Manufacturing method of carbon fiber reinforced resin composite

The carbon fiber reinforced resin composite addresses weight and noise issues through a non-woven prepreg and controlled manufacturing process, resulting in a lightweight and easily processable material for diverse applications.

JP7553391B2Active Publication Date: 2024-09-18MITSUBISHI PAPER MILLS LTD
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
JP2021052977
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2021-03-26
Publication Date
2024-09-18
Estimated Expiration
2041-03-26

AI Technical Summary

Technical Problem

Existing carbon fiber reinforced resin composites face challenges such as high weight, noise generation, and difficulty in processing due to high mechanical strength, making them unsuitable for certain applications.

Method used

A carbon fiber reinforced resin composite is developed using a non-woven prepreg containing discontinuous short carbon fibers and thermoplastic resin fibers, with a specific carbon fiber blend ratio, density, and manufacturing process that includes heating and cooling under controlled conditions to enhance adhesion and reduce noise.

Benefits of technology

The composite achieves lightweight properties, suppresses unpleasant noise, and is easier to process, making it suitable for various industrial applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007553391000001
    Figure 0007553391000001
  • Figure 0007553391000002
    Figure 0007553391000002
Patent Text Reader

Abstract

To provide a carbon fiber-reinforced resin complex that is light in weight, allows reduction in discomfort noise, and is also easy to process.SOLUTION: A carbon fiber-reinforced resin complex contains carbon fiber and thermoplastic resin fiber. The thermoplastic resin fiber is at least partially melted and fixed to the carbon fiber. The blending ratio of the carbon fiber is 25-75 mass%. The density is 0.35-0.8 g / cm3. The fragile permeability is 1.0 cm3 / cm2 s or more. The flexural modulus is 6 GPa or more. There is also provided a method for producing the carbon fiber-reinforced resin complex.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a carbon fiber reinforced resin composite and a method for producing the same. [Background technology]

[0002] Carbon fiber reinforced plastic (CFRP), which is made by compounding carbon fiber with a matrix resin, has strength and elastic modulus comparable to metal materials, but has a smaller specific gravity than metal materials, allowing for lighter components. In addition, it does not rust and is resistant to acids and alkalis. As a result, its use is expanding in electronic equipment materials, electrical equipment materials, civil engineering materials, building materials, automobile materials, aircraft materials, and in manufactured parts such as robots and rolls used in various manufacturing industries.

[0003] The most common carbon fiber reinforced resin composites are composites made by laminating and integrating prepregs made from long fiber woven fabrics, spread fabrics, or unidirectional (UD) sheets made of continuous carbon fibers with thermosetting resins. However, there are issues with these composites, such as the difficulty of designing the lamination to express mechanical properties, the fact that they are not homogeneous materials, the long molding processing time, and the high cost.

[0004] As a method for solving these problems, a carbon fiber reinforced resin composite made of a nonwoven prepreg containing discontinuous short carbon fibers and thermoplastic resin fibers has been proposed (see, for example, Patent Documents 1 to 3). The use of carbon fiber nonwoven fabric and thermoplastic resin makes it easier to design, allows long-term storage, and shortens the molding processing time. In addition, discontinuous carbon fibers recycled from leftover materials (residual yarn, fabric, etc.) generated from the manufacturing process, scraps of prepregs and carbon fiber reinforced resin composites, and retired waste materials can be used as inexpensive materials.

[0005] There are three methods for manufacturing nonwoven prepregs: wet manufacturing, dry pulp manufacturing, and dry manufacturing (carding). In the carding method, short fibers are combed and the fibers tend to be oriented in the longitudinal direction. There are methods that use a card web with oriented fibers as it is, methods that use a cross wrapper to fold the card web alternately in the width direction and then entangle the fibers by needle punching, and methods that melt a thermoplastic resin by heat treatment.

[0006] Carbon fiber reinforced resin composites made of these nonwoven fabric prepregs have improved mechanical properties by minimizing voids and gaps within the composite and increasing adhesion between the carbon fiber and resin through high density, with the aim of making them a substitute for metal materials.

[0007] However, this method makes it difficult to achieve further weight reduction. In addition, the high-pitched sound generated when a carbon fiber reinforced resin composite is struck becomes unpleasant in the structure using the carbon fiber reinforced resin composite or in the vicinity of the site where the composite is used, and it is necessary to use a separate soundproofing material or the like. In the case of replacing a material other than metal materials, for example a glass fiber reinforced resin composite, the mechanical strength may be excessive, and the carbon fiber reinforced resin composite has a high strength, so there remains a problem that it is hard and difficult to process, such as cutting. [Prior art documents] [Patent documents]

[0008] [Patent Document 1] Special Publication No. 2013-519546 [Patent Document 2] Patent No. 5309563 [Patent Document 3] International Publication No. 2014 / 021366 Brochure Summary of the Invention [Problem to be solved by the invention]

[0009] An object of the present invention is to provide a carbon fiber reinforced resin composite that is lightweight, capable of suppressing unpleasant noise, and is easy to process. [Means for solving the problem]

[0010] As a result of intensive research into solving the above problems, the following carbon fiber reinforced resin composite and manufacturing method were invented.

[0011] That is, the present invention comprises the following: (1) A composite material comprising carbon fibers and thermoplastic resin fibers, at least a part of the thermoplastic resin fibers being melt-bonded to the carbon fibers, the carbon fiber blending ratio being 25 to 75 mass%, and the density being 0.35 to 0.8 g / cm 3 and the Fragile air permeability is 1.0 cm 3 / cm 2 s or more, and a flexural modulus of elasticity of 6 GPa or more.

[0012] (2) The method for producing a carbon fiber reinforced resin composite according to (1) above, further comprising a molding step of heating a nonwoven prepreg containing carbon fibers and thermoplastic resin fibers at a temperature exceeding the melting point of the thermoplastic resin fibers under pressure or without pressure to melt at least a portion of the thermoplastic resin constituting the thermoplastic resin fibers, and then cooling the prepreg under pressure to solidify the thermoplastic resin, wherein the cooling start temperature in the molding step is a temperature equal to or higher than the glass transition temperature of the thermoplastic resin. Effect of the Invention

[0013] According to the present invention, it is possible to provide a carbon fiber reinforced resin composite that is lightweight, capable of suppressing unpleasant noise, and is easy to process. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0014] Carbon fibers are industrialized in various types, such as PAN (polyacrylonitrile), pitch (isotropic pitch, anisotropic pitch), phenol, and rayon, depending on the type of precursor fiber. The carbon fiber used in the present invention can be selected according to the intended use. In order to develop the mechanical properties of the carbon fiber reinforced resin composite, it is preferable to use a medium elasticity type carbon fiber with a tensile modulus of 200 GPa or more.

[0015] It is also possible to use recycled carbon fibers obtained by using prepreg and CFRP process scraps, defective parts, and retired waste materials generated during the CFRP manufacturing process as raw materials and removing the matrix resin (thermosetting resin or thermoplastic resin) using regeneration processing methods such as atmospheric pressure dissolution, subcritical decomposition, supercritical decomposition, electrolysis, thermal decomposition, and superheated steam method.

[0016] CFRP is lightweight and has high specific strength and specific rigidity, so it is used for golf shafts, tennis rackets, fishing rods, etc. Recently, it has also been used for the main structural components of large aircraft such as wings and fuselages, and the market size is expanding. Along with this market size expansion, the amount of CFRP discarded during the manufacturing process is also increasing. For example, in the case of aircraft, safety is very important, so the quality standards are particularly strict, and the yield rate of CFRP is said to be 50 to 60%. That is, there are many parts that are discarded due to trimming. In addition, prepregs cut to fit a mold, and prepregs in an expired uncured state, semi-cured state, or cured state are also types of discarded CFRP, and are similarly discarded in large quantities. In such a situation, it is preferable to actively use recycled carbon fibers from the viewpoint of reducing the environmental load. In addition, the carbon fibers recycled from the materials provided for recycling are in a discontinuous state, and are also suitable for use as nonwoven fabrics.

[0017] In the present invention, it is preferable to use a nonwoven fabric prepreg to manufacture a carbon fiber reinforced resin composite, and by using a low-density, high-area weight nonwoven fabric, the number of laminated nonwoven fabric prepregs can be reduced, making it easier to adjust the density of the carbon fiber reinforced resin composite. As a method for obtaining a low-density, high-area weight nonwoven fabric, a method is preferred in which a card web is produced by a dry method (card method), laminated by cross-wrapping, and then a very low-density, felt-like nonwoven fabric prepreg in which the fibers are entangled by a needle punch method is used.

[0018] The fiber diameter of the carbon fibers usable in the present invention is preferably 5 to 20 μm, and more preferably 5 to 15 μm. If the fiber diameter of the carbon fibers is smaller than 5 μm, the fiber opening becomes extremely insufficient, and the fibers may remain in the carding device, and a carded web may not be obtained stably. If the fiber diameter is larger than 20 μm, the carded web may have large unevenness in basis weight. Furthermore, the fiber length of the carbon fibers is preferably 25 to 100 mm, and more preferably 25 to 75 mm. If the fiber length of the carbon fibers is shorter than 25 mm, the fibers may easily fall off the carding device, and a carded web may not be obtained stably. If the fiber length is longer than 100 mm, the fibers may easily remain in the carding device, and neps may occur frequently.

[0019] Examples of the thermoplastic resin of the thermoplastic resin fiber include polyolefin resins such as polyethylene and polypropylene; styrene-based resins such as polystyrene, rubber-reinforced polystyrene, acrylonitrile-styrene copolymer, and ABS resin (acrylonitrile-butadiene-styrene copolymer synthetic resin); polyester resins such as polyethylene terephthalate and polybutylene terephthalate; polyamide resins such as nylon 6, nylon 66, and nylon 46; polyether-based resins such as polyphenylene ether and modified polyphenylene ether; engineering resins such as polycarbonate resin, polyarylate, polyphenylene sulfide, polysulfone, polyether sulfone, polyether ketone, polyether ether ketone, and polyether imide; and thermoplastic epoxy resins. These thermoplastic resins may be used alone or in combination of two or more. Examples of the use of two or more types include blend polymers such as polycarbonate / ABS, polyphenylene ether / polyamide, polycarbonate / polybutylene terephthalate, and polyphenylene ether / polybutylene terephthalate. The thermoplastic resin is not limited to these, and any thermoplastic resin suitable for the steps of the manufacturing method of the present invention may be applicable. From the viewpoint of mechanical properties, polyamide is preferable, from the viewpoint of heat resistance, polyphenylene sulfide, polyetherimide, and polyether ether ketone are preferable, and from the viewpoint of economy, polypropylene is preferable.

[0020] In addition, composite fibers using a plurality of thermoplastic resins are also preferred materials, and polyester-based sheath-core fibers, polyolefin-based sheath-core fibers, undrawn polyester fibers, etc., whose surfaces have been treated to have low melting points, can also be used.

[0021] The fiber diameter of the thermoplastic resin fiber is preferably 3 to 20 μm, and more preferably 5 to 15 μm. If the fiber diameter of the thermoplastic resin fiber is smaller than 3 μm, the fiber may be retained in the carding device, and a stable carded web may not be obtained. If the fiber diameter is larger than 20 μm, the carded web may have large unevenness in basis weight. The fiber length is preferably 25 to 100 mm, and more preferably 25 to 75 mm. If the fiber length of the thermoplastic resin fiber is shorter than 25 mm, the fiber may fall off the carding device, and a stable carded web may not be obtained. If the fiber length is longer than 100 mm, the fiber may be easily retained in the carding device, and many neps may occur.

[0022] In the present invention, the carbon fiber blend ratio is preferably 25 to 75 mass % and more preferably 35 to 60 mass % relative to the nonwoven fabric prepreg. If the carbon fiber blend ratio is less than 25 mass %, the mechanical properties of the carbon fiber reinforced resin composite may be insufficient. If the carbon fiber blend ratio exceeds 75 mass %, the amount of thermoplastic resin relative to the carbon fibers becomes small, and the continuity of the matrix resin between the carbon fibers and the adhesion to the carbon fibers may be insufficient, and the mechanical properties of the carbon fiber reinforced resin composite may be significantly reduced.

[0023] In the present invention, it is possible to mix small amounts of carbon fibers and thermoplastic resin fibers that are outside the above-mentioned preferred ranges of fiber length and fiber diameter, but the content of these fibers must not be in a range that impairs the performance of the carbon fiber reinforced resin composite.

[0024] In the present invention, a sizing agent having a surface modification effect on the thermoplastic resin fiber and the carbon fiber can be sprayed, coated, or impregnated. It is also possible to mix other natural fibers, synthetic fibers, inorganic fibers, etc., but the content of these fibers must not be in a range that inhibits the performance of the carbon fiber reinforced resin composite.

[0025] The density of the carbon fiber reinforced resin composite of the present invention is 0.35 to 0.8 g / cm 3 and more preferably 0.4 to 0.7 g / cm 30.35g / cm 3 If it is smaller than this, the mechanical strength will be poor, which is not preferable. 3 If the value is larger, the mechanical strength is increased, but the Frazier air permeability is decreased. As a result, when the carbon fiber reinforced resin composite is struck, an unpleasant high-pitched sound such as "clang clang" is generated. In other words, the Frazier air permeability of the carbon fiber reinforced resin composite of the present invention is 1.0 cm 3 / cm 2 s or more, and more preferably 3.0 cm 3 / cm 2 The upper limit of the Frazier air permeability is not particularly limited, but is preferably 30 cm 3 / cm 2 ·s or less. Fragile air permeability is 1.0 cm 3 / cm 2 If it is less than .s, it is not preferable because it generates unpleasant noise as described above. In the carbon fiber reinforced resin composite of the present invention, the density and Frazier air permeability are controlled and kept at a constant level, thereby making it possible to suppress such unpleasant noise.

[0026] The flexural modulus of the carbon fiber reinforced resin composite of the present invention is 6 GPa or more, and more preferably 7 GPa or more. If the flexural modulus is less than 6 GPa, the mechanical strength is insufficient and the composite is not suitable as a reinforcing material.

[0027] Next, the manufacturing method will be described. The materials are mixed in a blender, and a carded web made of carbon fiber and thermoplastic fiber is produced in a carding machine. The basis weight of the carded web obtained by this method is preferably 10 to 35 g / m 2 Using a cross wrapper, multiple sheets of the obtained web are laminated and needle punched to obtain a web of 100 to 1000 g / m 2 The density of the nonwoven prepreg is preferably 0.0045 to 0.01 g / cm 3 The density of the nonwoven prepreg is 0.01 g / cm 3If the density exceeds 0.0045 g / cm, the carbon fibers may break during needle punching, causing significant dust generation and contaminating the process. In addition, the mechanical strength of the carbon fiber reinforced resin composite may decrease. 3 If it is lower, the mechanical strength of the nonwoven fabric prepreg will be weak, breakage will occur easily, and fiber dropout may occur, which is undesirable.

[0028] The nonwoven fabric-like prepreg obtained by the above method can be laminated in a single layer or in multiple layers, and then heated, pressed, and cooled to form a carbon fiber reinforced resin composite.

[0029] The method for producing a carbon fiber reinforced resin composite of the present invention using the nonwoven fabric prepreg will now be described in detail.

[0030] The method for producing a carbon fiber reinforced resin composite of the present invention includes a molding step of heating a nonwoven fabric prepreg containing carbon fibers and thermoplastic resin fibers at a temperature exceeding the melting point of the thermoplastic resin fibers under pressure or non-pressurization to melt at least a part of the thermoplastic resin constituting the thermoplastic resin fibers, and then cooling under pressure to solidify the thermoplastic resin. The molding step is characterized in that the cooling start temperature in this molding step is a temperature equal to or higher than the glass transition temperature of the thermoplastic resin.

[0031] Examples of heating and cooling methods include a method in which a single layer or multiple layers of nonwoven fabric prepreg are inserted between heated upper and lower molds, heat treated for a certain period of time, and then cooled under the same pressure (heat and cool method), and a method in which after heating and pressurizing, the pressure is temporarily reduced to an unpressurized state, and the prepreg is inserted between upper and lower molds that have been cooled to a temperature lower than the melting point of the thermoplastic resin, and then cooled and pressed (cold press method).

[0032] A carbon fiber reinforced resin composite can be produced by placing a single layer or multiple layers of nonwoven fabric prepreg between the dies of a pressurizing device having a pair of male and female dies having flat or uneven surfaces treated with metal or polytetrafluoroethylene, etc., and adjusting the distance between the dies. In order to achieve the density of the carbon fiber reinforced resin composite of the present invention, a spacer having a certain thickness so as to obtain the desired density can be placed between the dies, and pressure can be applied while maintaining the distance so that the nonwoven fabric prepreg is not crushed too much.

[0033] The pressing device may be a single-stage press, or a multi-stage press equipped with a plurality of press devices.

[0034] The heating temperature is preferably at least 20° C. higher than the melting point of the thermoplastic resin constituting the thermoplastic resin fiber, but not exceeding the decomposition temperature of the thermoplastic resin.

[0035] The method of heating under pressure and then cooling and solidifying while maintaining the pressure is called the heat and cool method, and is preferable because the cooling start temperature in this method is necessarily equal to or higher than the glass transition temperature (Tg) of the thermoplastic resin. For example, when the thermoplastic resin is nylon 6, the Tg is 50°C.

[0036] The method of heating in an unpressurized state and then cooling in a pressurized state is called the cold press method, and in this method, the cooling start temperature is a temperature equal to or higher than the Tg of the thermoplastic resin. If cooling is performed at a temperature lower than the Tg, the cooling and solidification of the molten thermoplastic resin will proceed rapidly on the pressurized surface, and the resin will gather on the surface of the obtained carbon fiber reinforced resin composite to form a film, inhibiting breathability. In addition, the resin will be unevenly distributed in different places, and in places with little resin, the fluff of the carbon fiber will be exposed on the surface, and when the material is rubbed or processed by cutting, the carbon fiber will fall off, which is not preferable.

[0037] The cooling is preferably performed until the thermoplastic resin is solidified and the carbon fiber reinforced resin composite does not deform.

[0038] The pressure during pressing should be 0.1 MPa or more, and should be such that the spacer used does not deform.

[0039] In the present invention, the melting point and Tg are measured by differential scanning calorimetry (DSC) as described in JIS K 7121:1987 "Method for measuring transition temperature of plastics". EXAMPLES

[0040] The present invention will be specifically described below with reference to examples, but the present invention is not limited to these examples. All parts and percentages in the examples and comparative examples are by mass unless otherwise specified. The physical properties of the carbon fiber reinforced resin composites obtained in the examples and comparative examples were measured and evaluated to confirm the effectiveness of the present invention.

[0041] (Examples 1 to 7, Comparative Examples 1 to 4) PAN-based carbon fiber (Toray T-700, fiber diameter 7 μm, fiber length 51 mm) and nylon 6 fiber (Taiwan Kinlong Chemical, fineness 1.5 denier, fiber length 51 mm) were used as thermoplastic resin fiber. After mixing in a blender, they were carded with a roller card machine to produce a 25 g / m2 oriented fiber. 2 After laminating with a cross wrapper, the fibers were entangled by a needle punch method to obtain a carded web with a basis weight of 500 g / m. 2 A nonwoven fabric-like prepreg was obtained.

[0042] Two sheets of the nonwoven fabric prepreg were laminated and heated in an unpressurized state in an atmosphere of 260°C for 3 minutes. A carbon fiber reinforced resin composite was obtained by heating the laminate to 60°C in advance and pressing it at a pressure of 0.5 MPa using a press equipped with spacers to obtain the desired density. The laminate was then cooled for 3 minutes.

[0043] Comparative Example 5 A carbon fiber reinforced resin composite was obtained in the same manner as in Example 1, except that no spacer was used and pressing was performed at a pressure of 8 MPa.

[0044] Comparative Example 6 A glass fiber reinforced resin composite was obtained in the same manner as in Comparative Example 5, except that the PAN-based carbon fiber was replaced with glass fiber (manufactured by Kyoseki Group Co., Ltd., fiber diameter 11 μm, fiber length 50 mm).

[0045] Example 8 A carbon fiber reinforced resin composite was obtained in the same manner as in Example 1, except that the cooling start temperature was 50° C. (Tg of nylon 6).

[0046] Comparative Example 7 A carbon fiber reinforced resin composite was obtained in the same manner as in Example 1, except that the cooling start temperature was 40°C.

[0047] Example 9 A carbon fiber reinforced resin composite was obtained in the same manner as in Example 1, except that the heating and pressurizing method was to heat the material in advance to 260°C, then heat it at 0.5 MPa for 3 minutes, and cool it to 50°C while maintaining the pressurized state.

[0048] Example 10 A carbon fiber reinforced resin composite was obtained in the same manner as in Example 1, except that the number of the nonwoven fabric-like prepregs was one.

[0049] Table 1 shows the fiber blend ratio (mass %), heating temperature, cooling start temperature, and spacer thickness used in the above examples and comparative examples.

[0050] The physical properties of the carbon fiber reinforced resin composites obtained in the above Examples and Comparative Examples were measured and evaluated by the following methods, and the physical properties and evaluation results are shown in Table 2. In the present invention, unless otherwise specified, the physical properties and evaluation were performed under conditions of 25°C and 50% RH.

[0051] <Metsuke> The carbon fiber reinforced resin composite was cut into a size of 20 x 25 cm, and the mass of five pieces was averaged to determine the mass per unit area (weight per unit area). The unit is g / m 2 It is.

[0052] <Thickness> For the carbon fiber reinforced resin composites for which the above-mentioned weight per unit area was measured, the thickness was measured at four points per sheet using a micrometer, and the average value of each of the five sheets was calculated. The unit is mm.

[0053] <density> The density was calculated by dividing the basis weight by the thickness. The unit is g / cm 3 It is.

[0054] <Flexural modulus> The carbon fiber reinforced composite material was evaluated by measuring its flexural modulus by the three-point bending method according to JIS K 7074:1988. The unit is GPa. The flexural modulus of the glass fiber reinforced resin composite of Comparative Example 6 was used as the standard, and the quality was judged according to the following criteria. In addition, ⊚ and ◯ were regarded as "good".

[0055] "Flexural modulus of each Example or Comparative Example - Flexural modulus of Comparative Example 6" 1GPa or higher: ◎ 0GPa or more, less than 1GPa: Yes Less than 0GPa: ×

[0056] <Breathability> The air permeability was evaluated by measuring the Frazier air permeability using an air permeability tester (device name: KES-F8-AP1, manufactured by Kato Tech Co., Ltd.) in accordance with the Air Permeability A Method (Fragile method) specified in JIS L 1096:2010. The unit is cm 3 / cm 2 In addition, ◎ and ○ are categorized as "good".

[0057] Fragile Breathability 3.0cm 3 / cm 2 ·S or more:◎ 1.0cm 3 / cm 2 ·s or more, 3.0cm 3 / cm 2 Less than s:○ 1.0cm 3 / cm 2 Less than s: ×

[0058] <Reflected sound> When the surface of the carbon fiber reinforced resin composite was flicked with the nail of the index finger in the same way as flicking something, those that produced a high-pitched "clang" sound were rated as "X", those that produced a relatively low-pitched "bokoboko" sound were rated as "◎", and those that produced sounds in between were rated as "○". ◎ and ○ were rated as "good".

[0059] <Superficiality> The surface of the carbon fiber reinforced resin composite was visually observed, and was evaluated as follows: ⊚: the carbon fiber and the molten thermoplastic resin fiber were uniformly integrated; ◯: the composite was generally uniform with some unevenness; ×: the composite was mottled in parts. ⊚ and ◯ were rated as good.

[0060] <Workability> The carbon fiber reinforced resin composite was cut into pieces measuring 20 x 25 cm, placed against a ruler, and cut with a cutter knife to evaluate the condition. Those that could be easily cut without applying a lot of force were rated as ◎, those that were easy to cut but had a small amount of fiber falling off from the cut surface were rated as ○, those that had a lot of fiber falling off from the cut surface and had a lot of fuzz when cut were rated as △, and those that needed to be cut multiple times with the cutter knife or could not be cut with the cutter knife were rated as ×. ◎ and ○ were rated as good.

[0061] <Friction resistance> The surface of the carbon fiber reinforced resin composite was rubbed with an index finger and evaluated for the presence or absence of fiber shedding and fuzz. The composite was rated as follows: no shedding of carbon fibers, ◯, carbon fibers with a small amount of shedding but no fuzz on the surface, △, carbon fibers with shedding and fuzz on the surface, and ×, carbon fibers with a lot of shedding and fuzz. ◯ and ◯ were rated as good.

[0062] The results of the above evaluation are shown in Table 2.

[0063] [Table 1]

[0064] [Table 2] [Industrial Applicability]

[0065] The present invention can provide a carbon fiber reinforced resin composite that can be used for electronic device materials, electric device materials, civil engineering materials, building materials, automobile materials, aircraft materials, and manufactured parts such as robots and rolls used in various manufacturing industries. In particular, a carbon fiber reinforced resin composite that can be used as an automobile interior or exterior material, is lightweight, suppresses unpleasant noise, and has excellent processability.

Claims

[Claim 1] A method for producing a carbon fiber reinforced resin composite containing carbon fibers and thermoplastic resin fibers, at least a portion of the thermoplastic resin fibers being melt-bonded to the carbon fibers, the carbon fiber mixing ratio being 25 to 75 mass %, the density being 0.35 to 0.8 g / cm 3 , the Frazier air permeability being 1.0 cm 3 / cm 2 ·s or more, and the flexural modulus being 6 GPa or more, the method comprising a molding step of heating a nonwoven prepreg containing carbon fibers and thermoplastic resin fibers at a temperature above the melting point of the thermoplastic resin fibers under pressure or non-pressurization to melt at least a portion of the thermoplastic resin that constitutes the thermoplastic resin fibers, and then cooling under pressure to solidify the thermoplastic resin, wherein the cooling start temperature in the molding step is a temperature equal to or higher than the glass transition temperature of the thermoplastic resin.

Citation Information

Patent Citations

  • Side edge defect detection and size measurement apparatus of traveling materials

    JP1978009563A

  • Under cover for moving body and its manufacturing method

    JP2006076060A

  • Method for manufacturing sheet-like semi-finished products from fiber composite materials

    JP2013519546A

  • Carbon fiber non-woven fabric and composite

    JP2019157315A

  • Heat-resistant paper and process for producing same, fiber-reinforced heat-resistant molded resin, precursor therefor, and processes for producing said molded resin and precursor

    WO2014021366A1