Dual cure cyanate ester ink jet composition
A dual cure inkjet composition with balanced acryloyl and cyanate ester compounds addresses 3D printing challenges, ensuring stable viscosity and strong, crack-resistant 3D objects with improved mechanical properties and safety.
Patent Information
- Application Number
- JP2023517406
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2021-06-09
- Filing Date
- 2022-05-10
- Publication Date
- 2024-09-18
- Estimated Expiration
- 2042-05-10
AI Technical Summary
Existing 3D printing technologies face challenges with low mechanical properties, such as low heat distortion temperatures, brittleness, and aging, incomplete curing leading to weak interlayer adhesion, uncured resin leakage causing health hazards, and poor mechanical performance.
A dual cure inkjet composition comprising specific ratios of acryloyl groups, cyanate ester compounds, and catalysts, allowing for pre-curing and post-curing to achieve balanced mechanical properties and prevent resin leakage.
The composition ensures stable viscosity for printing, provides strong green bodies that withstand post-curing without cracking, and prevents resin leakage, resulting in high-quality 3D objects with improved mechanical properties.
Smart Images

Figure 0007553701000006 
Figure 0007553701000005 
Figure 0007553701000004
Abstract
Description
[Technical field]
[0001] explanation The present invention relates to an ink jet composition, its use, a method for printing three-dimensional objects, and to a three-dimensional object. [Background technology]
[0002] Three-dimensional (3D) printing, or additive manufacturing, is a process in which a 3D digital model is produced by the additive growth of a build material. 3D printed objects are produced by utilizing computer-aided design (CAD) data of an object in the successive construction of two-dimensional (2D) layers that correspond to cross sections of the 3D object. These layers are printed on top of each other, with the condition that each layer is rapidly cured (e.g. by UV curing) before the next layer is printed accordingly.
[0003] One method of performing said 3D printing is inkjet printing: in inkjet printing, small droplets of ink (with a defined viscosity) are projected directly onto the receiving surface without physical contact between the printing device and the ink receiving side. The printing device electronically stores the printing data and controls a mechanism for imagewise ejection of the droplets. Printing is achieved by moving the print head across the ink receiving side or vice versa, or both.
[0004] Three-dimensional inkjet printing is a relatively fast and flexible printing method for the production of prototype parts, creating and rapidly manufacturing three-dimensional complex structures directly from CAD files. Radiation-curable compositions used in three-dimensional printing methods of complex structures are described, for example, in WO2004 / 096514. However, in general, there are many radiation-curable compositions described in the art that can be used in the field of inkjet printing, such as in US2017 / 173866, WO2019 / 203134, WO2020 / 065654, and WO2020 / 211656. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0005] The challenges faced in said 3D printing are poor mechanical properties, such as low heat distortion temperature, brittleness, and aging, where aging means embrittlement over time and / or under temperature changes and / or humidity. Another challenge is incomplete curing of the (initial) printed 3D object (the so-called "green body"), as well as some quality issues with the final product (e.g. mechanical aspects and / or product aging). If the 3D object is completely cured during the 3D printing process, the interlayer adhesion may be too weak, causing the print to fail.
[0006] However, uncured resin inside the final product is also undesirable: Firstly, leakage of uncured liquid resin ("bleed") from the printed 3D object can cause health problems for the end user, since the liquid resin may contain reactive chemicals. Secondly, the printed 3D object does not reach optimal mechanical performance, since the uncured liquid resin may soften the object. Thirdly, the uncured resin may cause problems in some industrial applications of the object, where high chemical inertness is required. In order to fully cure the printed "green body" object (to avoid the aforementioned drawbacks), a corresponding post-curing of the 3D "green body" is necessary.
[0007] Therefore, a suitable inkjet printing ink must simultaneously combine (satisfy) the following conditions: have a sufficiently low viscosity (to allow printing of small droplets through the inkjet nozzle), provide high viscosity stability (e.g., should not polymerize in the printing device prior to printing), be sufficiently pre-curable (each printed ink layer needs to be pre-cured before the next layer is printed), and be efficiently post-curable (fully curable in a later step to provide the quality characteristics required for the 3D object).
[0008] It is therefore an object of the present invention to provide a high quality ink jet printing ink which meets the above requirements.
[0009] The solution for this purpose is an inkjet composition having 1.0 to 5.0 mol / kg of acryloyl groups, (i) a photopolymerizable reactive compound (M) containing exactly one acryloyl group; (ii) a photopolymerization reactive compound (N) containing at least two acryloyl groups; (iii) a radical photoinitiator (R), (iv) a cyanate ester compound (D) containing at least two cyanate groups, and (v) Cyanate ester curing catalyst (C) Including, (M) is different from (D), except that a cyanate ester compound containing exactly one acryloyl group and further containing at least two cyanate groups is to be included in (D); (N) is different from (D), except that a cyanate ester compound containing at least two acryloyl groups and further containing at least two cyanate groups should be included in (D); The ink-jet composition contains 25 to 50 mol % of the acryloyl groups provided by the reactive compound (N), and the molar ratio of the acryloyl groups to the cyanate groups contained in the compound (D) is 0.30 to 0.95. The present disclosure also includes the following: [Aspect 1] An inkjet composition having 1.0 to 5.0 mol / kg of an acryloyl group, the inkjet composition comprising: (i) a photopolymerizable reactive compound (M) containing exactly one acryloyl group; (ii) a photopolymerization reactive compound (N) containing at least two acryloyl groups; (iii) a radical photoinitiator (R), (iv) a cyanate ester compound (D) containing at least two cyanate groups, and (v) Cyanate ester curing catalyst (C) Including, (M) is different from (D), except that a cyanate ester compound containing exactly one acryloyl group and further containing at least two cyanate groups should be included in (D); The (N) is different from the (D), except that a cyanate ester compound containing at least two acryloyl groups and further containing at least two cyanate groups should be included in the (D); The ink-jet composition, wherein 25 to 50 mol % of the acryloyl groups contained therein are provided by the reactive compound (N), and the molar ratio of the acryloyl groups contained therein to the cyanate groups contained in the compound (D) is 0.30 to 0.95. [Aspect 2] The inkjet composition according to embodiment 1, having 1.7 to 3.5 mol / kg of acryloyl groups. [Aspect 3] The ink-jet composition according to the above-mentioned embodiment 1 or 2, wherein 30 to 45 mol % of the contained acryloyl groups are provided by the reactive compound (N). [Aspect 4] The inkjet composition according to any one of Aspects 1 to 3 above, wherein 80 to 100 mol %, preferably 90 to 100 mol %, of the reactive compound (N) is provided by a species containing three or less acryloyl groups. [Aspect 5] The ink-jet composition according to any one of the above-mentioned embodiments 1 to 4, wherein the molar ratio of the acryloyl group contained in the compound (D) to the cyanate group contained in the compound (D) is 0.36 to 0.94. [Aspect 6] 6. The ink-jet composition according to any one of Aspects 1 to 5, wherein at least 30% by weight of the species of (D), preferably at least 60% by weight of the species of (D) is provided by 4,4'-ethylidene diphenyl dicyanate. [Aspect 7] 7. The ink-jet composition according to any one of Aspects 1 to 6 above, wherein the species of the radical photoinitiator (R) is provided by a phosphine oxide based photoinitiator, preferably by diphenyl(2,4,6-trimethylbenzoyl)phosphine oxide, and / or phenylbis(2,4,6-trimethylbenzoyl)phosphine oxide. [Aspect 8] The ink-jet composition according to any one of the above embodiments 1 to 7, wherein the species of the cyanate ester curing catalyst (C) is provided by an aluminum metal catalyst, preferably by aluminum acetylacetonate. [Aspect 9] The inkjet composition according to any one of Aspects 1 to 8, wherein 90 to 100% by mass, and preferably 97 to 100% by mass, of the components contained therein are provided by the species of (M), (N), (R), (D), and (C). [Aspect 10] The viscosity is measured using a thermally controlled rotational rheometer with cone-plate geometry (cone diameter: 60 mm, zero-gap distance: 0.061 mm, cone angle: 0.5°, shear rate: 600 s -1 10. The inkjet composition according to any one of Aspects 1 to 9, wherein the viscosity is measured according to DIN EN ISO 3219 at a temperature of 40 to 60° C. with a heating rate of 2 K / min. [Aspect 11] The ink-jet composition according to any one of the above-mentioned aspects 1 to 10, which does not contain a cationic (photo)polymerization initiator or an anionic (photo)polymerization initiator. [Aspect 12] 12. The ink jet composition according to any one of the above embodiments 1 to 11, comprising less than 6% by mass, more preferably less than 2% by mass, of a radically polymerizable monomer not containing an acryloyl group. [Aspect 13] 13. The ink jet composition according to any one of the above embodiments 1 to 12, further comprising a stabilizer, a wetting agent, a defoaming agent, a radical polymerization inhibitor, and / or a pigment. [Aspect 14] Next steps: (a) spraying the ink jet composition according to any one of the above embodiments 1 to 13 with a printer to form a layer having a structural pattern corresponding to the shape of an object; (b) irradiating the formed layer to form a photohardened layer; (c) sequentially repeating steps (a) and (b) to form a plurality of photocured layers to prepare a green body of the three-dimensional object; and (d) heating the green body to post-cure the three-dimensional object. A method for printing a three-dimensional object, comprising: [Aspect 15] 15. The method of claim 14, further comprising printing and curing a support ink to stabilize the green body, the cured support ink being water-soluble and being removed after step c) and before performing step (d) by treatment with an aqueous washing liquid. [Aspect 16] 16. The method of claim 14 or 15, wherein step (d) is carried out such that a temperature of 110 to 140° C. is maintained for at least 5 hours. [Aspect 17] 17. The method of claim 16, wherein in the heating step (d), the associated temperature increase is limited to 2 K / min. [Aspect 18] 18. The method according to any one of Aspects 14 to 17, wherein in step (b), the irradiation is performed by a UV lamp and the exposure time of each ink layer is 0.1 to 2 seconds. [Aspect 19] A three-dimensional object produced by the method according to any one of the above aspects 14 to 18. [Aspect 20] Use of the inkjet composition according to any one of the above embodiments 1 to 13 for producing a three-dimensional object.
[0010] (R(-OCN) x The cyanate ester compound (D) of type (A) contains at least two cyanate groups (-OCN). The acryloyl group according to the present invention is defined as H2C=CH-C(=O)- (which may be part of an "acrylic ester group" of the type H2C=CH-C(=O)-O-). These groups are highly reactive and efficient free radical polymerization groups (much more reactive than, for example, methacrylic groups).
[0011] A photopolymerization reactive compound (M) "containing exactly one acryloyl group" means that it contains no more than one and no less than one acryloyl group.
[0012] By (M) is different from (D), it is meant that photopolymerization reactive compounds (related species) that contain exactly one acryloyl group and further contain at least two cyanate groups should be included in (D) (rather than (M)). However, the use of such "hybrid" components is not preferred (and may be avoided).
[0013] Accordingly, (N) is different from (D) means that the photopolymerization reactive compound (related species) containing at least two acryloyl groups and further containing at least two cyanate groups should be included in (D) (rather than (N)). However, the use of such "hybrid" components is not preferred (and may be avoided). According to the present invention, the inkjet composition comprises (M) and (N) photocurable compounds (based on "photoinitiation"), and further (D) a thermally curable compound.
[0014] Photocurable compounds can be polymerized and / or crosslinked in an initial step by free radical (photo)polymerization, while thermocurable compounds react (via polyaddition) in a later thermal post-cure step.
[0015] The inkjet composition according to the present invention meets the relevant quality requirements:
[0016] The composition provides the basis for a sufficiently low viscosity to allow the production of small (ink-jettable) ink droplets. In addition, the composition provides the basis for sufficient viscosity stability, which is a fundamental requirement to keep the printing process running (e.g., gelling of the ink would clog or even destroy the printer).
[0017] Furthermore, the inkjet composition according to the invention allows the production of pre-products with sufficient mechanical properties, in particular with sufficient "green body strength": the green body strength describes the stability of the object after photocuring and before thermal curing. The green body strength is a measure of the stability and crosslinking of the photocured object. However, it is not desirable to provide too high a green body strength: during post-processing (thermal curing), the UV system ensures the consistency of the shape, meaning that the thermal system is kept in place before and during its curing / fixing. However, once the thermal system starts to cure, depending on its properties (especially if the crosslinking in the first photopolymerization step is too strong), internal strains may occur, which may destroy (crack) the UV-cured structure. The inherent technically typical roughness of the relevant surfaces leads to easier crack formation due to the generation of internal strains. The use of the inkjet composition according to the invention offers a kind of "compromise" that takes into account all of these different issues involved - in particular: on the one hand the crosslinks need to be sufficiently rigid so as to provide strength for the green body and to keep the thermoset system in place, but on the other hand must not be too brittle in order to withstand the thermoset.
[0018] The special "crosslinking strategy" justifying the advantages according to the present invention is reflected in the "rules" underlying inkjet compositions, which are crucially justified by the conformity with the following (key) parameters (I), (II) and (III): (I) an inkjet composition having 1.0 to 5.0 mol / kg of an acryloyl group; (II) 25 to 50 mol % of the acryloyl groups contained therein are provided by the reactive compound (N); The molar ratio of the acryloyl group contained in (III) to the cyanate group contained in the compound (D) is 0.3 to 0.95.
[0019] (Key) Parameter(I): If the value is too high, relatively strong tensions will be created in the green body - promoting subsequent crack formation - and if the value is too low, the strength of the green body will deteriorate: what ultimately matters is a suitable compromise between providing strength, toughness and elasticity, among others.
[0020] (Key)Parameter(II): This parameter also offers a practical compromise between strength (of the green body) and elasticity. Too high a concentration of polyacrylate also causes a significant increase in the ink viscosity, so that printability by inkjet becomes more difficult. On the other hand, polyacrylate in particular is crucial for the formation of a network and thus for sufficient green body strength.
[0021] The monoacrylates especially contribute to the toughness-compatibility balance of the matrix network of the IPN with respect to tension compensation during thermal post-cure, and control of the hard and soft phases and phase domains.
[0022] The right balance between strength and flexibility of the green body is ensured by complying with parameter (II): too low values cause insufficient green strength, whereby too high values on the one hand usually cause viscosity problems, but especially unfavourable distortion (Distortion: serves the macroscopic / optical characterisation of the warping / bending of the cast specimen):
[0023] The strain (as bending of the "test specimen" compared to a smooth surface) increases with increasing degree of crosslinking. Indeed, in the injection process, such strain may occur layer by layer, which promotes subsequent crack formation between layers.
[0024] Warping due to distortion can also be an issue since the ink drops of the next inkjet layer should always be applied to a smooth surface (height control, dynamic effects).
[0025] (Key)Parameter(III): In the broadest sense, this parameter ensures a balanced ratio of pre-curing and post-curing stabilization, and particularly concerns a compromise between the strength of the green body and the strength of the final body.
[0026] As the degree of hardening of the first network (pre-cure) increases, stronger stresses arise in the green body during the formation of the second thermal network (post-cure), which promotes the formation of cracks (disadvantageously associated with too high values), but sufficient green body strength is essential (too low values are ultimately disadvantageous in this respect).
[0027] Parameter (III) is always understood in combination with parameter (I) as a relative ratio, which ultimately determines the network density of both networks.
[0028] A further advantage offered with respect to the use of the inkjet composition according to the invention is the avoidance of "bleeding" of the printed object before and during thermal curing (especially during removal of the support structure by the aqueous liquid and during thermal curing): leakage of liquid raw materials from the printed 3D object can cause health problems for the end user, since the liquid resin may contain reactive chemicals.
[0029] According to a particular embodiment of the present invention, the inkjet composition can be provided as a kit: the corresponding kit-in-part inkjet composition can comprise a combination of at least one photocurable compound and at least one thermally curable compound, and a separate photoinitiator. The kit-in-part inkjet composition can comprise a combination of at least one photocurable compound, at least one thermally curable compound, and a photoinitiator, and a separate curing catalyst. However, in most cases it is neither necessary nor advantageous to provide such a kit (the kit can be avoided).
[0030] According to a preferred embodiment, the inkjet composition according to the present invention has 1.7-3.5 mol / kg of acryloyl groups. Typically, in the inkjet composition, 30-45 mol% of the contained acryloyl groups are provided by the reactive compound (N). The appropriate (quantitative) combination of the two features "mol / kg of contained acryloyl groups" and "mol% of contained acryloyl groups provided by the reactive compound (N)" is also important with respect to providing a pre-product (and also a final product) which, on the one hand, is not too brittle (prone to cracks) and, on the other hand, is not too soft.
[0031] According to a preferred embodiment, in the inkjet composition, 80-100 mol %, preferably 90-100 mol %, of the reactive compound (N) is provided by species containing 3 or less acryloyl groups. However, it is important to pay attention to this regularity in combination with the other features "mol / kg of contained acryloyl groups" and "mol % of contained acryloyl groups provided by reactive compound (N)". Because it has been confirmed that the (appropriate quantitative) combination of these features is a fundamental requirement for providing a processing process on the one hand and for generating a high quality product on the other hand.
[0032] Monoacrylates (particularly compound (M)) often contribute to the medium viscosity of the inkjet composition (particularly species with medium molecular weight). The higher the amount of monoacrylate, the lower the degree of crosslinking.
[0033] The following monoacrylates can be used:
[0034] Ethyl acrylate, stearyl acrylate, tetrahydrofurfuryl acrylate, lauryl acrylate, 2-phenoxyethyl acrylate, isodecyl acrylate, isooctyl acrylate, tridecyl acrylate, caprolactone acrylate, ethoxylated nonylphenol acrylate, isobornyl acrylate, hexadecyl acrylate, monomethoxytripropylene glycol monoacrylate, monomethoxyneopentyl glycol propoxylate monoacrylate, B-carboxyethyl acrylate, and / or oxyethylated phenol acrylate.
[0035] According to a preferred embodiment, the monoacrylate may be selected from dihydrodipentadienyl acrylate (CAS: 12542-30-2), cyclic trimethylolpropane formal acrylate (CAS: 66492-51-1), tricyclodecane methanol acrylate (CAS: 93962-84-6), 2-phenylethyl acrylate (CAS: 3530-36-7), 2-hydroxy-3-phenoxypropyl acrylate (CAS: 16969-10-1), 2-[(butylcarbamoyl)oxy]ethyl acrylate (63225-53-6), and / or 4-hydroxybutyl acrylate (2478-10-6).
[0036] However, the most preferred monoacrylate species are isobornyl acrylate, acryloylmorpholine, 2-[(butylcarbamoyl)oxy]ethyl acrylate, or mixtures thereof.
[0037] The following diacrylates can be used: 1,3 butylene glycol diacrylate, 1,4 butanediol diacrylate, diethylene glycol diacrylate, 1,6 hexanediol diacrylate, neopentyl glycol diacrylate, polyethylene glycol diacrylate, tetraethylene glycol diacrylate, triethylene glycol diacrylate, dipropylene glycol diacrylate, tripropylene glycol diacrylate, polyethylene glycol diacrylate, ethoxylated bisphenol A diacrylate, propoxylated neopentyl glycol diacrylate, ethoxylated neopentyl glycol diacrylate, ethoxylated tripropylene glycol diacrylate, and / or monomethoxytrimethylolpropane ethoxylate diacrylate.
[0038] The following triacrylates can be used: trimethylolpropane triacrylate, tris(2-hydroxyethyl)isocyanurate triacrylate, ethoxylated trimethylolpropane triacrylate, propoxylated glycerol triacrylate ditrimethylolpropane triacrylate, pentaerythritol triacrylate, and / or propoxylated trimethylolpropane triacrylate.
[0039] However, preferred polyacrylates (especially as photopolymerization reactive compounds (N) containing at least two acryloyl groups) are trimethylolpropane triacrylate, tricyclodecane dimethanol diacrylate (CAS: 42594-17-2), polyethylene glycol diacrylate (CAS: 25322-68-3), polypropylene glycol diacrylate (CAS: 52496-08-9), poly(propylene glycol) dimethacrylate (CAS: 25852-47- 5), dipropylene glycol diacrylate (CAS: 57472-68-1), trimethylolpropane trimethacrylate (3290-92-4), bisphenol A glycerolate diacrylate (CAS: 4687-94-9), tris isocyanurate triacrylate (CAS: 40220-08-4), bisphenol A epoxy diacrylate (CAS: 55818-57-0), and / or trimethylolpropane tetraacrylate (CAS: 94108-97-1).
[0040] The one or more photocurable compounds are included in the inkjet composition in the molar amounts specified above, which may be, for example, an amount of 20 to 50% by weight, based on the total weight of the inkjet composition.
[0041] The photopolymerization reactive compounds (species (M) and (N)) and the radical photoinitiator (R) may be included in the inkjet composition in a weight ratio of 95:5 to 99.5:0.5, preferably 97:3 to 99:1.
[0042] Photoinitiators (R) generate reactive species (free radicals) when exposed to radiation (eg, UV light or visible light).
[0043] The photoinitiator may be included in the inkjet composition in an amount of 0.2 to 4% by weight, based on the total weight of the inkjet composition.
[0044] According to one embodiment, the radical photoinitiator (R) species is provided by a phosphine oxide based photoinitiator, preferably by diphenyl(2,4,6-trimethylbenzoyl)phosphine oxide and / or phenylbis(2,4,6-trimethylbenzoyl)phosphine oxide.
[0045] The thermosetting compound contained is a compound capable of addition polymerization (polyaddition) and / or crosslinking when exposed to heat. Preferably, the thermosetting compound does not polymerize and / or crosslink at a temperature below 100° C. According to the present invention, a cyanate ester compound (D) containing at least two cyanate groups is provided as the thermosetting compound.
[0046] With regard to the quality achieved (especially the mechanical properties), it is important that there is a suitable ratio of the inject composition with respect to the photoreactive groups on the one hand (pre-cure for the first step) and the thermoreactive groups on the other hand (post-cure activity). In this regard, preferably, in the inkjet composition, the molar ratio of the acryloyl groups contained therein to the cyanate groups contained in the compound (D) is 0.36 to 0.94.
[0047] Cyanate ester compounds (D) containing at least two cyanate groups are well known to those skilled in the art. Related species are known as polycyanate esters, preferably aromatic or aliphatic diisocyanates, in particular aromatic diisocyanate esters.
[0048] Related species may include cyanate esters based on bisphenol E (AroCy™ L-10), novolac-based cyanate esters (AroCy™ XU 371), bisphenol M-based cyanate esters (AroCy™ XU 366 and AroCy™ XU 378). The cyanate ester may preferably be a cyanate ester based on bisphenol E (AroCy™ L-10) or a novolac-based cyanate ester (AroCy™ XU 371).
[0049] The cyanate ester compound (D) containing at least two cyanate groups is contained in the inkjet composition in the amount defined above (defined indirectly by the molar ratio of the acryloyl groups contained therein to the cyanate groups contained in the compound (D)), which may be, for example, 35 to 75% by weight, based on the total weight of the inkjet composition.
[0050] According to a particular embodiment, at least 30% by weight of the species (D), preferably at least 60% by weight of the species (D) is provided by 4,4'-ethylidene diphenyl dicyanate (e.g., provided by "AroCy™ L-10").
[0051] The curing catalysts used should be wisely selected to initiate the thermal reaction at a certain temperature, much higher than the temperature during printing. This temperature should not be too high, since the UV system may not be able to withstand temperatures above 220° C. for long periods of time. At the same time, they should be as unreactive as possible under the printing conditions. They should work in such a way that they can lead the thermal reaction to the highest conversion rate. They should not destabilize the UV system, and they should withstand possible cleaning procedures for removing the support structure used (as described below). If the associated manufacturing procedures are to be successful and good product quality is to be achieved, it may be advantageous for the species of cyanate ester curing catalyst (C) to be provided by an aluminum metal catalyst, preferably by aluminum acetylacetonate.
[0052] However, the cyanate ester curing catalyst (C) will typically be a chelated metal catalyst, preferably based on a chelated aluminum catalyst.
[0053] The metal catalyst can be included in the inkjet composition in an amount of 100 to 3000 ppm, preferably 300 to 2000 ppm, based on the total weight of the cyanate ester compound (D) containing at least two cyanate groups in the inkjet composition.
[0054] According to a preferred embodiment, 90 to 100% by weight, preferably 97 to 100% by weight, of the components contained (in the inkjet composition) are provided by species (M), (N), (R), (D), and (C).
[0055] The addition of other components is possible, but in many cases is not advantageous (e.g. if there is no contribution in terms of the curing effect or if undesirable thermal reactivity occurs below 100° C.): It is usually not preferred to use (relatively high amounts) of inert solvents (which cannot be photopolymerized in a first step or post-cured in a second step). Preferably, the inkjet composition contains less than 8% by weight, more preferably less than 2% by weight of inert solvent. Furthermore, it is not preferred to use (relatively high amounts) of radically polymerizable monomers that do not contain acryloyl groups (such as methacrylates). Preferably, the inkjet composition contains less than 6% by weight, more preferably less than 2% by weight of radically polymerizable monomers that do not contain acryloyl groups. For example, methacrylates are not sufficiently reactive for (short) radical photopolymerization, for example. Preferably, the inkjet composition contains less than 6% by weight, more preferably less than 2% by weight of methacrylates (which do not contain acryloyl groups).
[0056] In order to avoid undesirable side reactions (which typically increase the viscosity), the inkjet composition preferably does not contain cationic (photo)initiators or anionic (photo)initiators. In any case, it is preferable to avoid compounds (especially high amounts of compounds) that react in the composition via one of the step-reaction types (polyaddition, polycondensation) at temperatures below 100°C. Such compounds (especially relatively high amounts of such compounds) may cause problems with the desired viscosity stability. To enable jetting through a narrow nozzle, it is necessary to limit the viscosity of the inkjet composition.
[0057] Typically, the inkjet composition has a viscosity of 10 to 40 mPa.s at 45° C., where the viscosity is measured on a thermally controlled rotational rheometer in cone-plate geometry (Anton Paar Physica MCR 300, cone diameter: 60 mm, zero-gap distance: 0.061 mm, cone angle: 0.5°, shear rate: 600 s -1 ).
[0058] However, the inkjet composition according to the present invention may further contain a stabilizer, a wetting agent, a defoamer, a radical polymerization inhibitor, and / or a pigment. Usually, dissolved oxygen acts as a radical polymerization inhibitor, but a synthesis inhibitor may be used in addition.
[0059] The present invention further relates to a method for printing a three-dimensional object, comprising the steps of: (a) jetting the ink jet composition by a printer to form a layer in a structured pattern corresponding to the shape of an object; (b) irradiating the formed layer to form a photohardened layer; (c) sequentially repeating steps (a) and (b) to form a plurality of photocured layers to prepare a green body of the three-dimensional object; and (d) heating the green body to post-cure the three-dimensional object.
[0060] Typically, in order to stabilise the green body, a supporting ink is further printed and cured, this cured supporting ink being water-soluble and being removed after step c) and before carrying out step (d) by treatment with an aqueous washing liquid.
[0061] Typically, step (d) is carried out such that a temperature of 110-140° C. is maintained for at least 5 hours.
[0062] Typically, in the heating step (d), the associated temperature increase is limited to 2 K / min.
[0063] Preferably, in step (b), the irradiation is carried out by a UV lamp, and the exposure time of each ink layer is 0.1-2 seconds.
[0064] A typical procedure may be as follows:
[0065] The inkjet composition can be filtered before it is used as an inkjet composition. Preferably, the inkjet composition is filtered so as not to contain particles with a particle size greater than 1 μm. The ink is then placed in the printer. The system is recirculated for at least 2 hours, and better more, to ensure uniformity and constant temperature. During printing, the support ink (e.g., acrylamide-based) is inkjetted and UV-cured to generate a mold for the object ink, which is later inkjetted and UV-cured (wet-on-dry printing). To control the layer thickness, all the inks are leveled once in their liquid state on the build tray, which occurs after the ink jetting during the dynamic wetting process on the substrate and before UV-curing. In this way, a 3D object is generated. Since the support ink is printed layer by layer (together with the layers of the green body), after the printing process the object (green body) becomes surrounded by the support material (e.g., polyacrylamide). To remove the support material, the entire structure is placed in a water bath and heated to 35-40 ° C in the presence of ultrasound. Depending on the support material and the geometry of the object, the cleaning process takes between 0.5 hours and 24 hours (sometimes longer). Once all support structures have been removed, the object is removed from the water bath and air dried at room temperature. After about 5 hours of drying, the object is placed in a heating chamber (a type of oven) and a well-suited temperature program is selected depending on the chemistry, geometry and application to thermally cure the thermal curing system present in the printed and now washed object. It is beneficial to start the thermal reaction slowly to avoid the generation of a strong exotherm and to allow time for the UV-cured system to relax. After a proper thermal cure, it is advantageous to cool slowly to avoid trapping internal stresses.
[0066] The present invention further relates to a three-dimensional object produced according to the above method.
[0067] The three-dimensional object may have a tensile strength of 21-40 MPa, preferably 41-100 MPa, and an elongation at break of 2.1-5%, preferably greater than 5%, and an E-modulus of 100-1000 MPa, preferably 1001-4500 MPa.
[0068] Additionally, the present invention relates to the use of the above ink-jet composition for producing a three-dimensional object.
[0069] General measurement method The viscosity was measured using a thermally controlled rotational rheometer with cone-plate geometry (Anton Paar Physica MCR 300, cone diameter: 60 mm, zero-gap distance: 0.061 mm, cone angle: 0.5°, shear rate: 600 s -1 ) at temperatures between 40 and 60°C at a heating rate of 2 K / min according to DIN EN ISO 3219. For comparison, the viscosity at 50°C or 60°C is given in the examples below. The storage stability of the inks was determined in the same experiments as above after storing closed sample jars at 60°C for 2, 5, 7 and / or 8 days.
[0070] The Shore hardness A and D were measured using a cylindrical specimen with a diameter of 40 mm and a thickness of 7 mm with an OS-2 measuring device (Hildebrand Pruf- und Messtechnik GmbH) according to DIN EN ISO standard 7619. The results were taken from the scale 3 seconds after the needle had entered the specimen. The measurements were repeated 5 times.
[0071] The strength of the green bodies is measured by generating, by UV irradiation, rectangular specimens of each formulation with dimensions 40 mm x 7 mm x 2 or 4 mm (b x a x c). The specimens were placed on two PTFE blocks with a volume of 100 mm x 5 mm x 5 mm. The span width was 35 or 75 mm. The configuration was kept at room temperature and after 1.5 hours, the bending / deformation was checked. To quantify the various formulations, a grading system was defined: A) means that no bending (i.e. 0% bending) or almost no bending (ranging from 5% or less, 3% or less, 1% or less from the initial rectangular specimen) was directly observed. The percentage of bending is defined in comparison with the central position of the rectangular specimen at the beginning of the configuration at time 0 (e.g. dimensions 20 mm x 3.5 mm x 2 mm (b x a x c)) and the central position of the rectangular specimen at the end of the configuration at time 1.5 hours. B) means that bending becomes significant and the specimen shows bending of more than 5% to 20%. C) means that the specimen shows bending of more than 20% to almost touching the substrate. D) means that the specimen touches the substrate. The same was carried out after curing in the oven curing program described above. Tensile tests were carried out on a Zwick-Roell tensile testing machine 1445 according to DIN EN ISO standard 527-1 with 5A specimens. The E-modulus was determined from the slope of the stress-strain curve at 0.05 to 0.25% deformation at 1 mm / min. The tensile strength and elongation at break were determined by pulling the specimens at 5 mm / min for rigid materials.
[0072] Three-point bending tests to determine flexural strength and modulus were carried out on a Zwick Roell 1445 with specimens of dimensions 80 x 10 x 4 mm and a 500 N bending transducer according to DIN EN ISO standard 178. Specimens were bent (in the range of 0.05-0.25% elongation) at a crosshead speed for flexural modulus of 2 mm / min with a compression fin of radius 5 mm, centred over a span distance of 64 mm, and then at a test speed of 10 mm / min until break.
[0073] The impact strength was measured using an IZOD constructed according to DIN EN ISO standard 180, using unnotched test specimens with dimensions 80x10x4 mm and an impact pendulum of 2.75 J on a Zwick HIT5.5P Plus.
[0074] The heat distortion temperature B (0.45 MPa) or A (1.80 MPa) as a three-point bending test was carried out with a HDT measuring device Compact 3 (Coesfeld) on specimens with dimensions of 80 × 10 × 4 mm according to DIN EN ISO 75. The heating rate was set at 2 K / min in the range from 30 °C up to the reaching of the HDT value.
[0075] The glass transition temperature and network density were determined using a thermomechanical analysis (TMA) three-point bending configuration (TMA / SDTA2+LN2) (Mettler Toledo) with specimen dimensions of 10 x 5 x 1.2 mm, with reference to DIN EN ISO 11359. The heating rate was 5 K / min in the range of 20-300 °C and the alternating load in sinusoidal mode was set at 0.02-1.0 N. The network density was then calculated by the T g The storage modulus 50 K higher than the experimental factor divided by 3, the gas constant R, and T g (Kelvin) at 50K above the
[0076] The warpage of 5A specimens from tensile testing after UV curing and thermal curing in the oven cure program described above was determined by inspecting the bending / deformation as a grading system was defined: A) means that no bending (i.e. 0% bending) or very little bending (ranging from 5% or less, 3% or less, 1% or less from the initial specimen) was observed. The percentage of bending is defined in comparison to the center location of the specimen on the base plate and the outer jaws that may lift off the base plate. B) means that bending becomes significant and the specimen shows more than 5% to 10% bending. C) means that the specimen shows 10 to 20% bending. D) indicates that the specimen bending is more than 20%.
[0077] The invention is further explained below by means of examples.
[0078] General Terms and Definitions Reactants used in the examples - Isobornyl acrylate (IBOA) - CAS No 5888-33-5, SARTOMER - Acryloylmorpholine (ACMO) - CAS No 5117-12-4, RAHN - Trimethylolpropane triacrylate (TMPTA) - CAS No 15625-89-5, SARTOMER - CN981-Polyetherester Urethane Diacrylate-CAS No 72162-39-1, SARTOMER - BHT-CAS No 128-37-0, SIGMA ALDRICH - Omnirad 819-CAS No 162881-26-7 Photoinitiator, IGM Resins - RAHN, a polymerization inhibitor that is a combination of Genorad 16-glycerol propoxylate (1PO / OH) and 4-methoxyphenol - AroCy 10L US - Bisphenol E Based Cyanate Ester - CAS No 47073-92-7, HUNTSMAN - Al(acac)3-CAS No 13963-57-0, SIGMA ALDRICH - Co(acac)3-CAS No 21679-46-9, SIGMA ALDRICH - BYK 333-Polyether modified polydimethylsiloxane additive, BYK
[0079] Example 1: Isobornyl acrylate (IBOA) (25.0 wt%), acryloylmorpholine (ACMO) (12.5 wt%), trimethylpropane triacrylate (TMPTA) (12.5 wt%), butylhydroxytoluene (BHT) (0.3 wt%), Omnirad 819 (1.0 wt%), Genorad 16 (0.5 wt%), BYK 333 (0.2 wt%), AroCy 10L US (48.2 wt%) (cyanate ester based on bisphenol E with two cyanate groups) and an additional 500 ppm Al(acac)3 were mixed and filtered at 1 μm. [Table 1]
[0080] The ink was inkjet UV printed and post-cured at a heating rate of 1 K / min from RT to 220°C.
[0081] The final properties of the final object were: Tensile strength: 75MPa Elongation at break: 2.5% E-elastic modulus: 3200MPa
[0082] Measurement of green body after UV curing (40×7×4mm) A Measurement of green body after heat curing (40×7×4mm): A
[0083] The inkjet composition comprises: (I) Mol / kg of acryloyl groups in (M) and (N): 3.35 (II) Mol% of acryloyl groups provided by reactive compound (N): 37.8 (III) Molar ratio of the acryloyl groups (M) and (N) contained in the compound (D) to the cyanate ester groups contained in the compound (D): 0.92
[0084] Example 2: Isobornyl acrylate (12.5% by weight), acryloylmorpholine (7.5%), trimethylolpropane triacrylate (7.5%), BHT (0.3% by weight), Omnirad 819 (1% by weight), Genorad 16 (0.5% by weight), BYK 333 (0.2% by weight), AroCy 10L US (68.2% by weight) as a cyanate ester based on bisphenol E, and an additional 1500 ppm Al(acac)3 were mixed and filtered at 1 μm. [Table 2]
[0085] The ink was inkjet UV printed and post-cured at a heating rate of 1 K / min from RT to 220°C.
[0086] The final properties of the final object were: Tensile strength: 80MPa Elongation at break: 2.7% E-elastic modulus: 2900MPa
[0087] HDT B: 196℃
[0088] Measurement of green body after UV curing (40×7×4mm) B Measurement of green body after heat curing (40×7×4mm): B
[0089] The viscosity stability of Example 2 is measured as follows: [Table 3]
[0090] The inkjet composition comprises: (I) Mol / kg of acryloyl groups in (M) and (N): 1.89 (II) Mol% of acryloyl groups provided by reactive compound (N): 40.2 (III) Molar ratio of the acryloyl groups (M) and (N) contained in the compound (D) to the cyanate ester groups contained in the compound (D): 0.37
[0091] Example 3 For AroCy 10L US as the thermally reactive component, the viscosity was measured after storage at 60° C. for different time intervals in the presence of different catalysts and concentrations (see table below). [Table 4]
[0092] The increase in viscosity in the presence of the cobalt catalyst is more pronounced than in the aluminum catalyst.
[0093] Example 4 Isobornyl acrylate (20.8% by weight), acryloylmorpholine (10.3% by weight), trimethylolpropane triacrylate (10.3% by weight), CN 981 (6.32% by weight), Omnirad 819 (1.0% by weight), Genorad 16 (0.25% by weight), BYK 333 (0.2% by weight), AroCy 10L US (51.0% by weight), and aluminum acetylacetonate (0.03% by weight) were mixed and filtered through a 1 μm sieve. [Table 5]
[0094] The inks were inkjet UV printed and post-cured as follows: 30-130°C at 1K / min, 130°C / 10 h, 130-150°C at 1K / min, 150°C / 2 h, 150-180°C at 1K / min, 180°C / 2 h, 180-200°C at 1K / min, 200°C / 2 h, 200-220°C at 1K / min, 220°C / 10 min, 220-30°C at -5K / min.
[0095] The final properties of the final object were: Tensile strength: 86MPa, Elongation at break: 3.9%, E-Modulus of Elasticity: 3500MPa. HDT B: 141℃ Measurement of green body after UV curing (40×7×4mm) A Measurement of green body after heat curing (40×7×4mm): A
[0096] The inkjet composition comprises: (I) Mol / kg of acryloyl groups in (M) and (N): 2.85 (II) Mol% of acryloyl groups provided by reactive compound (N): 39.3 (III) Molar ratio of the acryloyl groups (M) and (N) contained in the compound (D) to the cyanate ester groups contained in the compound (D): 0.74
[0097] Example 5 Isobornyl acrylate (17.1% by weight), acryloylmorpholine (7.8% by weight), trimethylolpropane triacrylate (7.3% by weight), CN 981 (6.3% by weight), Omnirad 819 (0.5% by weight), Genorad 16 (0.25% by weight), BYK 333 (0.2% by weight), AroCy 10L US (60.0% by weight), and aluminum acetylacetonate (0.03% by weight) were mixed and filtered through a 1 μm sieve. [Table 6]
[0098] The inks were inkjet UV printed and post-cured as follows: 30-130°C at 1K / min, 130°C / 10 h, 130-150°C at 1K / min, 150°C / 2 h, 150-180°C at 1K / min, 180°C / 2 h, 180-200°C at 1K / min, 200°C / 2 h, 200-220°C at 1K / min, 220°C / 10 min, 220-30°C at -5K / min.
[0099] The final properties of the final object were: Tensile strength: 86MPa, Elongation at break: 4.2%, E-Modulus: 3400MPa.
[0100] HDT B: 194℃ Measurement of green body after UV curing (40×7×4mm) A Measurement of green body after heat curing (40×7×4mm): A
[0101] The inkjet composition comprises: (I) Mol / kg of acryloyl groups in (M) and (N): 2.19 (II) Mol% of acryloyl groups provided by reactive compound (N): 37.2 (III) Molar ratio of the acryloyl groups (M) and (N) contained in the compound (D) to the cyanate ester groups contained in the compound (D): 0.48
[0102] Example 6 Isobornyl acrylate (20.7% by weight), trimethylolpropane triacrylate (6.7% by weight), CN 981 (4.4% by weight), Omnirad 819 (2.3% by weight), Genorad 16 (0.29% by weight), BYK 333 (0.2% by weight), AroCy 10L US (65.4% by weight), and aluminum acetylacetonate (0.033% by weight) were mixed and filtered to 1 μm. [Table 7]
[0103] The inks were inkjet UV printed and post-cured as follows: 30-130°C at 1K / min, 130°C / 10 h, 130-150°C at 1K / min, 150°C / 2 h, 150-180°C at 1K / min, 180°C / 2 h, 180-200°C at 1K / min, 200°C / 2 h, 200-220°C at 1K / min, 220°C / 10 min, 220-30°C at -5K / min.
[0104] The final properties of the final object were: Tensile strength: 86MPa Elongation at break: 3.5% E-elastic modulus: 3400MPa HDT B: 189℃ HDT A: 124℃
[0105] Bending strength: 111MPa Flexural modulus: 2800MPa Izod (without notch): 264J / m
[0106] The inkjet composition comprises: (I) Mol / kg of acryloyl groups in (M) and (N): 1.72 (II) Mol% of acryloyl groups provided by reactive compound (N): 42.5 (III) Molar ratio of the acryloyl groups (M) and (N) contained in the compound (D) to the cyanate ester groups contained in the compound (D): 0.35
[0107] Examples 7-11 To screen the ink and material properties of potential inkjet formulations, the molded specimens were placed in a translucent silicone mold at a distance of 15 cm from the bottom and illuminated with UV light (LED 395 nm, 16 W / cm 2 ) for 30 seconds on each side. A thermal post-cure is then performed. Thus, the photopolymerized, oven-cured bulk specimen test results closely highlight the final material performance of the jetted material and the post-cured formulation, despite the different preparation processes in the first cure step of the interpenetrating system.
[0108] Examples 7-11 show various formulation ratios where the degree of functional acrylate groups according to (N) falls within or borders the claimed dual cure inkjet inks to highlight the correlation between printing applications and material properties.
[0109] Isobornyl acrylate, acryloylmorpholine, trimethylpropane triacrylate, Omnirad 819, Genorad 16, AroCy 10L US, and Al(acac)3 were mixed in the ratios shown in Table 1.
[0110] Inks were cast as above and post-cured as follows: 30-130°C at 1K / min, 130°C / 10 h, 130-150°C at 1K / min, 150°C / 2 h, 150-180°C at 1K / min, 180°C / 2 h, 180-200°C at 1K / min, 200°C / 2 h, 200-220°C at 1K / min, 220°C / 10 min, 220-30°C at -5K / min.
[0111] As shown in Table 1, the ink and material properties change with increasing network density due to increasing mol% by (N). Thus, the strength of the green bodies labeled C is too low and the material in the green state is too soft, while the warpage of category D is too high and the internal tension of the material is too high to print and post-cure complex three-dimensional objects with sufficient dimensional accuracy for digital files. In addition, good final mechanical properties in terms of toughness and flexibility, preferably tensile strength of 70-100 MPa and elongation at break of preferably 3-5% are only achieved by balancing the degree of functional acrylate groups by (N). [Table 8] [Table 9]
Claims
1. An inkjet composition having 1.0 to 5.0 mol / kg of acryloyl groups, the inkjet composition comprising: (i) a photopolymerization reactive compound (M) containing exactly one acryloyl group; (ii) a photopolymerization reactive compound (N) containing at least two acryloyl groups; (iii) a radical photoinitiator (R); (iv) a cyanate ester compound (D) containing at least two cyanate groups, and (v) Cyanate ester curing catalyst (C) Including, (M) is different from (D), except that a cyanate ester compound containing exactly one acryloyl group and further containing at least two cyanate groups should be included in (D); The (N) is different from the (D), except that a cyanate ester compound containing at least two acryloyl groups and further containing at least two cyanate groups should be included in the (D); 25 to 50 mol % of the acryloyl groups contained therein are provided by the reactive compound (N), and a molar ratio of the acryloyl groups contained therein to the cyanate groups contained in the compound (D) is 0.30 to 0.
95.
2. The ink jet composition according to claim 1, having an acryloyl group content of 1.7 to 3.5 mol / kg.
3. 3. The ink-jet composition according to claim 1, wherein 30 to 45 mol % of the acryloyl groups contained therein are provided by the reactive compound (N).
4. 3. The ink jet composition of claim 1, wherein 80-100 mol % of the reactive compound (N) is provided by a species containing up to three acryloyl groups.
5. 3. The ink jet composition according to claim 1, wherein a molar ratio of the acryloyl group contained in the compound (D) to the cyanate group contained in the compound (D) is from 0.36 to 0.
94.
6. 3. The ink jet composition of claim 1 or 2, wherein at least 30% by weight of the (D) species is provided by 4,4'-ethylidene diphenyl dicyanate.
7. The ink jet composition of claim 1 or 2, wherein the radical photoinitiator (R) species is provided by a phosphine oxide based photoinitiator.
8. 3. The ink jet composition of claim 1 or 2, wherein the cyanate ester curing catalyst (C) species is provided by an aluminum metal catalyst.
9. 3. The ink jet composition according to claim 1, wherein 90 to 100 mass % of the components contained therein are provided by the species (M), the species (N), the species (R), the species (D), and the species (C).
10. The viscosity is measured at 45° C. in the range of 10 to 40 mPa.s using a thermally controlled rotational rheometer with cone-plate geometry (cone diameter: 60 mm, zero-gap distance: 0.061 mm, cone angle: 0.5°, shear rate: 600 s -1 3. The ink jet composition according to claim 1, wherein the viscosity is measured at 1000 s at 200 s in accordance with DIN EN ISO 3219 at a temperature of 40 to 60° C. with a heating rate of 2 K / min.
11. The ink jet composition according to claim 1 or 2, which does not contain a cationic (photo)polymerization initiator or an anionic (photo)polymerization initiator.
12. The ink jet composition according to claim 1 or 2, comprising less than 6% by weight of a radically polymerizable monomer not containing an acryloyl group.
13. The ink jet composition according to claim 1 or 2, further comprising a stabilizer, a wetting agent, a defoamer, a radical polymerization inhibitor, and / or a pigment.
14. Next steps: (a) jetting the ink jet composition according to claim 1 or 2 by a printer to form a layer of a structural pattern corresponding to the shape of an object; (b) irradiating the formed layer to form a photohardened layer; (c) sequentially repeating steps (a) and (b) to form a plurality of photocured layers to prepare a green body of the three-dimensional object; and (d) heating the green body to post-cure the three-dimensional object. A method for printing a three-dimensional object, comprising:
15. 15. The method of claim 14, further comprising printing and curing a supporting ink to stabilize the green body, the cured supporting ink being water-soluble and being removed after step c) and before performing step (d) by treating with an aqueous washing liquid.
16. 15. The method of claim 14, wherein step (d) is carried out such that a temperature of 110-140° C. is maintained for at least 5 hours.
17. 17. The method according to claim 16, wherein in the heating step (d) the associated temperature increase is limited to 2 K / min.
18. The method according to claim 14, wherein in step (b), the irradiation is performed by a UV lamp, and the exposure time of each ink layer is 0.1 to 2 seconds.
19. Use of the ink jet composition according to claim 1 or 2 for producing a three-dimensional object.
Citation Information
Patent Citations
Cyanate ester dual cure resins for additive manufacturing
CN108350145A
Cyanate Ester Dual-Curing Resin for Additive Manufacturing
JP2018527442A
High temperature three dimensional printing compositions
US20160369040A1
Polymerizable composition and method for producing three-dimensional modeled object
WO2019203134A1
Dual cure resin for the production of moisture-resistant articles by additive manufacturing
WO2020205212A1