structurally reinforced roughening features and without hot gas erosion on the interior of the component.

[0032] Additionally, applicants have discovered that the benefits of the present invention require only a single thermal spray component to be provided with the structurally enhanced roughening features. For example, an HVOF device in which only one of the combustion chamber and barrel has an exterior surface provided with the structurally enhanced roughening features can realize the benefits of extended source life and uniform coating properties.

[0033] While preferred embodiments of the present invention have been described above, the following tests are intended to provide a basis for comparing the present invention with conventional designs having smooth as-machined surfaces for the barrel and combustion tube, and should not be construed as limiting the present invention.

[0034] HVOF testing was performed at the PST TAFA Division site using a JP-8000 thermal spray system equipped with a Model 5220 HVOF thermal spray torch. Figure 3 shows photographs of the smooth barrel and smooth tube (conventional design) and the ribbed barrel and ribbed chamber (invention) in their pre-test condition. The water cooling circuit for the torch cooling water was the plant closed loop chilled water system. The parameters used for all tests were as follows:

[0035] Control Console Flow: Oxygen - 2000 scfh, Fuel - 6.5gph, Carrier - 26 scfh, Water-~10.9gpm

[0036] Gun Operation Traverse speed - 609mm / sec Incremental Step - 4mm Spray Distance - 14.5 inches

[0037] Coating material: Powder type - 88% by weight WC / 12% by weight Co Powder feed rate - 75 grams / min using a feed wheel rotation speed of 6.3 rpm

[0038] By maintaining constant parameters for all tests, a proper comparison of the present invention with conventional guns could be effectively performed. The gun shown in FIG. 1a (i.e., HVOF torch) represents the gun used for all tests described below. Oxygen was introduced into the oxygen inlet at 2000 scfh. Fuel was introduced into the fuel inlet at 6.5 gph. An electric current was sent to the electrode of the spark plug, which caused the fuel to ignite and burn in the presence of oxygen in the combustion chamber, producing combustion gases. This resulted in a flame. Tungsten carbide cobalt powder having the above composition was injected radially through a powder feeder at a rotational speed of 6.3 rpm to produce 75 grams / min of powder. A carrier gas at a flow rate of 26 scfh carried the powder from the powder feeder into the body of the gun. The powder particles were introduced into contact with the combustion gases as they traveled from the combustion chamber toward the barrel. The molten particles with the combustion gases flowed downstream from the combustion chamber into the barrel and then exited the tip of the barrel in an HVOF plume. The powder particles melted as they made their way to the surface of the substrate.Specific coating properties were measured at the start and end of the test to assess the variability of the specific coating properties.

[0039] Gun manipulation to apply the coating to the test samples was accomplished using a robotic system. The robotic system was programmed to operate according to the parameters listed above, allowing the gun to be maintained at a standoff distance of 14.5 inches from the substrate and traversed along it at a speed of 609 mm / sec during the coating pass. Upon completion of a coating pass, the robotic system incrementally moved the gun 4 mm upward or downward to allow the next coating pass to be made on the substrate.

[0040] Temperature control of the HVOF gun was achieved by controlling the circulation of cooling water through the torch at a flow rate of approximately 10.9 gpm. Cooling water from the TAFA plant was introduced into the cooling water inlet and flowed through the torch as shown by the flow arrows in Figure 1a. Heat from the combustion products in the barrel and in the combustion chamber was transferred to the cooling water. Additional heat from within the combustion chamber was extracted by the cooling water as it continued to flow through the cooling passages in the direction shown by the arrows.

[0041] A visual inspection of the barrel and chamber after each test run was performed to determine the extent of scale buildup along each outer diameter that may have occurred during the test run.

[0042] Comparative Example 1a (Baseline Conditions: HVOF Torch with Smooth Combustion Chamber and Smooth Barrel) The baseline test conditions consisted of a Model 5220 gun build with a standard OEM manufactured combustion tube and a standard manufactured gun barrel. The standard OEM manufactured components had a typical "smooth" as-machined finish (i.e., a finish of less than 84Ra) along the outside diameter (OD) surface. This smooth feature of the OD surface was in contact with the gun's cooling water during operation.

[0043] The gun was operated for a test period of just over 30 minutes using the procedure and parameters listed above to form a thermal spray coating. A thermal spray coating of the 88WC / 12Co powder was produced at the start of the run (i.e., about 2 minutes into the run) and at the end of the 30 minute "burn" cycle.

[0044] The barrel and chamber were removed from the gun for inspection, as shown in FIG. 4. Both the smooth barrel and the smooth chamber exhibited scale buildup on their respective OD surfaces. More than half of the surfaces of the smooth barrel and the smooth chamber were covered with scale deposits. The significant buildup of scale hindered the ability of the cooling water to extract internal heat. This was considered to be an undesirable condition. Given the significant amount of scale buildup during the relatively short test period, applicants expected that the internal surfaces of the gun would be hotter and, at some point, susceptible to damage in the form of surface melting and / or hot gas erosion.

[0045] Comparative Example 1b (Variation of Coating Properties from an HVOF Torch) The thermal spray coating produced in Comparative Example 1a was prepared for evaluation. All coating test samples were mounted on epoxy castable mounts and polished using a semi-automatic polisher. All samples were polished with the same settings.

[0046] The coating property results indicated that there was likely a heat gain imparted to the powder particles in the spray plume after the 30 minute test cycle. Table 1 below summarizes the variation in the measured coating properties. The observed decrease in porosity, hardness, and residual stress is indicative of more heat being retained in the flame due to reduced heat transfer to the cooling water. A decrease in deposition thickness was also noted from the start of the run to the end of the run. The observed cause of this possible heat gain was believed to be scaling contaminant buildup (fouling) on ​​the water jacket side of the combustion chamber and exterior of the barrel. This was believed to be an undesirable condition.

[0047] [Table 1]

[0048] Example 1a (HVOF torch of the present invention having a smooth combustion chamber and a ribbed barrel) In this test condition, a barrel having a "ribbed" feature on the OD surface in contact with the cooling water was attached to the gun. The smooth chamber used for this test was the same smooth surface chamber previously used in Comparative Example 1a. The gun was run for 30 minutes and metallurgical test samples were coated as described in Comparative Example 1a. After the 30 minute test, the ribbed barrel and smooth chamber were removed from the gun for inspection, as shown in Figure 5. The ribbed barrel showed no scale buildup. The ribbed finished barrel was found to have no scale buildup, which was the desired condition.

[0049] Example 1b (Variation of Coating Properties from an HVOF Torch of the Present Invention) The thermal spray coating produced in Example 1a was prepared for evaluation. All coating test samples were mounted on epoxy castable mounts and polished using a semi-automatic polisher. All samples were polished with the same settings.

[0050] As shown in Table 2, the test result values ​​for the Example 1b samples were substantially the same throughout the test period. The coating property results for this test condition showed much less deviation between the start and end of the 30 minute cycle coated test samples than those observed for Comparative Example 1b. In particular, the porosity variation from the start to the end of the test was reduced by only 11%, whereas the porosity variation from the start to the end of the test was reduced by 58%. The deposition variation from the start to the end of the test was reduced by only 0.7%, whereas the deposition variation from the start to the end of the test was reduced by 4.2% for Comparative Example 1b. The microhardness variation from the start to the end of the test was reduced by 2.5%, whereas the microhardness variation from the start to the end of the test was reduced by 4.2% for Comparative Example 1b. The residual stress variation from the start to the end of the test was reduced by 0%, whereas the residual stress variation from the start to the end of the test was reduced by 5.4% for Comparative Example 1b. The performance results were significantly improved over coatings produced by conventional HVOF torch designs.

[0051] In addition to the reduction in scale buildup as shown in Figure 5, Table 2 further verifies that heat transfer to the powder and spray plume was relatively consistent and unaffected by the use of the ribbed barrel over the 30 minute duration. The testing further demonstrates that having only a single thermal spray component with enhanced surface roughened features (e.g., ribbed features along the OD surface) can provide superior improvements in terms of reducing or eliminating scale buildup and producing uniform coating properties.

[0052] [Table 2]

[0053] Example 2a (HVOF torch of the present invention with ribbed combustion chamber and smooth barrel) For this test condition, the gun was equipped with a combustion chamber that had a ribbed feature on the OD surface that contacted the cooling water. The barrel used for this test condition was a standard production barrel with a smooth surface on the OD that contacted the cooling water.

[0054] The gun was run for 30 minutes and metallurgical test samples were coated as described below in Example 2b. After the 30 minute test, the smooth barrel and ribbed chamber were removed from the gun for inspection, as shown in FIG.

[0055] The ribbed chamber showed no scale buildup, which was a favorable condition. The smooth surfaced barrel showed significant scale buildup on the OD surfaces, which was an unfavorable result.

[0056] Example 2b (Variation of Coating Properties from an HVOF Torch of the Present Invention) The thermal spray coating produced in Example 2a was prepared for evaluation. All coating test samples were mounted on epoxy castable mounts and polished using a semi-automatic polisher. All samples were polished with the same settings.

[0057] The test result values ​​for the samples of Example 2b were substantially the same throughout the test period, as shown in Table 3 below. The coating property results for this test condition showed much less deviation between the start and end of the 30 minute cycle coated test samples than those observed for Comparative Example 1b. In particular, the porosity variation from the start to the end of the test was reduced by only 8.8%, while the porosity variation from the start to the end of the test was reduced by 58%. The deposition variation from the start to the end of the test was reduced by only 1.7%, while the deposition variation from the start to the end of the test was reduced by 4.2% for Comparative Example 1b. The microhardness variation from the start to the end of the test was reduced by 1.1%, while the microhardness variation from the start to the end of the test was reduced by 4.2% for Comparative Example 1b. The residual stress variation from the start to the end of the test was reduced by 4.7%, while the residual stress variation from the start to the end of the test was reduced by 5.4% for Comparative Example 1b. The performance results were significantly improved over coatings produced by conventional HVOF torch designs.

[0058] In addition to the reduction in scale buildup on the chamber as shown in Figure 6, Table 3 further verifies that over the course of 30 minutes, heat transfer to the powder and spray plume was relatively consistent and unaffected by the use of the ribbed chamber. The testing further demonstrates that having only a single thermal spray component with enhanced roughened surface features (e.g., ribbed features along the OD surface) can provide significant improvements in terms of reducing or eliminating scale buildup and producing uniform coating properties.

[0059] [Table 3]

[0060] Example 3a (HVOF torch of the present invention having a ribbed combustion chamber and a ribbed barrel) For this test condition, the gun was fitted with a chamber having a ribbed feature on the OD surface that comes into contact with the cooling water. The ribbed chamber for this test was the same as that used in Example 2a. The barrel used for this test condition was a ribbed barrel with a smooth surface on the OD that comes into contact with the cooling water.

[0061] The gun was run for 30 minutes and metallurgical test samples were coated as described below in Example 3b. After the 30 minute test, the ribbed barrel and ribbed chamber were removed from the gun for inspection, as shown in Figure 7. The ribbed chamber and ribbed barrel showed no scale build-up, which was a favorable condition.

[0062] Example 3b (Variation of Coating Properties from an HVOF Torch of the Present Invention) The thermal spray coating produced in Example 3a was prepared for evaluation. All coating test samples were mounted on epoxy castable mounts and polished using a semi-automatic polisher. All samples were polished with the same settings.

[0063] The test result values ​​for the samples of Example 3b were substantially the same throughout the test period, as shown in Table 4 below. The coating property results for this test condition had much less deviation between the start and end of the 30 minute cycle coated test samples than those observed for Comparative Example 1b. In particular, the porosity variation from the start to the end of the test increased by 34%, while the porosity variation from the start to the end of the test decreased by 58% for Comparative Example 1b. The deposition variation from the start to the end of the test decreased by only 0.8%, while the deposition variation from the start to the end of the test decreased by 4.2% for Comparative Example 1b. The microhardness variation from the start to the end of the test decreased by 1.4%, while the microhardness variation from the start to the end of the test decreased by 4.2% for Comparative Example 1b. The residual stress variation from the start to the end of the test increased by 8.6%, while the residual stress variation from the start to the end of the test decreased by 5.4% for Comparative Example 1b. With the exception of the higher residual stress variation, the performance results were significantly improved over coatings produced by conventional HVOF torch designs.

[0064] [Table 4]

[0065] Comparative Example 2 (Baseline Conditions: Plasma Torch with Smooth Anode) Plasma testing was performed on-site at the PST TAFA division using a Model 7700UPC system equipped with a Model SG100, 2086A extended plasma spray torch. The conventional plasma spray torch used a smooth as-machined surface finish along its outer diameter and had a surface finish of less than 32Ra. The modified plasma spray torch used a ribbed feature along the outer diameter of the anode.

[0066] The water cooling circuit for the torch cooling water was the plant closed loop cold water system. The parameters used for all tests were as follows:

[0067] Control Console Flow: Primary Gas - Argon: 150scfh Secondary Gas - Hydrogen: 3 scfh Carrier gas - Argon: NA (no powder feed used) Water: 5.4gpm

[0068] Operating Energy: Amperage 500 Voltage 54

[0069] Gun Operation: No metallurgical samples were produced. The gun was held in a stationary test stand.

[0070] By maintaining constant parameters for all testing, a proper comparison between the present invention and conventional guns could be effectively performed.

[0071] In conventional plasma torch operation, a potential was established between the positive and negative leads, creating an arc spanning the two. No powder was injected into the plasma torch. Rather, the plasma torch was held in a stationary test stand.

[0072] The gun was run for less than 30 minutes using the parameters listed above. Upon completion of the test cycle, the smooth anode was removed from the gun for visual inspection.

[0073] The smooth anode was found to have scale buildup on the outside diameter of its smooth surface, as shown in Figure 8. More than half of the outside surface was covered with scale buildup. This was considered to be an undesirable condition.

[0074] Example 4 (Plasma torch of the present invention having a ribbed anode) The smooth anode in the plasma torch used in Comparative Example 2 was replaced with an anode having a ribbed feature along the outside surface of its outer diameter. The gun was operated for just over 30 minutes using the same parameter settings as described in Comparative Example 2. No powder was injected into the plasma torch; rather, the plasma torch was held in a stationary test stand. Figure 8 shows that the ribbed anode did not form a buildup of scale along its outer surface, which was the desired condition.

[0075] Example 5 (HVOF Torch of the Present Invention with Grit Blasted Combustion Chamber and Grit Blasted Barrel) An HVOF torch with an alternative structurally enhanced roughening mechanism was tested. Specifically, both sides of the combustion chamber and the outer diameter of the barrel had a grit blasted profile. FIG. 9 shows a photograph of the chamber and barrel before testing. The outer diameter surface of the barrel was grit blasted with aluminum oxide abrasive. A portion of the outer diameter of the chamber was grit blasted with aluminum oxide abrasive. The grit blasted surface profile was measured to have an Ra of 303 microinches (0.0003 inches) and an Rz of 1804 micrometers (0.0018 inches). The test conditions consisted of using a Model 5220 gun build with a grit blasted chamber and a grit blasted barrel. The thermal spray system / equipment used for the test was a JP-8000 system with a Model 5220 HVOF thermal spray gun. The water cooling circuit for the gun cooling water used was the plant closed loop chilled water system.

[0076] The parameters used for the torch were as follows:

[0077] Control Console Flow: Oxygen - 2000 scfh, Fuel - 6.5gph, Carrier - 26 scfh, Water-~10.9gpm

[0078] Testing was conducted at the PST TAFA Division site. The gun was operated for just over 30 minutes using the parameters listed above. No metallurgical coating samples were produced in this evaluation. After testing was completed, the barrel and chamber were removed from the gun for visual inspection. The barrel and chamber were observed to be free of scale deposits on their respective grit blasted OD surfaces. These test results demonstrated that the grit blasted surface profile performed substantially equivalent to the ribbed surface feature. This was considered a desirable / positive condition.

[0079] Example 6 (Long Term Testing with an HVOF Torch of the Present Invention with a Ribbed Barrel and a Smooth Chamber) Testing prior to this particular long term test had been limited to 45 minute cycles or less. Therefore, long term testing using the previously described HVOF inventive torch was conducted to evaluate the build up of scale deposits (fouling) over extended periods of use. A 40 hour flame duration test was conducted. The chamber was a standard as machined OEM manufactured combustion tube. The barrel had a ribbed feature along the surface of its outer diameter as previously described.

[0080] The test conditions consisted of using a Model 5220 gun build with a smooth as-machined chamber and a ribbed barrel. The thermal spray system / equipment used for the test was a JP-8000 system with a Model 5220 HVOF thermal spray gun. The water cooling circuit for the gun cooling water used was the plant closed loop chilled water system.

[0081] The parameters used for the torch were as follows:

[0082] Control Console Flow: Oxygen - 2100 scfh, Fuel - 6.87gph, Carrier - 26 scfh, Water - ~11.1gpm

[0083] Testing was conducted at the PST TAFA Division site. The 40 hour test was conducted over a period of 8 days. To simulate typical end user operation, the torch was run with firing on for 15 minutes and then off for 5 minutes. This was repeated until 40 hours of accumulation was reached. After 40 hours of firing time was reached, the combustion tube and ribbed barrel were removed from the torch. The results are shown in FIG. 10. As expected, the combustion tube had quite significant scaling buildup. However, the ribbed barrel was found to be free of any fouling, confirming that the ribbed mechanism of the present invention protected the component surfaces from the buildup of scale buildup over extended operating conditions.

[0084] Example 7 (HVOF Torch of the Present Invention with Knurled Combustion Chamber and Smooth Barrel) An HVOF torch with an alternative structurally enhanced roughening mechanism was tested. Specifically, a portion of the outer diameter of the chamber was machined with the addition of a "knurled" surface as shown in Figure 11. The knurled raised profile had a cut depth that measured approximately 0.012 inches to 0.015 inches. The barrel had a smooth as-machined surface along its outer diameter as shown in Figure 11.

[0085] The remainder of the test parameters and test equipment were the same as those used in Example 5. No metallurgical coating samples were produced. The HVOF torch was operated to provide a burn duration of 60 minutes. After 60 minutes, the chamber was inspected. Figure 11 shows a photograph of the chamber and barrel. The chamber showed no scale buildup, which was a positive condition. The smooth barrel had scale buildup on its outer diameter surface.

[0086] While what are considered to be particular embodiments of the invention have been shown and described, it will of course be understood that various modifications and changes in form or detail can be readily made without departing from the spirit and scope of the invention. It is therefore intended that the invention not be limited to the exact forms and details shown and described herein, nor be limited to anything less than the full scope of the invention disclosed herein and claimed below.

Claims

1. An improved thermal spraying apparatus for use in producing a thermal spray coating, comprising: a high velocity fuel (HVOF) torch for spraying, the torch including a combustion chamber having an interior volume defined by an interior surface, the combustion chamber configured to receive oxygen and fuel and generate a heated flow therefrom to enable combustion reaction products to be produced in contact with the interior surface, the combustion chamber including a first exterior surface in contact with a cooling medium; a barrel operatively connected downstream of the combustion chamber, the barrel having an interior volume defined by an interior surface configured to contact the heated flow of the combustion reaction products and including a second exterior surface in contact with the cooling medium; Improved thermal spray apparatus, wherein at least one of the first exterior surface of the combustion chamber and the second exterior surface of the barrel features a structurally enhanced roughening feature, the structurally enhanced roughening feature configured to reduce accumulation of scale deposits on the first and / or second exterior surfaces when the first and / or second exterior surfaces are exposed to a cooling medium during operation of the HVOF torch.

2. The improved thermal spray component apparatus of claim 1 , wherein the structurally reinforced roughening features are contained along the second exterior surface of the barrel.

3. The improved thermal spray component apparatus of claim 1 , wherein the structurally reinforced roughening features are contained along the first exterior surface of the combustion chamber.

4. The improved thermal spray component apparatus of claim 1 , wherein the structurally reinforced roughening features are contained along the first exterior surface of the combustion chamber and the second exterior surface of the barrel.

5. 2. The improved thermal spray component apparatus of claim 1, wherein the structurally enhanced roughening features include a helical thread extending along all or a portion of the first and / or second exterior surface, the helical thread having a predetermined depth.

6. 10. The improved thermal spray component apparatus of claim 1, wherein said cooling medium is water-based.

7. 2. The improved thermal spray component apparatus of claim 1, wherein the structurally enhanced roughening features are characterized by an average surface roughness listed as greater than 84 (Ra) along the first exterior surface and / or the second exterior surface.

8. An improved thermal spraying apparatus for use in producing a thermal spray coating, comprising: A plasma torch for injection, the torch including a cathode arrangement and an anode, the anode having an exterior surface and an interior portion, the interior portion of the anode operatively connected to the cathode arrangement, and the exterior surface of the anode in fluid communication with a cooling medium; the outer surface of the anode characterized by structurally enhanced roughening features, the structurally enhanced roughening features configured to reduce the accumulation of scale deposits on the outer surface of the anode when exposed to a cooling medium during operation of the plasma torch; An improved thermal spray apparatus comprising:

9. 9. The improved thermal spray component apparatus of claim 8, wherein the structurally enhanced roughening features are characterized by an average surface roughness of the surface designated as (Ra) greater than 84.

10. 9. The improved thermal spray component apparatus of claim 8, wherein said cooling medium is water-based.

11. The improved thermal spray component apparatus of claim 8 , wherein the structurally enhanced roughened features extend helically along all or a portion of the exterior surface.

12. 1. An improved thermal spray component for use in a thermal spray apparatus to form a thermal spray coating, comprising: a body having a substantially tubular geometry, the substantially tubular geometry having a first end and a second end, a central longitudinal axis traversing the body from the first end to the second end, the body having a first surface adapted to be in contact with a plasma arc or combustion reaction products when the thermal spray component is operably connected within the thermal spray device, the body further having a second surface extending from the first end to the second end, the second surface configured to be in contact with a cooling medium during operation of the thermal spray device; structurally enhanced roughening features along at least a portion of the second surface, the structurally enhanced roughening features being oriented substantially parallel to the central longitudinal axis, the structurally enhanced roughening features being configured to reduce a buildup of scale deposits on the second surface when the second surface is exposed to the cooling medium during operation of the thermal spray device; Improved thermal spray component comprising:

13. The improved thermal sprayed component of claim 12 , wherein the first surface is an interior surface and the second surface is an exterior surface.

14. The improved thermal sprayed component of claim 12 , wherein the improved thermal sprayed component is an anode.

15. The improved thermal sprayed component of claim 12 , wherein the improved thermal sprayed component is a combustion chamber.

16. The improved thermal sprayed component of claim 12 , wherein the improved thermal sprayed component is a barrel.

17. The improved thermal spray component of claim 12 , wherein the structurally enhanced roughened features include a grit blasted profile along the second surface.

18. 13. The improved thermal sprayed component of claim 12, wherein the structurally enhanced roughened features are characterized by an average surface roughness along the second exterior surface listed as greater than 84 (Ra).

19. 13. The improved thermal sprayed component of claim 12, wherein the structurally enhanced roughened features include a knurled profile and the grooves extend circumferentially along the second surface in a spiral pattern.

20. 13. The improved thermal sprayed component of claim 12, wherein the structurally enhanced roughened features comprise grooves extending circumferentially along the second surface in a spiral pattern, the grooves being separated from one another by a predetermined distance, and the grooves further having a predetermined depth within the second surface.

21. 1. An improved thermal spray component for use in a thermal spray apparatus to form a thermal spray coating, comprising: a body having a substantially tubular geometry, the substantially tubular geometry having a first end and a second end, a central longitudinal axis traversing the body from the first end to the second end, the body having a first surface adapted to be in contact with a plasma arc or combustion reaction products when the thermal spray component is operably connected within the thermal spray device; The improved thermal spray component, wherein the body further has a second wetting surface extending from the first end to the second end, at least a portion of the second wetting surface including a structurally enhanced roughened feature configured to contact a cooling medium during operation of the thermal spray device.

22. 1. A method for producing consistent coating characteristics during operation of an improved thermal spray device, comprising: generating a high temperature energy source with an improved thermal spray apparatus including at least one thermal spray component having a wetting surface, the wetting surface having structurally enhanced roughened features therealong; introducing a powder or wire feedstock into an inlet of the improved thermal spray apparatus; heating the powder or wire feedstock to produce substantially molten particles; introducing a cooling medium into the improved thermal spray apparatus for contact along the wetting surface having the structurally enhanced roughened features; and directing the substantially molten particles onto a substrate to produce a coating, the coating comprising at least one coating characteristic that exhibits less variation during operation of the improved thermal spray device than a coating characteristic produced using a thermal spray device that does not include the at least one thermal spray component, the at least one coating characteristic being selected from the group consisting of porosity, deposition thickness, microhardness, and residual stress.

Citation Information

Patent Citations

  • Supersonic flame spraying spray gun

    CN201064747Y

  • Plasma spraying method

    JP1986119664A

  • Flame spray apparatus

    JP1990172551A

  • Thermal spraying apparatus using powder thermal spraying material

    JP2002273276A

  • Vaporization cooler

    JP2010266142A