Alumina and its manufacturing method
Surface modification of alumina with phosphono group-containing modifiers addresses the high viscosity issue of citric acid-modified aluminas, ensuring dispersibility and low viscosity at elevated pH without additional modifiers, enhancing processing efficiency.
Patent Information
- Application Number
- JP2021518650
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2018-10-03
- Filing Date
- 2019-10-02
- Publication Date
- 2024-09-19
- Estimated Expiration
- 2039-10-02
AI Technical Summary
Citric acid-modified aluminas exhibit high viscosity at pH 8 or higher, making them difficult to process, and the use of additional modifiers like malonic acid complicates manufacturing and introduces undesirable interactions.
Surface modification of alumina with a phosphono group-containing modifier, such as 2-phosphonobutane-1,2,4-tricarboxylic acid, at low loadings to achieve dispersibility and low viscosity at pH 8 or higher, without the need for additional modifiers.
The modified alumina maintains high dispersibility and low viscosity at elevated pH, reducing processing complications and potential interactions with other components.
Smart Images

Figure 0007554186000004 
Figure 0007554186000003 
Figure 0007554186000002
Abstract
Description
[Technical field]
[0001] The present invention relates to a process or processes for the preparation of surface modified alumina. In particular, the present invention relates to a process for the preparation of surface modified alumina which is dispersible at a pH above 8 and has low viscosity at a pH above 8. The present invention also extends to modified alumina prepared according to the process of the present invention and to modified alumina having unique characteristics. [Background technology]
[0002] Aluminas modified with citric acid are known to produce dispersible modified aluminas at pH levels above 8. However, the problem with these citric acid modified aluminas is that at pH levels above 8, these The viscosity of these materials increases rapidly to the point where the material becomes difficult to process.
[0003] To address this issue, a second carboxylic acid, such as malonic acid, is needed. The addition of malonic acid reduces the viscosity of the citric acid modified alumina at pH levels above 8.
[0004] While this solution is effective, it requires the use of a second modifier and substantially increases the amount of modifier added, which can be detrimental for some applications, such as ceramics, where the additional modifier can create complications during the forming and burnout stages of manufacture and can introduce undesirable interactions with other components of the system.
[0005] The object of the present invention is to overcome the drawbacks presented by what is known in the art.
[0006] The present inventors have surprisingly discovered a new method of modifying the surface of alumina to produce modified alumina that is dispersible at a pH of 8 or greater and has low viscosity at a pH of 8 or greater, as well as having a low loading of modifier. Summary of the Invention
[0007] According to one aspect of the present invention: i) providing alumina; and ii) Adding a phosphono group-containing modifier to the alumina to produce a surface-modified alumina. A method for producing modified alumina is provided, comprising the steps of:
[0008] The present invention may further comprise the step of drying the surface-modified alumina after the addition of the phosphono-group-containing modifier.
[0009] The present invention also relates to: a) Alumina before the addition of the phosphono group-containing modifier Aging and having a crystallite size of 35 to 450 Å (measured in the 120 plane). Aging the further step of forming alumina; or b) Surface-modified alumina Aging Let me Aging the further step of forming a surface modified alumina; or c) a) and b) above may include.
[0010] The present invention relates to a method for producing a composition comprising either (a) or (b) above. Aging step c), and drying step, or Aging The process may include both a pre-coating step and a drying step.
[0011] therefore: A first option of the first aspect of the invention is: i) providing alumina; ii) hydrothermally treating the alumina until the alumina has a crystallite size of 35 to 450 Å (as measured in the 120 plane); Aging Let me, Aging Forms alumina; iii) a phosphono group-containing modifier Aging In addition to alumina, surface-modified alumina is produced; and iv) optionally drying the surface modified alumina to produce a modified alumina; The method for producing modified alumina includes the steps of:
[0012] A second option of the first aspect of the invention is: i) providing alumina; ii) adding a phosphono group-containing modifier to the alumina to produce a surface-modified alumina; iii) heat treating the surface modified alumina (preferably at elevated temperature under autogenous pressure) to form a surface modified alumina. Aging Let me, Aging Forming a surface-modified alumina; and iv) In some cases Aging drying the surface modified alumina to produce modified alumina; The method for producing modified alumina includes the steps of:
[0013] A third option of the first aspect of the present invention is: i) providing alumina; ii) The alumina is hydrothermally treated until the alumina has a crystallite size of 35 to 450 Å (as measured in the 120 plane). Aging By Aging Let me, Aging Forms alumina; iii) adding a phosphono group-containing modifier to the alumina to produce a surface-modified alumina; iv) heat treating the surface modified alumina (preferably at elevated temperature under autogenous pressure) to form a surface modified alumina. Aging Let me, Aging Forming a surface-modified alumina; and v) In some cases Aging drying the surface modified alumina to produce modified alumina; The method for producing modified alumina includes the steps of:
[0014] All of the options according to the first aspect of the present invention preferably include a drying step.
[0015] According to a second aspect of the present invention there is provided a modified alumina produced according to the present invention.
[0016] According to a third aspect of the present invention there is provided a modified alumina which after dispersion at a pH of 8 or greater comprises at least one, preferably more than one, and most preferably all of the following characteristics: i) isoelectric point at pH less than 4; ii) greater than 90% dispersibility when dispersed in basic solution at loadings of 5, 10 or 20 wt.%; iii) D less than 250 nm when dispersed in basic solution at 5, 10 or 20 wt % loading 50 and / or iv) 500s -1 Viscosity less than 50 cP.
[0017] The isoelectric point is determined by zeta potential measurement starting at a pH of 10 and titrating with acid.
[0018] Dispersibility is measured such that the pH of the resulting suspension is maintained above the isoelectric point (IEP) of the material.
[0019] The particle size distribution is measured using a light scattering measurement device including a Horiba 950 and appropriate dilution.
[0020] A basic solution for measuring dispersibility and particle size distribution is a solution with a pH of 9 or higher. A suitable basic solution is an ammonium hydroxide solution.
[0021] Viscosity is measured by transferring an aliquot of the suspension into the concentric cylinder geometry of a TA Instruments DHR2 rheometer maintained at 25 °C. The shear sweep is from 0.1 to 3600 s -1 It works with.
[0022] The features of the modified alumina defined in the third aspect of the present invention apply to the modified alumina of the second aspect of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0023] Detailed Description of the Preferred Embodiments The present invention is directed to a method for producing modified alumina by modifying the surface of alumina with the addition of a phosphono group-containing modifier. Optionally, the present invention provides a method for modifying the surface of alumina by hydrothermal or hydrothermal addition of a phosphono group-containing modifier. Aging The present invention is directed to the modification of alumina to produce modified alumina. Accordingly, the present invention relates to one or more Aging The method may include a drying step. The present invention preferably includes a drying step. Various options of the first aspect of the present invention are outlined in the options for the first aspect of the present invention. The present invention further relates to modified aluminas produced according to the method of the present invention, and modified aluminas having unique characteristics.
[0024] The elements of the present invention are described below.
[0025] alumina The alumina comprises aluminum oxyhydroxide, aluminum oxide, aluminum hydroxide, or mixtures thereof. The alumina is preferably aluminum oxyhydroxide. The aluminum oxyhydroxide preferably comprises boehmite or pseudoboehmite, and is most preferably boehmite.
[0026] The alumina may be in the form of dry particles, in an aqueous slurry, an acidified alumina composition, or a mixture thereof. In a preferred embodiment of the invention, the alumina is in an aqueous slurry. The aqueous slurry is prepared by adding alumina, preferably boehmite, to at least water.
[0027] The alumina to be used by the present method has a controlled crystallite size.
[0028] In this regard, the alumina of the present invention may comprise particles having an average crystallite size of 30-500 Å, preferably 40-400 Å, and most preferably 80-200 Å, as measured by X-ray diffraction in the 120 plane. Aging Process (hot water AgingThis process involves heating the alumina at a temperature between 100 and 200° C. for a period of 0.5 to 4 hours until the alumina crystallite size is between 40 and 450 Å. This involves heating until just combined.
[0029] Furthermore, alumina is 80 to 300 m 2 / g BET surface area, preferably 120-250 m 2 / g BET surface area.
[0030] Phosphono group-containing modifier The phosphono group-containing modifier of the present invention comprises an organophosphorus compound, preferably a linear or branched alkyl group having from 1 to 20 carbon atoms. The phosphono group-containing modifier also preferably comprises at least one carboxyl (COOH) group and has at least one phosphono moiety. The phosphono moiety comprises a first phosphono-alkyl carboxylic acid, a second phosphono-alkyl carboxylic acid, a first dicarboxylic acid, a second alkyl dicarboxylic acid, a first phosphono-alkyl tricarboxylic acid, a phosphine alkane carboxylic acid, or mixtures thereof. The phosphono moiety is more preferably a first alkyl carboxylic acid, a second phosphono alkyl carboxylic acid, a first dicarboxylic acid, a second alkyl dicarboxylic acid, a first phosphono-alkyl tricarboxylic acid, a phosphine alkane carboxylic acid, or mixtures thereof. The most preferred phosphono group-containing modifier is 2-phosphonobutane-1,2,4-tricarboxylic acid.
[0031] The phosphono-containing modifier is mixed with the alumina so as to be distributed on the alumina surface.
[0032] The phosphono group-containing modifier is preferably added to the aqueous alumina slurry, or Aging It is added to an aqueous alumina slurry.
[0033] The phosphono group-containing modifier is present in an amount of less than 10% by weight based on the alumina, preferably between 3% and 10% by weight based on the alumina, more preferably less than 8% by weight based on the alumina, and most preferably between 3% and 8% by weight based on the alumina. The proportions are preferably based on the alumina in hydrated powder form.
[0034] Aging As is well known in the art, Aging What is hydrothermal Aging It is called.
[0035] Hydrothermal Deposition of Alumina Aging can be carried out at a temperature between 100 and 200° C. for a period of between 0.5 and 4 hours prior to adding the phosphono group-containing modifier.
[0036] Alternatively, or in addition, Aging can be carried out at a temperature between 95° C. and 125° C. for a period of between 0.5 and 2 hours after addition of the phosphono group-containing modifier.
[0037] After adding the phosphono group-containing modifier, the mixture is heated at a temperature between 95° C. and 125° C. for a period of between 0.5 and 2 hours. Aging It is preferable to carry out the following.
[0038] Drying process As is well known to those skilled in the art, the typical process for producing alumina involves a drying step.
[0039] The drying step can be by direct or indirect heating methods. These methods can include spray drying, contact drying, pan drying or other drying techniques. In a preferred method, the drying is carried out in a spray dryer.
[0040] The drying step can be carried out in an inert atmosphere, such as nitrogen, or air, and depending on which drying method is selected, drying can be carried out at a temperature between 85° C. and 250° C., preferably between 100° C. and about 250° C., and most preferably between 105° C. and 120° C. Further depending on the drying technique selected, one skilled in the art of the present invention will know how long to dry for, which can vary from a few seconds to 2 to 6 hours.
[0041] For example, if drying is performed using a spray dryer, the drying step is carried out at an outlet temperature, preferably about 100° C. to about 120° C., and with a residence time of a few seconds to a few minutes. If a contact dryer is used, the device can be heated from the outside with oil circulating inside the outer casing to the desired temperature, preferably in the range of 200° C. to 250° C., for a residence time of only a few minutes to a few hours.
[0042] Illustrative Method of the Invention In a first aspect of the present invention, the phosphono-containing modifier of the present invention is mixed with an aqueous alumina slurry under moderate conditions of temperature and pressure. A drying step may follow.
[0043] Optionally, the alumina slurry is first hydrothermally refined to the desired crystallite size. Aging Being Aging An alumina slurry is formed and then a phosphono group-containing modifier is added. Aging It can be added to an alumina slurry, which may be followed by a drying step.
[0044] As a further option, the alumina slurry is first hydrothermally refined to the desired crystallite size. Aging Being Aging An alumina slurry is formed and then a phosphono group-containing modifier is added. Aging The alumina slurry can then be added to the AgingThe process continues after addition of the phosphono group-containing modifier by heating for a sufficient time, preferably 1 to 4 hours, at a temperature between 95 and 125° C., for example in a closed reactor operated under autogenous pressure. A drying process may follow.
[0045] Drying is carried out without the need for any intermediate filtering or washing steps to form the modified alumina. Drying is preferred.
[0046] The invention will now be described, by way of example only, with reference to the following examples and drawings. [Brief description of the drawings]
[0047] drawing: [Figure 1] FIG. 1 shows the time dependent viscosity results of the modified alumina material compared to other high pH dispersible materials. [Diagram 2] FIG. 2 shows the time dependent viscosity results of the modified alumina material compared to other high pH dispersible materials. [Diagram 3] FIG. 3 shows the time dependent viscosity results of the modified alumina material compared to other high pH dispersible materials.
[0048] Analysis method The specific properties of the products of the present invention were determined using the following analytical techniques.
[0049] Alumina is identified using X-ray analysis. Samples are placed on a 2" plastic disk containing a 1" diameter aperture for X-ray diffraction. XDR data is obtained using a Bruker AXS D4-ENDEAVOR instrument. Boehmite and pseudoboehmite, aluminum oxide, aluminum hydroxide or mixtures are identified by X-ray diffraction as described in the ASTM DMX Linear Diffraction Index. The crystallite size of a single particle of boehmite is obtained by X-ray diffraction techniques using the Debye equation from the X-ray diffraction peaks. The crystallite size is represented by the length obtained for the diffraction peak 120 peak. Peak width analysis of the X-ray powder diffraction peak at 120 gives the commonly reported value for crystallite size.
[0050] The boehmite crystallite size by X-ray diffraction was measured using the 120 crystal size at 90° normal to the 120 plane. This peak (crystal plane) is most commonly obtained in the X-ray diffraction pattern of boehmite and has been used to characterize alumina.
[0051] The particle size of the dispersed alumina is measured using a Horiba instrument.
[0052] Surface area values are measured by N2 adsorption. Data are for samples heated at 550°C for 3 hours. The samples are then degassed under a nitrogen stream at 300°C for 0.5 h. Data are collected on a Quantachrome Apparatus. Surface area (m 2 / g) is B. Evaluate using the ET equation.
[0053] The isoelectric point value is measured using a Malverm Zetasizer. A dispersion of material is made at approximately 1% solids by weight and a pH of 10. An aliquot is injected into a capillary cell and zeta potential measurements are taken with the instrument. The pH of the solution is titrated down 0.5 pH at a time until a pH of 3 is reached. The isoelectric point is the pH at which the zeta potential crosses the x-axis.
[0054] The dispersibility of the alumina forming dispersion is evaluated by making a slurry at the indicated loading weight and pH (e.g., 5% by weight at pH 10) and stirring for 30 minutes. The slurry is then centrifuged at 1600 rpm for 20 minutes.
[0055] The viscosity of the dispersions is measured at the indicated concentrations by transferring an aliquot of the dispersion into the concentric cylinder geometry of a TA Instruments DHR2 rheometer maintained at 25° C. The shear sweep is from 0.1 to 3600 s -1 It works with.
[0056] In order to more fully illustrate the present invention, the following non-limiting examples are given. EXAMPLES
[0057] Example 1 Boehmite alumina was heated at 140°C for 2.5 hours under autogenous pressure. Aging The slurry was removed from the reactor and divided to produce identical batches.
[0058] A phosphono-containing modifier, Cublen P50, was diluted to 10% active using deionized water and stirred into the alumina slurry at 5% by weight based on Al2O3. The slurry was stirred for 30 minutes and dried in a Buchi 290 spray dryer.
[0059] Example 2 An alumina slurry prepared as in Example 1 was modified with 7 wt % Cublen P50 and dried using a Buchi B290 dryer.
[0060] Example 3 The alumina slurry prepared as in Example 1 was modified with 5 wt. % Cublen P50 and again placed in the reactor where it was heated at 105° C. for 1 hour. Aging And Buch Dried in a B290 dryer.
[0061] Comparative Example 1 The alumina slurry prepared as in Example 1 was modified with 5 wt% citric acid based on Al2O3 and heated at 105°C for 1 hour. Aging and spray dried.
[0062] Comparative Example 2 The alumina slurry prepared as in Example 1 was modified with 5 wt% citric acid based on Al2O3 and heated at 105°C for 1 hour. Aging Then, malonic acid was added to the mixture and spray-dried. Added as per the previous technology.
[0063] Comparative Example 3 An alumina slurry prepared as in Example 1 was doped with 1.5 wt % nitric acid based on Al2O3 and spray dried.
[0064] Comparative Example 4 Unmodified alumina was used as a control.
[0065] The dispersibility of the modified alumina of the present invention and the comparative examples is shown in Table 1, and the viscosities are shown in Figures 1-3.
[0066] [Table 1]
[0067] As can be seen, the modified alumina(s) of the present invention were highly dispersible at pH 10 with reasonably low loadings of phosphono-containing modifier. The dispersibility of the modified aluminas of the present invention is similar to that of the citric acid modified materials, although the viscosities of the materials when dispersed at 5, 10 and 20 wt % are substantially different (Figures 1-3). The unmodified and acid modified materials are not dispersible or effective under high pH conditions.
Claims
1. i) providing aluminum oxyhydroxide; and ii) aging the aluminum hydroxide by hydrothermal treatment at a temperature between 100° C. and 200° C. for a period between 0.5 and 4 hours to form alumina having a crystallite size of 35 to 450 Å measured in the 120 plane; and iii) adding a phosphono group-containing modifier to the alumina in an amount of less than 10% by weight based on the alumina to produce a surface-modified alumina; A method for producing modified alumina, comprising the steps of:
2. 10. The method of claim 1, further comprising aging the surface modified alumina by hydrothermally treating the surface modified alumina to form an aged surface modified alumina.
3. 3. The method of claim 1 or 2, further comprising drying the surface modified alumina or the aged surface modified alumina.
4. The method of claim 1 , wherein the phosphono-group-containing modifier comprises an organophosphorus compound.
5. The method of claim 4, wherein the organophosphorus compound contains at least one carboxyl (COOH) group and has at least one phosphono moiety.
6. 5. The method of claim 4, wherein the phosphono-group-containing modifier comprises a primary phosphono-alkyl carboxylic acid, a secondary phosphono-alkyl carboxylic acid, a primary dicarboxylic acid, a secondary alkyl dicarboxylic acid, a primary phosphono-alkyl tricarboxylic acid, a phosphine alkane carboxylic acid, or mixtures thereof.
7. 7. The method of claim 1, 4 or 6, wherein the phosphono-containing modifier is added in an amount between 3% and 10% by weight based on the alumina.
8. 8. The method of claim 7, wherein the phosphono-containing modifier is added in an amount between 3% and 8% by weight based on the alumina.
9. 3. The method of claim 2, wherein the surface modified alumina is aged at a temperature between 95°C and 125°C for a period of between 0.5 and 2 hours.
10. 4. The method of claim 3, wherein drying is carried out at a temperature between 85°C and 250°C.
11. 1. An alumina modified with a phosphono group-containing modifier, wherein the modified alumina exhibits at least one of the following characteristics after dispersion at a pH of 8 or greater: i) an isoelectric point at a pH of less than 4; ii) greater than 90% dispersibility when dispersed in basic solution at 5, 10 or 20% loading; iii) a particle size distribution when dispersed in a basic solution at a loading of 5, 10 or 20% having a D50 of less than 250 nm; and / or iv) Viscosity less than 50 cP at 500 s Including, alumina.
Citation Information
Patent Citations
Metal oxide particle composite, metal oxide composite sol, and method for producing metal oxide composite sol
JP2007031259A
Functionalized alumina particle for polymer composite material
JP2007126633A
Method of producing modified alumina particle dispersion sol, method of producing modified alumina particles and thermoplastic resin composition using the sol, and modified alumina particle dispersion sol, modified alumina particles and thermoplastic resin composition each prepared by the method
JP2007290943A
Surface-coated aluminum oxide nanoparticles and resin composition comprising same
JP2008056556A
Alumina fine particle and method for producing the same
JP2013177313A