Anode active material, secondary battery, and method for producing anode active material
A granular graphite structure with an uneven surface and a surface layer of dispersed silicon particles addresses the adhesive strength issue in existing materials, enhancing the performance of secondary batteries by improving initial discharge capacity and retention rates.
Patent Information
- Application Number
- JP2023111321
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2021-12-03
- Filing Date
- 2023-07-06
- Publication Date
- 2024-09-18
- Estimated Expiration
- 2042-10-27
AI Technical Summary
Existing negative electrode active materials for secondary batteries, such as those combining silicon and graphite, suffer from insufficient adhesive strength, leading to poor initial discharge capacity, capacity retention rate, and charge/discharge capacity due to volumetric expansion and contraction during charging and discharging.
A granular structure of graphite with an uneven surface and a surface layer containing dispersed silicon particles in a matrix phase, where the silicon particles are flaky and crystalline, with a specific depth of penetration and pore volume, enhances adhesive strength and stability, improving the balance of discharge capacity and retention.
The improved adhesive strength between graphite and silicon particles results in a secondary battery with high initial discharge capacity, capacity retention rate, and charge/discharge capacity, maintaining excellent balance of these characteristics.
Smart Images

Figure 0007552803000004 
Figure 0007552803000009 
Figure 0007552803000010
Abstract
Description
[Technical field]
[0001] The present invention relates to a negative electrode active material and a secondary battery including the negative electrode active material. The present invention also relates to a method for producing the negative electrode active material. [Background technology]
[0002] Non-aqueous electrolyte secondary batteries are used in portable devices, hybrid and electric vehicles, home storage batteries, and the like, and are required to have a good balance of multiple properties such as electric capacity, safety, and operational stability. In non-aqueous electrolyte secondary batteries, lithium intercalation compounds that release lithium ions from between layers are mainly used as negative electrode materials, and lithium ions can be absorbed and released between layers between crystal planes during charging and discharging. For example, various lithium ion batteries using carbonaceous materials such as graphite as negative electrode active materials have been developed and are in practical use. Furthermore, in recent years, with the miniaturization of various electronic devices and communication devices and the rapid spread of hybrid automobiles and the like, there is a strong demand for the development of secondary batteries that have higher capacity and further improved various battery characteristics, such as cycle characteristics and discharge rate characteristics, as the driving power source for these devices and the like.
[0003] In order to further increase the capacity of secondary batteries, attempts have been made to use silicon, an element that has a high theoretical capacity and is capable of absorbing and releasing lithium ions, in combination with graphite and the like that have conventionally been used as negative electrode active materials. For example, Patent Documents 1 and 2 disclose soft carbon materials for use as negative electrode materials in lithium-ion secondary batteries, which include a nanomaterial coating supported on the surface layer of soft carbon powder particles and a conductive carbon layer covering the outer surface of the nanomaterial coating. However, it is believed that the soft carbon supported with the nanomaterial has many voids. If many voids are present, the effect of suppressing contact between the nanomaterial and the electrolyte during charging and discharging is limited, and as a result, the decomposition reaction of the electrolyte proceeds on the nanoparticles, and the performance degradation of the active material may be unavoidable.
[0004] Patent Document 3 discloses an anode material including composite particles in which amorphous carbon containing specific nanosilicon is attached to the surface of graphite particles. Patent Document 4 discloses an anode material for lithium ion batteries including a granular active material made of graphite and a network structure having a plurality of CO-Si bonds provided on a part of the surface of the granular active material. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] JP 2015-128045 A [Patent Document 2] Special Publication No. 2017-526118 [Patent Document 3] WO2020 / 088248 issue [Patent Document 4] JP 2020-64876 A Summary of the Invention [Problem to be solved by the invention]
[0006] However, even with the negative electrode active material described in the above document, further improvements are required in the initial discharge capacity and capacity retention rate when used in a secondary battery, and further improvements are required in the charge / discharge capacity.
[0007] The inventors focused on the adhesive strength between graphite, which is the base material of the negative electrode active material, and the silicon particles used in combination, and discovered that by increasing the adhesive strength between the two, it is possible to further improve the performance of the negative electrode active material, thereby completing the present invention. That is, an object of the present invention is to provide a negative electrode active material which provides a secondary battery having high initial discharge capacity, high capacity retention rate and high charge / discharge capacity, and which is well-balanced among these properties. [Means for solving the problem]
[0008] The present invention has the following aspects. [1] A negative electrode active material having a granular structure mainly made of graphite having an uneven surface, and a surface layer on at least a part of the surface of the granular structure, in which silicon particles having an average particle size of 20 nm to 200 nm are dispersed in a matrix phase. [2] The negative electrode active material according to [1], wherein the silicon particles are flaky and crystalline, and have a crystallite size of 40 nm or less at 2θ of 28.4° in X-ray diffraction. [3] The negative electrode active material according to [1] or [2], wherein the penetration depth of the surface layer into the recesses of the granular structure satisfies the following formula (1): 0.01≦B / A≦0.3 (1) In the formula (1), A represents the average particle diameter of the granular structures, and B represents the penetration depth of the surface layer into the recesses. [4] The granular structure has a cumulative pore volume of 0.001 cm for pores with diameters in the range of 3 nm to 300 nm. 3 / g or more of the negative electrode active material according to any one of [1] to [3]. [5] The graphite is natural graphite or artificial graphite, with an average particle size of 1 μm to 25 μm and a specific surface area of 0.5 m 2 / g to 20m 2 / g of the negative electrode active material according to any one of [1] to [4]. [6] The negative electrode active material according to any one of [1] to [5], wherein the mass of the surface layer is 1% by mass to 80% by mass, with the total mass of the negative electrode active material being 100%. [7] The negative electrode active material according to any one of [1] to [6], wherein the surface layer contains silicon oxycarbide, amorphous carbon, and the silicon particles, and the silicon particles account for 1 to 80 mass%, with the total mass of the surface layer being 100 mass%. [8] The negative electrode active material according to [7], wherein the surface layer further contains nitrogen. [9] The negative electrode active material according to any one of [1] to [8], wherein the silicon particles have a particle size broadly distributed from 5 nm to 300 nm.
[10] The granular structure has an average particle size of 1 μm to 30 μm and a specific surface area of 1 m 2 / g to 30m 2 / g of the negative electrode active material according to any one of [1] to [9].
[11] The negative electrode active material according to any one of [1] to
[10] , further comprising a carbon coating on the surface of the granular structures.
[12] The negative electrode active material according to
[11] , wherein the carbon coating is present in an amount of 1 to 10 mass % relative to 100 mass % of the total mass of the negative electrode active material.
[0009] The present invention also has the following aspects.
[13] A method for producing the negative electrode active material according to any one of [1] to
[13] above, comprising the following steps (1) to (3): Step (1) Obtaining a precursor for producing a surface layer Step (2) A step of applying the precursor for producing a surface layer to the surface of a granular structure mainly made of graphite and having an uneven surface. Step (3) A step of obtaining a negative electrode active material by high-temperature firing at a firing temperature of 1000°C to 1300°C in an inert atmosphere.
[14] A method for producing a negative electrode active material, comprising coating the powder of the negative electrode active material obtained in
[13] with a carbon film in a chemical vapor deposition apparatus at a temperature ranging from 700°C to 1000°C in a flow of a pyrolyzable carbon source gas and a carrier inert gas.
[0010] Further, the present invention has the following aspects.
[15] A secondary battery comprising the negative electrode active material according to any one of [1] to
[14] . Effect of the Invention
[0011] According to the present invention, there are provided a negative electrode active material which provides a secondary battery having high initial discharge capacity, high capacity retention rate, and high charge / discharge capacity, and which has an excellent balance of these properties, and a secondary battery using the negative electrode active material. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0012] The negative electrode active material of the present invention (hereinafter also referred to as "the present negative electrode active material") has a granular structure (hereinafter also referred to as "the present granular structure") mainly made of graphite having unevenness on its surface, and a surface layer on at least a part of the surface of the present granular structure in which silicon particles having an average particle size of 20 nm to 200 nm are dispersed in a matrix phase. In the past, the use of silicon, which has a higher theoretical capacity than graphite, has been considered in order to increase the capacity of lithium secondary batteries. However, it is known that silicon expands in volume by up to about three to four times as lithium is inserted, causing it to collapse or peel off from the electrode. As a result, it is known that when an active material containing silicon is used in the negative electrode, the cycle characteristics of the resulting lithium secondary battery are reduced.
[0013] In order to suppress the volume expansion, methods have been proposed in which the surface of graphite is coated with or attached to silicon particles, methods of introducing a three-dimensional network structure, and the like, as described in Patent Documents 1 to 4. However, in Patent Documents 1 to 4, the strength between the graphite and the silicon particles is insufficient, and it is believed that peeling or detachment of the silicon particles due to the volume expansion and contraction of the active material during charging and discharging is not suppressed. The negative electrode active material uses a granular structure mainly composed of graphite with an uneven surface, and at least a part of the surface of the granular structure has a surface layer in which silicon particles are dispersed in a matrix phase, which is believed to improve the strength between the graphite and the silicon particles. As a result, the initial discharge capacity, capacity retention rate, and charge / discharge capacity of a secondary battery using the negative electrode active material are believed to be improved.
[0014] The present granular structure is mainly composed of graphite. The graphite content is preferably more than 50 mass%, and more preferably 80 mass% or more, based on 100 mass% of the mass of the present granular structure. Examples of the graphite that is the main component include natural graphite, artificial graphite, and amorphous carbon such as hard carbon or soft carbon. From the viewpoint of the initial discharge capacity or the charge / discharge capacity, the graphite is preferably natural graphite or artificial graphite. In addition to graphite, the granular structure may contain carbon nanotubes or carbon fibers, or a small amount of a binder used during the granulation process.
[0015] When the graphite is natural or artificial, the average particle size of the graphite is between 1 μm and 25 μm, and the specific surface area is 0.5 m 2 / g to 20m 2 / g is preferable from the viewpoint of achieving both an improvement in the surface layer adhesive strength by roughening the graphite particle surface and suppression of side effects on the graphite surface during charging and discharging. The average particle size is the D50 value, which can be measured using a laser diffraction particle size analyzer or the like. D50 can be measured by dynamic light scattering using a laser particle size analyzer or the like. The average particle size is the particle size at which the cumulative volume distribution curve is drawn from the small diameter side in the particle size distribution, and the cumulative volume distribution curve reaches 50%. Hereinafter, the average particle size refers to D50. The specific surface area is the BET specific surface area determined by nitrogen gas adsorption measurement using a specific surface area measuring device according to the BET formula. Hereinafter, the specific surface area refers to the BET specific surface area.
[0016] The present granular structure has an uneven surface. The uneven surface may be formed on a part of the surface of the present granular structure, and may be formed on the entire surface. The uneven surface may be formed continuously or discontinuously on the surface of the present granular structure. The uneven surface may be formed regularly or irregularly. The uneven portion may be formed, for example, by roughening the surface of the granular structure, or may be formed by forming a plurality of holes in the surface. When a plurality of holes are formed, the holes may be open holes or interconnected holes.
[0017] The depth of the unevenness, which is the average distance between the deepest and highest parts of adjacent uneven parts, is preferably 0.01 or more, more preferably 0.05 or more, in terms of the adhesive strength between the surface layer and the present granular structure, as described later. If the depth of the unevenness is 0.3 or more, the mechanical performance of the granular structure may be reduced, and the surface layer may not easily enter the uneven parts of the granular structure, resulting in voids in the active material, which may cause a reduction in performance due to the penetration of the electrolyte during charging and discharging. The cross-sectional shape of the uneven portion may be, for example, a triangle, a rectangle, a semicircle, a semi-ellipse, or the like, and a mixture of a plurality of these shapes may be used.
[0018] The average particle size of the granular structure is preferably from 1 μm to 30 μm, and more preferably from 3 μm to 20 μm. The specific surface area of the granular structure is 1 m 2 / g to 30m 2 / g is preferred, 3m 2 / g to 20m 2 When the specific surface area is within the above range, an appropriate surface void can be maintained in order to maintain the adhesion with the surface layer.
[0019] The granular structure has a cumulative pore volume of pores having diameters in the range of 3 nm to 300 nm of 0.001 cm3 from the viewpoint of maintaining adhesion to the surface layer. 3 / g or more is preferable. The cumulative pore volume of the pore diameter is the cumulative pore volume of the pores with a pore diameter in the range of 2 nm to 100 nm among the pores measured by mercury intrusion porosimetry. Here, the mercury intrusion porosimetry is a method of injecting mercury into the hardened body and measuring the pore diameter distribution from the relationship between the pressure and the amount of intrusion, and the calculation is performed assuming that the shape of the pores is cylindrical. The cumulative pore volume is 0.01 cm 3 The upper limit of the cumulative pore volume is usually 0.5 cm 3 / g.
[0020] The present negative electrode active material has a surface layer on at least a portion of the surface of the present granular structure, in which silicon particles (hereinafter also referred to as "the present silicon particles") having an average particle size of 20 nm to 200 nm are dispersed in a matrix phase. The average particle size of the silicon particles is the D50 value. From the viewpoint of improving cycle performance, the average particle size of the silicon particles is preferably 100 nm or less, more preferably 80 nm or less. Also, from the viewpoint of maintaining good dispersibility of silicon nanoparticles, the average particle size of the silicon particles is preferably 20 nm or more, more preferably 30 nm or more.
[0021] The particle size of the silicon particles is preferably distributed in a wide range of 5 nm to 300 nm while satisfying the average particle size. By using silicon particles with a wide range of different particle sizes, it is easy to increase the packing density of the silicon particles in the active material. The wide range of particle size distribution means that the particle size distribution shape is not particularly limited, and it is sufficient that the particles are present in the above particle size range. When the particle size of the silicon particles is distributed in a wide range, the particles may be concentrated in a part of the particle size range, and a normal distribution is preferable. Silicon particles with a wide range of particle size distribution can be produced, for example, by a dry or wet mechanical grinding method.
[0022] The silicon particles are composed of zero-valent silicon, and for example, a lump of silicon can be granulated by crushing or the like so that the average particle size falls within the above-mentioned range. Examples of the pulverizer used to pulverize the silicon lumps include pulverizers such as a ball mill, a bead mill, a jet mill, etc. The pulverization may be wet pulverization using an organic solvent, and as the organic solvent, for example, alcohols, ketones, etc. can be suitably used, but aromatic hydrocarbon solvents such as toluene, xylene, naphthalene, and methylnaphthalene can also be used. The conditions for crushing the silicon particles are appropriately controlled so that the average particle size falls within the above range, and the silicon particles are finally classified or otherwise processed to obtain the present silicon particles.
[0023] The shape of the silicon particles may be granular, needle-like, or flake-like as long as it satisfies the above-mentioned average particle size, but flake-like is preferred from the viewpoint of improving the active material performance. When the silicon particles are flake-like, they are crystalline, and it is preferred from the viewpoint of initial coulombic efficiency and capacity retention if the crystallite size obtained from the peak of 2θ of 28.4° in the X-ray diffraction spectrum is 40 nm or less. The crystallite size is more preferably 30 nm or less. Also, the crystallite size is more preferably 10 nm or more.
[0024] The compound constituting the matrix phase is preferably a compound containing silicon, oxygen, and carbon, and the compound containing silicon, oxygen, and carbon is preferably a three-dimensional network structure of a silicon-oxygen-carbon skeleton and a structure containing free carbon. Here, free carbon is carbon that is not contained in the three-dimensional skeleton of silicon-oxygen-carbon. Free carbon includes carbon that exists as a carbon phase, carbon that is bonded to carbon in the carbon phase, and carbon that is bonded to the silicon-oxygen-carbon skeleton and the carbon phase.
[0025] When the compound constituting the matrix phase is a compound containing silicon, oxygen, and carbon, and has a three-dimensional network structure of a silicon-oxygen-carbon skeleton and a structure containing free carbon, the silicon-oxygen-carbon skeleton in the matrix phase has high chemical stability, and the composite structure with the free carbon reduces the electronic transition resistance and facilitates the diffusion of lithium ions. The silicon particles are tightly wrapped in a composite structure of a silicon-oxygen-carbon skeleton and free carbon, preventing direct contact between the silicon particles and the electrolyte. As a result, when the negative electrode active material is used as a negative electrode, the silicon particles in the negative electrode play a role as a main component for expressing the charge / discharge performance, while chemical reactions between silicon and the electrolyte during charge / discharge are avoided, thereby preventing performance degradation of the silicon particles to the maximum extent possible.
[0026] In addition, when lithium ions approach the silicon-oxygen-carbon skeleton, the electron distribution inside the silicon-oxygen-carbon skeleton changes, forming electrostatic bonds and coordinate bonds between the silicon-oxygen-carbon skeleton and the lithium ions. These electrostatic bonds and coordinate bonds allow the lithium ions to be stored in the silicon-oxygen-carbon skeleton. On the other hand, because the coordinate bond energy is relatively low, the lithium ion desorption reaction occurs easily. In other words, it is believed that the silicon-oxygen-carbon skeleton can reversibly cause lithium ion insertion and desorption reactions during charging and discharging. When the matrix phase has a structure containing free carbon, the free carbon is preferably amorphous carbon.
[0027] When the compound constituting the matrix phase is a compound containing silicon, oxygen, and carbon, the matrix phase preferably contains silicon oxycarbide represented by the following formula (2). SiOxCy (2) In formula (2), x represents the molar ratio of oxygen to silicon, and y represents the molar ratio of carbon to silicon. When the present negative electrode active material is used in a secondary battery, from the viewpoint of obtaining an advantageous balance between charge / discharge performance and capacity retention rate, 1≦x≦2 is preferable, 1.1≦x≦1.8 is more preferable, and 1.2≦x≦1.7 is even more preferable. Furthermore, when the present negative electrode active material is used in a secondary battery, from the viewpoint of the balance between charge / discharge performance and initial charge / discharge efficiency, 1≦y≦20 is preferable, and 1.2≦y≦15 is more preferable.
[0028] The compound constituting the matrix phase may contain nitrogen in addition to silicon, oxygen, and carbon. Nitrogen can be introduced into the matrix phase by using raw materials, such as phenolic resins, dispersants, polysiloxane compounds, other nitrogen compounds, and nitrogen gas used in the firing process, in the manufacturing method of the present active material described below, by having an atomic group containing nitrogen as a functional group in the molecule. When the matrix phase contains nitrogen, the charge / discharge performance and capacity retention rate tend to be excellent when the present negative electrode active material is used. When the compound constituting the matrix phase is a compound containing silicon, oxygen, carbon and nitrogen, the matrix phase preferably contains a compound represented by the following formula (3). SiOxCyNz (3) In formula (3), x and y are as defined above, and z represents the molar ratio of nitrogen to silicon. When the matrix phase contains the compound represented by formula (3), from the viewpoint of charge / discharge performance and capacity retention rate when the active material is used in a secondary battery, it is preferable that 1≦x≦2, 1≦y≦20, and 0≦z≦0.5, and it is more preferable that 1.1≦x≦1.8, 1.2≦y≦15, and 0≦z≦0.4.
[0029] The x, y, and z can be determined by measuring the mass content of each element and then converting it into a molar ratio (atomic ratio). In this case, the oxygen and carbon contents can be quantified using an inorganic elemental analyzer, and the silicon content can be quantified using an inductively coupled plasma optical emission spectrometer (ICP-OES). It is preferable to measure x, y, and z by the above-mentioned method, but it is also possible to perform a local analysis of the active material, obtain a large number of measurement points of the content ratio data obtained thereby, and infer the content ratio of the entire negative electrode active material. Examples of local analysis include energy dispersive X-ray spectroscopy (SEM-EDX) and electron probe microanalyzer (EPMA).
[0030] The surface layer that the negative electrode active material has on at least a portion of the granular structure contains the silicon particles, the silicon oxycarbide as a matrix phase in which the silicon particles are dispersed, and amorphous carbon as the free carbon, and preferably contains the silicon particles in an amount of 1 to 80 mass%, with the total mass of the surface layer being 100 mass%. Examples of amorphous carbon include carbon obtained by pyrolysis of organic matter such as aromatic resins. In addition to the above, the surface layer preferably contains nitrogen from the viewpoint of the stability of the Si-O-C skeleton. When the surface layer contains nitrogen, the matrix phase preferably contains a compound represented by the above formula (3). The surface layer preferably contains 10% by mass or more of the present silicon particles, and more preferably 15% by mass or more, and preferably 80% by mass or less of the present silicon particles, and more preferably 70% by mass or less.
[0031] From the viewpoints of charge / discharge capacity, initial efficiency, and cycle performance, the present negative electrode active material preferably contains the surface layer in an amount of 1 to 80% by mass, based on the total mass of the present negative electrode active material being 100% by mass. From the viewpoint of improving charge / discharge capacity, the present negative electrode active material more preferably contains the surface layer in an amount of 5% by mass or more, and even more preferably contains 10% by mass or more, based on the total mass of the present negative electrode active material being 100% by mass. From the viewpoints of cycle performance and initial efficiency, the present negative electrode active material more preferably contains the surface layer in an amount of 70% by mass or less, and even more preferably contains 60% by mass or less, based on the total mass of the present negative electrode active material being 100% by mass. The total mass of the present negative electrode active material is the total mass of the present granular structure and the surface layer constituting the present negative electrode active material. When the matrix phase contains nitrogen, the total mass also includes nitrogen. When the present negative electrode active material contains a coating layer described below, the total mass of the present negative electrode active material is the total mass including the coating layer in addition to the above.
[0032] In addition, the present negative electrode active material has the surface layer on at least a portion of the surface of the present granular structure, but from the viewpoint of suppressing the specific surface area and streamlining the microstructure, it is preferable for the present granular structure to have the surface layer on more than 80% of the surface, and it is even more preferable for the present granular structure to have the surface layer on more than 90% of the surface.
[0033] In the present negative electrode active material, it is preferable that the penetration depth of the surface layer into the recesses of the granular structures satisfies the above formula (1). 0.01≦B / A≦0.3 (1) In the formula (1), A represents the average particle diameter of the granular structure, and B represents the penetration depth of the surface layer into the recesses, where A is the D50 and B is measured by SEM observation of the cross section of the particle. From the viewpoints of the strength of the granular structure and the surface layer adhesion, it is more preferable that A and B satisfy the following formula (4), and it is even more preferable that they satisfy the following formula (5). 0.05≦B / A≦0.25 (4) 0.10≦B / A≦0.20 (5)
[0034] The negative electrode active material may contain other necessary third components in addition to those mentioned above. The surface of the negative electrode active material may be coated with a coating material, which is preferably a material that is expected to have electronic conductivity, lithium ion conductivity, and the effect of inhibiting decomposition of the electrolyte.
[0035] When the surface of the present negative electrode active material is coated with the coating material, the average thickness of the coating is preferably 10 nm or more and 300 nm or less. The average thickness of the coating is preferably 20 nm or more and 200 nm or less. When the present negative electrode active material has a coating of the above average thickness, the present silicon particles exposed on the surface of the granular structure can be protected, and thus, when the present negative electrode active material is used, the chemical stability and thermal stability of the negative electrode active material are improved. As a result, the deterioration of the charge and discharge performance of the secondary battery can be further suppressed. When the surface of the present negative electrode active material is coated with the coating, the content of the coating is preferably 1 to 30 mass %, more preferably 3 to 25 mass %, based on the total mass of the present negative electrode active material being 100 mass %, from the viewpoint of improving the chemical stability and thermal stability of the negative electrode active material. The total mass of the present negative electrode active material is the same as that described above.
[0036] The coating film may be made of an electronic conductive material such as carbon, titanium, nickel, etc. Among these, from the viewpoint of improving the chemical stability and thermal stability of the negative electrode active material, carbon is preferred, and low-crystalline carbon is more preferred. When the coating is carbon, the average thickness of the carbon coating is preferably 10 nm to 300 nm, or the carbon content is preferably 1 to 10 mass % relative to the total amount of the present negative electrode active material, which is 100 mass %. The total amount of the present negative electrode active material is the same as above.
[0037] In the case of carbon coatings, the coating is preferably made by Chemical Vapor Deposition (CVD). In the case of a carbon coating, the scattering peak intensity ratio I (G band / D band) of the Raman spectrum is preferably in the range of 0.9 to 1.1. The specific surface area by the BET method is 3.5 m 2 / g or less, true density is 1.9g / cm 3 The above is preferred.
[0038] The present negative electrode active material has a high initial discharge capacity, a high capacity retention rate, and a high charge / discharge capacity, and also has an excellent balance of these properties. Therefore, a secondary battery using the present negative electrode active material as a battery negative electrode exhibits good charge / discharge properties. Specifically, a slurry containing the present negative electrode active material, an organic binder, and other components such as a conductive assistant as required can be applied to a copper foil current collector in the form of a thin film to form a negative electrode. Alternatively, a carbon material such as graphite can be added to the slurry to form a negative electrode. Examples of the carbon material include natural graphite, artificial graphite, and amorphous carbon such as hard carbon or soft carbon.
[0039] For example, the negative electrode active material and a binder, which is an organic binding material, are kneaded together with a solvent using a dispersing device such as a stirrer, a ball mill, a super sand mill, or a pressure kneader to prepare a negative electrode material slurry, which is then applied to a current collector to form a negative electrode layer. Alternatively, the negative electrode layer can be obtained by forming the paste-like negative electrode material slurry into a sheet, pellet, or other shape and integrating it with a current collector.
[0040] Examples of the organic binder include styrene-butadiene rubber copolymers (hereinafter also referred to as "SBR"); ethylenically unsaturated carboxylic acid esters such as methyl (meth)acrylate, ethyl (meth)acrylate, butyl (meth)acrylate, (meth)acrylonitrile, and hydroxyethyl (meth)acrylate, and unsaturated carboxylic acid copolymers such as (meth)acrylic copolymers composed of ethylenically unsaturated carboxylic acids such as acrylic acid, methacrylic acid, itaconic acid, fumaric acid, and maleic acid; and polymer compounds such as polyvinylidene fluoride, polyethylene oxide, polyepichlorohydrin, polyphosphazene, polyacrylonitrile, polyimide, polyamideimide, and carboxymethylcellulose (hereinafter also referred to as "CMC").
[0041] Depending on their physical properties, these organic binders may be dispersed or dissolved in water, or dissolved in an organic solvent such as N-methyl-2-pyrrolidone (NMP), etc. The content of the organic binder in the negative electrode layer of the lithium ion secondary battery negative electrode is preferably 1 mass % to 30 mass %, more preferably 2 mass % to 20 mass %, and even more preferably 3 mass % to 15 mass %.
[0042] When the content of the organic binder is 1% by mass or more, the adhesion is better and the destruction of the negative electrode structure due to the expansion or contraction during charging and discharging is more suppressed, whereas when the content is 30% by mass or less, the increase in the electrode resistance is more suppressed. Within this range, the present negative electrode active material has high chemical stability and can employ an aqueous binder, making it easy to handle in practical use.
[0043] In addition, the negative electrode material slurry may be mixed with a conductive assistant as necessary. Examples of the conductive assistant include carbon black, graphite, acetylene black, and oxides and nitrides that exhibit conductivity. The amount of the conductive assistant used may be about 1% by mass to 15% by mass with respect to the negative electrode active material of the present invention.
[0044] The material and shape of the current collector may be, for example, a strip of copper, nickel, titanium, stainless steel, etc. in the form of foil, perforated foil, mesh, etc. Also, porous materials such as porous metal (foamed metal) and carbon paper can be used.
[0045] Examples of the method for applying the negative electrode material slurry to the current collector include metal mask printing, electrostatic coating, dip coating, spray coating, roll coating, doctor blade, gravure coating, screen printing, etc. After application, it is preferable to perform a rolling treatment using a flat plate press, a calendar roll, etc., as necessary.
[0046] The negative electrode material slurry may be formed into a sheet or pellet shape, and this may be integrated with the current collector by, for example, rolling, pressing, or a combination of these.
[0047] The negative electrode layer formed on the current collector or the negative electrode layer integrated with the current collector is preferably heat-treated according to the organic binder used. For example, when SBR dispersed in water is used, the heat treatment may be performed at 100 to 130°C, and when an organic binder having a polyimide or polyamideimide as the main skeleton is used, the heat treatment is preferably performed at 150 to 450°C.
[0048] This heat treatment removes the solvent, hardens the binder, and increases the strength, improving the adhesion between the particles and between the particles and the current collector. Note that these heat treatments are preferably carried out in an inert atmosphere such as helium, argon, or nitrogen, or in a vacuum atmosphere, in order to prevent oxidation of the current collector during the treatment.
[0049] After the heat treatment, the negative electrode is preferably subjected to pressure treatment. In the negative electrode using this negative electrode active material, the electrode density is 1 g / cm 3 from 1.8 g / cm 3 and preferably 1.1 g / cm 3 to 1.7 g / cm 3 More preferably, it is 1.2 g / cm 3from 1.6 g / cm 3 It is more preferable that the electrode density is higher. The higher the electrode density, the more the adhesion and the volumetric capacity density of the electrode tend to improve. On the other hand, if the electrode density is too high, the voids in the electrode are reduced, which weakens the effect of suppressing the volumetric expansion of silicon and the like, and the capacity retention rate may decrease. Therefore, the optimal range of the electrode density is selected.
[0050] The secondary battery of the present invention contains the present negative electrode active material in the negative electrode. As a secondary battery having a negative electrode containing the present negative electrode active material, nonaqueous electrolyte secondary batteries and solid electrolyte secondary batteries are preferable, and the present negative electrode active material exhibits excellent performance particularly when used as the negative electrode of a nonaqueous electrolyte secondary battery.
[0051] When the secondary battery of the present invention is used as a wet electrolyte secondary battery, for example, the secondary battery of the present invention can be constructed by disposing a positive electrode and a negative electrode containing the negative electrode active material of the present invention opposite each other via a separator and injecting an electrolyte solution.
[0052] The positive electrode can be obtained by forming a positive electrode layer on the surface of a current collector in the same manner as the negative electrode. In this case, the current collector can be a strip of a metal or alloy such as aluminum, titanium, or stainless steel in the form of a foil, a perforated foil, a mesh, or the like.
[0053] There are no particular limitations on the positive electrode material used in the positive electrode layer. When preparing a lithium ion secondary battery among non-aqueous electrolyte secondary batteries, for example, a metal compound, metal oxide, metal sulfide, or conductive polymer material capable of doping or intercalating lithium ions may be used. For example, lithium cobalt oxide (LiCoO2), lithium nickel oxide (LiNiO2), lithium manganese oxide (LiMnO2), and composite oxides thereof (LiCoxNiyMnzO2, x+y+z=1), lithium manganese spinel (LiMn2O4), lithium vanadium compounds, V2O5, V6O 13, VO2, MnO2, TiO2, MoV2O8, TiS2, V2S5, VS2, MoS2, MoS3, Cr3O8, Cr2O5, olivine-type LiMPO4 (wherein M is Co, Ni, Mn, or Fe), conductive polymers such as polyacetylene, polyaniline, polypyrrole, polythiophene, polyacene, porous carbon, etc. can be used alone or in combination.
[0054] As the separator, for example, a nonwoven fabric, cloth, microporous film, or a combination thereof, mainly composed of polyolefin such as polyethylene or polypropylene can be used. Note that if the positive electrode and the negative electrode of the nonaqueous electrolyte secondary battery to be produced are not in direct contact with each other, there is no need to use a separator.
[0055] As the electrolyte, for example, a so-called organic electrolyte can be used in which a lithium salt such as LiClO4, LiPF6, LiAsF6, LiBF4, or LiSO3CF3 is dissolved in a non-aqueous solvent such as ethylene carbonate, propylene carbonate, butylene carbonate, vinylene carbonate, fluoroethylene carbonate, cyclopentanone, sulfolane, 3-methylsulfolane, 2,4-dimethylsulfolane, 3-methyl-1,3-oxazolidin-2-one, γ-butyrolactone, dimethyl carbonate, diethyl carbonate, ethyl methyl carbonate, methyl propyl carbonate, butyl methyl carbonate, ethyl propyl carbonate, butyl ethyl carbonate, dipropyl carbonate, 1,2-dimethoxyethane, tetrahydrofuran, 2-methyltetrahydrofuran, 1,3-dioxolane, methyl acetate, or ethyl acetate, or a mixture of two or more components.
[0056] The structure of the secondary battery of the present invention is not particularly limited, but usually, the positive electrode, the negative electrode, and a separator provided as necessary are wound into a flat spiral shape to form a wound electrode plate group, or these are stacked in a flat plate shape to form a stacked electrode plate group, and these electrode plate groups are sealed in an exterior body. Note that the half cells used in the examples of the present invention are mainly composed of the present active material in the negative electrode, and a simple evaluation was performed using metallic lithium in the counter electrode, in order to more clearly compare the cycle characteristics of the active material itself.
[0057] Secondary batteries using the present negative electrode active material are used, for example, as paper-type batteries, button-type batteries, coin-type batteries, laminated-type batteries, cylindrical batteries, square batteries, etc. The present negative electrode active material can also be applied to all electrochemical devices that use the insertion and desorption of lithium ions as a charge / discharge mechanism, such as hybrid capacitors and solid-state lithium secondary batteries.
[0058] The present negative electrode active material can be produced, for example, by a method including the following steps (1) to (3). Note that the following steps are exemplified by using a polysiloxane compound as the matrix phase, but the method is not limited to these steps. Step (1) Obtaining a precursor for producing a surface layer Step (2) A step of applying the precursor for producing a surface layer to the surface of a granular structure mainly made of graphite and having an uneven surface. Step (3) A step of obtaining a negative electrode active material by high-temperature firing at a firing temperature of 1000°C to 1300°C in an inert atmosphere.
[0059] <Process (1)> A precursor for forming the surface layer, which provides the surface layer having silicon particles dispersed in a matrix phase, is prepared by the following method. The silicon particles are obtained, for example, by crushing silicon chunks in a wet powder crushing device using an organic solvent. A dispersant may be used to promote crushing of the silicon chunks in the organic solvent. Commercially available silicon powder or large-diameter silicon particles are used as the silicon chunks. The wet grinding device is not particularly limited, and examples thereof include a roller mill, a high-speed rotary grinder, a container-driven mill, and a bead mill. In wet grinding, it is preferable to grind the silicon particles until they reach the particle size of the present silicon particles.
[0060] The organic solvent used in the wet method is an organic solvent that does not chemically react with silicon, such as ketones such as acetone, methyl ethyl ketone, methyl isobutyl ketone, and diisobutyl ketone; alcohols such as ethanol, methanol, normal propyl alcohol, and isopropyl alcohol; and aromatics such as benzene, toluene, and xylene.
[0061] The type of dispersant includes aqueous and non-aqueous dispersants. In order to suppress excessive oxidation on the surface of silicon particles, it is preferable to use a non-aqueous dispersant. The type of non-aqueous dispersant includes polymer types such as polyethers, polyalkylene polyamines, and polycarboxylic acid partial alkyl esters, low molecular types such as polyhydric alcohol esters and alkyl polyamines, and inorganic types such as polyphosphates. The concentration of silicon in wet grinding is not particularly limited, but when the solvent and, if necessary, a dispersant are included, the total amount of the dispersant and silicon is 100 mass%, and the amount of silicon is preferably in the range of 5 mass% to 40 mass%, more preferably 10 mass% to 30 mass%.
[0062] When silicon particles having a particle size broadly distributed from 5 nm to 300 nm are used as the silicon particles, such silicon particles can be produced by the following method. Using a wet bead mill device, multiple grinding conditions such as the amount of dispersant added, bead diameter, rotation speed, and grinding time can be controlled.
[0063] A polysiloxane compound can be used as a raw material for the matrix phase in which the silicon particles are dispersed. The polysiloxane compound is a resin containing at least one of a polycarbosilane structure, a polysilazane structure, a polysilane structure, and a polysiloxane structure. The resin may contain only these structures, or may be a composite resin having at least one of these structures as a segment and chemically bonded to other polymer segments. The form of the composite may be graft copolymerization, block copolymerization, random copolymerization, alternating copolymerization, etc. For example, there is a composite resin having a graft structure in which a polysiloxane segment is chemically bonded to the side chain of a polymer segment, and a composite resin having a block structure in which a polysiloxane segment is chemically bonded to the end of a polymer segment.
[0064] The polysiloxane segment preferably has a structural unit represented by the following general formula (S-1) and / or the following general formula (S-2): In particular, the polysiloxane compound more preferably has a carboxy group, an epoxy group, an amino group, or a polyether group on the side chain or terminal of the siloxane bond (Si-O-Si) main skeleton.
[0065] [ka]
[0066] [ka] (In the above general formulas (S-1) and (S-2), R 1 R represents an aromatic hydrocarbon group, an alkyl group, an epoxy group, a carboxy group, or the like, which may have a substituent. 2 and R 3 respectively represent an alkyl group, a cycloalkyl group, an aryl group or an aralkyl group, an epoxy group, a carboxy group, etc.)
[0067] Examples of the alkyl group include a methyl group, an ethyl group, a propyl group, an isopropyl group, a butyl group, an isobutyl group, a sec-butyl group, a tert-butyl group, a pentyl group, an isopentyl group, a neopentyl group, a tert-pentyl group, a 1-methylbutyl group, a 2-methylbutyl group, a 1,2-dimethylpropyl group, a 1-ethylpropyl group, a hexyl group, an isohexyl group, a 1-methylpentyl group, a 2-methylpentyl group, a 3-methylpentyl group, a 1,1-dimethylbutyl group, a 1,2-dimethylbutyl group, a 2,2-dimethylbutyl group, a 1-ethylbutyl group, a 1,1,2-trimethylpropyl group, a 1,2,2-trimethylpropyl group, a 1-ethyl-2-methylpropyl group, a 1-ethyl-1-methylpropyl group, etc. Examples of the cycloalkyl group include a cyclopropyl group, a cyclobutyl group, a cyclopentyl group, a cyclohexyl group, etc.
[0068] Examples of the aryl group include a phenyl group, a naphthyl group, a 2-methylphenyl group, a 3-methylphenyl group, a 4-methylphenyl group, a 4-vinylphenyl group, and a 3-isopropylphenyl group.
[0069] Examples of the aralkyl group include a benzyl group, a diphenylmethyl group, and a naphthylmethyl group.
[0070] Examples of polymer segments other than the polysiloxane segment contained in the polysiloxane compound include vinyl polymer segments such as acrylic polymers, fluoroolefin polymers, vinyl ester polymers, aromatic vinyl polymers, and polyolefin polymers, as well as polymer segments such as polyurethane polymer segments, polyester polymer segments, and polyether polymer segments. Among these, vinyl polymer segments are preferred.
[0071] The polysiloxane compound may be a composite resin in which a polysiloxane segment and a polymer segment are bonded in a structure represented by the following structural formula (S-3), or may have a three-dimensional network polysiloxane structure.
[0072] [ka] (In the formula, the carbon atom is a carbon atom constituting a polymer segment, and the two silicon atoms are silicon atoms constituting a polysiloxane segment).
[0073] The polysiloxane segment of the polysiloxane compound may have a functional group capable of reacting by heating, such as a polymerizable double bond, in the polysiloxane segment. By subjecting the polysiloxane compound to heat treatment before thermal decomposition, a crosslinking reaction progresses and the compound is solidified, which makes it easy to carry out the thermal decomposition treatment.
[0074] Examples of the polymerizable double bond include a vinyl group and a (meth)acryloyl group. The number of polymerizable double bonds in the polysiloxane segment is preferably 2 or more, more preferably 3 to 200, and even more preferably 3 to 50. In addition, by using a composite resin having 2 or more polymerizable double bonds as the polysiloxane compound, the crosslinking reaction can be easily promoted.
[0075] The polysiloxane segment may have a silanol group and / or a hydrolyzable silyl group. Examples of the hydrolyzable group in the hydrolyzable silyl group include a halogen atom, an alkoxy group, a substituted alkoxy group, an acyloxy group, a phenoxy group, a mercapto group, an amino group, an amide group, an aminooxy group, an iminoxy group, and an alkenyloxy group. The hydrolyzable silyl group becomes a silanol group by hydrolysis of these groups. In parallel with the thermosetting reaction, a hydrolysis condensation reaction proceeds between the hydroxyl group in the silanol group and the hydrolyzable group in the hydrolyzable silyl group, thereby obtaining a solid polysiloxane compound.
[0076] The silanol group in the present invention is a silicon-containing group having a hydroxyl group directly bonded to a silicon atom. The hydrolyzable silyl group in the present invention is a silicon-containing group having a hydrolyzable group directly bonded to a silicon atom, and specifically includes, for example, a group represented by the following general formula (S-4).
[0077] [ka] (In the formula, R 4 R represents a monovalent organic group such as an alkyl group, an aryl group, or an aralkyl group. 5 is a halogen atom, an alkoxy group, an acyloxy group, an allyloxy group, a mercapto group, an amino group, an amido group, an aminooxy group, an iminoxy group, or an alkenyloxy group, and b is an integer of 0 to 2.
[0078] Examples of the alkyl group include a methyl group, an ethyl group, a propyl group, an isopropyl group, a butyl group, an isobutyl group, a sec-butyl group, a tert-butyl group, a pentyl group, an isopentyl group, a neopentyl group, a tert-pentyl group, a 1-methylbutyl group, a 2-methylbutyl group, a 1,2-dimethylpropyl group, a 1-ethylpropyl group, a hexyl group, an isohexyl group, a 1-methylpentyl group, a 2-methylpentyl group, a 3-methylpentyl group, a 1,1-dimethylbutyl group, a 1,2-dimethylbutyl group, a 2,2-dimethylbutyl group, a 1-ethylbutyl group, a 1,1,2-trimethylpropyl group, a 1,2,2-trimethylpropyl group, a 1-ethyl-2-methylpropyl group, and a 1-ethyl-1-methylpropyl group.
[0079] Examples of the aryl group include a phenyl group, a naphthyl group, a 2-methylphenyl group, a 3-methylphenyl group, a 4-methylphenyl group, a 4-vinylphenyl group, and a 3-isopropylphenyl group.
[0080] Examples of the aralkyl group include a benzyl group, a diphenylmethyl group, and a naphthylmethyl group.
[0081] Examples of the halogen atom include a fluorine atom, a chlorine atom, a bromine atom, and an iodine atom.
[0082] Examples of the alkoxy group include a methoxy group, an ethoxy group, a propoxy group, an isopropoxy group, a butoxy group, a sec-butoxy group, and a tert-butoxy group.
[0083] Examples of the acyloxy group include a formyloxy group, an acetoxy group, a propanoyloxy group, a butanoyloxy group, a pivaloyloxy group, a pentanoyloxy group, a phenylacetoxy group, an acetoacetoxy group, a benzoyloxy group, and a naphthoyloxy group.
[0084] Examples of the allyloxy group include a phenyloxy group and a naphthyloxy group.
[0085] Examples of the alkenyloxy group include a vinyloxy group, an allyloxy group, a 1-propenyloxy group, an isopropenyloxy group, a 2-butenyloxy group, a 3-butenyloxy group, a 2-pentenyloxy group, a 3-methyl-3-butenyloxy group, and a 2-hexenyloxy group.
[0086] Examples of the polysiloxane segment having the structural unit represented by the above general formula (S-1) and / or the above general formula (S-2) include those having the following structures.
[0087] [ka]
[0088] [ka]
[0089] [ka]
[0090] The polymer segment may have various functional groups as necessary within the scope of not impairing the effects of the present invention. Examples of such functional groups include a carboxyl group, a blocked carboxyl group, a carboxylic anhydride group, a tertiary amino group, a hydroxyl group, a blocked hydroxyl group, a cyclocarbonate group, an epoxy group, a carbonyl group, a primary amide group, a secondary amide group, a carbamate group, and a functional group represented by the following structural formula (S-5).
[0091] [ka]
[0092] The polymer segment may also have a polymerizable double bond such as a vinyl group or a (meth)acryloyl group.
[0093] The polysiloxane compound is preferably produced, for example, by the following methods (4) to (6).
[0094] (4) A method in which a polymer segment containing a silanol group and / or a hydrolyzable silyl group is prepared in advance as a raw material for the polymer segment, and this polymer segment is mixed with a silane compound having both a silanol group and / or a hydrolyzable silyl group and a polymerizable double bond, followed by a hydrolysis and condensation reaction.
[0095] (5) A method in which a polymer segment containing a silanol group and / or a hydrolyzable silyl group is prepared in advance as a raw material for the polymer segment. A polysiloxane is also prepared in advance by subjecting a silane compound having both a silanol group and / or a hydrolyzable silyl group and a polymerizable double bond to a hydrolysis and condensation reaction. The polymer segment and the polysiloxane are then mixed together to carry out a hydrolysis and condensation reaction.
[0096] (6) A method in which the polymer segment, a silane compound having a silanol group and / or a hydrolyzable silyl group, and a polymerizable double bond, and a polysiloxane are mixed together to carry out a hydrolysis and condensation reaction. A polysiloxane compound can be obtained by the above method. Examples of polysiloxane compounds include the Ceranate (registered trademark) series (organic / inorganic hybrid coating resin; manufactured by DIC Corporation) and the Compocelan SQ series (silsesquioxane hybrid; manufactured by Arakawa Chemical Industries, Ltd.).
[0097] A carbon source resin is used as another raw material for the matrix phase. The carbon source resin has good miscibility with polysiloxane compounds, and is preferably made of synthetic resins or natural chemical raw materials that are carbonized by high-temperature firing in an inert atmosphere and have aromatic functional groups.
[0098] Examples of synthetic resins include thermoplastic resins such as polyvinyl alcohol and polyacrylic acid, and thermosetting resins such as phenol resins and furan resins. Examples of natural chemical raw materials include heavy oils, particularly tar pitches, such as coal tar, light tar oil, medium tar oil, heavy tar oil, naphthalene oil, anthracene oil, coal tar pitch, pitch oil, mesophase pitch, oxygen-crosslinked petroleum pitch, and heavy oil. From the viewpoints of cheap availability and removal of impurities, the use of phenol resins is more preferable.
[0099] In particular, the carbon source resin is preferably a resin containing an aromatic hydrocarbon moiety, and the above-mentioned resin containing an aromatic hydrocarbon moiety is preferably a phenol resin, an epoxy resin, or a thermosetting resin, and the phenol resin is preferably a resol type. Examples of phenolic resins include SUMILITE resin series (resole type phenolic resins, manufactured by Sumitomo Bakelite Co., Ltd.).
[0100] The slurry of silicon particles obtained above is mixed with the polysiloxane compound and the carbon source resin to obtain a suspension in which the silicon particles, polysiloxane compound and carbon source resin are uniformly dispersed. The obtained suspension is subjected to desolvation and drying to obtain a precursor for preparing a surface layer. The mixture containing the polysiloxane compound and the carbon source resin is preferably in a state in which the polysiloxane compound and the carbon source resin are uniformly mixed. The mixing is carried out using a device having a dispersing and mixing function. Examples of such a device include a stirrer, an ultrasonic mixer, and a premix dispersing machine. In the process of desolvation and drying for the purpose of distilling off the organic solvent, a dryer, a reduced pressure dryer, a spray dryer, and the like can be used.
[0101] The precursor for producing the surface layer preferably contains 3% to 50% by mass of the present silicon particles, 15% to 85% by mass of a solid content of the polysiloxane compound, and 3% to 70% by mass of a solid content of the carbon source resin, and more preferably contains 8% to 40% by mass of the present silicon particles, 20 to 70% by mass of a solid content of the polysiloxane compound, and 3% to 60% by mass of a solid content of the carbon source resin.
[0102] <Process (2)> In step (2), the surface of the granular structure is coated with the precursor for producing the surface layer obtained in step (1). For example, the coating method may include adding the present granular structure to a slurry containing the precursor for forming the surface layer, mixing the mixture, and then removing the solvent and drying. The mixing, removing the solvent, and drying are the same as in the above step (1).
[0103] A granular structure mainly made of graphite and having an uneven surface can be produced, for example, by uniformly mixing graphite with a pore-forming agent or a small amount of a resin binder, and forming the mixture into pellets, granules, flakes, etc., using, for example, a press. The pore-forming agent or resin binder is then removed to produce a granular structure having an uneven surface. The pore-forming agent is used to form pores in the molded body by being removed from the molded body after the molding by firing, etching, washing, etc. The material of the pore-forming agent is appropriately selected depending on the method for removing the pore-forming agent, and examples of the material include metals such as copper that are poor in acid resistance or alkali resistance, inorganic substances that have a firing temperature lower than that of graphite, and organic substances that are easily thermally decomposed.
[0104] <Process (3)> In step (3), the granular structure coated with the surface layer preparation precursor obtained in step (2) is fired at a high temperature of 1000°C to 1300°C in an inert atmosphere to obtain the negative electrode active material. Thermally decomposable organic components are completely decomposed by firing, and the other main components are converted into a fired product suitable for the negative electrode active material by precise control of firing conditions. Specifically, the raw material polysiloxane compound and carbon source resin are converted into a silicon-oxygen-carbon skeleton and free carbon by the energy of high-temperature treatment.
[0105] In step (3), the granular structure coated with the precursor for producing the surface layer obtained in step (2) is fired in an inert atmosphere within the above-mentioned temperature range, thereby enabling precise control of the microstructure of the negative electrode active material and preventing oxidation of the silicon particles during high-temperature firing, thereby obtaining better charge-discharge characteristics.
[0106] The calcination method is not particularly limited, but it is sufficient to use a reaction device having a heating function in an inert atmosphere, and treatment can be performed by a continuous method or a batch method. The calcination device can be appropriately selected from a fluidized bed reaction furnace, a rotary furnace, a vertical moving bed reaction furnace, a tunnel furnace, a batch furnace, a rotary kiln, etc. depending on the purpose.
[0107] The negative electrode active material obtained in the step (3) may be pulverized and classified as necessary. The pulverization may be performed using a bead mill, a jet mill, or the like. The classification may be performed using an air classifier, a wet classifier, or the like. Note that, if the precursor mixture is controlled to a shape close to the target particle size by spray drying or the like before the firing in the step (3), and the firing is performed in that shape, it is possible to omit the pulverization step.
[0108] When the present negative electrode active material has the carbon coating, the present negative electrode active material obtained in steps (1) to (3) can be subjected to chemical vapor deposition, for example, in a chemical vapor deposition apparatus under conditions of a flow of a pyrolytic carbon source gas and a carrier nitrogen gas and a high-temperature treatment in a temperature range of 700°C to 1000°C, to obtain the present negative electrode active material having the carbon coating formed thereon.
[0109] As described above, when the present negative electrode active material is used as the negative electrode active material for a secondary battery, it gives a secondary battery excellent in initial coulombic efficiency and capacity retention rate. The present active material can be used as a negative electrode by the above-mentioned method to produce a secondary battery having the negative electrode.
[0110] Although the present negative electrode active material, the secondary battery including the present negative electrode active material in the negative electrode, and the method for producing the present negative electrode active material have been described above, the present invention is not limited to the configurations of the above-mentioned embodiments. In the present active material and the secondary battery containing the present active material in the negative electrode, any other configuration may be added to the configuration of the above embodiment, or any other configuration that exerts the same function may be substituted. Furthermore, the method for producing the negative electrode active material according to the present embodiment may further include any other step in addition to the configuration of the above embodiment, or may be substituted with any other step that produces a similar effect. EXAMPLES
[0111] The present invention will be described in detail below with reference to examples, but the present invention is not limited to these. The half-cell used in the examples of the present invention has a negative electrode mainly made of the silicon-containing active material of the present invention, and a simple evaluation is performed using metallic lithium as the counter electrode, in order to more clearly compare the cycle characteristics of the active material itself.
[0112] Synthesis Example 1: Preparation of silicon particles Zirconia beads with a particle size of 0.1 mm to 0.2 mm and 100 ml of methyl ethyl ketone solvent (MEK) were placed in a 150 ml container of a small bead mill device at a filling rate of 60%. Silicon powder with an average particle size of 5 μm (commercially available product) and a cationic dispersant liquid (BYK Japan Co., Ltd.: BYK145) were then placed in the container and wet-pulverized using a bead mill under the conditions shown in Table 1, to obtain dark brown liquid silicon slurries Si1 to Si6 with a solid concentration of 30 mass%. The morphology and size of the silicon pulverized products were confirmed by TEM observation, and they were designated as Si1, Si2, Si3, Si4, Si5, and Si6, respectively, as shown in Table 1.
[0113] [Table 1]
[0114] Synthesis Example 2: Treatment to impart irregularities to the graphite particle surface For graphites 1 to 7, 200 g of spherical graphite powder having an average particle size in the range of 2.5 μm to 15 μm shown in Table 2 was added with 200 g of copper particles having an average particle size shown in Table 2, mixed in a tabletop mixer for 30 minutes, and then molded into a cylindrical shape at a pressure of 40 to 80 MPa in a molding machine as shown in Table 2. The molded product was pulverized in a mortar, and the pulverized product was immersed in a 10 mass % sulfuric acid solution at room temperature for 24 hours to dissolve and remove the copper. The mixture was filtered and then dried under reduced pressure at 110 °C for 12 hours to impart voids to the graphite powder surface. The depth of the irregularities on the graphite surface was measured by cross-sectional observation using a SEM, and the average particle size, specific surface area, and pore volume of the graphite particles were determined using a light scattering particle size measuring device and a specific surface area measuring device. The results are shown in Table 2.
[0115] Graphite 8 was prepared by grinding 15 μm spherical graphite powder with 5 mm particle diameter zirconia balls in a ball mill for 10 hours to make the average particle diameter of the graphite 1.5 μm, and then adding voids using copper particles with an average particle diameter of 1 μm, after which the copper was dissolved and removed. Graphite 9 was prepared by molding 15 μm spherical graphite powder and copper particles with an average particle diameter of 1 μm into a cylindrical shape at a pressure of 35 MPa in a molding machine, and then dissolving and removing the copper under the above conditions to add voids. Graphite 10 was prepared by molding spherical graphite powder having an average particle size of 2.5 μm and copper particles having an average particle size of 1 μm into a cylindrical shape at a pressure of 70 MPa using a molding machine, and then dissolving and removing the copper under the above-mentioned conditions to provide voids. The conditions for providing voids to graphites 1 to 10 are shown in Table 2.
[0116] [Table 2]
[0117] Synthesis Example 3: Preparation of polysiloxane compound (Synthesis of methyltrimethoxysilane condensation product) A reaction vessel equipped with a stirrer, a thermometer, a dropping funnel, a cooling tube, and a nitrogen gas inlet was charged with 1,421 parts by mass of methyltrimethoxysilane (hereinafter abbreviated as "MTMS") and heated to 60° C. Next, a mixture of 0.17 parts by mass of isopropyl acid phosphate ("Phoslex A-3" manufactured by SC Organic Chemical Co., Ltd.) and 207 parts by mass of deionized water was dropped into the reaction vessel over a period of 5 minutes, and the mixture was stirred at a temperature of 80° C. for 4 hours to carry out a hydrolysis condensation reaction. The condensate obtained by the above hydrolysis and condensation reaction was distilled at a temperature of 40 to 60°C and a reduced pressure of 40 to 1.3 kPa to remove the methanol and water generated during the reaction, thereby obtaining 1,000 parts by mass of a liquid containing 70% by mass of an active ingredient containing a condensate of MTMS having a number average molecular weight of 1,000 to 5,000. Note that "under a reduced pressure of 40 to 1.3 kPa" refers to a condition in which the reduced pressure condition is 40 kPa when the distillation of methanol begins, and is finally reduced to 1.3 kPa. The active ingredient is calculated by dividing the theoretical yield (parts by mass) when all the methoxy groups of silane monomers such as MTMS are condensed by the condensation reaction by the actual yield (parts by mass) after the condensation reaction [theoretical yield (parts by mass) when all the methoxy groups of silane monomers are condensed by the condensation reaction / actual yield (parts by mass) after the condensation reaction].
[0118] (Production of Curable Resin Composition (1)) A reaction vessel equipped with a stirrer, a thermometer, a dropping funnel, a cooling tube, and a nitrogen gas inlet was charged with 150 parts by mass of butanol (hereinafter also referred to as "BuOH"), 105 parts by mass of phenyltrimethoxysilane (hereinafter also referred to as "PTMS"), and 277 parts by mass of dimethyldimethoxysilane (hereinafter also referred to as "DMDMS"), and the temperature was raised to 80°C. Next, at the same temperature, a mixture containing 21 parts by mass of methyl methacrylate (hereinafter also referred to as "MMA"), 4 parts by mass of butyl methacrylate (hereinafter also referred to as "BMA"), 3 parts by mass of butyric acid (hereinafter also referred to as "BA"), 2 parts by mass of methacryloyloxypropyltrimethoxysilane (hereinafter also referred to as "MPTS"), 3 parts by mass of BuOH and 0.6 parts by mass of butylperoxy-2-ethylhexanoate (hereinafter also referred to as "TBPEH") was dropped into the reaction vessel over 6 hours. After the dropwise addition was completed, the mixture was further reacted at the same temperature for 20 hours to obtain an organic solvent solution of a vinyl polymer (a2-1) having a number average molecular weight of 10,000 and having a hydrolyzable silyl group.
[0119] Next, a mixture of 0.04 parts by mass of isopropyl acid phosphate ("Phoslex A-3" manufactured by SC Organic Chemical Co., Ltd.) and 112 parts by mass of deionized water was added dropwise over a period of 5 minutes, and the mixture was stirred at the same temperature for a further 10 hours to cause a hydrolysis condensation reaction, thereby obtaining a liquid containing a composite resin in which a hydrolyzable silyl group having a vinyl polymer (a2-1) is bonded to a hydrolyzable silyl group and a silanol group having a polysiloxane derived from the PTMS and DMDMS. Next, 472 parts by mass of the MTMS condensate (a1) obtained in Synthesis Example 1 and 80 parts by mass of deionized water were added to this liquid, and the mixture was stirred at the same temperature for 10 hours to cause a hydrolysis condensation reaction, and the resulting methanol and water were removed by distillation under the same conditions as in Synthesis Example 1. Next, 250 parts by mass of BuOH was added to obtain 1,000 parts by mass of a curable resin composition (1) with a non-volatile content of 60.1% by mass.
[0120] (Production of Curable Resin Composition (2)) A reaction vessel equipped with a stirrer, a thermometer, a dropping funnel, a cooling tube and a nitrogen gas inlet was charged with 150 parts by mass of BuOH, 249 parts by mass of PTMS and 263 parts by mass of DMDMS, and the temperature was raised to 80° C. Then, at the same temperature, a mixture containing 18 parts by mass of MMA, 14 parts by mass of BMA, 7 parts by mass of BA, 1 part by mass of acrylic acid (hereinafter also referred to as “AA”), 2 parts by mass of MPTS, 6 parts by mass of BuOH and 0.9 parts by mass of TBPEH was dropped into the reaction vessel over 5 hours, and after the dropwise addition was completed, the mixture was further reacted at the same temperature for 10 hours to obtain an organic solvent solution of a vinyl polymer (a2-2) having a number average molecular weight of 20,100 and having a hydrolyzable silyl group.
[0121] Next, a mixture of 0.05 parts by mass of isopropyl acid phosphate ("Phoslex A-3" manufactured by SC Organic Chemical Co., Ltd.) and 147 parts by mass of deionized water was added dropwise over a period of 5 minutes, and the mixture was stirred at the same temperature for a further 10 hours to cause a hydrolysis condensation reaction, thereby obtaining a liquid containing a composite resin in which the hydrolyzable silyl group of the vinyl polymer (a2-2) was bonded to the hydrolyzable silyl group and silanol group of the polysiloxane derived from the PTMS and DMDMS. Next, 76 parts by mass of 3-glycidoxypropyltrimethoxysilane, 231 parts by mass of the MTMS condensate, and 56 parts by mass of deionized water were added to this liquid, and the mixture was stirred at the same temperature for 15 hours to cause a hydrolysis and condensation reaction. The mixture was distilled under the same conditions as above to remove the produced methanol and water, and then 250 parts by mass of BuOH was added to obtain 1,000 parts by mass of a curable resin composition (2) having a non-volatile content of 60.0% by mass.
[0122] Example 1 The polysiloxane resin (curable resin (1)) with an average molecular weight of 3500 and the phenolic resin with an average molecular weight of 3000 prepared as in the above Synthesis Example 3 were added in a resin solid weight composition ratio of 45 / 55 so that the composition weight ratio after firing would be 50 / 50 SiOC / C, and the silicon slurry of Si3 obtained in Synthesis Example 1 and an appropriate amount of methyl ethyl ketone solvent were added so that the silicon particle content in the product after high-temperature firing would be 50% by weight, and thoroughly mixed in a stirrer. As a result, a silicon particle-containing resin mixed suspension with a solid concentration of 10% by mass was obtained. Graphite 2 treated in the above Synthesis Example 2 was added to 100 parts by mass of the silicon particle-containing resin mixed suspension so that the solid concentration would be 94% by mass after high-temperature firing, and after thorough mixing, the solvent was removed in a 120°C oil bath under nitrogen follow conditions. Thereafter, reduced pressure drying was performed at 110°C using a vacuum dryer for 10 hours, and finally high-temperature firing was performed at 1100°C for 4 hours in a nitrogen atmosphere to obtain black solid composite particles. The active material was prepared by grinding the powder in a planetary ball mill. The average particle size was about 16 μm in D50, and the specific surface area by the BET method was 3.1 m 2 The crystallite size was 21 nm, as calculated by the Scherrer equation based on the half-width of the diffraction peak at 2θ of 28.4°, which is assigned to the Si(111) crystal plane, from the results of powder X-ray diffraction (XRD) using Cu-Kα radiation.
[0123] A slurry was prepared by mixing 80 parts of the obtained active material powder with 10 parts of acetylene black as a conductive assistant and 10 parts of a mixture of CMC and SBR as a binder, and a film was formed on a copper foil. After drying under reduced pressure at 110°C, a half cell of a coin-type lithium secondary battery was prepared with a Li metal foil as the counter electrode, and the charge / discharge characteristics were evaluated using a secondary battery charge / discharge tester (manufactured by Hokuto Co., Ltd.). The cutoff voltage range was 0.005 to 1.5 V. The charge / discharge measurement results were an initial discharge capacity of 403 mAh / g and an initial coulombic efficiency of 90%. For the evaluation of the full cell, a positive electrode film was prepared using a single-layer sheet using LiCoO2 as the positive electrode active material and aluminum foil as the current collector, and a negative electrode film was prepared by mixing graphite powder and active material powder with a discharge capacity design value of 400mAh / g. A non-aqueous electrolyte solution was used in which lithium hexafluorophosphate was dissolved at a concentration of 1mol / L in a mixture of ethylene carbonate and diethyl carbonate in a volume ratio of 1 / 1, and a laminated lithium ion secondary battery was prepared using a 30μm thick polyethylene microporous film as a separator. The laminated lithium ion secondary battery was charged at a constant current of 1.2mA (0.25c based on the positive electrode) at room temperature until the voltage of the test cell reached 4.2V, and after reaching 4.2V, the current was reduced to keep the cell voltage at 4.2V and the discharge capacity was calculated. The capacity retention rate after 300 cycles at 25℃ was 91%. The results are shown in Table 3.
[0124] Examples 2 to 9 As in Example 1, the amount of graphite 2 treated in Synthesis Example 2 added to 100 parts by mass of the silicon particle-containing resin mixed suspension of Si3 obtained in Synthesis Example 1, which has a solid concentration of 10 mass%, was adjusted to 90 mass% to 50 mass% after firing, as shown in Table 3, and after thorough mixing, the solvent was removed in a 120°C oil bath under nitrogen gas flow conditions. The other conditions were the same as in Example 1 to obtain an active material. A secondary battery was evaluated using a negative electrode active material containing the obtained active material. The results are shown in Table 3.
[0125] Examples 10 to 17 Graphite 1 (Example 10), graphite 3 (Example 11), graphite 4 (Example 12), graphite 5 (Example 13), graphite 6 (Example 14), graphite 7 (Example 15), graphite 8 (Example 16) and graphite 3 (Example 17) treated in Synthesis Example 2 were added to the silicon particle-containing resin mixed suspension of Si3 obtained in Synthesis Example 1 with a solid concentration of 10 mass% using a curable resin (2) with an average molecular weight of 3200, so that each was 85 mass% after firing. After thorough mixing, the solvent was removed in an oil bath at 120 ° C. under nitrogen gas flow conditions. The other conditions were the same as in Example 1 to obtain an active material. A secondary battery using a negative electrode active material containing the obtained active material was evaluated. The results are shown in Table 4.
[0126] Examples 18 to 20 Graphite 2 treated in Synthesis Example 2 was added to 100 parts by mass of a silicon particle-containing resin mixed suspension of Si1 (Example 18), Si2 (Example 19) and Si4 (Example 20) obtained in Synthesis Example 1 with a solid concentration of 10% by mass, so that the graphite 2 was 85% by mass for high-temperature firing, and thoroughly mixed. Then, desolvation was performed in a 120°C oil bath under nitrogen gas flow conditions. The other conditions were the same as in Example 1 to obtain active materials. Then, 25 g of each of the powders of the active materials was placed in a reaction vessel of a chemical vapor deposition apparatus (CVD, disk rotary kiln, Takasago Kogyo Co., Ltd.), and the reaction time was changed to 1 hour, 2 hours and 3 hours at 900°C in a mixed gas flow with an acetylene flow rate of 0.3 L / min and a nitrogen flow rate of 0.7 L / min to perform carbon coating. According to the thermal analysis results, the carbon coating amount was 2%, 4% and 8%, respectively. The properties of the obtained carbon-coated active materials and the evaluation results of the secondary batteries are shown in Table 4.
[0127] Example 21 Using commercially available monodispersed spherical silicon particles (manufactured by Alfa Aesar) with an average particle size of 50 nm in D50, a resin mixed suspension containing 10 parts by mass of solid matter was prepared under the same conditions as in Example 1. Graphite 2 treated in Synthesis Example 2 was added to 100 parts by mass of the resin mixed suspension so that the graphite concentration after high-temperature firing was 85% by mass, and after thorough mixing, the solvent was removed in a 120°C oil bath under nitrogen gas flow conditions. The other conditions were the same as in Example 1 to obtain an active material. A secondary battery using a negative electrode active material containing the obtained active material was evaluated. The results are shown in Table 4.
[0128] Example 22 Using the silicon particles of Si3 obtained in Synthesis Example 1, a resin mixed suspension containing 10 parts by mass of solid matter was prepared under the same conditions as in Example 1. Graphite 9 treated in Synthesis Example 2 was added to 100 parts by mass of the resin mixed suspension so that the graphite concentration after high-temperature firing was 85% by mass, and after thorough mixing, the solvent was removed in a 120°C oil bath under nitrogen gas flow conditions. The other conditions were the same as in Example 1 to obtain an active material. A secondary battery using a negative electrode active material containing the obtained active material was evaluated. The results are shown in Table 4.
[0129] Example 23 Graphite 10 treated in Synthesis Example 2 was added to 100 parts by mass of the silicon particle-containing resin mixed suspension of Si3 obtained in Synthesis Example 1, which had a solid concentration of 10 mass%, so that the graphite was 85 mass% after high-temperature firing, and after thorough mixing, the solvent was removed under nitrogen gas flow conditions in an oil bath at 120°C. The other conditions were the same as in Example 1 to obtain an active material. A secondary battery was evaluated using a negative electrode active material containing the obtained active material. The results are shown in Table 4.
[0130] Comparative Example 1 Using spherical graphite with an average particle size of D50 of 15 μm, the particle size distribution and specific surface area were measured, and then an active material was obtained in the same manner as in Example 1. A secondary battery using a negative electrode active material containing the obtained active material was evaluated. The results are shown in Table 4.
[0131] Comparative Example 2 Commercially available graphite particles having an average particle size of 15 μm in D50 were added to 100 parts by mass of the Si5 silicon particle-containing resin mixed suspension obtained in Synthesis Example 1, which had a solid concentration of 10% by mass, so that the content after high-temperature firing was 85% by mass, and mixed thoroughly. After that, the solvent was removed in a 120° C. oil bath under nitrogen gas flow conditions. The other conditions were the same as in Example 1 to obtain an active material. A secondary battery was evaluated using a negative electrode active material containing the obtained active material. The results are shown in Table 4.
[0132] Comparative Example 3 Commercially available graphite particles having an average particle size of 15 μm in D50 were added to 100 parts by mass of the Si6 silicon particle-containing resin mixed suspension obtained in Synthesis Example 1, which had a solid concentration of 10% by mass, so that the content after high-temperature firing was 85% by mass, and mixed thoroughly. After that, the solvent was removed in a 120° C. oil bath under nitrogen gas flow conditions. The other conditions were the same as in Example 1 to obtain an active material. A secondary battery was evaluated using a negative electrode active material containing the obtained active material. The results are shown in Table 4.
[0133] [Table 3]
[0134] [Table 4]
[0135] [Evaluation method] In Tables 3 and 4, the evaluation methods are as follows: D50: Measured using a laser diffraction particle size distribution analyzer (Malvern Panalytical, Mastersizer 3000). Specific surface area: Measured by the BET method using a specific surface area measuring device (BELSORP-mini, manufactured by BELJAPAN) based on nitrogen adsorption measurement. 29 Si-NMR: JNM-ECA600 manufactured by JEOL RESONANCE was used.
[0136] Surface penetration depth: The cross section was processed using an FB-2100 (Hitachi High-Technologies Corporation) and measured using an FE-SEM (JSM-7900F, JEOL Ltd.). Accumulative pore volume: Measured with a mercury porotherm (Autopore IV9520, manufactured by Shimadzu Micromeritic).
[0137] Crystallite size: Measurement was performed using an X-ray diffractometer (SmartLab, manufactured by Rigaku Corporation), and calculation was performed using the Scherrer equation. Specific surface area: Measured using a specific surface measuring device (BELSORP VAC3, manufactured by Microtrack-Bel).
[0138] Battery characteristic evaluation: Battery characteristics were measured using a secondary battery charge / discharge tester (manufactured by Hokuto Denko Corporation). The charge / discharge characteristics were evaluated under the following set conditions: room temperature 25°C, cutoff voltage range 0.005 to 1.5V, charge / discharge rate 0.1C (1st to 3rd times) and 0.2C (after 4th cycle), constant current / constant voltage charge / constant current discharge. When switching between each charge / discharge cycle, the battery was left in an open circuit for 30 minutes. The initial discharge capacity, initial charge / discharge efficiency, and capacity retention rate at 300 cycles were calculated as follows: Initial discharge capacity Initial charge / discharge efficiency (%) = initial discharge capacity (mAh / g) / initial charge capacity (mAh / g) Capacity retention rate (%@300th cycle) = discharge capacity at 300th cycle (mAh / g) / initial discharge capacity (mAh / g)
[0139] As is clear from the above results, the secondary battery using this negative electrode active material has high initial discharge capacity of 400 or more, initial efficiency of 80% or more, and capacity retention rate at 300 cycles of 80% or more, and these are all excellent in balance. The reason for this is thought to be that compared with commercially available graphite, the graphite with irregularities on the surface has improved adhesion strength with the surface layer, and as a result, the characteristics of the secondary battery, such as the initial discharge capacity, are improved.
Claims
1. A negative electrode active material comprising a granular structure mainly made of graphite having an uneven surface, and a surface layer on at least a portion of the surface of the granular structure, in which silicon particles having an average particle size of 20 nm to 200 nm are dispersed in a matrix phase, the surface layer containing silicon oxycarbide, amorphous carbon and the silicon particles, the silicon particles accounting for 1 to 80 mass%, with the total mass of the surface layer being 100 mass%.
2. 2 . The negative electrode active material according to claim 1 , wherein the silicon particles are flaky and crystalline, and have a crystallite size of 40 nm or less at 2θ of 28.4° in X-ray diffraction.
3. The granular structure has a cumulative pore volume of 0.001 cm3 having pores with diameters in the range of 3 nm to 300 nm. 3 3. The negative electrode active material according to claim 1, wherein the molecular weight of the negative electrode active material is 1 / g or more.
4. The graphite is natural graphite or artificial graphite, and has an average particle size of 1 μm to 25 μm and a specific surface area of 0.5 m 2 / g to 20m 2 3. The negative electrode active material according to claim 1, wherein the molecular weight of the negative electrode active material is 1 / g.
5. 3 . The negative electrode active material according to claim 1 , wherein the mass of the surface layer is from 1 mass % to 80 mass % relative to the total mass of the negative electrode active material being 100%.
6. The negative electrode active material according to claim 1 , wherein the surface layer further contains nitrogen.
7. 3. The negative electrode active material according to claim 1, wherein the silicon particles have a particle size ranging from 5 nm to 300 nm.
8. The granular structure has an average particle size of 1 μm to 30 μm and a specific surface area of 1 m 2 / g to 30m 2 The negative electrode active material according to claim 1 or 2, wherein the molecular weight of the negative electrode active material is 1 / g.
9. 3. The negative electrode active material according to claim 1, further comprising a carbon coating on the surface of the granular structures.
10. 10. The negative electrode active material according to claim 9, wherein the carbon coating is present in an amount of 1 to 10 mass % relative to 100 mass % of the total mass of the negative electrode active material.
11. The method for producing the negative electrode active material according to claim 1 or 2, comprising the following steps (1) to (3): Step (1) Obtaining a precursor for preparing a surface layer Step (2) A step of applying the precursor for producing a surface layer to the surface of a granular structure mainly made of graphite and having an uneven surface. Step (3) A step of obtaining a negative electrode active material by high-temperature firing at a firing temperature of 1000° C. to 1300° C. in an inert atmosphere.
12. A method for producing a negative electrode active material, comprising coating a powder of the negative electrode active material obtained according to claim 11 with a carbon film in a chemical vapor deposition apparatus at a temperature in the range of 700°C to 1000°C in a flow of a pyrolyzable carbon source gas and a carrier inert gas.
13. A secondary battery comprising the negative electrode active material according to claim 1 or 2.
Citation Information
Patent Citations
Negative electrode active material for lithium secondary battery, negative electrode using the same, and manufacturing method
JP2008186732A
Negative electrode active material for lithium secondary battery, and lithium secondary battery containing same
JP2009266795A
Lithium ion secondary battery soft carbon anode material, method of manufacturing the same, and lithium ion secondary battery
JP2015128045A
Multicomponent composite anode material, method for manufacturing the same, and lithium-ion battery containing the same
JP2017526118A
Anode material for lithium-ion battery
JP2020064876A