Plasma etching method and semiconductor device manufacturing method

The plasma etching method using a chlorine-nitrogen gas mixture addresses the challenge of forming varied forward tapered shapes in GaAs substrates by controlling the etching selectivity, enabling precise semiconductor device manufacturing.

JP7555025B2Active Publication Date: 2024-09-24PANASONIC INTELLECTUAL PROPERTY MANAGEMENT CO LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
JP2020148256
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2020-09-03
Publication Date
2024-09-24
Estimated Expiration
2040-09-03

AI Technical Summary

Technical Problem

Conventional methods for etching GaAs compound semiconductor substrates struggle to form various forward tapered shapes, particularly those with small slopes, due to limitations in controlling the side surface slope.

Method used

A plasma etching method using a mixed gas containing chlorine and nitrogen gases is employed to etch III-V compound semiconductors, allowing for the formation of forward tapered shapes with controlled slopes by adjusting the etching selectivity ratio (Vs/Vr) through gas flow rate ratios.

Benefits of technology

This method enables the formation of diverse forward tapered shapes with acute slopes in compound semiconductor layers, enhancing the flexibility and precision of semiconductor device manufacturing processes.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007555025000007
    Figure 0007555025000007
  • Figure 0007555025000013
    Figure 0007555025000013
  • Figure 0007555025000002
    Figure 0007555025000002
Patent Text Reader

Abstract

To provide a plasma etching method for a substrate, capable of forming various forward tapered shapes.SOLUTION: A plasma etching method includes: a step (i) of disposing, in a chamber, a substrate 10 including a compound semiconductor layer 11 formed of a Group III-V compound semiconductor, and a resist mask 12 disposed on one surface 11a of the compound semiconductor layer 11; and a step (ii) of performing plasma etching of the compound semiconductor layer 11 and the resist mask 12 by exposing the compound semiconductor layer 11 and the resist mask 12 to plasma and accordingly, forming a tilt surface 11s forming a forward tapered shape to the compound semiconductor layer 11. The Group III-V compound semiconductor contains Ga and As. The plasma etching in the step (ii) is performed using mixed gas of chlorine-containing gas and nitrogen-containing gas as the etching gas.SELECTED DRAWING: Figure 5
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for etching a substrate and a method for manufacturing a semiconductor device. [Background technology]

[0002] Conventionally, semiconductor devices have been formed using substrates made of GaAs compound semiconductors. In the manufacturing process of semiconductor devices, a step of etching the GaAs compound semiconductor is performed.

[0003] Patent Document 1 (JP Patent Publication 2002-151466 A) discloses "a dry etching method for etching a compound substrate containing gallium and arsenic with an etching gas containing chlorine and boron trichloride, characterized in that an inert gas is added to the etching gas." Patent Document 1 discloses argon gas as the inert gas.

[0004] As disclosed in Patent Document 1, etching gases containing chlorine have been used for etching GaAs compound semiconductor substrates. By using an etching gas containing chlorine, the etching rate of the GaAs compound semiconductor substrate becomes high. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] JP 2002-151466 A Summary of the Invention [Problem to be solved by the invention]

[0006] In addition, in the manufacture of semiconductor devices using GaAs compound semiconductor substrates, GaAs compound semiconductor substrates have conventionally been etched to have a forward tapered shape. However, with conventional methods, it is difficult to significantly change the inclination of the side surface of a forward tapered shape, and it is particularly difficult to form a forward tapered shape with a small side surface gradient. In this situation, one of the objects of the present disclosure is to provide a plasma etching method for substrates and a manufacturing method for semiconductor devices that are capable of forming various forward tapered shapes. [Means for solving the problem]

[0007] One aspect of the present disclosure relates to a method for plasma etching a compound semiconductor layer made of a III-V compound semiconductor, the method comprising the steps of: (i) disposing a substrate including the compound semiconductor layer and a resist mask having an opening and disposed on one main surface of the compound semiconductor layer in a chamber; and (ii) exposing the compound semiconductor layer and the resist mask to plasma in the chamber to perform plasma etching of the compound semiconductor layer and the resist mask, thereby forming an inclined surface forming a forward tapered shape in the compound semiconductor layer, the III-V compound semiconductor including Ga and As, and the plasma etching in the step (ii) being performed using a mixed gas including a chlorine-containing gas and a nitrogen gas as an etching gas.

[0008] Another aspect of the present disclosure relates to a method for manufacturing a semiconductor device including a compound semiconductor layer made of a III-V compound semiconductor, the method including: a step (i) of disposing, in a chamber, a substrate including the compound semiconductor layer and a resist mask having an opening and disposed on one main surface of the compound semiconductor layer; and a step (ii) of exposing the compound semiconductor layer and the resist mask to plasma in the chamber to perform plasma etching of the compound semiconductor layer and the resist mask, thereby forming a slope constituting a forward tapered shape in the compound semiconductor layer, the III-V compound semiconductor including Ga and As but not N, and the plasma etching in the step (ii) being performed using a mixed gas including a chlorine-containing gas and a nitrogen gas as an etching gas. Effect of the Invention

[0009] According to the present disclosure, it is possible to form various forward tapered shapes in a substrate including a compound semiconductor layer constituted of a compound of As and a Group III element including Ga. [Brief description of the drawings]

[0010] [Figure 1A] 1A to 1C are diagrams illustrating a process of the plasma etching method according to the first embodiment. [Figure 1B] FIG. 1B is a diagram showing a schematic diagram of a step following FIG. 1A. [Diagram 2] FIG. 1 is a diagram illustrating an example of an apparatus used in the plasma etching method of the first embodiment. [Diagram 3] FIG. 2 is a schematic diagram for explaining an example of plasma etching in the case where the etching selectivity Vs / Vr=1. [Figure 4] FIG. 2 is a schematic diagram for explaining an example of plasma etching in which an etching selectivity ratio Vs / Vr>1. [Diagram 5] FIG. 2 is a schematic diagram for explaining an example of plasma etching in the case where an etching selectivity ratio Vs / Vr<1. [Figure 6]1 is a graph showing an example of experimental results of the plasma etching method of the present disclosure. [Figure 7] 7 is a graph showing etching selectivity corresponding to the results shown in FIG. 6. [Figure 8] 7 is a graph showing the relationship between the gas flow rate ratio and the gradient of the inclined surface in the experiment shown in FIG. 6. [Figure 9] 11 is a graph showing another example of experimental results of the plasma etching method of the present disclosure. [Figure 10] 10 is a graph showing etching selectivity corresponding to the results shown in FIG. 9. [Figure 11] 10 is a graph showing the relationship between the gas flow rate ratio and the gradient of the inclined surface in the experiment shown in FIG. [Figure 12] 11 is a graph showing another example of experimental results of the plasma etching method of the present disclosure. [Figure 13] 13 is a graph showing the etching selectivity corresponding to the results shown in FIG. 12. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0011] In the following, the embodiment of the present disclosure will be described with examples, but the present disclosure is not limited to the examples described below. In the following description, specific numerical values ​​and materials may be exemplified, but other numerical values ​​and materials may be applied as long as the effects of the present disclosure can be obtained. In this specification, when a "range of numerical value A to numerical value B" is mentioned, the range includes numerical value A and numerical value B.

[0012] (Plasma Etching Method) The plasma etching method of the present disclosure is a plasma etching method for a compound semiconductor layer made of a III-V group compound semiconductor, and includes steps (i) and (ii). Hereinafter, the plasma etching method may be referred to as an "etching method (EM)". The compound semiconductor layer may be referred to as a "compound semiconductor layer (L)".

[0013] Step (i) is a step of placing a substrate including a compound semiconductor layer (L) and a resist mask having an opening and disposed on one main surface of the compound semiconductor layer (L) in a chamber into which an etching gas is introduced to generate plasma.

[0014] Step (ii) is a step of performing plasma etching of the compound semiconductor layer (L) and the resist mask by exposing the compound semiconductor layer (L) and the resist mask to plasma in a chamber, thereby forming a slope constituting a forward tapered shape in the compound semiconductor layer (L). There may be only one slope that reforms the forward tapered shape. From another point of view, step (ii) is a step of forming a slope having a gradient α(s) of less than 90° in the compound semiconductor layer (L) by the above-mentioned plasma etching.

[0015] The III-V compound semiconductor constituting the compound semiconductor layer (L) contains Ga (gallium) and As (arsenic). The III-V compound semiconductor may contain a trace amount of impurities (dopants) in addition to the III group elements (group 13 elements) and the V group elements (group 15 elements).

[0016] The group III elements constituting the III-V compound semiconductor include at least Ga, and may further include at least one selected from the group consisting of Al (aluminum) and In (indium). The group V elements constituting the III-V compound semiconductor include at least arsenic (As), and may further include phosphorus (P). An example of the compound semiconductor layer (L) includes GaAs. A part of Ga may be replaced by Al and / or In, and a part of As may be replaced by P and / or nitrogen (N).

[0017] The V group element constituting the III-V compound semiconductor may contain nitrogen (N), but typically does not contain nitrogen (N) or contains only a small amount of nitrogen (N). The ratio of nitrogen in the V group element may be in the range of 0 to 100 atomic %, and is typically 0 to 30 atomic % (for example, in the range of 0 to 20 atomic %, 0 to 10 atomic %, or 0 to 5 atomic %). In the plasma etching method of the present disclosure, the etching gas contains N2, and Ga in the compound semiconductor layer (L) reacts with N2 in the etching gas to generate GaN, thereby reducing the etching rate. When the V group element contains a large amount of nitrogen, Ga in the compound semiconductor layer (L) is less likely to react with a gas (etching gas) containing chlorine. As a result, the etching rate becomes too slow and the etching process is likely to become unstable. Therefore, compared with the case where the compound semiconductor layer (L) is GaAs, when the compound semiconductor layer (L) contains a certain amount of nitrogen, it may be difficult to increase the gas ratio of N2 in the etching gas. That is, when the compound semiconductor layer (L) contains a certain amount of nitrogen, increasing the gas ratio of N2 in the etching gas to form a forward tapered side surface may cause the etching process to become unstable. Therefore, when the group V element in the compound semiconductor layer (L) contains a large amount of nitrogen, the effect of the method of the present disclosure may be reduced. In other words, the method of the present disclosure is preferably used for a compound semiconductor layer (L) in which the ratio of nitrogen in the group V element is small. For example, the method of the present disclosure can be preferably used for a compound semiconductor layer (L) in which the ratio of nitrogen in the group V element is in the range of 0 to 30 atomic % (for example, in the range of 0 to 10 atomic % or in the range of 0 to 5 atomic %), and is particularly preferably used for a compound semiconductor layer (L) that does not contain nitrogen.

[0018] The plasma etching in step (ii) is performed using a mixed gas containing a chlorine-containing gas (chlorine-containing gas) and nitrogen gas as an etching gas. The etching gas is a gas that is introduced into the chamber during plasma etching. Plasma is generated by inputting energy into the etching gas.

[0019] (Method of manufacturing semiconductor device) The manufacturing method disclosed herein is a method for manufacturing a semiconductor device including a compound semiconductor layer (L) composed of a III-V group compound semiconductor. Hereinafter, this manufacturing method may be referred to as the "manufacturing method (PM)". The manufacturing method (PM) includes the same steps as the etching method (EM). Therefore, matters explained about the etching method (EM) can be applied to the manufacturing method (PM), and matters explained about the manufacturing method (PM) can be applied to the etching method (EM). Therefore, overlapping explanations may be omitted.

[0020] The manufacturing method (PM) includes the above-mentioned steps (i) and (ii). As in the etching method (EM), the plasma etching in step (ii) of the manufacturing method (PM) is performed using a mixed gas containing a chlorine-containing gas and a nitrogen gas as an etching gas.

[0021] In the manufacturing method (PM), a semiconductor device is manufactured using a substrate including a compound semiconductor layer (L). During the manufacturing process, the compound semiconductor layer (L) is etched.

[0022] There is no particular limitation on the semiconductor element manufactured by the manufacturing method (PM). The manufacturing method (PM) can be applied to any semiconductor element including a compound semiconductor layer (L). Examples of semiconductor elements manufactured by the manufacturing method (PM) include transistors such as HEMT and MESFET, and semiconductor lasers.

[0023] In the etching method (EM) and the manufacturing method (PM), in step (ii), the compound semiconductor layer (L) and the resist mask are both etched. The plasma etching in step (ii) is performed using a mixed gas containing a chlorine-containing gas and a nitrogen gas as an etching gas. By using such a mixed gas, the value of Vs / Vr (etching selectivity), which is the ratio of the etching rate Vs of the compound semiconductor layer to the etching rate Vr of the resist mask, can be reduced. By etching the semiconductor layer (L) and the resist mask together under conditions where the value of Vs / Vr is small, the gradient α(s) of the slope constituting the forward tapered shape can be made smaller. Therefore, according to the method of the present disclosure, it is possible to form various forward tapered shapes. The method of the present disclosure is particularly preferably used when it is necessary to form a shape (for example, a forward tapered shape) having a slope with an acute gradient α(s) in the compound semiconductor layer (L).

[0024] (Items common to etching method (EM) and manufacturing method (PM)) The substrate used in the method of the present disclosure may include layers other than the compound semiconductor layer (L) and the resist mask. When manufacturing a semiconductor device, the substrate may include layers necessary for constituting the semiconductor device. Of course, after the step (ii) is completed, at least a part of a layer other than the compound semiconductor layer (L) may be formed. The layer other than the compound semiconductor layer (L) is selected according to the type of semiconductor device to be formed. After the step (ii) is completed, the resist mask may be removed as necessary.

[0025] The resist mask is a mask that is etched by the plasma etching in step (ii). A known resin mask may be used as the resist mask. An example of the resin mask includes a photoresist mask. An example of the material of the resin resist mask includes a novolac resin.

[0026] The openings in the resist mask are formed in the areas where the compound semiconductor layer (L) is to be etched. The compound semiconductor layer (L) is etched from the openings in the resist mask. When the resist mask is etched, the openings widen, and the compound semiconductor layer (L) is also etched in the widened openings.

[0027] In the plasma etching in step (ii), etching (anisotropic etching) is usually performed by applying a bias voltage to the generated plasma. The high frequency power and the bias voltage applied to generate the plasma can be appropriately selected from appropriate ranges.

[0028] The gas used to generate the plasma, i.e., the gas introduced into the chamber where the plasma is generated, contains a chlorine-containing gas and nitrogen gas (N2) as described above. By changing the flow rate ratio of the chlorine-containing gas and the nitrogen gas, the etching selectivity (Vs / Vr) can be changed. As a result, the gradient α(s) of the slope that constitutes the forward tapered shape can be changed.

[0029] There is no particular limitation on the apparatus for carrying out the etching method (EM) and the manufacturing method (PM), and they can be carried out using a known plasma etching apparatus. For example, an inductively coupled plasma etching apparatus (ICP etching apparatus) may be used.

[0030] The gas containing chlorine (chlorine-containing gas) may contain at least one gas selected from the group consisting of BCl3 (boron trichloride gas) and Cl2 (chlorine gas). The chlorine-containing gas may be, for example, only chlorine gas, only boron trichloride gas, or a mixture thereof.

[0031] In step (ii), the volume ratio of the gases constituting the mixed gas may be controlled so that the ratio Vs / Vr, which is the ratio of the etching rate Vs of the compound semiconductor layer to the etching rate Vr of the resist mask, is less than 1. Specifically, the ratio of the chlorine-containing gas to the nitrogen gas may be controlled so that the value of Vs / Vr is less than 1. With these configurations, the gradient α(s) of the slope constituting the forward tapered shape can be reduced. The value of Vs / Vr may be 0.1 or more and less than 1 (for example, in the range of 0.3 to 0.9 or 0.3 to 0.6).

[0032] The ratio (volume ratio) of the chlorine-containing gas to the entire etching gas may be in the range of 2 to 20% (for example, in the range of 3 to 5%). By decreasing the ratio of the chlorine-containing gas, the value of Vs / Vr can be decreased.

[0033] The gradient α(s) of the slope of the compound semiconductor layer (L) formed in step (ii) may be controlled by controlling the volume ratio of the gases constituting the mixed gas.

[0034] In the substrate in step (i), the angle (gradient α(r)) between one main surface of the compound semiconductor layer and the side surface of the resist mask may be in the range of 10° to 90°. The angle (gradient α(r)) may be in the range of 10° to 45°. By reducing the angle, the gradient of the inclined surface formed in the compound semiconductor layer (L) can be made smaller.

[0035] The volume ratio of the gases constituting the mixed gas may be controlled so that the slope gradient α(s) of the slope of the compound semiconductor layer (L) formed by step (ii) is 60° or less, 45° or less, 30° or less, or 12° or less. For example, by lowering the ratio of the chlorine-containing gas in the mixed gas, it is possible to lower the value of Vs / Vr (etching selectivity). As a result, it is possible to reduce the slope gradient.

[0036] The mixed gas may contain Ar gas. When the mixed gas contains Ar gas, the ion sputtering property is enhanced. As a result, it becomes possible to remove a layer (e.g., an oxide layer) that is present on the surface of the compound semiconductor layer (L) and that is difficult to etch, and it becomes possible to efficiently remove redeposited reaction products of nitrogen and carbon. Therefore, when the mixed gas contains Ar gas, it may be easier to smooth the sidewall surface of the compound semiconductor layer (L).

[0037] In the following, examples of embodiments according to the present disclosure will be specifically described with reference to the drawings. The method described below can be modified based on the above description. In addition, the matters described below may be applied to the above embodiment. In addition, in the embodiment described below, matters that are not essential to the method of the present disclosure may be omitted.

[0038] (Embodiment 1) In the first embodiment, an example of a plasma etching method (EM) will be described. First, as shown in FIG. 1A, a substrate 10 including a compound semiconductor layer 11 and a resist mask (resist pattern) 12 arranged on one main surface 11a of the compound semiconductor layer 11 is prepared. The compound semiconductor layer 11 is the above-mentioned compound semiconductor layer (L). The compound semiconductor layer 11 may be a compound semiconductor substrate. That is, the substrate 10 may include a compound semiconductor substrate and a resist mask 12 formed on one main surface of the compound semiconductor substrate. Alternatively, the substrate 10 may include a layer other than the compound semiconductor layer 11.

[0039] The resist mask 12 has openings 12h (through holes). The compound semiconductor layer 11 is exposed in the openings 12h. The resist mask 12 can be formed by a known method. For example, first, a resist film is formed on one main surface 11a by a spin coating method or the like. Next, the resist film is patterned by a photolithography / etching process or the like. In this manner, the resist mask 12 having the predetermined openings 12h can be formed.

[0040] The thickness of the resist mask 12 may be selected depending on the etching rate Vs of the compound semiconductor layer 11, the etching rate Vr of the resist mask 12, and the shape to be formed by etching (the shape of the compound semiconductor layer 11). Usually, the thickness of the resist mask 12 is selected so that a part of the resist mask 12 remains when the step (ii) is completed. In one example, the thickness of the resist mask 12 may be in the range of 0.4 μm to 1.2 μm. When the compound semiconductor layer 11 is to be deeply etched, the resist mask 12 may be made accordingly thick. For example, the thickness of the resist mask 12 may be thicker than 1.2 μm, or may be 2 μm or more.

[0041] The resist mask 12 has a side surface 12s facing the opening 12h. The side surface 12s has an acute angle gradient α(r) with respect to one main surface 11a of the compound semiconductor layer 11. A portion 12p of the resist mask 12 sandwiched between the two side surfaces 12s has a forward tapered shape. That is, the resist mask 12 includes a portion 12p having a forward tapered shape. Here, the forward tapered shape is, for example, a shape that becomes thinner as it moves away from the center of the compound semiconductor layer 11 in the thickness direction. The portion 12p may be in the shape of an elongated ridge, or in the shape of a quadrangular pyramid or a truncated cone.

[0042] The method for forming the opening 12h with an acute angle of gradient α is not particularly limited, and any known method may be used. For example, the opening 12h may be formed by adjusting exposure conditions and development conditions using photolithography. In addition, the gradient α(r) may be made even more acute by baking a resist pattern formed by photolithography or the like.

[0043] Conventionally, in order to obtain a forward tapered processed shape, it has been considered desirable to make the gradient of the resist mask formed by photolithography or the like as small as possible. For this reason, the resist mask shape has been controlled by baking or the like after the resist mask is formed, but there has been an issue with the stability of shape control. The method disclosed herein can control the gradient α(s) by controlling the volume ratio of the gases that make up the etching gas, without relying too much on the gradient α(r) of the resist mask.

[0044] 1B, the resist mask 12 and the compound semiconductor layer 11 are etched to form a slope 11s constituting a forward tapered shape in the compound semiconductor layer 11. The etching of the resist mask 12 and the compound semiconductor layer 11 is performed by exposing the compound semiconductor layer 11 and the resist mask 12 to plasma. The above-mentioned mixed gas is used as an etching gas for the plasma etching.

[0045] 1B, the outer edge 12x of the resist mask 12 before etching is indicated by a dotted line. Also shown in FIG. 1B is the gradient α(s) of the slope 11s of the compound semiconductor layer 11. The gradient α(s) is the gradient of the slope 11s with respect to a plane Sf perpendicular to the thickness direction Ds of the substrate 10.

[0046] The gradient α(s) is less than 90°. The surface of such a sloping surface 11s can be seen from the one principal surface 11a side. On the other hand, the surface of a sloping surface that forms an inverted taper shape cannot be seen from the one principal surface 11a side.

[0047] Of the portions removed by plasma etching, a recess 11v is formed in a portion sandwiched between two adjacent slopes 11s. The recess 11v is a recess whose opening area increases with increasing distance from the center of the compound semiconductor layer 11 in the thickness direction.

[0048] In the compound semiconductor layer 11, a portion 11p sandwiched between two slopes 11s has a forward tapered shape. That is, the compound semiconductor layer 11 includes the portion 11p having a forward tapered shape. The portion 11p may have a ridge shape, a quadrangular pyramid shape, or a circular cone shape.

[0049] In the manufacturing method (PM) of a semiconductor device, a part of the structure of the semiconductor device is formed by etching the compound semiconductor layer (L) using the above-mentioned etching method (EM). Other steps are not particularly limited and may be performed using known techniques.

[0050] (Plasma Etching Equipment) An example of an apparatus used in the plasma etching in step (ii) is shown in FIG. 2. The apparatus 100 in FIG. 2 includes a chamber 110, an upper electrode (antenna) 121, a first high frequency power supply 122, a first matching circuit 123, a substrate stage 131, a second high frequency power supply 132, a second matching circuit 133, a pressure regulator 141, a gas flow control unit 150, a control device 170, and a pressure gauge (not shown). The control device 170 is connected to devices that need to be controlled, and performs the control required for plasma etching. In FIG. 1, only a part of the connection between the control device 170 and the devices is shown. Since known devices can be applied to the devices included in the apparatus 100, detailed description is omitted. In addition, as long as the method of the present invention can be implemented, these devices and configurations (including arrangement) can be changed.

[0051] The chamber 110 is a chamber capable of maintaining the inside in a reduced pressure state. The chamber 110 includes a gas inlet 110a, a gas outlet 110b, and a dielectric window 111. The dielectric window 111 is made of a dielectric material (e.g., aluminum nitride, alumina, quartz, etc.). An upper electrode 121 is disposed adjacent to the dielectric window 111.

[0052] The substrate 10 to be plasma etched in the apparatus 100 is placed on the substrate stage 131. The substrate stage 131 is connected to a second high frequency power supply 132, and also functions as a lower electrode.

[0053] The pressure regulator 141 is connected to the gas exhaust port 110b and reduces the pressure inside the chamber 110. A vacuum pump or the like is used as the pressure regulator 141. The pressure regulator 141 may include a pressure adjustment valve or the like. The apparatus 100 includes a pressure gauge for monitoring the pressure inside the chamber 110. The control device 170 controls the pressure regulator 141 based on the output of the pressure gauge to adjust the pressure inside the chamber 110.

[0054] A gas supply source 201 (e.g., a gas cylinder) of the gas to be supplied into the chamber 110 is connected to the gas flow control unit 150. The control device 170 controls the gas flow control unit 150 to adjust the flow rate of each gas. The gas flow control unit 150 includes a mass flow controller (MFC) disposed in a flow path of each gas to be supplied. The gas supplied from the gas supply source 201 is introduced into the chamber 110 through the gas flow control unit 150 and the gas inlet 110a. FIG. 2 shows an example of an apparatus in which three types of gas are used.

[0055] The chamber 110 includes a mechanism (e.g., an opening / closing mechanism) for loading and unloading the substrate 10 (not shown). When performing plasma etching using the apparatus 100, first, the substrate 10 is placed on the substrate stage 131. Next, the pressure inside the chamber 110 is reduced by the pressure adjusting device 141, and a predetermined gas is introduced into the chamber 110 from the gas supply source 201. At this time, the pressure inside the chamber 110 is adjusted to a desired pressure as described above.

[0056] The pressure in the chamber 110 when performing plasma etching is not particularly limited, and a pressure suitable for the plasma etching may be selected. In one example, the pressure in the chamber 110 may be set in the range of 0.4 Pa to 5 Pa.

[0057] The above-mentioned multiple gases are introduced into the chamber 110. That is, a mixed gas is introduced into the chamber 110. The composition ratio (volume ratio) of the gases constituting the mixed gas can be controlled by adjusting the flow rate of each gas constituting the mixed gas by the gas flow rate control unit 150. The flow rate ratio of the gases introduced into the chamber 110 can be regarded as the composition ratio of the mixed gas. The composition ratio of the gases constituting the mixed gas and other etching conditions may be changed during etching.

[0058] Next, a high frequency power is applied to the upper electrode 121 by the first high frequency power supply 122 to generate plasma in the chamber 110. The substrate 10 is exposed to the generated plasma, and plasma etching is performed. During plasma etching, a bias voltage is usually applied by the second high frequency power supply 132. In this way, the resist mask 12 and the compound semiconductor layer 11 are simultaneously etched. There is no particular limitation on the power input to the upper electrode 121 and the lower electrode (substrate stage 131), and an appropriate power may be selected. In one example, a high frequency power in the range of 400 W to 1000 W at 13.56 MHz is applied to the upper electrode 121. By increasing the high frequency power input to the upper electrode 121, the plasma density can be increased, and more etchants (Cl radicals in the case of Cl2 and BCl3) can be obtained, enabling high-speed etching. By increasing the bias voltage, it is possible to extract chlorine ions from the plasma, which increases the etching speed and also improves the anisotropic etching property.

[0059] By changing the etching selectivity (Vs / Vr), it is possible to change the shape formed in the compound semiconductor layer 11 by etching. An example of the etching process when the etching selectivity Vs / Vr is changed is shown in Figs. 3 to 5. Figs. 3 to 5 show the stepwise change from the initial shape of the substrate 10 to the shape of the substrate 10 at the end of etching. Note that the diagrams shown in Figs. 3 to 5 are schematic diagrams for easy understanding and may differ from the actual shape. Also, the results shown in Figs. 3 to 5 are the results when a bias voltage is applied.

[0060] 3 to 5 are schematic diagrams showing examples of changes in the shape of the substrate 10 due to changes in the etching selectivity ratio Vs / Vr. In FIGS. 3 to 5, the shape of the substrate 10 changes in accordance with the progress of plasma etching, as indicated by the arrows. In FIGS. 3 to 5, the outer edge 12x of the initial resist mask 12 is shown by a dotted line. Also, FIGS. 3 to 5 show an example in which the resist mask 12 includes a portion having a forward tapered shape.

[0061] An example of the change in the shape of the substrate 10 due to etching when the etching selectivity ratio Vs / Vr=1 is shown in Fig. 3. As shown in Fig. 3, both the compound semiconductor layer 11 and the resist mask 12 are simultaneously etched by plasma etching. As a result, a portion 11p having a forward tapered shape is finally formed in the compound semiconductor layer 11. Fig. 3 also shows the recession width Br of the resist mask 12.

[0062] An example of the change in the shape of the substrate 10 due to etching when the etching selectivity ratio Vs / Vr>1 is shown in Fig. 4. As shown in Fig. 4, when Vs / Vr>1, the angle of the gradient α(s) of the slope 11s becomes larger than the gradient α(s) in Fig. 3.

[0063] An example of the change in the shape of the substrate 10 due to etching when the etching selectivity ratio Vs / Vr<1 is shown in FIG. 5. In this case, the recession width Br of the resist mask 12 increases. As shown in FIG. 5, when Vs / Vr<1, the angle of the gradient α(s) of the slope 11s becomes smaller than the gradient α(s) in FIG. 3.

[0064] 6 to 8 show the results of plasma etching when a mixed gas of BCl3 gas and N2 gas is used as the etching gas for plasma etching. Also, FIG. 9 to FIG. 11 show the results of plasma etching when a mixed gas of Cl2 gas, N2 gas and Ar gas is used as the etching gas for plasma etching. FIG. 6 to FIG. 11 show the results when a GaAs substrate is etched as the compound semiconductor layer 11. FIG. 6 and FIG. 9 show the relationship between the etching rate Vs of the GaAs substrate and the etching rate Vr of the resist mask 12 and the flow rate ratio of the gas. FIG. 7 and FIG. 10 show the relationship between the etching selectivity (Vs / Vr) and the flow rate ratio of the gas. FIG. 8 and FIG. 11 show the relationship between the gradient α(s) of the formed slope 11s and the flow rate ratio of the gas. In the following figures, "GaAs_E / R" represents the etching rate of the GaAs substrate, and "PR_E / R" represents the etching rate of the resist mask 12.

[0065] The results shown in Figures 6 to 11 were obtained by using a resist mask 12 in which the gradient α(r) of the side surface 12s is an acute angle. Plasma was generated by applying a high frequency power of 800 W at 13.56 MHz to the upper electrode. A bias voltage of 100 W was applied during plasma etching. The pressure in the chamber was set to 1.0 Pa.

[0066] As shown in Figures 6 and 9, the lower the proportion of the chlorine-containing gas, the smaller the etching selectivity ratio. Also, by including N2 gas in the mixed gas, the etching selectivity ratio could be made smaller than 1. As a result, as shown in Figures 9 and 11, the gradient α(s) of the slope 11s could be made 12° or less. To reduce the gradient α(s) of the slope 11s, it is preferable that the gradient α(r) of the side surface 12s of the resist mask 12 is 45° or less. To further reduce the gradient α(s), it is preferable that the gradient α(r) be an even more acute angle.

[0067] Also, etching was performed similarly to the etching in Figures 9 to 11, except that N2 gas and Ar gas were replaced with N2 gas. That is, the same etching was performed using a mixed gas of Cl2 gas and N2 gas as the etching gas. Even when Ar gas was not added, the same results as in Figures 9 to 11 were obtained as long as the flow rate ratio of Cl2 gas to the total flow rate of the mixed gas was the same.

[0068] On the other hand, when the mixed gas does not contain N2 gas, the etching selectivity ratio becomes larger (for example, 1 or more), and the gradient α(s) becomes larger. The reason for this is not clear at present, but it can be considered as follows. When a compound semiconductor layer (L) containing Ga and As is plasma etched, the relatively light As is easily removed. When the mixed gas does not contain N2 gas, Ga is easily removed following the removal of As. On the other hand, when the mixed gas contains N2 gas, it is considered that Ga present in the compound semiconductor layer (L) reacts with nitrogen in the etching gas to generate GaN, etc. As a result, the etching rate Vs of the compound semiconductor layer (L) may decrease. In addition, when the mixed gas contains N2 gas, the etching rate Vr of the resist mask may increase due to the reaction between the resist mask and nitrogen.

[0069] The results of etching a GaAs substrate by changing the high frequency power applied to the upper electrode 121 to generate plasma and the high frequency power applied to the lower electrode to apply a bias voltage are shown in Figs. 12 and 13. Figs. 12 and 13 show the results when the high frequency power (ICP) applied to the upper electrode 121 is 960 W and the high frequency power (Bias) applied to the lower electrode is 120 W, and the results when the high frequency power (ICP) is 800 W and the high frequency power (Bias) is 100 W. A mixed gas of Cl2 gas, N2 gas, and Ar gas was used as the etching gas for the plasma etching. The relationship between the gas flow rate ratio and the etching rate is shown in Fig. 12. The relationship between the gas flow rate ratio and the etching selectivity is shown in Fig. 13. When the high frequency power (ICP) is 960 W and the high frequency power (Bias) is 120 W, the etching selectivity Vs / Vr can be kept low while the etching rate Vs can be increased.

[0070] As a method for decreasing the etching rate Vs of the compound semiconductor layer (L), it is possible to decrease the power of the high frequency power applied to the upper electrode and the lower electrode. However, in that case, there is a problem that the plasma becomes unstable. In addition, even if Vs / Vr can be decreased, the processing takes time because Vs is small, and there is a problem that the productivity decreases. According to the method of the present disclosure, it is possible to decrease the etching selectivity ratio Vs / Vr under the condition that the plasma can be generated stably. Also, according to the method of the present disclosure, as shown in FIG. 12 and FIG. 13, it is possible to achieve both a relatively high Vs (for example, Vs>98 nm / min) and Vs / Vr<1, so that the productivity can be improved. [Industrial Applicability]

[0071] The present disclosure can be used in a plasma etching method and a method for manufacturing a semiconductor device. [Explanation of symbols]

[0072] 10: Substrate 11: Compound semiconductor layer 11a: One principal surface 11s: Slope 12: Resist mask 12h: opening 12s: Side 110: Chamber Vr: Etching rate Vs: Etching rate α : Gradient

Claims

1. A method for plasma etching a compound semiconductor layer made of a III-V compound semiconductor, comprising the steps of: (i) placing a substrate including the compound semiconductor layer and a resist mask having an opening and disposed on one main surface of the compound semiconductor layer in a chamber; and (ii) exposing the compound semiconductor layer and the resist mask to plasma in the chamber to perform plasma etching of the compound semiconductor layer and the resist mask, thereby forming a slope constituting a forward tapered shape in the compound semiconductor layer; the III-V compound semiconductor includes Ga and As; The plasma etching in the step (ii) is performed using a mixed gas containing a chlorine-containing gas and a nitrogen gas as an etching gas, a volume ratio of gases constituting the mixed gas is controlled to thereby control the gradient of the slope of the compound semiconductor layer formed in the step (ii); Plasma etching method.

2. The chlorine-containing gas is BCl 3 and Cl 2 10. The plasma etching method of claim 1, further comprising at least one gas selected from the group consisting of:

3. 3. The plasma etching method according to claim 1, wherein in the step (ii), a volume ratio of gases constituting the mixed gas is controlled so that a value of Vs / Vr, which is a ratio of an etching rate Vs of the compound semiconductor layer to an etching rate Vr of the resist mask, is less than 1.

4. 4. The plasma etching method according to claim 1, wherein the mixed gas contains Ar gas.

5. A method for manufacturing a semiconductor device including a compound semiconductor layer made of a III-V group compound semiconductor, comprising: (i) placing a substrate including the compound semiconductor layer and a resist mask having an opening and disposed on one main surface of the compound semiconductor layer in a chamber; and (ii) exposing the compound semiconductor layer and the resist mask to plasma in the chamber to perform plasma etching of the compound semiconductor layer and the resist mask, thereby forming a slope constituting a forward tapered shape in the compound semiconductor layer; the III-V compound semiconductor includes Ga and As; The plasma etching in the step (ii) is performed using a mixed gas containing a chlorine-containing gas and a nitrogen gas as an etching gas, a gradient of the slope of the compound semiconductor layer formed in the step (ii) is controlled by a volume ratio of gases constituting the mixed gas. A method for manufacturing a semiconductor device.

6. The chlorine-containing gas is BCl 3 and Cl 2 The method for manufacturing a semiconductor device according to claim 5 , further comprising at least one gas selected from the group consisting of:

7. 7. The method for manufacturing a semiconductor element according to claim 5, wherein in the step (ii), a volume ratio of gases constituting the mixed gas is controlled so that a value of Vs / Vr, which is a ratio of an etching rate Vs of the compound semiconductor layer to an etching rate Vr of the resist mask, is less than 1.

8. The method for manufacturing a semiconductor device according to any one of claims 5 to 7, wherein the mixed gas contains Ar gas.

Citation Information

Patent Citations

  • Dry etching method

    JP1988136526A

  • Manufacture of surface emission semiconductor laser

    JP1998294528A

  • Dry etching method

    JP2002151466A

  • Method and apparatus for dry etching

    JP2003100710A

  • Manufacturing method for semiconductor device

    JP2018200970A