Towel fabric and its manufacturing method
The towel fabric uses specific fiber lengths and twist directions in silo spun yarns to enhance yarn uniformity and texture, ensuring a soft, puffy, and durable fabric with improved water absorption.
Patent Information
- Application Number
- JP2024095433
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2024-06-12
- Publication Date
- 2024-09-18
- Estimated Expiration
- 2044-06-12
AI Technical Summary
Conventional towel fabrics face issues with pile raising property and soft, puffy texture, requiring further improvements.
A towel fabric composed of pile yarn, warp yarn, and weft yarn, where the pile yarn is made from medium or long fiber cotton with specific fiber length and micronaire values, and is non-twisted or lightly twisted silo spun yarn, with secondary twists in the opposite direction, and all yarns are bleached, to enhance yarn uniformity and texture.
The fabric achieves reduced yarn unevenness, maintains raised pile properties, and provides a soft, puffy texture with improved water absorption and durability, maintaining quality after washing.
Smart Images

Figure 0007553171000001
Abstract
Description
[Technical field]
[0001] The present invention relates to a towel fabric using siro spun pile yarn and a method for producing the same. [Background technology]
[0002] Traditionally, towel fabrics have been made by weaving pile yarns, warp yarns, and weft yarns into a pile fabric. To improve water absorption, towel fabrics have a relatively high basis weight (mass per unit area) and are made of thick, fine yarns. Patent Document 1 proposes using synthetic sirospun yarn to make heathered pile yarn. Patent Documents 2 and 3 propose using loosely twisted sirospun yarn to make pile knitted fabric. In Patent Document 4, the present inventor proposes a towel fabric using untwisted or loosely twisted sirospun yarn as the pile yarn. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] Japanese Patent Application Publication No. 10-088440 [Patent Document 2] JP 2019-137941 A [Patent Document 3] JP 2019-137942 A [Patent Document 4] Patent No. 7372718 Summary of the Invention [Problem to be solved by the invention]
[0004] However, the above-mentioned conventional techniques have problems with respect to pile standing and soft, fluffy feel, and further improvements are required.
[0005] To provide a towel fabric and a method for producing the same, which has little yarn unevenness and retains the pile raising property, soft and fluffy texture, water absorbency, etc. of the towel fabric in the woven state, as a result of intensive research aimed at producing an unprecedented high-class towel fabric. [Means for solving the problem]
[0006] One embodiment of the present invention relates to a towel fabric composed of pile yarns, warp yarns, and weft yarns, in which the fiber material of the pile yarns is medium-fiber cotton or long-fiber cotton with an average fiber length of 28.6 to 34.7 mm and a micronaire of 4.1 to 5.8 μg / inch, and the content of short fibers with an average fiber length of 17 mm or less is 10 mass% or less, the pile yarns are untwisted or loosely twisted single yarns of sirospun yarn, and the pile yarns, warp yarns, and weft yarns are bleached.
[0007] Another embodiment of the present invention relates to a method for producing a towel fabric, in which the fiber material of the pile yarn is medium-fiber cotton or long-fiber cotton with an average fiber length of 28.6 to 34.7 mm and a micronaire of 4.1 to 5.8 μg / inch, and the content of short fibers having an average fiber length of 17 mm or less is reduced to 10 mass% or less by combing treatment, the pile yarn is a sirospun yarn, the twist direction of the sirospun yarn is opposite to the primary twist direction of the three roving yarns, and a secondary twist having the same or more number of twists as the primary twist is added to form an untwisted or loosely twisted single yarn, the pile yarn, warp yarn, and weft yarn are subjected to a yarn bleaching treatment, and the pile yarn, warp yarn, and weft yarn are supplied to a jacquard loom to produce a towel woven fabric. Effect of the Invention
[0008] In the towel of the present invention, the fiber material of the pile yarn is medium-fiber cotton or long-fiber cotton with an average fiber length of 28.6 to 34.7 mm and a micronaire of 4.1 to 5.8 μg / inch, and the content of short fibers with an average fiber length of 17 mm or less is 10 mass % or less, the pile yarn is a single yarn of untwisted or loosely twisted sirospun yarn, and the pile yarn, warp yarn, and weft yarn are bleached, so that there is little yarn unevenness, and a towel fabric and its manufacturing method can be provided that retains the pile standing property, soft and fluffy texture, water absorbency, etc. of the towel fabric in the woven state. That is, by cutting the short fibers of the medium-fiber cotton or long-fiber cotton at a specific ratio, it is possible to reduce yarn unevenness, and the towel fabric after weaving is made into a towel fabric product in a state after washing and drying without post-bleaching or post-dyeing. As a result, the quality of the towel fabric in the woven state becomes the quality of the product itself, resulting in a high-quality towel fabric. [Brief description of the drawings]
[0009] [Figure 1] FIG. 1 is a schematic perspective view of a triple sirospun spinning device according to one embodiment of the present invention. [Diagram 2] FIG. 2A is a schematic explanatory diagram of a towel fabric in one embodiment of the present invention, and FIG. 2B is a woven fabric diagram of the same. [Diagram 3] FIG. 3A is a schematic explanatory diagram of a towel fabric in another embodiment of the present invention, and FIG. 3B is a woven fabric diagram of the same. [Figure 4] FIG. 4 is a staple diagram of a card sliver (fiber bundle) used in one embodiment of the present invention. [Diagram 5] FIG. 5 is a staple diagram of a sliver (fiber bundle) that has been combed once and is used in one embodiment of the present invention. [Figure 6] FIG. 6 is a staple diagram of a sliver (fiber bundle) that has been combed twice for use in one embodiment of the present invention. [Figure 7] FIG. 7 is a side photograph (magnification: 30 times) of the pile portion of the towel fabric in Example 1 of the present invention. [Figure 8] FIG. 8 is a side photograph (magnification: 30 times) of the pile portion of the towel fabric of Comparative Example 1. [Figure 9] FIG. 9 is a side photograph (magnification: 30 times) of the pile portion of the towel fabric of Comparative Example 2. [Figure 10] FIG. 10 is a plan view photograph (magnification: 10 times) of the towel fabric of Example 1 of the present invention. [Figure 11] FIG. 11 is a plan view photograph (magnification: 10 times) of the towel fabric of Comparative Example 1. [Figure 12] FIG. 12 is a plan view photograph (magnification: 10 times) of the towel fabric of Comparative Example 2. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0010] The present invention is a towel fabric composed of pile yarn, warp yarn, and weft yarn. Pile yarn, which accounts for about 70% of the constituent yarns of the towel fabric, is an important yarn that determines the functionality such as pile standing, the texture of the towel fabric, and shedding. The fiber material of the pile yarn is medium-fiber cotton or long-fiber cotton with an average fiber length of 28.6 to 34.7 mm and a micronaire of 4.1 to 5.8 μg / inch, and the content of short fibers with an average fiber length of 17 mm or less is 10 mass% or less. This reduces the unevenness of the spun yarn, resulting in a high-quality yarn. The pile yarn fiber material, medium staple cotton or long staple cotton, has an average fiber length of 28.6-34.7 mm and a fineness of 4.1-5.8 μg / inch micronaire, and has a large amount of crimp and high crimp strength. Therefore, when applied to the spun spun yarn of the present invention, the twist tendency of the first twist and migration of the first twist (the phenomenon in which single fibers are twisted inward or outward) tend to remain, the fibers tend to entangle with each other, and since it is a non-twisted yarn or a loosely twisted yarn, each constituent fiber exists in a free state. The above-mentioned "long staple cotton" refers to the "long staple cotton" shown in Table 1 below, and is internationally recognized.
[0011] The pile yarn of the present invention is a single yarn of untwisted or loosely twisted sirospun yarn. That is, a secondary twist is added to the direction opposite to the primary twist of a plurality of roving yarns, the secondary twist being equal to or greater than the number of twists in the primary twist. This provides the following effects. (1) Less shedding. (2) Bulky. (3) It has a large amount of fluffiness and is very soft before washing. (4) The fluffiness is less likely to be lost after washing, and deterioration due to washing is less likely to occur. (5) There is little re-wetting, making wiping comfortable. (6) Less likely to change dimensions when washed (less likely to shrink). (7) It dries quickly.
[0012] The constituent yarns of the towel fabric of the present invention (pile yarns, warp yarns, and weft yarns) are bleached. This allows the quality of the towel fabric in the woven state to directly reflect the quality of the finished product, resulting in a high-quality towel fabric.
[0013] In the present invention, sirospun yarn is used as pile yarn. Sirospun yarn is a yarn in a state similar to a two-ply yarn or a three-ply yarn, which is made by drafting two or three roving yarns separately at a certain interval and then twisting them together. Compared to two-ply yarn or three-ply yarn made by twisting multiple yarns together, the fibers of the sirospun yarn are regularly arranged on the yarn surface, and there is less fuzz. Therefore, it can be used as a pile yarn as a single yarn. In addition, due to the yarn structure unique to sirospun yarn, even if it is a non-twisted yarn or a loosely twisted yarn, the fibers are entangled with each other, so there is no problem with winding, and yarn breakage during weaving is unlikely to occur, and it is easy to pass through the weaving process.
[0014] The number of the sirospun yarn is preferably 5 to 100 in English cotton count. For thin fabrics, a thin number of 100 to 40 is preferably applied, for medium-weight fabrics, a thick number of 30 to 16 is preferably applied, and for heavy fabrics, a thick number of 12 to 5 is preferably applied.
[0015] The spun spun yarn of the present invention preferably has a twist factor K of 0 to 3.5, more preferably 0 to 3.3, and even more preferably 0 to 3.0. The twist factor K is calculated by the following formula (Math 1).
number
[0016] The sirospun yarn is preferably untwisted or loosely twisted by adding a secondary twist equal to or greater than the number of twists in the primary twist in the opposite direction to the primary twist direction of multiple rovings. For example, if the primary twist directions of two or three rovings are both Z-direction, the secondary twist is S-direction, and the number of secondary twists is equal to or greater than the number of twists in the primary twist. This allows each component fiber to exist in a more free state, resulting in a pile yarn with good nap standing and a soft, fluffy texture. Here, untwisted refers to a case where the twist coefficient K is zero, and loosely twisted refers to a case where the twist coefficient K is greater than zero and is 3.3 or less.
[0017] The sirospun yarn is preferably a two-strand sirospun yarn or a three-strand (triple) sirospun yarn, more preferably a three-strand (triple) sirospun yarn having a round cross section. The sirospun yarn is preferably 100% cotton. If it is 100% cotton, it has a soft and fluffy texture and is also absorbent.
[0018] The warp yarns and weft yarns are preferably ring-spun yarns using extra-long staple cotton with an average fiber length of 34.8 to 44.5 mm and a fineness of 3.0 to 4.1 μg / inch micronaire. The warp yarns and weft yarns are preferably fine with an English cotton count of 10 to 50. The pile yarns form loop pile while being held by the ground fabric made of the warp yarns and weft yarns, so if the warp yarns and weft yarns are made of extra-long staple cotton and have a fine count, the holding force of the pile yarns can be increased and pile loss can be prevented. Furthermore, the texture is good. The above-mentioned "extra-long staple cotton" is as shown in Table 1 below and is internationally recognized.
[0019] [Table 1]
[0020] The twist coefficient K of the warp yarns and weft yarns is preferably 3.5 to 4.5, more preferably 3.7 to 4.2, and even more preferably 3.8 to 4.0. The twist coefficient (K) is calculated using the above formula (Math 1). This allows for high yarn strength and long durability of the towel.
[0021] The pile yarn is preferably combed yarn. This allows the content of short fibers with an average fiber length of 17 mm or less to be 10% by mass or less, preferably 8% by mass or less, more preferably 6% by mass or less, and even more preferably 4% by mass or less. The pile yarn of the present invention can be used for both warp pile yarn and weft pile yarn, but is preferably used for warp pile yarn.
[0022] The method for producing the towel fabric of the present invention includes the following steps. (1) Combing process of pile cotton long staple As the fiber material for the pile yarn, medium-fiber cotton or long-fiber cotton with an average fiber length of 28.6 to 34.7 mm and micronaire of 4.1 to 5.8 μg / inch is used, and the content of short fibers with an average fiber length of 17 mm or less is adjusted to 10% by mass or less by combing. The combing process (combing step) is preferably performed twice, and the number of combing needles is increased, the lap width is adjusted as thin as possible, and the process is performed slowly at about 1 / 3 the normal speed. This allows the content of short fibers with an average fiber length of 17 mm or less to be 10% by mass or less, preferably 8% by mass or less, more preferably 6% by mass or less, and even more preferably 4% by mass or less. (2) Pile yarn spinning process Using a sirospun spinning machine, two or three rovings are twisted in the opposite direction to the primary twist direction and with a secondary twist equal to or greater than the number of twists in the primary twist to produce a non-twisted or loosely twisted single yarn. The twist factor K of the sirospun yarn is preferably 0 to 3.5. (3) Spinning process of warp and weft yarns The warp and weft yarns are made of extra-long staple cotton with an average fiber length of 34.8 to 44.5 mm and a micronaire fineness of 3.0 to 4.1 μg / inch, which are spun into yarns using a ring spinning frame. The warp and weft yarns are preferably made of fine cotton with an English cotton count of 10 to 50. (4) Pile yarn, warp yarn, and weft yarn bleaching process The pile yarn, warp yarn and weft yarn are subjected to a yarn bleaching process. Yarn bleaching refers to scouring and bleaching the spun yarn. In the case of white goods, the yarn may be bleached alone, or may be dyed with a white dye and / or a fluorescent dye. In the case of colored goods, a dyeing process may be added after the yarn bleaching. Dyeing is preferably performed with reactive dyes at a temperature of 60 to 80°C for about 20 to 60 minutes. (5) Weaving process Pile yarns, warp yarns, and weft yarns are fed into a jacquard loom to weave a towel fabric, for example, in a 3-pick terry motion weave or 4-pick terry motion weave. A 4-pick terry motion weave is preferable. Compared to a 3-pick terry motion weave, a 4-pick terry motion weave has the advantage that the pile yarns are fixed to the ground weave, the pilling rate is lower, and the pile has good standing properties, so it is bulky, voluminous, and has good ventilation and dries quickly. After weaving, the fabric is washed and dried in rolls, and then hemmed to make a towel product. Scouring and bleaching after weaving is not preferable because the loops are crushed or disordered due to the kneading process in water.
[0023] The method for producing towel fabric of the present invention has the following actions and effects. (1) Although a second twist is applied, the twist tendency of the first twist remains, migration from the first twist also remains, there is entanglement between the fibers, and since it is a non-twisted yarn or a loosely twisted yarn, each component fiber exists in a free state, the pile has good nap standing, and becomes a pile yarn with a soft and fluffy texture. Because of its soft and fluffy texture, it can be gently touched against the skin and can efficiently wipe away sweat and moisture (texture effect, wiping effect). (2) Since pile yarn is either untwisted or loosely twisted, the constituent fibers are more likely to absorb moisture, and at the same time, this swelling promotes air movement, improving breathability (water absorption effect, ventilation effect). (3) The intertwining of the constituent fibers reduces pilling (impact of reduced pilling), reduces changes in texture after washing, and maintains the original soft, fluffy texture (effect of durability of texture after washing). (4) When producing spun yarn, there is no need to use water-soluble fibers (such as water-soluble vinylon), which reduces costs. Also, if water-soluble fibers (such as water-soluble vinylon) are used and then removed after the fabric is made, the high quality of the finished fabric will be reduced. (5) Since there is no need to use water-soluble fibers (such as water-soluble vinylon) when producing spun yarn, the environmental load caused by factory wastewater containing these can be reduced.
[0024] The towel of the present invention is suitable for use as a bath towel (towel after bathing), a bath towel, a skin towel for bedding, a face towel, a towel handkerchief (handkerchief), a hand towel, a wash towel, a hand towel, a bath mat, a sports towel, a beach towel (body towel), etc. The fabric blend ratio, yarn type, yarn usage, mass per unit (basis weight), etc. are appropriately set according to the required properties such as shedding resistance and water absorbency. The basis weight can be controlled by changing the pile length (long to short) of the pile yarn to control the basis weight (large to small). Here, examples of preferable basis weights that can exert the effects of the present invention include a basis weight of 100 to 250 g / m for thin fabrics. 2 The medium-weight fabric has a basis weight of 250 to 500 g / m 2 The thickness is 500~1000g / m 2 In addition, 100 g / m 2 Those that are less than 1000g / m are thin and have no bulk. 2 Anything over that is too thick and heavy, and neither is recommended.
[0025] The following description will be given with reference to the drawings. In the following drawings, the same reference numerals denote the same parts. 1 is a schematic perspective view of a triple sirospun spinning device according to an embodiment of the present invention. In this triple sirospun spinning device 10, three roving bobbins 11a, 11b, and 11c are hung from one spindle on a creel (roving supplying tool), and rovings 12a, 12b, and 12c supplied from the three roving bobbins 11a, 11b, and 11c are sent in parallel to a draft device 15 through a three-mouth trumpet guide 13 provided on the upstream side (roving bobbin side) of a back roller 14. The rovings 12a, 12b, and 12c are drafted at a predetermined interval between the back roller 14 and an apron 16, and between the apron 16 and a front roller 17, respectively, to form fleeces 18a, 18b, and 18c. The fleeces 18a, 18b, 18c are spun from the front roller 17, and twisted downstream of the front roller 17 by a twisting mechanism caused by the rotation of the spindle 21 to form one spun yarn 19, which is then taken up onto a bobbin 22 via a snail wire 20 and a traveler 21. For example, the twist directions of the primary twist of the three rovings 12a, 12b, 12c are all in the Z direction, and the twist direction by the spindle 21 is in the S direction, and they are twisted in the untwisting direction. In addition, the number of twists by the spindle 21 (secondary twist number) is set to be the same as or greater than the number of twists in the primary twist to produce a non-twisted or loosely twisted yarn.
[0026] FIG. 2A is a schematic explanatory diagram of a towel fabric 1 according to one embodiment of the present invention. This towel fabric 1 is composed of warp pile yarns 2a, 2b, weft yarn 3, and warp yarns 4a, 4b, and the warp pile yarns 2a, 2b form loop piles while being engaged with a ground structure composed of the weft yarn 3 and the warp yarns 4a, 4b. The obtained towel fabric 1 is cut to a predetermined size, and the ends are processed to form a towel. FIG. 2B is a weave diagram of the towel fabric. This weave structure is a three-weft towel structure (three-pick terry motion structure). The warp pile yarns cross once for every three weft yarns. The warp yarns G and the warp pile yarns P are arranged alternately. The weft yarns 1 to 3 indicate the order. In FIG. 2B, as viewed from the warp yarns, black and x indicate floating yarns, and white indicates sinking yarns.
[0027] FIG. 3A is a schematic explanatory diagram of a towel fabric 1 according to another embodiment of the present invention. This towel fabric 1 is composed of warp pile yarns 2a, 2b, weft yarns 3, and warp yarns 4a, 4b, and the warp pile yarns 2a, 2b form loop piles while being engaged with a ground structure composed of the weft yarns 3 and the warp yarns 4a, 4b. The obtained towel fabric 1 is cut to a predetermined size, and the ends are processed to form a towel. FIG. 3B is a weave diagram of the towel fabric. This weave is a four-weft towel structure (four-pick terry motion structure). The warp pile yarns are crossed once for every four weft yarns. The warp yarns G and the warp pile yarns P are arranged alternately. Compared to a three-weft towel structure, a four-weft towel structure has pile yarns that are more firmly fixed to the ground structure, resulting in a lower rate of pilling and good pile standing, and therefore has the advantages of being bulky, voluminous, and quick drying due to good ventilation. The weft threads 1 to 4 indicate their order. In Fig. 3B, from the perspective of the warp threads, black and x indicate floating threads, and white indicates sinking threads. EXAMPLES
[0028] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to the following examples. <Evaluation of the texture of finished towel fabric> (1) Evaluation of soft texture The softness of the texture is expressed as the volume per gram of towel fabric and is calculated using the following bulk height formula. The higher the value, the softer and better the texture. The thickness was measured according to JIS L 1096 (2010) 8.5 Bulkiness Test, and the basis weight was measured by precisely weighing the weight of a 1m square. Measurements were taken at five points and the average value was expressed. Umbrella height (cm 3 / g) = Thickness (mm) / Weight (g / m 2 ) x 1000 (2) Evaluation of fluffy texture The towel fabric is compressed at a constant speed using a compression measuring device: KES-G5 (manufactured by Kato Tech Co., Ltd.) and the compression work: WC = (gf.cm 2 The measurements were taken at five locations, and the average value was calculated. The WC value is the amount of energy required to compress the fabric; the higher the value, the better the towel is compressed, the more fluffier it is, and the fluffier it is. (3) Evaluation of wash durability of texture The towel fabric was washed 30 times in a washing machine according to JIS L 0217 (1995), Method 103. After drying, the compression work: WC = (gf.cm 2 ) was measured at five locations and the average value was expressed. The smaller the difference in WC value before and after washing, the less the loss of fluffy texture due to washing, and the more durable and good the product is. (4) Evaluation of drainage during washing A 35cm wide piece of towel fabric was cut to a length so that it weighed 80g, the weight was accurately measured to one decimal place, and the piece was soaked in water for 20 minutes. The wet towel fabric was then taken out and centrifugally dehydrated in the spin tub of a washing machine for 4 minutes, the weight was accurately measured, and the residual moisture content (%) of the towel fabric was calculated using the following formula. The smaller the value, the better the drainage. Better drainage tends to lead to a faster subsequent drying speed. Three measurements were taken and the average value was used. Residual moisture content of fabric (%) = (Weight of fabric after soaking in water and dehydrating (W1)) - (Weight of fabric before soaking in water (W0)) / (Weight of fabric before soaking in water (W0)) x 100 (5) Drying property evaluation The wet towel fabric after dehydration prepared in the above (4) evaluation of drainage in washing was hung to dry, and the fabric weight was measured every 30 minutes as the drying time, and the time required for the fabric to reach a residual moisture content of 10% was calculated by dividing it by the time. The test environment was standard conditions, with a temperature of 20±4°C and a relative humidity of 65±4%RH. (6) Evaluation of pilling of towel fabric after washing The amount of shedding due to washing was measured according to JIS L0217 (1995), method 103. The percentage of shedding (%) was calculated using the following formula. The smaller the value, the less shedding and the better the result. The number of measurements was 5, and the average value was used. Lint shedding rate (%) = (weight of lint that fell off after washing (g1)) / (weight of towel before washing (g0)) x 100 (7) Water absorption evaluation (modified Larose method) The measurement was performed five times according to the modified Larose method of JIS L 1907 (2010), and the average value was calculated. The Larose index (water absorption index) was calculated according to the following formula. Larose index (water absorption index)=2545V×1411W+79 V: Maximum water absorption rate (ml / s), W: Water absorption amount at the maximum water absorption rate (ml) The higher the value, the faster and larger the amount of moisture absorbed from the skin, which is preferable. (8) Dimensional change rate The test was conducted in accordance with JIS L 1096 (2010) 8,39,6 G method (method for pulsator-type domestic electric washing machines). That is, the measurement was calculated using the following formula from the dimension (L1, mm) measured before washing and the dimension (L2, mm) measured after 30 washes and tumble drying. Dimensional change rate (ΔL%) = [(L2-L1) / L1] x 100 (9) Water absorption rate (dropping method) The water absorption rate of the terry cloth was measured and evaluated based on the Vuillet method, a drop method in JIS L 1907 (2010). The test outline was to drop a single drop of water onto the terry cloth from a height of 10 cm, measure the water absorption time (seconds) until the mirror-like surface of the drop disappeared three times, and calculate the average value. The shorter the time, the faster and better the water absorption. <Rewetting rate test method> The water-rewet rate is described in Patent Publication No. 6991633 proposed by the applicant, and is a test method in which water droplets are dropped onto a test specimen of the fabric, the water is absorbed, and the fabric is evaluated as the property of not releasing the water, i.e., the water-rewet rate, which coincides with the evaluation of the water absorbency felt by people when using a fiber fabric such as a towel. The lower the water-rewet rate, the greater the water absorbency of the fabric, and the better it can be evaluated to be. (1) Test environment and other conditions The test environment was standard, with a temperature of 20±4°C and a relative humidity of 65±4%. The filter papers were stored for at least 24 hours under standard conditions (temperature 20±4℃, relative humidity 65±4% RH). The test specimens were stored for at least 24 hours under standard conditions at a temperature of 20±4℃ and a relative humidity of 65±4%RH. The temperature of the water used for dripping was 20±15℃ (5~35℃). (2) Operation procedure The size of the test specimen of the fiber towel fabric was 10cm in length and 10cm in width. The test specimen was placed on the sample stand. The filter paper used was made of α-cellulose, conforming to the JIS P 3801 (1976) Class 1 standard, with a diameter of 110 mm and a thickness of 0.22 mm, and the weight of the filter paper was measured. The filter paper used was Advantec's "Circular Qualitative Filter Paper No. 1". Measure 0.8ml of water into a pipette, drop it into the test specimen, and wait 5 seconds to allow the test specimen to absorb the water. A filter paper was placed on top and a load of 1.3 kg (1274 Pa) was placed on top of it. Wait 5 seconds and then remove the load. The weight of the filter paper after absorbing water was measured. (3) Calculation of water rewetting rate Calculation was made using the following formula. W = [(B A) / A] × 100 Where W: Water rewetting rate (%) A: Weight of filter paper before measurement (g) B: Weight of filter paper after absorbing water (g) <Pile standing property> The pile portion of the towel fabric was observed using an optical microscope, with side photographs (magnification 30x). <Characteristics of sliver> Measurements were performed in accordance with JIS L 1019 (2006). <Other physical properties> The measurements were made according to the methods used in the industry.
[0029] Example 1 (1) Warp pile yarn Cotton with an average fiber length of 30.5 mm and a micronaire of 5.6 μg / inch was used as the fiber material for the warp pile yarn, and after passing it through a carding machine, it was combed twice (combed process), with the number of combing needles increased, the lap width adjusted as thin as possible, and the process was performed slowly at about 1 / 3 the normal speed. As a result, the short fiber content with an average fiber length of 17 mm or less was 3.8 mass%. The effective fiber length, short fiber content, and cut rate after each process are shown in Table 2. Staple diagrams of each sliver (fiber bundle) are shown in Figures 4 to 6.
[0030] [Table 2]
[0031] (2) Spinning of warp pile yarn Warp pile yarns were produced using a triple spun spinning device shown in Figure 1. The twist directions of the three rovings 12a, 12b, and 12c in the primary twist were all Z-direction, the twist direction by the spindle 21 was S-direction, and they were twisted in the untwisting direction. The fineness of the roving was 5g / 6 yards (9113 decitex), and the Z-direction twist number of the roving was 5 turns / inch (twist factor K=1 in terms of cotton count). The obtained spun yarn had a cotton count of 16.1 and a twist number of 11.5 turns / inch (twist factor K=2.875). The physical properties of the obtained warp pile yarns are shown in Table 3. (3) Spinning of warp and weft yarns The warp and weft yarns were made of cotton (extra-long staple cotton) with an average fiber length of 36.5 mm and a micronaire fineness of 3.5 μg / inch, which was spun into yarn using a ring spinning frame. The British cotton count was 20 and the twist factor K was 3.8. (4) Pile yarn, warp yarn, and weft yarn bleaching process The pile yarn, warp yarn and weft yarn were bleached. According to the usual method, they were scoured in a dilute caustic soda and alcohol ethoxylate-added bath at 98°C for 50 minutes, then bleached in a hydrogen peroxide bath at 98°C for 50 minutes, then sized at 95°C at 100 m / min, and finished by drying at 120°C (off-white finish). (5) Weaving process Pile yarn, warp yarn, and weft yarn were fed into a jacquard loom to weave a towel fabric with a four-pick terry motion weave as shown in Figures 3A-B. After weaving, the fabric was washed and dried in rolls, and then hemmed to produce a towel product. The pile length was 1.18 cm. Other physical properties are shown in Table 4.
[0032] Comparative Example 1 The same procedure as in Example 1 was carried out, except that card sliver was used as the warp pile yarn.
[0033] Comparative Example 2 The same procedure as in Example 1 was carried out, except that the warp pile yarns were not bleached, but were bleached after being woven into a fabric. The results for the warp pile yarns are shown in Table 3, and the results for the towel fabric are shown in Table 4.
[0034] [Table 3]
[0035] [Table 4]
[0036] As is clear from Table 4, the following effects were confirmed for the towel fabric of Example 1 compared to Comparative Examples 1 and 2. (1) Less shedding. (2) Bulky. (3) It has a large amount of fluffiness and is very soft before washing. (4) The fluffiness is less likely to be lost after washing, and deterioration due to washing is minimal. (5) There is little re-wetting, making wiping comfortable. (6) It is less likely to change dimensions when washed and is less likely to shrink. (7) It dries quickly and the residual moisture content drops to 10% or less in a short time. [Industrial Applicability]
[0037] The towel fabric of the present invention is suitable for use as a fabric for bath towels (towels for after a bath), bath towels, skin towels for bedding, face towels, towel handkerchiefs, sports towels, bathrobes, towel blankets, as well as for clothing, socks, rugs, bedding, etc. [Explanation of symbols]
[0038] 1. Towel fabric 2a, 2b warp pile yarn 3 Weft thread 4a, 4b Warp thread 10. Silospun spinning device 11a, 11b, 11c roving bobbin 12a,12b,12c roving 13 Trumpet Guide 14 Back roller 15 Draft device 16 Apron 17 Front roller 18a, 18b, 18c Fleece 19 Spun Yarn 20 Snell Wire 21 Spindle 22 Bobbin
Claims
1. A towel fabric composed of pile yarns, warp yarns and weft yarns, The pile yarn fiber material is medium-fiber cotton or long-fiber cotton having an average fiber length of 28.6 to 34.7 mm and a micronaire of 4.1 to 5.8 μg / inch, and the content of short fibers having an average fiber length of 17 mm or less is 10 mass % or less; The pile yarn is a single yarn of a sirospun yarn having no twist or a loose twist, The warp yarn and the weft yarn are ring-spun yarns using extra-long staple cotton having an average fiber length of 34.8 to 44.5 mm and a micronaire of 3.0 to 4.1 μg / inch; The towel fabric is characterized in that the pile yarns, warp yarns and weft yarns are bleached.
2. 2. The towel fabric according to claim 1, wherein the sirospun yarn has a count of 5 to 100 in English cotton count.
3. The towel fabric according to claim 1, wherein the twist coefficient K of the silo spun yarn is 0 to 3.
5. The twist factor (K) is calculated using the following formula (1). [0010] Where, t: number of twists (twists / 25.4mm), S: British cotton count
4. 2. The towel fabric according to claim 1, wherein the twist direction of the silo spun yarn is opposite to the primary twist direction of the multiple roving yarns, and a secondary twist is added that is equal to or greater than the number of twists in the primary twist.
5. The towel fabric according to claim 1, wherein the sirospun yarn is a two-strand sirospun yarn or a three-strand (triple) sirospun yarn.
6. 2. The towel fabric according to claim 1, wherein the warp yarns and the weft yarns have a count of 10 to 50 in English cotton count.
7. 2. The towel fabric according to claim 1, wherein the twist coefficient K of the warp yarns and the weft yarns is 3.5 to 4.
5. However, the twist factor (K) is calculated using the above formula (Math 1).
8. 2. The towel fabric according to claim 1, wherein the pile yarn is combed yarn.
9. A method for producing a towel fabric according to any one of claims 1 to 8, The pile yarn fiber material is medium-fiber cotton or long-fiber cotton having an average fiber length of 28.6 to 34.7 mm and a micronaire of 4.1 to 5.8 μg / inch, and the content of short fibers having an average fiber length of 17 mm or less is reduced to 10 mass% or less by combing treatment; The pile yarn is a triple spun yarn, and the twist direction is opposite to the primary twist direction of the three roving yarns, and a secondary twist number equal to or greater than the number of twists in the primary twist is added to form a non-twisted or loosely twisted single yarn. The pile yarns, warp yarns and weft yarns are subjected to a yarn bleaching treatment, A method for producing a towel fabric, comprising the steps of: supplying the pile yarns, warp yarns and weft yarns to a jacquard loom to produce a woven towel fabric.
10. The method for producing a towel fabric according to claim 9, further comprising dyeing the yarn after the bleaching treatment.
Citation Information
Patent Citations
Woven fabric and its production
JP1994025938A
Spun yarn and loop pile towel using the same
JP2022026952A
Towel fabric and its manufacturing method
JP7372718B1
Grandrelle yarn for pile yarn and woven or knitted fabric composed of grandrelle yarn for pile yarn
JP1998088440A
Soft twist spun yarn and method for producing soft twist spun yarn
JP2019137941A
Cited By
Woven pile fabric and method for manufacturing the same
JP7919104B1