Adhesive sheets for semiconductor processing
The adhesive sheet for semiconductor processing maintains low peeling forces through specific peel strength criteria and UV irradiation, addressing the issue of high-temperature adhesive residue and damage, ensuring reliable semiconductor processing.
Patent Information
- Application Number
- JP2019225599
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2019-12-13
- Publication Date
- 2024-09-24
- Estimated Expiration
- 2039-12-13
AI Technical Summary
Conventional UV-curable adhesive sheets for semiconductor processing lose peeling strength at high temperatures, leading to potential adhesive residue or damage during peeling after high-temperature processes.
The adhesive sheet is designed with specific peel strength criteria (Conditions A, B, C, D, and E) to maintain low peeling forces even after exposure to high temperatures, ensuring easy release without damaging the adherend, using UV irradiation and optional water peeling methods.
The adhesive sheet maintains effective adhesion and easy release properties, preventing adhesive residue and damage during high-temperature processes, ensuring reliable semiconductor processing.
Smart Images

Figure 0007555186000003 
Figure 0007555186000006 
Figure 0007555186000007
Abstract
Description
[Technical field]
[0001] The present invention relates to an adhesive sheet for semiconductor processing. [Background technology]
[0002] In the manufacturing process of semiconductor elements, a process of processing a semiconductor wafer on which a circuit is formed, such as grinding or cutting, is generally carried out in a state where an adhesive sheet (adhesive sheet for semiconductor processing) is attached to the circuit-formed surface side of the semiconductor wafer (adherend) in order to protect and fix the semiconductor wafer. For example, when grinding (backgrinding) the back surface of a semiconductor wafer, a backgrinding tape is used to protect the circuit-formed surface (front surface) of the semiconductor wafer and to hold (fix) the semiconductor wafer (for example, Patent Document 1). [Prior art documents] [Patent documents]
[0003] [Patent Document 1] JP 2017-212441 A Summary of the Invention [Problem to be solved by the invention]
[0004] After the backgrind tape and other adhesive sheets for semiconductor processing have achieved their intended purpose, they are peeled off from the adherend at a desired timing. From the viewpoint of preventing damage to the adherend at this time, the adhesive sheet for semiconductor processing is required to have easy peelability from the adherend. In order to realize such easy peelability, it is known to use an ultraviolet (UV) curable adhesive. The adhesive sheet for semiconductor processing using a UV curable adhesive is irradiated with UV at an appropriate timing before peeling from the adherend to reduce the peeling force, thereby suppressing damage to the adherend due to the load when peeling the adhesive sheet. However, when the conventional adhesive sheet for semiconductor processing using a UV curable adhesive is exposed to a high temperature condition of a predetermined temperature or higher after being attached to the adherend, the peeling force is difficult to reduce even if UV is irradiated thereafter, so it was difficult to apply it to a processing process (high temperature process) in which it is exposed to high temperatures. For example, there was a concern that peeling after a high temperature process would cause glue residue on the adherend or damage to the adherend due to the load during peeling.
[0005] The present invention has been created in view of the above circumstances, and has an object to provide an adhesive sheet for semiconductor processing that is suitable for use in applications including high-temperature processes. [Means for solving the problem]
[0006] The adhesive sheet for semiconductor processing disclosed herein includes an adhesive layer constituting an adhesive surface. In some embodiments of the adhesive sheet for semiconductor processing (hereinafter, sometimes simply referred to as "adhesive sheet"), the adhesive sheet is prepared by the following method: The adhesive surface was attached to a silicon wafer and subjected to heat treatment at 175°C for 15 minutes with an integrated light dose of 1000 mJ / cm 2 After the UV irradiation treatment, the peel strength is measured at a pulling speed of 300 mm / min and a peel angle of 180 degrees; Normal peel force Fd measured by a2 The normal peel strength Fd of the adhesive sheet is 0.50N / 20mm or less (hereinafter referred to as "Condition A"). a2 By limiting the above, the pressure-sensitive adhesive sheet can be peeled off with reduced load on the adherend even after exposure to high temperature conditions.
[0007] In some embodiments of the adhesive sheet for semiconductor processing disclosed herein, the adhesive sheet is prepared by the following method: The adhesive surface was attached to a silicon wafer and subjected to heat treatment at 175°C for 15 minutes with an integrated light dose of 1000 mJ / cm 2 After the UV irradiation treatment, water is supplied to the front of the pressure-sensitive adhesive sheet peeled off from the silicon wafer, and the peel strength is measured under the conditions of a pulling speed of 300 mm / min and a peel angle of 180 degrees; Water peel force Fw measured by a2 The water peel strength Fw of the adhesive sheet is 0.30 N / 20 mm or less (hereinafter referred to as "Condition B"). a2 By limiting the above, the PSA sheet can be peeled off with reduced load on the adherend even after exposure to high temperature conditions. PSA sheets that satisfy both condition A and condition B are preferred.
[0008] In some embodiments of the adhesive sheet for semiconductor processing disclosed herein, the adhesive sheet is prepared by the following method: The adhesive surface was attached to a silicon wafer and subjected to heat treatment at 200°C for 15 minutes with an integrated light dose of 1000 mJ / cm 2 After the UV irradiation treatment, the peel strength is measured at a pulling speed of 300 mm / min and a peel angle of 180 degrees; Normal peel force Fd measured by b2 The normal peel strength Fd of the adhesive sheet is 2.00N / 20mm or less (hereinafter referred to as "Condition C"). b2 By limiting the above, the PSA sheet can be peeled off with reduced load on the adherend even after being exposed to more severe high-temperature conditions.
[0009] In some embodiments of the adhesive sheet for semiconductor processing disclosed herein, the adhesive sheet is prepared by the following method: The adhesive surface was attached to a silicon wafer and subjected to heat treatment at 200°C for 15 minutes with an integrated light dose of 1000 mJ / cm 2After the UV irradiation treatment, water is supplied to the front of the pressure-sensitive adhesive sheet peeled off from the silicon wafer, and the peel strength is measured under the conditions of a pulling speed of 300 mm / min and a peel angle of 180 degrees; Water peel force Fw measured by b2 The water peel strength Fw of the adhesive sheet is 1.00 N / 20 mm or less (hereinafter referred to as "Condition D"). b2 By limiting condition C, the PSA sheet can be peeled off with reduced load on the adherend even after exposure to more severe high-temperature conditions. PSA sheets that satisfy both condition C and condition D are preferred.
[0010] In some embodiments of the adhesive sheet for semiconductor processing disclosed herein, the adhesive sheet has a normal peel strength Fd a2 [N / 20mm] and the above normal peel strength Fd except that the heat treatment is performed at 200°C for 15 minutes instead of the above 175°C for 15 minutes. a2 The normal peel force Fd is measured in the same manner as b2 [N / 20mm] and the following formula: Fd b2 -Fd a2 The normal peel strength difference calculated by (hereinafter also referred to as "normal peel strength difference after heating / UV") is 1.50 N / 20 mm or less (hereinafter also referred to as "Condition E"). This means that the adhesive sheet is less susceptible to the effects of uneven processing, such as temperature unevenness, in a high-temperature process.
[0011] In some embodiments of the adhesive sheet for semiconductor processing disclosed herein, the adhesive sheet is prepared by the following method: The adhesive surface is attached to a silicon wafer, and then the peel strength is measured at a pulling speed of 300 mm / min and a peel angle of 180 degrees; (hereinafter also referred to as "condition F.") Such a pressure-sensitive adhesive sheet exhibits appropriate adhesiveness as a pressure-sensitive adhesive sheet for semiconductor processing, and can favorably contribute to improved processability.
[0012] In some embodiments of the adhesive sheet for semiconductor processing disclosed herein, the adhesive sheet is prepared by the following method: The adhesive surface was attached to a silicon wafer, and the cumulative light intensity was 1000 mJ / cm 2 After the UV irradiation treatment, the peel strength is measured at a pulling speed of 300 mm / min and a peel angle of 180 degrees; Unheated normal peel force Fd measured by U1 (hereinafter, also referred to as "Condition G"). Such a pressure-sensitive adhesive sheet is used, for example, in semiconductor processing that does not include high-temperature processes, and can exhibit excellent easy peeling properties when peeled off after UV irradiation.
[0013] In some embodiments of the adhesive sheet for semiconductor processing disclosed herein, the adhesive sheet is prepared by the following method: The adhesive surface was attached to a silicon wafer, and the cumulative light intensity was 1000 mJ / cm 2 After the UV irradiation treatment, water is supplied to the front of the pressure-sensitive adhesive sheet peeled off from the silicon wafer, and the peel strength is measured under the conditions of a pulling speed of 300 mm / min and a peel angle of 180 degrees; Unheated water peel force Fw measured by U1 The adhesive strength is 0.05 N / 20 mm or less (hereinafter referred to as "Condition H"). Such a pressure-sensitive adhesive sheet is used, for example, in semiconductor processing that does not include high-temperature processes, and can be particularly effectively reduced stress on the adherend by peeling it off with a water peeling method after UV irradiation.
[0014] In addition, any suitable combination of the above-mentioned elements may also be included within the scope of the invention for which patent protection is sought through this patent application. [Brief description of the drawings]
[0015] [Figure 1] FIG. 2 is a cross-sectional view showing a schematic configuration example of a pressure-sensitive adhesive sheet. [Diagram 2] FIG. 4 is a cross-sectional view that illustrates a schematic configuration example of the pressure-sensitive adhesive sheet. [Diagram 3] FIG. 4 is a cross-sectional view that illustrates a schematic configuration example of the pressure-sensitive adhesive sheet. [Figure 4] FIG. 4 is a cross-sectional view that illustrates a schematic configuration example of the pressure-sensitive adhesive sheet. [Diagram 5] FIG. 4 is a cross-sectional view that illustrates a schematic configuration example of the pressure-sensitive adhesive sheet. [Figure 6] FIG. 4 is a cross-sectional view that illustrates a schematic configuration example of the pressure-sensitive adhesive sheet. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0016] A preferred embodiment of the present invention will be described below. Note that matters other than those specifically mentioned in this specification and necessary for carrying out the present invention can be understood by a person skilled in the art based on the teachings on carrying out the invention described in this specification and the common general knowledge at the time of filing. The present invention can be carried out based on the contents disclosed in this specification and the common general knowledge in the field. In addition, in the following drawings, components and parts having the same function may be described by using the same reference numerals, and duplicated descriptions may be omitted or simplified. In addition, the embodiments described in the drawings are schematic in order to clearly explain the present invention, and do not necessarily accurately represent the size or scale of the product actually provided.
[0017] In this specification, peeling a pressure-sensitive adhesive sheet from an adherend using an aqueous stripping liquid such as water (typically, peeling by supplying an aqueous stripping liquid to the peel front from the adherend) is sometimes referred to as "water peeling" or "water peeling method".
[0018] In this specification, the main chain of a polymer refers to the chain structure that forms the backbone of the polymer, and the side chain of a polymer refers to a group (pendant, side group) that is bonded to the main chain, or a molecular chain that can be considered as a pendant.
[0019] In this specification, the term "acrylic polymer" refers to a polymer derived from a monomer raw material containing more than 50% by weight (preferably more than 70% by weight, for example more than 90% by weight) of an acrylic monomer. The acrylic monomer refers to a monomer having at least one (meth)acryloyl group in one molecule. In this specification, "(meth)acryloyl" refers to acryloyl and methacryloyl in a comprehensive sense. Similarly, "(meth)acrylate" refers to acrylate and methacrylate, and "(meth)acrylic" refers to acrylic and methacrylic in a comprehensive sense.
[0020] In this specification, the term "active energy rays" is a concept that encompasses light such as ultraviolet rays, visible light, and infrared rays, as well as radiation such as α rays, β rays, γ rays, electron beams, neutron beams, and X-rays.
[0021] <Adhesive sheet configuration example> The pressure-sensitive adhesive sheet disclosed herein includes a pressure-sensitive adhesive layer. This pressure-sensitive adhesive layer typically constitutes at least one surface of the pressure-sensitive adhesive sheet. The pressure-sensitive adhesive sheet may be a substrate-attached pressure-sensitive adhesive sheet having a pressure-sensitive adhesive layer on one or both surfaces of a substrate (support), or may be a substrate-free pressure-sensitive adhesive sheet. The concept of the adhesive sheet here may include those called adhesive tapes, adhesive labels, adhesive films, etc. In addition, the above-mentioned adhesive layer is typically formed continuously, but is not limited to such a form, and may be an adhesive layer formed in a regular or random pattern such as a dotted or striped pattern. In addition, the adhesive sheet provided by the present specification may be in the form of a roll or a sheet. Alternatively, it may be an adhesive sheet in the form of a processed form into various shapes.
[0022] The adhesive sheet disclosed herein may have a cross-sectional structure, for example, as shown in Fig. 1 to Fig. 6. Among these, Fig. 1 and Fig. 2 show an example of the structure of a substrate-attached adhesive sheet (substrate-attached single-sided adhesive sheet). The adhesive sheet 1 shown in Fig. 1 has a structure in which an adhesive layer 21 is provided on one side 10A (non-releasable) of a substrate 10, and a surface (adhesive surface) 21A of the adhesive layer 21 is protected by a release liner 31, at least the adhesive layer side of which is a release surface. The adhesive sheet 2 shown in Fig. 2 has a structure in which an adhesive layer 21 is provided on one side 10A (non-releasable) of a substrate 10. In this adhesive sheet 2, the other side 10B of the substrate 10 is a release surface, and when the adhesive sheet 2 is rolled up, the adhesive layer 21 comes into contact with the other side 10B, and the surface (adhesive surface) 21A of the adhesive layer is protected by the other side 10B of the substrate 10.
[0023] 3 and 4 are configuration examples of a double-sided adhesive type substrate-attached pressure-sensitive adhesive sheet (substrate-attached double-sided pressure-sensitive adhesive sheet). The pressure-sensitive adhesive sheet 3 shown in FIG. 3 has a configuration in which a pressure-sensitive adhesive layer (first pressure-sensitive adhesive layer) 21 and a pressure-sensitive adhesive layer (second pressure-sensitive adhesive layer) 22 are provided on the first surface 10A and the second surface 10B (both of which are non-releasable) of the substrate 10, respectively, and the surface (first adhesive surface) of the first pressure-sensitive adhesive layer 21 and the surface (second adhesive surface) of the second pressure-sensitive adhesive layer 22 are protected by release liners 31 and 32, at least the pressure-sensitive adhesive layer side of which is a release surface. The pressure-sensitive adhesive sheet 4 shown in FIG. 4 has a configuration in which a first pressure-sensitive adhesive layer 21 and a second pressure-sensitive adhesive layer 22 are provided on the first surface 10A and the second surface 10B (both of which are non-releasable), respectively, of the substrate 10, and the surface (first adhesive surface) of the first pressure-sensitive adhesive layer 21 is protected by a release liner 31, both of which are release surfaces. The adhesive sheet 4 can be configured so that the second adhesive surface is also protected by the release liner 31 by rolling up the adhesive sheet 4 and abutting the surface (second adhesive surface) of the second adhesive layer 22 against the back surface of the release liner 31.
[0024] 5 and 6 are configuration examples of a substrate-less double-sided adhesive sheet (substrate-less double-sided adhesive sheet). The adhesive sheet 5 shown in FIG. 5 has a configuration in which one surface (first adhesive surface) 21A and the other surface (second adhesive surface) 21B of the substrate-less adhesive layer 21 are protected by release liners 31 and 32, at least the adhesive layer side being the release surface. The adhesive sheet 6 shown in FIG. 6 has a configuration in which one surface (first adhesive surface) 21A of the adhesive layer 21 is protected by a release liner 31, both of which are release surfaces, and when this is rolled up, the other surface (second adhesive surface) 21B of the adhesive layer 21 abuts against the back surface of the release liner 31, so that the other surface 21B is also protected by the release liner 31. A substrate-less or substrate-attached double-sided PSA sheet can be used as a substrate-attached single-sided PSA sheet by laminating a non-releasable substrate to one of the adhesive surfaces.
[0025] The pressure-sensitive adhesive sheet before use (before attachment to an adherend) may be in the form of a pressure-sensitive adhesive sheet with a release liner, in which the adhesive surface is protected by a release liner, as shown in, for example, Figures 1 to 6. The release liner is not particularly limited, and examples that can be used include release liners in which the surface of a liner substrate such as a resin film or paper has been release-treated, and release liners made of low-adhesion materials such as fluorine-based polymers (polytetrafluoroethylene, etc.) and polyolefin-based resins (polyethylene, polypropylene, etc.). For the release treatment, for example, a silicone-based or long-chain alkyl-based release treating agent can be used. In some embodiments, a release-treated resin film can be preferably used as the release liner.
[0026] When the pressure-sensitive adhesive sheet disclosed herein is in the form of a substrate-attached double-sided pressure-sensitive adhesive sheet or a substrate-less double-sided pressure-sensitive adhesive sheet, the pressure-sensitive adhesive (first pressure-sensitive adhesive) constituting the first adhesive surface and the pressure-sensitive adhesive (second pressure-sensitive adhesive) constituting the second adhesive surface may have the same composition or different compositions. A substrate-less double-sided pressure-sensitive adhesive sheet having different compositions on the first adhesive surface and the second adhesive surface can be realized, for example, by a multilayered pressure-sensitive adhesive layer in which two or more pressure-sensitive adhesive layers having different compositions are directly laminated (without a substrate).
[0027] The adhesive sheet disclosed herein preferably has an adhesive surface constituted by an adhesive layer having active energy ray curability (active energy ray curable adhesive layer). In the case of a double-sided adhesive sheet having a first adhesive surface and a second adhesive surface, it is preferable that at least one adhesive surface is an adhesive surface constituted by an active energy ray curable adhesive layer. The other adhesive surface may be an adhesive surface constituted by an active energy ray curable adhesive layer, or may be an adhesive surface constituted by an adhesive layer not having active energy ray curability (non-active energy ray curable adhesive layer). The adhesive sheet disclosed herein may be preferably implemented in the form of a single-sided adhesive sheet with a substrate having an adhesive surface constituted by an active energy ray curable adhesive layer. The active energy ray curable adhesive layer preferably contains a compound A described later.
[0028] <Adhesive layer> The adhesive layer (preferably a UV-curable adhesive layer) constituting the adhesive surface of the adhesive sheet disclosed herein may be an adhesive layer containing one or more types of adhesive selected from various known adhesives such as acrylic adhesives, rubber adhesives (natural rubber, synthetic rubber, a mixture of these, etc.), silicone adhesives, polyester adhesives, urethane adhesives, polyether adhesives, polyamide adhesives, and fluorine adhesives. Here, the acrylic adhesive refers to an adhesive that uses an acrylic polymer as the base polymer. The same applies to rubber adhesives and other adhesives. In this specification, the "base polymer" of a PSA refers to the main component of the polymer contained in the PSA. In addition, in this specification, the "main component" refers to a component contained in the PSA at more than 50% by weight, unless otherwise specified.
[0029] (Acrylic adhesive layer) In some embodiments of the pressure-sensitive adhesive sheet disclosed herein, the pressure-sensitive adhesive layer may be an acrylic pressure-sensitive adhesive layer containing an acrylic pressure-sensitive adhesive as a main component. In a pressure-sensitive adhesive sheet having an acrylic pressure-sensitive adhesive layer, it is possible to preferably achieve both adhesive properties suitable for semiconductor processing and easy releasability by water peeling. The acrylic pressure-sensitive adhesive layer is also preferable from the viewpoint of easily imparting active energy ray curability, which will be described later.
[0030] As the acrylic adhesive, for example, one containing an acrylic polymer, which is a polymer of a monomer raw material containing an alkyl(meth)acrylate or a modified product thereof by chemical modification or the like, as a base polymer is preferable. As a constituent component of the monomer raw material, an alkyl(meth)acrylate having a linear or branched alkyl group having 1 to 20 carbon atoms at the ester terminal can be preferably used. Hereinafter, an alkyl(meth)acrylate having an alkyl group having X to Y carbon atoms at the ester terminal is referred to as "C X-Y It is sometimes written as "alkyl (meth)acrylate". It is often used because it has adhesive properties suitable for semiconductor processing applications. 1-20 As alkyl (meth)acrylate, C 1-14 (For example, C 1-12 ) alkyl (meth)acrylate is preferred. 1-20 As alkyl acrylate, C 1-20 (For example, C 1-14 , typically C 1-12 ) Alkyl acrylates are preferred.
[0031] C 1-20Non-limiting examples of alkyl (meth)acrylates include methyl (meth)acrylate, ethyl (meth)acrylate, propyl (meth)acrylate, isopropyl (meth)acrylate, n-butyl (meth)acrylate, isobutyl (meth)acrylate, s-butyl (meth)acrylate, pentyl (meth)acrylate, isopentyl (meth)acrylate, hexyl (meth)acrylate, heptyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, octyl (meth)acrylate, isooctyl (meth)acrylate, and ethylhexyl (meth)acrylate. Examples of the alkyl (meth)acrylate include ethyl acrylate, nonyl (meth)acrylate, isononyl (meth)acrylate, decyl (meth)acrylate, isodecyl (meth)acrylate, undecyl (meth)acrylate, dodecyl (meth)acrylate, tridecyl (meth)acrylate, tetradecyl (meth)acrylate, pentadecyl (meth)acrylate, hexadecyl (meth)acrylate, heptadecyl (meth)acrylate, octadecyl (meth)acrylate, nonadecyl (meth)acrylate, and eicosyl (meth)acrylate. These alkyl (meth)acrylates can be used alone or in combination of two or more. Examples of preferred alkyl (meth)acrylates include ethyl acrylate (EA), n-butyl acrylate (BA), 2-ethylhexyl acrylate (2EHA), and lauryl acrylate (LA). In some embodiments, the monomer feedstock comprises at least one of EA, BA, 2EHA and LA, preferably at least one of EA, BA and 2EHA, and more preferably at least one of BA and 2EHA.
[0032] In some embodiments, among the above monomer raw materials, C is used because it is easy to balance the properties. 1-20 The proportion of alkyl (meth)acrylate is usually 40% by weight or more, preferably more than 50% by weight, and may be, for example, 55% by weight or more, 60% by weight or more, 65% by weight or more, or 70% by weight or more. For the same reason, the proportion of C in the above monomer raw material is 1-20The proportion of alkyl (meth)acrylate is usually 99.9% by weight or less, and may be 99% by weight or less, or may be 98% by weight or less. From the viewpoint of facilitating the formation of a pressure-sensitive adhesive sheet suitable for easy peeling by supplying an aqueous stripping liquid to the peel front from the adherend, in some embodiments, C in the above-mentioned monomer raw material is 1-20 The proportion of alkyl (meth)acrylate may be, for example, 95% by weight or less, 85% by weight or less, less than 80% by weight, 70% by weight or less, or 65% by weight or less.
[0033] In some preferred embodiments, the alkyl (meth)acrylate is an alkyl (meth)acrylate A1 having an alkyl group having 9 or less carbon atoms at the ester end (i.e., C 1-9 The alkyl (meth)acrylate A1 may be used alone or in combination of two or more. In this way, the structure in which the length of the side chain alkyl group is limited tends to provide high cohesive strength capable of preventing adhesive residue to a high degree. For example, in a structure in which the side chain (typically the side chain terminal) of the polymer has a carbon-carbon double bond, the reaction of the carbon-carbon double bond can proceed smoothly during the curing treatment due to the limited length of the side chain alkyl group. In addition, due to the limited length of the side chain alkyl group, a pressure-sensitive adhesive sheet having a pressure-sensitive adhesive layer containing a polymer obtained from the monomer can be efficiently peeled off from the adherend by a peeling method in which an aqueous peeling liquid such as water is supplied to the peeling front from the adherend.
[0034] The proportion of the alkyl (meth)acrylate A1 in the entire monomer raw material is suitably about 30% by weight or more, and from the viewpoint of better exerting the action of the alkyl (meth)acrylate A1, it is preferably about 40% by weight or more, more preferably about 55% by weight or more. In some embodiments, the proportion of the alkyl (meth)acrylate A1 may be, for example, about 65% by weight or more, about 75% by weight or more, or about 80% by weight or more. In some other embodiments, the proportion of the alkyl (meth)acrylate A1 may be, for example, about 85% by weight or more, about 90% by weight or more, or about 95% by weight or more. The upper limit of the proportion of the alkyl (meth)acrylate A1 in the monomer raw material is not particularly limited, and is usually suitably 99.5% by weight or less, and can be, for example, 99% by weight or less. In some embodiments, for example, from the viewpoint of favorably exerting the effect of the carbon-carbon double bond in an adhesive layer containing a polymer having a carbon-carbon double bond, the proportion of the alkyl (meth)acrylate A1 in the entire monomer raw material is preferably about 95% by weight or less, more preferably about 90% by weight or less, may be about 85% by weight or less, may be about 75% by weight or less, or may be about 70% by weight or less.
[0035] The proportion of the alkyl (meth)acrylate A1 in the entire alkyl (meth)acrylate is suitably about 50% by weight or more, and from the viewpoint of favorably exerting the action of the alkyl (meth)acrylate A1, it is preferably about 70% by weight or more, more preferably about 80% by weight or more, may be about 90% by weight or more, may be about 95% by weight or more, or may be about 99% by weight or more. The upper limit of the proportion of the alkyl (meth)acrylate A1 in the entire alkyl (meth)acrylate is 100% by weight.
[0036] In some embodiments, the alkyl (meth)acrylate A1 may contain one or more alkyl (meth)acrylates A3 having an alkyl group with less than 7 carbon atoms at the ester end. A pressure-sensitive adhesive containing a polymer obtained from a monomer raw material containing the alkyl (meth)acrylate A3 is easy to provide a pressure-sensitive adhesive sheet that can be efficiently peeled off by a peeling method in which a peeling liquid such as water is supplied to the peeling front from the adherend. In addition, in an active energy ray-curable pressure-sensitive adhesive containing a polymer obtained from a monomer raw material containing the alkyl (meth)acrylate A3, a curing reaction due to irradiation with active energy rays can proceed favorably. From such a viewpoint, the number of carbon atoms of the alkyl group in the alkyl (meth)acrylate A3 is preferably 6 or less, more preferably 4 or less, and may be 3 or less or 2 or less. In addition, the number of carbon atoms of the alkyl group in the alkyl (meth)acrylate A3 may be 1 or more, and is preferably 2 or more from the viewpoint of adhesion to the adherend.
[0037] In an embodiment in which the monomer raw material contains an alkyl (meth)acrylate A3, the proportion of the alkyl (meth)acrylate A3 in the entire monomer raw material may be, for example, about 1% by weight or more, and is usually about 5% by weight or more. From the viewpoint of favorably expressing the action of the alkyl (meth)acrylate A3, it is preferably about 20% by weight or more, more preferably about 30% by weight or more, even more preferably about 40% by weight or more, and particularly preferably about 50% by weight or more, and may be, for example, 60% by weight or more, about 70% by weight or more, about 80% by weight or more, or about 90% by weight or more. The upper limit of the proportion of the alkyl (meth)acrylate A3 in the entire monomer raw material is not particularly limited, and is usually about 99% by weight or less, and can be, for example, 90% by weight or less. In some embodiments, for example, from the viewpoint of favorably exerting the action of the carbon-carbon double bond in a pressure-sensitive adhesive layer containing a polymer having the carbon-carbon double bond, the proportion of the alkyl (meth)acrylate A3 in the entire monomer raw material is preferably about 80% by weight or less, more preferably about 70% by weight or less, and even more preferably about 60% by weight or less. The above-mentioned embodiment may be, for example, an embodiment in which a reactive group for curing treatment or a functional group serving as a crosslinking point is introduced into the polymer.
[0038] The proportion of the alkyl (meth)acrylate A3 in the entire alkyl (meth)acrylate is suitably about 5% by weight or more, and from the viewpoint of favorably expressing the action of the alkyl (meth)acrylate A3, it is preferably about 20% by weight or more, more preferably about 35% by weight or more, even more preferably about 45% by weight or more, particularly preferably about 55% by weight or more, for example, it may be about 65% by weight or more, about 75% by weight or more, about 85% by weight or more, or about 90% by weight or more. The upper limit of the proportion of the alkyl (meth)acrylate A3 in the entire alkyl (meth)acrylate is 100% by weight, and may be, for example, about 98% by weight or less. In some embodiments, for example, in the case where the alkyl (meth)acrylate A2 described later is used in combination with the alkyl (meth)acrylate A3, from the viewpoint of favorably exhibiting its function, the proportion of the alkyl (meth)acrylate A3 in the total alkyl (meth)acrylate may be, for example, about 90% by weight or less, about 85% by weight or less, about 75% by weight or less, about 60% by weight or less, about 45% by weight or less, about 30% by weight or less, or about 15% by weight or less. The alkyl (meth)acrylate A3 may not be used.
[0039] In some embodiments, the alkyl (meth)acrylate may contain an alkyl (meth)acrylate A2 having an alkyl group having 7 or more carbon atoms at the ester end as the alkyl (meth)acrylate A1 or as a monomer different from the alkyl (meth)acrylate A1. The use of the alkyl (meth)acrylate A2 may be advantageous, for example, from the viewpoint of adhesion to an adherend. The number of carbon atoms of the alkyl group in the alkyl (meth)acrylate A2 is preferably 8 or more, and may be 9 or more. In addition, from the viewpoint of adhesion properties such as adhesive strength, the number of carbon atoms of the alkyl group in the alkyl (meth)acrylate A2 is preferably 14 or less, more preferably 12 or less, and even more preferably 10 or less, for example, 9 or less, and may be less than 9.
[0040] In an embodiment in which the monomer raw material contains an alkyl (meth)acrylate A2, the proportion of the alkyl (meth)acrylate A2 in the entire monomer raw material may be, for example, about 1% by weight or more, and is usually about 5% by weight or more. From the viewpoint of better exerting the action of the alkyl (meth)acrylate A2, it is preferably about 20% by weight or more, more preferably about 30% by weight or more, even more preferably about 40% by weight or more, and particularly preferably about 50% by weight or more, and may be, for example, 60% by weight or more, about 70% by weight or more, about 80% by weight or more, or about 90% by weight or more. The upper limit of the proportion of the alkyl (meth)acrylate A2 in the entire monomer raw material is not particularly limited, and is usually about 99.5% by weight or less, and can be, for example, about 99% by weight or less. In some embodiments, for example, from the viewpoint of favorably exerting the effect of the carbon-carbon double bond in an adhesive layer containing a polymer having a carbon-carbon double bond, the proportion of the alkyl (meth)acrylate A2 in the entire monomer raw material is preferably approximately 95% by weight or less, may be approximately 90% by weight or less, may be approximately 85% by weight or less, may be approximately 75% by weight or less, or may be approximately 70% by weight or less.
[0041] The proportion of the alkyl (meth)acrylate A2 in the total alkyl (meth)acrylate contained in the monomer raw material is suitably about 5% by weight or more, and from the viewpoint of favorably expressing the action of the alkyl (meth)acrylate A2, it is preferably about 20% by weight or more, more preferably about 35% by weight or more, and even more preferably about 45% by weight or more, for example, about 55% by weight or more, about 65% by weight or more, about 75% by weight or more, about 85% by weight or more, about 90% by weight or more, or about 95% by weight or more. The upper limit of the proportion of the alkyl (meth)acrylate A2 in the total alkyl (meth)acrylate is 100% by weight. In some embodiments, for example, in the case where the alkyl (meth)acrylate A3 is used in combination with the alkyl (meth)acrylate A2, from the viewpoint of favorably expressing its function, the ratio of the alkyl (meth)acrylate A2 to the whole alkyl (meth)acrylate may be, for example, about 95% by weight or less, about 90% by weight or less, about 80% by weight or less, about 70% by weight or less, about 60% by weight or less, about 45% by weight or less, about 30% by weight or less, about 20% by weight or less, about 10% by weight or less, or about 5% by weight or less. The alkyl (meth)acrylate A2 may not be used.
[0042] The monomer raw material used in the synthesis of the acrylic polymer may further contain a secondary monomer having copolymerizability with the alkyl (meth)acrylate as described above. The secondary monomer may be useful for introducing a crosslinking point into the acrylic polymer or for increasing the cohesive strength of the acrylic polymer. In addition, for example, in the monomer raw material used in the synthesis of a polymer having a carbon-carbon double bond, it is preferable to adopt, as the secondary monomer, a monomer having a functional group (hereinafter also referred to as "functional group A") that can react with the functional group (hereinafter also referred to as "functional group B") of the carbon-carbon double bond-containing monomer described later.
[0043] As the secondary monomer, for example, the following functional group-containing monomers can be used alone or in combination of two or more. Hydroxyl group-containing monomers: for example, hydroxyalkyl (meth)acrylates such as 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 3-hydroxypropyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate, (4-hydroxymethylcyclohexyl)methyl (meth)acrylate, etc.; unsaturated alcohols such as vinyl alcohol, allyl alcohol, etc.; ether compounds such as 2-hydroxyethyl vinyl ether, 4-hydroxybutyl vinyl ether, diethylene glycol monovinyl ether, etc. Carboxy group-containing monomers: for example, ethylenically unsaturated monocarboxylic acids such as acrylic acid (AA), methacrylic acid (MAA), crotonic acid, isocrotonic acid, etc.; ethylenically unsaturated dicarboxylic acids such as maleic acid, fumaric acid, itaconic acid, citraconic acid, etc. Acid anhydride group-containing monomers: for example, maleic anhydride, itaconic anhydride. Monomers having a nitrogen atom-containing ring: for example, N-vinyl-2-pyrrolidone, methyl-N-vinylpyrrolidone, vinylpyridine, vinylpyrazine, vinylpyrimidine, N-vinylpiperidone, N-vinylpiperazine, N-vinylpyrrole, N-vinylimidazole, N-vinyloxazole, N-vinylmorpholine, N-vinyl-3-morpholinone, N-vinyl-2-caprolactam, N-vinyl-1,3-oxazin-2-one, N-vinyl-3,5-morpholinedione, N-vinylpyrazole, N-vinylisoxazole, N-vinylthiazole, N-vinylisothiazole, N-(meth)acryloylmorpholine, N-(meth)acryloyl-2-pyrrolidone, N-(meth)acryloylpiperidine, N-(meth)acryloylpyrrolidine, and the like. Amide group-containing monomers: for example, (meth)acrylamide; N,N-dialkyl(meth)acrylamides such as N,N-dimethyl(meth)acrylamide, N,N-diethyl(meth)acrylamide, N,N-dipropyl(meth)acrylamide, N,N-diisopropyl(meth)acrylamide, N,N-di(n-butyl)(meth)acrylamide, and N,N-di(t-butyl)(meth)acrylamide; N-alkyl(meth)acrylamides such as N-ethyl(meth)acrylamide, N-isopropyl(meth)acrylamide, N-butyl(meth)acrylamide, and Nn-butyl(meth)acrylamide; N-vinyl carboxylic acid amides such as N-vinylacetamide; monomers having a hydroxyl group and an amide group, for example, N-(2-hydroxyethyl)(meth)acrylamide, N- N-hydroxyalkyl (meth)acrylamides such as (2-hydroxypropyl) (meth)acrylamide, N-(1-hydroxypropyl) (meth)acrylamide, N-(3-hydroxypropyl) (meth)acrylamide, N-(2-hydroxybutyl) (meth)acrylamide, N-(3-hydroxybutyl) (meth)acrylamide, and N-(4-hydroxybutyl) (meth)acrylamide; monomers having an alkoxy group and an amide group, for example, N-alkoxyalkyl (meth)acrylamide such as N-methoxymethyl (meth)acrylamide, N-methoxyethyl (meth)acrylamide, and N-butoxymethyl (meth)acrylamide; and N,N-dialkylaminoalkyl (meth)acrylamide such as N,N-dimethylaminopropyl (meth)acrylamide. Amino group-containing monomers: for example, aminoethyl (meth)acrylate, N,N-dimethylaminoethyl (meth)acrylate, t-butylaminoethyl (meth)acrylate. Monomers having a succinimide skeleton: for example, N-(meth)acryloyloxymethylene succinimide, N-(meth)acryloyl-6-oxyhexamethylene succinimide, N-(meth)acryloyl-8-oxyhexamethylene succinimide, and the like. Maleimides: for example, N-cyclohexylmaleimide, N-isopropylmaleimide, N-laurylmaleimide, N-phenylmaleimide, and the like. Itaconimides: for example, N-methylitaconimide, N-ethylitaconimide, N-butylitaconimide, N-octylitaconimide, N-2-ethylhexylitaconimide, N-cyclohexylitaconimide, N-laurylitaconimide, and the like. Epoxy group-containing monomers: for example, glycidyl (meth)acrylate, methyl glycidyl (meth)acrylate, allyl glycidyl ether. Cyano group-containing monomers: for example acrylonitrile, methacrylonitrile. Keto group-containing monomers: for example, diacetone (meth)acrylamide, diacetone (meth)acrylate, vinyl methyl ketone, vinyl ethyl ketone, allyl acetoacetate, vinyl acetoacetate. Alkoxysilyl group-containing monomers: for example, alkoxysilyl group-containing (meth)acrylates such as 3-(meth)acryloxypropyltrimethoxysilane, 3-(meth)acryloxypropyltriethoxysilane, 3-(meth)acryloxypropylmethyldimethoxysilane, and 3-(meth)acryloxypropylmethyldiethoxysilane; alkoxysilyl group-containing vinyl compounds such as vinyltrimethoxysilane and vinyltriethoxysilane; and the like. Amino group-containing monomers: for example, aminoethyl (meth)acrylate, N,N-dimethylaminoethyl (meth)acrylate, t-butylaminoethyl (meth)acrylate. Monomers having an epoxy group: for example, glycidyl (meth)acrylate, methyl glycidyl (meth)acrylate, allyl glycidyl ether. Monomers containing a sulfonic acid group or a phosphoric acid group: for example, styrene sulfonic acid, allyl sulfonic acid, sodium vinyl sulfonate, 2-(meth)acrylamido-2-methylpropanesulfonic acid, (meth)acrylamidopropanesulfonic acid, sulfopropyl (meth)acrylate, (meth)acryloyloxynaphthalenesulfonic acid, 2-hydroxyethyl acryloyl phosphate, etc. Isocyanate group-containing monomers: for example, 2-isocyanatoethyl (meth)acrylate, (meth)acryloyl isocyanate, m-isopropenyl-α,α-dimethylbenzyl isocyanate.
[0044] The amount of the functional group-containing monomer is not particularly limited, and may be appropriately selected so as to realize the desired cohesive force. Usually, from the viewpoint of achieving a good balance between cohesive force and other properties (e.g., adhesiveness), the amount of the functional group-containing monomer (when two or more functional group-containing monomers are used, the total amount of them) is appropriate to be 0.1% by weight or more of the entire monomer raw material, preferably 0.3% by weight or more, for example 1% by weight or more. In addition, the amount of the functional group-containing monomer may be, for example, 50% by weight or less of the entire monomer raw material, preferably 40% by weight or less, for example 35% by weight or less, may be 30% by weight or less, may be 25% by weight or less, or may be 20% by weight or less.
[0045] In some embodiments, the monomer raw material may contain a hydroxyl group-containing monomer as the functional group-containing monomer. The amount of the hydroxyl group-containing monomer used is not particularly limited, and may be, for example, 0.01% by weight or more, 0.1% by weight or more, 0.5% by weight or more, 1% by weight or more, 5% by weight or more, or 10% by weight or more of the entire monomer raw material. In some embodiments, the amount of the hydroxyl group-containing monomer used may be, for example, 50% by weight or less of the entire monomer raw material, and from the viewpoint of suppressing water absorption of the adhesive, it is usually appropriate to set it to 40% by weight or less, and may be 30% by weight or less, 25% by weight or less, or 20% by weight or less. In some embodiments, the amount of the hydroxyl group-containing monomer used may be 15% by weight or less, 10% by weight or less, or 5% by weight or less of the entire monomer raw material. Alternatively, the hydroxyl group-containing monomer may not be used.
[0046] In some embodiments, the monomer raw material may contain a carboxyl group-containing monomer as the functional group-containing monomer. The ratio of the carboxyl group-containing monomer in the entire monomer raw material used for the synthesis of the acrylic polymer may be, for example, 15% by weight or less, or 10% by weight or less, and is preferably 7% by weight or less from the viewpoint of suppressing water absorption of the adhesive layer during semiconductor processing, and may be 5% by weight or less, 3% by weight or less, 2% by weight or less, 1% by weight or less, 0.5% by weight or less, or less than 0.1% by weight. The monomer raw material may be substantially free of a carboxyl group-containing monomer. Here, substantially free of a carboxyl group-containing monomer means that a carboxyl group-containing monomer is not used at least intentionally. For example, in the monomer raw material used for preparing a polymer having a carbon-carbon double bond in a side chain, a configuration in which the ratio of the carboxyl group monomer is limited as described above may be preferably adopted.
[0047] In some embodiments, the monomer raw material may contain a monomer having a nitrogen atom as the functional group-containing monomer. The use of a monomer having a nitrogen atom may impart appropriate polarity to the adhesive. This may be advantageous in realizing an adhesive sheet suitable for easy peeling by supplying an aqueous stripping solution such as water. A preferred example of a monomer having a nitrogen atom is a monomer having a nitrogen atom-containing ring. As the monomer having a nitrogen atom-containing ring, from the viewpoint of compatibility and the like, N-vinyl type compounds (N-vinyl cyclic amides, etc.) such as N-vinyl-2-pyrrolidone and N-(meth)acryloyl type compounds such as N-(meth)acryloylmorpholine may be preferably used.
[0048] When a monomer having a nitrogen atom (e.g., a monomer having a nitrogen atom-containing ring) is used, the amount of the monomer having a nitrogen atom is not particularly limited, and may be, for example, 1% by weight or more, 2% by weight or more, 3% by weight or more, 5% by weight or more, or 7% by weight or more of the total monomer raw material. From the viewpoint of obtaining a higher effect, in some embodiments, the amount of the monomer having a nitrogen atom may be 10% by weight or more, 15% by weight or more, or 20% by weight or more of the total monomer raw material. In addition, from the viewpoint of easily balancing the properties, the amount of the monomer having a nitrogen atom is usually, for example, 40% by weight or less of the total monomer raw material, and may be 35% by weight or less, 30% by weight or less, or 25% by weight or less. In some embodiments, the amount of the monomer having a nitrogen atom may be, for example, 20% by weight or less, 15% by weight or less, 10% by weight or less, or 5% by weight or less of the total monomer raw material. Alternatively, the monomer having a nitrogen atom may not be used.
[0049] When the monomer raw material is used to prepare a polymer having a carbon-carbon double bond, it is preferable to use a functional group-containing monomer having a functional group (functional group A) that can react with a functional group (functional group B) of a compound having a carbon-carbon double bond described later as a secondary monomer. In such a case, the type of functional group-containing monomer is determined by the above-mentioned compound type. As the secondary monomer having functional group A, for example, a hydroxyl group-containing monomer, a carboxyl group-containing monomer, an epoxy group-containing monomer, or an isocyanate group-containing monomer is preferable, and a hydroxyl group-containing monomer is particularly preferable. By using a hydroxyl group-containing monomer as a secondary monomer, the acrylic polymer has a hydroxyl group. On the other hand, by using an isocyanate group-containing monomer as a compound having a carbon-carbon double bond, the hydroxyl group (functional group A) of the acrylic polymer reacts with the isocyanate group (functional group B) of the compound, and a carbon-carbon double bond derived from the compound is introduced into the acrylic polymer.
[0050] In addition, when a secondary monomer is used for the purpose of reacting with a compound having a carbon-carbon double bond, the amount of the secondary monomer (preferably a hydroxyl group-containing monomer) is about 1% by weight or more in the total monomer raw material from the viewpoint of easily obtaining a pressure-sensitive adhesive layer suitable for water peeling, preferably about 5% by weight or more, more preferably about 10% by weight or more, even more preferably about 12% by weight or more, for example about 14% by weight or more. In addition, in order to maintain good adhesive properties such as adhesion, the amount of the secondary monomer is about 40% by weight or less in the total monomer raw material, preferably about 30% by weight or less, more preferably about 20% by weight or less, for example about 15% by weight or less.
[0051] The monomer raw material used in the preparation of the acrylic polymer may contain a sub-monomer (hereinafter also referred to as a copolymerizable monomer) other than the functional group-containing monomer described above, for the purpose of increasing the cohesive strength of the acrylic polymer, etc. Non-limiting specific examples of the copolymerizable monomer include the following. Alkoxy group-containing monomers: for example, alkoxyalkyl (meth)acrylates (alkoxyalkyl (meth)acrylates) such as 2-methoxyethyl (meth)acrylate, 3-methoxypropyl (meth)acrylate, 2-ethoxyethyl (meth)acrylate, etc.; alkoxy(poly)alkylene glycol (meth)acrylates such as methoxyethylene glycol (meth)acrylate, methoxypolyethylene glycol (meth)acrylate, methoxypolypropylene glycol (meth)acrylate, etc. Vinyl esters: for example, vinyl acetate, vinyl propionate, etc. Vinyl ethers: for example, vinyl alkyl ethers such as methyl vinyl ether and ethyl vinyl ether. Aromatic vinyl compounds: for example, styrene, α-methylstyrene, vinyltoluene, etc. Olefins: For example, ethylene, butadiene, isoprene, isobutylene, etc. (Meth)acrylic acid esters having an alicyclic hydrocarbon group: for example, (meth)acrylates containing an alicyclic hydrocarbon group such as cyclopentyl (meth)acrylate, cyclohexyl (meth)acrylate, isobornyl (meth)acrylate, dicyclopentanyl (meth)acrylate, and adamantyl (meth)acrylate. Aromatic ring-containing (meth)acrylates: for example, aryl (meth)acrylates such as phenyl (meth)acrylate, aryloxyalkyl (meth)acrylates such as phenoxyethyl (meth)acrylate, and arylalkyl (meth)acrylates such as benzyl (meth)acrylate. Other examples include heterocyclic ring-containing (meth)acrylates such as tetrahydrofurfuryl (meth)acrylate, halogen atom-containing monomers such as vinyl chloride and fluorine atom-containing (meth)acrylates, organosiloxane chain-containing monomers such as silicone (meth)acrylates, and (meth)acrylic acid esters obtained from alcohols derived from terpene compounds. Such copolymerizable monomers can be used alone or in combination of two or more. The amount of such other copolymerizable monomers is not particularly limited and may be appropriately selected depending on the purpose and application, but is preferably 20% by weight or less (e.g., 2 to 20% by weight, typically 3 to 10% by weight) of the total monomer raw material of the acrylic polymer, for example.
[0052] In a preferred embodiment, the total proportion of alkoxyalkyl (meth)acrylate and alkoxypolyalkylene glycol (meth)acrylate in the monomer raw material is preferably limited to less than 20% by weight from the viewpoint of suppressing gelation. The total proportion of the alkoxyalkyl (meth)acrylate and alkoxypolyalkylene glycol (meth)acrylate is more preferably less than 10% by weight, even more preferably less than 3% by weight, and particularly preferably less than 1% by weight. In one embodiment, the monomer raw material is substantially free of alkoxyalkyl (meth)acrylate and alkoxypolyalkylene glycol (meth)acrylate (content 0 to 0.3% by weight). Similarly, in one embodiment, the monomer raw material may contain an alkoxy group-containing monomer at a ratio of less than 20% by weight, or may contain no alkoxy group-containing monomer. The amount of the alkoxy group-containing monomer in the monomer raw material is preferably less than 10% by weight, more preferably less than 3% by weight, and even more preferably less than 1% by weight. In a particularly preferred embodiment, the monomer raw material is substantially free of an alkoxy group-containing monomer (content of 0 to 0.3% by weight).
[0053] The method of polymerizing the monomer raw material is not particularly limited, and various polymerization methods known as a synthesis method for acrylic polymers, such as solution polymerization, emulsion polymerization, bulk polymerization, and suspension polymerization, can be appropriately adopted. For example, solution polymerization can be preferably adopted. As a monomer supply method when performing solution polymerization, a lump-sum charging method in which all monomer raw materials are supplied at once, a continuous supply (dropping) method, a divided supply (dropping) method, and the like can be appropriately adopted. The solvent (polymerization solvent) used in solution polymerization can be appropriately selected from conventionally known organic solvents. For example, any one solvent selected from aromatic compounds such as toluene (typically aromatic hydrocarbons); esters such as ethyl acetate and butyl acetate; aliphatic or alicyclic hydrocarbons such as hexane and cyclohexane; halogenated alkanes such as 1,2-dichloroethane; lower alcohols such as isopropyl alcohol (for example, monohydric alcohols having 1 to 4 carbon atoms); ethers such as tert-butyl methyl ether; ketones such as methyl ethyl ketone; and the like, or a mixed solvent of two or more solvents can be used. The polymerization temperature can be appropriately selected depending on the type of monomer and solvent used, the type of polymerization initiator, etc., and can be, for example, about 20°C to 120°C (typically 40°C to 80°C). According to solution polymerization, a polymerization reaction liquid in the form of a polymer of a monomer raw material dissolved in a polymerization solvent is obtained. The pressure-sensitive adhesive composition used for forming the pressure-sensitive adhesive layer can be preferably produced using the above-mentioned polymerization reaction liquid. The production of the pressure-sensitive adhesive composition using the above-mentioned polymerization reaction liquid can include, for example, chemical modification such as introduction of a carbon-carbon double bond to the polymer contained in the above-mentioned polymerization reaction liquid.
[0054] In the polymerization, a known or conventional thermal polymerization initiator or photopolymerization initiator may be used depending on the polymerization method, polymerization mode, etc. Examples of the thermal polymerization initiator include azo-based polymerization initiators, peroxide-based initiators, redox-based initiators formed by combining peroxides with reducing agents, and substituted ethane-based initiators. Examples of the photopolymerization initiator include α-ketol-based photoinitiators, acetophenone-based photoinitiators, benzoin ether-based photoinitiators, ketal-based photoinitiators, aromatic sulfonyl chloride-based photoinitiators, photoactive oxime-based photoinitiators, benzophenone-based photoinitiators, thioxanthone-based photoinitiators, and acylphosphinoxide-based photoinitiators. The polymerization initiator may be used alone or in appropriate combination of two or more.
[0055] The amount of the polymerization initiator used may be a normal amount, and may be selected, for example, from the range of about 0.005 to 1 part by weight (typically 0.01 to 1 part by weight) relative to 100 parts by weight of the total monomer raw materials. In addition, when the polymerization initiator is also used as a photoinitiator, the amount of the polymerization initiator used may be set taking this into consideration.
[0056] In the above polymerization, various conventionally known chain transfer agents (which may also be understood as molecular weight regulators or polymerization degree regulators) may be used as necessary. As the chain transfer agent, mercaptans such as n-dodecyl mercaptan, t-dodecyl mercaptan, thioglycolic acid, and α-thioglycerol may be used. Alternatively, a chain transfer agent that does not contain a sulfur atom (non-sulfur chain transfer agent) may be used. Specific examples of non-sulfur chain transfer agents include anilines such as N,N-dimethylaniline and N,N-diethylaniline; terpenoids such as α-pinene and terpinolene; styrenes such as α-methylstyrene and α-methylstyrene dimer; compounds having a benzylidenyl group such as dibenzylideneacetone, cinnamyl alcohol, and cinnamylaldehyde; hydroquinones such as hydroquinone and naphthohydroquinone; quinones such as benzoquinone and naphthoquinone; olefins such as 2,3-dimethyl-2-butene and 1,5-cyclooctadiene; alcohols such as phenol, benzyl alcohol, and allyl alcohol; and benzyl hydrogens such as diphenylbenzene and triphenylbenzene. The chain transfer agent can be used alone or in combination of two or more. When using a chain transfer agent, the amount of the agent can be, for example, about 0.01 to 1 part by weight based on 100 parts by weight of the monomer raw material. The technology disclosed herein can also be preferably implemented in an embodiment in which no chain transfer agent is used.
[0057] The molecular weight of the acrylic polymer is not particularly limited and can be set in an appropriate range according to the required performance. The weight average molecular weight (Mw) of the acrylic polymer is usually about 10 × 10 4 or more (e.g. 20×10 4 From the viewpoint of achieving a good balance between cohesive strength and adhesive strength, 4 It is appropriate to say that it is more than 40 × 10 4 It is preferable that the value is equal to or larger than 50×10 4 More than 55 x 10 is fine. 4The upper limit of the Mw of the acrylic polymer is not particularly limited. From the viewpoint of the coatability of the pressure-sensitive adhesive composition, the Mw of the acrylic polymer is usually about 500×10 4 It is appropriate to set the value to be equal to or less than 150×10. 4 It may be less than or equal to about 75×10 4 The above Mw may be the Mw of the acrylic polymer in either the pressure-sensitive adhesive composition or the pressure-sensitive adhesive layer. Here, Mw refers to a value calculated based on standard polystyrene obtained by gel permeation chromatography (GPC). As the GPC device, for example, a model named "HLC-8320GPC" (column: TSKgelGMH-H(S), manufactured by Tosoh Corporation) can be used. The same applies to the examples described later.
[0058] The acrylic pressure-sensitive adhesive layer may further contain a polymer other than the acrylic polymer as a sub-polymer, if necessary. Suitable examples of the sub-polymer include those other than the acrylic polymer among the various polymers exemplified as the polymer that can be contained in the pressure-sensitive adhesive layer. When the pressure-sensitive adhesive layer disclosed herein is an acrylic pressure-sensitive adhesive layer containing a sub-polymer in addition to the acrylic polymer, the content of the sub-polymer is suitably less than 100 parts by weight relative to 100 parts by weight of the acrylic polymer, preferably 50 parts by weight or less, more preferably 30 parts by weight or less, and even more preferably 10 parts by weight or less. The content of the sub-polymer may be 5 parts by weight or less, or 1 part by weight or less, relative to 100 parts by weight of the acrylic polymer. The technology disclosed herein may be preferably implemented, for example, in an embodiment in which 99.5 to 100% by weight of the polymer contained in the pressure-sensitive adhesive layer is an acrylic polymer.
[0059] (Non-acrylic adhesive layer) The adhesive layer constituting the adhesive surface in the adhesive sheet disclosed herein may be an adhesive layer having a polymer other than an acrylic polymer as a base polymer, i.e., a non-acrylic adhesive layer. The non-acrylic adhesive layer may further contain a sub-polymer other than the base polymer as necessary, in addition to the base polymer. In this case, the content of the sub-polymer in the non-acrylic adhesive layer may be selected from the above contents exemplified as the content of the sub-polymer in the acrylic adhesive layer. The non-acrylic adhesive layer may be an adhesive layer containing an acrylic polymer as a sub-polymer.
[0060] (glass transition temperature) The glass transition temperature (Tg) of the base polymer (e.g., acrylic polymer) of the adhesive layer constituting the adhesive surface is preferably about 15°C or lower. In some embodiments, the Tg is suitably 10°C or lower from the viewpoint of adhesion to the adherend (e.g., conformity to the surface shape of the adherend) and the like, and is preferably 0°C or lower, and may be -10°C or lower or -20°C or lower. In addition, from the viewpoint of the cohesiveness of the adhesive and the ease of easy peeling by water peeling, the Tg of the base polymer may be, for example, -75°C or higher, -60°C or higher, or -50°C or higher. In some embodiments, the Tg of the base polymer may be -45°C or higher, or -40°C or higher.
[0061] Here, in this specification, the glass transition temperature (Tg) of a polymer refers to the glass transition temperature calculated by the Fox formula based on the composition of the monomer raw materials constituting the polymer. The Fox formula is a relational expression between the Tg of a copolymer and the glass transition temperature Tgi of a homopolymer obtained by homopolymerizing each of the monomers constituting the copolymer, as shown below. 1 / Tg=Σ(Wi / Tgi) In the above Fox formula, Tg represents the glass transition temperature (unit: K) of the copolymer, Wi represents the weight fraction of monomer i in the copolymer (copolymerization ratio on a weight basis), and Tgi represents the glass transition temperature (unit: K) of the homopolymer of monomer i.
[0062] The glass transition temperature of the homopolymer used to calculate Tg is a value described in a publicly known document. For example, for the monomers listed below, the following values are used as the glass transition temperatures of the homopolymers of the monomers. 2-Ethylhexyl acrylate -70℃ n-Butyl acrylate -55℃ Isostearyl acrylate -18℃ Methyl methacrylate 105℃ Methyl acrylate 8℃ Ethyl acrylate -22℃ N-vinyl-2-pyrrolidone 54℃ N-Acryloylmorpholine 145℃ 2-Hydroxyethyl acrylate -15℃ 4-Hydroxybutyl acrylate -40℃ Acrylic acid 106℃ Methacrylic acid 228℃
[0063] For the glass transition temperatures of homopolymers of monomers other than those listed above, the values given in "Polymer Handbook" (3rd Edition, John Wiley & Sons, Inc., 1989) shall be used. When multiple values are given in this document, the highest value shall be used.
[0064] For monomers for which the glass transition temperature of the homopolymer is not described in the Polymer Handbook, the value obtained by the following measurement method shall be used (see JP 2007-51271 A). Specifically, 100 parts by weight of monomer, 0.2 parts by weight of azobisisobutyronitrile, and 200 parts by weight of ethyl acetate as a polymerization solvent are charged into a reactor equipped with a thermometer, a stirrer, a nitrogen inlet tube, and a reflux condenser, and stirred for 1 hour while passing nitrogen gas through. After removing oxygen from the polymerization system in this way, the temperature is raised to 63°C and reacted for 10 hours. Then, the mixture is cooled to room temperature to obtain a homopolymer solution with a solid concentration of 33% by weight. Then, the homopolymer solution is cast and applied onto a release liner, and dried to prepare a test sample (sheet-shaped homopolymer) with a thickness of about 2 mm. This test sample was punched out into a disk with a diameter of 7.9 mm, sandwiched between parallel plates, and subjected to a shear strain of 1 Hz using a viscoelasticity tester (ARES, Rheometrics Corporation). Viscoelasticity was measured in shear mode at a temperature range of -70 to 150°C and a heating rate of 5°C / min. The peak top temperature of tan δ was taken as the Tg of the homopolymer.
[0065] (Compound A) The adhesive layer (preferably a UV-curable adhesive layer) may contain a heat-resistant release agent as necessary. As the heat-resistant release agent, at least one compound A selected from the group consisting of surfactants and compounds having a polyoxyalkylene skeleton is used. By containing such a heat-resistant release agent in the adhesive layer, an effect of suppressing the phenomenon in which the peel strength of the adhesive sheet after UV irradiation increases due to exposure to high temperatures can be exhibited. For example, by containing a heat-resistant release agent in the adhesive layer, the normal peel strength Fd a2 , Fd b2 and water peeling force Fw a2 , Fw b2The reason for obtaining such an effect is not particularly limited, but generally, the adhesion between the adherend and the pressure-sensitive adhesive layer is promoted by exposure to high temperatures, and the peeling force may increase. However, the presence of a heat-resistant release agent on the surface of the pressure-sensitive adhesive layer suppresses the increase in peeling force, and the surfactant and the compound having a polyoxyalkylene skeleton used as the heat-resistant release agent all have a hydrophilic region, which makes them easily distributed unevenly on the surface of the pressure-sensitive adhesive layer, and therefore it is believed that the increase in peeling force is effectively suppressed. In addition, the heat-resistant release agent has a hydrophilic region as described above, and is easily distributed unevenly on the surface of the pressure-sensitive adhesive layer, and therefore it can also be useful as a water-peeling additive that promotes easy peeling of the pressure-sensitive adhesive sheet by water peeling after UV irradiation.
[0066] As the surfactant and the compound having polyoxyalkylene skeleton, one or more of known surfactants and compounds having polyoxyalkylene skeleton can be used without any particular limitation.Compound A is typically preferably contained in the adhesive layer in free form.It is to be noted that, among the above surfactants, compounds having polyoxyalkylene skeleton are present, and vice versa.
[0067] As the surfactant that can be used as compound A, known nonionic surfactants, anionic surfactants, cationic surfactants, etc. can be used. Among them, nonionic surfactants are preferable. The surfactants can be used alone or in combination of two or more.
[0068] Examples of nonionic surfactants include polyoxyethylene alkyl ethers such as polyoxyethylene lauryl ether, polyoxyethylene cetyl ether, polyoxyethylene stearyl ether, and polyoxyethylene oleyl ether; polyoxyethylene alkyl phenyl ethers such as polyoxyethylene octylphenyl ether and polyoxyethylene nonylphenyl ether; polyoxyethylene fatty acid esters such as polyoxyethylene monolaurate, polyoxyethylene monostearate, and polyoxyethylene monooleate; sorbitan monolaurate, sorbitan monopalmitate, sorbitan monostearate, and sorbitan monostearate. Examples of the nonionic surfactant include sorbitan fatty acid esters such as sorbitan stearate and sorbitan monooleate; polyoxyethylene sorbitan fatty acid esters such as polyoxyethylene sorbitan monolaurate, polyoxyethylene sorbitan monopalmitate, polyoxyethylene sorbitan monostearate, polyoxyethylene sorbitan tristearate, polyoxyethylene sorbitan triisostearate, polyoxyethylene sorbitan monooleate and polyoxyethylene sorbitan trioleate; polyoxyethylene glyceryl ether fatty acid esters; polyoxyethylene-polyoxypropylene block copolymers; and the like. The nonionic surfactant may be a reactive surfactant having a radical polymerizable functional group such as a propenyl group, a (meth)allyl group, a vinyl group, or a (meth)acryloyl group (for example, a nonionic reactive surfactant such as polyoxyethylene nonylpropenyl phenyl ether). These nonionic surfactants may be used alone or in combination of two or more. From the viewpoint of optimally exerting the effect of compound A being appropriately unevenly distributed on the surface of the adhesive layer and enhancing the performance stability of the adhesive sheet, it is preferable to use a nonionic surfactant that does not have a radically polymerizable functional group (that is, is nonreactive) as described above.
[0069] Examples of anionic surfactants include alkylbenzene sulfonates such as nonylbenzene sulfonate and dodecylbenzene sulfonate (e.g., sodium dodecylbenzene sulfonate); alkyl sulfates such as lauryl sulfate (e.g., sodium lauryl sulfate, ammonium lauryl sulfate) and octadecyl sulfate; fatty acid salts; polyoxyethylene alkyl ether sulfates such as polyoxyethylene octadecyl ether sulfate and polyoxyethylene lauryl ether sulfate (e.g., sodium polyoxyethylene alkyl ether sulfate); polyoxyethylene alkyl phenyl ether sulfates such as polyoxyethylene lauryl phenyl ether sulfate (e.g., polyoxyethylene alkyl phenyl ether ammonium sulfate); polyoxyethylene alkyl ether phosphates such as polyoxyethylene stearyl ether phosphate and polyoxyethylene lauryl ether phosphate; polyoxyethylene alkyl ether phosphate salts such as sodium salts and potassium salts of the above polyoxyethylene alkyl ether phosphates; sulfosuccinates such as lauryl sulfosuccinate and polyoxyethylene lauryl sulfosuccinate (for example, sodium polyoxyethylene alkyl sulfosuccinate); polyoxyethylene alkyl ether acetates; and the like. When the anionic surfactant forms a salt, the salt may be, for example, a metal salt (preferably a salt of a monovalent metal) such as a sodium salt, a potassium salt, a calcium salt, or a magnesium salt, an ammonium salt, or an amine salt. The anionic surfactant may be used alone or in combination of two or more kinds. From the same viewpoint as the nonionic surfactant, a non-reactive anionic surfactant may be preferably used.
[0070] Examples of the cationic surfactant include polyether amines such as polyoxyethylene laurylamine, polyoxyethylene stearylamine, etc. The cationic surfactants may be used alone or in combination of two or more.
[0071] Examples of compounds having a polyoxyalkylene skeleton that can be used as compound A include polyalkylene glycols such as polyethylene glycol (PEG) and polypropylene glycol (PPG); polyethers containing polyoxyethylene units, polyethers containing polyoxypropylene units, compounds containing oxyethylene units and oxypropylene units (these units may be arranged randomly or in blocks); and derivatives thereof. In addition, compounds having a polyoxyalkylene skeleton among the above-mentioned nonionic, anionic, and cationic surfactants can also be used. These can be used alone or in combination of two or more. Among them, it is preferable to use a compound having a polyoxyethylene skeleton (also called a polyoxyethylene segment), and PEG is more preferable.
[0072] The molecular weight (chemical formula weight) of the compound having a polyoxyalkylene skeleton (e.g., polyethylene glycol) is not particularly limited. From the viewpoint of uniform mixing, it is appropriate that the molecular weight is, for example, less than 1000, and preferably about 600 or less (e.g., 500 or less). The lower limit of the molecular weight of the compound having a polyoxyalkylene skeleton (e.g., polyethylene glycol) is not particularly limited, and those having a molecular weight of about 100 or more (e.g., about 200 or more, and further about 300 or more) are preferably used.
[0073] The adhesive layer containing compound A is typically formed from an adhesive composition containing the compound A. The adhesive composition containing compound A can be preferably prepared by a method including adding compound A in a solvent-free form or in the form of an organic solvent solution. The above-mentioned solvent-free form refers to a form that is not diluted with an organic solvent or water that does not form an adhesive layer, and may be, for example, a form consisting of compound A. The organic solvent used for preparing the organic solvent solution can be appropriately selected from conventionally known organic solvents. Specific examples of such organic solvents include those similar to those used in solution polymerization described below. Suitable examples include ethyl acetate, a mixed solvent containing ethyl acetate (which may be a mixed solvent of ethyl acetate and toluene), toluene, and a mixed solvent containing toluene. For example, ethyl acetate or a mixed solvent containing ethyl acetate as a main component may be preferably used. In the case of a solvent-based or active energy ray-curable adhesive composition, from the viewpoint of preventing water from being brought into the adhesive composition, in some embodiments, it is preferable to add compound A in the form of an organic solvent solution that does not substantially contain water (for example, the content of water is less than 10 parts by weight, less than 5 parts by weight, or less than 1 part by weight relative to 100 parts by weight of compound A). This allows the formation of a more homogeneous pressure-sensitive adhesive layer.
[0074] In some embodiments, a nonionic compound is preferably used as compound A because it is easy to blend uniformly into the adhesive composition. A pressure-sensitive adhesive composition in which compound A is blended uniformly tends to form an adhesive layer in which compound A is uniformly present on the surface. This is preferable from the viewpoint of smoother peeling of the adhesive sheet from the adherend and reducing the load on the adherend caused by fluctuations in peel force (for example, vibrations and impacts associated with the fluctuations).
[0075] The HLB of compound A is not particularly limited. The HLB of compound A may be, for example, 1 or more or 3 or more. The HLB of compound A is preferably 5 or more, may be 6 or more, may be 8 or more, or may be 9 or more. This tends to favorably develop water peelability. The HLB of compound A is more preferably 10 or more, even more preferably 11 or more, even more preferably 12 or more, particularly preferably 13 or more, may be 14 or more, may be 15 or more, or may be 16 or more. Compound A having an HLB in the above range can more effectively develop light peelability by water peeling. The upper limit of the HLB is 20 or less, and may be, for example, 18 or less. In some embodiments, for example, from the viewpoint of compatibility, the HLB of compound A may be 16 or less, for example, 15 or less.
[0076] In this specification, HLB is the hydrophile-lipophile balance according to Griffin, which is a value indicating the degree of affinity of a surfactant to water or oil, and is a ratio of hydrophilicity to lipophilicity expressed as a number between 0 and 20. The definition of HLB is as described in WC Griffin: J. Soc. Cosmetic Chemists, 1, 311 (1949), Takahashi Kotami, Namba Yoshiro, Koike Motoo, and Kobayashi Masao, "Surfactant Handbook", 3rd Edition, Kogaku Toshosha Publishing, November 25, 1972, pp. 179-182, etc. Compound A having the above HLB can be selected based on the technical common sense of a person skilled in the art, by referring to the above reference literature as necessary.
[0077] In some cases, from the viewpoint of affinity with the aqueous stripping solution, the compound A preferably has two or more hydroxyl groups in one molecule, and more preferably has three or more hydroxyl groups in one molecule. Examples of the compound A having two or more hydroxyl groups in one molecule include sorbitan monoester, polyoxyalkylene sorbitan monoester, polyoxyalkylene glyceryl ether, polyoxyalkylene diglyceryl ether, polyoxyalkylene glyceryl ether monoester, etc. The upper limit of the number of hydroxyl groups that the compound A has in one molecule is not particularly limited, but from the viewpoint of solubility in an organic solvent and ease of preparation of the adhesive composition, it is usually appropriate that the number is 10 or less, preferably 8 or less, and may be 6 or less, or may be 4 or less.
[0078] In some cases, a nonionic compound having a fatty acid ester structure may be preferably selected as compound A from the viewpoint of solubility in an organic solvent (e.g., esters such as ethyl acetate). Compound A having a fatty acid ester structure may also be advantageous in terms of compatibility in the adhesive layer. For example, a compound A having a fatty acid ester structure may be preferably used as compound A to be contained in an acrylic adhesive layer. Examples of nonionic compounds having a fatty acid ester structure include sorbitan fatty acid esters, polyoxyalkylene fatty acid esters, polyoxyalkylene fatty acid monoesters, etc.
[0079] In some embodiments, compound A is preferably in the form of 100% solids and in a liquid state at room temperature (here, 25° C.) from the viewpoint of ease of preparation of an organic solvent solution. In some embodiments, Compound A is preferably one that dissolves without phase separation in the following Test II, and more preferably one that dissolves without phase separation in the following Test I. Note that the following Tests I and II are carried out using Compound A in the form of 100% solid content under a room temperature (23 to 25°C) environment. [Test I] 90 g of ethyl acetate and 10 g of compound A are placed in a 200 milliliter (mL) container, stirred with a glass rod for 1 minute, allowed to stand, and visually observed after 5 minutes for the presence or absence of phase separation. [Test II] 90 g of ethyl acetate and 10 g of compound A are placed in a 200 mL container and stirred with a glass rod for 1 minute, then treated with an ultrasonic disperser at 35 kHz for 10 minutes, stirred with a glass rod for another minute, allowed to stand, and visually observed after 5 minutes for the presence or absence of phase separation. As the ultrasonic dispersion device, a model named "ULTRASONIC CLEANER" manufactured by AS ONE or an equivalent product can be used.
[0080] The amount of compound A used is not particularly limited, and can be set so that the effect of use (for example, one or both of the effect of suppressing the phenomenon in which the peeling force of the adhesive sheet after UV irradiation increases due to exposure to high temperatures and the effect of promoting light peeling by water peeling) according to the purpose is appropriately exhibited. In some embodiments, the amount of compound A used may be, for example, about 5 parts by weight or less relative to 100 parts by weight of base polymer, and from the viewpoint of bonding reliability to the adherend and water resistance reliability at a stage where peeling is not intended, it is appropriate to set it to about 3 parts by weight or less, preferably less than 2 parts by weight, more preferably less than 1 part by weight, less than 0.8 parts by weight, less than 0.6 parts by weight, less than 0.4 parts by weight, less than 0.2 parts by weight, or less than 0.1 parts by weight. Compound A with a high HLB (for example, 5 or more, preferably 10 or more) tends to exhibit good water peeling properties even when added in a small amount. The amount of compound A relative to 100 parts by weight of base polymer can be, for example, 0.001 parts by weight or more, and from the viewpoint of making compound A uniformly present on the surface of the adhesive layer and smoother peeling of the adhesive sheet from the adherend, it is usually appropriate to make it 0.01 parts by weight or more, and preferably 0.03 parts by weight or more (for example, 0.1 parts by weight or more). In a composition that emphasizes water peelability, the amount of compound A relative to 100 parts by weight of base polymer may be 0.3 parts by weight or more (for example, 0.5 parts by weight or more).
[0081] (Crosslinking agent) In the adhesive layer (preferably a UV-curable adhesive layer), a crosslinking agent may be used as necessary for the purpose of adjusting the cohesive force, etc. The crosslinking agent may be included in the adhesive layer in a form after the crosslinking reaction, or in a form before the crosslinking reaction. The type of crosslinking agent is not particularly limited, and may be selected from conventionally known crosslinking agents so that the crosslinking agent exerts an appropriate crosslinking function in the adhesive layer, for example, according to the composition of the adhesive composition. Examples of crosslinking agents that can be used include isocyanate-based crosslinking agents, epoxy-based crosslinking agents, oxazoline-based crosslinking agents, aziridine-based crosslinking agents, carbodiimide-based crosslinking agents, melamine-based crosslinking agents, urea-based crosslinking agents, metal alkoxide-based crosslinking agents, metal chelate-based crosslinking agents, metal salt-based crosslinking agents, hydrazine-based crosslinking agents, and amine-based crosslinking agents. These may be used alone or in combination of two or more. In some preferred embodiments, at least an isocyanate-based crosslinking agent is used as the crosslinking agent. An isocyanate-based crosslinking agent may be used in combination with another crosslinking agent (for example, an epoxy-based crosslinking agent).
[0082] As the isocyanate-based crosslinking agent, a polyfunctional isocyanate compound having two or more functionalities can be used. For example, aromatic isocyanates such as tolylene diisocyanate, xylene diisocyanate, polymethylene polyphenyl diisocyanate, tris(p-isocyanatophenyl)thiophosphate, diphenylmethane diisocyanate, etc.; alicyclic isocyanates such as isophorone diisocyanate, etc.; aliphatic isocyanates such as hexamethylene diisocyanate, etc. can be mentioned. Examples of commercially available products include isocyanate adducts such as trimethylolpropane / tolylene diisocyanate trimer adduct (manufactured by Tosoh Corporation, product name "Coronate L"), trimethylolpropane / hexamethylene diisocyanate trimer adduct (manufactured by Tosoh Corporation, product name "Coronate HL"), and isocyanurate of hexamethylene diisocyanate (manufactured by Tosoh Corporation, product name "Coronate HX"), etc.
[0083] As the epoxy crosslinking agent, those having two or more epoxy groups in one molecule can be used without any particular limitation. An epoxy crosslinking agent having 3 to 5 epoxy groups in one molecule is preferable. Specific examples of the epoxy crosslinking agent include N,N,N',N'-tetraglycidyl-m-xylylenediamine, 1,3-bis(N,N-diglycidylaminomethyl)cyclohexane, 1,6-hexanediol diglycidyl ether, polyethylene glycol diglycidyl ether, polyglycerol polyglycidyl ether, and the like. Commercially available epoxy crosslinking agents include Mitsubishi Gas Chemical Company's product names "TETRAD-X" and "TETRAD-C", DIC Corporation's product name "Epicron CR-5L", Nagase ChemteX Corporation's product name "Denacol EX-512", Nissan Chemical Industries' product name "TEPIC-G", and the like.
[0084] As the oxazoline-based crosslinking agent, any agent having one or more oxazoline groups in one molecule can be used without any particular limitation. Examples of the aziridine crosslinking agent include trimethylolpropane tris[3-(1-aziridinyl)propionate], trimethylolpropane tris[3-(1-(2-methyl)aziridinylpropionate)], and the like. As the carbodiimide crosslinking agent, a low molecular weight compound or a high molecular weight compound having two or more carbodiimide groups can be used.
[0085] The metal chelate crosslinking agent may typically have a structure in which a polyvalent metal is covalently or coordinately bonded to an organic compound. Examples of the polyvalent metal atom include Al, Zr, Co, Cu, Fe, Ni, V, Zn, In, Ca, Mg, Mn, Y, Ce, Ba, Mo, La, Sn, and Ti. Among these, Al, Zr, and Ti are preferred. Examples of the organic compound include alkyl esters, alcohol compounds, carboxylic acid compounds, ether compounds, and ketone compounds. The metal chelate crosslinking agent may typically be a compound in which an oxygen atom in the organic compound is bonded (covalently or coordinately bonded) to the polyvalent metal.
[0086] In some embodiments, peroxides may be used as crosslinking agents. Examples of peroxides include di(2-ethylhexyl)peroxydicarbonate, di(4-t-butylcyclohexyl)peroxydicarbonate, di-sec-butylperoxydicarbonate, t-butylperoxyneodecanoate, t-hexylperoxypivalate, t-butylperoxypivalate, dilauroylperoxide, di-n-octanoylperoxide, 1,1,3,3-tetramethylbutylperoxyisobutyrate, and dibenzoylperoxide. Among these, examples of peroxides that are particularly excellent in crosslinking reaction efficiency include di(4-t-butylcyclohexyl)peroxydicarbonate, dilauroylperoxide, and dibenzoylperoxide. In addition, when peroxides are used as the polymerization initiator, it is also possible to use the remaining peroxides that are not used in the polymerization reaction in the crosslinking reaction. In this case, the remaining amount of peroxide is quantified, and if the ratio of peroxide is less than the predetermined amount, peroxide is added as necessary to reach the predetermined amount. The amount of peroxide can be quantified by the method described in Japanese Patent No. 4971517.
[0087] The amount of crosslinking agent used (the total amount when two or more crosslinking agents are used) is not particularly limited and can be appropriately set so as to obtain the desired effect of use. In a pressure-sensitive adhesive sheet having an adhesive surface constituted by an active energy ray curable pressure-sensitive adhesive layer, from the viewpoint of exhibiting appropriate cohesiveness before curing treatment by active energy rays, the amount of crosslinking agent used per 100 parts by weight of base polymer (e.g., acrylic polymer) is usually about 0.005 parts by weight or more, preferably about 0.01 parts by weight or more, may be about 0.05 parts by weight or more, may be about 0.1 parts by weight or more, or may be about 0.2 parts by weight or more. Increasing the amount of crosslinking agent used can be advantageous from the viewpoint of suppressing the phenomenon in which the peeling force after curing treatment increases due to exposure to high temperatures after application. From this viewpoint, in some embodiments, the amount of crosslinking agent used relative to 100 parts by weight of base polymer is preferably more than 0.3 parts by weight, more preferably more than 0.5 parts by weight, and may be more than 1.0 parts by weight, more than 1.5 parts by weight, more than 2.0 parts by weight, more than 3.0 parts by weight, or more than 4.0 parts by weight. In a PSA sheet that can be used in an embodiment that is peeled off with water after curing treatment with active energy rays, if the amount of crosslinking agent used is large, distortion due to cure shrinkage is more likely to be maintained until the time when the aqueous stripping solution is supplied, and the effect of light peeling by application of the water stripping method can be better exhibited. In addition, the amount of the crosslinking agent used relative to 100 parts by weight of the base polymer is usually about 15 parts by weight or less, and from the viewpoint of adhesion to the adherend during semiconductor processing and bonding reliability, it is preferably about 12 parts by weight or less, more preferably about 10 parts by weight or less. In some embodiments that place more importance on the initial normal peel strength Fd0, the amount of the crosslinking agent used relative to 100 parts by weight of the base polymer may be, for example, less than 7.0 parts by weight, less than 5.0 parts by weight, less than 3.0 parts by weight, less than 2.0 parts by weight, less than 1.0 parts by weight, or less than 0.5 parts by weight. In embodiments that contain a certain amount of compound A (for example, more than 0.2 parts by weight relative to 100 parts by weight of the base polymer), not using too much crosslinking agent can be advantageous from the viewpoint of suppressing a decrease in the initial normal peel strength Fd0 due to excessive uneven distribution of compound A on the surface of the pressure-sensitive adhesive layer.
[0088] In an embodiment using an isocyanate-based crosslinking agent as a crosslinking agent, the amount of the isocyanate-based crosslinking agent used relative to 100 parts by weight of the base polymer is usually about 0.005 parts by weight or more, preferably about 0.01 parts by weight or more, may be about 0.05 parts by weight or more, may be about 0.1 parts by weight or more, may be about 0.2 parts by weight or more, may be more than 0.3 parts by weight, may be more than 0.5 parts by weight, may be more than 1.0 parts by weight, may be more than 1.5 parts by weight, may be more than 2.0 parts by weight, may be more than 3.0 parts by weight, or may be more than 4.0 parts by weight. In a pressure-sensitive adhesive sheet that can be used in an embodiment that is peeled off with water after curing treatment with active energy rays, the effect of light peeling due to the application of the water peeling method can be better exhibited by increasing the amount of the isocyanate-based crosslinking agent used. In addition, the amount of the isocyanate-based crosslinking agent used per 100 parts by weight of the base polymer is usually about 15 parts by weight or less, and from the viewpoint of adhesion to the adherend during semiconductor processing and bonding reliability, it is preferably about 12 parts by weight or less, more preferably about 10 parts by weight or less, and may be less than 7.0 parts by weight, less than 5.0 parts by weight, less than 4.0 parts by weight, less than 3.0 parts by weight, less than 2.0 parts by weight, less than 1.0 parts by weight, or less than 0.5 parts by weight. In an embodiment containing a certain amount of compound A (for example, more than 0.2 parts by weight per 100 parts by weight of the base polymer), it is advantageous to not use too much isocyanate-based crosslinking agent from the viewpoint of suppressing the decrease in the initial normal peel strength Fd0 due to excessive uneven distribution of compound A on the surface of the adhesive layer.
[0089] A crosslinking catalyst may be used to promote the crosslinking reaction more effectively. Examples of the crosslinking catalyst include metal-based crosslinking catalysts such as tetra-n-butyl titanate, tetraisopropyl titanate, nursem ferric, butyltin oxide, and dioctyltin dilaurate. Among them, tin-based crosslinking catalysts such as dioctyltin dilaurate are preferred. The amount of the crosslinking catalyst used is not particularly limited. The amount of the crosslinking catalyst used relative to 100 parts by weight of the base polymer may be, for example, approximately 0.0001 parts by weight or more and 1 part by weight or less, 0.001 parts by weight or more and 0.1 parts by weight or less, or 0.005 parts by weight or more and 0.5 parts by weight or less.
[0090] (Polyfunctional Monomer) A polyfunctional monomer may be used in the adhesive layer as necessary. The polyfunctional monomer may be used in place of the crosslinking agent as described above or in combination with the crosslinking agent to serve the purpose of adjusting the cohesive strength. As the polyfunctional monomer, a compound having two or more carbon-carbon double bonds (for example, an ethylenically unsaturated group such as a (meth)acryloyl group) may be used. The polyfunctional monomer may be contained in the adhesive layer in an unreacted form, or may be contained in the adhesive layer in a reacted (crosslinked) form. The adhesive layer containing the unreacted polyfunctional monomer may be an active energy ray curable adhesive layer that can form a crosslinked structure by reacting the polyfunctional monomer by irradiating the adhesive layer with active energy rays such as ultraviolet rays.
[0091] Examples of the polyfunctional monomer include ethylene glycol di(meth)acrylate, propylene glycol di(meth)acrylate, polyethylene glycol di(meth)acrylate, polypropylene glycol di(meth)acrylate, neopentyl glycol di(meth)acrylate, pentaerythritol di(meth)acrylate, pentaerythritol tri(meth)acrylate, dipentaerythritol hexa(meth)acrylate, ethylene glycol di(meth)acrylate, 1,6-hexanediol di(meth)acrylate, 1,12-dodecanediol di(meth)acrylate, trimethylolpropane tri(meth)acrylate, tetramethylolmethane tri(meth)acrylate, allyl (meth)acrylate, vinyl (meth)acrylate, divinylbenzene, epoxy acrylate, polyester acrylate, urethane acrylate, butyl diol (meth)acrylate, and hexyl diol di(meth)acrylate. Among them, trimethylolpropane tri(meth)acrylate, 1,6-hexanediol di(meth)acrylate, and dipentaerythritol hexa(meth)acrylate can be preferably used. The polyfunctional monomers can be used alone or in combination of two or more.
[0092] The appropriate amount of polyfunctional monomer used varies depending on the molecular weight, the number of functional groups, etc., but is usually in the range of about 0.01 to 3.0 parts by weight relative to 100 parts by weight of base polymer (e.g., acrylic polymer). In some embodiments, the amount of polyfunctional monomer used relative to 100 parts by weight of base polymer may be, for example, 0.02 parts by weight or more, 0.1 parts by weight or more, 0.5 parts by weight or more, 1.0 parts by weight or more, or 2.0 parts by weight or more. By increasing the amount of polyfunctional monomer used, there is a tendency to obtain higher cohesive strength. On the other hand, from the viewpoint of avoiding a decrease in adhesion to the adherend or a decrease in the storage stability of the pressure-sensitive adhesive sheet due to an excessive increase in cohesive strength, the amount of polyfunctional monomer used relative to 100 parts by weight of base polymer may be, for example, 10 parts by weight or less, 5.0 parts by weight or less, or 3.0 parts by weight or less. Alternatively, polyfunctional monomer may not be used. For example, a pressure-sensitive adhesive layer containing a polymer having a structure (such as a carbon-carbon double bond or a benzophenone structure) that induces a crosslinking reaction upon irradiation with active energy rays may be a pressure-sensitive adhesive layer that is substantially free of unreacted polyfunctional monomers, or may be a pressure-sensitive adhesive layer formed from a pressure-sensitive adhesive composition that is substantially free of polyfunctional monomers. Here, the term "a pressure-sensitive adhesive composition that is substantially free of polyfunctional monomers" means that the amount of polyfunctional monomer relative to 100 parts by weight of the base polymer is less than 0.05 parts by weight (e.g., less than 0.01 parts by weight).
[0093] (Other optional ingredients) The adhesive layer (preferably a UV-curable adhesive layer) may contain, as necessary, various additives common in the field of adhesives, such as tackifier resins (e.g., rosin-based, petroleum-based, terpene-based, phenol-based, ketone-based, etc. tackifier resins), viscosity adjusters (e.g., thickeners), leveling agents, plasticizers, fillers, colorants such as pigments and dyes, stabilizers, preservatives, antioxidants, antiaging agents, etc., as other optional components. As for such various additives, those conventionally known can be used in the usual manner, and they do not particularly characterize the present invention, so detailed explanations will be omitted. From the viewpoint of achieving a good balance between adhesion to the adherend during semiconductor processing and peelability (e.g., peelability by water peeling) when removing the adherend, in some embodiments, the content of the tackifier resin in the adhesive layer can be, for example, less than 5 parts by weight, or even less than 3 parts by weight, less than 1 part by weight, less than 0.5 parts by weight, or less than 0.1 parts by weight, relative to 100 parts by weight of the base polymer. The adhesive layer may be substantially free of tackifier resin (for example, the content of the adhesive layer relative to 100 parts by weight of the base polymer is 0 to 0.05 parts by weight). Limiting the content of the tackifier resin in this way can be advantageous from the viewpoint of improving the curability of the active energy ray-curable adhesive layer, for example.
[0094] In some preferred embodiments, the adhesive layer may have a composition in which the content of the polymer (typically the base polymer) is about 80% by weight or more of the total weight of the adhesive layer. This can preferably achieve the effect of reducing the peeling force by applying water peeling (light peeling effect). From this viewpoint, the content of the polymer is preferably about 85% by weight or more of the total weight of the adhesive layer, more preferably about 90% by weight or more, and may be about 92% by weight or more, or may be about 95% by weight or more.
[0095] (Active energy ray curable adhesive layer) The adhesive layer constituting at least one adhesive surface of the adhesive sheet disclosed herein is preferably an adhesive layer (active energy ray curable adhesive layer) composed of an active energy ray curable adhesive. In particular, an active energy ray curable adhesive layer is preferably configured so that the peeling force from the adherend is reduced compared to before irradiation by irradiating active energy rays after application to the adherend. An adhesive sheet having such an active energy ray curable adhesive layer has good bonding reliability to the adherend before irradiation of active energy rays, and can quickly reduce the peeling force from the adherend by irradiation of active energy rays (preferably by supplying an aqueous stripping solution thereafter).
[0096] In addition, the active energy ray curable adhesive layer can be cured by irradiation with active energy rays while attached to an adherend, and then peeled off by a water peeling method, thereby effectively reducing the peeling force from the adherend. The reason for this is not particularly limited, but it is considered that when the active energy ray curable adhesive layer while attached to an adherend is irradiated with active energy rays, the adhesive layer undergoes rapid curing shrinkage, causing microscopic lifting from the adherend, or distortion accumulates in the adhesive layer, and when an aqueous peeling liquid is supplied in this state, the aqueous peeling liquid quickly penetrates into the interface between the adhesive layer and the adherend, effectively reducing the peeling force. By peeling off the adhesive sheet by a water peeling method after irradiation with active energy rays, a particularly remarkable light peeling effect can be achieved by the synergistic effect of the reduction in peeling force due to the curing of the adhesive layer and the reduction in water peeling force due to the above-mentioned rapid curing shrinkage.
[0097] A preferred example of an active energy ray-curable adhesive layer is one that exhibits curability by containing a carbon-carbon double bond in the adhesive layer. Carbon-carbon double bonds are chemically stable and do not react with moisture or acidity in the air in a normal storage environment that can be applied industrially. On the other hand, when active energy rays are irradiated to generate radicals, they react (for example, polymerization reaction or crosslinking reaction) and cure. A preferred active energy ray from the viewpoint of ease of handling, etc. is light (for example, ultraviolet light).
[0098] In the pressure-sensitive adhesive layer that exhibits curability by containing a carbon-carbon double bond, the form of the carbon-carbon double bond in the pressure-sensitive adhesive layer is not particularly limited. The carbon-carbon double bond can be contained in the pressure-sensitive adhesive layer in the form of, for example, a polymer having a carbon-carbon double bond (e.g., a base polymer) or a monomer having a carbon-carbon double bond (e.g., the unreacted multifunctional monomer as described above). These may be used alone or in combination of two or more.
[0099] The form of the carbon-carbon double bond contained in the polymer or the form of the carbon-carbon double bond contained in the monomer is not particularly limited. For example, the carbon-carbon double bond may be present in the polymer or monomer in the form of an ethylenically unsaturated group. Examples of the ethylenically unsaturated group include a (meth)acryloyl group, a vinyl group, an allyl group, and a methallyl group. From the viewpoint of reactivity, a (meth)acryloyl group is preferred.
[0100] (Polymers with carbon-carbon double bonds) In some embodiments, the active energy ray curable pressure-sensitive adhesive layer preferably contains a polymer having a carbon-carbon double bond. Hereinafter, the polymer having a carbon-carbon double bond is also referred to as "polymer (PD)". For example, a polymer (PD) having a carbon-carbon double bond in the form of an ethylenically unsaturated group is preferable. In some preferred embodiments, the polymer (PD) may be contained in the active energy ray curable pressure-sensitive adhesive layer as a base polymer of the pressure-sensitive adhesive layer. In some other embodiments, the polymer (PD) may be contained in the active energy ray curable pressure-sensitive adhesive layer as a subcomponent used in addition to a base polymer not containing a carbon-carbon double bond. The active energy ray curable pressure-sensitive adhesive layer may contain the polymer (PD) as a base polymer and further contain a monomer having a carbon-carbon double bond (e.g., an unreacted multifunctional monomer) as a subcomponent.
[0101] The form of the carbon-carbon double bond in the polymer (PD) is not particularly limited. The polymer (PD) may be a polymer having a carbon-carbon double bond in a side chain, or may be a polymer having a carbon-carbon double bond in the main chain. Here, having a carbon-carbon double bond in the main chain includes the presence of a carbon-carbon double bond in the main chain skeleton of the polymer (PD) and the presence of a carbon-carbon double bond at the end of the main chain. From the viewpoint of the reactivity of the carbon-carbon double bond, a polymer (PD) having a carbon-carbon double bond in a side chain can be preferably used. The method of incorporating a carbon-carbon double bond in the polymer (PD) is not particularly limited, and an appropriate method can be selected from among methods known to those skilled in the art.
[0102] The polymer (PD) is not particularly limited, and an appropriate polymer can be selected and used in consideration of the properties of the pressure-sensitive adhesive layer, etc. As the polymer (PD), a polymer (primary polymer) that does not contain carbon-carbon double bonds or has a lower content of carbon-carbon double bonds than the target substance, and a polymer (secondary polymer) in which carbon-carbon double bonds have been introduced by a method such as chemical modification can be preferably used.
[0103] A specific example of a method for introducing a carbon-carbon double bond into a primary polymer is to prepare a primary polymer in which a monomer having a functional group (functional group A) is copolymerized, and then react the primary polymer with a compound having a functional group (functional group B) capable of reacting with the functional group A and a carbon-carbon double bond in one molecule (hereinafter also referred to as a "functional group B-containing unsaturated compound") in such a way that the carbon-carbon double bond does not disappear. The reaction between functional group A and functional group B is preferably a reaction that does not involve the generation of radicals, such as a condensation reaction or an addition reaction.
[0104] Examples of the combination of functional group A and functional group B include a combination of a carboxy group and an epoxy group, a combination of a carboxy group and an aziridyl group, and a combination of a hydroxyl group and an isocyanate group. Among them, from the viewpoint of reaction tracing, a combination of a hydroxyl group and an isocyanate group is preferable. In addition, as for the combination of the functional groups A and B, as long as a polymer having a carbon-carbon double bond is obtained, one of the functional groups in the combination may be functional group A and the other may be functional group B, or one of the functional groups may be functional group B and the other may be functional group A. For example, in the combination of a hydroxyl group and an isocyanate group, the functional group A may be a hydroxyl group (in that case, the functional group B is an isocyanate group), or may be an isocyanate group (in that case, the functional group B is a hydroxyl group). Among them, a combination in which the primary polymer has a hydroxyl group and the compound has an isocyanate group is preferable. This combination is particularly preferable when the primary polymer is an acrylic polymer.
[0105] In addition, a method of using a vinyl alcohol-based polymer (typically polyvinyl alcohol) as the primary polymer and reacting the vinyl alcohol-based polymer (typically a vinyl alcohol-based polymer not containing a carbon-carbon double bond) with a vinyl halide such as vinyl bromide or an allyl halide such as allyl bromide is also cited as a suitable example of a method for obtaining a polymer having a carbon-carbon double bond. In this method, the reaction is carried out under suitable basic conditions, and a vinyl alcohol-based polymer containing a vinyl group in the side chain is obtained by the reaction. In addition, a method of preparing a polymer having a carbon-carbon double bond using a microorganism that produces a polymer as disclosed in Japanese Patent No. 4502363 may be adopted. The various conditions in this method, such as the microorganism species and the microorganism culture conditions, may be set by adopting the conditions described in the above patent publication, or by appropriately modifying them within the scope of the technical common sense of a person skilled in the art.
[0106] The moles of the functional group A (M A ) and moles of functional group B (M B ) molar ratio (M A / M B From the viewpoint of the reactivity of the two, the molar ratio (M A / M B For example, when the functional group A is used in another reaction (such as a crosslinking reaction with a crosslinking agent), the molar ratio (M A / M B It is preferable that the molar ratio (M A / M B ) may be, for example, 20 or less. In some embodiments, from the viewpoint of achieving a good balance between adhesion to an adherend before light irradiation and releasability from the adherend after light irradiation (for example, releasability by water stripping), the molar ratio (M A / M B ) is preferably 10 or less, may be 5.0 or less, may be 2.5 or less, may be 1.8 or less, may be 1.5 or less, or may be 1.3 or less.
[0107] The amount of the compound having a functional group B and a carbon-carbon double bond (hereinafter also referred to as the "functional group B-containing unsaturated compound") used is determined based on the above-mentioned molar ratio (M A / M B ) can be, for example, 1.0 parts by weight or more, 3.0 parts by weight or more, 5.0 parts by weight or more, or 7.0 parts by weight or more, relative to 100 parts by weight of the primary polymer having a functional group A, in order to achieve a higher level of both adhesion before light irradiation and peelability after light irradiation (for example, peelability by water peeling), in some embodiments, the amount of the functional group B-containing unsaturated compound used relative to 100 parts by weight of the primary polymer is preferably 9.0 parts by weight or more, more preferably 10 parts by weight or more, may be 12 parts by weight or more, may be 14 parts by weight or more, or may be 16 parts by weight or more. In addition, the amount of the functional group B-containing unsaturated compound used relative to 100 parts by weight of the primary polymer can be, for example, less than 40 parts by weight, and is usually appropriate to be less than 35 parts by weight, and is preferably less than 30 parts by weight, may be less than 25 parts by weight, or may be less than 20 parts by weight. In some embodiments, the amount of the unsaturated compound containing functional group B used per 100 parts by weight of the primary polymer may be less than 18 parts by weight, less than 16 parts by weight, less than 13 parts by weight, less than 10 parts by weight, or less than 7 parts by weight.
[0108] A suitable example of the polymer having a carbon-carbon double bond is, for example, an acrylic polymer having a (meth)acryloyl group introduced into the side chain. Such an acrylic polymer can be obtained, for example, by reacting an acrylic primary polymer having a hydroxyl group (functional group A) introduced by copolymerization with a compound having a carbon-carbon double bond and an isocyanate group (functional group B) in such a way that the carbon-carbon double bond does not disappear.
[0109] The polymer having a carbon-carbon double bond may be, for example, a diene-based polymer (typically a conjugated diene-based polymer). A diene-based polymer (typically a conjugated diene-based polymer) is typically a polymer obtained by polymerizing or copolymerizing a diene (typically a conjugated diene). Examples of the diene-based polymer (typically a conjugated diene-based polymer) include butadiene-based polymers such as polybutadiene and styrene-butadiene copolymer; isoprene-based polymers such as polyisoprene and styrene-isoprene copolymer; and chloroprene-based polymers such as polychloroprene.
[0110] Another example of the active energy ray curable adhesive layer is an adhesive layer containing a polymer having a structure that causes a crosslinking reaction by irradiation with active energy rays and has a structure other than a carbon-carbon double bond.For example, an adhesive containing a polymer having a benzophenone structure in a side chain can exhibit active energy ray curability by photocrosslinking using the benzophenone structure.As the polymer having a benzophenone structure in a side chain, an acrylic polymer having a benzophenone structure in a side chain can be preferably used.
[0111] (Photoinitiator) When ultraviolet rays are used as the active energy rays for curing the active energy ray-curable pressure-sensitive adhesive layer, it is preferable for the pressure-sensitive adhesive layer to contain a photoinitiator from the viewpoint of promoting the reaction or improving the efficiency of using light energy. Examples of the photoinitiator include benzoin ether-based photoinitiators, acetophenone-based photoinitiators, α-hydroxyketone-based photoinitiators, aromatic sulfonyl chloride-based photoinitiators, photoactive oxime-based photoinitiators, benzoin-based photoinitiators, benzyl-based photoinitiators, benzophenone-based photoinitiators, ketal-based photoinitiators, thioxanthone-based photoinitiators, α-aminoketone-based photoinitiators, acylphosphine oxide-based photoinitiators, etc. The photoinitiators can be used alone or in combination of two or more.
[0112] Examples of benzoin ether photoinitiators include benzoin methyl ether, benzoin ethyl ether, benzoin propyl ether, benzoin isopropyl ether, benzoin isobutyl ether, 2,2-dimethoxy-1,2-diphenylethan-1-one, and anisole methyl ether. Examples of acetophenone photoinitiators include 2,2-diethoxyacetophenone, 2,2-dimethoxy-2-phenylacetophenone, 1-hydroxy-cyclohexyl-phenyl ketone, 4-phenoxydichloroacetophenone, and 4-t-butyl-dichloroacetophenone. Examples of α-hydroxyketone photoinitiators include 2-hydroxy-2-methyl-1-phenyl-propan-1-one, 1-[4-(2-hydroxyethoxy)-phenyl]-2-hydroxy-2-methyl-1-propan-1-one, and the like. Examples of aromatic sulfonyl chloride photoinitiators include 2-naphthalenesulfonyl chloride, and the like. Examples of photoactive oxime photoinitiators include 1-phenyl-1,1-propanedione-2-(o-ethoxycarbonyl)-oxime. Examples of benzoin photoinitiators include benzoin. Examples of benzyl photoinitiators include benzyl. Examples of benzophenone photoinitiators include benzophenone, benzoylbenzoic acid, 3,3'-dimethyl-4-methoxybenzophenone, polyvinyl benzophenone, α-hydroxycyclohexyl phenyl ketone. Examples of ketal photoinitiators include benzyl dimethyl ketal. Examples of thioxanthone photoinitiators include thioxanthone, 2-chlorothioxanthone, 2-methylthioxanthone, 2,4-dimethylthioxanthone, isopropylthioxanthone, 2,4-dichlorothioxanthone, 2,4-diethylthioxanthone, 2,4-diisopropylthioxanthone, dodecylthioxanthone, etc. Examples of the α-aminoketone photoinitiator include 2-methyl-1-[4-(methylthio)phenyl]-2-morpholinopropan-1-one, 2-benzyl-2-dimethylamino-1-(4-morpholinophenyl)-butanone-1, and the like.Examples of the acylphosphine oxide photoinitiator include 2,4,6-trimethylbenzoyldiphenylphosphine oxide and bis(2,4,6-trimethylbenzoyl)-phenylphosphine oxide.
[0113] The photoinitiator may be a commercially available product, such as Omnirad 651, Omnirad 184, Omnirad 2959, Omnirad 907, Omnirad 369, Omnirad 1173, or Omnirad TPO, manufactured by IGM Regins.
[0114] In some embodiments, a photoinitiator that is difficult to decompose or generate radicals by heating may be preferably used as the photoinitiator. For example, a heat-resistant photoinitiator having a 10% weight reduction temperature of 200°C or higher may be used as the photoinitiator. By using such a heat-resistant photoinitiator, even if it is exposed to high temperatures before the curing treatment, the effect of reducing the peeling force by the curing treatment with active energy rays is not easily impaired. The 10% weight reduction temperature means the environmental temperature at which the weight of the photoinitiator is reduced by 10% by weight compared to the weight before the temperature increase (i.e., the weight of the photoinitiator is 90% by weight compared to the weight before the temperature increase) when the photoinitiator is placed under a nitrogen atmosphere and the environmental temperature is increased from 23°C to 300°C at a heating rate of 2°C / min. The 10% weight reduction temperature of the photoinitiator is more preferably 210°C or higher, and even more preferably 220°C or higher. Examples of photoinitiators having a 10% weight loss temperature in this range include those manufactured by IGM Regins under the trade names "Omnirad 369," "Omnirad 127," "Omnirad 379," and "Omnirad 819"; those manufactured by BASF Japan under the trade name "Irgacure OXE02"; those manufactured by Lamberti under the trade names "Esacure one" and "Esacure 1001m"; and those manufactured by Asahi Denka Kogyo Co., Ltd. under the trade names "ADEKA OPTOMER N-1414," "ADEKA OPTOMER N-1606," and "ADEKA OPTOMER N-1717."
[0115] The adhesive layer containing a photoinitiator can be formed using an adhesive composition containing the photoinitiator. The method of adding the photoinitiator to the adhesive composition is not particularly limited. For example, it is preferable to add and mix the photoinitiator into the adhesive composition, typically a liquid containing a polymer (polymer in which polymerization has been completed). In this method, the photoinitiator can be added to the composition together with other added components (e.g., a crosslinking agent, etc.). As another method, a method in which a polymerization initiator that can function as a photoinitiator is added during polymer polymerization is exemplified. In this method, the polymerization initiator is added so that a predetermined amount remains after polymerization. The remaining amount of the polymerization initiator (amount of the photoinitiator present) can be adjusted not only by the amount of the polymerization initiator added, but also by the polymer polymerization conditions, drying conditions and curing conditions during the formation of the adhesive layer, etc.
[0116] When the adhesive layer contains a photoinitiator, the content of the photoinitiator in the adhesive layer is not particularly limited and can be set so that the desired effect is appropriately exhibited. In some embodiments, the content of the photoinitiator may be, for example, about 0.05 parts by weight or more, preferably about 0.1 parts by weight or more, and more preferably about 0.5 parts by weight or more, relative to 100 parts by weight of the base polymer of the adhesive layer. The increase in the content of the photoinitiator improves the active energy ray curability of the adhesive layer. In some embodiments, the content of the photoinitiator relative to 100 parts by weight of the base polymer may be, for example, about 0.8 parts by weight or more, may be about 2.0 parts by weight or more, or may be about 2.5 parts by weight or more. In addition, the content of the photoinitiator relative to 100 parts by weight of the base polymer may be, for example, about 20 parts by weight or less, and is usually appropriate to be about 10 parts by weight or less, and is preferably about 8 parts by weight or less, may be about 6 parts by weight or less, or may be about 4 parts by weight or less. A not high content of photoinitiator is preferred from the viewpoint of storage stability of the pressure-sensitive adhesive layer pressure-sensitive adhesive sheet (for example, ability to suppress performance changes due to storage of the pressure-sensitive adhesive sheet before use).
[0117] <Formation of adhesive layer> The adhesive layer (preferably a UV-curable adhesive layer) constituting the adhesive surface of the adhesive sheet disclosed herein may be an adhesive layer formed from an adhesive composition containing a base polymer (e.g., an acrylic polymer) and, if necessary, other optional components. The adhesive composition may be in various forms, such as a solvent-based adhesive composition containing an adhesive (adhesive component) in an organic solvent, an active energy ray-curable adhesive composition prepared to be cured by active energy rays such as ultraviolet rays or radiation to form an adhesive, a water-dispersed adhesive composition in which an adhesive is dispersed in water, or a hot melt-type adhesive composition that is applied in a heated and molten state and forms an adhesive when cooled to around room temperature. The active energy-curable adhesive composition is typically a liquid composition that exhibits fluidity to an extent that it can be applied at room temperature (approximately 0°C to 40°C, for example, about 25°C) and is cured by irradiation with active energy to form an adhesive (viscoelastic body). The pressure-sensitive adhesive sheet according to some embodiments may have a pressure-sensitive adhesive layer formed using a solvent-based pressure-sensitive adhesive composition or an active energy ray-curable pressure-sensitive adhesive composition. As the pressure-sensitive adhesive composition for forming the active energy ray-curable pressure-sensitive adhesive layer, a solvent-based pressure-sensitive adhesive composition may be preferably used from the viewpoint of ease of controlling the active energy ray curability.
[0118] The adhesive layer of the adhesive sheet disclosed herein can be formed by applying (e.g., coating) an adhesive composition to a suitable surface, followed by a suitable curing treatment (drying, crosslinking, polymerization, etc.). When two or more types of curing treatments are performed, they can be performed simultaneously or in multiple stages. An adhesive layer having a multi-layer structure of two or more layers can be prepared by laminating adhesive layers that have been previously formed. Alternatively, an adhesive composition may be applied onto a first adhesive layer that has been previously formed, and the adhesive composition may be cured to form a second adhesive layer.
[0119] The pressure-sensitive adhesive composition can be applied using a conventional coater such as a gravure roll coater, a reverse roll coater, a kiss roll coater, a dip roll coater, a bar coater, a knife coater, a spray coater, etc. In a pressure-sensitive adhesive sheet having a support, a method for providing a pressure-sensitive adhesive layer on a support may be a direct method in which a pressure-sensitive adhesive composition is directly applied to the support to form a pressure-sensitive adhesive layer, or a transfer method in which a pressure-sensitive adhesive layer formed on a release surface is transferred to a support.
[0120] In the pressure-sensitive adhesive sheet disclosed herein, the thickness of the pressure-sensitive adhesive layer is not particularly limited and can be appropriately selected according to the purpose. Usually, the thickness of the pressure-sensitive adhesive layer is about 5 to 200 μm, and from the viewpoint of adhesion, etc., it is preferably about 10 μm or more (e.g., 15 μm or more), may be 25 μm or more, and is preferably 150 μm or less, more preferably 100 μm or less, further preferably about 80 μm or less (e.g., 60 μm or less, typically 40 μm or less), and may be 35 μm or less or less than 30 μm. When the pressure-sensitive adhesive sheet disclosed herein is a double-sided pressure-sensitive adhesive sheet having pressure-sensitive adhesive layers on both sides of a substrate, the thicknesses of the pressure-sensitive adhesive layers may be the same or different.
[0121] <Additional adhesive layer> In some embodiments of the adhesive sheet disclosed herein, the adhesive sheet may have a configuration in which an additional adhesive layer is laminated on the back side (opposite side to the adhesive surface) of the adhesive layer constituting the adhesive surface. The adhesive layer constituting the adhesive surface and the additional adhesive layer are preferably laminated in direct contact with each other. That is, it is preferable that a separator layer (e.g., a resin film such as a polyester film) that completely separates both adhesive layers is not interposed between the adhesive layer constituting the adhesive surface and the additional adhesive layer. The additional adhesive layer may be an adhesive layer that includes one or more adhesives selected from various known adhesives such as, for example, acrylic adhesives, rubber adhesives (natural rubber-based, synthetic rubber-based, mixed systems thereof, etc.), silicone adhesives, polyester adhesives, urethane adhesives, polyether adhesives, polyamide adhesives, and fluorine-based adhesives. In terms of transparency, weather resistance, etc., in some embodiments, an acrylic adhesive may be preferably used as a constituent material of the additional adhesive layer. As for other details of the additional adhesive layer, the same configuration as that of the adhesive layer described above can be adopted, or an appropriate configuration can be adopted depending on the application and purpose based on publicly known or commonly used technologies and technical common sense, so detailed explanations are omitted here.
[0122] <Base material> In a single-sided or double-sided adhesive substrate-attached adhesive sheet, the substrate supporting (backing) the adhesive layer can be, for example, a resin film, paper, cloth, rubber sheet, foam sheet, metal foil, or a composite of these. The substrate can be a single layer or a laminate of the same or different substrates. In this specification, the term "single layer" refers to a layer of the same composition, and includes a form in which multiple layers of the same composition are laminated.
[0123] In a preferred embodiment, a substrate (resin film substrate) mainly made of a resin sheet can be used. Examples of the resin constituting the substrate include low-density polyethylene, linear low-density polyethylene, medium-density polyethylene, high-density polyethylene, very low-density polyethylene, random copolymer polypropylene, block copolymer polypropylene, homopolypropylene, polybutene, polymethylpentene, ethylene-vinyl acetate copolymer (EVA), ionomer, ethylene-(meth)acrylic acid copolymer, ethylene-(meth)acrylic acid ester (random, alternating) copolymer, ethylene-butene copolymer, ethylene-hexene copolymer and other polyolefin resins; polyurethane; polyesters such as polyethylene terephthalate (PET), polyethylene naphthalate, and polybutylene terephthalate (PBT); polycarbonates; polyimides; polyether ether ketones; polyetherimides; polyamides such as aramids and fully aromatic polyamides; polyphenylsulfides; fluororesins; polyvinyl chloride; polyvinylidene chloride; cellulose resins; silicone resins; and the like. The above resins may be used alone or in combination to form the whole or part of the substrate (for example, any layer in a substrate having a laminated structure of two or more layers). When the adhesive layer constituting the adhesive surface is an active energy ray curable adhesive layer, the substrate preferably has active energy ray transparency. In some embodiments, a substrate having an ultraviolet ray transmittance of 40% to 100% (more preferably 60% to 100%) at a wavelength of 365 nm may be preferably used. When a substrate having high transparency is used, the adhesive layer can be easily cured.
[0124] The base material may contain various additives, such as fillers (inorganic fillers, organic fillers, etc.), antioxidants, antioxidants, UV absorbers, antistatic agents, lubricants, plasticizers, colorants (pigments, dyes, etc.), etc., as necessary.
[0125] The substrate can be produced by any suitable method. For example, it can be produced by known methods such as a calendar method, a casting method, an inflation extrusion method, a T-die extrusion method, etc. If necessary, it may be produced by carrying out a stretching treatment.
[0126] The surface of the substrate on the side of the adhesive layer may be subjected to known or conventional surface treatments, such as physical treatments (e.g., corona discharge treatment, plasma treatment, sand mat processing treatment, ozone exposure treatment, flame exposure treatment, high-voltage shock exposure treatment, ionizing radiation treatment, etc.), chemical treatments (e.g., acid treatment, alkali treatment, chromate treatment, etc.), and adhesion-improving treatments using a coating agent (primer). In addition, a conductive vapor deposition layer containing a metal, an alloy, or an oxide thereof may be provided on the substrate surface for the purpose of imparting antistatic properties, etc.
[0127] In some preferred embodiments, an undercoat layer is provided on the adhesive layer side surface of the substrate. In other words, an undercoat layer may be disposed between the substrate and the adhesive layer. The undercoat layer forming material is not particularly limited, and one or more of urethane (polyisocyanate) resin, polyester resin, acrylic resin, polyamide resin, melamine resin, olefin resin, polystyrene resin, epoxy resin, phenol resin, isocyanurate resin, polyvinyl acetate resin, etc. may be used. When an acrylic adhesive layer is provided on a resin film substrate via an undercoat layer, a polyester, urethane, or acrylic undercoat layer is preferred. When an acrylic adhesive layer is provided on a polyester substrate such as a PET film via an undercoat layer, a polyester undercoat layer is particularly preferred. The thickness of the undercoat layer is not particularly limited, and may usually be in the range of about 0.1 μm to 10 μm (for example, 0.1 μm to 3 μm, typically 0.1 μm to 1 μm). The undercoat layer can be formed by using a known or conventional coater such as a gravure roll coater or a reverse roll coater.
[0128] In the case where the pressure-sensitive adhesive sheet disclosed herein is a one-sided adhesive sheet in which a pressure-sensitive adhesive layer is provided on one side of a substrate, the surface of the substrate on which the pressure-sensitive adhesive layer is not formed (back surface) may be subjected to a release treatment with a release treatment agent (back surface treatment agent). The back surface treatment agent that can be used to form the back surface treatment layer is not particularly limited, and a silicone-based back surface treatment agent, a fluorine-based back surface treatment agent, a long-chain alkyl-based back surface treatment agent, or other known or commonly used treatment agent can be used depending on the purpose or use.
[0129] The thickness of the substrate is not particularly limited and can be appropriately selected depending on the purpose, but generally can be about 3 μm to 800 μm. From the viewpoint of the processability and handling of the pressure-sensitive adhesive sheet (for example, the workability when attaching to the adherend and peeling off), the thickness of the substrate is suitably 5 μm or more, suitably 10 μm or more, and from the viewpoint of enhancing the protection of the adherend, it is preferably 20 μm or more, may be 30 μm or more, or may be 40 μm or more. In some embodiments in which the protection is more important, the thickness of the substrate can be, for example, 55 μm or more, 75 μm or more, or 90 μm or more. In addition, from the viewpoint of reducing the load on the adherend when peeling off from the adherend, the thickness of the substrate is usually suitably 300 μm, preferably 200 μm or less, may be 150 μm or less, may be 125 μm or less, may be 80 μm or less, or may be 60 μm or less.
[0130] The total thickness of the adhesive sheet disclosed herein (which may include an adhesive layer and a substrate, but does not include a release liner) is not particularly limited, and is suitably in the range of about 10 μm to 1000 μm. In consideration of adhesion and ease of handling, the total thickness of the adhesive sheet is preferably in the range of about 15 μm to 300 μm, more preferably in the range of about 20 μm to 300 μm, and may be in the range of 20 μm to 200 μm. From the viewpoint of enhancing the protection of the adherend, the total thickness of the adhesive sheet is advantageously about 30 μm or more, preferably about 40 μm or more, and more preferably about 50 μm or more (for example, 60 μm or more). In some embodiments in which greater importance is placed on protection, the total thickness of the adhesive sheet may be more than 65 μm, may be more than 80 μm, or may be more than 100 μm.
[0131] <Adhesive sheet> (Normal peel force Fd a2 ) In the pressure-sensitive adhesive sheet disclosed herein, the normal peel strength Fd a2 (hereinafter also referred to as "normal peel strength after 175°C heating / UV irradiation") is preferably 0.50 N / 20 mm or less. This makes it possible to suppress the load on the adherend when peeling after UV irradiation, even if the pressure-sensitive adhesive sheet is exposed to high temperatures after application to the adherend. By peeling from the adherend using a water peeling method, the load on the adherend during peeling can be further reduced. The normal peel strength after 175°C heating / UV irradiation is measured by the method described above, more specifically, by the method described in the Examples below.
[0132] Here, the normal peel strength after 175°C heating / UV is equal to or less than a predetermined value, which means that at least one of the values obtained by the process procedure A (i.e., a process in which heat treatment is first performed, followed by UV irradiation, followed by peeling) described in the examples below and the values obtained by the process procedure B (i.e., a process in which UV irradiation is first performed, followed by heat treatment, followed by peeling) described in the examples below is equal to or less than the predetermined value. From the viewpoint of favorably achieving both bonding reliability in the heating process and easy peelability when peeling from the adherend, it is preferable that at least the value obtained by the process procedure A is equal to or less than the predetermined value. Moreover, the normal peel strength after 175°C heating / UV is equal to or more than a predetermined value, which means that at least one of the values obtained by the process procedure A and the values obtained by the process procedure B described in the examples below (preferably both) is equal to or more than the predetermined value. The same applies to the normal peel strength after 200°C heating / UV, the water peel strength after 175°C heating / UV, the water peel strength after 200°C heating / UV, the normal peel strength difference after heating / UV, and the water peel strength difference after heating / UV, which will be described later.
[0133] In some embodiments, the normal peel strength after 175°C heating / UV is more preferably 0.40N / 20mm or less, more preferably 0.30N / 20mm or less, and may be 0.25N / 20mm or less, 0.20N / 20mm or less, or 0.15N / 20mm or less, from the viewpoint of reducing the load on the adherend during peeling. The lower limit of the normal peel strength after 175°C heating / UV is not particularly limited, but from the viewpoint of facilitating compatibility with bonding reliability during processing, it may be, for example, 0.001N / 20mm or more, 0.010N / 20mm or more, 0.050N / 20mm or more, or 0.10N / 20mm or more. The normal peel strength after 175°C heating / UV can be adjusted by the selection of the base polymer, the selection of the type and amount of compound A when compound A is used, the selection of the type and amount of crosslinking agent when a crosslinking agent is used, and the like.
[0134] In addition, the normal peel force Fd a2 Even if the PSA sheet has a water peel strength Fw that is higher than any of the above upper limits, it may be used as long as the PSA sheet is in an embodiment that allows for sufficiently light peeling by water peeling (for example, a2 is 0.30 N / 20 mm or less), the pressure-sensitive adhesive sheet can be suitably prevented from causing load on the adherend or leaving adhesive residue by peeling after heating / UV irradiation using a water peeling method. Therefore, in this embodiment, the normal peel strength Fd a2 The normal peel strength Fd of the pressure-sensitive adhesive sheet in this embodiment may be greater than 0.50 N / 20 mm. a2 is not particularly limited, and may be, for example, 2.00 N / 20 mm or less or 1.00 N / 20 mm or less.
[0135] (Normal peel force Fd b2 ) The adhesive sheet disclosed herein generally has a peel strength Fd b2(hereinafter also referred to as "normal peel strength after heating at 200°C / UV") is preferably 2.00 N / 20 mm or less. This makes it possible to suppress the load on the adherend during peeling after UV irradiation, even when exposed to more severe high temperature conditions. By performing peeling from the adherend by a water peeling method, the load on the adherend during peeling can be further reduced. The normal peel strength after heating at 200°C / UV is measured by the method described above, more specifically, by the method described in the Examples below. In some embodiments, the normal peel strength after 200°C heating / UV may be 1.50N / 20mm or less, 1.20N / 20mm or less, 1.00N / 20mm or less, or 0.80N / 20mm or less, from the viewpoint of reducing the load on the adherend during peeling. The lower limit of the normal peel strength after 200°C heating / UV is not particularly limited, but from the viewpoint of facilitating compatibility with bonding reliability during processing, it may be, for example, 0.001N / 20mm or more, 0.050N / 20mm or more, 0.10N / 20mm or more, or 0.30N / 20mm or more. The normal peel strength after 200°C heating / UV can be adjusted by selecting the base polymer, selecting the type and amount of compound A when compound A is used, selecting the type and amount of crosslinking agent when a crosslinking agent is used, and the like.
[0136] In addition, the normal peel force Fd b2 Even if the PSA sheet has a water peel strength Fw that is higher than any of the above upper limits, it may be used as long as the PSA sheet is in an embodiment that allows for sufficiently light peeling by water peeling (for example, b2 If the normal peel strength Fd of the PSA sheet is 1.00 N / 20 mm or less, the PSA sheet can be peeled off after heating / UV irradiation using a water peeling method, thereby suitably suppressing the load on the adherend and the occurrence of adhesive residue. b2 The normal peel strength Fd of the PSA sheet in this embodiment may be greater than 2.00 N / 20 mm. b2 is not particularly limited, but may be, for example, 5.00 N / 20 mm or less or 3.00 N / 20 mm or less.
[0137] (Water peeling force Fw a2 ) The pressure-sensitive adhesive sheet disclosed herein has a water peel strength Fw a2(hereinafter also referred to as "water peeling strength after heating at 175°C / UV exposure") is preferably 0.30 N / 20 mm or less. This makes it possible to suppress the load on the adherend when peeling after UV irradiation, even if the pressure-sensitive adhesive sheet is exposed to high temperatures after attachment to the adherend. The water peeling strength after heating at 175°C / UV exposure is measured by the method described above, more specifically, by the method described in the Examples below. In some embodiments, the water peeling force after 175°C heating / UV is more preferably 0.20N / 20mm or less, more preferably 0.15N / 20mm or less, and may be 0.10N / 20mm or less, or may be 0.05N / 20mm or less, from the viewpoint of reducing the load on the adherend during peeling. The lower limit of the water peeling force after 175°C heating / UV is not particularly limited, but from the viewpoint of facilitating compatibility with bonding reliability during processing, it may be, for example, 0.001N / 20mm or more, 0.005N / 20mm or more, 0.010N / 20mm or more, or 0.020N / 20mm or more. The water peeling force after 175°C heating / UV can be adjusted by selecting the base polymer, selecting the type and amount of compound A when compound A is used, selecting the type and amount of crosslinking agent when a crosslinking agent is used, and the like.
[0138] (Water peeling force Fw b2 ) The pressure-sensitive adhesive sheet disclosed herein has a water peel strength Fw b2 (hereinafter also referred to as "water peeling force after heating at 200°C / UV irradiation") is preferably 1.00 N / 20 mm or less. This makes it possible to suppress the load on the adherend during peeling after UV irradiation even when exposed to more severe high temperature conditions. The water peeling force after heating at 200°C / UV irradiation is measured by the method described above, more specifically, by the method described in the Examples below. In some embodiments, the water peeling force after 200°C heating / UV may be 0.80N / 20mm or less, 0.60N / 20mm or less, 0.40N / 20mm or less, or 0.30N / 20mm or less, from the viewpoint of reducing the load on the adherend during peeling. The lower limit of the water peeling force after 200°C heating / UV is not particularly limited, but may be, for example, 0.001N / 20mm or more, 0.050N / 20mm or more, or 0.10N / 20mm or more, from the viewpoint of facilitating compatibility with bonding reliability during processing. The water peeling force after 200°C heating / UV can be adjusted by selecting the base polymer, selecting the type and amount of compound A when compound A is used, selecting the type and amount of crosslinking agent when a crosslinking agent is used, and the like.
[0139] (Normal peel force difference Fd b2 -Fd a2 ) The adhesive sheet disclosed herein has a peel strength difference between normal peel strength after heating at 175°C / UV and normal peel strength after heating at 200°C / UV (Fd b2 -Fd a2 (i.e., normal peeling force difference after heating / UV) is preferably 1.50N / 20mm or less. This makes the peeling force of the pressure-sensitive adhesive sheet after a high-temperature process less susceptible to the effects of temperature unevenness that may occur in the high-temperature process. Such a pressure-sensitive adhesive sheet is preferable because it can reduce the risk of adhesive residue when peeling off the pressure-sensitive adhesive sheet that has been subjected to a high-temperature process while attached to an adherend, and can also reduce the load on the adherend due to fluctuations in peeling force. From the viewpoint of further reducing the effects of the temperature unevenness, the normal peeling force difference after heating / UV is more preferably 1.20N / 20mm or less, may be 0.90N / 20mm or less, or may be 0.70N / 20mm or less. The normal peeling force difference after heating / UV is usually 0N / 20mm or more, so there is no particular lower limit, and the closer to 0N / 20mm, the more preferable.
[0140] (Water peeling force difference Fw b2 -Fw a2 ) The pressure-sensitive adhesive sheet disclosed herein has a difference between the water peel strength after heating at 175°C / UV and the water peel strength after heating at 200°C / UV (Fw b2-Fw a2 hereinafter also referred to as "heating / UV post-water peeling force difference". ) is preferably 1.00 N / 20 mm or less. This makes the peeling force of the pressure-sensitive adhesive sheet after a high-temperature process less susceptible to the effects of temperature unevenness that may occur in the high-temperature process. Such a pressure-sensitive adhesive sheet is preferable from the viewpoint of reducing the load on the adherend and reducing the risk of adhesive residue when peeling the pressure-sensitive adhesive sheet that has been subjected to a high-temperature process while attached to the adherend. From the viewpoint of further reducing the effects of temperature unevenness, the heating / UV post-water peeling force difference is more preferably 0.90 N / 20 mm or less, even more preferably 0.70 N / 20 mm or less, and may be 0.50 N / 20 mm or less, or may be 0.30 N / 20 mm or less. The heating / UV post-water peeling force difference is usually 0 N / 20 mm or more, so there is no particular lower limit, and the closer to 0 N / 20 mm, the more preferable.
[0141] (Initial normal peel force Fd0) The adhesive sheet disclosed herein preferably has an initial normal peel strength Fd0 of 0.10 N / 20 mm or more. This allows the adhesive sheet to exhibit appropriate adhesion as an adhesive sheet for semiconductor processing, and can contribute to improving processability. For example, when the adhesive sheet disclosed herein is used as a backglide tape for protecting the circuit-forming surface of a semiconductor wafer (adherend) in a backglide process of the semiconductor wafer, peeling of the adhesive sheet during backglide and chipping of the semiconductor wafer can be prevented. The initial normal peel strength Fd0 is measured by the above-mentioned method, more specifically, by the method described in the Examples below. From the viewpoint of adhesion to the adherend and protection during processing, the initial normal peel strength Fd0 is preferably 0.20 N / 20 mm or more, more preferably 0.30 N / 20 mm or more. From the viewpoint of enhancing the above-mentioned adhesion and protective properties, in some embodiments, the initial normal peel strength Fd0 may be, for example, 0.50 N / 20 mm or more, 1.00 N / 20 mm or more, or 2.00 N / 20 mm or more. The upper limit of the initial normal peel strength Fd0 is not particularly limited. From the viewpoint of making it easier to lower the peel strength after heating / UV, the initial normal peel strength Fd0 may be, for example, 10.0 N / 20 mm or less, 8.00 N / 20 mm or less, 5.00 N / 20 mm or less, or 3.50 N / 20 mm or less. In some embodiments of the pressure-sensitive adhesive sheet disclosed herein, the initial normal peel strength Fd0 may be, for example, 2.50 N / 20 mm or less, 2.00 N / 20 mm or less, 1.50 N / 20 mm or less, 1.00 N / 20 mm or less, or 0.50 N / 20 mm or less. The initial normal peel force Fd0 can be adjusted by selecting the base polymer, the type and amount of compound A when compound A is used, the type and amount of crosslinking agent when a crosslinking agent is used, and the like.
[0142] (Normal peel force without heating Fd U1 ) The pressure-sensitive adhesive sheet disclosed herein has a non-heated normal peel strength Fd U1is preferably 0.10 N / 20 mm or less. This allows the pressure-sensitive adhesive sheet to exhibit excellent light peelability, for example, in an embodiment used in semiconductor processing that does not involve a high-temperature process (e.g., a high-temperature process of 100° C. or higher, preferably 60° C. or higher), and can reduce the load on the adherend during peeling. This allows, for example, in a pressure-sensitive adhesive sheet used as a backglide tape, to efficiently peel the pressure-sensitive adhesive sheet from a semiconductor wafer that has been thinned by backgrinding while avoiding damage to the semiconductor wafer. Non-heating normal peel force Fd U1 A low peel strength Fd is also preferable from the viewpoint of making it easier to reduce the peel strength after heating / UV. U1 is measured by the method described above, more specifically, by the method described in the Examples below. In some embodiments, the non-heated normal peel force Fd U1 may be, for example, 0.080 N / 20 mm or less, 0.060 N / 20 mm or less, 0.040 N / 20 mm or less, 0.030 N / 20 mm or less, or 0.020 N / 20 mm or less. U1 A pressure-sensitive adhesive sheet with a low peel strength is preferred because the peel strength can be further reduced by water peeling. U1 The lower limit of the non-heating normal peel force Fd is not particularly limited, and from the viewpoint of reducing the load on the adherend, the smaller the better. On the other hand, from the viewpoint of balancing the adhesion to the adherend and the protection during processing, in some embodiments, U1 can be, for example, 0.001 N / 20 mm or more. U1 can be adjusted by selecting the base polymer, the type and amount of compound A when compound A is used, the type and amount of crosslinking agent when a crosslinking agent is used, and the like.
[0143] (Non-heated water peeling force Fw U1 ) The pressure-sensitive adhesive sheet disclosed herein has a non-heated water peel strength Fw U1is preferably 0.050 N / 20 mm or less. This allows the pressure-sensitive adhesive sheet to exhibit excellent light peelability, for example, in an embodiment used in semiconductor processing that does not involve a high-temperature process (e.g., a high-temperature process of 100° C. or higher, preferably 60° C. or higher), and can reduce the load on the adherend during peeling. This allows the pressure-sensitive adhesive sheet to be efficiently peeled off from a semiconductor wafer that has been thinned by backgrinding, for example, in a pressure-sensitive adhesive sheet used as a backglide tape, while avoiding damage to the semiconductor wafer. Non-heated water peel force Fw U1 A low Fw is also preferable from the viewpoint of making it easier to reduce the peel strength after heating / UV. U1 is measured by the method described above, more specifically, by the method described in the Examples below. In some embodiments, the non-heated water peel force Fw U1 is preferably less than 0.030 N / 20 mm, more preferably less than 0.020 N / 20 mm, may be less than 0.010 N / 20 mm, may be less than 0.007 N / 20 mm, or may be less than 0.005 N / 20 mm. U1 The lower limit of Fw is not particularly limited, and the smaller the better from the viewpoint of reducing the load on the adherend. On the other hand, in some embodiments, the non-heated water peeling force Fw is preferably set to 100% in order to achieve a good balance between adhesion to the adherend and protection during processing. U1 For example, the non-heated water peeling force Fw may be 0.0005 N / 20 mm or more, or 0.001 N / 20 mm or more. U1 can be adjusted by selecting the base polymer, the type and amount of compound A when compound A is used, the type and amount of crosslinking agent when a crosslinking agent is used, and the like.
[0144] The tensile tester used to measure the above-mentioned normal peel strength and water peel strength may be Shimadzu Corporation's precision universal testing machine "Autograph EZ-S" or an equivalent. When making the measurements, if necessary, the pressure-sensitive adhesive sheet to be measured may be reinforced by attaching an appropriate backing material (e.g., a PET film with a thickness of about 25 μm).
[0145] In the examples described later, the normal peel strength and the water peel strength were measured consecutively for each test piece, but the normal peel strength and the water peel strength may be measured using different test pieces. For example, when it is difficult to prepare a test piece of sufficient length to perform consecutive measurements, a mode in which measurements are performed using different test pieces can be adopted.
[0146] In a preferred embodiment of the pressure-sensitive adhesive sheet disclosed herein, the non-heated water peel strength Fw U1 [N / 20mm] ratio, i.e. Fw U1 / Fd0 (hereinafter also referred to as "residual peel force") may be, for example, less than 10.0%. In a usage mode in which such a pressure-sensitive adhesive sheet is temporarily attached to an adherend during the manufacturing process of a product, it exhibits good adhesion and protection to the adherend at a stage where peeling is not intended, and can effectively reduce the load on the adherend during peeling. The residual peel force is preferably less than 5.0%, more preferably less than 3.0%, and may be less than 2.0%, less than 1.0%, or may be less than 0.70%, less than 0.50%, or less than 0.30%. U1 The lower limit of / Fd0 is not particularly limited, and from the viewpoint of reducing the load on the adherend, U1 On the other hand, from the viewpoint of practicality such as cost, in the PSA sheet according to some embodiments, Fw U1 / Fd0 may be, for example, 0.01% or more, 0.05% or more, or 0.10% or more.
[0147] In some preferred embodiments of the pressure-sensitive adhesive sheet disclosed herein, the non-heated normal peel strength Fd U1 [N / 20mm] Non-heated water peeling force Fw U1 The rate of decrease in [N / 20 mm] may be, for example, more than 30%. That is, the rate of decrease in water peeling force calculated by the following formula is preferably more than 30%. Water peeling force reduction rate = 1-(Fw U1 / Fd U1 ) A pressure-sensitive adhesive sheet with a high water peel strength reduction rate can be peeled off by a water peeling method after UV irradiation, and the peel strength can be significantly reduced compared to peeling off by a normal peeling method, and the load on the adherend during peeling can be effectively reduced. In some preferred embodiments of the pressure-sensitive adhesive sheet, the water peel strength reduction rate can be 55% or more, 65% or more, or 75% or more. The upper limit of the water peel strength reduction rate is not particularly limited, but is usually 100% or less, and may be, for example, 95% or less or 90% or less from a practical viewpoint.
[0148] <Application> The adhesive sheet disclosed herein can be used in the processing of various semiconductor wafers. The semiconductor wafer can be, for example, a silicon wafer, a silicon carbide (SiC) wafer, a nitride semiconductor wafer (silicon nitride (SiN), gallium nitride (GaN), etc.), a compound semiconductor wafer such as a gallium arsenide wafer, etc. The adhesive sheet disclosed herein can be preferably used as an adhesive sheet for semiconductor processing for protecting and / or fixing the semiconductor wafer during processing of the semiconductor wafer, typically in a form of being laminated to the semiconductor wafer on which a circuit is formed in a previous process, during the process of manufacturing a semiconductor element (e.g., a semiconductor chip) from such a semiconductor wafer. Examples of processing that can be performed on the semiconductor wafer after laminating the adhesive sheet disclosed herein and before peeling off the adhesive sheet include, but are not limited to, back grinding and dicing. In this specification, even if the shape of the semiconductor wafer to be processed changes due to processing (for example, thinning of the whole or part by back grinding, individual pieces by dicing, etc.), the processed article may still be called a semiconductor wafer.
[0149] The adhesive sheet disclosed herein may be bonded to a semiconductor wafer by any suitable method. The temperature when bonding the adhesive sheet may be around room temperature (e.g., 10°C to 35°C), or may be a temperature higher than the room temperature range (e.g., over 35°C, preferably 60°C to 90°C). Bonding the adhesive sheet at a temperature higher than the room temperature range may be advantageous in terms of improving the adhesion of the adhesive sheet to the semiconductor wafer. After bonding the adhesive sheet in the room temperature range, a heating and pressurizing treatment may be performed in which a temperature higher than the room temperature range (e.g., 40°C to 90°C, preferably 40°C to 60°C) and a pressure higher than atmospheric pressure (e.g., 1.5 to 10 atm, preferably 3 to 7 atm) are applied. The time for carrying out the heating and pressurizing treatment is not particularly limited, and can be set so as to obtain an appropriate treatment effect. In some embodiments, the time for carrying out the heating and pressurizing treatment may be set to 3 minutes to 1 hour (e.g., 5 minutes to 30 minutes) in consideration of the balance between the stability of the treatment effect and the productivity.
[0150] By satisfying at least one of the above conditions A to D, the adhesive sheet disclosed herein can be easily peeled off from the adherend even if it is exposed to high temperatures between the time of attachment to the adherend and the time of peeling off, and can suppress, for example, adhesive residue and load on the adherend. Taking advantage of such characteristics, the adhesive sheet disclosed herein can be preferably used in an embodiment in which a high-temperature process is performed between the time of attachment to the adherend and the time of peeling off from the adherend. Non-limiting examples of the high-temperature process include an ion implantation process into a semiconductor wafer, an ashing process for removing resist, and an annealing process such as laser annealing. Such a high-temperature process can be performed, for example, before and / or after the backgrinding process with a semiconductor processing adhesive sheet (backgrinding tape) used in the backgrinding process attached. Therefore, the adhesive sheet disclosed herein can be preferably used as an adhesive sheet for semiconductor processing used in an embodiment including a backgrinding process and a high-temperature process performed before and / or after the backgrinding process between the time of attachment to the adherend and the time of peeling off from the adherend.
[0151] The pressure-sensitive adhesive sheet disclosed herein can be preferably used in an embodiment in which it is irradiated with active energy rays after being attached to an adherend and before being peeled off from the adherend. The conditions for irradiating the active energy rays are not particularly limited and can be set so as to allow the adhesive layer to be cured appropriately. A person skilled in the art can set appropriate irradiation conditions without excessive burden based on the technical common sense in the field, so detailed explanations are omitted. As an example, when UV is used as the active energy rays, the UV irradiation conditions are, for example, an integrated light amount of about 50 mJ / cm. 2 ~5000mJ / cm 2 range, approximately 50 mJ / cm 2 ~2000mJ / cm 2 or approximately 100 mJ / cm 2 ~2000mJ / cm 2 and the irradiation time can be in the range of about 1 second to 30 minutes.
[0152] When the pressure-sensitive adhesive sheet disclosed herein is laminated to an adherend and then irradiated with active energy rays before peeling from the adherend, the irradiation with active energy rays may be performed after the high-temperature process (for example, treatment procedure A in the examples described later) or before the high-temperature process (for example, treatment procedure B in the examples described later). The pressure-sensitive adhesive sheet disclosed herein can be favorably used in an embodiment in which active energy rays are irradiated after a high-temperature process, since it can be easily peeled by irradiation with active energy rays even after the high-temperature process. According to this embodiment, there is an advantage that the adhesive sheet has good bonding reliability to the adherend in the high-temperature process. On the other hand, the pressure-sensitive adhesive sheet disclosed herein can also be favorably used in an embodiment in which active energy rays are irradiated before a high-temperature process. This use embodiment can achieve effects such as further reducing the peel force after the high-temperature process and further reducing the effect of processing unevenness (temperature unevenness, etc.) in the high-temperature process on the peel force.
[0153] The adhesive sheet disclosed herein may be peeled off from the adherend by a normal peeling method (i.e., a peeling method that does not use an aqueous peeling solution such as water) or by a water peeling method. From the viewpoint of improving peelability, in some embodiments, the water peeling method may be preferably adopted. As the aqueous peeling solution used in the water peeling method, water or a mixed solvent mainly composed of water may be used, which contains a small amount of additives as necessary. As the solvent other than water constituting the mixed solvent, lower alcohols (e.g., ethyl alcohol) and lower ketones (e.g., acetone) that can be mixed uniformly with water may be used. As the additives, known surfactants, pH adjusters, etc. may be used. From the viewpoint of avoiding contamination of the adherend, in some embodiments, an aqueous peeling solution that does not substantially contain additives may be preferably used. From the viewpoint of environmental hygiene, it is particularly preferable to use water as the aqueous peeling solution. There are no particular limitations on the water, and in consideration of the purity required depending on the application and ease of availability, for example, distilled water, ion-exchanged water, tap water, etc. may be used.
[0154] The adhesive sheet disclosed herein can be peeled off from an adherend while highly suppressing the load on the adherend, for example, by using a water peeling method, and is therefore suitable as an adhesive sheet that can be used in a form that is peeled off from a hard and brittle thin portion (for example, a portion of 150 μm or less, 100 μm or less, 50 μm or less, or 30 μm or less) of an adherend having a thin portion (hereinafter also referred to as a hard and brittle thin portion) made of a hard and brittle material (for example, the constituent material of the semiconductor wafer described above, various ceramic materials such as sapphire, glass, etc.). The adhesive sheet disclosed herein is preferably used as an adhesive sheet that is temporarily attached to such an adherend, and can prevent the occurrence of cracks or chips in the hard and brittle thin portion due to the load when peeling off the adhesive sheet. The hard and brittle thin portion may be a portion formed by processing the adherend after attaching the adhesive sheet to the adherend.
[0155] <Semiconductor device manufacturing method> One embodiment of a method for manufacturing a semiconductor device using the adhesive sheet disclosed herein is described below. The method for manufacturing a semiconductor device of this embodiment includes a step (1) of attaching an adhesive surface of an adhesive sheet for semiconductor processing to a circuit-forming surface side of a semiconductor wafer having a circuit-forming surface, a step (2) of processing the semiconductor wafer with the adhesive sheet attached from the side opposite to the adhesive sheet, and a step (3) of peeling the adhesive sheet from the semiconductor wafer after the processing.
[0156] The above step (3) is preferably carried out by supplying an aqueous stripping solution to the front of the peeling of the pressure-sensitive adhesive sheet from the processed semiconductor wafer (adherend). This allows the pressure-sensitive adhesive sheet to be peeled lightly, thereby suppressing adhesive residue and reducing the load on the adherend (processed semiconductor wafer). In some embodiments, the above step (3) can be preferably carried out by the pressure-sensitive adhesive sheet peeling method described below.
[0157] Preferably, the high-temperature process as described above is carried out after the step (1) and before the step (3). Also, preferably, the pressure-sensitive adhesive sheet is irradiated with active energy rays in or before the step (3). Typically, the peeling force of the pressure-sensitive adhesive sheet is reduced by the irradiation treatment. The irradiation treatment may be carried out in the step (3), or may be carried out before the step (3) and before the high-temperature process. By peeling the pressure-sensitive adhesive sheet (preferably with water) after such an irradiation treatment, the load applied to the adherend (processed semiconductor wafer) during peeling can be effectively reduced. From the viewpoint of achieving both the adhesion reliability to the adherend in the step (2) and the easy peeling property in the step (3), the irradiation treatment is preferably carried out after the step (2).
[0158] In some embodiments, the step (2) may be a backgrinding step. In this case, the pressure-sensitive adhesive sheet is used as a backgrinding tape. The backgrinding step may be performed by any appropriate method. The backgrinding step may be a step of thinning the semiconductor wafer to which the pressure-sensitive adhesive sheet is attached until the thickness of the semiconductor wafer is, for example, 150 μm or less, 100 μm or less, 50 μm or less, or 30 μm or less. In such a thinning embodiment, the effect of peeling the pressure-sensitive adhesive sheet with water in the step (3) may be preferably exhibited. The backgrinding step may be performed so that the inside of the annular convex portion becomes a concave portion (i.e., so that a TAIKO (registered trademark) wafer is obtained). In this case, the thickness of the thinned semiconductor wafer refers to the thickness of the concave portion. In addition, although not particularly limited, the thickness of the semiconductor wafer before backgrinding may be, for example, about 500 μm to 1000 μm.
[0159] The semiconductor device manufacturing method disclosed herein may further include any appropriate step. Examples of such optional steps include, but are not limited to, an etching step, a photolithography step, an ion implantation step, a dicing step, a die bonding step, a wire bonding step, a packaging step, etc. Each of the steps exemplified above may be performed in the step (2), after the step (2), before the step (3), or after the step (3).
[0160] <How to remove the adhesive sheet> According to this specification, a method for peeling a pressure-sensitive adhesive sheet attached to an adherend is provided, which peels the pressure-sensitive adhesive sheet from the adherend. The method may include a water peeling step of peeling the pressure-sensitive adhesive sheet from the adherend while advancing the intrusion of the aqueous peeling solution into the interface in accordance with the movement of the peeling front, in a state where an aqueous peeling solution is present at the interface between the adherend and the pressure-sensitive adhesive sheet at the peeling front of the pressure-sensitive adhesive sheet from the adherend. Here, the peeling front refers to the location where the adhesive surface of the pressure-sensitive adhesive sheet begins to separate from the adherend when the peeling of the pressure-sensitive adhesive sheet from the adherend progresses. According to the water peeling step, the aqueous peeling solution can be effectively used to peel the pressure-sensitive adhesive sheet from the adherend. The peeling method may be preferably carried out, for example, in an embodiment in which any of the pressure-sensitive adhesive sheets disclosed herein are peeled from the adherend.
[0161] The adherend in the peeling method disclosed herein may be any of the various semiconductor wafers exemplified above. The semiconductor wafer may be a semiconductor wafer on which a circuit is formed. The peeling method disclosed herein may be preferably used as a method for peeling an adhesive sheet attached to a circuit-forming surface of a semiconductor wafer on which a circuit is formed, from the circuit-forming surface. After the adhesive sheet is attached to the adherend, a high-temperature process may be performed before the start of the water peeling.
[0162] As the PSA sheet to be peeled off from the adherend by the above peeling method, any of the PSA sheets disclosed herein can be preferably used, and therefore the above peeling method is suitable as a method for peeling off any of the PSA sheets disclosed herein.
[0163] In some embodiments, the peeling method can be preferably carried out in an embodiment including: forcibly lifting the adhesive sheet from the adherend at one end of the outer edge of the adhesive sheet attached to the adherend to form an initial peeling front; supplying an aqueous peeling liquid to the peeling front; and peeling the adhesive sheet from the adherend while advancing the intrusion of the aqueous peeling liquid into the interface between the adhesive sheet and the adherend in accordance with the movement of the peeling front. The formation of the initial peeling front can be carried out in such an embodiment as inserting the tip of a tool such as a cutter knife or a needle into the interface between the adhesive sheet and the adherend, scratching and lifting the adhesive sheet with a hook or a claw, or attaching a highly adhesive adhesive tape or a suction cup to the back surface of the adhesive sheet to lift the edge of the adhesive sheet. In this way, the initial peeling front is formed, and then an aqueous peeling liquid is supplied to the peeling front to start water peeling, thereby efficiently supplying the aqueous peeling liquid to the peeling front. Furthermore, in this peeling method and the pressure-sensitive adhesive sheet used in this peeling method, it is possible to advantageously achieve both good water peelability after an operation for forcibly forming an initial peel front is performed to trigger peeling, and high water resistance reliability when such an operation is not performed.
[0164] In some embodiments, the peeling method can be preferably carried out in such a manner that after the aqueous peeling liquid is supplied to the initial peeling front (i.e., after the aqueous peeling liquid is supplied at the start of the aqueous peeling), the peeling of the pressure-sensitive adhesive sheet is allowed to proceed without supplying a new aqueous peeling liquid. Alternatively, if the aqueous peeling liquid that is allowed to enter the interface between the pressure-sensitive adhesive sheet and the adherend following the movement of the peeling front is exhausted or insufficient during the progress of the aqueous peeling, the aqueous peeling liquid may be additionally supplied intermittently or continuously after the start of the aqueous peeling. For example, in cases where the length of the peeling front increases with the progress of the peeling (for example, when the aqueous peeling is advanced from one end of the outer edge of the disc-shaped adherend in the radial direction of the circle) or when the aqueous peeling liquid is likely to remain on the adherend surface, a mode in which the aqueous peeling liquid is additionally supplied after the start of the aqueous peeling can be preferably adopted. In addition, the position where the aqueous peeling liquid is supplied may be one or more positions. When the aqueous peeling liquid is additionally supplied after the start of the aqueous peeling, the number of positions where the aqueous peeling liquid is supplied after the start of the aqueous peeling may be increased or decreased.
[0165] The peeling method disclosed herein can be preferably carried out using a pressure-sensitive adhesive sheet having an adhesive surface constituted by an active energy ray curable pressure-sensitive adhesive layer. In some preferred embodiments of the peeling method using such a pressure-sensitive adhesive sheet, the pressure-sensitive adhesive sheet is irradiated with active energy rays after the pressure-sensitive adhesive sheet is bonded to an adherend and before the water peeling is started. This can particularly effectively reduce the peeling force due to water peeling.
[0166] The matters disclosed in this specification include the following. [1] An adhesive sheet for semiconductor processing comprising an adhesive layer constituting an adhesive surface, comprising the following method A: The adhesive surface was attached to a silicon wafer and subjected to heat treatment at 175°C for 15 minutes with an integrated light dose of 1000 mJ / cm 2 After the ultraviolet irradiation treatment, the peel strength is measured under the conditions of a pulling speed of 300 mm / min and a peel angle of 180 degrees; Normal peel force Fd measured by a2 Adhesive sheet for semiconductor processing, with a strength of 0.50N / 20mm or less. [2] A semiconductor processing adhesive sheet comprising an adhesive layer constituting an adhesive surface, comprising the following method B: The adhesive surface was attached to a silicon wafer and subjected to heat treatment at 175°C for 15 minutes with an integrated light dose of 1000 mJ / cm 2 After the ultraviolet irradiation treatment, water is supplied to the front of the pressure-sensitive adhesive sheet from the silicon wafer, and the peel strength is measured under the conditions of a pulling speed of 300 mm / min and a peel angle of 180 degrees; Water peel force Fw measured by a2 Adhesive sheet for semiconductor processing, with a compressive strength of 0.30N / 20mm or less. [3] A semiconductor processing adhesive sheet comprising an adhesive layer constituting an adhesive surface, comprising the following method C: The adhesive surface was attached to a silicon wafer and subjected to heat treatment at 200°C for 15 minutes with an integrated light dose of 1000 mJ / cm 2 After the ultraviolet irradiation treatment, the peel strength is measured under the conditions of a pulling speed of 300 mm / min and a peel angle of 180 degrees; Normal peel force Fd measured by b2 Adhesive sheet for semiconductor processing, with a strength of 2.00N / 20mm or less. [4] A semiconductor processing adhesive sheet comprising an adhesive layer constituting an adhesive surface, comprising the following method D: The adhesive surface was attached to a silicon wafer and subjected to heat treatment at 200°C for 15 minutes with an integrated light dose of 1000 mJ / cm 2 After the ultraviolet irradiation treatment, water is supplied to the front of the pressure-sensitive adhesive sheet from the silicon wafer, and the peel strength is measured under the conditions of a pulling speed of 300 mm / min and a peel angle of 180 degrees; Water peel force Fw measured by b2 Adhesive sheet for semiconductor processing, with a compressive strength of 1.00N / 20mm or less. [5] Normal peel force Fd measured by method A above a2 [N / 20mm] and the normal peel force Fd measured by method C above b2 [N / 20mm] and the following formula: Fd b2 -Fd a2The adhesive sheet for semiconductor processing according to any one of the above [1] to [4], wherein the normal peel strength difference calculated by the above formula is 1.50 N / 20 mm or less (preferably 0.90 N / 20 mm or less). [6] Water peeling force Fw measured by method B above a2 [N / 20mm] and the water peeling force Fw measured by method D above b2 [N / 20mm], the following formula: Fw b2 -Fw a2 The pressure-sensitive adhesive sheet for semiconductor processing according to any one of the above [1] to [5], wherein the water peeling force difference calculated by the above formula is 0.10 N / 20 mm or less (preferably 0.30 N / 20 mm or less). [7] Method E below: The adhesive surface is attached to a silicon wafer, and then the peel strength is measured at a pulling speed of 300 mm / min and a peel angle of 180 degrees; The pressure-sensitive adhesive sheet for semiconductor processing according to any one of the above [1] to [6], having an initial normal peel strength Fd0 measured by 0.30 N / 20 mm or more. [8] Method F below: The adhesive surface was attached to a silicon wafer, and the cumulative light intensity was 1000 mJ / cm 2 After the ultraviolet irradiation treatment, the peel strength is measured under the conditions of a pulling speed of 300 mm / min and a peel angle of 180 degrees; Unheated normal peel force Fd measured by U1 The adhesive sheet for semiconductor processing according to any one of the above [1] to [7], having a compressive strength of 0.10 N / 20 mm or less. [9] The following method G: The adhesive surface was attached to a silicon wafer, and the cumulative light intensity was 1000 mJ / cm 2 After the ultraviolet irradiation treatment, water is supplied to the front of the pressure-sensitive adhesive sheet from the silicon wafer, and the peel strength is measured under the conditions of a pulling speed of 300 mm / min and a peel angle of 180 degrees; Unheated water peel force Fw measured by U1 The adhesive sheet for semiconductor processing according to any one of the above [1] to [8], having a compressive strength of 0.050 N / 20 mm or less.
[0167]
[10] An adhesive sheet for semiconductor processing, comprising an adhesive layer constituting an adhesive surface, the adhesive sheet having the following conditions: (Condition A) Normal peel force Fd measured by method A above a2 is 0.50N / 20mm or less (preferably 0.30N / 20mm or less); (Condition B) Water peeling force Fw measured by method B above a2 is 0.30N / 20mm or less (preferably 0.20N / 20mm or less); (Condition C) Normal peel force Fd measured by method C above b2 is 2.00 N / 20 mm or less (preferably 1.50 N / 20 mm or less, more preferably 1.00 N / 20 mm or less); and (Condition D) Water peeling force Fw measured by method D above b2 is 1.00 N / 20 mm or less (preferably 0.80 N / 20 mm or less, more preferably 0.40 N / 20 mm or less); An adhesive sheet for semiconductor processing, which satisfies at least one of the above conditions.
[11] The adhesive sheet for semiconductor processing according to
[10] above, which satisfies at least the above condition D.
[12] The adhesive sheet for semiconductor processing according to any one of the above [1] to
[11] , wherein the adhesive layer is an active energy ray-curable adhesive layer.
[13] The pressure-sensitive adhesive layer according to any one of [1] to
[12] , wherein the pressure-sensitive adhesive layer contains a photoinitiator.
[14] The pressure-sensitive adhesive sheet for semiconductor processing according to any one of the above [1] to
[13] , wherein the pressure-sensitive adhesive layer is an acrylic pressure-sensitive adhesive layer.
[15] The adhesive sheet for semiconductor processing according to any one of [1] to
[14] above, wherein the adhesive layer contains at least one compound A selected from the group consisting of surfactants and compounds having a polyoxyalkylene skeleton as a heat-resistant release agent.
[16] The adhesive sheet for semiconductor processing according to any one of the above [1] to
[15] , wherein a crosslinking agent is used in the adhesive layer.
[17] The adhesive layer according to any one of [1] to
[16] , further comprising a substrate supporting the adhesive layer.
[0168]
[19] A method for producing a semiconductor element using the adhesive sheet for semiconductor processing according to any one of [1] to
[17] above, A step (1) of bonding the adhesive surface of the adhesive sheet for semiconductor processing to a circuit-forming surface side of a semiconductor wafer having a circuit-forming surface; (2) processing the semiconductor wafer to which the adhesive sheet is attached from the side opposite to the adhesive sheet; a step (3) of peeling the adhesive sheet from the processed semiconductor wafer; A method for manufacturing a semiconductor device comprising the steps of:
[20] The method for producing a semiconductor device according to
[19] above, further comprising the step of irradiating the pressure-sensitive adhesive sheet with active energy rays in the step (3) or before the step (3) and after the step (1).
[21] The method for producing a semiconductor device according to
[19] or
[20] above, further comprising carrying out a high-temperature process (e.g., a high-temperature process at 100° C. or higher, preferably 60° C. or higher) after step (1) and before step (3).
[22] A high temperature exposure step of performing a high temperature process (e.g., a high temperature process of 100°C or higher, preferably 60°C or higher) after the above step (1) and before the above step (3); an irradiation step of irradiating the pressure-sensitive adhesive sheet with active energy rays, which is performed either before the step (3) or after the step (1); The method for manufacturing a semiconductor device according to
[19] above, further comprising:
[23] The method for producing a semiconductor device according to
[22] above, wherein the irradiation step is carried out after the high-temperature exposure step.
[24] The method for producing a semiconductor device according to
[22] above, wherein the irradiation step is carried out before the high-temperature exposure step.
[25] The method for producing a semiconductor device according to any one of
[19] to
[24] above, wherein the step (3) is carried out by a water stripping method. EXAMPLES
[0169] Some examples of the present invention will be described below, but it is not intended that the present invention be limited to those shown in these examples. In the following description, "parts" and "%" are by weight unless otherwise specified.
[0170] <Evaluation method> 1. Measurement of initial normal peel force Fd0 The pressure sensitive adhesive sheet to be measured is cut into a strip of 20 mm width to prepare a test piece. In an environment of 23°C and 50% RH, a 6-inch silicon wafer (6-inch N, manufactured by Shin-Etsu Chemical Co., Ltd.) is used as an adherend. <100> The adhesive side of the above test piece is attached to the mirror surface of a 100 mm thick paper (-100) using a hand roller, and left for 30 minutes to prepare a sample for evaluation. Thereafter, in an environment of 23°C and 50% RH, a cutter knife is inserted into the interface between the test piece of the evaluation sample and the adherend to peel one end of the test piece in the longitudinal direction from the adherend, and the peel strength is measured according to "10.4.1 Method 1: 180° peel adhesion to test plate" of JIS Z0237:2009, specifically, at a test temperature of 23°C using a tensile tester (Shimadzu Corporation's precision universal testing machine "Autograph EZ-S") at a tensile speed of 300 mm / min and a peel angle of 180°. The peel strength is measured so that the peel of the test piece attached to the adherend proceeds from bottom to top. The measurement is performed three times, and the average value is taken as the initial normal peel strength Fd0 [N / 20mm].
[0171] 2.Normal peel strength without heating Fd U1 Measurement An evaluation sample prepared in the same manner as in the measurement of the initial normal peel strength Fd0 is irradiated with ultraviolet light from the substrate side of the pressure-sensitive adhesive sheet (the side opposite the adhesive surface to be measured; hereinafter, also referred to as the "back side") under the following UV irradiation conditions A in an environment of 23°C and 50% RH. Then, in an environment of 23°C and 50% RH, a cutter knife is inserted into the interface between the test piece of the evaluation sample and the adherend to peel one end of the test piece in the longitudinal direction from the adherend, and the peel strength is measured in the same manner as in the measurement of the initial normal peel strength Fd0. The measurement is performed three times, and the average value is calculated as the non-heated normal peel strength Fd U1 [N / 20mm]. (UV irradiation condition A) UV irradiation equipment: Nitto Seiki Co., Ltd., product name "NEL SYSTEM UM810" (high pressure mercury lamp light source) Irradiation amount; illuminance 60mW / cm 2 , cumulative light intensity 1000mJ / cm 2
[0172] 3. Non-heated water peeling force Fw U1 Measurement The above non-heated normal peel strength Fd U1 In the measurement of Fw, 20 μL of distilled water is supplied to the location where the test piece starts to separate from the adherend (the peel front) while the test piece is being peeled off from the adherend, and the peel strength after the distilled water supply is measured. The measurement is performed for each peel strength measurement (i.e., three times), and the average value of these measurements is taken as the non-heated water peel strength Fw. U1 [N / 20mm].
[0173] 4. Measurement of normal peel strength after heating / UV (Normal peel force Fd a2 , Fd b2 Measurement of The evaluation sample prepared in the same manner as in the measurement of the initial normal peel strength Fd0 is heated at 175°C for 15 minutes. After heating, the sample is allowed to cool in a room temperature (25°C) environment for 30 minutes. After cooling, the sample is irradiated with ultraviolet light under the above UV irradiation conditions A, and the peel strength is measured in the same manner as in the measurement of the initial normal peel strength Fd0. The measurement is performed three times, and the average value is taken as the normal peel strength Fd by treatment procedure A. a2 [N / 20mm]. Normal peel force Fd by treatment procedure A b2 [N / 20mm] was measured using the normal peel force Fd according to the above procedure A, except that the heating conditions were changed to 200°C and 15 minutes. a2 This is done in the same manner as the measurement of . (Normal peeling force Fd a2 , Fd b2 Measurement of The evaluation sample prepared in the same manner as in the measurement of the initial normal peel strength Fd0 is irradiated with ultraviolet light under the above UV irradiation conditions A. The irradiated sample is heated at 175°C for 15 minutes, and then allowed to cool in a room temperature (25°C) environment for 30 minutes. After cooling, the above non-heated normal peel strength Fd U1 The peel strength is measured in the same manner as in the measurement of the normal peel strength Fd by the treatment procedure B. The measurement is carried out three times, and the average of the three measurements is taken as the normal peel strength Fd by the treatment procedure B. a2 [N / 20mm]. Normal peel force Fd by treatment procedure B b2 [N / 20mm] was measured using the normal peel force Fd according to the above procedure B, except that the heating conditions were changed to 200°C and 15 minutes. a2 This is done in the same manner as the measurement of .
[0174] 5. Measurement of water peeling force Fw2 after heating / UV (Water peeling force Fw a2 , Fw b2 Measurement of Normal peel force Fd after heat / UV treatment according to treatment procedure A above a2 , Fd b2 In the measurement of the peel strength after heating / UV, 20 μL of distilled water is supplied to the point where the test piece starts to separate from the adherend (the peel front) while the test piece is being peeled off from the adherend, and the peel strength after the supply of distilled water is measured. The measurement is performed for each peel strength measurement (i.e., three times), and the average value of these measurements is taken as the water peel strength after heating / UV, Fw. a2 , Fw b2 [N / 20mm]. (Water peeling force Fw a2 , Fw b2 Measurement of Normal peel force Fd after heat / UV treatment according to treatment procedure B above a2 , Fd b2 In the measurement of the peel strength after heating / UV, 20 μL of distilled water is supplied to the point where the test piece starts to separate from the adherend (the peel front) while the test piece is being peeled off from the adherend, and the peel strength after the supply of distilled water is measured. The measurement is performed for each peel strength measurement (i.e., three times), and the average value of these measurements is taken as the water peel strength after heating / UV, Fw. a2 , Fw b2 [N / 20mm].
[0175] <Example 1> (Preparation of Pressure-Sensitive Adhesive Composition) A monomer composition was prepared by mixing 100 parts of 2-ethylhexyl acrylate (2EHA), 25.5 parts of N-acryloylmorpholine (ACMO), and 18.5 parts of 2-hydroxyethyl acrylate (HEA) as monomer raw materials with 0.3 parts of benzoyl peroxide (BPO) as a polymerization initiator and toluene as a polymerization solvent. The above monomer composition was put into a polymerization experimental apparatus equipped with a 1-liter round-bottom separable flask, a separable cover, a separating funnel, a thermometer, a nitrogen inlet tube, a Liebig condenser, a vacuum seal, a stirring rod, and a stirring blade, and the mixture was substituted with nitrogen at room temperature for 6 hours while stirring. After that, the mixture was polymerized at 60°C for 8 hours under a nitrogen stream while stirring, to obtain a solution of polymer Q1. The weight-average molecular weight (Mw) of this polymer Q1 was about 900,000. The Tg calculated from the Fox formula based on the composition of the above monomer raw materials was -42.7°C.
[0176] After cooling the solution of polymer Q1 to room temperature, 12.3 parts of 2-isocyanatoethyl methacrylate (manufactured by Showa Denko K.K., trade name "Karenz MOI") was added, and 0.1 parts of dibutyltin (IV) dilaurate (manufactured by Wako Pure Chemical Industries, Ltd.) was further added. The mixture was stirred at 50°C for 24 hours in an air atmosphere to perform an addition reaction of MOI with polymer Q1, thereby obtaining a solution of polymer P1 having a carbon-carbon double bond. The amount of MOI used was determined based on the moles (M A ) and the moles of isocyanate groups (functional group B) contained in the above MOI (M B ) and the ratio (M A / M B ) is approximately 2.0.
[0177] To the solution of polymer P1, 5.0 parts of isocyanate-based crosslinking agent X1 (trimethylolpropane / tolylene diisocyanate trimer adduct, manufactured by Tosoh Corporation, product name "Coronate L", solid content concentration 75 wt%) was added based on solid content per 100 parts of polymer P1 in the solution, and 1 part of photoinitiator H1 (manufactured by IGM Regins, product name "Omnirad 369") was further added and mixed to prepare adhesive composition C1.
[0178] (Preparation and evaluation of adhesive sheets) The adhesive composition C1 was applied to the release surface of a 38 μm-thick release film R1 (Mitsubishi Plastics, MRF38) in which one side of a polyethylene terephthalate (PET) film was treated with silicone to form a release surface, and the adhesive composition C1 was dried at 140° C. for 2 minutes to form an adhesive layer with a thickness of 20 μm. The adhesive layer was attached to the easy-adhesion surface of an easy-adhesion treated PET film (thickness 50 μm) as a substrate, and then aged at 50° C. for 2 days to obtain an adhesive sheet according to this example. This adhesive sheet is an adhesive sheet with a substrate having an adhesive surface constituted by an active energy ray-curable adhesive layer. The obtained pressure-sensitive adhesive sheet was subjected to the above-mentioned method to measure the initial normal peel strength Fd0, non-heated normal peel strength Fd U1 , Non-heated water peeling force Fw U1 Furthermore, the normal peel force Fd a2 , Fd b2 and water peeling force Fw a2 , Fw b2 The peel force difference after heating / UV (Fd b2 -Fd a2 The results are shown in Table 1.
[0179] <Example 2> To the solution of the polymer P1, 0.50 parts of a nonionic surfactant A1 (polyoxyethylene sorbitan monolaurate, sorbitan fatty acid ester manufactured by Kao Corporation, product name "Rheodol TW-L 120", ethylene oxide added mole number 20, HLB 16.7), which is a compound A that dissolves in ethyl acetate without phase separation in the above-mentioned test I, was further added per 100 parts of the polymer P1 in the solution as a heat-resistant release agent. Except for the above points, the pressure-sensitive adhesive composition C2 was prepared in the same manner as the preparation of the pressure-sensitive adhesive composition C1. The nonionic surfactant A1 was used in the form of an ethyl acetate solution so that the above amount was added based on the solid content. The same applies to the preparation of the following pressure-sensitive adhesive compositions C3 to C5. An adhesive sheet according to this example was obtained in the same manner as in Example 1, except that the above adhesive composition C2 was used. The obtained pressure-sensitive adhesive sheet was evaluated in the same manner as in Example 1. The results are shown in Table 1.
[0180] <Example 3> A solution of polymer P2 having a carbon-carbon double bond was obtained in the same manner as in the synthesis of polymer P1, except that the amount of 2-isocyanatoethyl methacrylate (manufactured by Showa Denko K.K., product name "Karenz MOI") added to the solution of polymer Q1 was changed to 22.5 parts. The amount of MOI used was determined based on the moles (M A ) and the moles of isocyanate groups (functional group B) contained in the above MOI (M B ) and the ratio (M A / M B ) is approximately 1.1. To the solution of polymer P2, 0.5 parts of nonionic surfactant A1 and 5.0 parts of isocyanate-based crosslinking agent X1 were added per 100 parts of polymer P2 in the solution, and 1 part of photoinitiator H1 was further added and mixed to prepare pressure-sensitive adhesive composition C3.
[0181] (Preparation and evaluation of adhesive sheets) An adhesive sheet according to this example was obtained in the same manner as in the preparation of the adhesive sheet according to Example 1, except that the above adhesive composition C3 was used. The obtained pressure-sensitive adhesive sheet was evaluated in the same manner as in Example 1 (Example 3A). In addition, the normal peel strength Fd a2 , Fd b2 and water peeling force Fw a2 , Fw b2 The peel force difference after heating / UV (Fd b2 -Fd a2 The results are shown in Table 1. The initial normal peel strength Fd0 and the non-heated normal peel strength Fd U1 and non-heated water peeling force Fw U1 The column shows the same measurements as in Example 3A.
[0182] <Example 4> (Preparation of Pressure-Sensitive Adhesive Composition) A monomer composition was prepared by mixing 100 parts of n-butyl acrylate (BA), 78 parts of ethyl acrylate (EA) and 40 parts of HEA as monomer feedstocks with 0.3 parts of BPO and toluene as a polymerization solvent. The above monomer composition was put into a 1L round bottom separable flask, a polymerization experimental apparatus equipped with a separable cover, a separating funnel, a thermometer, a nitrogen inlet tube, a Liebig condenser, a vacuum seal, a stirring rod, and a stirring blade, and the mixture was substituted with nitrogen at room temperature for 6 hours while stirring. After that, the mixture was polymerized under a nitrogen stream at 60°C for 6 hours and then at 78°C for 1 hour, to obtain a solution of polymer Q3 (Mw about 500,000). The Tg calculated from the Fox formula based on the composition of the above monomer raw materials is -37.2°C. After cooling the solution of polymer Q3 to room temperature, 43.6 parts of 2-isocyanatoethyl methacrylate (manufactured by Showa Denko K.K., trade name "Karenz MOI") was added, and 0.2 parts of dibutyltin (IV) dilaurate (manufactured by Wako Pure Chemical Industries, Ltd.) was further added, and the mixture was stirred at 50°C for 24 hours in an air atmosphere to perform an addition reaction of MOI with polymer Q3, thereby obtaining a solution of polymer P3 having a carbon-carbon double bond. The amount of MOI used was determined based on the moles (M A) and the moles of isocyanate groups (functional group B) contained in the above MOI (M B ) and the ratio (M A / M B ) is approximately 1.2.
[0183] (Preparation and evaluation of adhesive sheets) To the solution of polymer P3, 0.5 parts of nonionic surfactant A1 and 5.0 parts of isocyanate-based crosslinking agent X1 were added per 100 parts of polymer P3 in the solution, and 1 part of photoinitiator H1 was further added and mixed to prepare pressure-sensitive adhesive composition C4. An adhesive sheet according to this example was obtained in the same manner as in the preparation of the adhesive sheet according to Example 1, except that the above adhesive composition C4 was used. The obtained pressure-sensitive adhesive sheet was evaluated in the same manner as in Example 1 (Example 4A). In addition, the normal peel strength Fd a2 , Fd b2 and water peeling force Fw a2 , Fw b2 The peel force difference after heating / UV (Fd b2 -Fd a2 The results are shown in Table 1. The initial normal peel strength Fd0 and the non-heated normal peel strength Fd U1 and non-heated water peeling force Fw U1 The column shows the same measurements as in Example 4A.
[0184] <Example 5> The amount of the isocyanate-based crosslinking agent X1 per 100 parts of the polymer P3 was changed to 1.0 part based on the solid content, and the adhesive composition C5 was prepared in the same manner as the adhesive composition C4. The adhesive sheet of this example was obtained in the same manner as the adhesive sheet of Example 1, except that the adhesive composition C5 was used. The obtained pressure-sensitive adhesive sheet was evaluated in the same manner as in Example 1. The results are shown in Table 1.
[0185] <Example 6> A pressure-sensitive adhesive composition C6 was prepared in the same manner as in Example 5, except that the nonionic surfactant A1 was not used. A pressure-sensitive adhesive sheet according to this example was obtained in the same manner as in the preparation of the pressure-sensitive adhesive sheet according to Example 1, except that the pressure-sensitive adhesive composition C6 was used. The obtained pressure-sensitive adhesive sheet was evaluated in the same manner as in Example 1. The results are shown in Table 1.
[0186] [Table 1]
[0187] As shown in Table 1, among the pressure-sensitive adhesive sheets of Examples 1 to 6 which were subjected to heat / UV treatment by treatment procedure A, Examples 3 to 6 had clearly reduced peel strength after exposure to high temperatures compared to the pressure-sensitive adhesive sheets of Examples 1 and 2. Moreover, Examples 3B and 4B which were subjected to heat / UV treatment by treatment procedure B had lower peel strength after exposure to high temperatures compared to Examples 3A and 4A which were subjected to treatment procedure A.
[0188] Although specific examples of the present invention have been described in detail above, these are merely examples and do not limit the scope of the claims. The technology described in the claims includes various modifications and changes of the specific examples exemplified above. [Explanation of symbols]
[0189] 1,2,3,4,5,6 Adhesive sheet 10 Base material 10A front page 10B Second side 21, 22 Adhesive layer 21A First adhesive side 21B Second adhesive surface 31,32 Release liner
Claims
1. An adhesive sheet for semiconductor processing comprising an adhesive layer constituting an adhesive surface, the pressure-sensitive adhesive layer contains a polymer having a carbon-carbon double bond as a base polymer, the pressure-sensitive adhesive layer further comprises, relative to 100 parts by weight of the base polymer, 0.05 parts by weight or more and 12 parts by weight or less of a crosslinking agent and 0.1 parts by weight or more and 3 parts by weight or less of a compound A; The base polymer is a polymer obtained by chemically modifying a primary polymer obtained by copolymerizing a monomer having a functional group A with a compound having a functional group B and a carbon-carbon double bond, and the molar ratio (M A ) and the moles of functional group B (M B ) to the molar ratio (M A / M B ) is in the range of more than 1.0 and not more than 1.5, The compound A is at least one compound selected from the group consisting of surfactants and compounds having a polyoxyalkylene skeleton, The adhesive surface of the adhesive sheet is attached to a silicon wafer, and the adhesive sheet is subjected to a heat treatment at 175° C. for 15 minutes with an integrated light dose of 1000 mJ / cm 2 2 After the ultraviolet irradiation treatment, the normal peel strength Fd is measured under the conditions of a pulling speed of 300 mm / min and a peel angle of 180 degrees. a2 The adhesive sheet for semiconductor processing has a compressive strength of 0.50 N / 20 mm or less.
2. The adhesive surface is attached to a silicon wafer, and the wafer is subjected to a heat treatment at 175°C for 15 minutes with an accumulated light dose of 1000 mJ / cm 2 After the ultraviolet irradiation treatment, water is supplied to the peel front of the pressure-sensitive adhesive sheet from the silicon wafer, and the water peel force Fw is measured under the conditions of a pulling speed of 300 mm / min and a peel angle of 180 degrees. a2 The adhesive sheet for semiconductor processing according to claim 1, wherein the adhesive strength is 0.30 N / 20 mm or less.
3. The adhesive surface is attached to a silicon wafer, and the wafer is subjected to a heat treatment at 200°C for 15 minutes and an accumulated light dose of 1000 mJ / cm 2 After the ultraviolet irradiation treatment, the normal peel strength Fd is measured under the conditions of a pulling speed of 300 mm / min and a peel angle of 180 degrees. b2 The adhesive sheet for semiconductor processing according to claim 1, wherein the compressive strength is 2.00 N / 20 mm or less.
4. The adhesive surface is attached to a silicon wafer, and the wafer is subjected to a heat treatment at 200°C for 15 minutes and an accumulated light dose of 1000 mJ / cm 2 After the ultraviolet irradiation treatment, water is supplied to the peel front of the pressure-sensitive adhesive sheet from the silicon wafer, and the water peel force Fw is measured under the conditions of a pulling speed of 300 mm / min and a peel angle of 180 degrees. b2 The adhesive sheet for semiconductor processing according to claim 1, wherein the compressive strength is 1.00 N / 20 mm or less.
5. The adhesive surface was attached to a silicon wafer, and the wafer was subjected to a heat treatment at 175° C. for 15 minutes with an integrated light dose of 1000 mJ / cm 2 2 Normal peel strength Fd measured under conditions of a pulling speed of 300 mm / min and a peel angle of 180 degrees after ultraviolet irradiation treatment. a2 [N / 20 mm], and the normal peel force Fd is the same as above, except that the heat treatment is performed at 200° C. for 15 minutes instead of at 175° C. for 15 minutes. a2 Normal peel force Fd measured in the same manner as b2 [N / 20mm], the following formula: Fd b2 -Fd a2 The adhesive sheet for semiconductor processing according to any one of claims 1 to 4, wherein the normal peel force difference calculated by the above formula is 1.50 N / 20 mm or less.
6. After the adhesive surface is attached to a silicon wafer, the initial normal peel force Fd is measured under the conditions of a tensile speed of 300 mm / min and a peel angle of 180 degrees. 0 The adhesive sheet for semiconductor processing according to any one of claims 1 to 5, wherein the compressive strength is 0.30 N / 20 mm or more.
7. The adhesive surface is attached to a silicon wafer, and an integrated light dose of 1000 mJ / cm 2 After the ultraviolet irradiation treatment, the non-heated normal peel strength Fd is measured under the conditions of a pulling speed of 300 mm / min and a peel angle of 180 degrees. U1 The adhesive sheet for semiconductor processing according to any one of claims 1 to 6, wherein the adhesive strength is 0.10 N / 20 mm or less.
8. The adhesive surface is attached to a silicon wafer, and an integrated light quantity of 1000 mJ / cm 2 After the ultraviolet irradiation treatment, water is supplied to the peel front of the pressure-sensitive adhesive sheet from the silicon wafer, and the non-heated water peel force Fw is measured under the conditions of a pulling speed of 300 mm / min and a peel angle of 180 degrees. U1 The adhesive sheet for semiconductor processing according to any one of claims 1 to 7, wherein the compressive strength is 0.050 N / 20 mm or less.
Citation Information
Patent Citations
Adhering and peeling method
JP2002203821A
Adhesive sheet for processing semiconductor wafer and / or substrate
JP2008103516A
Surface protection sheet
JP2017088823A
Back grind tape
JP2017212441A
Adhesieve sheet for temporary-attamchment and methode for producing semiconductor device using the same
KR1020190113633A