Circuit board manufacturing method
By arranging ceramic substrates with metal sheets and using epoxy or silicone to fill gaps, and employing vapor deposition layers, the method enhances bonding strength and reduces etching complexity, leading to cost-effective and efficient circuit board manufacturing.
Patent Information
- Application Number
- JP2024535553
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2021-12-24
- Filing Date
- 2022-12-05
- Publication Date
- 2024-12-05
AI Technical Summary
Existing methods for manufacturing circuit boards using ceramic substrates face challenges in reducing production costs and addressing issues during the etching process of metal sheets.
A method involving the arrangement of multiple ceramic substrates side by side with metal sheets, filling gaps with epoxy or silicone, and using a diffusion bonding process with vapor deposition layers to enhance bonding strength and reduce etching complexity.
This approach results in a circuit board with improved bonding strength between ceramic substrates and metal sheets, reducing production costs and minimizing etching issues, while allowing for efficient production of more circuit boards in less time.
Smart Images

Figure 2024545223000001_ABST
Abstract
Description
[Technical field]
[0001] This embodiment relates to a method for manufacturing a circuit board. [Background technology]
[0002] Generally, a circuit board refers to a board on which wiring for connecting electric or electronic elements is arranged.
[0003] A circuit board can be manufactured by bonding metal sheets, such as copper sheets, to both opposing sides of a ceramic substrate, such as alumina (Al2O3), aluminum nitride (AlN), or silicon nitride (Si3N4).
[0004] There are three main bonding methods for circuit boards that use ceramic substrates: active metal brazing (AMB), which uses a bonding material made of active metal, direct bonding, which uses the oxide film on the ceramic substrate, and diffusion bonding, which uses metal deposition and a diffusion reaction.
[0005] The diffusion bonding method can form a thin deposition layer of several hundred nanometers thick through a solid-state reaction, and has the advantage that it uses a much smaller amount of metal than the active metal method and has excellent bonding strength, making it possible to manufacture printed circuit boards with excellent thermal shock properties. Summary of the Invention [Problem to be solved by the invention]
[0006] In this context, an object of the present invention is to provide a method for manufacturing a circuit board that can reduce production costs and solve problems that may occur during the etching process of a metal sheet. [Means for solving the problem]
[0007] In order to achieve the above-mentioned object, one embodiment provides a method for manufacturing a circuit board, including the steps of: arranging two or more ceramic substrates side by side on a plane; arranging the two or more ceramic substrates in a plane in which an upper metal sheet and a lower metal sheet face each other; injecting epoxy or silicone into gaps formed between the two or more ceramic substrates; bonding the upper metal sheet to the two or more ceramic substrates, and the lower metal sheet to the two or more ceramic substrates; and etching the upper metal sheet and the lower metal sheet.
[0008] In order to achieve the above-mentioned object, another embodiment provides a method for manufacturing a circuit board, including the steps of: arranging two or more ceramic substrates side by side on a plane; arranging the two or more ceramic substrates in a plane in which an upper metal sheet and a lower metal sheet face each other; inserting a metal block into a gap formed between the two or more ceramic substrates; bonding the upper metal sheet to the two or more ceramic substrates, and the lower metal sheet to the two or more ceramic substrates; and etching the upper metal sheet and the lower metal sheet. Effect of the Invention
[0009] As described above, according to the present embodiment, a printed circuit board having excellent bonding strength between a ceramic substrate and a metal sheet can be manufactured, the manufacturing cost can be reduced, and problems that may occur during the etching process of the metal sheet can be solved. [Brief description of the drawings]
[0010] [Figure 1] FIG. 1 is a diagram for explaining the positional relationship between a metal sheet and a ceramic substrate according to this embodiment. [Diagram 2]FIG. 2 is a diagram for explaining the injection of silicone or epoxy in the method for manufacturing a circuit board according to this embodiment. [Diagram 3] FIG. 3 is a diagram for explaining the insertion of a metal block in the method for manufacturing a circuit board according to the present embodiment. [Figure 4] FIG. 4 is a cross-sectional view of the ceramic substrate, the deposition layer, and the metal sheet according to the method for producing a circuit board according to the present embodiment. [Diagram 5] FIG. 5 is a diagram for explaining a bonding layer formed by the method for manufacturing a circuit board according to this embodiment. [Figure 6] FIG. 6 is a cross-sectional image of the ceramic substrate and deposition layer formed according to this embodiment, taken by a scanning electron microscope (SEM). [Figure 7] FIG. 7 is an image of a cross section of the ceramic substrate, the bonding layer, and the metal sheet formed in this example, taken with a scanning electron microscope (SEM). DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0011] FIG. 1 is a diagram for explaining the positional relationship between a metal sheet and a ceramic substrate according to this embodiment.
[0012] The method for manufacturing a circuit board according to this embodiment may use a ceramic substrate 100 and a metal sheet 200, and may additionally use an adhesion prevention sheet 300 for preventing adhesion of the metal sheet 200.
[0013] The method for manufacturing a circuit board according to this embodiment includes a step of arranging two or more ceramic substrates so that they are positioned side by side on a plane.
[0014] The ceramic substrate 100 can provide heat dissipation performance in a circuit board, and the ceramic substrate 100 is made of a component for providing heat dissipation performance. For example, the ceramic substrate 100 is made of Si3N 4、 It may include at least one of AlN and Al2O3.
[0015] The flexural strength of Si3N4 is generally in the range of 600 to 1,400 MPa, which is excellent. Si3N4 has a bending strength of about 3.2 × 10 -6 / K, it can be used at high temperatures. In addition, Si3N4 has a thermal expansion coefficient of about 3.2 g / cm 3 It can have a density of 0.01 mm, a thermal conductivity in the range of 30 to 178 W / (m·K), and high thermal shock resistance in the range of 800 to 1000 K.
[0016] The ceramic substrate 100 is manufactured through a process of preparing a slurry containing ceramic powder, a tape casting process, a punching process, a burnout process, a sintering process, and the like.
[0017] The slurry preparation process may be a process of preparing a slurry by mixing an organic solvent, a sintering aid, a plasticizer, and a dispersant with a powder. The ceramic powder may include at least one of Si3N4 powder, AlN powder, and Al2O3 powder. The ceramic powder may be prepared using a ball mill or the like, and the average particle size of the powder is formed to be 0.8 μm or less. The average particle size may refer to the size of a particle that is the median in the particle size distribution of n particles.
[0018] When Si3N4 powder is used for the ceramic substrate 100, the Si3N4 powder may include at least one of β-Si3N4 and α-Si3N4. When a mixture of β-Si3N4 and α-Si3N4 is used as the Si3N4 powder, the content ratio between the components is not particularly limited.
[0019] The type of organic solvent is not particularly limited, but one or more selected from the group consisting of toluene, benzene, xylene, methyl ethyl ketone (MEK), propylene glycol monomethyl ether acetate (PGMEA), propylene glycol monomethyl ether (PGME), ethanol, butanol, and methanol can be used.
[0020] The type of sintering aid is not particularly limited, and rare earth element oxides, alkaline earth metal oxides, and combinations thereof can be used.
[0021] The type of plasticizer is not particularly limited, but one or more selected from the group consisting of di-2-ethylhexyl phthalate, di-n-butyl phthalate, butyl phthalyl butyl glycolate, polyethylene glycol, and dioctyl phthalate can be used as the plasticizer.
[0022] The dispersant is not particularly limited, and one or more types selected from the group consisting of polyester-based dispersants, polyacrylate-based dispersants, polyurethane-based dispersants, and polyether-based dispersants can be used.
[0023] The tape casting process may involve coating the slurry at a consistent thickness onto a polymer film, which is then passed through a drying chamber to produce a ceramic tape.
[0024] The punching process may be a process of pressing and cutting a ceramic tape to produce a ceramic green sheet.
[0025] The burnout process may be a process performed by heat treating the ceramic green sheet. Specifically, the burnout process may be performed by heat treatment in air or nitrogen atmosphere. Specific heat treatment conditions are not particularly limited, but for example, the heat treatment may be performed at a temperature in the range of 400 to 800°C for 6 to 18 hours.
[0026] The sintering process may be a process of sintering the ceramic green sheet after the debinding process. The sintering process may be performed by gas pressure sintering (GPS). The specific gas pressure sintering conditions are not particularly limited, but a gas pressure sintering furnace having a temperature in the range of 1600 to 2000°C, a nitrogen atmosphere, and 8 to 12 atm conditions may be used in the sintering process.
[0027] After sintering, the product is processed by grinding and other post-processing to produce Si3N 4、 A ceramic substrate 100 is fabricated that includes one or more of AlN and Al2O3.
[0028] The ceramic substrate 100 may have a rectangular plate shape as shown in FIG. 1, or may have a polygonal, circular, elliptical, or other shape.
[0029] The size of the ceramic substrate 100 is not particularly limited, but may be 150 to 220 mm wide and 100 to 160 mm long. The size of the ceramic substrate 100 is variable in both width and length, specifically, it may be 138 mm wide and 190 mm long.
[0030] The thickness of the ceramic substrate 100 is not particularly limited, but may be formed to be 0.05 to 2.0 mm.
[0031] When two or more ceramic substrates 100 are used, each of the two or more ceramic substrates 100 may be the same or different in size and shape.
[0032] When two or more ceramic substrates 100 are used, the two or more ceramic substrates 100 are arranged to lie side-by-side in a plane, which may mean that the two or more ceramic substrates 100 do not overlap or stack on top of each other.
[0033] The lower surfaces of the two or more ceramic substrates 100 are all bonded to a lower metal sheet, and the upper surfaces of the two or more ceramic substrates 100 are all bonded to an upper metal sheet.
[0034] The method for manufacturing a circuit board according to this embodiment includes a step of arranging the two or more ceramic substrates 100 in a plane where an upper metal sheet and a lower metal sheet face each other.
[0035] Here, the upper metal sheet and the lower metal sheet are named according to the position where the metal sheet 200 is placed, and the upper metal sheet and the lower metal sheet may be interchanged depending on the direction from which the observer looks or the position where the metal sheet 200 is placed.
[0036] The area of the metal sheet 200 may be the same as or larger than the area of two or more ceramic substrates 100. Specifically, the area of the metal sheet 200 may be 6.0 times or less, 5.0 times or less, 4.0 times or less, 3.0 times or less, or 2.5 times or less, 1.5 times or more, 1.6 times or more, 1.7 times or more, 1.8 times or more, 1.9 times or more, or 2.0 times or more, and may be 2.4 times or less, 2.3 times or less, 2.2 times or less, or 2.1 times or less, of the area of the ceramic substrate 100.
[0037] If the area of the metal sheet 200 is too large, it may be difficult to wash off the etching solution, and problems may occur such as the etching solution accumulating on the substrate (residual etching solution) or uneven etching.
[0038] According to one example of this embodiment, when one side of the metal sheet 200 has a rectangular shape, the width may be 250 to 300 mm and the length may be 160 to 210 mm. The width and length of the metal sheet 200 may be interchangeable.
[0039] The thickness of the metal sheet 200 is not particularly limited, but may be in the range of 0.05 to 3.0 mm.
[0040] The metal contained in the metal sheet 200 is not particularly limited, but may include at least one of Cu, Al, Ni, and Fe.
[0041] The method for manufacturing a circuit board according to this embodiment includes the steps of bonding an upper metal sheet to two or more ceramic substrates, and bonding a lower metal sheet to two or more ceramic substrates.
[0042] The metal sheet 200 and the two or more ceramic substrates 100 may be bonded by forming a deposition layer on the ceramic substrate 100 and hot pressing the deposition layer, or may be bonded by using a bonding material, which will be described in detail later with reference to FIGS. 4 and 5.
[0043] In the method for manufacturing a circuit board according to the present embodiment, a step of etching the upper metal sheet and the lower metal sheet is performed.
[0044] The etching of the metal sheet 200 can be performed using an etching solution. Although not particularly limited, the etching solution used for etching the metal sheet 200 can be any known etching solution.
[0045] In this embodiment, a metal sheet 200 is used whose area is at least 1.5 times larger than that of the ceramic substrate 100. Etching is performed in the manufacture of circuit boards, and when two or more ceramic substrates are subjected to one etching process using the arrangement of this embodiment, the effective area increases, more etched pieces are produced, and at the same time, the amount of waste is reduced. In addition, since two substrates to be etched can be fed into the etching line at a time, rather than feeding them one by one, the process time is shortened and related costs (e.g., labor costs, etc.) are reduced.
[0046] According to one example of the present embodiment, with regard to the arrangement of the metal sheet 200 and the ceramic substrates 100, two or more ceramic substrates 100 are arranged on one side of the metal sheet 200 while being spaced apart from the edge of the metal sheet 200 by a predetermined distance. When spaced apart from the edge of the metal sheet 200, a location to be clamped by a jig during processing can be secured, and the distance between the two or more ceramic substrates 100 becomes closer, thereby reducing dead zones and preventing waste of raw materials.
[0047] The laminate having the structure of "metal sheet / two or more ceramic substrates / metal sheet" according to this embodiment can be called a set of master cards (MC).
[0048] According to one example of this embodiment, a master card laminate in which master cards are stacked can be manufactured, and in this case, an anti-adhesion sheet 300 is used between each set of master cards to prevent adhesion between the metal sheets 200.
[0049] The components of the adhesion prevention sheet 300 are not particularly limited, but may include graphite, and the adhesion prevention sheet 300 may be called a carbon plate.
[0050] FIG. 2 is a diagram for explaining the injection of silicone or epoxy in the method for manufacturing a circuit board according to this embodiment.
[0051] When two or more ceramic substrates 100 are arranged side by side on a plane by the method for manufacturing a circuit board according to the present embodiment, gaps are inevitably formed between the two or more ceramic substrates 100.
[0052] As a result, when performing the step of etching the metal sheet 200, the etching solution may flow into the gaps formed between two or more ceramic substrates 100, which may cause problems such as weakening the bonding strength between the metal sheet 200 and the ceramic substrates 100 or corrosion of the back surface of the metal sheet 200 (the surface bonded to the ceramic substrate).
[0053] Therefore, in the method for manufacturing a circuit board according to this embodiment, a step of injecting epoxy or silicone into gaps formed between two or more ceramic substrates 100 is performed.
[0054] Specifically, two or more ceramic substrates 100 may be arranged on opposing surfaces of the metal sheets 200, and one or more of epoxy or silicone may be injected into the gap formed between the two or more ceramic substrates 100 using an epoxy gun or a silicone gun.
[0055] In addition, one or more of epoxy and silicone are injected into both ends of the gap formed by the upper metal sheet, the lower metal sheet, and the two or more ceramic substrates 100. Both ends of the gap formed between the two or more ceramic substrates 100 may refer to end portions of the gap located at a cross section where the gap formed by the two or more ceramic substrates 100 is visible among the cross sections of the metal sheet / ceramic substrate / metal sheet laminate.
[0056] As a result, the gaps formed between two or more ceramic substrates 100 are filled with one or more of epoxy and silicone to fill the gaps, thereby preventing the etching solution from flowing into the gaps between the two or more ceramic substrates 100 during the etching process using the etching solution.
[0057] FIG. 3 is a diagram for explaining the insertion of a metal block in the method for manufacturing a circuit board according to the present embodiment.
[0058] As mentioned in the description of Figure 2, when two or more ceramic substrates 100 are arranged side by side on a plane by the method for manufacturing a circuit board according to this embodiment, gaps are inevitably formed between the two or more ceramic substrates 100.
[0059] As a result, when performing the step of etching the metal sheet 200, the etching solution may flow into the gaps formed between two or more ceramic substrates 100, which may cause problems such as weakening the bonding strength between the metal sheet 200 and the ceramic substrates 100 or corrosion of the back surface of the metal sheet 200 (the surface bonded to the ceramic substrate).
[0060] Therefore, in the method for manufacturing a circuit board according to this embodiment, a step of inserting a metal block 500 into a gap formed between two or more ceramic substrates 100 is performed.
[0061] Two or more ceramic substrates 100 are arranged on opposing surfaces of the metal sheet 200, and a metal block 500 is placed between the arranged ceramic substrates 100, thereby filling the gaps formed between the two or more ceramic substrates 100.
[0062] Specifically, the metal block 500 is inserted between two or more ceramic substrates 100, and after the metal block 500 is inserted, hot pressure is applied to the outside of the upper metal sheet and the lower metal sheet to bond the metal sheet 200 and the ceramic substrates 100, and the metal block 500 is deformed to fit the shape of the gap, filling the gap so that there is no space left.
[0063] The metal block 500 is formed of a metal that does not react with an etchant used in an etching process. The metal block 500 may include at least one of Fe, Ti, Ni, Mo, and W, but is not limited thereto.
[0064] The metal block 500 may be formed to have the same thickness as the ceramic substrate 100 or to have a thickness greater than that of the ceramic substrate 100 .
[0065] The metal blocks 500 are inserted into the gap formed by the upper metal sheet, the lower metal sheet and the two or more ceramic substrates 100, one at each end.
[0066] The two ends of the gap formed between two or more ceramic substrates 100 may refer to the end portions of the gap located at a cross section of the metal sheet / ceramic substrate / metal sheet laminate where the gap formed by the two or more ceramic substrates 100 is visible.
[0067] FIG. 4 is a cross-sectional view of the ceramic substrate, the deposition layer, and the metal sheet according to the method for producing a circuit board according to the present embodiment.
[0068] According to an example according to this embodiment, a deposition layer 400 is formed on an upper surface and a lower surface of the ceramic substrate 100, which may be referred to as an upper deposition layer and a lower deposition layer, respectively. The deposition layer 400 formed on the ceramic substrate 100 may have the same area as the ceramic substrate 100, or may have an area smaller than the area of the ceramic substrate 100. Specifically, the area of the deposition layer 400 may be 50% or 100% of the area of the ceramic substrate 100.
[0069] The material forming the deposition layer 400 is not particularly limited, and may include at least one of Ag and Ti. When at least one of Ag and Ti is used for the deposition layer 400, the deposition amount of Ag per unit area is 3.50 to 6.10 g / m 2 The deposition amount of Ti per unit area can be in the range of 0.61 to 1.30 g / m 2 Here, the deposition amount per unit area may refer to the content of the deposition component relative to the area of the deposition layer. The bonding strength of the deposition layer can be adjusted by adjusting the components used in the deposition layer and the deposition amount.
[0070] According to one example of this embodiment, the deposition amount of Ti contained in the deposition layer 400 per unit area is 0.61 to 1.30 g / m 2 In order to provide a stronger bonding strength between the metal sheet 200 and the ceramic substrate 100, the deposition amount of Ti per unit area may be in the range of 1.02 to 1.30 g / m 2 Specifically, the range is 1.04 to 1.20 g / m 2 The range may be:
[0071] The deposition amount of Ag contained in the deposition layer 400 per unit area is 3.50 to 6.10 g / m 2 In order to provide a stronger adhesive strength between the metal sheet 200 and the ceramic substrate 100, the deposition amount of Ag per unit area may be in the range of 4.00 to 4.60 g / m. 2 The range may be:
[0072] Furthermore, the deposition layer 400 formed on the upper and lower surfaces of the ceramic substrate 100 may have the same shape as the upper and lower surfaces of the ceramic substrate 100, or may have a different shape.
[0073] The process for forming the deposition layer 400 is not particularly limited, but may be a process such as sputtering for physical vapor deposition (PVD) or chemical vapor deposition (CVD).
[0074] Through the deposition layer forming process, an upper deposition layer and a lower deposition layer are formed on the upper and lower surfaces of the ceramic substrate 100, respectively.
[0075] The upper deposition layer is disposed to face the upper metal sheet, and the lower deposition layer is disposed to face the lower metal sheet. The deposition layer 400 can also serve as a medium for bonding the metal sheet 200 and the ceramic substrate 100 by hot pressing.
[0076] When two or more ceramic substrates 100 are used, the deposition layer 400 is formed on each of the two or more ceramic substrates 100, and the two or more ceramic substrates 100 and the metal sheet 200 are bonded together by hot pressing.
[0077] According to an example according to this embodiment, at least one of the upper deposition layer and the lower deposition layer may include a first deposition layer 410 and a second deposition layer 420 having different components.
[0078] Specifically, the first deposition layer 410 may include Ti, and the second deposition layer 420 may include Ag. The first deposition layer 410 may refer to a layer closer to the ceramic substrate 100 than the second deposition layer 420. For example, as shown in FIG 4, the first deposition layer 410 is formed on the ceramic substrate 100, and the second deposition layer 420 is formed on the first deposition layer 410.
[0079] With regard to the first deposition layer 410 and the second deposition layer 420, the manufacturing method of the circuit board according to this embodiment may include a step of forming a first deposition layer 410 containing Ti on the upper and lower surfaces of the ceramic substrate 100, respectively, and a step of forming a second deposition layer 420 containing Ag on the first deposition layer 410.
[0080] As a result, as shown in FIG. 1, a laminate is manufactured in which the second deposition layer 420, the first deposition layer 410, the ceramic substrate 100, the first deposition layer 410, and the second deposition layer 420 are sequentially arranged.
[0081] The first deposition layer 410 and the second deposition layer 420 may have the same area as the upper and lower surfaces of the ceramic substrate 100, or may have a smaller area, and may have the same shape or may be formed into different shapes.
[0082] The deposition amount of Ti contained in the first deposition layer 410 per unit area is 0.61 to 1.30 g / m 2 and the deposition amount of Ti per unit area is 1.02 to 1.30 g / m 2In order to provide a stronger bonding strength between the metal sheet 200 and the ceramic substrate 100, the range of 1.04 to 1.20 g / m 2 The range may be:
[0083] The deposition amount of Ag contained in the second deposition layer 420 per unit area is 3.50 to 6.10 g / m 2 The deposition amount of Ag per unit area on the side that provides stronger bonding strength between the metal sheet and the ceramic substrate can range from 4.00 to 4.60 g / m 2 The range may be:
[0084] The upper and lower metal sheets on which the deposition layer 400 is formed may be hot pressed to bond the ceramic substrate 100 to the upper and lower metal sheets.
[0085] The hot pressing is performed by hot pressing the upper and lower metal sheets in the direction of the ceramic substrate 100 at a temperature of 450 to 1,300° C. and a pressure of 1 to 25 MPa. The hot pressing is not particularly limited, but may be performed, for example, at a temperature of about 10 -1 ~10 -5 This is done at torr.
[0086] In this embodiment, the lower limit of the temperature during hot pressing may be 500° C. or more, 600° C. or more, 700° C. or more, or 800° C. or more, and the upper limit may be 1050° C. or less, 1000° C. or less, 950° C. or less, or 900° C. or less.
[0087] According to this embodiment, the lower limit of the pressure during hot pressing may be 5 MPa or more, or 10 MPa or more, and the upper limit may be 20 MPa or less, or 15 MPa or less.
[0088] In the method for manufacturing a circuit board according to this embodiment, two or more ceramic substrates 100 are used, and a deposition layer 400 is formed on two opposing surfaces of the ceramic substrate 100. Then, a metal sheet 200 is placed on the deposition layer 400, and the ceramic substrate 100 and the metal sheet 200 are bonded to each other by applying hot pressure to the outside of the metal sheet 200.
[0089] FIG. 5 is a diagram for explaining a bonding layer formed by the method for manufacturing a circuit board according to this embodiment.
[0090] The upper and lower metal sheets 200 and the ceramic substrate 100 may be bonded to each other by hot pressing using the deposition layer 400. As shown in Fig. 5, a bonding layer 430 is formed on the ceramic substrate 100, and the metal sheet 200 is disposed on the bonding layer 430. Here, the bonding layer 430 may refer to a layer formed by subjecting the deposition layer 400 or other bonding material to a bonding step.
[0091] Explaining this embodiment with reference to FIGS. 4 and 5, diffusion between materials contained in the ceramic substrate 100, deposition layer 400, and metal sheet 200 is caused by hot pressing.
[0092] For example, when the first deposition layer 410 contains Ti and the ceramic substrate 100 contains Si3N4, a reaction occurs between Ti and Si3N4 as shown in the following reaction formula 1.
[0093] [Reaction Scheme 1] 4Ti+Si3N4→3Si+4TiN That is, the material contained in the deposition layer 400 and the material contained in the ceramic substrate 100 react with each other by hot pressing to form the bonding layer 430, and the bonding layer 430 may include TiN.
[0094] The bonding layer 430 in one embodiment according to this embodiment is a layer containing TiN, and can act as a strong bonding medium layer between the ceramic substrate 100 and the metal sheet 200. That is, the bonding layer 430 is formed by a diffusion bonding method, thereby bonding the ceramic substrate 100 and the metal sheet 200.
[0095] When bonding layers containing different materials, stress is transferred to the layer containing the material with a relatively low strength, and delamination between the layers occurs easily. Therefore, increasing the strength of the layer containing the material with a relatively low strength is more effective in improving the bonding strength in bonding between layers containing different materials.
[0096] For example, Ag contained in the second deposition layer 420 can diffuse into the metal sheet 200 containing Cu during hot pressing to compensate for the weak strength of the metal sheet 200 at the interface. Based on the above principle, Ag contained in the second deposition layer 420 can improve the bonding strength between the ceramic substrate 100 and the metal sheet 200. In addition, Ag contained in the second deposition layer 420 can form a liquid phase consisting of a ternary system of Cu-Ti-Ag together with Ti contained in the first deposition layer 210 and Cu contained in the metal sheet 200 to improve wettability and support the promotion of reaction layer formation.
[0097] If the deposition amount per unit area of Ag included in the second deposition layer 420 is less than the range according to this embodiment, the strength of the metal sheet 200 cannot be sufficiently increased, and the bonding strength between the ceramic substrate 100 and the metal sheet 200 is deteriorated. If the deposition amount per unit area of Ag included in the second deposition layer 420 exceeds the range according to this embodiment, more Ag than necessary is deposited to form Ag remnants that are not diffused, which may result in a decrease in the bonding strength between the ceramic substrate 100 and the metal sheet 200.
[0098] The method for manufacturing a circuit board according to the present embodiment can manufacture a board having excellent interlayer adhesion, and therefore, even when the circuit board according to the present embodiment is exposed to a repeated thermal shock environment, peeling does not occur or peeling is greatly suppressed.
[0099] After the bonding step, the bonded ceramic substrate 100 and / or metal sheet 200 are subjected to a resist printing process, an etching process, a plating process, etc. to manufacture a circuit board.
[0100] FIG. 6 is a cross-sectional image of the ceramic substrate and deposition layer formed according to this embodiment, taken by a scanning electron microscope (SEM).
[0101] 6 is a cross-sectional image after the deposition step and before the bonding step, from which it can be seen that a first deposition layer 410 containing Ti and a second deposition layer 420 containing Ag were formed on the ceramic substrate 100.
[0102] FIG. 7 is an image of a cross section of the ceramic substrate, the bonding layer, and the metal sheet formed in this example, taken with a scanning electron microscope (SEM).
[0103] 7 is a cross-sectional image after the bonding step, from which it can be seen that a bonding layer 430 is formed after the bonding step using the diffusion bonding method, and the ceramic substrate 100 and the metal sheet 200 are bonded to each other.
[0104] The functions and effects of the present invention will be described in more detail below with reference to specific examples, however, these are presented as examples of the invention and are not intended to limit the scope of the invention in any way.
[0105] Manufacturing example (manufacturing ceramic substrates) A ball mill is used to produce Si3N4 powder with an average particle size of 0.8μm or less. Organic solvents (e.g. toluene, methanol, ethanol), sintering aids (e.g. Y2O3, MgO), plasticizers (e.g. dioctyl phosphate (DOP), polyethylen glycol (PEG)) and dispersants (e.g. BYK-111) are added to the Si3N4 powder to produce a slurry, which is then passed through a drying chamber to produce a Si3N4 tape. The Si3N4 tape is pressed and cut to produce a Si3N4 green sheet, which is then heat-treated at 600℃ for 12 hours to perform a degreasing process. The sheet is then sintered at 1850℃ and 1MPa in a nitrogen atmosphere using a gas pressure sintering method to produce a ceramic substrate (silicon nitride Si3N4 substrate) of a specified size (190mm wide x 138mm long x 0.32mm thick).
[0106] Experimental example 1: Confirmation of production cost reduction Ti (first deposition layer) and Ag (second deposition layer) were deposited in this order on the opposing upper and lower surfaces of the ceramic substrate of the manufacturing example. At this time, Ti was about 1.0 g / m 2 The Ag was evaporated at about 6.08 g / m 2 Two ceramic substrates were prepared as described above, on both of which the first and second deposition layers were deposited on the upper and lower surfaces facing each other.
[0107] In addition, two copper sheets measuring 270 mm x 190 mm x 0.3 mm were prepared.
[0108] One copper sheet was placed, and two ceramic substrates were placed adjacent to each other so that there was as little gap between them as possible, and then two ceramic substrates were placed on one side of the copper sheet (at this time, two or more ceramic substrates were placed parallel to each other on the copper sheet, and the deposition layer (Ag deposition layer) of each ceramic substrate was placed in contact with the copper sheet), and the remaining copper sheet was placed on top of them in the same manner to produce a non-bonded laminate in the form of copper sheet / two ceramic substrates (placed parallel to each other on the same plane) / copper sheet. At this time, the overlapping area between the two ceramic substrates and the copper sheet was about 90%.
[0109] Then, the laminate was heated for about 10 minutes in a hot press. ‐4 The treatment was carried out in a torr atmosphere at a temperature of 980°C under a pressure of 15 MPa. As a result, a sample was obtained in which the copper sheet and silicon nitride substrate were bonded to each other: copper sheet / two ceramic substrates (placed parallel to one another on a plane) / copper sheet.
[0110] Copper was etched to manufacture copper circuits using the above sample. Specifically, dry film was attached to both outer sides of the laminate, and then UV was irradiated onto the film, leaving only the areas where copper should not be etched (circuit areas), and the film was peeled off from the remaining areas other than the circuit areas. This was then fed into an etching line to perform copper etching.
[0111] As a result, it was confirmed that etching the sample manufactured according to the present application (copper sheet / two ceramic substrates (placed parallel to one another) / copper sheet) can reduce the time required to produce the same number of circuits by about half compared to etching two comparative samples (copper sheet / one ceramic substrate / copper sheet) in which ceramic substrates are bonded one by one, and can produce more circuit substrate pieces in the same etching process time (e.g., increase production by about 30% or more). Thus, the present application has a significant cost-saving effect.
[0112] Experimental example 2: Evaluation of bonding strength According to ASTM D6682, the bonding strength (N / mm) was measured for the test specimens of the following Examples 1 to 6 and Comparative Examples 1 to 6. Specifically, a sample of a copper sheet / silicon nitride substrate / copper sheet structure in which a copper sheet and a silicon nitride substrate were bonded to each other was etched to prepare a sample in which a copper strip with a width of 5 mm and a length of 100 mm was bonded to a ceramic substrate. Before the test, about 10 mm of the edge of the Cu strip was manually separated so that the Cu strip could be gripped by the grip of a universal testing machine (LS5 manufactured by Ametek). The test specimen was fixed to the universal testing machine, the Cu strip was gripped by the grip, and the stress on the grip was measured while separating at a speed of 50 mm / min, and the bonding strength was calculated.
[0113] The results are shown in Tables 1 to 3 below.
[0114] Example 1 (Ti deposition amount 1.076 g / m 2 , Ag deposition amount 4.005g / m 2 ) For the ceramic substrate of the manufacturing example, 0.0282 g of Ti was deposited for 70 seconds by sputtering to form a first deposition layer. Then, 0.105 g of Ag was deposited for 30 seconds on the first layer to form a second deposition layer. At this time, the formation area of the first and second deposition layers was adjusted to be the same as that of the ceramic substrate (190 mm wide x 138 mm long). Here, the deposition amount of Ti per unit area was 1.076 g / m 2 The deposition amount of Ag per unit area is 4.005 g / m 2 It is.
[0115] Two ceramic substrates and two copper sheets (270mm wide x 185mm long x 0.3mm thick) were prepared as described above. The two ceramic substrates were placed adjacent to each other to minimize the gap between them, and the two ceramic substrates were placed on one side of the prepared copper sheet (at this time, the two ceramic substrates were placed parallel to each other on the copper sheet, and the deposition layer (second deposition layer containing Ag) of each ceramic substrate was placed in contact with the copper sheet), and the remaining copper sheet was placed on top of them in the same manner to prepare a non-bonded laminate in the form of copper sheet / two ceramic substrates (placed parallel to each other on the plane) / copper sheet. At this time, the overlapping area between the two ceramic substrates and the copper sheet was about 95%.
[0116] Thereafter, the laminate was ‐4 The mixture was hot pressed at a temperature of 980°C and a pressure of 15 MPa in a torr atmosphere.
[0117] Through the above series of steps, a test specimen was fabricated, which included a Cu metal sheet, a TiN bonding layer, and Si3N4.
[0118] Example 2 (Ti deposition amount 1.194 g / m 2 , Ag deposition amount 4.005g / m 2 ) A test piece including a Cu metal sheet, a TiN bonding layer, and a Si3N4 ceramic substrate was manufactured in the same manner as in Example 1, except that 0.0313 g of Ti was deposited to form the first layer. At this time, the deposition amount of Ti per unit area was 1.194 g / m 2 The deposition amount of Ag per unit area is 4.005 g / m 2 It is.
[0119] Example 3 (Ti deposition amount 1.030 g / m 2 , Ag deposition amount 5.339g / m 2 ) A test piece including a Cu metal sheet, a TiN bonding layer, and a Si3N4 ceramic substrate was manufactured in the same manner as in Example 1, except that 0.0270 g of Ti was deposited to form the first layer, and 0.1400 g of Ag was deposited to form the second layer. At this time, the deposition amount of Ti per unit area was 1.030 g / m 2 The deposition amount of Ag per unit area is 5.339 g / m 2 It is.
[0120] Example 4 (Ti deposition amount 1.220 g / m 2 , Ag deposition amount 5.339g / m 2 ) A test piece including a Cu metal sheet, a TiN bonding layer, and a Si3N4 ceramic substrate was manufactured in the same manner as in Example 1, except that 0.0320 g of Ti was deposited to form the first layer, and 0.1400 g of Ag was deposited to form the second layer. At this time, the deposition amount of Ti per unit area was 1.220 g / m 2 The deposition amount of Ag per unit area is 5.339 g / m 2 It is.
[0121] Example 5 (Ti deposition amount 1.003 g / m 2 , Ag deposition amount 4.005g / m 2 ) A test piece including a Cu metal sheet, a TiN bonding layer, and a Si3N4 ceramic substrate was manufactured in the same manner as in Example 1, except that 0.0263 g of Ti was deposited to form the first layer. At this time, the deposition amount of Ti per unit area was 1.003 g / m 2 The deposition amount of Ag per unit area is 4.005 g / m 2 It is.
[0122] Example 6 (Ti deposition amount 0.961 g / m 2 , Ag deposition amount 4.005g / m 2 ) A test piece including a Cu metal sheet, a TiN bonding layer, and a Si3N4 ceramic substrate was manufactured in the same manner as in Example 1, except that 0.0252 g of Ti was deposited to form the first layer. At this time, the deposition amount of Ti per unit area was 0.961 g / m2 The deposition amount of Ag per unit area is 4.005 g / m 2 It is.
[0123] Comparative Example 1 (Ti deposition amount 0.374 g / m 2 , Ag deposition amount 2.868g / m 2 ) A test piece including a Cu metal sheet, a TiN bonding layer, and a Si3N4 ceramic substrate was manufactured in the same manner as in Example 1, except that 0.0098 g of Ti was deposited to form the first layer, and 0.0752 g of Ag was deposited to form the second layer. At this time, the deposition amount of Ti per unit area was 0.374 g / m 2 The deposition amount of Ag per unit area is 2.868 g / m 2 It is.
[0124] Comparative Example 2 (Ti deposition amount 0.599 g / m 2 , Ag deposition amount 2.868g / m 2 ) A test piece including a Cu metal sheet, a TiN bonding layer, and a Si3N4 ceramic substrate was manufactured in the same manner as in Example 1, except that 0.0157 g of Ti was deposited to form the first layer, and 0.0752 g of Ag was deposited to form the second layer. At this time, the deposition amount of Ti per unit area was 0.599 g / m 2 The deposition amount of Ag per unit area is 2.868 g / m 2 It is.
[0125] Comparative Example 3 (Ti deposition amount 0.843 g / m 2 , Ag deposition amount 2.868g / m 2 ) A test piece including a Cu metal sheet, a TiN bonding layer, and a Si3N4 ceramic substrate was manufactured in the same manner as in Example 1, except that 0.0221 g of Ti was deposited to form the first layer, and 0.0752 g of Ag was deposited to form the second layer. At this time, the deposition amount of Ti per unit area was 0.843 g / m 2 The deposition amount of Ag per unit area is 2.868 g / m 2 It is.
[0126] Comparative Example 4 (Ti deposition amount 1.034 g / m 2 , Ag deposition amount 2.868g / m 2 ) A test piece including a Cu metal sheet, a TiN bonding layer, and a Si3N4 ceramic substrate was manufactured in the same manner as in Example 1, except that 0.0342 g of Ti was deposited to form the first layer, and 0.0752 g of Ag was deposited to form the second layer. At this time, the deposition amount of Ti per unit area was 1.304 g / m 2 The deposition amount of Ag per unit area is 2.868 g / m 2 It is.
[0127] Comparative Example 5 (Ti deposition amount 1.041 g / m 2 , Ag deposition amount 6.808g / m 2 ) A test piece including a Cu metal sheet, a TiN bonding layer, and a Si3N4 ceramic substrate was manufactured in the same manner as in Example 1, except that 0.0273 g of Ti was deposited to form the first layer, and 0.1785 g of Ag was deposited to form the second layer. At this time, the deposition amount of Ti per unit area was 1.041 g / m 2 The deposition amount of Ag per unit area is 6.808 g / m 2 It is.
[0128] Comparative Example 6 (Ti deposition amount 0.599 g / m 2 , Ag deposition amount 4.005g / m 2 ) A test piece including a Cu metal sheet, a TiN bonding layer, and a Si3N4 ceramic substrate was manufactured in the same manner as in Example 1, except that 0.0157 g of Ti was deposited to form the first layer. At this time, the deposition amount of Ti per unit area was 0.599 g / m 2 The deposition amount of Ag per unit area is 4.005 g / m 2 It is.
[0129] [Table 1]
[0130] [Table 2]
[0131] [Table 3]
[0132] First, comparing the test pieces of Examples 1 and 2 and Comparative Examples 1 to 4, the deposition amount of Ag per unit area was 3.50 g / m 2 The test pieces of Examples 1 and 2 showed excellent bonding strengths of 21.4 N / mm and 22.1 N / mm, respectively, but the deposition amount of Ag per unit area was 3.50 g / m 2 The test pieces of Comparative Examples 1 to 4, which are less than 7.5 N / mm, all showed low bonding strengths of 7.5 N / mm or less. In particular, although the amount of Ti deposited per unit area of the test piece of Comparative Example 4 was higher than that of the test pieces of Examples 1 and 2, the test piece of Comparative Example 4 showed a much lower bonding strength due to its low Ag content. This is considered to be the result of the strength of the metal sheet changing (improving) depending on the amount of Ag deposited. Next, comparing the test pieces of Examples 1 and 3 and Comparative Example 5, there is no significant difference in the amount of Ti deposited per unit area. However, the amount of Ag deposited per unit area of 6.10 g / m 2 The test pieces of Examples 1 and 3 below showed excellent adhesion strengths of 21.4 N / mm and 16.3 N / mm, respectively, while the test piece of Comparative Example 5 showed a decreased adhesion strength of 15.6 N / mm. This is believed to be due to the formation of Ag residue at the interface caused by excessive Ag deposition.
[0133] Next, comparing the test pieces of Examples 1, 2, 5, and 6 and Comparative Example 6, the deposition amount of Ag per unit area is almost the same. The deposition amount of Ti per unit area is 0.61 g / m 2 The test pieces of Examples 1, 2, 5, and 6 showed a minimum bonding strength of 9.4 N / mm or more, but the deposition amount of Ti per unit area was 0.61 g / m 2The test piece of Comparative Example 6, which has a bonding strength of less than 8.6 N / mm, exhibited a low bonding strength of less than 8.6 N / mm. This is believed to be the result of the strength of the bonding layer changing (improving) depending on the amount of Ti deposition. In particular, when the amount of Ti deposition per unit area was 1.02 g / m 2 The test pieces of Examples 1 and 2 exhibited excellent bonding strengths of 21.4 N / mm and 22.1 N / mm, respectively.
[0134] Next, looking at the test pieces of Examples 1, 2, and 4, the deposition amount of Ti per unit area was 1.30 g / m 2 The test pieces of Examples 1, 2, and 4 below all showed excellent bonding strength of 20 N / mm or more. However, the deposition amount of Ti per unit area was 1.02 g / m 2 Above this level, it can be confirmed that the increase in the amount of Ti deposition is so small that the bonding strength reaches a saturation value. Therefore, in order to prevent the cost of raw materials from being wasted and to provide optimal bonding strength between the interfaces, the amount of Ti deposition per unit area is set to 1.30 g / m 2 It is preferable that:
Claims
1. Positioning two or more ceramic substrates side-by-side in a plane; placing the two or more ceramic substrates in opposing planes with an upper metal sheet and a lower metal sheet; injecting an epoxy or silicone into a gap formed between the two or more ceramic substrates; bonding the upper metal sheet to the two or more ceramic substrates and the lower metal sheet to the two or more ceramic substrates; Etching the upper metal sheet and the lower metal sheet; A method for manufacturing a circuit board, comprising:
2. The method for manufacturing a circuit board according to claim 1 , wherein the two or more ceramic substrates each have an upper deposition layer and a lower deposition layer.
3. The method for manufacturing a circuit board according to claim 2 , wherein the upper deposition layer and the lower deposition layer contain Ag and Ti.
4. A bonding layer is formed by reacting a material contained in the upper deposition layer and the lower deposition layer with a material contained in the ceramic substrate by hot pressing, The method for manufacturing a circuit board according to claim 2 , wherein the bonding layer contains at least TiN.
5. The deposition amount of Ag per unit area is 3.50 to 6.10 g / m 2 is in the range The deposition amount of Ti per unit area is 0.61 to 1.30 g / m 2 The method for manufacturing a circuit board according to claim 3, wherein the thickness of the circuit board is in the range of 0.1 to 1.0 mm.
6. The method of claim 1 , wherein the areas of the upper metal sheet and the lower metal sheet are the same as or larger than the two or more ceramic substrates.
7. The method of claim 1 , wherein the joining step is performed by hot pressing the upper metal sheet and the lower metal sheet together.
8. The ceramic substrate is Si 3 N 4、 AlN and Al 2 O 3 The method for manufacturing a circuit board according to claim 1 , further comprising at least one of the steps of:
9. The method of claim 1 , wherein the upper metal sheet and the lower metal sheet include at least one of Cu, Al, Ni, and Fe.
10. The method of claim 1 , wherein the epoxy or silicone is injected into both ends of the gap formed by the upper metal sheet, the lower metal sheet and the two or more ceramic substrates.
11. Positioning two or more ceramic substrates side-by-side in a plane; placing the two or more ceramic substrates in opposing planes with an upper metal sheet and a lower metal sheet; inserting a metal block into a gap formed between the two or more ceramic substrates; bonding the upper metal sheet to the two or more ceramic substrates and the lower metal sheet to the two or more ceramic substrates; Etching the upper metal sheet and the lower metal sheet; A method for manufacturing a circuit board, comprising:
12. The method for manufacturing a circuit board according to claim 11 , wherein the metal block is a metal that does not react with an etching solution used in the etching.
13. The method for manufacturing a circuit board according to claim 11 , wherein the metal block includes at least one of Fe, Ti, Ni, Mo, and W.
14. The method of claim 11, wherein the thickness of the metal block is equal to or greater than the thickness of the two or more ceramic substrates.
15. The method of claim 11 , wherein the metal blocks are inserted into both ends of the gap formed by the upper metal sheet, the lower metal sheet, and the two or more ceramic substrates, one at a time.