Method for producing porous resin sheet, flow path-containing sheet and roll body

By forming a pore-forming agent-containing resin sheet and channel-containing sheet in a roll body, the method ensures efficient extraction of the porosity agent, addressing non-uniform electrical characteristics and discoloration issues in porous resin sheets.

JP7555253B2Active Publication Date: 2024-09-24NITTO DENKO CORP
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
JP2020203638
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2019-12-19
Filing Date
2020-12-08
Publication Date
2024-09-24
Estimated Expiration
2040-12-08

AI Technical Summary

Technical Problem

The existing method for producing porous resin sheets using supercritical carbon dioxide extraction results in non-uniform electrical characteristics and discoloration due to incomplete extraction of the porosity-forming agent, as the radially outer and inner surfaces of the membrane are in contact with the copper foil, leading to uneven porosity and electrical properties.

Method used

A method involving the formation of a pore-forming agent-containing resin sheet and a channel-containing sheet, which are wound together to form a roll body, allowing supercritical fluid to flow through channels with a volume ratio of 50% or more, ensuring efficient extraction of the porosity agent and uniform electrical characteristics.

Benefits of technology

This method produces a porous resin sheet with suppressed discoloration and uniform electrical properties in the radial direction by efficiently extracting the porosity agent, maintaining consistent electrical characteristics throughout the roll body.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007555253000006
    Figure 0007555253000006
  • Figure 0007555253000007
    Figure 0007555253000007
  • Figure 0007555253000002
    Figure 0007555253000002
Patent Text Reader

Abstract

To provide a method for producing a porous resin sheet in which discoloration is suppressed, a flow channel-containing sheet used in the same, and a roll body having a porous resin sheet.SOLUTION: A method for producing a porous resin sheet 1 includes: a first step of forming a porous agent-containing resin sheet 3 containing a resin and a porous agent 6; a second step of bringing a flow channel-containing sheet 4 having a flow channel therein into contact with one surface in a thickness direction of the porous agent-containing resin sheet 3, and preparing a roll body 5 constituted by winding a porous agent-containing laminate 9 having the porous agent-containing resin sheet 3 and the flow channel-containing sheet 4 in a thickness direction in order; and a third step of circulating a supercritical fluid in the flow channel-containing sheet 4 of the roll body 5, extracting a porous agent 6 by the supercritical fluid, and preparing a porous resin sheet 1. A volume ratio of the flow channel in the flow channel-containing sheet 4 determined by a mercury press-in method according to JIS R 1655 (2003) is 50% or more.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for producing a porous resin sheet, a flow path-containing sheet, and a roll body. [Background technology]

[0002] In recent years, it has become known that porous resin sheets are used for various industrial applications.

[0003] In an industrial manufacturing method of such a porous resin sheet, a solution containing a porogen and a resin precursor is applied to a long copper foil, dried to obtain a film, and then the film is wound into a roll to create a roll. In this roll, the film has a microphase structure in which a discontinuous phase of the porogen is dispersed in a continuous phase of the resin precursor. Then, the porogen is extracted from the film in the roll by supercritical carbon dioxide to form a porous resin sheet with a porous structure (see, for example, Patent Document 1 below). [Prior art documents] [Patent documents]

[0004] [Patent Document 1] International Publication No. 2018 / 186486 Summary of the Invention [Problem to be solved by the invention]

[0005] However, in the method described in Patent Document 1, the outer and inner radial surfaces of the membrane in the roll are in contact with the copper foil, so that the supercritical carbon dioxide cannot sufficiently contact both sides of the membrane. Therefore, the porosity-inducing agent cannot be sufficiently extracted from the membrane. As a result, the porous resin sheet has a problem in that the color of the porousness-inducing agent is changed due to a large amount of the remaining porosity-inducing agent.

[0006] In addition, the extraction efficiency of the porosifying agent in the porous resin sheet in the inner part of the wound body is likely to be significantly different from that in the porous resin sheet in the outer part of the wound body, which causes a problem that the electrical characteristics of the porous resin sheet in the inner part of the wound body are significantly different from that in the porous resin sheet in the inner part of the wound body. In other words, there is a problem that the electrical characteristics of the porous resin sheet become non-uniform in the radial direction of the wound body.

[0007] The present invention provides a method for producing a porous resin sheet in which discoloration is suppressed and unevenness in electrical properties in the radial direction of the roll is suppressed, a flow path-containing sheet used therein, and a roll body including a porous resin sheet. [Means for solving the problem]

[0008] The present invention (1) includes a method for producing a porous resin sheet, the method comprising: a first step of forming a porogen-containing resin sheet containing a resin and a porogen; a second step of bringing a flow path-containing sheet having a flow path therein into contact with one surface in the thickness direction of the porogen-containing resin sheet, and winding a laminate having the porogen-containing resin sheet and the flow path-containing sheet in order in the thickness direction to produce a roll body; and a third step of circulating a supercritical fluid through the flow path-containing sheet of the roll body to extract the porogen with the supercritical fluid, thereby producing a porous resin sheet, wherein the volume ratio of the flow paths in the flow path-containing sheet, as determined by mercury intrusion porosimetry in accordance with JIS R 1655 (2003), is 50% or more.

[0009] According to this manufacturing method, the supercritical fluid can be smoothly passed through the flow path-containing sheet having a flow path volume ratio of 50% or more, and the porogen can be efficiently extracted by the supercritical fluid, so that a porous resin sheet can be manufactured in which discoloration caused by the porogen remaining in the porous resin sheet is suppressed.

[0010] Furthermore, according to this manufacturing method, since the supercritical fluid can be smoothly circulated through the flow path-containing sheet in which the volume ratio of the flow paths is 50% or more, in the third step, the extraction efficiency of the porosifying agent in the porous resin sheet in the inner part of the roll body can be made close to the extraction efficiency of the porosifying agent in the porous resin sheet in the outer part of the roll body. Therefore, the electrical characteristics of the porous resin sheet in the inner part of the roll body can be made close to the electrical characteristics of the porous resin sheet in the inner part of the roll body. In other words, it is possible to prevent the electrical characteristics of the porous resin sheet from becoming non-uniform in the radial direction of the roll body.

[0011] The present invention (2) includes the method for producing a porous resin sheet according to (1), wherein the median size of the flow paths, as determined by the mercury intrusion porosimetry, is 30 μm or more and 250 μm or less.

[0012] In this manufacturing method, since the median size of the flow passage is 250 μm or less, the supercritical fluid can be uniformly contacted with one surface in the thickness direction of the flow passage-containing sheet in the third step, and therefore a homogeneous porous resin sheet can be manufactured. Also, since the median size of the flow passage is 30 μm or more, the porosifying agent can be efficiently extracted in the third step.

[0013] The present invention (3) includes the method for producing a porous resin sheet described in (1) or (2), in which the ratio of the volume of the flow path to the mass of the flow path-containing sheet, determined by the mercury intrusion method, is 1 mL / g or more.

[0014] In this manufacturing method, the ratio of the volume of the flow path to the mass of the flow path-containing sheet is 1 mL / g or more as described above, so that the volume ratio of the flow path in the flow path-containing sheet can be reliably adjusted to the desired value, specifically, to 50% or more.

[0015] The present invention (4) includes the method for producing a porous resin sheet according to any one of (1) to (3), in which the static friction coefficient of the flow path-containing sheet determined by a static friction coefficient test method conforming to JIS K 7125 (1999) is 0.6 or less.

[0016] In this manufacturing method, since the static friction coefficient of the flow path-containing sheet is 0.6 or less, even if the flow path-containing sheet swells due to the flow of a supercritical fluid through the flow path-containing sheet in the third step, the stress applied from the flow path-containing sheet to the porogen-containing resin sheet can be reduced, and therefore the occurrence of wrinkles in the roll body due to the increase in the above-mentioned stress can be suppressed.

[0017] The present invention (5) includes the method for producing a porous resin sheet according to any one of (1) to (4), wherein the flow path-containing sheet is made of fibers and / or mesh.

[0018] According to this manufacturing method, since the flow channel-containing sheet is formed from fibers and / or mesh, the flow channel-containing sheet can reliably form flow channels, and therefore the supercritical fluid can reliably circulate within the flow channel-containing sheet.

[0019] The present invention (6) includes a flow path-containing sheet used in the method for producing a porous resin sheet according to any one of (1) to (5).

[0020] By passing a supercritical fluid through a flow path-containing sheet in which the volume ratio of the flow paths is 50% or more, the porogen can be efficiently extracted by the supercritical fluid. Therefore, a porous resin sheet can be manufactured in which discoloration caused by the porogen remaining in the porous resin sheet is suppressed. In addition, in the third step, the extraction efficiency of the porogen in the porous resin sheet in the inner part of the roll body can be made even closer to the extraction efficiency of the porogen in the porous resin sheet in the outer part of the roll body. Therefore, it is possible to further suppress the electrical properties of the porous resin sheet from becoming non-uniform in the radial direction of the roll body.

[0021] The present invention (7) includes a roll body in which a porous resin sheet and a void-containing sheet having voids therein are arranged alternately toward the outside in the radial direction so as to be in contact with each other, and the volume fraction of the voids in the void-containing sheet determined by mercury intrusion porosimetry in accordance with JIS R 1655 (2003) is 50% or more.

[0022] This roll body includes a void-containing sheet with a void volume ratio of 50% or more, so that the porosifying agent is efficiently extracted by the supercritical fluid. Therefore, discoloration of the porous resin sheet caused by the porosifying agent remaining in the porous resin sheet is suppressed. In addition, this roll body can suppress the electrical properties of the porous resin sheet from becoming non-uniform in the radial direction of the roll body. Effect of the Invention

[0023] The method for producing a porous resin sheet and the flow path-containing sheet of the present invention can produce a porous resin sheet in which discoloration is suppressed and non-uniformity in electrical properties in the radial direction of the roll body is suppressed.

[0024] In the roll body of the present invention, discoloration of the porous resin sheet is suppressed. [Brief description of the drawings]

[0025] [Figure 1] 1A to 1C are manufacturing process diagrams of one embodiment of the manufacturing method for a porous resin sheet of the present invention, in which FIG. 1A shows a first step of forming a porogen-containing resin sheet, FIG. 1B shows a second step of forming a roll body, and FIG. 1C shows a third step of extracting the porogen to manufacture a porous resin sheet and a porous roll body comprising the same. [Diagram 2] FIG. 2 is an exploded perspective view of the supercritical fluid device and the roll body in the third step. [Diagram 3] FIG. 3 is a cross-sectional view of the supercritical fluid device and the roll body in the third step. [Figure 4] Figures 4A to 4C are cross-sectional views of a porous resin sheet obtained by the manufacturing method shown in Figures 1A to 1C and examples of its use, where Figure 4A shows a porous laminate, Figure 4B shows a step of removing a flow path-containing sheet from the porous laminate, and Figure 4C shows a step of patterning a base sheet. [Diagram 5]5A and 5B are modified examples of the embodiment shown in FIGS. 1B and 1C (an embodiment in which the porosifying-agent-containing laminate does not include a base sheet), in which FIG. 5A shows a step of winding the porosifying-agent-containing laminate to produce a roll body, and FIG. 5B is a cross-sectional view of the porous roll body including a porous resin sheet. [Figure 6] 6A and 6B are modified examples of the embodiment shown in FIGS. 1B and 1C (an embodiment in which the porogen-containing laminate does not include a second flow path-containing sheet), in which FIG. 6A shows a step of winding the porogen-containing laminate to produce a roll body, and FIG. 6B is a cross-sectional view of the porous roll body including a porous resin sheet. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0026] An embodiment of the method for producing a porous resin sheet of the present invention will be described with reference to Figs. 1 to 4C.

[0027] The method for producing a porous resin sheet 1 includes a first step (see FIG. 1A) of forming a porogen-containing resin sheet 3 on one surface in the thickness direction of a base sheet 2, a second step (see FIG. 1B) of contacting a flow path-containing sheet 4 with one surface in the thickness direction of the porogen-containing resin sheet 3 to produce a roll body 5, and a third step (see FIG. 1C) of circulating a supercritical fluid through the flow path-containing sheet 4 of the roll body 5 to extract the porogen 6 with the supercritical fluid to produce a porous resin sheet 1. In this production method, the first step to the third step are carried out in order.

[0028] The base sheet 2 has a predetermined thickness and is in the form of a long flat belt. Examples of the material of the base sheet 2 include metals and resins. Examples of the metals include copper, iron, silver, gold, aluminum, nickel, and alloys thereof (stainless steel, bronze). Examples of the resins include polymers such as polyolefins, such as polyethylene and polypropylene, and polyesters, such as polyethylene terephthalate. These materials are used alone or in combination. Among these materials, from the viewpoint of patterning the base sheet 2 to form the wiring 29 (see FIG. 4C), preferably, metals are used, and more preferably, copper is used. If the material of the base sheet 2 is a metal, it can be precisely patterned to function as the wiring 29. The thickness of the base sheet 2 is, for example, 0.1 μm or more, preferably 1 μm or more, and, for example, 100 μm or less, preferably 50 μm or less.

[0029] Examples of the material for the porogene-containing resin sheet 3 include resins such as thermosetting resins and thermoplastic resins.

[0030] Examples of thermosetting resins include polycarbonate resins, thermosetting polyimide resins, thermosetting fluorinated polyimide resins, epoxy resins, phenolic resins, urea resins, melamine resins, diallyl phthalate resins, silicone resins, thermosetting urethane resins, fluororesins (fluorine-containing olefin polymers (specifically, polytetrafluoroethylene (PTFE) and the like)), liquid crystal polymers (LCPs), etc. These can be used alone or in combination of two or more.

[0031] Examples of thermoplastic resins include olefin resins, acrylic resins, polystyrene resins, polyester resins, polyacrylonitrile resins, maleimide resins, polyvinyl acetate resins, ethylene-vinyl acetate copolymers, polyvinyl alcohol resins, polyamide resins, polyvinyl chloride resins, polyacetal resins, polyphenylene oxide resins, polyphenylene sulfide resins, polysulfone resins, polyethersulfone resins, polyetheretherketone resins, polyarylsulfone resins, thermoplastic polyimide resins, thermoplastic fluorinated polyimide resins, thermoplastic urethane resins, polyetherimide resins, polymethylpentene resins, cellulose resins, liquid crystal polymers, ionomers, etc. These can be used alone or in combination of two or more.

[0032] Among the above-mentioned resins, from the viewpoint of mechanical strength, preferably, a thermosetting resin is used, more preferably, a polyimide resin is used. Details of the physical properties and manufacturing method of the above-mentioned suitable resins are described in, for example, JP2018-021171A and JP2018-021172A.

[0033] To form the porogen-containing resin sheet 3 on the base sheet 2, first, prepare a varnish containing the above-mentioned resin precursor, the porogen (reference numeral 6 in FIG. 1A), a nucleating agent (PTFE, etc.), and a solvent (NMP, etc.). The types and blending ratios of the porogen 6, nucleating agent, and solvent in the varnish are described, for example, in JP-A-2018-021171 and JP-A-2018-021172. In particular, the porogen is preferably polyoxyethylene dimethyl ether, and the ratio is preferably 20 parts by mass or more, more preferably 50 parts by mass or more, and even more preferably 100 parts by mass or more, relative to 100 parts by mass of the precursor, and is, for example, 500 parts by mass or less, more preferably 400 parts by mass or less, and even more preferably 300 parts by mass or less.

[0034] Next, the varnish is applied to one surface in the thickness direction of the base sheet 2 to form a coating film. The coating film is then dried by heating. By heating, a part of the solvent in the varnish is removed from the porogen-containing resin sheet 3, and a phase-separated structure of the porogen 6 and the precursor 7 is formed with the nucleating agent as a nucleus.

[0035] In this way, a porogen-containing resin sheet 3 having at least the porogen 6 therein is formed on one surface of the base sheet 2 in the thickness direction.

[0036] The porogene-containing resin sheet 3 has a predetermined thickness and has the same shape as the base sheet 2 in a plan view.

[0037] The porogen-containing resin sheet 3 has a hardness that allows it to maintain its shape (specifically, its thickness and the flatness of one side and the other side in the thickness direction) even when it is included in a roll body 5 (see FIG. 1B), that is, when it is wound around the roll body 5. Specifically, the tensile modulus of the porogen-containing resin sheet 3 at 25° C. is the tensile modulus of the porogen-containing resin sheet 3 in the B stage when it contains a thermosetting resin, and is, for example, 0.1 GPa or more, preferably 1 GPa or more. The tensile modulus of the porogen-containing resin sheet 3 at 25° C. is, for example, 10 GPa or less, preferably 5 GPa or less.

[0038] The thickness T1 of the porogen-containing resin sheet 3 is, for example, 1 μm or more, preferably 2 μm or more, more preferably 5 μm or more, and for example, 1,000 μm or less, preferably 500 μm or less, more preferably 300 μm or less. If the thickness T1 of the porogen-containing resin sheet 3 is the above-mentioned lower limit or more, the mechanical strength of the porogen-containing laminate 9 can be improved. If the thickness T1 of the porogen-containing resin sheet 3 is the above-mentioned upper limit or less, the porogen 6 can be efficiently extracted from the porogen-containing resin sheet 3.

[0039] In the second step, the flow path-containing sheet 4 is brought into contact with one surface in the thickness direction of the porogen-containing resin sheet 3 .

[0040] As shown in FIG. 1A, the flow path-containing sheet 4 has a predetermined thickness and is in the form of a long flat belt.

[0041] Specifically, the flow channel-containing sheet 4 is formed, for example, from fibers and / or mesh. Fibers are mesh-like sheets that are not fused or woven. In contrast, mesh is a mesh-like sheet that is fused or woven. As a result, the flow channel-containing sheet 4 has voids (gaps) partitioned by the fibers and / or mesh. The flow channel-containing sheet 4 is also a void-containing sheet 14. These voids form flow channels for the supercritical fluid flowing through the flow channel-containing sheet 4.

[0042] The presence or absence of fibers in the flow path-containing sheet 4 and the presence or absence of woven fibers can be confirmed by observation with an optical microscope.

[0043] Preferably, the flow path-containing sheet 4 is made of fibers. Fibers are advantageous because they have better continuity in the longitudinal direction of the flow paths than meshes. The average fiber length is, for example, 100 nm or more and, for example, 10 μm or less, and the average fiber thickness is, for example, 3 nm or more and, for example, 50 nm or less.

[0044] The material of the flow channel-containing sheet 4 is not particularly limited as long as it is substantially insoluble in the supercritical fluid, and examples thereof include organic materials, inorganic materials, and hybrid materials thereof. Examples of organic materials include cellulose, polyester (PET, PBT, etc.), polyolefin (polyethylene, polypropylene, etc.), polyacetal, polyamide, polycarbonate, polyimide, polyether ether ketone, polyether sulfone, and polyphenylene oxide. Examples of inorganic materials include metals such as copper, iron, aluminum, and stainless steel. The material of the flow channel-containing sheet 4 is preferably an organic material, and more preferably cellulose from the viewpoint of reducing the amount of supercritical carbon dioxide dissolved in the flow channel-containing sheet 4.

[0045] The shape of the voids is not particularly limited, but is preferably continuous at least in the longitudinal direction and thickness direction.

[0046] The volume fraction of the flow channels in the flow channel-containing sheet, as determined by mercury intrusion porosimetry in accordance with JIS R 1655 (2003), is, in percentage, 50% or more, preferably 60% or more, more preferably 70% or more, even more preferably 75% or more, and particularly preferably 80% or more. The volume fraction of the flow channels is, for example, 95% or less, preferably 90% or less. The volume fraction of the flow channels is synonymous with the volume fraction of voids.

[0047] If the volume ratio of the flow paths is less than 50%, the porogen 6 cannot be efficiently extracted in the third step described below, and therefore discoloration caused by a large amount of the porogen 6 remaining in the porous resin sheet 1 cannot be suppressed, and the electrical properties of the porous resin sheet 1 become non-uniform in the radial direction of the porous roll body 15. In other words, if the volume ratio of the flow paths is equal to or greater than the above-mentioned lower limit, the porogen 6 can be efficiently extracted in the third step, and therefore discoloration caused by the porogen 6 remaining in the porous resin sheet 1 can be suppressed. Furthermore, the electrical properties of the porous resin sheet 1 can be made uniform in the radial direction of the porous roll body 15.

[0048] In addition, if the volume ratio of the flow paths is equal to or less than the above-mentioned upper limit, the flow paths of the flow path-containing sheet 4 in the roll body 5 can be reliably secured.

[0049] The method for determining the volume ratio of the flow path will be described in detail in the Examples.

[0050] The median size of the flow path determined by mercury intrusion porosimetry in accordance with JIS R 1655 (2003) is, for example, 10 μm or more, preferably 30 μm or more, more preferably 40 μm or more, and for example, 250 μm or less, preferably 150 μm or less, more preferably 100 μm or less.

[0051] If the median size of the flow paths is equal to or less than the above upper limit, the supercritical fluid can be uniformly brought into contact with one surface in the thickness direction of the flow path-containing sheet 4 in the third step, and therefore a homogeneous porous resin sheet 1 can be produced.

[0052] If the median size of the flow path is equal to or greater than the above-mentioned lower limit, the porosifying agent 6 can be efficiently extracted in the third step.

[0053] When the channels are pores, the median size of the channels is determined as the "pore diameter" in the channel-containing sheet 4. The median size of the channels (median diameter) will be described in detail in the Examples.

[0054] The ratio (mL / g) of the volume (mL) of the flow path to the mass (g) of the flow path-containing sheet 4 determined by mercury intrusion porosimetry in accordance with JIS R 1655 (2003) is, for example, 0.75 mL / g or more, preferably 1 mL / g or more, more preferably 2 mL / g or more, even more preferably 3 mL / g or more, particularly preferably 4 mL / g or more, and for example, 10 mL / g or less, preferably 9 mL / g or less, more preferably 8 mL / g or less, even more preferably 7 mL / g or less, and particularly preferably 6 mL / g or less.

[0055] If the ratio (mL / g) of the volume of the flow passage to the mass of the flow passage-containing sheet 4 is equal to or greater than the above-mentioned lower limit, the volume ratio of the flow passage in the flow passage-containing sheet can be adjusted to a desired value (50% or more). Therefore, the supercritical fluid can be smoothly circulated through the flow passage-containing sheet, and the porogen can be efficiently extracted by the supercritical fluid. As a result, a porous resin sheet can be manufactured in which discoloration caused by the porogen remaining in the porous resin sheet is suppressed.

[0056] The method for determining the ratio of the volume of the flow passage to the mass of the flow passage-containing sheet 4 will be described in detail in the Examples.

[0057] The static friction coefficient of the flow path-containing sheet 4, as determined by a static friction coefficient test method conforming to JIS K 7125 (1999), is, for example, 0.80 or less, preferably 0.70 or less, more preferably 0.60 or less, and is, for example, 0.20 or more, preferably 0.30 or more.

[0058] If the static friction coefficient of the flow path-containing sheet 4 is equal to or less than the above upper limit, even if a supercritical fluid flows through the flow path-containing sheet 4 in the roll body 5 in the third step and the flow path-containing sheet 4 swells, the stress applied from the flow path-containing sheet 4 to the porogen-containing resin sheet 3 can be reduced. Therefore, the occurrence of wrinkles in the roll body 5 due to the increase in the above-mentioned stress can be suppressed.

[0059] On the other hand, if the static friction coefficient of the flow path-containing sheet 4 is equal to or greater than the lower limit described above, the slippage when winding the porosifier-containing laminate 9 becomes excessive, and winding misalignment may occur between the flow path-containing sheet 4 and the porosifier-containing resin sheet 3 on the roll body 5.

[0060] A detailed method for measuring the static friction coefficient of the flow channel-containing sheet 4 will be described in the examples below.

[0061] The thickness T2 of the flow path-containing sheet 4 is, for example, 10 μm or more, preferably 20 μm or more, more preferably 100 μm or more, and for example, 800 μm or less, preferably 400 μm or less, more preferably 200 μm or less.

[0062] If the thickness T2 of the flow path-containing sheet 4 is equal to or greater than the above-mentioned lower limit, a sufficient amount of supercritical fluid can flow smoothly through the flow path-containing sheet 4.

[0063] If the thickness T2 of the flow path-containing sheet 4 is equal to or less than the above upper limit, the thickness of the flow path-containing sheet 4 per unit thickness of the roll body 5 can be reduced. Therefore, the thickness of the porous resin sheet 1 per unit thickness of the roll body 5 can be increased. Therefore, the production efficiency of the roll body 5 can be improved.

[0064] The ratio (T2 / T1) of the thickness T2 of the flow path-containing sheet 4 to the thickness T1 of the porosifying agent-containing resin sheet 3 is, for example, 0.3 or more, preferably 0.5 or more, more preferably more than 1, and for example, 20 or less, preferably 10 or less, more preferably 5 or less. When the ratio (T2 / T1) of the thickness T2 of the flow path-containing sheet 4 is within the above-mentioned range, the porosifying agent 6 can be efficiently extracted from the porosifying agent-containing resin sheet 3 while the roll body 5 is produced with good productivity.

[0065] The flow path-containing sheet 4 may be a commercially available product. For example, the Bemliese series (manufactured by Asahi Kasei Corporation) may be used as a flow path-containing sheet 4 made of fiber, and the Mesh #2500 series (manufactured by KB Seiren) may be used as a flow path-containing sheet 4 made of mesh.

[0066] 1A and the left side of FIG. 1B, to form the porogen-containing resin sheet 3 on one thickness-wise surface of the base sheet 2, the porogen-containing resin sheet 3 is placed on one thickness-wise surface of the base sheet 2. Specifically, the other thickness-wise surface of the porogen-containing resin sheet 3 and one thickness-wise surface of the base sheet 2 are brought into contact with each other.

[0067] In this way, a sheet-like porogen-containing laminate (porogen-containing laminate sheet) 9 is obtained, which comprises the base sheet 2, the porogen-containing resin sheet 3, and the flow path-containing sheet 4 in that order toward one side in the thickness direction.

[0068] Next, the porosifying agent-containing laminate 9 is wound. Specifically, one end in the longitudinal direction of the porosifying agent-containing laminate 9 is fixed to the surface of the core 8, and then the intermediate part and the other end in the longitudinal direction of the porosifying agent-containing laminate 9 are wound around the core 8. The core 8 is a winding core and has a substantially cylindrical or columnar shape.

[0069] For example, the porogene-containing laminate 9 is wound around the core 8 so that one end of the base sheet 2 in the longitudinal direction is in contact with the surface of the core 8 .

[0070] As a result, a layer structure is formed on the radially outer side of the core 8, in which the base sheet 2, the porogen-containing resin sheet 3, and the flow path-containing sheet 4 are repeatedly arranged.

[0071] In this way, a roll body 5 is produced, which has the core 8 and the base sheet 2, the porogen-containing resin sheet 3, and the flow path-containing sheet 4, which are repeatedly arranged radially outwardly of the core 8.

[0072] 2, the outer diameter R1 of the roll body 5 is (R2+2×R3) obtained by adding the outer diameter R2 of the core 8 to twice the total thickness R3 of the base sheet 2, the porogen-containing resin sheet 3, and the flow path-containing sheet 4. The outer diameter R1 of the roll body 5 is substantially the same as the inner diameter ID of the tank body 22 in the third step.

[0073] As shown in FIGS. 2 and 3, in the third step, the roll body 5 is set in the supercritical fluid extraction device 20, and then the supercritical fluid is caused to flow through the roll body 5.

[0074] Examples of the supercritical fluid include supercritical carbon dioxide and supercritical nitrogen, and preferably supercritical carbon dioxide.

[0075] The supercritical fluid extraction apparatus 20 includes, for example, an extraction tank 21, and a circulation device (not shown) and a storage tank (not shown) connected to the extraction tank 21.

[0076] The extraction tank 21 includes, for example, a tank body 22 having a substantially cylindrical shape with a bottom whose axis extends along a vertical line and opens upward, and a lid 23 that closes the open end (upper end) of the tank body 22. The tank body 22 integrally includes a disk-shaped bottom wall 25 and a peripheral side wall 24 that extends upward from the peripheral edge of the bottom wall 25. The peripheral side wall 24 has a cylindrical shape. The inner diameter ID of the peripheral side wall 24 is the same as the outer diameter R1 of the roll body 5 described above. The bottom wall 25 and the lid 23 each have an inlet 26 and an outlet 27 for the supercritical fluid. In addition, the bottom wall 25 and the lid 23 each have a fixing portion 28 that fixes both axial ends of the core 8.

[0077] The circulation device (not shown) includes a pump and piping. The pump compresses a gas (such as carbon dioxide) to generate a supercritical fluid (such as supercritical carbon dioxide). The piping is connected to the inlet 26 and outlet 27 described above, and forms a circulation path for the supercritical fluid.

[0078] A storage tank (not shown) is connected midway through the piping. The capacity of the storage tank is greater than the capacity of extraction tank 21. The capacity of the storage tank relative to an internal volume of extraction tank 21 of 100 parts by volume is, for example, 500 parts by volume or more, or even 1000 parts by volume or more, and is, for example, 100,000 parts by volume or less.

[0079] To set the roll body 5 in the supercritical fluid extraction apparatus 20, one end of the core 8 of the roll body 5 is fixed to the fixing portion 28 of the bottom wall 25. At this time, the outer peripheral surface of the roll body 5 and the inner peripheral surface of the peripheral side wall 24 are in contact with each other. In addition, the surfaces of the base sheet 2, the porosifying agent-containing resin sheet 3, and the flow path-containing sheet 4 on one width direction side (one axial direction side of the core 8) in the roll body 5 are spaced apart from the bottom surface of the bottom wall 25 and the inlet 26.

[0080] Thereafter, the peripheral side wall 24 is closed with the lid 23. At this time, the other end of the core 8 is fixed to the fixing part 28 of the lid 23. At this time, the surfaces on the other width direction side (the other axial direction side of the core 8) of the base sheet 2, the porosifying agent-containing resin sheet 3, and the flow path-containing sheet 4 in the roll body 5 are spaced apart from the bottom surface of the bottom wall 25 and the outlet 27.

[0081] The supercritical fluid extraction device 20 may be any of various commercially available supercritical fluid extraction devices (eg, manufactured by Mitsubishi Kako, ITEC, Toyo Koatsu, and Kobe Steel Air Tech).

[0082] Then, the supercritical fluid extraction device 20 is driven. Specifically, a supercritical fluid is generated by driving the pump, and the supercritical fluid flows into the extraction tank 21 from the inlet 26, and then flows through the flow path-containing sheet 4. In the flow path-containing sheet 4, the supercritical fluid moves upward along the axial direction of the core 8, contacts the porogen-containing resin sheet 3, and extracts the porogen 6 in the porogen-containing resin sheet 3. The supercritical fluid from which the porogen 6 has been extracted, that is, the supercritical fluid containing the porogen 6, is stored in a storage tank (not shown) through a pipe from the outlet 27. A part of the supercritical fluid containing the porogen 6 is depressurized in the storage tank and returns to gas, and the remaining part circulates again through the circulation path and is sent to the extraction tank 21.

[0083] In the roll body 5, the flow path-containing sheet 4 is allowed to swell due to the flow of the supercritical fluid through the inside, and this allows the flow path-containing sheet 4 to apply stress to the porogen-containing resin sheet 3. However, since the static friction coefficient of the flow path-containing sheet 4 is equal to or lower than the above-mentioned upper limit, the above-mentioned stress is reduced.

[0084] As a result, the porogen 6 in the porogen-containing resin sheet 3 is extracted by the supercritical fluid through the flow path-containing sheet 4. In other words, the porogen 6 is removed from the porogen-containing resin sheet 3.

[0085] The extraction rate of the porosifying agent 6 is the ratio ([M1-M2] / M1) of the mass (M1) of the porosifying agent 6 contained in the porosifying agent-containing resin sheet 3 to the mass (M1) of the porosifying agent 6 remaining in the porous resin sheet 1 minus the mass (M2) of the porosifying agent 6 remaining in the porous resin sheet 1, and is, for example, 35% or more, preferably 45% or more, more preferably 50% or more, and for example, 90% or less.

[0086] The extraction rate of the porosity-forming agent 6 (specifically, the object to be extracted that contains the porosity-forming agent 6) is determined as follows, taking as an example a case where the resin is a polyimide resin and the solvent is NMP.

[0087] Approximately 3 mg of each of the porogen-containing resin sheet 3 before extraction and the porous resin sheet 1 after extraction is taken, placed in an aluminum pan for measurement, and set in a thermogravimetric-differential calorimeter. The thermogravimetric-differential calorimeter is heated from 23°C to 450°C, and the mass ratio of the extraction target (NMP, porogen, water) and the mass ratio of the polyimide resin contained in the porogen-containing resin sheet 3 before extraction and the porous resin sheet 1 after extraction are calculated as follows. Mass ratio of the extracted material = [Sample mass before heating (g) - Sample mass after heating (g)] / Sample mass before heating (g) Mass ratio of polyimide resin = 1-Mass ratio of the object to be extracted Based on this, the extraction rate is calculated as follows:

[0088] (Definition of symbols) Mass of porosifying agent-containing resin sheet 3 sample before extraction: A (g) Mass ratio of the object to be extracted in the three samples of the resin sheet containing the porosifying agent before extraction: R A Mass ratio of polyimide in the three samples of porosifying agent-containing resin sheets before extraction: P A Mass of one porous resin sheet sample after extraction: B (g) Mass ratio of the extracted object in one sample of porous resin sheet after extraction: R B Mass ratio of polyimide in one sample of porous resin sheet after extraction: P B

[0089] Here, since the remaining extraction target is uniformly distributed in the porous resin sheet 1 after extraction, regardless of the value of the mass B of the porous resin sheet 1 sample after extraction, R B and P B The value of is constant. On the premise of this, the mass of polyimide in the porosifying agent-containing resin sheet sample 3 before extraction is the same as the mass of polyimide in the porous resin sheet sample 1 after extraction, that is, B=(P A / P B)A is true, calculate the extraction rate.

[0090] Extraction rate (%) = (mass (g) of extracted object to be extracted / mass (g) of object to be extracted in 3 samples of porogene-containing resin sheet before extraction) x 100 ={[A-(P A / P B )A] / (R A A)}×100 =[(P B -P A ) / (R A P B )] x 100

[0091] In addition, the porous resin sheet 1 can be collected from a location 16 (inner part of the roll body 5) 1 mm radially outward from the surface of the core 8 in the roll body 5, and used as a sample of the inner part 16. A sample can be collected from a location 17 (outer part of the roll body 5) 1 mm radially inward from the surface (outer surface) of the roll body 5 in the roll body 5, and used as a sample of the outer part 17. In the roll body 5, the outer part 17 is disposed radially outward at a distance from the inner part 16. The extraction rates of the sample of the inner part 16 and the sample of the outer part 17 can be determined in the same manner as above.

[0092] The ratio of the extraction efficiency of the porosifying agent in the inner portion 16 to the extraction efficiency of the porosifying agent in the outer portion 17 is, for example, 0.3 or more, preferably 0.5 or more, more preferably 0.8 or more, even more preferably 0.90 or more, particularly preferably 0.95 or more, and is, for example, 2 or less, preferably 1.5 or less, more preferably 1.00 or less. When the above ratio is equal to or more than the above lower limit and equal to or less than the above upper limit, it is possible to suppress the electrical properties of the porous resin sheet 1 from becoming non-uniform in the radial direction of the porous roll body 15.

[0093] If necessary, the porogene-containing resin sheet 3 is heated to promote imidization if the precursor is a polyimide precursor. This brings the porogene-containing resin sheet 3 into the C stage. The heating temperature is, for example, 200° C. or more, preferably 300° C. or more, and, for example, 500° C. or less, preferably 400° C. or less.

[0094] 1C, the roll body 5 is thereby transformed into a porous roll body 15 including a porous laminate 19 (see FIG. 4A). The porous roll body 15 includes a base sheet 2, a porous resin sheet 1, and a flow path-containing sheet 4, which are repeatedly arranged radially outward.

[0095] The porosity of the porous resin sheet 1 is, for example, 60% or more, more preferably 70% or more, even more preferably 80% or more, and particularly preferably 85% or more. The porosity of the porous resin sheet 1 is, for example, less than 100%, or even 99% or less. The porosity can be determined, for example, by image analysis of a cross-sectional SEM photograph of the porous resin sheet 1. Alternatively, the porosity can be calculated based on the following formula (1).

[0096] Porosity (%) = (1 - specific gravity of porogen-containing resin sheet 3 / specific gravity of porogen-containing resin sheet 3) x 100 (1)

[0097] The dielectric constant of the porous resin sheet 1 at a frequency of 10 GHz is, for example, 2.5 or less, preferably 2.0 or less, and for example, more than 1.0. The dielectric constant of the porous resin sheet 1 is actually measured by a resonator method using a frequency of 10 GHz.

[0098] The dielectric constants of the porous resin sheet 1 of the inner portion 16 and the porous resin sheet 1 of the outer portion 17 can be obtained in the same manner as described above. The dielectric constants of the inner portion 16 and the outer portion 17 are within the above-mentioned ranges. The ratio of the dielectric constant of the inner portion 16 to the dielectric constant of the outer portion 17 is, for example, more than 0.95, preferably 0.97 or more, more preferably 0.98 or more, and even more preferably 0.99 or more, and is, for example, 1.5 or less, preferably 1.2 or less, and more preferably 1.1 or less. If the ratio is equal to or more than the above-mentioned lower limit and equal to or less than the above-mentioned upper limit, the dielectric constant of the porous resin sheet 1 in the radial direction of the porous roll body 15 can be suppressed from becoming non-uniform.

[0099] The dielectric loss tangent of the porous resin sheet 1 at a frequency of 10 GHz is, for example, 0.01 or less, preferably 0.005 or less, and is, for example, greater than 0. The dielectric loss tangent of the porous resin sheet 1 is actually measured by a resonator method using a frequency of 10 GHz.

[0100] The dielectric loss tangents of the porous resin sheet 1 of the inner portion 16 and the porous resin sheet 1 of the outer portion 17 can be obtained in the same manner as above. The dielectric loss tangents of the inner portion 16 and the outer portion 17 are within the above-mentioned ranges. The ratio of the dielectric loss tangent of the inner portion 16 to the dielectric loss tangent of the outer portion 17 is, for example, more than 0.80, preferably 0.85 or more, more preferably 0.90 or more, and is, for example, 1.5 or less, preferably 1.2 or less, more preferably 1.1 or less. If the ratio is equal to or more than the above-mentioned lower limit and equal to or less than the above-mentioned upper limit, the dielectric loss tangent of the porous resin sheet 1 in the radial direction of the porous roll body 15 can be prevented from becoming non-uniform.

[0101] The thickness T5 of the porous resin sheet 1 is substantially the same as the thickness of the porogen-containing resin sheet 3.

[0102] Such a porous resin sheet 1 is preferably compatible with the fifth generation (5G) standard and high-speed FPC and is used as a low dielectric substrate material.

[0103] For example, a sheet-shaped porous laminate 19 shown in Fig. 4A is unwound from a roll 5 shown in Fig. 1C. Then, as shown in Fig. 4B, the flow path-containing sheet 4 is removed from the porous laminate 19. Specifically, the flow path-containing sheet 4 is peeled off from one surface of the porous resin sheet 1 in the thickness direction.

[0104] 4C, when the material of the base sheet 2 is a metal, the base sheet 2 is patterned into wiring 29 for an antenna or a high-speed FPC board compatible with the fifth generation (5G) standard. Specifically, the base sheet 2 is etched (wet etched).

[0105] <Effects of one embodiment> According to this manufacturing method, in the third step, the supercritical fluid can be smoothly circulated through the flow path-containing sheet 4 in which the volume ratio of the flow paths is 50% or more, and the porogen 6 can be efficiently extracted by the supercritical fluid. Therefore, it is possible to manufacture a porous resin sheet 1 in which discoloration caused by the porogen 6 remaining in the porous resin sheet 1 is suppressed.

[0106] Furthermore, according to this manufacturing method, since the supercritical fluid can be smoothly circulated through the flow path-containing sheet 4 in which the volume ratio of the flow paths is 50% or more, in the third step, the extraction efficiency of the porogen in the porogen-containing resin sheet 3 in the inner portion 16 of the roll body 5 can be made close to the extraction efficiency of the porogen in the porogen-containing resin sheet 3 in the outer portion of the roll body 5. Therefore, the electrical characteristics of the porous resin sheet 1 in the inner portion of the porous roll body 15 can be made close to the electrical characteristics of the porous resin sheet 1 in the inner portion of the porous roll body 15. In other words, it is possible to suppress the electrical characteristics of the porous resin sheet 1 from becoming non-uniform in the radial direction of the porous roll body 15.

[0107] Furthermore, if the median size of the flow paths is 250 μm or less, the supercritical fluid can be uniformly brought into contact with one surface in the thickness direction of the flow path-containing sheet 4 in the third step, and therefore a homogeneous porous resin sheet 1 can be produced. If the median size of the flow paths is 30 μm or more, the porosifying agent 6 can be efficiently extracted in the third step.

[0108] Furthermore, if the ratio of the volume of the flow channels to the mass of the flow channel-containing sheet 4 is equal to or higher than the above-mentioned lower limit, the volume ratio of the flow channels in the flow channel-containing sheet 4 can be reliably adjusted to a desired value, specifically, 50% or more.

[0109] If the static friction coefficient of the flow path-containing sheet 4 is 0.6 or less, even if a supercritical fluid flows through the flow path-containing sheet 4 in the third step and the flow path-containing sheet 4 swells, the stress applied from the flow path-containing sheet 4 to the porogen-containing resin sheet 3 can be reduced. Therefore, the occurrence of wrinkles in the roll body 5 due to the increase in the above-mentioned stress can be suppressed.

[0110] Furthermore, if the flow channel-containing sheet 4 is formed from fibers and / or mesh, the flow channels can be reliably formed in the flow channel-containing sheet 4. Therefore, the supercritical fluid can be reliably circulated within the flow channel-containing sheet 4.

[0111] Since the porous roll body 15 includes the void-containing sheet 14 with a void volume ratio of 50% or more, a supercritical fluid is passed through the void-containing sheet 14, and the porosifying agent 6 is efficiently extracted by the supercritical fluid. Therefore, it is possible to manufacture a porous resin sheet 1 in which discoloration caused by the porosifying agent 6 remaining in the porous resin sheet 1 is suppressed. Furthermore, with this porous roll body 15, it is possible to suppress the dielectric constant and dielectric loss tangent of the porous resin sheet from becoming non-uniform in the radial direction of the porous roll body 15.

[0112] <Modification> Next, modified examples of one embodiment will be described. In each of the following modified examples, the same reference numerals are used for the same members and steps as those of the above-described one embodiment, and detailed descriptions thereof will be omitted. In addition, one embodiment and each modified example can be appropriately combined. Furthermore, each modified example can achieve the same effects as the one embodiment, unless otherwise specified.

[0113] As shown in Fig. 5A, each of the porogen-containing laminate 9 and the roll body 5 does not include a base sheet 2, but only includes a porogen-containing resin sheet 3 and a flow path-containing sheet 4 (void-containing sheet 14). As shown in Fig. 5B, the porous roll body 15 does not include a base sheet 2, but only includes a porous resin sheet 1 and a flow path-containing sheet 4 (void-containing sheet 14). Although not shown in Figs. 5A and 5B, the porous laminate 19 does not include a base sheet 2, but only includes a porous resin sheet 1 and a flow path-containing sheet 4 (void-containing sheet 14).

[0114] 6A, each of the porogen-containing laminate 9 and the roll body 5 includes a second flow path-containing sheet 44 in place of the base sheet 2. That is, each of the porogen-containing laminate 9 and the roll body 5 includes a second flow path-containing sheet 44, a porogen-containing resin sheet 3, and a flow path-containing sheet 4 (void-containing sheet 14) in that order toward one side in the thickness direction.

[0115] As shown in Fig. 6B, the porous roll body 15 comprises a second flow path-containing sheet 44, a porous resin sheet 1, and a flow path-containing sheet 4 (void-containing sheet 14). Although not shown in Figs. 6A to 6B, the porous laminate 19 comprises the second flow path-containing sheet 44, a porous resin sheet 1, and a flow path-containing sheet 4 (void-containing sheet 14). The proportion of flow paths in the second flow path-containing sheet 44 is not particularly limited, and is preferably 50% or more.

[0116] In one embodiment, as shown in Fig. 3, in the third step, the supercritical fluid flows from the bottom to the top in extraction tank 21. On the other hand, in a modified example (not shown), in the third step, the supercritical fluid flows from the top to the bottom in extraction tank 21.

[0117] In a modified embodiment (not shown), the axis of extraction tank 21 is aligned horizontally. The supercritical fluid flows through extraction tank 21 horizontally. EXAMPLES

[0118] The present invention will be described in more detail below with reference to examples and comparative examples. The present invention is not limited to the examples and comparative examples. The specific numerical values ​​of the blending ratio (content ratio), physical property values, parameters, etc. used in the following description can be replaced with the upper limit (a numerical value defined as "not more than" or "less than") or lower limit (a numerical value defined as "not less than" or "exceeding") of the corresponding blending ratio (content ratio), physical property values, parameters, etc. described in the above "Form for carrying out the invention".

[0119] Example 1 In a 3000 mL flask equipped with a stirrer and a thermometer, 130 g of p-phenylenediamine (PDA) and 60 g of diaminophenyl ether (DPE) were placed, and 2960 g of N-methyl-2-pyrrolidone (NMP) was added as a solvent and stirred to dissolve. Next, 441 g of biphenyltetracarboxylic dianhydride (BPDA) was gradually added to this solution, stirred at room temperature for 3 hours, heated to 80°C, and then stirred for 20 hours to obtain a polyimide precursor solution.

[0120] To the polyimide precursor solution, 200 parts by weight of polyoxyethylene dimethyl ether (manufactured by NOF Corp., grade: MM400) having a weight average molecular weight of 400 as a porosifying agent and 3 parts by weight of PTFE powder having a particle size of 1 μm or less as a nucleating agent were added to 100 parts by weight of the polyimide resin precursor, and the mixture was stirred to prepare a transparent and uniform varnish. The varnish was applied to one side in the thickness direction of a substrate sheet 2 made of copper foil having a thickness of 12.5 μm, and dried with hot air at 120° C. for 7 minutes to prepare a porosifying agent-containing resin sheet 3 having a phase separation structure with a thickness T1 of 60 μm (see FIG. 1A). In the above drying, a part of the NMP was removed from the porosifying agent-containing resin sheet 3.

[0121] Thereafter, Bemliese SH25G (thickness T2: 160 μm) (manufactured by Asahi Kasei Corporation) made of fiber was prepared as the flow path-containing sheet 4. The flow path-containing sheet 4 was brought into contact with one surface in the thickness direction of the porogen-containing resin sheet 3 to prepare a porogen-containing laminate 9 including the base sheet 2, the porogen-containing resin sheet 3, and the flow path-containing sheet 4 in that order toward one side in the thickness direction.

[0122] As shown in FIG. 1B and FIG. 2, the porosi-agent-containing laminate 9 was wound around a stainless steel core 8 having an outer diameter R2 of 280 mm to prepare a roll body 5 having an outer diameter R1 of 1700 mm.

[0123] Next, a supercritical fluid extraction apparatus 20 manufactured by Kobe Steel Air-Tech Co., Ltd. was prepared as shown in Figures 2 and 3. The inner diameter ID of the tank body 22 in the supercritical fluid extraction apparatus 20 was 1700 mm.

[0124] The roll body 5 was housed in the tank body 22 of the supercritical fluid extraction device 20 , and the lid 23 was attached to the tank body 22 while both ends of the core 8 were fixed by the bottom wall 25 and the lid 23 .

[0125] Then, supercritical carbon dioxide at 60°C and 30 MPa was circulated through the extraction tank 21 at 60 kg / hour. The supercritical carbon dioxide was circulated through the flow path-containing sheet 4 along the axial direction of the core 8, and extracted the porosifying agent 6 from the porosifying agent-containing resin sheet 3. At the same time, the remaining NMP was extracted into the supercritical fluid. As a result, a porous roll body 15 including a porous resin sheet 1 in the B stage was obtained, as shown in FIG. 1C.

[0126] Thereafter, the porous roll body 15 was removed from the supercritical fluid extraction apparatus 20 .

[0127] Thereafter, a porous laminate 19 including the porous resin sheet 1 was unwound from the porous roll body 15 and heated for 2 hours in a heating device at 380°C to bring the porous resin sheet 1 to the C stage. After that, the porous laminate 19 was wound up around another core 8, and the porous roll body 15 was obtained again.

[0128] Example 2 3, Reference Example 4 and Comparative Example 1 The same treatment as in Example 1 was carried out except that the type of flow path-containing sheet 4 was changed according to Table 1.

[0129] (evaluation) The following items were measured, and the results are shown in Table 1. (1) Measurement of channels (voids) in a channel-containing sheet using mercury intrusion porosimetry Mercury intrusion method according to JIS R 1655 (2003) was performed on the flow path-containing sheet 4 to determine the volume fraction (%) of the flow paths in the flow path-containing sheet 4, the median size (μm) of the flow paths, and the ratio (mL / g) of the volume of the flow paths to the mass of the flow path-containing sheet 4.

[0130] Specifically, about 0.03 to 0.4 g of the flow path-containing sheet 4 was placed in a 5 mL cell, which was then set in a pore size distribution measuring device (product name "Autopore IV", Model 9520, manufactured by Shimadzu Corporation-Micromeritics) to carry out mercury intrusion porosimetry. In the mercury intrusion porosimetry, the initial pressure was set to 2.6 kPa. In addition, in the mercury intrusion porosimetry, the contact angle of mercury was set to 130 degrees, and the surface tension of mercury was set to 0.485 N / m to calculate the above-mentioned physical properties.

[0131] In this way, the volume ratio (%) of the flow paths in the flow path-containing sheet was determined.

[0132] In addition, the integrated value of the volume of mercury forced into the flow channel up to the maximum pressure measured was divided by the weight of the sample to obtain the ratio (mL / g) of the volume of the flow channel to the mass of the flow channel-containing sheet.

[0133] Furthermore, in the cumulative pore (channel) distribution, the midpoint (μm) between the minimum and maximum pore volumes on the curve was determined as the median of the channel size.

[0134] (2) Static friction coefficient of the channel-containing sheet The static friction coefficient of the flow path-containing sheet 4 was measured in accordance with the friction coefficient test method of JIS K 7125 (with spring).

[0135] In the friction coefficient test method of JIS K 7125, a sliding sample of 63×63 mm and a fixed sample of 300×200 mm were prepared from the flow path-containing sheet 4. The sliding sample was fixed to the back of a box-shaped weight of 200 g, the same size as the sliding piece. The weight was pulled horizontally with a force of 10 N at a speed of 100 mm / min. The test atmosphere was a temperature of 23±2°C and a humidity of 50±10% RH. The maximum load in the above tension was taken as the static friction force, and the static friction coefficient μ was obtained by dividing this by the weight of the weight (200 g). This was repeated four times, and the average value of the five times was obtained as the "static friction coefficient of the flow path-containing sheet."

[0136] (3) Observation of porous resin sheet (discoloration, wrinkles) After extraction, the base sheet 2 of the porous roll body 15 was observed to visually check for discoloration and wrinkles.

[0137] (4) Porosity of Porous Resin Sheet The porosity of the porous resin sheet 1 was calculated based on the following formula.

[0138] Dielectric constant of porous resin sheet 1=dielectric constant of air×porosity+dielectric constant of polyimide×(1-porosity) Here, the dielectric constant of air is 1 and the dielectric constant of polyimide is 3.6, so Dielectric constant of porous resin sheet 1=porosity+3.6(1-porosity) Porosity=(3.6-dielectric constant of porous resin sheet 1) / 2.6 Porosity (%)=[(3.6-dielectric constant of porous resin sheet 1) / 2.6]×100

[0139] (5) Dielectric constant and dielectric loss tangent of porous resin sheet The dielectric constants at a frequency of 10 GHz of the porous resin sheet 1 in the inner portion 16 of the porous roll body 15 and the porous resin sheet 1 in the outer portion 17 of the porous roll body 15 were determined by a resonator method. The dielectric tangents of the porous resin sheet 1 in the inner portion 16 of the porous roll body 15 and the porous resin sheet 1 in the outer portion 17 of the porous roll body 15 were also determined in the same manner as above.

[0140] (6) Extraction rate of porosifier The extraction rates of the porosifying agent in the porous resin sheet 1 (porosifying agent-containing resin sheet 3) in the inner portion 16 of the porous roll body 15 (roll body 5) and in the porous resin sheet 1 (porosifying agent-containing resin sheet 3) in the outer portion 17 were determined according to the method described in the above-mentioned embodiment.

[0141] [Table 1] [Explanation of symbols]

[0142] 1 Porous resin sheet 3. Porous agent-containing resin sheet 4. Flow path-containing sheet 5 Roll body 9. Porous agent-containing laminate 15 Porous roll body

Claims

1. A first step of forming a porogene-containing resin sheet containing a resin and a porogene-containing agent; a second step of contacting a flow path-containing sheet having a flow path therein with one surface in a thickness direction of the porogen-containing resin sheet, and winding a laminate including the porogen-containing resin sheet and the flow path-containing sheet in that order in a thickness direction to prepare a roll body; A third step of passing a supercritical fluid through the flow path-containing sheet of the roll body and extracting the porosifying agent with the supercritical fluid to produce a porous resin sheet; a volume ratio of the flow passage in the flow passage-containing sheet determined by mercury intrusion porosimetry in accordance with JIS R 1655 (2003) is 50% or more; A method for producing a porous resin sheet, characterized in that the flow path-containing sheet has a static friction coefficient of 0.6 or less, as determined by a static friction coefficient test method in accordance with JIS K 7125 (1999).

2. The method for producing a porous resin sheet according to claim 1 , wherein a median size of the flow paths determined by the mercury intrusion method is 30 μm or more and 250 μm or less.

3. 3. The method for producing a porous resin sheet according to claim 1, wherein a ratio of a volume of the flow path to a mass of the flow path-containing sheet, determined by the mercury intrusion method, is 1 mL / g or more.

4. The method for producing a porous resin sheet according to any one of claims 1 to 3, wherein the flow path-containing sheet is made of fiber and / or mesh.

5. A flow path-containing sheet, which is used in the method for producing a porous resin sheet according to any one of claims 1 to 4.

6. The porous resin sheets and the void-containing sheets having voids therein are alternately arranged toward the outside in the radial direction so as to be in contact with each other, The volume fraction of the voids in the void-containing sheet, as determined by mercury intrusion porosimetry in accordance with JIS R 1655 (2003), is 50% or more; A roll body, characterized in that the static friction coefficient of the porous sheet determined by a static friction coefficient testing method in accordance with JIS K 7125 (1999) is 0.6 or less.

Citation Information

Patent Citations

  • Manufacturing method of porous membrane

    JP2006100120A

  • Method for producing thermosetting resin porous sheet, and composite separation membrane using the same

    JP2012031399A

  • Film for millimetric wave antenna

    JP2019123851A

  • Film for millimeter-wave antenna

    WO2018186486A1