Reactive modifier for thermosetting resins

The reactive modifier for thermosetting resins addresses the issues of weak adhesive force and poor flexibility in conventional resins by using a copolymer with specific molecular characteristics, improving bonding and electrical properties in flexible printed wiring boards and laminates.

JP7553363B2Active Publication Date: 2024-09-18SANYO CHEM IND LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
JP2021001821
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2021-01-08
Publication Date
2024-09-18
Estimated Expiration
2041-01-08

AI Technical Summary

Technical Problem

Conventional thermosetting resins used in printed wiring boards and contact IC cards face issues with weak adhesive force, poor electrical properties, and low flexibility due to their low polarity and rigid molecular structures, making it difficult to manufacture parts for flexible printed wiring boards (FPCs) and laminates.

Method used

A reactive modifier for thermosetting resins is developed, comprising a copolymer with structural units derived from monofunctional radically polymerizable monomers with aromatic and saturated aliphatic groups, which improves adhesive strength, heat resistance, and electrical properties by incorporating a copolymer (A) with specific molecular weight, solubility parameters, and concentration of radically polymerizable groups.

Benefits of technology

The reactive modifier enhances the adhesive strength, flexibility, and electrical properties of cured thermosetting resin products, ensuring effective bonding and reduced dielectric constant, suitable for applications in flexible printed wiring boards and laminates.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007553363000002
    Figure 0007553363000002
  • Figure 0007553363000001
    Figure 0007553363000001
Patent Text Reader

Abstract

To provide a reactive modifier for thermosetting resin that can give a cured product of thermosetting resin excellent adhesive strength, heat thermostability, bendability and electric characteristics (low dielectric constants), and a thermosetting resin composition comprising the same, and a cured product.SOLUTION: A reactive modifier for thermosetting resin contains a copolymer (A) that contains, as essential constitutional units, a constitutional unit derived from a monofunctional radical-polymerizable monomer (a) having an aromatic group, a constitutional unit derived from a monofunctional radical-polymerizable monomer (b) having no aromatic group but having a saturated aliphatic group, and a constitutional unit (e) having a radical-polymerizable group. The saturated aliphatic group included in the monomer (b) has 6-22 carbon atoms. The monomer (b) has a solubility parameter of 8.0 or more and less than 9.5. The copolymer (A) has a weight average molecular weight of 3000-70000.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a reactive modifier for thermosetting resins. [Background technology]

[0002] In recent years, the demand for faster transmission signals in printed wiring boards has led to a remarkable increase in the frequency of transmission signals. This has led to a demand for materials used in printed wiring boards that can reduce electrical signal loss in the high frequency range, specifically in the frequency range of 1 GHz or higher. In response to this demand, substrates with low dielectric properties, such as liquid crystal polymers (LCPs), syndiotactic polystyrene (sPS), and polyphenylene sulfide (PPS), have been proposed as substrates for printed wiring boards, particularly flexible printed wiring boards (FPCs), instead of conventional polyimide (PI) and polyethylene terephthalate films. In addition, since thermosetting resins are cured by heating, they are widely used as adhesives when manufacturing wiring boards such as printed wiring boards and contact-type IC cards. Known examples of such thermosetting resins include epoxy resins (Patent Document 1) and polyimide resins (Patent Documents 2-3). However, since substrates with low dielectric properties (such as LCP) have low polarity, when conventional thermosetting resins such as epoxy resins and polyimide resins are used, the adhesive strength is weak, making it difficult to manufacture FPC components such as coverlay films and laminates. In addition, thermosetting resins such as epoxy resins and polyimide resins have poor electrical properties, which impair the dielectric properties of FPCs. Furthermore, these thermosetting resins contain many rigid molecular structures within the molecule, which results in low flexibility. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] JP 2016-188303 A [Patent Document 2] JP 2009-299040 A [Patent Document 3] JP 2014-045076 A Summary of the Invention [Problem to be solved by the invention]

[0004] The present invention aims to provide a reactive modifier for thermosetting resins that can impart excellent adhesive strength, heat resistance, flexibility, and electrical properties (low dielectric constant) to a cured product of a thermosetting resin, as well as a thermosetting resin composition and a cured product containing the same. [Means for solving the problem]

[0005] As a result of investigations aimed at achieving the above object, the present inventors arrived at the present invention. That is, the present invention relates to a reactive modifier for thermosetting resins, which contains a copolymer (A) having essential structural units, that is, a structural unit derived from a monofunctional radically polymerizable monomer (a) having an aromatic group, a structural unit derived from a monofunctional radically polymerizable monomer (b) having no aromatic group and a saturated aliphatic group, and a structural unit (e) having a radically polymerizable group, the thermosetting resin is an epoxy resin, The number of carbon atoms in the saturated aliphatic group of the monomer (b) is 6 to 22, and the solubility parameter of the monomer (b) is 8.0 (cal / cm 3 ) 1 / 2 More than 9.5(cal / cm 3 ) 1 / 2 is less than The concentration of the radical polymerizable group in the copolymer (A) is 0.2 to 1.2 mol / kg;a reactive modifier for thermosetting resins, in which the copolymer (A) has a weight average molecular weight of 3,000 to 70,000, and the weight ratio of the structural units derived from the monomer (a) is 10 to 80% by weight, the weight ratio of the structural units derived from the monomer (b) is 10 to 80% by weight, and the weight ratio of the structural unit (e) is 2 to 30% by weight, based on the weight of all structural units constituting the copolymer (A); a thermosetting resin composition containing the reactive modifier for thermosetting resins and a thermosetting resin (X); a laminate in which a resin substrate and a resin substrate or a metal substrate are bonded by the thermosetting resin composition; an adhesive sheet having the laminate; a printed wiring board containing the adhesive sheet as a component; and a cured product obtained by curing the thermosetting resin composition. Effect of the Invention

[0006] The reactive modifier for thermosetting resins and the thermosetting resin composition of the present invention have the effect of providing a cured product having excellent adhesive strength, heat resistance, flexibility and electrical properties (low dielectric constant). In the present invention, the reactive modifier for thermosetting resin means an additive that can impart excellent adhesive strength, flexibility, and electrical properties to a cured product of a thermosetting resin without impairing heat resistance. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0007] The reactive modifier for thermosetting resins of the present invention is a copolymer (A) having essential structural units, which are a structural unit derived from a monofunctional radically polymerizable monomer (a) having an aromatic group, a structural unit derived from a monofunctional radically polymerizable monomer (b) having no aromatic group and a saturated aliphatic group, and a structural unit (e) having a radically polymerizable group, wherein the number of carbon atoms in the saturated aliphatic group of the monomer (b) is 6 to 22, and the solubility parameter of the monomer (b) is 8.0 (cal / cm 3 ) 1 / 2 More than 9.5(cal / cm 3 ) 1 / 2the weight average molecular weight of the copolymer (A) is 3,000 to 70,000, the weight ratio of the structural units derived from the monomer (a) is 10 to 80% by weight, the weight ratio of the structural units derived from the monomer (b) is 10 to 80% by weight, and the weight ratio of the structural units (e) is 2 to 20% by weight, based on the weight of all structural units constituting the copolymer (A).

[0008] <Copolymer (A)> In the present invention, the copolymer (A) is a copolymer having, as essential constituent units, a constituent unit derived from a monofunctional radically polymerizable monomer (a) having an aromatic group, a constituent unit derived from a monofunctional radically polymerizable monomer (b) having no aromatic group and having a saturated aliphatic group, and a constituent unit (e) having a radically polymerizable group, the copolymer has a radically polymerizable carbon-carbon double bond, the saturated aliphatic group of the monofunctional radically polymerizable monomer (b) has 6 to 22 carbon atoms, and the solubility parameter of the monofunctional radically polymerizable monomer (b) is 8.0 (cal / cm 3 ) 1 / 2 More than 9.5(cal / cm 3 ) 1 / 2 The copolymer has a weight average molecular weight of 3,000 to 70,000, and the weight proportion of the structural units derived from the monomer (a) is 10 to 80% by weight, the weight proportion of the structural units derived from the monofunctional radically polymerizable monomer (b) is 10 to 80% by weight, and the weight proportion of the structural units (e) is 2 to 20% by weight, based on the weight of all structural units constituting the copolymer (A). In this specification, "radically polymerizable" means having a carbon-carbon double bond capable of radical polymerization. In addition, radically polymerizable monomers include compounds having a radically polymerizable vinyl group (HC=CH-), vinylidene group, or vinylene group (-HC=CH-), and examples thereof include monomers having a (meth)acryloyl group, a carbon-carbon double bond {-OC(O)HC=CH-C(O)O-} in a mono- or diesterification product of (anhydride) maleic acid or fumaric acid, a vinyl ether group, a styryl group, or the like. In addition, a monomer means one having 30 or less carbon atoms. In addition, in this specification, "(meth)acrylate" means "acrylate and / or methacrylate", "(meth)acrylic acid" means "acrylic acid and / or methacrylic acid", "(meth)acrylic resin" means "acrylic resin and / or methacrylic resin", "(meth)acryloyl group" means "acryloyl group and / or methacryloyl group", and "(meth)acryloyloxy group" means "acryloyloxy group and / or methacryloyloxy group".

[0009] <Monomer (a)> Monomer (a) is a compound having one radical polymerizable group and an aromatic group, and includes those having 8 to 25 carbon atoms, and examples of such monomers include styrene-based monomers {e.g., styrene, α-methylstyrene, etc.}, (meth)acrylates having an aromatic ring {e.g., benzyl (meth)acrylate, naphthyl (meth)acrylate, phenoxyethyl (meth)acrylate, phenoxypropyl (meth)acrylate, phenoxybutyl (meth)acrylate, m-phenoxybenzyl (meth)acrylate, 2-(1-naphthyloxy)ethyl (meth)acrylate, 2-methylphenyl ... 1-(2-naphthyloxy)ethyl (meth)acrylate, 6-(1-naphthyloxy)hexyl (meth)acrylate, 6-(2-naphthyloxy)hexyl (meth)acrylate, 8-(1-naphthyloxy)octyl (meth)acrylate, 8-(2-naphthyloxy)octyl (meth)acrylate, ethoxylated-o-phenylphenol acrylate, etc.}, vinyl ethers having an aromatic ring {for example, benzyl vinyl ether, phenoxyethyl vinyl ether, cyclohexylphenoxyethyl vinyl ether, etc.}, and the like. In addition, those having one radically polymerizable group and an aromatic group, and further having a hydroxyl group, an isocyanate group, a carboxyl group or an epoxy group are defined as monomer (c) and / or monomer (d) described later.

[0010] Among these, from the viewpoints of adhesive strength and heat resistance, styrene, benzyl (meth)acrylate, phenoxyethyl (meth)acrylate, m-phenoxybenzyl (meth)acrylate, and ethoxylated-o-phenylphenol acrylate are preferred.

[0011] From the viewpoint of adhesive strength and heat resistance, the copolymer (A) is preferably a copolymer containing at least one monomer selected from the group consisting of styrene, benzyl (meth)acrylate, phenoxyethyl (meth)acrylate, and m-phenoxybenzyl (meth)acrylate as a constituent monomer.

[0012] <Monomer (b)> Monomer (b) is a compound having one radical polymerizable group and a saturated aliphatic group (having 6 to 22 carbon atoms) and no aromatic ring, and has a solubility parameter of 8.0 (cal / cm 3 ) 1 / 2 More than 9.5(cal / cm 3 ) 1 / 2 It is a compound having a molecular weight of less than 1. Solubility parameter (hereinafter sometimes abbreviated as SP value, unit (cal / cm 3 ) 1 / 2 SP is an abbreviation for solubility parameter, and is a measure of solubility. The larger the SP value, the higher the polarity, and conversely, the smaller the SP value, the lower the polarity. The SP value is calculated at 25°C according to the method described in Polymer Engineering and Science, Vol. 14, pp. 151-154, by Robert F. Fedors et al. Examples of the monomer (b) include alkyl (meth)acrylates having an alkyl group with 6 to 22 carbon atoms {e.g., n-hexyl acrylate (SP value: 8.77), n-hexyl methacrylate (SP value: 8.77), n-heptyl acrylate (SP value: 8.75), n-heptyl methacrylate (SP value: 8.76), n-octyl (meth)acrylate, 2-ethylhexyl acrylate (SP value: 8.62), 2-ethylhexyl methacrylate (SP value: 8.63), isooctyl (meth)acrylate, (meth)acrylate, n-nonyl acrylate (SP value: 8.73), n-nonyl methacrylate (SP value: 8.73), isononyl (meth)acrylate, n-decyl (meth)acrylate, isodecyl acrylate (SP value: 8.61), isodecyl methacrylate (SP value: 8.62), undecyl (meth)acrylate, lauryl acrylate (SP value: 8.70), lauryl methacrylate (SP value: 8.70), tridecyl (meth)acrylate, tetradecyl (meth)acrylate cetyl (meth)acrylate, stearyl (meth)acrylate, isostearyl acrylate (SP value: 8.59), isostearyl methacrylate (SP value: 8.60), behenyl acrylate (SP value: 8.65), behenyl methacrylate (SP value: 8.65), etc.}, alicyclic skeleton-containing (meth)acrylates having 9 to 26 carbon atoms [for example, cyclohexyl acrylate (SP value: 9.26), cyclohexyl methacrylate (SP value: 9.22), t-butyl cyclohexyl acrylate (SP value: 9.26 ... (SP value: 8.72), t-butylcyclohexyl methacrylate (SP value: 8.72), dicyclopentanyl (meth)acrylate, isobornyl (meth)acrylate, trimethylcyclohexyl (meth)acrylate {for example, 3,5,5-trimethylcyclohexyl acrylate (SP value: 8.73), 3,5,5-trimethylcyclohexyl methacrylate (SP value: 8.73), etc.}, vinyl ether compounds having 8 to 30 carbon atoms {for example, n-nonyl vinyl ether (SP value 8.03), n-decyl vinyl ether, undecyl vinyl ether, lauryl vinyl ether, tridecyl vinyl ether, tetradecyl vinyl ether, cetyl vinyl ether, stearyl vinyl ether, isostearyl vinyl ether, behenyl vinyl ether (SP value: 8.30), cyclohexyl vinyl ether, cyclohexylethyl vinyl ether, etc.}, diesters of aliphatic monoalcohols having 6 to 22 carbon atoms with maleic acid {for example, , dihexyl maleate (SP value: 9.21), bis(2-ethylhexyl) maleate, dibehenyl maleate (SP value: 8.80), hexylheptyl maleate, n-hexyl(n-decyl) maleate, etc.}, diesters of aliphatic monoalcohols having 6 to 22 carbon atoms with fumaric acid {for example, dihexyl fumarate, bis(2-ethylhexyl) fumarate, hexylheptyl fumarate, n-hexyl(n-decyl) fumarate, etc.}, etc. In addition, those having one radically polymerizable group, a saturated aliphatic group (having 6 to 22 carbon atoms), and further having a hydroxyl group, an isocyanate group, a carboxyl group, or an epoxy group are defined as monomer (c) and / or monomer (d) described later.

[0013] Of these, from the viewpoints of dielectric constant and flexibility, 2-ethylhexyl (meth)acrylate, n-nonyl (meth)acrylate, isodecyl (meth)acrylate, lauryl (meth)acrylate, isostearyl (meth)acrylate, behenyl (meth)acrylate, cyclohexyl (meth)acrylate, t-butylcyclohexyl (meth)acrylate, and trimethylcyclohexyl (meth)acrylate are preferred. From the viewpoint of dielectric constant, the SP value of the monomer (b) is preferably from 8.0 to 9.4, and more preferably from 8.0 to 9.0.

[0014] From the viewpoints of dielectric constant and flexibility, the copolymer (A) is preferably a copolymer containing, as a constituent monomer, at least one selected from the group consisting of 2-ethylhexyl (meth)acrylate, nonyl (meth)acrylate, isodecyl (meth)acrylate, lauryl (meth)acrylate, isostearyl (meth)acrylate, behenyl (meth)acrylate, cyclohexyl (meth)acrylate, t-butylcyclohexyl (meth)acrylate, and trimethylcyclohexyl (meth)acrylate.

[0015] In the present invention, the copolymer (A) has a constituent unit (e) having a radical polymerizable group as an essential constituent unit, and (A) has a radical polymerizable group derived from the above (e). Examples of the radical polymerizable group that the copolymer (A) has include a (meth)acryloyl group, a carbon-carbon double bond in an ester of maleic anhydride {—OC(O)HC=CH—C(O)O—}, and a vinyl ether group. The copolymer (A) can be made into a copolymer having a structural unit (e) having a radical polymerizable group by, for example, adding a compound (d) having a radical polymerizable group and a group reactive with the reactive group in (c) to a copolymer (S) obtained by radical polymerization of monomers (a), (b) and a monomer (c) having a reactive group. In this method, the structural unit (e) is obtained by adding (d) to the structural unit derived from monomer (c). Specifically, for example, the following reactions (1) to (5) can be mentioned. A plurality of reactions (1) to (5) may be combined. Among these, reactions (1) to (3) are preferred from the viewpoint of thermosetting property. Examples of the monomer (c) include the following monomers (c1) to (c5), examples of the monomer (d) include the following monomers (d1) to (d5), and examples of the copolymer (S) include the following monomers (S1) to (S5).

[0016] Specific methods for converting the copolymer (A) into a copolymer having a (meth)acryloyl group include the following (1) to (3). (1) A polymer (S1) obtained by copolymerizing the monomers (a) and (b) and, in addition, a monofunctional radically polymerizable monomer (c1) having one hydroxyl group and / or a monofunctional radically polymerizable monomer (c2) having one carboxyl group is subjected to a urethane reaction (addition reaction) with a compound (d1) having one isocyanate group and a (meth)acryloyl group. (2) A compound (d2) having one epoxy group and a (meth)acryloyl group is added to a polymer (S2) obtained by copolymerizing the monomers (a) and (b) and, in addition, a monofunctional radically polymerizable monomer (c1) having one hydroxyl group and / or a monofunctional radically polymerizable monomer (c2) having one carboxyl group. (3) A compound (d3) having one carboxyl group and a (meth)acryloyl group is added to a polymer (S3) obtained by copolymerizing the monomers (a) and (b) and a monofunctional radically polymerizable monomer (c3) having one epoxy group.

[0017] Specific examples of the method for making the copolymer (A) into a copolymer having a carbon-carbon double bond {—OC(O)HC=CH—C(O)O—} in an ester of maleic anhydride include the following (4). (4) A polymer (S4) obtained by copolymerizing the monomers (a) and (b) and a monofunctional radically polymerizable monomer (c1) having one hydroxyl group is subjected to a half-esterification reaction (addition reaction) with maleic anhydride (d4).

[0018] Specific examples of the method for converting the copolymer (A) into a copolymer having a vinyl ether group include the following method (5). (5) A polymer (S5) obtained by copolymerizing the monomers (a) and (b) and a monofunctional radically polymerizable monomer (c5) having one isocyanate group is subjected to a urethane reaction with a compound (d5) having one hydroxyl group and a vinyl ether group.

[0019] The monofunctional radically polymerizable monomer (c1) having one hydroxyl group includes those having 2 to 9 carbon atoms, such as vinyl alcohol, hydroxyalkyl (alkyl group having 1 to 5 carbon atoms) vinyl ether {e.g., hydroxymethyl vinyl ether, hydroxyethyl vinyl ether, hydroxypropyl vinyl ether, hydroxybutyl vinyl ether, hydroxypentyl vinyl ether, etc.}, and hydroxyalkyl (alkyl group having 1 to 5 carbon atoms) (meth)acrylate {e.g., hydroxymethyl (meth)acrylate, hydroxyethyl (meth)acrylate, hydroxypropyl (meth)acrylate, hydroxybutyl (meth)acrylate, hydroxypentyl (meth)acrylate, etc.}. Among these, from the viewpoint of radical polymerizability, hydroxyalkyl (alkyl group having 1 to 5 carbon atoms) (meth)acrylates are preferred, and hydroxyethyl (meth)acrylate, hydroxypropyl (meth)acrylate, and hydroxybutyl (meth)acrylate are more preferred.

[0020] The monofunctional radically polymerizable monomer (c2) having one carboxyl group includes those having 3 to 30 carbon atoms, such as (meth)acrylic acid, crotonic acid, monoesters of aliphatic dicarboxylic acids having 2 to 7 carbon atoms and hydroxyalkyl (having 1 to 5 carbon atoms) (meth)acrylates {for example, 2-(meth)acryloyloxyethyl succinic acid, 3-(meth)acryloyloxypropyl succinic acid, 4-(meth)acryloyloxybutyl succinic acid, 5-(meth)acryloyloxypentyl succinic acid, etc.}, monoesters of aliphatic monoalcohols having 1 to 26 carbon atoms and maleic acid {for example, n-hexyl maleate, n-heptyl maleate, n-octyl maleate, 2-ethylhexyl maleate, isooctyl maleate, n-nonyl maleate, fumarate, isononyl fumarate, n-decyl maleate, isodecyl maleate, undecyl maleate, lauryl maleate, tridecyl maleate, tetradecyl maleate, cetyl maleate, stearyl maleate, isostearyl maleate, behenyl maleate, etc.}, monoesters of aliphatic monoalcohols having 1 to 26 carbon atoms with fumaric acid {for example, n-hexyl fumarate, n-heptyl fumarate, n-octyl fumarate, 2-ethylhexyl fumarate, isooctyl fumarate, n-nonyl fumarate, isononyl fumarate, n-decyl fumarate, isodecyl fumarate, undecyl fumarate, lauryl fumarate, tridecyl fumarate, tetradecyl fumarate, cetyl fumarate, stearyl fumarate, isostearyl fumarate, behenyl fumarate, etc.}, and the like. Among these, (meth)acrylic acid and 2-(meth)acryloyloxyethyl succinic acid are preferred from the viewpoint of radical polymerizability.

[0021] The monofunctional radically polymerizable monomer (c3) having one epoxy group includes those having 5 to 30 carbon atoms, and examples thereof include glycidyl vinyl ether, glycidyl ethers of hydroxyalkyl (alkyl group having 1 to 5 carbon atoms) vinyl ether {e.g., hydroxymethyl vinyl ether, 2-hydroxyethyl vinyl ether glycidyl ether, 3-hydroxypropyl vinyl ether glycidyl ether, 4-hydroxybutyl vinyl ether glycidyl ether, 5-hydroxypentyl vinyl ether glycidyl ether, etc.}, glycidyl (meth)acrylate, glycidyl ethers of hydroxyalkyl (1 to 5 carbon atoms) (meth)acrylate {e.g., 2-hydroxyethyl (meth)acrylate glycidyl ether, 3-hydroxypropyl (meth)acrylate glycidyl ether, 4-hydroxybutyl (meth)acrylate glycidyl ether, 5-hydroxypentyl (meth)acrylate glycidyl ether, etc.}, and the like. Of these, glycidyl (meth)acrylate is preferred from the viewpoint of radical polymerizability.

[0022] Examples of the monofunctional radically polymerizable monomer (c5) having one isocyanate group include (meth)acryloyloxyalkyl (alkyl group having 2 to 5 carbon atoms) isocyanates {e.g., 2-(meth)acryloyloxyethyl isocyanate, 3-(meth)acryloyloxypropyl isocyanate, 4-(meth)acryloyloxybutyl isocyanate, 5-(meth)acryloyloxypentyl isocyanate, etc.} and isocyanatoalkyl (carbon number: 1 to 5) vinyl ethers {e.g., 2-isocyanatoethyl vinyl ether, 3-isocyanatopropyl vinyl ether, 4-isocyanatobutyl vinyl ether, 5-isocyanatopentyl vinyl ether, etc.}. Of these, 2-(meth)acryloyloxyethyl isocyanate is preferred from the viewpoint of radical polymerizability.

[0023] Examples of the compound (d1) having one isocyanate group and a (meth)acryloyl group include the above-mentioned (meth)acryloyloxyalkyl (alkyl group having 2 to 5 carbon atoms) isocyanates. Of these, 2-(meth)acryloyloxyethyl isocyanate is preferred from the viewpoint of addition reactivity.

[0024] Examples of the compound (d2) having one epoxy group and a (meth)acryloyl group include glycidyl (meth)acrylate and glycidyl ether of hydroxyalkyl (having 1 to 5 carbon atoms) (meth)acrylate {for example, 2-hydroxyethyl (meth)acrylate glycidyl ether, 3-hydroxypropyl (meth)acrylate glycidyl ether, 4-hydroxybutyl (meth)acrylate glycidyl ether, 5-hydroxypentyl (meth)acrylate glycidyl ether, etc.}. Of these, 2-hydroxyethyl (meth)acrylate glycidyl ether is preferred from the viewpoint of addition reactivity.

[0025] Examples of the compound (d3) having one carboxyl group and a (meth)acryloyl group include (meth)acrylic acid, and monoesters of aliphatic dicarboxylic acids having 2 to 7 carbon atoms and hydroxyalkyl (having 1 to 5 carbon atoms) (meth)acrylates {e.g., 2-(meth)acryloyloxyethyl succinic acid, 3-(meth)acryloyloxypropyl succinic acid, 4-(meth)acryloyloxybutyl succinic acid, 5-(meth)acryloyloxypentyl succinic acid, etc.}. Of these, (meth)acrylic acid is preferred from the viewpoint of addition reactivity.

[0026] Examples of the compound (d5) having one hydroxyl group and a vinyl ether group include hydroxyalkyl (alkyl group having 1 to 5 carbon atoms) vinyl ethers {e.g., hydroxymethyl vinyl ether, hydroxyethyl vinyl ether, hydroxypropyl vinyl ether, hydroxybutyl vinyl ether, hydroxypentyl vinyl ether, etc.}. Of these, hydroxyethyl vinyl ether is preferred from the viewpoint of addition reactivity.

[0027] As the structural unit (e), from the viewpoints of adhesive strength, heat resistance, flexibility and electrical properties, a structural unit obtained by addition reaction of a structural unit derived from a monomer (c) with (d), in which (c) is a monofunctional radically polymerizable monomer (c1) having one hydroxyl group and / or a monofunctional radically polymerizable monomer (c2) having one carboxyl group, and (d) is a compound (d1) having one isocyanate group and a (meth)acryloyl group, a monofunctional radically polymerizable monomer (c1) having one hydroxyl group and / or a monofunctional radically polymerizable monomer (c2) having one carboxyl group, and (d) is a compound (d2) having one epoxy group and a (meth)acryloyl group, and a monofunctional radically polymerizable monomer (c1) having one hydroxyl group and / or a monofunctional radically polymerizable monomer (c2) having one carboxyl group, and (d) is a compound (d2) having one epoxy group and a (meth)acryloyl group, and and (c3)), in which (d) is a compound (d3) having one carboxyl group and a (meth)acryloyl group, are preferred, and more preferred are those obtained by addition reaction of a structural unit derived from monomer (c) with (d), in which (c) is a monofunctional radically polymerizable monomer (c1) having one hydroxyl group and / or a monofunctional radically polymerizable monomer (c2) having one carboxyl group, and (d) is a compound (d1) having one isocyanate group and a (meth)acryloyl group, and those in which (c) is a monofunctional radically polymerizable monomer (c1) having one hydroxyl group and / or a monofunctional radically polymerizable monomer (c2) having one carboxyl group, and (d) is a compound (d2) having one epoxy group and a (meth)acryloyl group.

[0028] The weight proportion of the monomer (a) in the monomers constituting the copolymer (S) is preferably 10 to 80% by weight, more preferably 20 to 70% by weight, based on the total weight of the monomers constituting (S), from the viewpoints of dielectric constant, flexibility, adhesive strength and heat resistance. The weight proportion of the monomer (b) in the monomers constituting the copolymer (S) is preferably 10 to 80% by weight, more preferably 20 to 70% by weight, based on the total weight of the monomers constituting (S), from the viewpoints of adhesive strength, heat resistance, dielectric constant and flexibility. The weight proportion of (c) in the monomers constituting the copolymer (S) is preferably 2 to 20% by weight, more preferably 2 to 10% by weight, based on the total weight of the monomers constituting (S), from the viewpoints of dielectric constant, flexibility and heat resistance.

[0029] The weight proportion of monomer (a) in the monomers constituting copolymer (A) is preferably 10 to 80% by weight, and more preferably 20 to 70% by weight, based on the total weight of the monomers constituting (A) (the total weight of (a), (b), and (c) that have not reacted with (d), the reaction product of (c) and (d), and other monomer (f) described below; the same applies hereinafter), from the viewpoints of dielectric constant, flexibility, adhesive strength, and heat resistance. The weight proportion of the monomer (b) in the monomers constituting the copolymer (A) is preferably 10 to 80% by weight, more preferably 20 to 80% by weight, based on the total weight of the monomers constituting (A), from the viewpoints of dielectric constant, flexibility, adhesive strength and heat resistance. The weight ratio of the reaction product of (c) and (d) in the monomers constituting copolymer (A) is preferably 2 to 30% by weight, more preferably 2 to 20% by weight, based on the total weight of the monomers constituting (A), from the viewpoint of achieving both thermosetting property and dielectric constant.

[0030] The weight proportion of the structural units derived from the monomer (a) constituting the copolymer (A) is 10 to 80% by weight, and preferably 20 to 70% by weight, based on the weight of all structural units constituting (A). If the weight ratio of (a) is less than 10% by weight, the adhesive strength and heat resistance tend to be insufficient, whereas if it exceeds 80% by weight, the dielectric constant tends to be high and the flexibility tends to be poor. The weight proportion of the structural units derived from the monomer (b) constituting the copolymer (A) is 10 to 80% by weight, and preferably 20 to 80% by weight, based on the weight of all structural units constituting (A). If the weight proportion of (b) is less than 10% by weight, the dielectric constant of the thermoset product will be high and the flexibility will tend to be insufficient, whereas if it exceeds 80% by weight, the adhesive strength and heat resistance will tend to be insufficient. The weight proportion of the structural unit (e) constituting the copolymer (A) is 2 to 30% by weight, and preferably 2 to 20% by weight, based on the weight of all structural units constituting (A), from the viewpoints of thermosetting property, heat resistance, and dielectric constant. If the weight ratio of (e) is less than 2% by weight, the heat resistance tends to deteriorate, whereas if it exceeds 30% by weight, the dielectric constant tends to deteriorate.

[0031] The copolymer (A) may contain a structural unit derived from a monomer (c) and a structural unit derived from another monomer (f), if necessary. Examples of (f) include (meth)acrylamide, monofunctional radically polymerizable monomers having a saturated aliphatic group with an SP value of less than 8.0 or 9.5 or more {e.g., N-alkyl(meth)acrylamide (e.g., N-methyl(meth)acrylamide, etc.), dialkyl(meth)acrylamide (e.g., N,N-dimethyl(meth)acrylamide, etc.), etc.}. From the viewpoint of dielectric constant, the weight proportion of the structural units derived from the monomers (c) and (f) constituting the copolymer (A) is preferably 30% by weight or less, and more preferably 20% by weight or less, based on the weight of all structural units constituting (A).

[0032] The weight average molecular weight (hereinafter sometimes abbreviated as Mw) of the copolymer (A) is from 3,000 to 70,000, preferably from 5,000 to 60,000, and more preferably from 7,000 to 50,000. If Mw is less than 3,000, the dielectric constant will be high, and flexibility and heat resistance will tend to be insufficient, whereas if it exceeds 70,000, adhesive strength will tend to be insufficient.

[0033] The Mw of the copolymer (A) is measured by dissolving the copolymer (A) in tetrahydrofuran (THF) and using the resulting sample solution as a gel permeation chromatography (GPC) under the following conditions. Equipment: Tosoh Corporation HLC-8120 Column: TSK GEL GMH6 x 2 (Tosoh Corporation) Measurement temperature: 40℃ Sample solution: 0.25% by weight in THF Solution injection volume: 100μL Detector: Refractive index detector Reference material: Tosoh standard polystyrene [TSKstandard POLYSTYRENE] 12 points (molecular weight: 500,1050,2800,5970,9100,18100,37900,96400,190000,355000,1090000,2890000)

[0034] The concentration of the radically polymerizable group in the copolymer (A) is preferably from 0.1 to 1.5 mol / kg, and more preferably from 0.2 to 1.2 mol / kg, from the viewpoints of flexibility and heat resistance. The concentration of the radical polymerizable group in the copolymer (A) can be calculated from the amounts of the monomers (a) to (c) and the compound (d) used in the production of the copolymer (A) and the concentration of the radical polymerizable group in the compound (d).

[0035] The glass transition point of the copolymer (A) (hereinafter, the glass transition point may be abbreviated as Tg. This means the glass transition point of (A), not of the polymer of the copolymer (A)) is preferably -30 to 80°C, more preferably -20 to 70°C, from the viewpoints of flexibility and heat resistance. In the present invention, the glass transition point is measured by the method specified in ASTM D3418-82 (DSC method) using DSC20 and SSC / 580 manufactured by Seiko Instruments Inc. When two or more glass transition points exist, the lowest temperature is defined as the glass transition point Tg. The glass transition point of the copolymer (A) can be lowered by using a large amount of a monomer having a low homopolymer glass transition point as a constituent monomer, and can be raised by using a large amount of a monomer having a high homopolymer glass transition point as a constituent monomer. The glass transition point can be lowered by decreasing the molecular weight of the copolymer (A), and can be raised by increasing the molecular weight.

[0036] The SP value of the copolymer (A) is preferably from 8.7 to 9.7, and more preferably from 8.8 to 9.5, from the viewpoint of dielectric constant. The SP value of the copolymer (A) can be determined by calculating the average value based on the solids weight ratio in the monomers constituting the copolymer (A) using the SP value of each monomer. The SP value of the copolymer (A) can be adjusted by the type and amount of the monomer used. Specifically, the SP value can be decreased by increasing the number of alkyl groups having a long carbon number, and can be increased by increasing the number of alkyl groups having a short carbon number or a large proportion of polar groups.

[0037] The acid value of the copolymer (A) is preferably 50 mgKOH / g or less, more preferably 45 mgKOH / g or less, from the viewpoint of dielectric constant. The acid value can be measured in accordance with JIS K0070.

[0038] The hydroxyl value of the copolymer (A) is preferably 50 mgKOH / g or less, more preferably 45 mgKOH / g or less, from the viewpoint of dielectric constant. The hydroxyl value can be measured in accordance with JIS K0070.

[0039] The total of the acid value and the hydroxyl value of the copolymer (A) is preferably 70 mgKOH / g or less, more preferably 60 mgKOH / g or less, from the viewpoint of dielectric constant.

[0040] The dielectric constant of the copolymer (A) measured at 25° C. and 1 MHz is preferably 3.5 or less, more preferably 3.2 or less, and particularly preferably 3.0 or less, from the viewpoint of electrical properties. The dielectric constant of the copolymer (A) can be reduced by increasing the content of (b) as a constituent monomer in the copolymer (A). The dielectric constant can be measured by an LCR meter. Specifically, a xylene solution containing 50% by weight of copolymer (A) is applied to a release film having a thickness of 50 μm so that the thickness after drying is 30 μm, and the solution is dried at 130° C. for 3 minutes, then heat-treated at 140° C. for 4 hours to harden the solution, and peeled off from the release film. The obtained sample can be measured using a PRECISION LCR meter HP-4284A under conditions of 25° C., 58% RH, and a frequency of 1 MHz.

[0041] <Reactive modifier for thermosetting resin> The reactive modifier for thermosetting resins of the present invention is a reactive modifier for thermosetting resins containing the copolymer (A). The reactive modifier for thermosetting resins may contain a radical reaction initiator for the purpose of initiating and / or accelerating the curing reaction of the copolymer (A).

[0042] As the radical reaction initiator, known ones can be used. For example, dialkyl peroxide radical reaction initiators such as α,α'-bis(t-butylperoxy)diisopropylbenzene, dicumyl peroxide, di-t-hexyl peroxide, 2,5-dimethyl-2,5-bis(t-butylperoxy)hexane, 2,5-dimethyl-2,5-bis(t-butylperoxy)hexyne, and di-t-butyl peroxide; p-menthahydroperoxide; diisopropyl peroxide; Hydroperoxide radical reaction initiators such as propylbenzene hydroperoxide, 1,1,3,3,-tetramethylbutyl hydroperoxide, cumene hydroperoxide, and t-butyl hydroperoxide, t-butylcumyl peroxide, benzoyl peroxide, 1,1-bis(t-hexylperoxy)-3,3,5-trimethylcyclohexane, 1,1-bis(t-butylperoxy)-2-methylcyclohexane, and 1,1-bis(t-hexyl 2,2-bis(4,4-di(t-butylperoxy)cyclohexyl)propane, 2,5-dimethylhexane-2,5-dihydroperoxide, di-t-butylperoxyisophthalate, t-butylperoxybenzoate, t-butylperoxyacetate, 2,2-bis(t-butylperoxy)butane, 2,2-bis(t-butylperoxy)octane, 2,5-dimethyl-2 Examples of peroxides include 5-di(benzoylperoxy)hexane, bis(t-butylperoxy)isophthalate, isobutyryl peroxide, di(trimethylsilyl)peroxide, trimethylsilyltriphenylsilyl peroxide, etc., 2-hydroxy-2-methyl-1-phenyl-propan-1-one, 1-(4-isopropylphenyl)-2-hydroxy-2-methylpropan-1-one, benzoin methyl ether, and methyl-o-benzoylbenzoate.

[0043] The content of the radical reaction initiator in the reactive modifier for thermosetting resins is preferably 0.01 to 5% by weight, more preferably 0.2 to 2% by weight, based on the weight of copolymer (A) from the viewpoint of the thermosetting property of the reactive groups in (A).

[0044] The reactive modifier for thermosetting resins of the present invention may further contain additives such as a solvent, an antioxidant, etc. From the viewpoint of ease of mixing with the thermosetting resin (X), it is preferable that the reactive modifier for thermosetting resins contains a solvent.

[0045] The solvent is not particularly limited as long as it can dissolve the copolymer (A). The use of an organic solvent improves the handling properties of the reactive modifier for thermosetting resins. Specific examples include, but are not limited to, ketones such as acetone, methyl ethyl ketone, and methyl cellosolve, aromatic hydrocarbons such as toluene and xylene, amides such as dimethylformamide, and propylene glycol methyl ether and its acetate. The solvents can be used alone or in combination of two or more. Of the above organic solvents, aromatic hydrocarbons are preferred.

[0046] Examples of the antioxidant include phenol compounds [monocyclic phenols (2,6-di-t-butyl-p-cresol, etc.), bisphenols [2,2'-methylenebis(4-methyl-6-t-butylphenol), etc.], polycyclic phenols [1,3,5-trimethyl-2,4,6-tris(3,5-di-t-butyl-4-hydroxybenzyl)benzene, etc.], sulfur compounds (dilauryl 3,3'-thiodipropionate, etc.), phosphorus compounds (triphenyl phosphite, etc.), and amine compounds (octylated diphenylamine, etc.).

[0047] From the viewpoint of handleability, the content of the copolymer (A) in the reactive modifier for thermosetting resins is preferably 10 to 90% by weight, more preferably 20 to 80% by weight, based on the weight of the reactive modifier for thermosetting resins. From the viewpoint of handleability, the content of the solvent in the reactive modifier for thermosetting resins is preferably 10 to 90% by weight, and more preferably 20 to 80% by weight, based on the weight of the reactive modifier for thermosetting resins. From the viewpoint of heat resistance of the cured product, the content of the antioxidant in the reactive modifier for thermosetting resins is preferably 0.2 to 10% by weight, and more preferably 0.5 to 5% by weight, based on the weight of the reactive modifier for thermosetting resins.

[0048] The cured product of the reactive modifier for thermosetting resins of the present invention has excellent flexibility and electrical properties, and therefore can impart excellent flexibility and electrical properties to the cured product of a thermosetting resin composition containing the reactive modifier for thermosetting resins and a thermosetting resin.

[0049] <Thermosetting resin composition> The thermosetting resin composition of the present invention contains the reactive modifier for thermosetting resins of the present invention and a thermosetting resin (X). The thermosetting resin (X) is not particularly limited as long as it cures (reacts) with heat to become a high molecular weight resin, and examples of the thermosetting resin include epoxy resins, thermosetting polyimide resins, alcohol-based resins, amide-based resins, ether-based resins, amine-based resins, aromatic resins, oxetane resins, phenolic resins, urea resins, melamine resins, unsaturated polyester resins, silicone resins, polyurethane resins, and diallyl phthalate resins. Among these, from the viewpoint of easily exerting the effect of the reactive modifier for thermosetting resin, epoxy resin, phenol resin, urea resin and melamine resin are preferred, and epoxy resin is more preferred.

[0050] As the epoxy resin, it is preferable to use a polyfunctional epoxy resin having two or more epoxy groups in one molecule. The polyfunctional epoxy resin is a compound containing at least two epoxy groups in the molecule, and examples thereof include bisphenol A type epoxy resin, bisphenol F type epoxy resin, bisphenol S type epoxy resin, hydrogenated bisphenol A type epoxy resin, biphenyl type epoxy resin, phenoxy type epoxy resin, naphthalene type epoxy resin, phenol novolac type epoxy resin, cresol novolac type epoxy resin, trisphenol methane type epoxy resin, dicyclopentadiene type epoxy resin, and amine type epoxy resin. The epoxy resin may be a modified epoxy resin with urethane, rubber, chelate, dimer acid, or the like. As the epoxy resin, a commercially available epoxy resin may be used as it is.

[0051] From the viewpoint of flexibility, the epoxy equivalent of the epoxy resin (mass (g) of a compound containing 1 equivalent of an epoxy group) is preferably 2000 or less, and more preferably 1500 or less. The weight average molecular weight of the epoxy resin is preferably about 150 to 3000, and more preferably about 200 to 2000.

[0052] When the thermosetting resin (X) is an epoxy resin, it may contain a known epoxy resin curing agent, epoxy resin curing accelerator, and the like.

[0053] As the curing agent for the epoxy resin, a polyhydric phenol compound, an amine compound, an acid anhydride, or the like can be used. Specifically, polyhydric phenol compounds {for example, bisphenol A, bisphenol F, bisphenol AD, hydroquinone, resorcin, methylresorcin, biphenol, tetramethylbiphenol, dihydroxynaphthalene, dihydroxydiphenyl ether, thiodiphenols, phenol novolac resins, cresol novolac resins, phenol aralkyl resins, terpene phenol resins, dicyclopentadiene phenol resins, bisphenol A type novolac resins, naphthol novolac resins, biphenyls, terpene phenol resins, dicyclopentadiene phenol resins, bisphenol A type novolac resins, naphthol novolac resins, biphenyls, terpene phenol resins, diphenyl ether ... phenylphenol resins, brominated bisphenol A, brominated phenol novolak resins, and polyhydric phenol resins obtained by condensation reaction of these polyhydric phenol compounds with aldehydes such as benzaldehyde, hydroxybenzaldehyde, crotonaldehyde, glyoxal, etc.}, acid anhydrides {for example, methyltetrahydrophthalic anhydride, hexahydrophthalic anhydride, pyromellitic anhydride, methylnadic acid, etc.}, amine compounds {for example, diethylenetriamine, isophoronediamine, diaminodiphenylmethane, diaminodiphenylsulfone, dicyandiamide, aliphatic polyamines, polyamides, etc.}, and the like.

[0054] Specific examples of epoxy resin curing accelerators (heat curing type) include phosphine compounds such as triphenylphosphine; phosphonium salts such as tetraphenylphosphonium; alcohol amine compounds such as trimethanolamine, triethanolamine, and tetraethanolamine; borate salts such as tetraphenylborate; imidazole, 2-ethylimidazole, 2-ethyl-4-methylimidazole, 2-phenylimidazole, 2-undecylimidazole, 1-benzyl-2-methylimidazole, 2-heptadecylimidazole, 2-isopropylimidazole, 2,4-dimethylimidazole, and 2-phenyl-4-methylimidazole. imidazolines such as 2-methylimidazoline, 2-ethylimidazoline, 2-isopropylimidazoline, 2-phenylimidazoline, 2-undecylimidazoline, 2,4-dimethylimidazoline, and 2-phenyl-4-methylimidazoline; azine-based imidazoles such as 2,4-diamino-6-[2'-methylimidazolyl-(1')]-ethyl-s-triazine, 2,4-diamino-6-[2'-undecylimidazolyl-(1')]-ethyl-s-triazine, and 2,4-diamino-6-[2'-ethyl-4'-methylimidazolyl-(1')]-ethyl-s-triazine; and dicyandiamide.

[0055] Examples of phenolic resins include resins obtained by condensation of phenols such as phenol, cresol, xylenol, t-butylphenol, nonylphenol, cashew oil, lignin, resorcin, and catechol with aldehydes such as formaldehyde, acetaldehyde, and furfural, and examples of such resins include novolac resins and resol resins. Novolac resins are obtained by reacting phenol and formaldehyde in the presence of an acid catalyst such as oxalic acid under conditions of equal amounts or excess phenol. Resole resins are obtained by reacting phenol and formaldehyde in the presence of a base catalyst such as sodium hydroxide, ammonia, or organic amine under conditions of equal amounts or excess formaldehyde. Commercially available resins include the "Sumilite Resin Series" [manufactured by Sumitomo Bakelite Co., Ltd.].

[0056] The urea resin may be a resin obtained by condensation of urea and formaldehyde. Commercially available urea resins include "UA-144" (manufactured by Sunbake Co., Ltd.).

[0057] The melamine resin may be a resin obtained by polycondensation of melamine and formaldehyde. Commercially available examples include the "Nicalac series" (manufactured by Sanwa Chemical Co., Ltd.).

[0058] The thermosetting resin composition of the present invention may further contain a solvent. From the viewpoint of ease of application to a substrate, which will be described later, it is preferable that the thermosetting resin composition contains a solvent, and is dried and cured after application to obtain a cured product. The solvent used in the present invention is not particularly limited as long as it dissolves the reactive modifier for thermosetting resin (copolymer (A)) and the thermosetting resin (X). Specific examples of such solvents include aromatic hydrocarbons such as benzene, toluene, and xylene; aliphatic hydrocarbons such as hexane, heptane, octane, and decane; alicyclic hydrocarbons such as cyclohexane, cyclohexene, methylcyclohexane, and ethylcyclohexane; halogenated hydrocarbons such as trichloroethylene, dichloroethylene, chlorobenzene, and chloroform; alcohol solvents such as methanol, ethanol, isopropyl alcohol, butanol, pentanol, hexanol, propanediol, and phenol; acetone, methyl isobutyl ketone, methyl ethyl ketone, pentanone, hexanone, cyclohexanone, isophorone, and acetophenone. ketone-based solvents, cellosolves such as methyl cellosolve and ethyl cellosolve, ester-based solvents such as methyl acetate, ethyl acetate, butyl acetate, methyl propionate, and butyl formate, and glycol ether-based solvents such as ethylene glycol mono-n-butyl ether, ethylene glycol mono-iso-butyl ether, ethylene glycol mono-tert-butyl ether, diethylene glycol mono-n-butyl ether, diethylene glycol mono-iso-butyl ether, triethylene glycol mono-n-butyl ether, and tetraethylene glycol mono-n-butyl ether, and these can be used alone or in combination of two or more. Of the above solvents, aromatic hydrocarbons are preferred.

[0059] The content of the copolymer (A) in the thermosetting resin composition of the present invention is preferably 2 to 50% by weight, more preferably 5 to 40% by weight, based on the weight of the solid content in the thermosetting resin composition, from the viewpoints of adhesive strength, solder heat resistance, dielectric constant, and flexibility. The content of the thermosetting resin (X) in the thermosetting resin composition of the present invention is preferably 50 to 98% by weight, more preferably 60 to 95% by weight, based on the weight of the solid content in the thermosetting resin composition, from the viewpoints of adhesive strength, solder heat resistance, dielectric constant, and flexibility. In the present invention, the solid content refers to the residue remaining after 1 g of a sample is dried by heating at 120° C. for 2 hours in a circulating air dryer. The weight ratio (A / X) of the copolymer (A) to the thermosetting resin (X) in the thermosetting resin composition of the present invention is preferably 2 / 98 to 50 / 50, more preferably 5 / 95 to 40 / 60, from the viewpoints of adhesive strength, solder heat resistance, dielectric constant, and flexibility. From the viewpoint of handleability, the content of the solvent in the thermosetting resin composition of the present invention is preferably 20 to 80% by weight, and more preferably 30 to 70% by weight, based on the weight of the thermosetting resin composition.

[0060] If necessary, various additives (F) may be further contained in the thermosetting resin composition of the present invention within the range not impairing the effects of the present invention. The additive (F) may be one or more selected from the group consisting of flame retardants (F1), tackifiers (F2), fillers (F3), silane coupling agents (F4), colorants (F5), bulking agents (F6), lubricants (F7), antistatic agents (F8), dispersants (F9), antioxidants (F10), release agents (F11), antibacterial agents (F12), compatibilizers (F13), ultraviolet absorbers (F14) and curing accelerators (F15).

[0061] The thermosetting resin composition of the present invention may contain a flame retardant (F1) as necessary. Examples of the flame retardant include bromine-based, phosphorus-based, nitrogen-based, and metal hydroxide compounds. Among them, phosphorus-based flame retardants are preferred, and known phosphorus-based flame retardants such as phosphoric acid esters, e.g., trimethyl phosphate, triphenyl phosphate, and tricresyl phosphate, phosphates, e.g., aluminum phosphinate, and phosphazenes can be used.

[0062] The thermosetting resin composition of the present invention may contain a tackifier (F2) as needed. Examples of the tackifier include polyterpene resins, rosin resins, aliphatic petroleum resins, alicyclic petroleum resins, copolymer petroleum resins, styrene resins, and hydrogenated petroleum resins.

[0063] The thermosetting resin composition of the present invention may contain a filler (F3) such as silica, if necessary. The incorporation of silica is highly preferable since it improves heat resistance. Generally, hydrophobic silica and hydrophilic silica are known as silica, but in this case, hydrophobic silica treated with dimethyldichlorosilane, hexamethyldisilazane, octylsilane, etc. is better for imparting moisture absorption resistance.

[0064] The thermosetting resin composition of the present invention may contain a silane coupling agent (F4) as necessary. The incorporation of a silane coupling agent is highly preferred because it improves the adhesive strength to metal and heat resistance. The silane coupling agent is not particularly limited, but examples thereof include those having an unsaturated group, those having a glycidyl group, and those having an amino group. Among these, from the viewpoint of heat resistance, silane coupling agents having a glycidyl group are preferred, and more preferred are γ-glycidoxypropyltrimethoxysilane, β-(3,4-epoxycyclohexyl)ethyltrimethoxysilane, and β-(3,4-epoxycyclohexyl)ethyltriethoxysilane.

[0065] The thermosetting resin composition of the present invention may contain a colorant (F5) as needed. Examples of the colorant include inorganic pigments (white pigments, cobalt compounds, iron compounds, sulfides, etc.), organic pigments (azo pigments, polycyclic pigments, etc.), and dyes (azo-based, indigoid-based, sulfide-based, alizarin-based, acridine-based, thiazole-based, nitro-based, aniline-based, etc.).

[0066] The thermosetting resin composition of the present invention may contain a filler (F6) as needed. Examples of the filler include inorganic fillers (calcium carbonate, talc, clay, etc.) and organic fillers (urea, calcium stearate, etc.).

[0067] The thermosetting resin composition of the present invention may contain a lubricant (F7) as needed. Examples of the lubricant include calcium stearate, butyl stearate, oleic acid amide, polyolefin wax, and paraffin wax.

[0068] The thermosetting resin composition of the present invention may contain an antistatic agent (F8) as needed. Examples of the antistatic agent include nonionic, cationic, anionic or amphoteric surfactants as described below and in U.S. Patent Nos. 3,929,678 and 4,331,447. (1) Nonionic surfactants Alkylene oxide (AO) adduct type nonionics, for example, (poly)oxyalkylene derivatives (AO adducts and higher fatty acid mono- or diesters of polyalkylene glycols) of active hydrogen atom-containing compounds having hydrophobic groups (C8-24 or more) [saturated and unsaturated higher alcohols (C8-18), higher aliphatic amines (C8-24) and higher fatty acids (C8-24), etc.]; (poly)oxyalkylene derivatives of higher fatty acid (C8-24) esters of polyhydric alcohols (C3-60) (Tween type nonionics, etc.); (poly)oxyalkylene derivatives of (alkanol)amides of higher fatty acids (above); poly (poly)oxyalkylene derivatives of polyhydric alcohol (above) alkyl (C3-60) ethers; polyoxypropylene polyols [polyoxypropylene derivatives of polyhydric alcohols and polyamines (C2-10) (Pluronic (registered trademark) type and Tetronic type nonionics)]; polyhydric alcohol (above) type nonionics (for example, fatty acid esters of polyhydric alcohols, polyhydric alcohol alkyl (C3-60) ethers and fatty acid alkanolamides); and amine oxide type nonionics [for example, (hydroxy)alkyl (C10-18) di(hydroxy)alkyl (C1-3) amine oxides].

[0069] (2) Cationic surfactants Quaternary ammonium salt type cationics [tetraalkylammonium salts (C11-100), alkyl (C8-18) trimethylammonium salts and dialkyl (C8-18) dimethylammonium salts, etc.]; trialkylbenzylammonium salts (C17-80) (lauryl dimethylbenzylammonium salts, etc.); alkyl (C8-60) pyridinium salts (cetyl pyridinium salts, etc.); (poly)oxyalkylene (C2-4) trialkylammonium salts (C12-100) (polyoxyethylene lauryl dimethylammonium salts, etc.); and acyl (C8-18) aminoalkyl (C2-4) or acyl (C8-18) oxyalkyl (C2-4) tri[(hydroxy)alkyl (C1-4)] ammonium. salts (sapamine-type quaternary ammonium salts) [these salts include, for example, halides (chlorides, bromides, etc.), alkyl sulfates (methosulfates, etc.) and salts of organic acids (C2-22)]; and amine salt-type cationics: inorganic acid (hydrochloric acid, sulfuric acid, nitric acid, phosphoric acid, etc.) salts and organic acid (above) salts of primary to tertiary amines [for example, higher aliphatic amines (C12-60), polyoxyalkylene derivatives (EO [ethylene oxide] adducts, etc.) of aliphatic amines (methylamine, diethylamine, etc.), and acylaminoalkyl or acyloxyalkyl (above) di(hydroxy)alkyl (above) amines (stearoyloxyethyl dihydroxyethylamine, stearamidoethyl diethylamine, etc.)].

[0070] (3) Anionic surfactants Salts of higher fatty acids (mentioned above) (sodium laurate, etc.), ether carboxylic acids [carboxymethylated products of EO (1-10 mol) adducts, etc.] and their salts; sulfate salts (alkyl and alkyl ether sulfates, etc.), sulfated oils, sulfated fatty acid esters, and sulfated olefins; sulfonates [alkylbenzenesulfonates, alkylnaphthalenesulfonates, dialkyl sulfosuccinates, α-olefin (C12-18) sulfonates, N-acyl-N-methyltaurines (Igepone T type, etc.)]; and phosphate salts (alkyl, alkyl ether, and alkylphenyl ether phosphates, etc.).

[0071] (4) Amphoteric surfactants: Carboxylic acid (salt) type amphoterix [amino acid type amphoterix (laurylaminopropionic acid (salt) etc.) and betaine type amphoterix (alkyl dimethyl betaine and alkyl dihydroxyethyl betaine etc.)]; sulfate ester (salt) type amphoterix [laurylamine sulfate ester (salt), hydroxyethyl imidazoline sulfate ester (salt), etc.]; sulfonic acid (salt) type amphoterix [pentadecylsulfotaurine and imidazoline sulfonic acid (salt), etc.]; and phosphate ester (salt) type amphoterix, etc. [glycerol laurate phosphate ester (salt), etc.].

[0072] Salts of the above anionic and amphoteric surfactants include metal salts, such as alkali metal (lithium, sodium, potassium, etc.), alkaline earth metal (calcium, magnesium, etc.) and Group IIB metal (zinc, etc.) salts; ammonium salts; and amine salts and quaternary ammonium salts.

[0073] The thermosetting resin composition of the present invention may contain a dispersant (F9) if necessary. Examples of the dispersant include polymers having Mn of 1,000 to 20,000, such as vinyl resins, and include vinyl resins other than the polyolefin (A) [polyvinyl halides [polyvinyl chloride and polyvinyl bromide, etc.], polyvinyl acetate, polyvinyl alcohol, polymethyl vinyl ether, poly(meth)acrylic acid, poly(meth)acrylic acid esters [polymethyl (meth)acrylate, etc.] and styrene resins [polystyrene, acrylonitrile / styrene (AS) resin, etc.], etc.]; polyester resins [polyethylene terephthalate, etc.], polyamide resins [6,6-nylon and 12-nylon, etc.], polyether resins [polyethersulfone, etc.], polycarbonate resins [polycondensates of bisphenol A and phosgene, etc.] and block copolymers thereof.

[0074] The thermosetting resin composition of the present invention may contain an antioxidant (F10) if necessary. Examples of the antioxidant include phenol compounds (monocyclic phenols (e.g., 2,6-di-t-butyl-p-cresol), bisphenols (e.g., 2,2'-methylenebis(4-methyl-6-t-butylphenol)), polycyclic phenols (e.g., 1,3,5-trimethyl-2,4,6-tris(3,5-di-t-butyl-4-hydroxybenzyl)benzene), sulfur compounds (e.g., dilauryl 3,3'-thiodipropionate), phosphorus compounds (e.g., triphenyl phosphite), and amine compounds (e.g., octylated diphenylamine).

[0075] The thermosetting resin composition of the present invention may contain a release agent (F11) if necessary. Examples of the release agent include lower (C1-4) alcohol esters of fatty acids (C8-24) (butyl stearate, etc.), polyhydric (dihydric to tetrahydric or higher) alcohol esters of fatty acids (C2-24) (hydrogenated castor oil, etc.), glycol (C2-8) esters of fatty acids (C2-24) (ethylene glycol monostearate, etc.), and liquid paraffin.

[0076] The thermosetting resin composition of the present invention may contain an antibacterial agent (F12) if necessary. Examples of the antibacterial agent include benzoic acid, sorbic acid, halogenated phenols, organic iodine, nitriles (e.g., 2,4,5,6-tetrachloroisophthalonitrile), thiocyano (methylenebisthiocyanate), N-haloalkylthioimide, copper agents (e.g., 8-oxyquinoline copper), benzimidazole, benzothiazole, trihaloallyl, triazole, organic nitrogen sulfur compounds (e.g., Slaof 39), quaternary ammonium compounds, and pyridine compounds.

[0077] The thermosetting resin composition of the present invention may contain a compatibilizer (F13) as needed. The compatibilizer may be a compound selected from the group consisting of an amino group, a hydroxyl group, and a polyoxyalkylene group. Modified vinyl polymers having at least one functional group (polar group) selected from the group consisting of: for example, polymers described in JP-A-3-258850, modified vinyl polymers having sulfonic acid groups described in JP-A-6-345927, block polymers having a polyolefin portion and an aromatic vinyl polymer portion, and the like.

[0078] The thermosetting resin composition of the present invention may contain an ultraviolet absorber (F14) as needed. Examples of ultraviolet absorbers include benzotriazoles [2-(2'-hydroxy-5'-methylphenyl)benzotriazole, etc.], benzophenones [2-hydroxy-4-methoxybenzophenone, etc.], salicylates [phenyl salicylate, etc.], and acrylates [2-ethylhexyl-2-cyano-3,3-diphenylacrylate, etc.].

[0079] The thermosetting resin composition of the present invention may contain a curing accelerator (F15) as required. Examples of the curing accelerator include aliphatic polyamines, aromatic polyamines, secondary amines, tertiary amines, acid anhydrides, imidazole derivatives, organic acid hydrazides, dicyandiamide and its derivatives, and urea derivatives.

[0080] The total content of the additives (F) is, for example, preferably 300% by weight or less based on the total weight of the copolymer (A) and the thermosetting resin (X), and from the viewpoint of functional expression of each additive (F) and industrial considerations, is more preferably 0.05 to 250% by weight, and even more preferably 0.1 to 200% by weight. The amount of each additive used based on the total weight of the copolymer (A) and the thermosetting resin (X) is, for example, 200% by weight or less, preferably 10 to 150% by weight; (F2) is, for example, 50% by weight or less, preferably 10 to 40% by weight; (F3) is, for example, 50% by weight or less, preferably 10 to 30% by weight; (F4) is, for example, 30% by weight or less, preferably 10 to 20% by weight; (F5) is, for example, 5% by weight or less, preferably 0.1 to 3% by weight; (F6) is, for example, 5% by weight or less, preferably 0.1 to 1% by weight; (F7) is, for example, 8% by weight or less, preferably 1 to 5% by weight; (F8) is, for example, 8% by weight or less, preferably 1 to 5% by weight; (F9) is, for example, 8% by weight or less, preferably 1 to 3% by weight; (F10) is, for example, 1% by weight or less, preferably 0.1 to 0.5% by weight; (F11) is, for example, 5% by weight or less, preferably 0.01 to 3% by weight; (F12) is, for example, 25% by weight or less, preferably 0.5 to 20% by weight; (F13) is, for example, 15% by weight or less, preferably 0.5 to 10% by weight; (F14) is, for example, 2% by weight or less, preferably 0.05 to 0.5% by weight; and (F15) is, for example, 2% by weight or less, preferably 0.05 to 0.5% by weight.

[0081] When the compounds in (F1) to (F15) overlap, each compound should not be used in the amount necessary to achieve the corresponding additive effect, but should be adjusted according to the purpose of use, taking into consideration that the effects of other additives can also be obtained at the same time.

[0082] The thermosetting resin composition of the present invention is not particularly limited in its production method as long as it is possible to mix the reactive modifier for thermosetting resins of the present invention (the copolymer (A) contained in the reactive modifier for thermosetting resins) and the thermosetting resin (X). For example, the thermosetting resin composition may be obtained by mixing the reactive modifier for thermosetting resins, the thermosetting resin (X), and, if necessary, other additives (F) in a solvent. The mixing temperature is preferably from 10 to 40°C, more preferably from 15 to 30°C, from the viewpoint of pot life. From the viewpoint of solubility, the mixing time is preferably from 20 minutes to 5 hours, and more preferably from 30 minutes to 4 hours.

[0083] The thermosetting resin composition of the present invention is excellent in flexibility and electrical properties, and further excellent in adhesive strength and heat resistance, so that it can be suitably used for electronic material applications. For example, it can be used for aviation and in-vehicle electric control unit (ECU) applications, die attachment agents in power device applications, etc. In addition, it can be used for, for example, adhesives for power overlay packages, adhesives for printed wiring boards, adhesives for each layer of flexible printed wiring boards, copper-clad laminates, adhesives for semiconductor bonding, interlayer insulating films, prepregs, LED sealants, adhesives for structural materials, etc. Among them, it is suitably used for adhesive applications, and is particularly suitably used as an adhesive for each layer of flexible printed wiring boards.

[0084] <Laminate> The thermosetting resin composition of the present invention can be used for various applications, but is preferably used for adhesion, and more preferably for adhesion between a resin substrate and another resin substrate or a metal substrate. The laminate of the present invention is a laminate of a thermosetting resin composition on a substrate (a two-layer laminate of substrate / adhesive layer), or a three-layer laminate of substrate / adhesive layer / substrate). Here, the adhesive layer refers to a layer of the adhesive composition after the thermosetting resin composition of the present invention is applied to a substrate and dried. The laminate of the present invention can be obtained by applying the thermosetting resin composition of the present invention to various substrates and drying it according to a conventional method, and further laminating another substrate.

[0085] <Base material> In the present invention, the substrate is not particularly limited as long as it is possible to apply the thermosetting resin composition of the present invention and dry it to form an adhesive layer. Examples of the substrate include resin substrates such as film-like resins, metal substrates such as metal plates and metal foils, and papers.

[0086] Examples of the resin substrate include polyester resin, polyamide resin, polyimide resin, polyamideimide resin, liquid crystal polymer, polyphenylene sulfide, syndiotactic polystyrene, polyolefin resin, and fluorine resin. A film-like resin (hereinafter also referred to as a substrate film layer) is preferable.

[0087] As the metal substrate, any conventionally known conductive material that can be used for a circuit board can be used. Examples of materials include various metals such as SUS, copper, aluminum, iron, steel, zinc, and nickel, as well as their alloys, plated products, and metals treated with other metals such as zinc and chromium compounds. Metal foil is preferred, and copper foil is more preferred. The thickness of the metal foil is preferably 1 μm or more, more preferably 3 μm or more, and even more preferably 10 μm or more. It is also preferably 50 μm or less, more preferably 30 μm or less, and even more preferably 20 μm or less. If the thickness is too thin, it may be difficult to obtain sufficient electrical performance of the circuit, and on the other hand, if the thickness is too thick, the processing efficiency during circuit production may decrease. The metal foil is provided, for example, in a roll form. The shape of the metal foil used in manufacturing the printed wiring board of the present invention is not particularly limited. When using a ribbon-shaped metal foil, its length is not particularly limited. Its width is also not particularly limited, but is preferably about 250 to 500 cm.

[0088] Examples of the paper include fine paper, craft paper, roll paper, glassine paper, etc. Examples of the composite material include glass epoxy, etc.

[0089] Of the above-mentioned substrates, from the viewpoints of adhesion to the adhesive composition and durability, preferred are polyester resin, polyamide resin, polyimide resin, polyamideimide resin, liquid crystal polymer, polyphenylene sulfide, syndiotactic polystyrene, polyolefin resin, fluorine-based resin, SUS steel plate, copper foil, aluminum foil, and glass epoxy.

[0090] <Adhesive sheet> The adhesive sheet of the present invention is an adhesive sheet having the laminate. That is, the adhesive sheet is obtained by laminating the laminate and a release substrate via a thermosetting resin composition [preferably a cured product of the thermosetting resin composition]. Specific configurations include laminate / adhesive layer / release substrate, or release substrate / adhesive layer / laminate / adhesive layer / release substrate. By laminating the release substrate, it functions as a protective layer for the substrate. In addition, by using a release substrate, the release substrate can be released from the adhesive sheet and the adhesive layer can be transferred to another substrate.

[0091] The adhesive sheet of the present invention can be obtained by applying the thermosetting resin composition of the present invention to various laminates and drying them by a known method. In addition, by attaching a release substrate to the adhesive layer after drying, it is possible to wind the adhesive without causing offset to the substrate, which is excellent in operability, and the adhesive layer is protected, which is excellent in storage stability and easy to use. In addition, if another release substrate is attached as necessary after applying and drying to the release substrate, the adhesive layer itself can be transferred to another substrate.

[0092] <Release base material> Examples of the release substrate include a paper such as fine paper, craft paper, roll paper, or glassine paper, on both sides of which a coating layer of a filler such as clay, polyethylene, or polypropylene is provided, and a silicone-based, fluorine-based, or alkyd-based release agent is further applied on each coating layer. Other examples include various olefin films such as polyethylene, polypropylene, ethylene-α-olefin copolymer, and propylene-α-olefin copolymer alone, and films such as polyethylene terephthalate on which the release agent is applied. Due to the release force between the release substrate and the adhesive layer, and the adverse effect of silicone on electrical properties, it is preferable to use a polypropylene-sealed film on both sides of fine paper and an alkyd-based release agent thereon, or a polyethylene terephthalate film on which an alkyd-based release agent is applied.

[0093] In the present invention, examples of the method for coating the thermosetting resin composition on the substrate include a comma coater and a reverse roll coater. Alternatively, if necessary, the adhesive layer can be provided directly or by a transfer method on the rolled copper foil or polyimide film, which is a printed wiring board constituent material. The thickness of the adhesive layer after drying can be appropriately changed if necessary, but is preferably in the range of 5 to 200 μm. If the adhesive film thickness is less than 5 μm, the adhesive strength is insufficient. If it is 200 μm or more, there is a problem that drying is insufficient, the residual solvent increases, and blisters occur during pressing in the production of printed wiring boards. The drying conditions are not particularly limited, but the residual solvent rate after drying is preferably 1 wt% or less. If it exceeds 1 wt%, the residual solvent tends to foam during pressing of the printed wiring board, causing blisters.

[0094] <Printed wiring board> The "printed wiring board" in the present invention includes, as a component, a laminate formed from a metal foil and a resin substrate that form a conductor circuit. The printed wiring board is manufactured, for example, by a conventionally known method such as a subtractive method using a metal-clad laminate. If necessary, the printed wiring board is a general term for so-called flexible circuit boards (FPCs), flat cables, circuit boards for tape automated bonding (TAB), etc., in which a conductor circuit formed from a metal foil is partially or entirely covered with a cover film, screen printing ink, etc.

[0095] The printed wiring board of the present invention can have any laminated structure that can be used as a printed wiring board. For example, it can be a printed wiring board composed of four layers: a base film layer, a metal foil layer, an adhesive layer, and a cover film layer. It can also be a printed wiring board composed of five layers: a base film layer, an adhesive layer, a metal foil layer, an adhesive layer, and a cover film layer.

[0096] Furthermore, if necessary, two or more of the above printed wiring boards may be laminated.

[0097] The thermosetting resin composition of the present invention can be suitably used for each adhesive layer of a printed wiring board. In particular, when the thermosetting resin composition of the present invention is used as an adhesive, it has high adhesive strength with not only conventional polyimide, polyester film, and copper foil constituting a printed wiring board, but also with low-polarity resin substrates such as LCP, has excellent flexibility, and the adhesive layer itself has excellent low dielectric properties. Therefore, it is suitable as an adhesive composition used for coverlay films, laminates, resin-coated copper foils, and bonding sheets.

[0098] In the printed wiring board of the present invention, any resin film that has been used as a substrate for a printed wiring board can be used as the substrate film. Examples of the resin of the substrate film include polyester resin, polyamide resin, polyimide resin, polyamideimide resin, liquid crystal polymer, polyphenylene sulfide, syndiotactic polystyrene, polyolefin resin, and fluorine resin. In particular, the substrate film has excellent adhesive strength even to low polar substrates such as liquid crystal polymer, polyphenylene sulfide, syndiotactic polystyrene, and polyolefin resin.

[0099] <Cover film> As the cover film, any insulating film that is conventionally known as an insulating film for printed wiring boards can be used. For example, films made of various polymers such as polyimide, polyester, polyphenylene sulfide, polyethersulfone, polyetheretherketone, aramid, polycarbonate, polyarylate, polyimide, polyamideimide, liquid crystal polymer, polyphenylene sulfide, syndiotactic polystyrene, and polyolefin resin can be used. More preferably, it is a polyimide film or a liquid crystal polymer film.

[0100] The printed wiring board of the present invention can be manufactured by any conventionally known process, except for using the materials for each layer described above.

[0101] In a preferred embodiment, a semi-finished product is manufactured by laminating an adhesive layer on a cover film layer (hereinafter referred to as a "cover film side semi-finished product"). On the other hand, a semi-finished product is manufactured by laminating a metal foil layer on a base film layer to form a desired circuit pattern (hereinafter referred to as a "base film side two-layer semi-finished product"), or a semi-finished product is manufactured by laminating an adhesive layer on a base film layer and laminating a metal foil layer thereon to form a desired circuit pattern (hereinafter referred to as a "base film side three-layer semi-finished product") (hereinafter, the base film side two-layer semi-finished product and the base film side three-layer semi-finished product are collectively referred to as a "base film side semi-finished product"). By bonding the cover film side semi-finished product thus obtained and the base film side semi-finished product together, a four-layer or five-layer printed wiring board can be obtained.

[0102] The base film semi-finished product can be obtained, for example, by a manufacturing method including: (1) a step of applying a solution of a resin that will become the base film to the metal foil and initially drying the coating; and (2) a step of heat-treating and drying the laminate of the metal foil and the initially dried coating obtained in (1) (hereinafter referred to as the "heat treatment and desolvation step").

[0103] The formation of the circuit in the metal foil layer can be performed by a conventionally known method. Either an active method or a subtractive method can be used. The subtractive method is preferable.

[0104] The obtained semi-finished product on the base film side may be used as it is for bonding to the semi-finished product on the cover film side, or may be used for bonding to the semi-finished product on the cover film side after a release film has been bonded thereto and stored.

[0105] The cover film side semi-finished product is produced, for example, by applying an adhesive to the cover film. If necessary, a crosslinking reaction in the applied adhesive can be carried out. In a preferred embodiment, the adhesive layer is semi-cured.

[0106] The obtained semi-finished product on the cover film side may be used as it is for bonding to the semi-finished product on the substrate side, or may be used for bonding to the semi-finished product on the substrate film side after a release film has been bonded thereto and stored.

[0107] The substrate film-side semi-finished product and the cover film-side semi-finished product are stored, for example, in the form of a roll, and then laminated together to produce a printed wiring board. Any method can be used as a lamination method, and for example, they can be laminated together using a press or a roll. In addition, they can be laminated together while heating them by a method using a hot press or a hot roll device.

[0108] The semi-finished product on the reinforcing material side is a soft reinforcing material that can be rolled up, such as a polyimide film. In the case of a reinforcing material, it is preferable to manufacture the reinforcing material by applying an adhesive to the reinforcing material. In addition, in the case of a reinforcing plate that is too hard to be wound, such as a metal plate such as SUS or aluminum, or a plate made of glass fiber cured with epoxy resin, it is preferable to manufacture the reinforcing plate by transfer-coating an adhesive that has been applied in advance to a release substrate. In addition, a crosslinking reaction in the applied adhesive can be carried out as necessary. In a preferred embodiment, the adhesive layer is semi-cured.

[0109] The obtained semi-finished product on the reinforcing material side may be used as it is for bonding to the rear surface of a printed wiring board, or may be used for bonding to a semi-finished product on the base film side after a release film has been attached and storage.

[0110] The base film side semi-finished product, the cover film side semi-finished product, and the reinforcing agent side semi-finished product are all laminates for printed wiring boards in the present invention.

[0111] <Cured product> The cured product of the present invention is a cured product obtained by curing the thermosetting resin composition, that is, the cured product can be obtained by, for example, applying and casting the thermosetting resin composition, removing the organic solvent if necessary, and heating (preferably at 90 to 200° C., preferably for 1 minute to 6 hours). The shape of the cured product can be appropriately selected depending on the application, and examples of the shape include a coating film (preferably with a thickness of 5 to 1000 μm) and a cast product.

[0112] The method for preparing the thermosetting resin composition is not particularly limited, and may be a method of mixing the reactive modifier for thermosetting resins, the thermosetting resin (X), and, if necessary, other additives. EXAMPLES

[0113] The present invention will be further described below with reference to examples and comparative examples, but the present invention is not limited to these.

[0114] <Example 1: Production of reactive modifier for thermosetting resin containing copolymer (A-1)> (1) Radical polymerization reaction 87.1 parts of xylene was charged into a glass reaction vessel equipped with a heating / cooling / stirring device, a reflux condenser, a dropping funnel, and a nitrogen inlet tube, and heated to 90° C. A solution in which 50 parts by weight of styrene (a-1), 45 parts by weight of 2-ethylhexyl acrylate (b-1), 5 parts by weight of methacrylic acid (c-1), and 0.4 parts by weight of dodecyl mercaptan were uniformly mixed, and a solution in which 1 part by weight of 2,2-azobis(2-methylbutyronitrile) and 12 parts of xylene were uniformly mixed was dropped into the reaction vessel, and radical polymerization was carried out in the glass reaction vessel to obtain a styrene-acrylic resin solution. (2) Addition reaction To the obtained styrene-acrylic resin solution, 7 parts by weight of glycidyl methacrylate and 3 parts by weight of triethylamine were further added and subjected to an addition reaction (addition reaction of glycidyl group and carboxyl group) for 5 hours at 90° C. Furthermore, the solution was diluted with xylene so that the resin content became 50% by weight, and a 50% by weight xylene solution of copolymer (A-1) having a radical polymerizable group, which is the reactive modifier for thermosetting resin of the present invention, was obtained.

[0115] <Example 2: Production of reactive modifier for thermosetting resin containing copolymer (A-2)> (1) Radical polymerization reaction A styrene-acrylic resin solution was obtained in the same manner as in "(1) Radical polymerization reaction" of Example 1, except that the raw materials shown in Table 1 were used. (2) Addition reaction The obtained styrene-acrylic resin solution was further charged with 12 parts by weight of glycidyl methacrylate and 5 parts by weight of triethylamine, and subjected to addition reaction (addition reaction of glycidyl group and carboxyl group) at 90° C. for 5 hours. Then, 7 parts by weight of 2-isocyanatoethyl acrylate and 0.02 parts by weight of dibutyltin dilaurate were charged, and subjected to urethane reaction at 80° C. for 3 hours. The solution was further diluted with xylene so that the resin content was 50% by weight, to obtain a 50% by weight xylene solution of copolymer (A-2) having a radical polymerizable group, which is a reactive modifier for thermosetting resins of the present invention.

[0116] <Example 3: Production of reactive modifier for thermosetting resin containing copolymer (A-3)> (1) Radical polymerization reaction A styrene-acrylic resin solution was obtained in the same manner as in "(1) Radical polymerization reaction" of Example 1, except that the raw materials shown in Table 1 were used. (2) Addition reaction To the obtained styrene-acrylic resin solution, 6 parts by weight of hydroxybutyl acrylate (d-4) and 0.02 parts by weight of dibutyltin dilaurate were further added, and a urethane reaction was carried out at 80° C. for 3 hours. The solution was then diluted with xylene so that the resin content was 50% by weight, to obtain a 50% by weight xylene solution of copolymer (A-3) having a radical polymerizable group, which is the reactive modifier for thermosetting resins of the present invention.

[0117] <Example 4: Production of reactive modifier for thermosetting resin containing copolymer (A-4)> (1) Radical polymerization reaction A styrene-acrylic resin solution was obtained in the same manner as in "(1) Radical polymerization reaction" of Example 1, except that the raw materials shown in Table 1 were used. (2) Addition reaction To the obtained styrene-acrylic resin solution, 3 parts by weight of 2-isocyanatoethyl acrylate (d-2), 3 parts by weight of 2-isocyanatoethyl methacrylate (d-3), and 0.02 parts by weight of dibutyltin dilaurate were further added, and a urethane reaction was carried out for 3 hours at 80° C. Furthermore, the solution was diluted with xylene so that the resin content became 50% by weight, and a 50% by weight xylene solution of copolymer (A-4) having a radical polymerizable group, which is the reactive modifier for thermosetting resins of the present invention, was obtained.

[0118] <Example 5: Production of reactive modifier for thermosetting resin containing copolymer (A-5)> (1) Radical polymerization reaction A styrene-acrylic resin solution was obtained in the same manner as in "(1) Radical polymerization reaction" of Example 1, except that the raw materials shown in Table 1 were used. (2) Addition reaction The obtained styrene-acrylic resin solution was subjected to an addition reaction in the same manner as in Example 1, except that the raw materials shown in Table 1 were used, and the mixture was diluted with xylene so that the resin content was 50% by weight, thereby obtaining a 50% by weight xylene solution of copolymer (A-5) having a radical polymerizable group, which is a reactive modifier for thermosetting resins of the present invention.

[0119] <Example 6: Production of reactive modifier for thermosetting resin containing copolymer (A-6)> (1) Radical polymerization reaction A styrene-acrylic resin solution was obtained in the same manner as in "(1) Radical polymerization reaction" of Example 1, except that the raw materials shown in Table 1 were used. (2) Addition reaction The obtained styrene-acrylic resin solution was subjected to an addition reaction in the same manner as in Example 1, except that the raw materials shown in Table 1 were used, and the mixture was diluted with xylene so that the resin content was 50% by weight, thereby obtaining a 50% by weight xylene solution of copolymer (A-6) having a radical polymerizable group, which is a reactive modifier for thermosetting resins of the present invention.

[0120] <Example 7: Production of reactive modifier for thermosetting resin containing copolymer (A-7)> (1) Radical polymerization reaction A styrene-acrylic resin solution was obtained in the same manner as in "(1) Radical polymerization reaction" of Example 1, except that the raw materials shown in Table 1 were used. (2) Addition reaction The obtained styrene-acrylic resin solution was used to carry out a urethane reaction in the same manner as in Example 3, except that the raw materials shown in Table 1 were used, to obtain a 50 wt % xylene solution of copolymer (A-7) having a radical polymerizable group, which is a reactive modifier for thermosetting resins of the present invention.

[0121] <Example 8: Production of reactive modifier for thermosetting resin containing copolymer (A-8)> (1) Radical polymerization reaction A styrene-acrylic resin solution was obtained in the same manner as in "(1) Radical polymerization reaction" of Example 1, except that the raw materials shown in Table 1 were used. (2) Addition reaction The obtained styrene-acrylic resin solution was subjected to an addition reaction in the same manner as in Example 1, except that the raw materials shown in Table 1 were used, and the mixture was diluted with xylene so that the resin content was 50% by weight, thereby obtaining a 50% by weight xylene solution of copolymer (A-8) having a radical polymerizable group, which is a reactive modifier for thermosetting resins of the present invention.

[0122] <Example 9: Production of reactive modifier for thermosetting resin containing copolymer (A-9)> (1) Radical polymerization reaction A styrene-acrylic resin solution was obtained in the same manner as in "(1) Radical polymerization reaction" of Example 1, except that the raw materials shown in Table 1 were used. (2) Addition reaction To the obtained styrene-acrylic resin solution, 8 parts by weight of maleic anhydride (d-7) was further added and reacted at 90°C for 5 hours (single esterification reaction between the acid anhydride group and alcohol).The solution was then diluted with xylene so that the resin content was 50% by weight, to obtain a 50% by weight xylene solution of copolymer (A-9) having a radical polymerizable group, which is the reactive modifier for thermosetting resins of the present invention.

[0123] <Example 10: Production of reactive modifier for thermosetting resin containing copolymer (A-10)> (1) Radical polymerization reaction A styrene-acrylic resin solution was obtained in the same manner as in "(1) Radical polymerization reaction" of Example 1, except that the raw materials shown in Table 1 were used. (2) Addition reaction To the obtained styrene-acrylic resin solution, 5 parts by weight of methacrylic acid (d-6) and 3 parts by weight of triethylamine were further added and subjected to an addition reaction (addition reaction of glycidyl group and carboxyl group) at 90° C. for 5 hours. The solution was further diluted with xylene so that the resin content was 50% by weight, to obtain a 50% by weight xylene solution of copolymer (A-10) having a radical polymerizable group, which is a reactive modifier for thermosetting resins of the present invention.

[0124] <Comparative Example 1: Production of reactive modifier for thermosetting resin containing copolymer (A'-1)> (1) Radical polymerization reaction A styrene-acrylic resin solution was obtained in the same manner as in "(1) Radical polymerization reaction" of Example 1, except that the raw materials shown in Table 1 were used. (2) Addition reaction The obtained styrene-acrylic resin solution was subjected to an addition reaction in the same manner as in Example 1, except that the raw materials shown in Table 1 were used, and then diluted with xylene so that the resin content was 50% by weight, to obtain a 50% by weight xylene solution of copolymer (A'-1) having a radical polymerizable group, which is a comparative reactive modifier for thermosetting resins.

[0125] <Comparative Example 2: Production of reactive modifier for thermosetting resin containing copolymer (A'-2)> (1) Radical polymerization reaction A styrene-acrylic resin solution was obtained in the same manner as in "(1) Radical polymerization reaction" of Example 1, except that the raw materials shown in Table 1 were used. (2) Addition reaction The obtained styrene-acrylic resin solution was subjected to an addition reaction in the same manner as in Example 1, except that the raw materials shown in Table 1 were used, and the mixture was diluted with xylene so that the resin content was 50% by weight, thereby obtaining a 50% by weight xylene solution of copolymer (A'-2) having a radical polymerizable group, which is a comparative reactive modifier for thermosetting resins.

[0126] <Comparative Example 3: Production of reactive modifier for thermosetting resin containing copolymer (A'-3)> (1) Radical polymerization reaction In the same manner as in "(1) Radical polymerization reaction" of Example 1, except that the raw materials shown in Table 1 were used, a styrene-acrylic resin solution was obtained, and the solution was further diluted with xylene so that the resin content was 50% by weight, to obtain a 50% by weight xylene solution of copolymer (A'-3), which is a comparative reactive modifier for thermosetting resins.

[0127] <Comparative Example 4: Production of reactive modifier for thermosetting resin containing copolymer (A'-4)> (1) Radical polymerization reaction A styrene-acrylic resin solution was obtained in the same manner as in "(1) Radical polymerization reaction" of Example 1, except that the raw materials shown in Table 1 were used. (2) Addition reaction The obtained styrene-acrylic resin solution was subjected to an addition reaction in the same manner as in Example 1, except that the raw materials shown in Table 1 were used, and the mixture was diluted with xylene so that the resin content was 50% by weight, thereby obtaining a 50% by weight xylene solution of copolymer (A'-4) having a radical polymerizable group, which is a comparative reactive modifier for thermosetting resins.

[0128] <Comparative Example 5: Production of reactive modifier for thermosetting resin containing copolymer (A'-5)> (1) Radical polymerization reaction A styrene-acrylic resin solution was obtained in the same manner as in "(1) Radical polymerization reaction" of Example 1, except that the raw materials shown in Table 1 were used. (2) Addition reaction The obtained styrene-acrylic resin solution was subjected to an addition reaction in the same manner as in Example 1, except that the raw materials shown in Table 1 were used, and then diluted with xylene so that the resin content was 50% by weight, to obtain a 50% by weight xylene solution of copolymer (A'-5) having a radical polymerizable group, which is a comparative reactive modifier for thermosetting resins.

[0129] [Table 1]

[0130] The raw materials used in Examples 1 to 10 and Comparative Examples 1 to 5, and the SP values, radical polymerizable group concentrations, dielectric constants, glass transition points, hydroxyl values, acid values, and Mw of the resulting copolymers (A-1) to (A-10) and (A'-1) to (A'-5) are summarized in Table 1.

[0131] (a-1): Styrene [Tokyo Chemical Industry Co., Ltd.] (a-2): Benzyl acrylate [Tokyo Chemical Industry Co., Ltd.] (a-3): Phenoxyethyl acrylate [Tokyo Chemical Industry Co., Ltd.] (a-4): m-phenoxybenzyl acrylate [Light Acrylate POB-A, manufactured by Kyoeisha Chemical Co., Ltd.] (a-5): Ethoxylated o-phenylphenol acrylate [NK Ester A-LEN-10, manufactured by Shin-Nakamura Chemical Co., Ltd.] (b-1): 2-ethylhexyl acrylate [Tokyo Chemical Industry Co., Ltd.] (b-2): Nonyl acrylate [Viscoat #197, manufactured by Osaka Organic Chemical Industry Co., Ltd.] (b-3): Isodecyl acrylate [IDAA, manufactured by Osaka Organic Chemical Industry Co., Ltd.] (b-4): Lauryl acrylate [LA, manufactured by Osaka Organic Chemical Industry Co., Ltd.] (b-5): Isostearyl acrylate [ISTA, manufactured by Osaka Organic Chemical Industry Co., Ltd.] (b-6): Behenyl acrylate [Blenmer VA, NOF Corporation] (b-7): Cyclohexyl acrylate [Viscoat #155, manufactured by Osaka Organic Chemical Industry Co., Ltd.] (b-8): t-Butylcyclohexyl acrylate [Tokyo Chemical Industry Co., Ltd.] (b-9): Trimethylcyclohexyl acrylate [Viscoat #196, manufactured by Osaka Organic Chemical Industry Co., Ltd.] (c-1): Methacrylic acid [MAA, manufactured by Mitsubishi Chemical] (c-2): 2-isocyanatoethyl acrylate [AOI-VM, Showa Denko K.K.] (c-3): Hydroxyethyl acrylate [HEA, manufactured by Osaka Organic Chemical Industry Co., Ltd.] (c-4): Hydroxybutyl acrylate [HBA, manufactured by Osaka Organic Chemical Industry Co., Ltd.] (c-5): Glycidyl methacrylate [Tokyo Chemical Industry Co., Ltd.] (d-1) Glycidyl methacrylate [Tokyo Chemical Industry Co., Ltd.] (d-2) 2-Isocyanatoethyl acrylate [AOI-VM, Showa Denko K.K.] (d-3) 2-isocyanatoethyl methacrylate [Kalends AOI, Showa Denko K.K.] (d-4) 4-Hydroxybutyl acrylate [HBA, manufactured by Osaka Organic Chemical Industry Co., Ltd.] (d-5) 2-Hydroxyethyl vinyl ether [Maruzen Petrochemical Co., Ltd.] (d-6) Methacrylic acid [MAA, manufactured by Mitsubishi Chemical Corporation] (d-7) Maleic anhydride [Mitsubishi Chemical Corporation]

[0132] <Example 11> 30 parts by weight of the reactive modifier for thermosetting resins obtained in Example 1 {50% by weight solution of (A-1) in xylene}, 25 parts by weight of epoxy resin (X-1), 2.5 parts by weight of diaminodiphenylmethane (product name "Sumicure M", manufactured by Sumitomo Chemical Co., Ltd.) (Y-1) as a curing agent, and 1 part by weight of dicumyl peroxide (containing approximately 60% by weight of calcium carbonate) (Y-2) were added to 25 parts by weight of xylene, and the mixture was stirred at 25°C for 1 hour to completely dissolve, thereby obtaining a thermosetting resin composition (Z-1).

[0133] <Examples 12 to 29 and Comparative Examples 6 to 10> Thermosetting resin compositions (Z-2) to (Z-19) and (Z'-1) to (Z'-5) were obtained in the same manner as in Example 11, except for those shown in Table 2. The adhesive strength, solder heat resistance, electrical properties (dielectric constant: frequency 1 MHz) and flexibility of each of the obtained thermosetting resin compositions were evaluated, and the results are shown in Table 2.

[0134] (1) Adhesive strength (peel strength) Each thermosetting resin composition was applied to a 25 μm thick polyimide film [Apical, manufactured by Kaneka Corporation] so that the thickness after drying would be 25 μm, and then dried at 130° C. for 3 minutes. The adhesive film (B stage product) thus obtained was laminated to 18 μm rolled copper foil. The lamination was performed at 160° C. and 40 kgf / cm with the shiny side of the rolled copper foil in contact with the adhesive. 2 The pieces were pressed for 30 seconds under a pressure of 1000 psi to bond them together. The film was then heat treated at 140°C for 4 hours to harden it, and a sample for evaluating peel strength was obtained. The peel strength was measured by a 90° peel test at 25°C, with the film pulled at a tensile speed of 50mm / min. This test indicates the adhesive strength at room temperature.

[0135] <Evaluation criteria> ◎:1.5N / mm or more ○: 1.0N / mm or more and less than 1.5N / mm ×: Less than 1.0N / mm

[0136] (2) Solder heat resistance (heat resistance) Samples were prepared in the same manner as the samples for peel strength evaluation above (1), and 2.5 cm x 2.5 cm sample pieces were flowed for 1 minute in molten solder baths at various temperatures (265°C, 270°C, 275°C, 280°C, 285°C, 290°C, 295°C, 300°C, 305°C), and the temperatures at which no appearance changes such as swelling occurred were measured.

[0137] <Evaluation criteria> ◎: 300℃ or higher ○: 290℃ or higher and less than 300℃ △: 270℃ or higher but less than 290℃ ×: Less than 270℃

[0138] (3) Dielectric constant (ε) [Electrical property] Each thermosetting resin composition was applied to a release film having a thickness of 50 μm so as to give a dried thickness of 30 μm, and then dried at 130° C. for 3 minutes. The film was then cured by heat treatment at 140°C for 4 hours, and then peeled off from the release film for measurement. Measurements were performed using a PRECISION LCR meter HP-4284A under conditions of 22°C, 58% RH, and a frequency of 1 MHz, and the results were evaluated as follows.

[0139] <Evaluation criteria for dielectric constant> ◎: 3.3 or less ○: More than 3.3 and 3.4 or less △: More than 3.4 and 3.6 or less ×:Over 3.6

[0140] (4) Flexibility (seam bending test (evaluation of flexibility)) The crack bending test was performed by bending the specimen at a radius of 15 mm. A sample was prepared in the same manner as the sample for evaluating peel strength in (1) above, and a sample having a length of 200 mm and a width of 50 mm was prepared. The sample was then folded in half, with a spacer 30 mm thick and 100 mm long sandwiched between the center of the long side, and pressed down from above and below with stainless steel mirror plates weighing 200 g to form a bent section with a radius of 15 mm. After five minutes, the evaluation board was returned to its original position, and the presence or absence of folds or cracks in the bent section was visually confirmed, and the number of times it could be bent without cracks appearing was evaluated. Three samples were prepared, and the same evaluation was carried out for each sample, and the evaluation results were expressed as an average value. The evaluation criteria are as follows: ◎: 3 times or more. Extremely good. ○: 2 or more times, but less than 3 times. Good. △: 1 or more times but less than 2 times. No problem in practical use. ×: Less than once. Not practical.

[0141] [Table 2]

[0142] In Table 2, the raw materials are as follows: (X-1): o-cresol novolac type epoxy resin [YDCN-700-10, manufactured by Nippon Steel & Sumikin Chemical Co., Ltd.] (X-2): Bisphenol A type epoxy resin [JER-828, manufactured by Mitsubishi Chemical Corporation] (X-3): Dicyclopentadiene type epoxy resin [HP-7200, manufactured by DIC Corporation] (Y-1): Diaminodiphenylmethane (product name "Sumicure M", manufactured by Sumitomo Chemical Co., Ltd.) (Y-2): Dicumyl peroxide (containing approximately 60% by weight of calcium carbonate)

[0143] From the results in Table 2, it can be seen that the thermosetting resin composition containing the reactive modifier for thermosetting resins of the present invention has excellent adhesive strength, heat resistance, electrical properties, and flexibility of the cured product compared to the comparative compositions. In particular, when comparing Comparative Example 6, which contains a copolymer (A'-1) in which the weight ratio of the monomer (a) is outside the lower limit range as a reactive modifier for thermosetting resin, with Example 16, which is the same except that the weight ratio of the monomer (a) is within the lower limit range, it is found that Comparative Example 6 has extremely poor adhesive strength and heat resistance. Also, when comparing Comparative Example 7, which contains a copolymer (A'-2) in which the weight ratio of the monomer (b) is outside the lower limit range, with Example 15, which is the same except that the weight ratio of the monomer (b) is within the lower limit range, it is found that the dielectric constant is extremely poor. Also, Comparative Example 8, which contains a copolymer (A'-3) that does not have a radical polymerizable group, is found to have extremely poor heat resistance. Also, Comparative Example 9, which contains a copolymer (A'-4) in which the weight average molecular weight is outside the lower limit range as a reactive modifier for thermosetting resin, is found to have extremely poor heat resistance, dielectric constant and flexibility compared to Example 11, which is the same except that. In addition, Comparative Example 10, in which the weight average molecular weight of the copolymer (A'-5) contained as the reactive modifier for thermosetting resin is outside the upper limit range, shows extremely poor adhesion compared to Example 11, which is otherwise identical. [Industrial Applicability]

[0144] The cured product of the thermosetting resin composition of the present invention has excellent flexibility and electrical properties (low dielectric constant), and also has excellent adhesive strength and heat resistance, so it can be used for various applications, for example, it can be used for electronic materials applications, and can be used as a die attachment agent in aviation and in-vehicle electric control units (ECUs) and power device applications. It can also be used preferably for adhesion, more preferably for adhesion between a resin substrate and a resin substrate or a metal substrate, and can also be used as an adhesive for power overlay packages, an adhesive for printed wiring boards, an adhesive for each layer of a flexible printed wiring board, a copper-clad laminate, an adhesive for semiconductor bonding, an interlayer insulating film, a prepreg, an encapsulant for LEDs, an adhesive for structural materials, etc. Among them, it can be particularly preferably used as an adhesive for each layer of a flexible printed wiring board.

Claims

1. A reactive modifier for thermosetting resins, comprising a copolymer (A) having as essential constituent units a constituent unit derived from a monofunctional radically polymerizable monomer (a) having an aromatic group, a constituent unit derived from a monofunctional radically polymerizable monomer (b) having no aromatic group and having a saturated aliphatic group, and a constituent unit (e) having a radically polymerizable group, wherein the thermosetting resin is an epoxy resin, the saturated aliphatic group of the monomer (b) has 6 to 22 carbon atoms, and the solubility parameter of the monomer (b) is 8.0 (cal / cm 3 ) 1/2 More than 9.5 (cal / cm 3 ) 1/2 a concentration of radically polymerizable groups in said copolymer (A) being 0.2 to 1.2 mol / kg or less; a weight average molecular weight of said copolymer (A) being 3,000 to 70,000; a weight ratio of structural units derived from said monomer (a) being 10 to 80% by weight, a weight ratio of structural units derived from said monomer (b) being 10 to 80% by weight, and a weight ratio of structural units (e) being 2 to 30% by weight, based on the weight of all structural units constituting said copolymer (A).

2. The reactive modifier for thermosetting resins according to claim 1, wherein the radical polymerizable monomer (a) comprises at least one selected from the group consisting of styrene, benzyl (meth)acrylate, phenoxyethyl (meth)acrylate and m-phenoxybenzyl (meth)acrylate.

3. The reactive modifier for thermosetting resins according to claim 1 or 2, wherein the monofunctional (meth)acrylate (b) comprises at least one selected from the group consisting of 2-ethylhexyl (meth)acrylate, n-nonyl (meth)acrylate, isodecyl (meth)acrylate, lauryl (meth)acrylate, isostearyl (meth)acrylate, behenyl (meth)acrylate, cyclohexyl (meth)acrylate, t-butylcyclohexyl (meth)acrylate, and trimethylcyclohexyl (meth)acrylate.

4. 4. The reactive modifier for thermosetting resins according to claim 1, wherein the copolymer (A) has a dielectric constant of 3.5 or less, measured at 25° C. and 1 MHz.

5. The reactive modifier for thermosetting resins according to any one of claims 1 to 4, wherein the copolymer (A) has a glass transition point of -30 to 80°C.

6. The solubility parameter of the copolymer (A) is 8.7 to 9.7 (cal / cm 3 ) 1/2 The reactive modifier for thermosetting resins according to any one of claims 1 to 5,

7. A thermosetting resin composition comprising the reactive modifier for thermosetting resins according to any one of claims 1 to 6 and a thermosetting resin (X).

8. The thermosetting resin composition according to claim 7, which is used as an adhesive.

9. A laminate comprising a resin substrate and a resin substrate or a metal substrate bonded together with the thermosetting resin composition according to claim 7 or 8.

10. An adhesive sheet comprising the laminate according to claim 9 .

11. A printed wiring board comprising the adhesive sheet according to claim 10 as a component.

12. A cured product obtained by curing the thermosetting resin composition according to claim 7 or 8.

Citation Information

Patent Citations

  • Polyimide and polyamic acid

    JP2009299040A

  • Curable resin composition

    JP2012046733A

  • Substrate for high-frequency circuit

    JP2014045076A

  • Curable resin composition and use thereof

    JP2015067699A

  • Thermosetting adhesive resin composition, adhesive film, coverlay film, metal-clad laminate, and flexible printed wiring board

    JP2016188303A