Molding composition and method for producing three-dimensional shaped object

A composition of powder, wax, adhesive, and plasticizer with controlled properties addresses the viscosity and fluidity issues in three-dimensional printing, ensuring stable and accurate object formation with high powder filling rates and reduced thermal shrinkage.

JP7552125B2Active Publication Date: 2024-09-18SEIKO EPSON CORP
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
JP2020130205
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2020-07-31
Publication Date
2024-09-18
Estimated Expiration
2040-07-31

AI Technical Summary

Technical Problem

Conventional three-dimensional printing compounds used in MIM (Metal Injection Molding) exhibit high viscosity and lack fluidity, leading to unstable object formation and reduced shape accuracy due to limited compound injection and potential instability.

Method used

A molding composition comprising powder, wax, adhesive component, and plasticizer, with specific melt flow rates and densities, is used to enhance fluidity and stability, allowing for high powder filling rates and reduced binder loss during degreasing and sintering.

Benefits of technology

The composition achieves low viscosity, enabling stable and accurate three-dimensional object formation with high powder filling rates, reducing thermal shrinkage and warpage, and maintaining shape integrity during high-temperature processes.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007552125000001
    Figure 0007552125000001
Patent Text Reader

Abstract

To provide a molding composition that can ensure good shape accuracy of a shaped object even with reduced viscosity.SOLUTION: A molding composition contains powder, a wax, an adhesive component, a molding component, and a plasticizer, in which a melt flow rate of the adhesive component at 190°C is 200 g / 10 min or more, and a density of the plasticizer is 1.0 g / cm3 or less.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a molding composition and a method for producing a three-dimensional object. [Background technology]

[0002] It is becoming common to mold three-dimensional objects without using machining or casting. For example, Patent Document 1 discloses a manufacturing method for manufacturing metal or ceramic products by forming a molded object using a fused deposition modeling (FDM) three-dimensional printer using a compound containing inorganic powder as a raw material, and then degreasing and sintering the molded object. The document describes that the manufacturing method makes it possible to rapidly mold metal or ceramic products in shapes that are impossible to achieve by machining or casting, and that the method is suitable for small-scale production of products. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] JP 2000-144205 A Summary of the Invention [Problem to be solved by the invention]

[0004] However, when a compound similar to that used in conventional MIM (Metal Injection Molding) is applied to a three-dimensional modeling device, the compound has a high viscosity and lacks fluidity, which can cause the amount of compound injected from the three-dimensional modeling device to become unstable, resulting in a risk of reduced accuracy of the shape of the model. Therefore, there is a need to lower the viscosity of the compound to obtain good shape accuracy of the model. [Means for solving the problem]

[0005] One aspect of the molding composition according to the present invention is The composition includes a powder, a wax, an adhesive component, a molding component, and a plasticizer, The melt flow rate of the adhesive component at 190°C is 200 g / 10 min or more, and the density of the plasticizer is 1.0 g / cm 3 The following is the result.

[0006] One aspect of the method for producing a three-dimensional object according to the present invention includes: The method includes a layer-forming step of discharging the molding composition of the above embodiment, and the layer-forming step is carried out multiple times. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0007] Several embodiments of the present invention will be described below. The embodiments described below are merely examples of the present invention. The present invention is not limited to the following embodiments, and includes various modified forms that are implemented within the scope of the present invention. Note that not all of the configurations described below are necessarily essential configurations of the present invention.

[0008] 1. Molding composition The molding composition according to the present embodiment includes a powder, a wax, an adhesive component, a molding component, and a plasticizer. The adhesive component has a melt flow rate of 200 g / 10 min or more at 190° C., and the plasticizer has a density of 1.0 g / cm 3 Each component will be described below. In this specification, the components other than the powder contained in the molding composition may be collectively referred to as "binder".

[0009] 1.1. Powder The molding composition of the present embodiment contains a powder. The powder is obtained by degreasing and baking the molding composition. In other words, the powder used in the molding composition of the present embodiment may be any powder that can remain even if the binder is lost during degreasing and sintering, and examples of the powder include inorganic powders and organic powders.

[0010] Examples of the inorganic powder include metal powder, ceramic powder, cermet powder, metal oxide powder, and intermetallic compound powder. A mixture of two or more of these powders may also be used.

[0011] Specifically, examples of metal powders include powders of pure iron, iron-nickel, iron-cobalt, iron-silicon, iron-based alloys such as stainless steel, tungsten, tungsten carbide (WC), cemented carbide (WC-Co based alloys, etc.), aluminum alloys, copper, and copper alloys.

[0012] In addition, ceramic powders and metal oxide powders include Al 2 O 3 , BeO, TiO 2 , ZrO 2 Oxides such as TiC, ZrC, B 4 Carbides such as C, CrB, ZrB 2 Borides such as TiN and ZrN, and nitrides such as TiN and ZrN are also included as cermet powders. 2 O 3 -Fe system, TiC-Ni system, TiC-Co system, B 4 Examples include the C-Fe system.

[0013] Examples of organic powders include silicone elastomer powder, silicone powder, silicone resin-coated silicone elastomer powder, polyamide resin powder (nylon powder), polyethylene powder, polystyrene powder, styrene-acrylic acid copolymer resin powder, benzoguanamine resin powder, polytetrafluoroethylene powder, and cellulose powder.

[0014] The powder used in the molding composition of the present embodiment is preferably an inorganic powder, since it has a sufficiently higher combustion temperature, decomposition temperature, evaporation temperature, etc. than the binder. Among inorganic powders, a metal powder is more preferable, since the surface of the metal powder is easily melted during sintering, and the shape of the shaped object, which is a sintered body, can be precisely formed.

[0015] The amount of powder in the molding composition is preferably 64.8% by volume or more relative to the total volume of the molding composition. In other words, the volumetric filling rate of the powder in the molding composition is preferably 64.8% or more. When the amount of powder is within this range, the amount of components other than the powder is reduced, and the volume change upon heating and cooling is suppressed to a smaller extent. Furthermore, when the amount of powder is within this range, the amount of components lost during debinding and sintering is reduced, and a molded object with a higher density can be obtained.

[0016] 1.2.Wax The molding composition contains a wax. The wax has a function of improving the fluidity of the molding composition when it is extruded or injected from a three-dimensional modeling device, etc. The wax constitutes a binder, and is a component that disappears when the molding composition is degreased and sintered.

[0017] Examples of waxes include natural waxes and synthetic waxes. Examples of natural waxes include vegetable waxes such as candelilla wax, carnauba wax, rice wax, Japan wax, and jojoba oil, animal waxes such as beeswax, lanolin, and spermaceti, and mineral waxes such as montan wax, ozokerite, and ceresin. Examples of synthetic waxes include petroleum waxes such as paraffin wax, microcrystalline wax, and petrolatum. The waxes can be used in combination of one or more of the above-mentioned types.

[0018] The amount of wax in the molding composition is preferably 25% by mass or more and 35% by mass or less, based on 100% by mass of the components of the molding composition excluding the powder, i.e., the binder. The wax content is preferably from 26% by mass to 33% by mass, more preferably from 27% by mass to 30% by mass, and even more preferably from 27% by mass to 29% by mass. When the wax content is within this range, the molding composition has excellent fluidity.

[0019] 1.3.Adhesive components The molding composition contains an adhesive component. The adhesive component constitutes a binder. The adhesive component has the function of bonding powder particles together in the molding composition. A small amount of the adhesive component remains in the molding composition after degreasing. This has the function of bonding powder particles together and maintaining the shape of the shaped object in the degreasing state before sintering. The adhesive component is a component that disappears when the molding composition is sintered, like other binders.

[0020] The adhesive component has a melt flow rate (MFR) of 200 g / 10 min or more at 190° C. When the adhesive component has a MFR of 200 g / 10 min or more, the molding composition can have high fluidity.

[0021] Examples of the adhesive component include copolymers of two or more monomers selected from ethylene, acrylic, and vinyl monomers. More specifically, examples of the adhesive component include ethylene-glycidyl (meth)acrylate copolymers, ethylene-vinyl acetate copolymers, and the like.

[0022] The MFR of the adhesive component can be adjusted, for example, by changing the molecular weight of the polymer compound that constitutes the adhesive component.

[0023] The melt flow rate of the adhesive component can be measured under conditions of 190° C. and 21.2 N load (2160 g load) according to JIS K 7210, and under conditions of 190° C. and 21.2 N load (2160 g load) according to ASTM D1238 and ISO1133.

[0024] The amount of the adhesive component in the molding composition is 20% by mass or more and 35% by mass or less, preferably 22% by mass or more and 33% by mass or less, more preferably 23% by mass or more and 30% by mass or less, and even more preferably 25% by mass or more and 27% by mass or less, when the components of the molding composition excluding the powder, i.e., the binder, are taken as 100% by mass. If the amount of the adhesive component is within this range, a molded object molded using the molding composition can have better shape stability.

[0025] 1.4. Molding components The molding composition contains a molding component. The molding component constitutes a binder. A small amount of the molding component remains in the molding composition after degreasing. This fixes both between the powder particles and maintains the shape of the molded object in the degreasing state before sintering. The molding component is a component that disappears when the molding composition is sintered, like other binders.

[0026] The molding component is preferably composed of a polymer compound. The polymer compound is not particularly limited, but examples thereof include polystyrene, polyacetal, polyoxymethylene, polyoxyethylene, polyacrylic acid, polyacrylic acid ester, acrylonitrile-butadiene-styrene copolymer (ABS), polypropylene, polyamide, polybutylene terephthalate, polyethylene terephthalate, polycarbonate, acrylonitrile styrene copolymer, alkyl (meth)acrylate polymer, and copolymers of monomers constituting these, as well as modified or unmodified forms of these polymer compounds. Furthermore, the molding component may be a blend of two or more of the above-mentioned polymer compounds.

[0027] When the molding composition contains a polymer compound as a molding component, the weight average content of the polymer compound is The molecular weight is preferably 4000 or less. If the molecular weight of the polymer compound of the molding component is 4000 or less, the flowability of the molding composition can be further improved. This makes it possible to more quickly and stably form a molded object with good shape accuracy. In addition, if the weight average molecular weight is within this range, the softening point can also be lowered, which also makes it possible to further increase the flowability of the molding composition.

[0028] The blending amount of the molding components in the molding composition is 25% by mass or more and 35% by mass or less, preferably 27% by mass or more and 33% by mass or less, more preferably 28% by mass or more and 32% by mass or less, and even more preferably 29% by mass or more and 31% by mass or less, when the components of the molding composition excluding the powder, i.e., the binder, is taken as 100% by mass. If the blending amount of the molding components is within this range, a shaped object formed using the molding composition can have better shape stability.

[0029] 1.5. Plasticizers The molding composition of the present embodiment may contain a plasticizer. The plasticizer has a function of promoting mixing of the binder component and the molding composition, thereby making the molding composition into a homogeneous mixture.

[0030] Examples of the plasticizer include bis(2-ethylhexyl) terephthalate (specific gravity 0.984 (density 0.981), boiling point 416°C), diisononyl phthalate (specific gravity 0.976 (density 0.981), boiling point 403°C), diundecyl phthalate (specific gravity 0.955 (density 0.952), boiling point 523°C), diisodecyl phthalate (density 0.970, boiling point 420°C), bis(2-ethylhexyl) adipate (specific gravity 0.927 (density 0.924), boiling point 335°C), and ℃), diisononyl adipate (specific gravity 0.924 (density 0.921), boiling point 250℃ or higher), di-n-alkyl adipate (specific gravity 0.926 (density 0.923), boiling point 198 to 244℃ (665Pa)), diisodecyl adipate (specific gravity 0.92 (density 0.917), boiling point 244℃ (0.667kPa)), bis(2-butoxyethyl) adipate (specific gravity 1.00 (density 0.997), boiling point (217℃ / 1.5kPa)), etc. The plasticizers exemplified here are also environmentally friendly.

[0031] If the molding compound contains a plasticizer, the density of the plasticizer is 1.0 g / cm 3 It is preferable that the density is 0.990 g / cm or less. 3 More preferably, it is 0.985 g / cm or less. 3It is more preferable that the content of the plasticizer is not more than 1. When such a plasticizer is contained, the plasticizer can generate voids at the molecular level in the composition, thereby making it possible to further improve the fluidity of the composition.

[0032] When a plasticizer is contained in the molding composition, the blending amount of the plasticizer is 5% by mass or more and 25% by mass or less, preferably 10% by mass or more and 20% by mass or less, more preferably 13% by mass or more and 19% by mass or less, and even more preferably 15% by mass or more and 17% by mass or less, based on 100% by mass of the components of the molding composition excluding the powder, i.e., the binder. If the blending amount of the plasticizer is within this range, the molding composition can have better fluidity.

[0033] 1.6. Binder ratio etc. When considering reducing the viscosity of a molding composition, it is thought that the viscosity can be reduced by increasing the proportion of the binder in the molding composition. However, simply increasing the amount of binder in this way results in the binder being lost during sintering, which makes the molded product more susceptible to thermal shrinkage, and makes the molded product more susceptible to warping, cracking, and distortion.

[0034] In contrast, in the molding composition of the present embodiment, when the powder volumetric filling rate is high, for example, 64.8% or more, the thermal shrinkage of the molded object can be suppressed. When the blending amount of dye is less than about 35.2 volume %, the amount of components lost during debinding and sintering is small, which allows for the production of high density molded objects.

[0035] Generally, when the amount of binder is kept low, the viscosity of the molding composition increases, and the injection amount from the molding device may decrease. However, the molding composition of the present embodiment has a specific binder composition, and while keeping the amount of binder low, it is possible to obtain viscosity characteristics and injection amount characteristics that are equal to or greater than those when a larger amount of binder is blended.

[0036] In three-dimensional modeling, a high-temperature modeling process is stably carried out on a scale of several to several tens of hours, so that a high-boiling point material is often blended into the molding composition used. The relatively low-boiling point material in the binder composition in the molding composition of this embodiment is a wax having a fluidity function and a plasticizer blended as necessary. In general, the use of a high-boiling point material shows a tendency for the viscosity to increase, and it has been difficult to achieve both suitability for high-temperature processes and low viscosity. However, according to the molding composition of this embodiment, it is possible to suppress the viscosity of the molding composition low and obtain good fluidity while using a high-boiling point material.

[0037] 1.7. Other Effects In an injection molding machine, generally, as described in Japanese Patent Nos. 5970895, 5970794, and 5857688, an injection pressure of 5 to 500 MPa is required. However, when the molding composition of the present embodiment is used, the injection pressure is required to be 500 MPa or less at a shear rate of 0.1 s -1 This makes it possible to improve the powder filling rate while suppressing a decrease in the injection amount.

[0038] The molding composition of this embodiment contains the binder as described above, but the binder is composed of a plurality of components. This allows the components to melt, decompose, and evaporate at different times during the degreasing and sintering processes. For example, when the molding composition is heated to about 500°C for degreasing, the flow component and plasticizer decompose at a temperature of about 200 to 300°C, and the adhesive component and molding component decompose at a temperature of about 300 to 500°C. This can further increase the shape stability during degreasing.

[0039] 2. Examples and Comparative Examples The present invention will be described in more detail below with reference to examples and comparative examples, but the present invention can be modified in various ways without departing from the spirit of the invention, and is not limited to the following examples. Note that percentages and parts used for the amounts of components are by weight unless otherwise specified.

[0040] 2.1. Preparation of the molding composition Each example molding composition was prepared as follows. Using a pressure kneader mixer (TD0.3-3M manufactured by Toshin Corporation), the mixture was mixed at a temperature of 110°C, a rotation speed of 30 rpm, and a pressure of 0 MPa ((1) about 900 g of metal powder was added and mixed for 5 minutes, (2) the wax, adhesive component, and molding component were added, followed by the remaining metal powder and mixed for 3 minutes, and (3) the plasticizer was added and mixed for 2 minutes), followed by mixing at a temperature of 110°C, a rotation speed of 30 rpm, and a pressure of 0.5 MPa. The component compositions of each example are shown in Table 1.

[0041] [Table 1]

[0042] In the table, the materials and compounds are as follows. PW130: Paraffin Wax 130 (manufactured by Nippon Seiro Co., Ltd., melting point 56°C) ·PW115: Paraffin Wax 115 (manufactured by Nippon Seiro Co., Ltd., melting point 48°C) ·CG-5001: Bondfast (registered trademark) CG-5001 (manufactured by Sumitomo Chemical Co., Ltd., MFR = 380g / 10min) LOTADER 8210: LOTADER (registered trademark) 8210 (ARKEMA Corporation, MFR = 200g / 10min) BF-7M: Bondfast (registered trademark) BF-7M (manufactured by Sumitomo Chemical Co., Ltd., MFR = 7g / 10min) ST-95: Hymer (registered trademark) ST-95 (manufactured by Sanyo Chemical Industries, Ltd., polystyrene, weight average molecular weight = 4000) DIDP: Diisodecyl phthalate (Kanto Chemical Co., Ltd. (density 0.970, boiling point 420℃)) DBP: Dibutyl phthalate (Kanto Chemical Co., Ltd. (density 1.048)) Metal powder: (SUS630, PF-5K D50~4μm) manufactured by Epson Atmix Corporation

[0043] The molding composition kneaded as described above was made into a pellet state at 50 to 100° C. using a hand truder (PM-1, manufactured by Toyo Seiki Seisakusho Co., Ltd.).

[0044] 2.2. Evaluation of molding compositions 2.2.1. Viscosity The viscosity of each molding composition was measured using a rheometer (manufactured by UBC Corporation, Rheosol G3000NT-HR). -1 Measured up to around 0.1s -1 The viscosity at this time was read, and the value normalized with the viscosity of Example 1 is shown in Table 1.

[0045] 2.2.2.Evaluation of injection volume The molding composition of each example was introduced into a three-dimensional modeling device and injected for 30 seconds under conditions of 125°C and 2 MPa. The weight of the injected composition was measured, and the injection amount of each example was calculated. An injection amount that was 80% or more of the injection amount of Example 1 was judged as "A", and an injection amount that was less than 80% was judged as "B".

[0046] 2.2.3.Warpage evaluation Using a three-dimensional modeling device, a molded object with a minor axis width of 5 mm, a major axis width of 65 mm, and a thickness of 2 mm was molded using the molding composition of each example. Then, each test piece was placed on a horizontal table, and an image was taken from the direction along the minor axis using a camera. From the captured image, the distance Δx in the thickness direction between the end of the major axis width and the table was measured at both ends. Then, the warpage angle θ was calculated based on the following formula (1). tan θ = 2×Δx / 65 (1)

[0047] 2.2.4. Evaluation Results The adhesive composition includes a powder, a wax, an adhesive component, a molding component, and a plasticizer, and the adhesive component has a melt flow rate of 200 g / 10 min or more at 190° C., and the density of the plasticizer is 1.0 g / cm 3 The molding compositions of the following Examples had significantly lower viscosities than the compositions of the other Comparative Examples, and also had very good injection volumes.

[0048] In addition, warping was observed in the molded object when the metal filling rate was about 55%. At all levels of the Examples and Comparative Examples shown in Table 1, the filling rate was high at over 64.8%, so warping was almost zero. As a result of the above, the effect of reducing the number of binder parts was observed.

[0049] The present invention has substantially the same configuration, e.g., function, method, and This includes configurations that achieve the same results or have the same purpose and effect. The present invention also includes configurations that replace non-essential parts of the configurations described in the embodiments. The present invention also includes configurations that achieve the same effects as the configurations described in the embodiments or that can achieve the same purpose. The present invention also includes configurations that add publicly known technology to the configurations described in the embodiments.

[0050] The following can be derived from the above-described embodiment and modified examples.

[0051] One embodiment of the molding composition is The composition includes a powder, a wax, an adhesive component, a molding component, and a plasticizer, The melt flow rate of the adhesive component at 190°C is 200 g / 10 min or more, and the density of the plasticizer is 1.0 g / cm 3 The following is the result.

[0052] This molding composition has a low viscosity and therefore good flowability, which makes it possible to rapidly and stably form a model with good shape accuracy when used in a three-dimensional modeling apparatus.

[0053] In the above molding composition embodiment, The powder may have a volumetric packing rate of 64.8% or more.

[0054] This molding composition contains few components other than the powder. Therefore, this molding composition is less likely to experience thermal shrinkage than a molding composition containing many components other than the powder. In addition, this molding composition loses few components during debinding and sintering. This allows for the production of high-density molded objects.

[0055] In the above molding composition embodiment, The molding component includes a polymer compound, The polymer compound may have a weight average molecular weight of 4000 or less.

[0056] This molding composition contains a molding component having a low molecular weight, and therefore has better flowability, which makes it possible to more quickly and stably form a shaped object having good shape accuracy.

[0057] In the above molding composition embodiment, The powder may be a metal powder.

[0058] This molding composition makes it possible to rapidly and stably form a sintered body of metal powder with good shape accuracy.

[0059] One aspect of the method for producing a three-dimensional object includes a layer-forming step of discharging the molding composition, and the layer-forming step is carried out a plurality of times.

[0060] According to this method for manufacturing a three-dimensional object, the injection amount can be kept stable, so that a three-dimensional object can be manufactured with high accuracy.

Claims

1. The composition includes a powder, a wax, an adhesive component, a molding component other than the adhesive component, and a plasticizer, the adhesive component is a copolymer of two or more monomers selected from ethylene-based, acrylic-based, and vinyl-based monomers; The adhesive component has a melt flow rate of 200 g / 10 min or more at 190° C.; The density of the plasticizer is 0.97 g / cm 3 A molding composition, which is:

2. In claim 1, A molding composition, wherein the powder has a volumetric filling rate of 64.8% or more.

3. In any one of claims 1 and 2, The molding component includes a polymer compound, The weight average molecular weight of the polymer compound is 4,000 or less.

4. In any one of claims 1 to 3, The molding composition, wherein the powder is a metal powder.

5. A method for producing a three-dimensional object, comprising: a layer-forming step of discharging the molding composition according to claim 1 ; and performing the layer-forming step a plurality of times.

Citation Information

Patent Citations

  • Composition for injection-molding metal powder

    JP1991013502A

  • Manufacture of metallic or ceramic product

    JP2000144205A

  • Composition for three-dimensional printer

    JP2019188744A

  • Composition for three-dimensional printer, and method for manufacturing large-sized laminate molded article using the composition

    JP2020015848A

  • Composition for 3D printer

    WO2020003901A1