Method for manufacturing a friction brake and device for manufacturing a friction brake

By separately supplying and controlling the residence times of different powdered additives in the laser beam, the method optimizes the bonding of wear protection layers on friction braking bodies, enhancing durability and resistance.

JP7554540B2Active Publication Date: 2024-09-20ROBERT BOSCH GMBH +1
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
JP2022577139
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2020-06-15
Filing Date
2021-06-10
Publication Date
2024-09-20
Estimated Expiration
2041-06-10

AI Technical Summary

Technical Problem

Existing methods for producing wear protection layers on friction braking bodies, such as brake discs, using laser deposition welding do not optimally utilize the properties of different powdered additives, leading to suboptimal bonding and potential delamination.

Method used

The method involves separately supplying at least two powdered additives to the laser metallization welding process, controlling their residence times in the laser beam by varying angles and positions, ensuring optimal bonding by adjusting the melting degrees of each additive.

Benefits of technology

This approach enhances the material-bonding connection between the additives and the base body, improving the wear protection layer's durability and resistance to corrosion and abrasion.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007554540000003
    Figure 0007554540000003
  • Figure 0007554540000002
    Figure 0007554540000002
  • Figure 0007554540000001
    Figure 0007554540000001
Patent Text Reader

Abstract

The present invention relates to a method for manufacturing a friction braking body, in particular a brake disc (1), having a base body (3) with a friction contact area, in which a wear protection layer (5) is produced in the friction contact area by laser deposition welding using a laser beam (9) directed at the friction contact area, the wear protection layer (5) being formed by at least one powdered additive during the laser deposition welding. It is specified that at least two powdered additives are added simultaneously, and that the at least two powdered additives have different dwell times in the laser beam (9).
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method and an apparatus for producing a friction braking body, in particular a brake disc, having a base body with a friction contact area, in which a wear protection layer is produced by laser deposition welding using a laser beam directed at the friction contact area, the wear protection layer being formed by at least one powdered additive during the laser deposition welding.

[0002] Background technology Methods for producing friction brakes of the above-mentioned type are already known from the prior art. In order to reduce wear caused by friction during operation, it is known to provide friction brakes with a wear protection layer that is wear-resistant and ensures a long service life for the friction brakes. Laser build-up welding has already proven advantageous for producing this wear protection layer. In this case, the surface of the base body to be coated is locally melted by a laser beam and a powdered additive is added. The additive is at least partially liquefied or completely melted by the laser beam before reaching the molten surface, so that a material-bonding bond is created between the molten surface and the additive. Compared to sprayed layers, layers applied by laser build-up welding usually provide a higher layer adhesion and better delamination resistance due to the material-bonding bond. From EP 3034902 A1, for example, a corresponding production method is already known for carrying out laser build-up welding.

[0003] Disclosure of the Invention The method according to the invention with the features of claim 1 has the advantage that, when combining at least two different powdered additives, these are not fed as a mixture but separately to the laser deposition welding process and melted separately by the laser beam, as a result of which an optimal joint is ensured in the wear protection layer. For this purpose, it is specified according to the invention that the at least two powdered additives are added simultaneously and that the at least two powdered additives have different residence times in the laser beam. This achieves that the different additives are influenced differently by the laser beam, so that it is ensured, for example, that both additives are melted completely or purposefully melted to different intensities by the laser beam.

[0004] Preferably, each of the additives is jetted toward the substrate by at least one nozzle each and arrives within the laser beam before reaching the substrate. Jetting the additives toward the substrate by one nozzle each allows for a targeted orientation of the additive jet, which allows for a targeted arrival at the laser beam and a cost-effective use of the laser beam.

[0005] Particularly preferably, at least two additives are injected into the laser beam at different angles relative to the laser beam. The different injection angles ensure that the additives stay in the laser beam for different periods before reaching the substrate. If the angle relative to the laser beam is, for example, selected to be larger, the dwell period is shorter compared to a smaller angle. This allows the dwell period in the laser beam to be easily and optimally adapted to the respective additive depending on the adjusted angle.

[0006] Preferably, at least two additives are injected at equal or different radial distances from the laser beam and at equal or different axial heights from the laser beam. The radial or lateral distance of the nozzles from the laser beam and the axial distance from the substrate (corresponding to the axial height or distance in the direction of the laser beam) can also advantageously adapt the residence time of each additive in the laser beam.

[0007] Furthermore, it is preferably specified to select the angle such that each additive is melted by the laser beam, in particular as completely or as incompletely as possible. Complete melting ensures, in particular, an advantageous material-connective bond between each additive and the melted area of ​​the substrate, in particular the molten iron-based alloy in the substrate. Incomplete melting makes it possible to avoid undesirable excessively high melting or dissociation of each additive.

[0008] It is further specified that each additive is preferably injected into the laser beam with at least two material jets from at least two nozzles, so that the material jets of each additive collide in the laser beam. By injecting from two sides, it is achieved that the material jets colliding in the laser beam are advantageously mixed with each other and / or are uniformly distributed in the molten surface of the base body. By injecting the additive from two lateral sides, therefore, an impingement point occurs, particularly within the laser beam, where both material jets collide and are mixed with each other. In this case, the injection angles of both material jets are preferably selected equally, so that a uniform distribution is ensured. If the material jets are different due to different material densities and / or volume flows, different injection angles may be advantageous.

[0009] Preferably, the material jets of each additive are injected from at least two nozzles, either diametrically opposite each other relative to the laser beam or evenly distributed over the entire circumference of the laser beam.

[0010] Furthermore, it is specified that preferably the material jets of at least two additives are impinged at one impact point in the laser beam. Thus, all material jets used during the laser metallization of the present invention impinge at one point in the laser beam and are preferably mixed together. In this case, due to the different angles of incidence or different radial distances to the laser beam, the material jets already reside in the laser beam for different periods before reaching the impact point, and are thus processed by the laser beam for different periods.

[0011] According to a preferred refinement of the invention, the material jet of the first additive impinges at a first impingement point in the laser beam, and the material jet of the second additive impinges at a second impingement point in the extension of the laser beam, both impingement points being located at a distance from each other in the direction of emission of the laser beam. This also further influences the residence time of the additive in the laser beam. The second impingement point is located in the laser beam, in particular before reaching the substrate, or alternatively in the substrate, whereby the second impingement point is merely a virtual impingement point.

[0012] According to a preferred refinement of the invention, two groups of additives are added: alloys, in particular iron-based alloys, and hard materials, which may be sufficiently homogeneous compounds, for example carbides, nitrides or borides, which result in advantageous properties of the wear protection layer with regard to corrosion resistance and wear resistance.

[0013] The device according to the invention having the features of claim 11 has at least two nozzles for injecting material streams, each containing a different additive, into the laser beam of the laser beam source, which nozzles are oriented such that the material streams are injected into the laser beam at different angles. This gives rise to the advantages already described. Further advantages, preferred features and feature combinations are evident from the above description and the claims.

[0014] The present invention will now be described in detail with reference to the drawings. [Brief description of the drawings]

[0015] [Figure 1] FIG. 1 is a simplified perspective view of an advantageous friction damping body. [Diagram 2] 1 shows an advantageous embodiment of a device and method for manufacturing a friction brake body; [Diagram 3] 1 shows an advantageous embodiment of a device and method for manufacturing a friction brake body;

[0016] 1 shows a friction braking body in the form of a brake disc 1 of a friction brake 2 (not shown in detail in FIG. 1) of a motor vehicle in a simplified perspective view. The brake disc 1 is of annular design and is intended to cooperate with displaceable brake shoes of the friction brake 2, which can be pressed against at least one end face of the brake disc 1. An optionally present brake disc hat is not shown in FIG. 1.

[0017] The brake disc 1 has a base body 3 which is of annular design and which has at each of its end faces a friction contact surface 4 which is used to cooperate with a brake shoe of the friction brake 2. The base body 3 is preferably made of grey cast iron. The friction contact surface 4 is preferably formed by a wear protection layer 5 which is applied to the base body 3.

[0018] According to the present embodiment, the wear protection layer 5 is produced by laser deposition welding. For this purpose, a preferred device 6 for carrying out the laser deposition welding method is shown in a simplified diagram in Fig. 2. The device 6 has a working head 7 carrying a laser beam source 8 which generates a laser beam 9 and a device 10 for ejecting different powdered additives.

[0019] The device 10 has, for example, a number of nozzles 11, 12, 13, 14 held in the working head 7. In this case, the nozzle pairs 13, 14 or 11, 12 are arranged rotationally symmetrically around the laser beam and are only shown as pairs for reasons of representation. In particular, at least three nozzles per rotational symmetry are advantageous. When three nozzles are used, they are arranged with an angular offset of 120°, when four nozzles are used, an angular offset of 90° is preferred.

[0020] The distribution of nozzles 11-14 allows maximum use of the rotational symmetry along the laser beam 9. When using 2x3 nozzles, the nozzles can be staggered by only 60°.

[0021] Alternatively to individual nozzles (injectors), annular gap nozzles may be used, which allow continuous pumping (similar to the profile of a cone rising at an apex and having a circular base). The nozzles 11-14 are oriented at a defined angle to the laser beam 9, so that the material jets S11-S14 issuing from each nozzle 11-14 are oriented at a defined angle α11, α12 or α13, α14 to the laser beam 9 or to the central longitudinal axis 9' of the laser beam 9.

[0022] The nozzles 11 and 12 are used to blow out the first additive material. The nozzles 13 and 14 are used to blow out the second additive material. As shown in FIG. 2, the additive material is blown into the laser beam 9 at preset angles α11-α14. The blowing angles of the nozzles 11 and 12 correspond to each other and are different from the equally equal blowing angles α13 and α14 of the nozzles 13 and 14 (α11=α12≠α13=α14). The nozzles 11 and 12 are arranged on different sides or diametrically opposite sides of the working head 7, as are the nozzles 13 and 14. Thereby, the material jets S11, S12, S13 and S14 of the nozzles 11, 12, 13 and 14 collide at one collision point TP1 in the laser beam 9. The nozzles 11, 12 are arranged in the work head 7 at a further radial distance from the laser beam or laser beam source 8 than the nozzles 13, 14. Due to the difference between the blowing angles α11, α12 on the one hand and the blowing angles α13, α14 on the other hand, it is nevertheless ensured that the material jets S11-S14 impinge on the substrate 3 at an internal impingement point TP1 of the laser beam 9 at an axial distance therefrom.

[0023] Due to the advantageous arrangement and orientation of the nozzles 11-14, it is achieved that the two additives stay in the laser beam 9 for different periods of time. Due to the smaller angles α13, α14 and the lateral distance to the laser beam source 8, it is achieved that the second additive blown out by the nozzles 13, 14 stays in the laser beam 9 for a longer period of time than the first additive blown out by the nozzles 11, 12. The impact point TP1 is selected such that the material jets S11-S14 impinge on the substrate 3 within the range of the laser beam 9, so that the additive is melted and an advantageous material-connective connection between the blown additive and the melted area of ​​the substrate 3 is ensured. In the illustrated configuration, therefore, an additive is used as the first additive for melting, which requires a shorter residence time in the laser beam compared to the second additive. Conversely, this principle can also be used if, for example, it is not desired to melt the additive. For example, when processing an iron-based alloy with chromium carbide, it has been found to be advantageous for the chromium carbide to have as low a degree of melting as possible, whereas the iron-based alloy must be completely melted, and the chromium carbide is then preferably provided so that its interaction time (dwell time) with the laser beam 9 is as short as possible.

[0024] In the case of particularly high thermophysical differences of the additive materials, a specific impingement point is respectively set for both additive materials by the blowing angle and blowing position of the nozzles 11-14. For this purpose, another embodiment is shown in a simplified diagram in FIG. 3. In FIG. 3, the same elements are provided with the same reference symbols, and in this respect reference is made to the above description. In the following, substantially only the differences are described.

[0025] As in the previously described embodiment, the material jets S13, S14 impinge on the substrate 3 at the previously described impact point TP1, with a distance therebetween. In contrast, the material jets S11, S12 impinge on the substrate 3 at a second impact point TP2, which is located at a distance from the impact point TP1 in the axial direction or in the direction of emission of the laser beam 9. In the illustrated configuration, this impact point TP2 is indeed located in the direction of emission of the laser beam 9, but inside the substrate 3. For this reason, the blowing angles α11, α12 are selected smaller than in the previously described embodiment. This achieves that the second additive has a significantly longer residence time in the laser beam 9 than the first additive blown out by the nozzles 11, 12.

[0026] According to a further embodiment, the wear protection layer contains niobium carbide (NbC) and stainless steel (e.g. Cr steel or CrNi steel). Due to the higher thermal stability of NbC compared to stainless steel, it is necessary to require a longer interaction time with the laser for NbC. By matching the residence time of the niobium carbide and the stainless steel above the substrate 3 in the laser beam 9 with each other, an effective melting of both additives is ensured until complete melting is reached. The molten parts of the niobium carbide precipitate finely distributed as NbC in the stainless steel matrix during solidification, thus resulting in a homogeneous hardness distribution inside the coating layer. Furthermore, the melting of the surface of the remaining parts of the carbide allows a material-tight bond between the matrix and the hard material. This prevents the hard material or the carbides from dissolving out when the friction brake is subjected to thermomechanical loads. Therefore, according to the present embodiment, it is specified that niobium carbide is used as the second additive and is exposed to a longer dwell period in the laser beam 9 until complete melting is reached.

[0027] According to a further embodiment, the wear protection layer is formed from silicon carbide and special steel. The high thermal conductivity of silicon carbide ensures favorable heat transfer from the wear protection layer to the substrate. This increases the thermal load-bearing capacity of the friction brake. By adapting the impact point TP2 for the silicon carbide used as the first additive according to FIG. 3, the thermal energy delivered to the silicon carbide during laser cladding is reduced. This reduces the dissociation of SiC and substantially prevents the formation of undesirable Fe-Si compounds in the wear protection layer 5, in particular preventing embrittlement of the wear protection layer 5.

Claims

1. A method for manufacturing a friction braking body having a base body (3) with a friction contact area, comprising the steps of: producing a wear protection layer (5) in said friction contact area by laser deposition welding using a laser beam (9) directed at said friction contact area, The wear protection layer (5) is formed by at least one powdered additive material during the laser cladding welding; Adding at least two powdered additives simultaneously and providing different residence times for the at least two powdered additives within the laser beam (9); each of said additive materials is sprayed onto said substrate (3) through at least one nozzle (11-14) so ​​that it reaches said laser beam (9) before reaching said substrate (3); In the method, The material jets (S11 to S14) of the at least two types of additive materials are caused to collide at one collision point (TP1) within the laser beam (9); A method comprising:

2. 2. The method according to claim 1, characterized in that the at least two additive materials are injected at different angles (α11 to α14) relative to the laser beam (9).

3. 3. The method according to claim 2, characterized in that the angles (α11 to α14) are selected such that each of the additive materials is melted by the laser beam (9).

4. 4. The method according to claim 1, wherein the at least two additives are injected at equal or different radial distances from the laser beam (9) and at equal or different axial heights from the laser beam (9).

5. 5. The method according to claim 1, characterized in that each of the additive materials is injected into the laser beam (9) with at least two material jets (S11-S14) from at least two nozzles (11-14), whereby the material jets (S11-S14) of each of the additive materials collide within the laser beam (9).

6. 6. The method according to claim 5, characterized in that the additive material is injected from each of the at least two nozzles (11-14) on diametrically opposite sides of the laser beam (9).

7. An apparatus for manufacturing a friction brake, which implements the method according to any one of claims 1 to 6, A laser beam source (8) for generating a laser beam; at least two nozzles (11-14) for ejecting a material stream into the laser beam (9); Equipped with the nozzles (11-14) are oriented such that the material streams can be injected into the laser beam (9) at different angles (α11-α14) relative to the laser beam (9); Device.

Citation Information

Patent Citations

  • Double-layer-gradient laser material increase manufacturing method

    CN105755464A

  • Dissimilar metal joining method

    JP2018065144A

  • Method for manufacturing steam turbine member

    JP2021156267A

  • Brake disk and method for producing a brake disk

    US20200072307A1

  • Processing nozzle, processing head, processing device

    WO2016151781A1