Method for manufacturing abrasive grindstone, and abrasive grindstone

A method to manufacture a glass-based polishing wheel with controlled porosity and surface roughness addresses the limitations of Arkansas whetstone, providing a uniform and cost-effective alternative for polishing metals and ceramics.

JP7551234B2Active Publication Date: 2024-09-17DISCO CORP
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
JP2020099136
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2020-06-08
Publication Date
2024-09-17
Estimated Expiration
2040-06-08

AI Technical Summary

Technical Problem

The existing Arkansas whetstone, being a natural product, is expensive, non-uniform, and has significant individual variations, making it a costly and unreliable substitute for polishing metal and ceramic surfaces.

Method used

A method involving the formation of a glass block by heating glass grains at a temperature above the softening point and below the melting point, with air bubbles retained in the gaps, to create a polishing wheel with controlled porosity and surface roughness, eliminating the need for abrasive grains.

Benefits of technology

The resulting polishing wheel offers uniform properties, reduces individual differences, and provides effective polishing without surface damage, serving as a reliable substitute for Arkansas whetstone at a lower cost.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007551234000004
    Figure 0007551234000004
  • Figure 0007551234000001
    Figure 0007551234000001
  • Figure 0007551234000002
    Figure 0007551234000002
Patent Text Reader

Abstract

To provide a manufacturing method of a polishing grindstone and the polishing grindstone, usable for polishing a surface of a metal and a ceramics.SOLUTION: A manufacturing method of a polishing grindstone includes: a glass particle supply step of supplying glass particles to a frame mold; and a firing step of heating the frame mold accommodating the glass particles at a temperature higher than a softening point of the glass particles and lower than a melting point thereof and forming glass blocks which become a polishing grindstone, and which firing step terminates heating in a state that cells are dispersed in gaps of the glass particles. Preferably, the glass particles comprise a soda glass, feldspar, or a borosilicate glass. Preferably, the glass block after executing the firing step has a surface roughness (Ra) of 0.2 μm or over and 1.5 μm or under and a porosity of 2% or over and 8% or under. More preferably, the firing step is executed within 1 to 2 hours.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for making an abrasive wheel for use in abrading metal or ceramic surfaces, and to the abrasive wheel. [Background technology]

[0002] When the surface of a metal or ceramic is processed, minute irregularities or minute protrusions called burrs may occur on the surface. Arkansas grindstones are known as polishing stones used to remove such irregularities and burrs from the surface. Arkansas grindstones are used, for example, to clean a table base that supports a chuck table that holds a workpiece in a processing device that processes a workpiece such as a semiconductor wafer (see Patent Document 1). [Prior art documents] [Patent documents]

[0003] [Patent Document 1] JP 2004-37009 A Summary of the Invention [Problem to be solved by the invention]

[0004] Arkansas whetstones are natural oilstones produced in Arkansas, USA. Because they are natural products, Arkansas whetstones are expensive and valuable, and their properties tend to be uneven and there are large individual differences. Therefore, there is a demand for polishing wheels that can be used as substitutes for Arkansas whetstones, and for polishing wheels of higher quality with less variation than Arkansas whetstones.

[0005] The present invention has been made in consideration of the above problems, and an object of the present invention is to provide a new method for manufacturing a polishing wheel that can be used to polish the surfaces of metals and ceramics, and a polishing wheel that can be used to polish the surfaces of metals and ceramics. [Means for solving the problem]

[0006] According to one aspect of the present invention, a method for manufacturing a grinding wheel includes the steps of: supplying glass particles to a mold; and forming a mold containing the glass particles. (However, this does not include cases where a foaming agent is included.) and a firing step of heating the glass block to a temperature above the softening point and below the melting point of the glass particles to form a glass block that will become the abrasive wheel, wherein the firing step is terminated in a state where air bubbles remain dispersed in the gaps between the glass particles.

[0007] Preferably, the glass particles are soda glass, feldspar, or borosilicate glass.

[0008] Furthermore, preferably, the glass block after the firing step has a surface roughness (Ra) of 0.2 μm or more and 1.5 μm or less and a porosity of 2% or more and 8% or less.

[0009] Further, preferably, the calcination step is carried out for a period of not less than 1 hour and not more than 2 hours.

[0010] According to another aspect of the present invention, there is provided a polishing wheel for polishing metal or ceramic surfaces, characterized in that the polishing wheel is made of a glass block having a surface roughness (Ra) of 0.2 μm or more and 1.5 μm or less and a porosity of 2% or more and 8% or less.

[0011] Preferably, it does not contain abrasive grains. Effect of the Invention

[0012] In the method for manufacturing the grinding wheel according to one aspect of the present invention, glass particles are fed into a mold, and a glass block that becomes the grinding wheel is formed by heating the glass particles at a temperature above the softening point and below the melting point. At this time, the heating is terminated in a state where air bubbles are dispersed and remain in the gaps between the glass particles. The grinding wheel according to one aspect of the present invention has a moderate amount of pores, is uniform in properties, and has small individual differences. The grinding wheel can be used as a substitute for an Arkansas grinding wheel to polish the surfaces of metals and ceramics.

[0013] Therefore, one aspect of the present invention provides a new method for manufacturing a polishing wheel and a polishing wheel that can be used to polish the surfaces of metals and ceramics. [Brief description of the drawings]

[0014] [Figure 1] FIG. 4 is a cross-sectional view showing a glass particle supplying step. [Diagram 2] FIG. 4 is a cross-sectional view showing a schematic diagram of a firing step. [Diagram 3] FIG. 3(A) is a perspective view that shows a schematic diagram of an example of the polishing wheel, and FIG. 3(B) is a perspective view that shows a schematic diagram of another example of the polishing wheel. [Figure 4] 3 is a flowchart showing the steps of a method for manufacturing a polishing wheel. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0015] An embodiment of the present invention will be described. The grindstone manufactured by the method for manufacturing the grindstone according to this embodiment can be used as a substitute for the Arkansas grindstone. Conventionally, the Arkansas grindstone has been used as a grindstone for removing minute irregularities and minute protrusions called burrs from the surface of metals or ceramics that are generated when the surface of the metals or ceramics is processed.

[0016] When polishing the processed surface of metal or ceramic, there is a demand for reliable removal of minute irregularities and burrs on the surface, while at the same time, it is also required not to excessively wear or damage the surface by polishing. The Arkansas grinding wheel is a relatively hard grinding wheel mainly composed of quartz, but contains pores (air bubbles) that can appropriately retain oil (oil) or water, which is used as a lubricant during polishing, and is therefore suitable for polishing the surfaces of metals and ceramics.

[0017] However, since Arkansas whetstones are a natural product, their reserves are limited and valuable, and their quality is prone to unevenness and individual differences are large. Therefore, there was a demand for artificial abrasive stones that could replace Arkansas whetstones. However, it was not easy to manufacture an artificial abrasive stone that was made of a hard material while having good properties, such as a moderate distribution of pores.

[0018] The manufacturing method of the grinding wheel according to this embodiment makes it possible to manufacture a grinding wheel with such good properties. Each step of the manufacturing method will be described below. Fig. 4 is a flow chart showing the flow of each step. In this manufacturing method, first, a glass grain supply step S10 is performed in which glass grains are supplied to a mold, and then a firing step S20 is performed in which the mold is heated to form a glass block that will become the grinding wheel.

[0019] Fig. 1 is a cross-sectional view showing the glass grain supply step S10. Fig. 1 shows a side view of a container 2 containing glass grains 1, which are raw material for a glass block that becomes a polishing wheel, and a cross-sectional view of a mold 4. The mold 4 has a main body 6 made of ceramics or the like that can withstand the heating temperature in a firing step S20 described later. A concave container 8 into which the glass grains 1 are poured is provided in the center of the upper surface of the main body 6. In the glass grain supply step S10, the glass grains 1 are poured into the container 8 from a supply port 2a of the container 2.

[0020] The glass particles 1 put into the storage section 8 are fired at high temperature to become a glass block. The formed glass block may be used as a grinding wheel as it is, or may be shaped into a predetermined shape and used as a grinding wheel. The shape of the glass block reflects the shape of the storage section 8. Therefore, when the glass block is to be used as a grinding wheel as it is, it is advisable to select and use, in the glass particle supply step S10, a mold 4 having a storage section 8 of a shape that matches the shape of the grinding wheel to be manufactured.

[0021] The material of the glass particles 1 is, for example, soda glass, feldspar, borosilicate glass, etc. The glass particles 1 preferably have a particle size of about φ50 μm to φ150 μm. However, the particle size of some of the glass particles 1 contained in the container 8 may be outside this range, as long as the particle size of the majority of the glass particles 1 falls within this range.

[0022] For example, if the particle size of the main glass particles 1 is less than φ50 μm, the glass particles 1 are difficult to handle, and the glass particles 1 are difficult to fit into the storage section 8 of the mold 4. On the other hand, if the particle size of the main glass particles 1 is greater than φ150 μm, it is difficult to form pores of an appropriate size and that are appropriately distributed in the glass block to be formed. For example, the pores may be connected to each other in the glass block, allowing a lubricant such as oil or water supplied to the polishing wheel when polishing the workpiece to be polished to penetrate into the inside, and the lubricant may not be sufficiently retained on the surface that contacts the workpiece to be polished.

[0023] In the glass particle supply step S10, glass particles 1 are supplied to the storage section 8 of the mold 4 in an amount corresponding to the volume to be formed. At this time, it is preferable to vibrate the mold 4 so that the upper surfaces of the glass particles 1 stored in the storage section 8 are flattened and no extra space is left. For example, it is preferable to vibrate the mold 4 for a time period of less than one minute. Vibration is one of the factors that contribute to the production of a homogeneous grinding wheel.

[0024] Following the glass particle supply step S10, a firing step S20 is performed. FIG. 2 is a cross-sectional view that shows a schematic diagram of the firing step S20. As shown in FIG. 2, the form 4, which contains the glass particles 1 in the container 8, is housed in the internal space 12 of the heating furnace 10 and heated. When housed in the heating furnace 10, a lid 14 for closing the container 8 of the form 4 is placed on the top of the form 4. The lid 14 is made of, for example, the same material as the form 4, and can withstand the heating temperature when the glass particles 1 are fired.

[0025] The heating furnace 10 is equipped with a heat source (not shown) such as an electric heating wire for heating the internal space 12 to a predetermined temperature. In the firing step S20, the mold 4 containing the glass particles 1 is heated to a temperature above the softening point and below the melting point of the glass particles 1 to form a glass block that will become the grinding wheel. Here, the softening point of the glass particles 1 refers to the temperature at which the glass particles 1 begin to deform as the temperature is increased. The softening point varies depending on the properties of the glass particles 1, such as the material and structure, and is a temperature lower than the melting point.

[0026] In the firing step S20, if the glass particles 1 are soda glass, the form 4 is heated to a temperature higher than 720°C and lower than 1000°C. If the glass particles 1 are feldspar, the form 4 is heated to a temperature higher than 900°C and lower than 1350°C. If the glass particles 1 are borosilicate glass, the form 4 is heated to a temperature higher than 820°C and lower than 1250°C.

[0027] Then, in the firing step S20, the heating is terminated in a state where air bubbles remain dispersed in the gaps between the glass particles 1. For example, when the temperature of the glass particles 1 exceeds the melting point, the glass particles 1 are liquefied and the air bubbles in the gaps between the glass particles 1 are released. In this case, even if the formed glass block is used as a polishing wheel, the polishing wheel will no longer retain the lubricant, and the object to be polished cannot be polished properly.

[0028] Even if the temperature of the glass particles 1 does not exceed the melting point, if the glass particles 1 are exposed to a temperature higher than the softening point for a long period of time, the air bubbles between the glass particles 1 will escape. Therefore, in the firing step S20, it is preferable to heat the glass particles 1 for a time period of 1 hour or more and 2 hours or less. When the firing step S20 is performed, a glass block that can be used as a grinding wheel is formed. Thereafter, the mold 4 is removed from the heating furnace 10, and the glass block is removed from the mold 4.

[0029] Fig. 3(A) is a perspective view showing a polishing wheel 3 made of a rectangular parallelepiped glass block, and Fig. 3(B) is a perspective view showing a polishing wheel 5 made of a disk-shaped glass block. In the method for manufacturing a polishing wheel according to this embodiment, a polishing wheel of any shape can be manufactured by changing the shape of the housing portion 8 of the mold 4.

[0030] Here, when the surface roughness (Ra) of the surfaces 3a, 5a of the glass block (polishing wheels 3, 5) after the firing step S20 is measured, it is 0.2 μm or more and 1.5 μm or less. In other words, it is understood that the surfaces 3a, 5a are very flat. In the manufacturing method of the polishing wheel according to this embodiment, abrasive grains are not mixed with the glass grains 1, so that the polishing wheels 3, 5 that do not contain abrasive grains are obtained. Therefore, the flatness of the surfaces 3a, 5a is extremely high, and even if the surfaces of metals or ceramics are polished with the polishing wheels 3, 5, damage such as scratches does not occur on the polished surface.

[0031] The porosity of the manufactured grinding wheels 3,5 is set to be 2% or more and 8% or less. Here, the porosity refers to the ratio of the volume of pores to the total volume of the grinding wheels 3,5. If the porosity of the grinding wheels 3,5 is less than 2%, it becomes difficult to retain an appropriate amount of oil as a lubricant. On the other hand, if the porosity exceeds 8%, the pores are connected to each other, making it easier for the lubricant to penetrate into the grinding wheels 3,5, and it becomes difficult for the necessary amount of oil to remain on the surface.

[0032] In addition, if the porosity is too high and many pores are exposed on the surfaces 3a, 5a of the polishing wheels 3, 5, burrs and the like on the surface of the workpiece are likely to hit the pores. When burrs and the like hit the pores, damage such as chipping is likely to occur in the workpiece at that part. Therefore, too many pores can be a factor in reducing the processing quality.

[0033] In the method for manufacturing the grindstone according to the present embodiment, after the firing step S20, a polishing step may be further performed to polish the surface of the formed glass block in order to further improve the flatness of the surface. In order to ensure the flatness required for the application of the manufactured grindstones 3 and 5, the surfaces 3a and 5a may be appropriately polished.

[0034] Furthermore, after the firing step S20, a shaping step may be performed in which the glass block is shaped into a grinding wheel of a predetermined shape. In the shaping step, for example, the glass block is shaped by cutting with an annular cutting blade or grinding with a disk-shaped grinding wheel. This allows grinding wheels of various shapes to be manufactured according to the application.

[0035] When the manufactured grinding wheel is used to grind metals, ceramics, and other objects to be ground, the resulting processing debris may accumulate on the surface of the grinding wheel, causing clogging. In this case, the grinding ability of the grinding wheel can be restored by polishing or grinding the surface of the grinding wheel to remove the clogged parts and expose a new surface.

[0036] As described above, the method for manufacturing the grindstone according to this embodiment makes it possible to manufacture the grindstones 3 and 5 that can be used as substitutes for the Arkansas grindstone. The formed grindstones 3 and 5 have high surface flatness and moderate porosity, making them suitable for use in polishing the surfaces of processed metals and ceramics.

[0037] Furthermore, the manufactured grinding wheels 3, 5 are homogeneous, unlike Arkansas grinding wheels, which are naturally produced, and the variation in individual differences is small. In particular, if soda glass is used for the glass particles 1 supplied to the mold 4 in the glass particle supply step, the heating temperature of the mold 4 in the firing step S20 can be kept relatively low, so that the grinding wheels 3, 5 can be manufactured easily and inexpensively, and the properties are more stable.

[0038] In the above embodiment, the polishing wheels 3 and 5 are described as being used for polishing the surfaces of metals and ceramics, but one aspect of the present invention is not limited to this. That is, the polishing wheels 3 and 5 may be used for other purposes.

[0039] In the above embodiment, the mold is vibrated in the glass particle supply step S10 to remove air bubbles and flatten the upper surfaces of the glass particles 1, but this aspect of the present invention is not limited to this. For example, the upper surfaces of the glass particles 1 may be flattened by other methods or may be flattened by a jig having a flat shape.

[0040] In addition, the structures, methods, etc. according to the above-described embodiments can be modified as appropriate without departing from the scope of the object of the present invention. [Explanation of symbols]

[0041] 1 glass pellet 3,5 Grinding wheels 3a,5a surface 2 containers 2a Supply port 4. Formwork 6 Main unit 8. Storage section 10 Furnace 12 Interior Space 14 Lid

Claims

1. A method for manufacturing a grinding wheel, comprising the steps of: A glass grain supplying step of supplying glass grains to a mold; and a firing step of heating the form containing the glass particles (except when a foaming agent is contained therein) at a temperature higher than the softening point of the glass particles and lower than the melting point thereof to form a glass block to be used as a grinding wheel. The method for manufacturing an abrasive wheel is characterized in that the firing step is terminated in a state where air bubbles remain dispersed in the gaps between the glass particles.

2. 2. The method for manufacturing an abrasive wheel according to claim 1, wherein the glass particles are soda glass, feldspar, or borosilicate glass.

3. 3. The method for manufacturing an abrasive wheel according to claim 1, wherein the glass block after the firing step has a surface roughness (Ra) of 0.2 μm to 1.5 μm and a porosity of 2% to 8%.

4. 4. The method for manufacturing an abrasive wheel according to claim 1, wherein the firing step is carried out for at least one hour and not more than two hours.

5. A grinding wheel for grinding metal or ceramic surfaces, comprising: A grinding wheel comprising a glass block having a surface roughness (Ra) of 0.2 μm or more and 1.5 μm or less and a porosity of 2% or more and 8% or less.

6. 6. The grinding wheel according to claim 5, which does not contain abrasive grains.

Citation Information

Patent Citations

  • Bond for abrasive material raw grindstone

    JP1989246076A

  • Grinding stone and manufacture thereof

    JP1992111777A

  • Synthetic polishing grindstone and its manufacturing method

    JP1995507241A

  • Finishing grinding wheel and method of manufacture

    JP2002283244A

  • Cooling container

    JP2004037009A