Fabrication of low linewidth W-type hexagonal microwave ferrite material

By replacing Fe ions with Gd and using low melting point fluxes, the method addresses high linewidth issues in hexagonal ferrite materials, achieving a low linewidth and high density suitable for miniaturized radar components.

JP2024545267AActive Publication Date: 2024-12-05HENGDIAN GRP DMEGC MAGNETICS CO LTD
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
JP2024536272
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2022-06-29
Filing Date
2023-05-25
Publication Date
2024-12-05
Estimated Expiration
2043-05-25

AI Technical Summary

Technical Problem

Current hexagonal ferrite materials exhibit high ferromagnetic resonance linewidths and high losses, hindering their ability to meet the demands of miniaturization and integration in active phased array radar components.

Method used

A method for manufacturing a W-type hexagonal microwave ferrite material with low linewidth by replacing some Fe ions with the rare earth element Gd and using a specific chemical formula, along with low melting point fluxes like Bi2O3, V2O5, SiO2, and ZnO, to improve microstructure and reduce porosity.

Benefits of technology

The method achieves a stable process with good reproducibility, resulting in a W-type hexagonal microwave ferrite material with a line width of <400 Oe and a density >5.0 g/cm³, suitable for large-scale production and integration in miniaturized components.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024545267000001
    Figure 2024545267000001
  • Figure 2024545267000002
    Figure 2024545267000002
  • Figure 2024545267000003
    Figure 2024545267000003
Patent Text Reader

Abstract

This paper discloses a method for producing a W-type hexagonal microwave ferrite material with low linewidth. The method includes weighing → first ball milling → drying → first sintering → second ball milling → granulation molding → second sintering to obtain a W-type hexagonal microwave ferrite material with low linewidth. The method of the present application replaces some Fe ions with rare earth element Gd, and obtains appropriate saturation magnetization, remanence and linewidth by utilizing the electromagnetic properties and compensation points of Gd and Fe, and also adds an appropriate amount of low melting point fluxes Bi2O3, V2O5, SiO2 and ZnO to improve the microstructure of the W-type hexagonal microwave ferrite material, reduce pores, reduce linewidth and increase remanence. The method of the present application has a stable process, good reproducibility and is suitable for mass production.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The embodiments of the present application relate to the field of magnetic materials, for example, the fabrication of low linewidth W-type hexagonal microwave ferrite materials. [Background technology]

[0002] With the rapid development of electronic information technology, the importance of radar in military and civilian applications is increasing day by day. Here, active phased array radar adopts a large number of radiating units arranged in the form of an array, and a transmitting and receiving component is connected to each of the multiple radiating units on the antenna array surface. The transmitting and receiving component is the core member of the active phased array radar antenna array element, and it is necessary to complete the transmission and reception of RF signals with a very small volume limit. Although the component is highly integrated by monolithic microwave integrated circuit technology, it is limited by the size of the circulator and cannot be sufficiently miniaturized and chipped. Due to its non-reciprocity, the circulator is an essential part that connects the three modules of the transmitter, antenna and receiver in the transmitting and receiving component. However, the traditional circulator designed based on garnet and spinel ferrite needs to provide a bias magnetic field by externally attaching a large-sized permanent magnet to realize the circulation function, and the higher the operating frequency of the circulator, the larger the volume of the permanent magnet required. Therefore, reducing the size of the circulator is an unavoidable important issue to realize further miniaturization and integration of the transmitting and receiving components.

[0003] CN106747391A discloses a method for manufacturing a circulator substrate based on a casting process, which includes the following steps: 1. Main raw material recipe: Y 3-x Ca x Sn x Fe 5-x O 12(x=0.06) is adopted; 2. Primary ball milling; 3. Pre-calcination: Pre-calcination at 1000℃~1200℃ and kept warm for 1~3 hours; 4. Doping: Add additives of 0.2wt% Bi2O3 and 0.10wt% BaTiO3; 5. Secondary ball milling: Add 40~50wt% organic binder and 40~50wt% anhydrous ethanol to the powder material and ball mill for 4~8 hours; 6. Casting: Obtain green film tape with a thickness of 100~120μm by casting the slurry; 7. Lamination: Depending on the thickness needs, laminate the green film tape into 8~15 layers and press mold at 6MPa; 8. Sintering: Keep warm in air atmosphere at 1360~1440℃ for 4 hours. This method of manufacturing allows for the production of smooth ferrite dielectric substrates for circulators with different thicknesses, and has the advantages of being suitable for the X-band, good temperature stability, small line width, low dielectric loss, etc.

[0004] CN102584200A discloses an ultra-low loss, fine linewidth microwave ferrite material and its manufacturing method, the main phase of the material is a garnet structure, and the chemical formula is Y 3-2x-y Ca 2x+y Fe 5-x-y-z V x Zr y Al z O 12 where 0.02≦x≦0.25, 0.05≦y≦0.25, 0.01≦z≦0.25. The manufacturing method includes the steps of stoichiometrically calculating and weighing the raw materials, and then performing vibration ball milling, calcination, coarse grinding with a vibration mill, fine grinding with a sand mill, spray granulation, press molding and sintering. Tests have shown that the ferromagnetic resonance linewidth ΔH of the obtained material is 1.27KA / m, and the dielectric loss tgδe is 0.5×10 -4 The insertion loss of the mounted microwave device is ≦0.21 dB, and its stability and reliability are greatly improved and its application range is expanded. The fabricated microwave ferrite device has the advantages of wide operating band and low insertion loss.

[0005] CN111732427A discloses a hexagonal ferrite material with low ferromagnetic resonance linewidth for self-biased circulators, which is composed of a main component and a doping component, where the main component includes (6.5-7) mol Fe2O3, (1-1.17) mol BaCO3, and (0-1) mol Ga2O3, and the doping component includes (0.01-1) wt% CuO, (0.01-3) wt% Bi2O3, and (0.01-1.5) wt% B2O3. The present invention further discloses a method for manufacturing the above-mentioned material, and the manufactured material has a high anisotropy magnetic field, a high saturation magnetization, a low ferromagnetic resonance linewidth and a suitable coercive force. The manufacturing method is simple and easy to operate. Since the material has a high anisotropy magnetic field, it can replace an external permanent magnet in a circulator, reduce the size of the circulator, and improve the operating frequency of the device. The low ferromagnetic resonance linewidth can effectively reduce the loss of a self-biased circulator.

[0006] Current hexagonal ferrite materials have high ferromagnetic resonance linewidths and high losses, making them unable to meet new engineering demands.

[0007] Therefore, the development of a manufacturing method for W-type hexagonal microwave ferrite material with low linewidth is of great significance. Summary of the Invention [Problem to be solved by the invention]

[0008] The following is a brief summary of the subject matter described in greater detail in the present text. This summary does not limit the scope of the claims. [Means for solving the problem]

[0009] To solve the above technical problems, an embodiment of the present application provides a method for manufacturing a W-type hexagonal microwave ferrite material with a low linewidth, replacing some Fe ions with a rare earth element Gd, and utilizing the electromagnetic properties and compensation points of Gd and Fe to obtain appropriate saturation magnetization, residual magnetic permeability, and linewidth. Moreover, by adding an appropriate amount of low melting point fluxes Bi2O3, V2O5, SiO2, and ZnO, the microstructure of the W-type hexagonal microwave ferrite material is improved, pores are reduced, the linewidth is reduced, and the residual magnetic permeability is increased. The manufacturing method according to the present application has a stable process, good reproducibility, and is suitable for mass production.

[0010] An embodiment of the present application is a method for manufacturing a W-type hexagonal microwave ferrite material with a low linewidth, comprising: chemical formula BaGd x Ni2Fe (16~x) O 27 (where 0.1 < x < 0.25), after calculating and weighing the raw materials BaCO3, Gd2O3, Ni2O, and Fe2O3, performing a first ball milling process to obtain a slurry after the first ball milling with a particle size X50 of 0.9 - 1.2 μm in step (1); sequentially performing drying and a first sintering process at a temperature of 1200 - 1280 °C on the slurry after the first ball milling to obtain a mixed powder material in step (2); mixing the mixed powder material with fluxes, performing a second ball milling process to obtain a slurry after the second ball milling with a particle size X50 of 0.8 - 1.1 μm, and the composition and mass % of the fluxes are respectively Bi2O3: 0.01 - 0.1%, V2O5: 0.01 - 0.1%, SiO2: 0.01 - 0.1%, and ZnO: 0.01 - 0.1% in step (3); sequentially performing granulation molding and a second sintering process on the slurry after the second ball milling to obtain the W-type hexagonal microwave ferrite material with a low linewidth, the second sintering process includes performing air sintering and then oxygen sintering at a temperature of 1150 °C - 1250 °C, and the linewidth of the W-type hexagonal microwave ferrite material with a low linewidth is < 400 Oe in step (4). A manufacturing method is provided.

[0011] The manufacturing method of the low line-width W-type hexagonal microwave ferrite material according to the present application replaces some Fe ions with the rare earth element Gd, and the chemical formula is BaGd x Ni2Fe (16~x) O 27 in which 0.1 < x < 0.25 is limited, and by utilizing the electromagnetic properties and compensation points of Gd and Fe, appropriate saturation magnetization, residual magnetic permeability, and line width are obtained. Moreover, by adding, in mass percentage, Bi2O3: 0.01 - 0.1%, V2O5: 0.01 - 0.1%, SiO2: 0.01 - 0.1%, and ZnO: 0.01 - 0.1% together with low melting point fluxes, the microstructure of the W-type hexagonal microwave ferrite material is improved, pores are reduced, the line width is reduced, and the residual magnetic permeability is increased. The manufacturing method according to the present application further employs oxygen sintering at a temperature of 1150°C - 1250°C to reduce the pores of the W-type hexagonal microwave ferrite material, effectively reduce its line width, and suppress the appearance of Fe 2+ and prevent the reduction of the dielectric loss of the material.

[0012] The manufacturing method according to the present application further limits the particle size X50 of the slurry after the first ball milling treatment to 0.9 - 1.2 μm and the particle size X50 of the slurry after the second ball milling treatment to 0.8 - 1.1 μm. Its role is to make most of the particles in the single-domain state, contribute to the rolling of the magnetic moment under the action of the orientation magnetic field, obtain a good orientation effect, improve the residual magnetic permeability, and effectively reduce the porosity. Furthermore, the temperature of the first sintering treatment is 1200 - 1280°C. When the temperature is lower than 1200°C, the grain size of the crystal grains has not fully grown, the density is low, the porosity is increased, and the line width is increased. When the temperature is higher than 1280°C, crystal grains of excessive size appear, pores increase, the residual magnetic permeability decreases, and the line width is increased.

[0013] In the present application, x is 0.1 < x < 0.25. For example, it may be 0.11, 0.13, 0.15, 0.18, 0.2, or 0.24, etc., but it is not limited to the listed numerical values, and other unlisted numerical values within this numerical range are similarly applicable.

[0014] The particle size X50 of the slurry after the first ball milling process is 0.9 to 1.2 μm, and may be, for example, 0.9 μm, 0.95 μm, 1 μm, 1.05 μm, 1.1 μm, or 1.2 μm, but is not limited to the recited values, and other unrecited values ​​within the numerical range also apply.

[0015] The temperature of the first sintering process is 1200 to 1280°C, and may be, for example, 1200°C, 1210°C, 1220°C, 1250°C, 1270°C, or 1280°C, but is not limited to the listed values, and other unlisted values ​​within the numerical range also apply.

[0016] The particle size X50 of the slurry after the second ball milling process is 0.8 to 1.1 μm, and may be, for example, 0.8 μm, 0.85 μm, 0.9 μm, 0.95 μm, 1 μm, or 1.1 μm, but is not limited to the recited values, and other unrecited values ​​within the numerical range also apply.

[0017] The composition and mass% of the flux are Bi2O3: 0.01-0.1%, V2O5: 0.01-0.1%, SiO2: 0.01-0.1%, and ZnO: 0.01-0.1%. However, Bi2O3 is 0.01-0.1%, and may be, for example, 0.01%, 0.02%, 0.04%, 0.05%, 0.08%, or 0.1%, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable. V2O5 is 0.01-0.1%, and may be, for example, 0.01%, 0.02%, 0.04%, 0.05%, 0.08%, or 0.1%, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable. SiO2 may be 0.01-0.1%, for example, 0.01%, 0.02%, 0.04%, 0.05%, 0.08%, or 0.1%, but is not limited to the recited values, and other unrecited values ​​within the range apply as well. ZnO may be 0.01-0.1%, for example, 0.01%, 0.02%, 0.04%, 0.05%, 0.08%, or 0.1%, but is not limited to the recited values, and other unrecited values ​​within the range apply as well.

[0018] The temperature of the oxygen sintering is 1150°C to 1250°C, and may be, for example, 1150°C, 1155°C, 1180°C, 1200°C, 1220°C, or 1250°C, but is not limited to the recited values, and other unrecited values ​​within the range apply as well.

[0019] The linewidth of the low linewidth W-type hexagonal microwave ferrite material may be <400 Oe, for example, 399 Oe, 390 Oe, 380 Oe, 370 Oe, 350 Oe, or 320 Oe, but is not limited to the recited values, and other unrecited values ​​within the numerical range also apply.

[0020] Preferably, the rotation speed of the first ball milling process described in step (1) is 60 to 80 r / min, and may be, for example, 60 r / min, 62 r / min, 65 r / min, 70 r / min, 75 r / min, or 80 r / min, but is not limited to the enumerated values, and other unenumerated values ​​within the numerical range also apply.

[0021] Preferably, the time for the first ball milling treatment is 20 to 40 h, for example, 20 h, 23 h, 25 h, 30 h, 35 h, 38 h, or 40 h, but is not limited to the recited values, and other unrecited values ​​within the range also apply.

[0022] Preferably, a dispersant is added in the first ball milling process at a mass fraction of 0.01 to 0.05%, which may be, for example, 0.01%, 0.02%, 0.03%, 0.04%, or 0.05%, but is not limited to the recited values, and other unrecited values ​​within the range also apply.

[0023] The present application does not specifically limit the type of dispersant, and any dispersant for ball milling well known to those skilled in the art may be employed.

[0024] Preferably, the drying temperature in step (2) is 120 to 150°C, and may be, for example, 120°C, 125°C, 130°C, 140°C, 145°C, or 150°C, but is not limited to the recited values, and other unrecited values ​​within the range apply as well.

[0025] Preferably, the drying time is 16 to 20 hours, for example, 16 hours, 16.5 hours, 17 hours, 18 hours, 19 hours, or 20 hours, but is not limited to the recited values, and other unrecited values ​​within the range also apply.

[0026] Preferably, the heating rate of the first sintering process described in step (2) is 1.0 to 1.5°C / min, and may be, for example, 1.0°C / min, 1.1°C / min, 1.2°C / min, 1.3°C / min, or 1.5°C / min, but is not limited to the recited values, and other unrecited values ​​within the numerical range also apply.

[0027] Preferably, the rotation speed of the second ball milling process described in step (3) is 60 to 80 r / min, and may be, for example, 60 r / min, 62 r / min, 65 r / min, 70 r / min, 75 r / min, or 80 r / min, but is not limited to the enumerated values, and other unenumerated values ​​within the numerical range also apply.

[0028] Preferably, the time for the second ball milling treatment is 15 to 24 hours, for example, 15 hours, 18 hours, 20 hours, 21 hours, 23 hours, or 24 hours, but is not limited to the recited values, and other unrecited values ​​within the range also apply.

[0029] Preferably, in the second ball milling process described in step (3), a dispersant is added in a mass fraction of 0.01 to 0.05%, which may be, for example, 0.01%, 0.02%, 0.03%, 0.04%, or 0.05%, but is not limited to the recited values, and other unrecited values ​​within the numerical range also apply.

[0030] Preferably, the solids content of the slurry before granulation described in step (4) is 70% or more, and may be, for example, 70%, 72%, 75%, 80%, 85%, or 90%, but is not limited to the recited values, and other unrecited values ​​within the range of values ​​also apply.

[0031] Preferably, the density of the sample after granulation is 3.4 to 3.6 g / cm 3 For example, 3.4g / cm 3 , 3.41g / cm 3 , 3.45g / cm 3 , 3.5g / cm3 , 3.55g / cm 3 or 3.6 g / cm 3 etc., but are not limited to the recited numerical values, and other unrecited numerical values ​​within the numerical range also apply.

[0032] Preferably, the air sintering in step (4) includes increasing the temperature from room temperature to 120° C. at a rate of 1.0° C. / min, maintaining the temperature for 2 h, and then increasing the temperature to 1000° C. at a rate of 2° C. / min.

[0033] Preferably, the oxygen sintering described in step (4) includes aerating oxygen having an oxygen content of ≧98% at a flow rate of 30-50 L / min, heating to an oxygen sintering temperature at a rate of 2.5° C. / min, keeping the temperature for 3-8 h, lowering the temperature to 700° C. at a rate of 2.5° C. / min, stopping the aeration of oxygen, and cooling in the furnace.

[0034] However, the flow rate is 30 to 50 L / min, and may be, for example, 30 L / min, 35 L / min, 38 L / min, 40 L / min, 45 L / min, or 50 L / min, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable. The oxygen content is 98% or more, and may be, for example, 98%, 98.2%, 98.5%, 99%, 99.3%, or 99.5%, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable. The temperature is kept warm for 3 to 8 h, and may be, for example, 3 h, 4 h, 5 h, 7 h, or 8 h, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0035] As a preferred technical solution of the present application, the manufacturing method includes: Chemical formula BaGd x Ni2Fe (16~x) O 27(However, according to 0.1 < x < 0.25), after calculating and weighing the raw materials BaCO3, Gd2O3, Ni2O and Fe2O3, a first ball milling treatment with a rotation speed of 60 - 80 r / min is carried out for 20 - 40 h to obtain a slurry after the first ball milling with a particle size X50 of 0.9 - 1.2 μm, and in the first ball milling treatment, a dispersant with a mass fraction of 0.01 - 0.05% is added (step (1)); The slurry after the first ball milling is sequentially dried at a temperature of 120 - 150 °C for 16 - 20 h and then subjected to a first sintering treatment at a temperature of 1200 - 1280 °C and a heating rate of 1.0 - 1.5 °C / min to obtain a mixed powder material (step (2)); The mixed powder material and the flux are mixed, and a second ball milling treatment with a rotation speed of 60 - 80 r / min is carried out for 15 - 24 h to obtain a slurry after the second ball milling with a particle size X50 of 0.8 - 1.1 μm, where the composition and mass% of the flux are respectively Bi2O3: 0.01 - 0.1%, V2O5: 0.01 - 0.1%, SiO2: 0.01 - 0.1% and ZnO: 0.01 - 0.1%, and in the second ball milling treatment, a dispersant with a mass fraction of 0.01 - 0.05% is added (step (3)); The slurry after the second ball milling is sequentially subjected to granulation molding and a second sintering treatment to obtain the low linewidth W - type hexagonal microwave ferrite material, where the linewidth of the low linewidth W - type hexagonal microwave ferrite material < 400 Oe; The solid content of the slurry before granulation molding ≧ 70%, and the density of the sample after granulation molding is 3.4 - 3.6 g / cm 3 ; The second sintering step includes air sintering followed by oxygen sintering, in which the air sintering step includes increasing the temperature from room temperature to 120°C at a rate of 1.0°C / min, maintaining the temperature for 2 hours, and then increasing the temperature to 1000°C at a rate of 2°C / min. The oxygen sintering step includes aerating oxygen at a flow rate of 30-50 L / min and an oxygen content of ≧98%, increasing the temperature to a sintering temperature of 1150°C-1250°C at a rate of 2.5°C / min, maintaining the temperature for 3-8 hours, and then decreasing the temperature to 700°C at a rate of 2.5°C / min., and stopping the aeration of oxygen and cooling in a furnace (4). Effect of the Invention

[0036] Compared with the related art, the embodiments of the present application have at least the following beneficial effects:

[0037] The method for producing a low linewidth W-type hexagonal microwave ferrite material according to the embodiment of the present application is a stable process with good reproducibility. The obtained W-type hexagonal microwave ferrite material has a linewidth of <400 Oe, a saturation magnetization of 3700-3900 Gs, a remanence of >0.9, and a density of >5.0 g / cm. 3 and there is a prospect for large-scale adoption.

[0038] Other aspects may be understood upon reading and understanding the detailed description. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0039] In order to facilitate understanding of the present application, the present application provides the following examples. Those skilled in the art should understand that the above examples are merely for understanding the present application, and should not be considered as specific limitations of the present application.

[0040] The present application will be described in more detail below. The following examples are merely illustrative of the present application, and do not represent or limit the scope of the claims of the present application, and the scope of protection of the present application is based on the claims.

[0041] Example 1 This embodiment provides a method for manufacturing a low linewidth W-type hexagonal microwave ferrite material, and the method includes the following steps:

[0042] (1') Chemical formula BaGd x Ni2Fe (16~x) O 27 The raw materials BaCO3, Gd2O3, Ni2O and Fe2O3 were calculated and weighed according to (where x = 0.2), where the purity of BaCO3 was 99.65%, the purity of Gd2O3 was 99.5%, the purity of Ni2O was 99.5%, and the purity of Fe2O3 was 99.5%.

[0043] (2') The raw materials were placed in a ball mill pot and mixed using a ball mill. The raw materials:deionized water:zirconia balls (large:small) were charged in a weight ratio of 1000:1000:(4000:1000). A first ball milling process was carried out at a rotation speed of 70 r / min for 24 hours. A dispersant was added in a mass fraction of 0.02% during the first ball milling process. The particle size X50 of the slurry after the first ball milling process was 0.9 to 1.2 μm.

[0044] (3') The slurry after the first ball milling process was placed in an oven and dried at 140°C for 18 hours. The dried powder was then sieved through a 60 mesh sieve and placed in an air sintering furnace for the first sintering process for 5 hours. The temperature was then raised to 1250°C for the first sintering process at a rate of 1.5°C / min to obtain a mixed powder.

[0045] (4') The mixed powder, flux, and dispersant with a mass fraction of 0.02% were mixed, then placed in a ball mill pot and mixed using a horizontal ball mill. The mixture was charged in a weight ratio of material: deionized water: zirconia balls (large: small) = 1000: 1000: (4000: 1000), and a second ball milling process was performed at a rotation speed of 70 r / min for 16 hours. The particle size X50 of the slurry after the second ball milling process was 0.8 to 1.1 μm, and the composition and mass% of the flux were Bi2O3: 0.06%, V2O5: 0.06%, SiO2: 0.06%, and ZnO: 0.06%, respectively.

[0046] (5') After the second ball milling treatment, excess water was filtered through a filter cloth to make the solid content of the slurry 70% or more.

[0047] (6') The treated slurry was subjected to orientation molding, and the obtained sample size was Z42*8, and the molding density was 3.4g / cm 3 It was.

[0048] (7') The sample was subjected to air sintering and then oxygen sintering. The air sintering was performed by increasing the temperature from room temperature to 120°C at a rate of 1.0°C / min, maintaining the temperature for 2 hours, and then increasing the temperature to 1000°C at a rate of 2°C / min. The oxygen sintering included aerating oxygen with a flow rate of 40 L / min and an oxygen content of 98%, increasing the temperature to a sintering temperature of 1180°C at a rate of 2.5°C / min, maintaining the temperature for 6 hours, decreasing the temperature to 700°C at a rate of 2.5°C / min, stopping the aeration of oxygen, and cooling in a furnace. The low linewidth W-type hexagonal microwave ferrite material was obtained.

[0049] Example 2 This embodiment provides a method for preparing a low linewidth W-type hexagonal microwave ferrite material, and the method is the same as that in embodiment 1, except that in step (1'), x=0.18.

[0050] Comparative Example 1 This comparative example provides a method for preparing a low linewidth W-type hexagonal microwave ferrite material, which is the same as Example 1, except that in step (1'), x=0.

[0051] Comparative Example 2 This comparative example provides a method for preparing a low linewidth W-type hexagonal microwave ferrite material, and the method is the same as Example 1, except that in step (1'), x=0.3.

[0052] Comparative Example 3 This comparative example provides a method for preparing a low linewidth W-type hexagonal microwave ferrite material, and the method is the same as that of Example 1, except that in step (3'), the temperature of the first sintering process is 1150°C.

[0053] Comparative Example 4 This comparative example provides a method for preparing a low linewidth W-type hexagonal microwave ferrite material, and the method is the same as that of Example 1, except that in step (3'), the temperature of the first sintering process is 1300°C.

[0054] Comparative Example 5 This comparative example provides a method for producing a low linewidth W-type hexagonal microwave ferrite material, and the method is the same as that of Example 1, except that in step (4'), the composition and mass percentage of the flux are Bi2O3: 0.12%, V2O5: 0.12%, SiO2: 0.12% and ZnO: 0.06%, respectively.

[0055] Comparative Example 6 This comparative example provides a method for preparing low linewidth W-type hexagonal microwave ferrite material, and the method is the same as Example 1, except that no flux is added in step (4').

[0056] Comparative Example 7 This comparative example provides a method for producing a low linewidth W-type hexagonal microwave ferrite material, and the method is the same as that of Example 1, except that in step (4'), the composition and mass% of the flux are V2O5: 0.12%, SiO2: 0.12% and ZnO: 0.06%, respectively.

[0057] Comparative Example 8 This comparative example provides a method for producing a low linewidth W-type hexagonal microwave ferrite material, which is the same as Example 1, except that in step (2'), the first ball milling time is h, and the particle size X50 of the obtained slurry after the first ball milling is μm.

[0058] Comparative Example 9 This comparative example provides a method for producing a low linewidth W-type hexagonal microwave ferrite material, which is the same as Example 1, except that in step (4'), the second ball milling time is h, and the particle size X50 of the obtained slurry after the second ball milling is μm.

[0059] Comparative Example 10 This comparative example provides a method for preparing low linewidth W-type hexagonal microwave ferrite material, and the method is the same as that in Example 1, except that the oxygen sintering temperature in step (7') is 1100°C.

[0060] Comparative Example 11 This comparative example provides a method for preparing low linewidth W-type hexagonal microwave ferrite material, and the method is the same as that in Example 1, except that the oxygen sintering temperature in step (7') is 1280°C.

[0061] Comparative Example 12 This comparative example provides a method for preparing a low linewidth W-type hexagonal microwave ferrite material, which is the same as that of Example 1, except that in step (7'), the temperature is lowered directly in air without oxygen sintering.

[0062] The W-type hexagonal microwave ferrite materials obtained in the above examples and comparative examples were machined into spheres with a diameter of 2.5 mm, and the saturation magnetization was measured.

[0063] The W-type hexagonal microwave ferrite materials obtained in the above examples and comparative examples were processed into Z38*6 samples, and their remanence was measured.

[0064] The W-type hexagonal microwave ferrite materials obtained in the above examples and comparative examples were processed into spheres with a diameter of 1 mm, and the line widths were measured.

[0065] The density of the W-type hexagonal microwave ferrite materials obtained in the above examples and comparative examples was measured by using an underwater substitution method, and the test results are shown in Table 1.

[0066] [Table 1]

[0067] As can be seen from Table 1, the W-type hexagonal microwave ferrite material obtained by the manufacturing method according to the present application has a line width of <400 Oe, a saturation magnetization of 3700 to 3900 Gs, a remanence of >0.9, and a density of >5.0 g / cm. 3 and there is a prospect for large-scale adoption.

[0068] When Gd is not added to the raw material or the ratio of Gd is too high, the line width of the obtained W-type hexagonal microwave ferrite material is high. When the temperature of the first sintering process is low, the other performances are equivalent to those of Example 1, but the line width is high. When no flux is added or the composition and content of each substance of the flux are not within the range of the present application, the line width of the W-type hexagonal microwave ferrite material is high and the remanence is low. When the particle size of the slurry after the first ball milling process and the particle size of the slurry after the second ball milling process are large, the line width of the W-type hexagonal microwave ferrite material is high, the remanence is low, and the density is low. When the oxygen sintering temperature is not within the range of the present application, the line width of the W-type hexagonal microwave ferrite material is high and the remanence is low.

[0069] In summary, the manufacturing method of the low linewidth W-type hexagonal microwave ferrite material according to the present invention has a stable process, good reproducibility, and is expected to be widely used.

[0070] The applicant declares that the above description is merely a specific embodiment of the present application, but the scope of protection of the present application is not limited thereto, and that any modification or replacement that a person skilled in the art can easily conceive within the technical scope disclosed in the present application should be understood to be included in the scope of protection and disclosure of the present application.

Claims

1. 1. A method for producing a low linewidth W-type hexagonal microwave ferrite material, comprising: Chemical formula BaGd x Ni 2 Fe (16~x) O 27 (where 0.1 < x < 0.25) depending on the raw material BaCO 3 , Gd 2 O 3 , Ni 2 O and Fe 2 O 3 (1) calculating and weighing the slurry, and then performing a first ball milling process to obtain a slurry after the first ball milling having a particle size X50 of 0.9 to 1.2 μm; (2) drying the slurry after the first ball milling and then performing a first sintering process at a temperature of 1200 to 1280° C. to obtain a mixed powder material; A step of mixing the mixed powder material and a flux, performing a second ball milling process, and obtaining a slurry after the second ball milling having a particle size X50 of 0.8 to 1.1 μm, wherein the composition and mass % of the flux are Bi 2 O 3 :0.01~0.1%, V 2 O 5 :0.01~0.1%, SiO 2 : 0.01 to 0.1% and ZnO: 0.01 to 0.1%; and (4) sequentially carrying out granulation molding and a second sintering process on the slurry after the second ball milling to obtain the low linewidth W-type hexagonal microwave ferrite material, the second sintering process including air sintering followed by oxygen sintering at a temperature of 1150°C to 1250°C, and the low linewidth W-type hexagonal microwave ferrite material has a linewidth of <400 Oe; Manufacturing method.

2. The rotation speed of the first ball milling process described in step (1) is 60 to 80 r / min; The method of claim 1 .

3. The time of the first ball milling treatment is 20 to 40 h; The method according to claim 1 or 2.

4. Adding a dispersant in a mass fraction of 0.01 to 0.05% in the first ball milling process; The method according to any one of claims 1 to 3.

5. The drying temperature in step (2) is 120 to 150° C. Preferably, the drying time is 16 to 20 h. The method according to any one of claims 1 to 4.

6. The heating rate of the first sintering treatment described in step (2) is 1.0 to 1.5 ° C. / min; The method according to any one of claims 1 to 5.

7. The rotation speed of the second ball milling process described in step (3) is 60 to 80 r / min; Preferably, the second ball milling treatment is performed for a period of 15 to 24 hours. The method according to any one of claims 1 to 6.

8. In the second ball milling process described in step (3), a dispersant is added at a mass fraction of 0.01 to 0.05%. The method according to any one of claims 1 to 7.

9. The solid content of the slurry before granulation described in step (4) is ≧70%; Preferably, the density of the sample after granulation is 3.4 to 3.6 g / cm 3 That is, The method according to any one of claims 1 to 8.

10. The air sintering described in step (4) includes increasing the temperature from room temperature to 120° C. at a rate of 1.0° C. / min, maintaining the temperature for 2 h, and then increasing the temperature to 1000° C. at a rate of 2° C. / min; The method according to any one of claims 1 to 9.

11. The oxygen sintering described in step (4) includes: passing oxygen at a flow rate of 30-50 L / min and an oxygen content of ≧98%, raising the temperature to the oxygen sintering temperature at a rate of 2.5° C. / min, keeping the temperature for 3-8 h, and then lowering the temperature to 700° C. at a rate of 2.5° C. / min, stopping the oxygen passage and cooling in the furnace; The method according to any one of claims 1 to 10.

12. Chemical formula BaGd x Ni 2 Fe (16~x) O 27 (where 0.1 < x < 0.25) depending on the raw material BaCO 3 , Gd 2 O 3 , Ni 2 O and Fe 2 O 3 (1) calculating and weighing the slurry, and then performing a first ball milling process at a rotation speed of 60 to 80 r / min for 20 to 40 hours to obtain a slurry after the first ball milling process having a particle size X50 of 0.9 to 1.2 μm, and adding a dispersant at a mass fraction of 0.01 to 0.05% in the first ball milling process; (2) drying the slurry after the first ball milling at a temperature of 120 to 150 ° C. for 16 to 20 h and then performing a first sintering process at a temperature of 1200 to 1280 ° C. and a heating rate of 1.0 to 1.5 ° C. / min to obtain a mixed powder material; The mixed powder material and the flux are mixed, and a second ball milling process is performed at a rotation speed of 60 to 80 r / min for 15 to 24 hours to obtain a slurry after the second ball milling process having a particle size X50 of 0.8 to 1.1 μm, and the composition and mass % of the flux are each Bi 2 O 3 :0.01~0.1%, V 2 O 5 :0.01~0.1%, SiO 2: 0.01-0.1% and ZnO: 0.01-0.1%, and a step (3) of adding a dispersant having a mass fraction of 0.01-0.05% in the second ball milling process; (4) The slurry after the second ball milling is subjected to a granulation molding and a second sintering process in order to obtain the low line width W-type hexagonal microwave ferrite material, and the low line width W-type hexagonal microwave ferrite material has a line width of <400 Oe; The solid content of the slurry before granulation is ≧70%, and the density of the sample after granulation is 3.4 to 3.6 g / cm 3 and The second sintering step includes air sintering followed by oxygen sintering, the air sintering includes increasing the temperature from room temperature to 120°C at a rate of 1.0°C / min, maintaining the temperature for 2 hours, and then increasing the temperature to 1000°C at a rate of 2°C / min, and the oxygen sintering includes aerating oxygen with a flow rate of 30-50L / min and an oxygen content of ≧98%, increasing the temperature to a sintering temperature of 1150°C-1250°C at a rate of 2.5°C / min, maintaining the temperature for 3-8 hours, and then decreasing the temperature to 700°C at a rate of 2.5°C / min, and stopping the aeration of oxygen and cooling in a furnace (4); The method according to any one of claims 1 to 11.

Citation Information

Patent Citations

  • High-coercivity low-loss composite hexagonal ferrite material and preparation method thereof

    CN114409393A

  • Ferrite sintered magnet, ferrite particle, bond magnet and electrical rotating machine

    JP2020161656A

  • Ferrite magnet powder, sintered magnet, bond magnet and magnetic recording medium

    WO2004077458A1