Crimped multicomponent fiber
Multicomponent fibers with asymmetric ethylene/alpha-olefin interpolymer regions address the need for improved crimpability and efficiency, enhancing the performance of polyethylene-based fibers in non-woven fabrics.
Patent Information
- Application Number
- JP2021525858
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2018-11-20
- Filing Date
- 2019-11-20
- Publication Date
- 2024-09-24
- Estimated Expiration
- 2039-11-20
AI Technical Summary
There is a need to develop fibers with improved crimpability and efficiency in crimping, particularly for polyethylene-based fibers used in non-woven fabrics, to enhance their performance in applications such as filters and disposable medical materials.
The development of multicomponent fibers with distinct regions of ethylene/alpha-olefin interpolymer compositions, characterized by specific comonomer distribution and molecular weight profiles, which are arranged asymmetrically to achieve enhanced crimpability.
The fibers exhibit a unique and unexpected degree of crimpability, leading to improved processability and crimp formation, resulting in higher performance in non-woven fabrics.
Smart Images

Figure 0007555338000024 
Figure 0007555338000023 
Figure 0007555338000008
Abstract
Description
[Technical field]
[0001] CROSS-REFERENCE TO RELATED APPLICATIONS This application claims the benefit of U.S. Application No. 62 / 769,615, filed November 20, 2018, which is incorporated by reference in its entirety.
[0002] The field of the invention is crimped or curled fibers of ethylene / alpha-olefin polymers. [Background technology]
[0003] Polyethylene-based fibers are used in consumer products, especially nonwoven fabrics. Such fibers are desirable due to their drapeability and smoothness. Nonwoven fabrics have a myriad of applications, such as filters, disposable materials in medical applications, and diaper stock. It has been proposed to crimp or crinkle the fibers to reduce the weight of the final product.
[0004] There remains a need to form fibers with improved crimpability (also known as crimp), and to be able to do so efficiently. Summary of the Invention
[0005] Disclosed herein are multicomponent fibers that exhibit a unique and unexpected degree of crimpability or crimp as compared to multicomponent fibers having different component polyethylene-based materials.
[0006] Specifically disclosed herein is a crimped fiber having a fiber centroid, comprising a first region having a first centroid and a second region having a second centroid, the first region comprising an ethylene / alpha olefin interpolymer composition in an amount of at least 75 weight percent based on the total weight of the first region, the ethylene / alpha olefin interpolymer composition characterized by a low temperature peak and a high temperature peak in an elution profile via an improved comonomer composition distribution (ICCD) procedure, the high temperature peak having a full width at half maximum of less than 6.0° C., the second region being a material comprising a polymer different from the ethylene / alpha-olefin interpolymer of the first region, the regions being positioned such that at least one of the first centroid and the second centroid is not the same as the fiber centroid.
[0007] As used herein, fiber centroid means the arithmetic average of all points in the cross section of the fiber. For an area, the centroid means the arithmetic average of all points in the area as viewed in the cross section of the fiber. [Brief description of the drawings]
[0008] [Figure 1] 1 is an ICCD elution plot of the ethylene / alpha-olefin composition of Sample 1. [Diagram 2] This is a scanning electron microscope (SEM) cross-sectional image of a highly eccentric core-sheath structure fiber made using the resin of sample 1 as the sheath and polypropylene as the core. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0009] Disclosed herein are crimped multicomponent fibers having at least first and second regions. The fibers may be characterized as eccentric (i.e., the cross section of the fiber is not symmetrical in at least one view point, e.g., not a concentric core / sheath, etc.).
[0010] The fibers may be bicomponent fibers. The fibers may have three or more components. The fibers may have a core-sheath configuration, where the cross section of the fiber shows one region (core) surrounded by another region (sheath). In multicomponent fibers, there may be one or more internal cores, one or more internal sheaths, and an external sheath. The fibers may have a side-by-side configuration. The fibers may have a segmented pie configuration, where the cross section of the fiber shows one region occupying a portion, for example, a quarter, a third, half of the cross section, and a second region occupies the remainder of the cross section. In multicomponent fibers, a third or fourth region may occupy a portion of the pie cross section. In multicomponent fibers, the core-sheath configuration may be combined with a segmented pie. For example, the core may have two components in a segmented pie structure surrounded by a sheath. In a multicomponent system, a third component may be contained within a first or second region of an islands-in-the-sea configuration. For example, the third component may form a separate region within the first region that forms the core and is surrounded by the sheath.
[0011] A fiber has a center of gravity, and each region of a fiber has its own center of gravity. As used herein, center of gravity means the arithmetic average of all points of the area of the cross section of the fiber. In a concentric core-sheath, the fiber, the core region, and the sheath region have substantially the same center of gravity. The fiber center of gravity and the center of gravity of either the first region or the second region, or both, may be different. At least two of the regions may have different centers of gravity. These latter configurations are also referred to as eccentric configurations. The center of gravity of a fiber is C f and the center of gravity of the region can be expressed as C rx For example, the first region may be represented as r1 C f The average distance from the fiber to the outer surface is "r" and can be calculated as follows:
number
[0012] The inventors have found that using a particular ethylene / alpha-olefin interpolymer composition as described herein in one of the regions improves crimp, while the fiber includes a different polymer in one of the other regions.
[0013] Ethylene / Alpha-Olefin Interpolymer An important feature of the nonwoven fabric is the fiber made of a specific ethylene / alpha-olefin interpolymer composition. By interpolymer, it is meant that the polymer is a polymer of two, three, or more monomers, i.e., a copolymer, a terpolymer, etc. In this case, the first monomer is ethylene. The second monomer is an alpha-olefin. Such alpha-olefins have at least three carbon atoms and can have, for example, up to 20, or up to 10, or up to 8 carbon atoms. Exemplary α-olefin comonomers include, but are not limited to, propylene, 1-butene, 1-pentene, 1-hexene, 1-heptene, 1-octene, 1-nonene, 1-decene, and 4-methyl-1-pentene. The optional third, fourth, or more monomers can be alpha-olefins. The interpolymer composition is bimodal and can be conveniently made by combining two ethylene / alpha olefin interpolymers having different molecular weights and / or different densities and / or at least two different peaks in the ICCD elution, as described in more detail below.
[0014] The interpolymer may be a random interpolymer. The interpolymer may comprise at least 50 mole percent, or at least 60 mole percent, or at least 70 mole percent, of ethylene-based repeat units, based on the total moles of repeat units in the interpolymer. The interpolymer may comprise 99.9 or less, or 99.5 or less, or 99 or less, or 95 or less, or 90 or less, or 85 mole percent or less, of ethylene-based repeat units, based on the total moles of repeat units in the interpolymer. The interpolymer may comprise at least 0.1, or at least 0.5, or at least 1, or at least 5, or at least 10 mole percent, of alpha-olefin-based repeat units, based on the total moles of repeat units in the interpolymer (i.e., the second, and optional third and fourth monomers). The interpolymer may comprise 50 or less, or 30 or less, of alpha-olefin-based repeat units, based on the total moles of repeat units in the interpolymer (i.e., the second, and optional third and fourth monomers).
[0015] These ethylene / alpha-olefin interpolymer compositions have a viscosity of at least 0.930 g / cm 3 , and 0.965g / cm3 or less, or 0.940g / cm 3 The bicomponent fibers comprising the disclosed ethylene / alpha olefin interpolymers may be characterized by the following density. Density is measured according to ASTM D792. The bicomponent fibers comprising the disclosed ethylene / alpha olefin interpolymers exhibit good crimp. The bimodal polymer composition has a density of about 0.900 to about 0.940 g / cm. 3 and a low density fraction having a density in the range of at least about 0.950 g / cm 3 The high density fraction may be characterized as having a density of
[0016] These ethylene / alpha-olefin interpolymer compositions may be characterized by a melt index (I2) in the range of 10 to 60 g / 10 min, where I2 is measured according to ASTM D1238, 190° C., 2.16 kg. The ratio of I10 / I2 may be less than 6.9, or less than 6.8, or less than 6.7, where I10 is measured according to ASTM D1238, 190° C., 10 kg. A lower I10 / I2 ratio may indicate lower long chain branching resulting in better spinnability / processability.
[0017] These ethylene / alpha-olefin interpolymer compositions have a ratio of weight average molecular weight to number average molecular weight (M) in the range of less than, or equal to, 2.6, or less than, or equal to, 2.5 and at least 1.5, or at least 1.7, or at least 2.0. w(GPC) / M n(GPC) The molecular weight distribution of the ethylene / alpha olefin interpolymers may be characterized by the molecular weight distribution according to the method described below, expressed as (I10 / I2) greater than -4.63. Interpolymer compositions having a molecular weight distribution in this range are believed to have better processability (e.g., fiber spinning) than interpolymers having higher molecular weight distributions. Ethylene / alpha olefin interpolymers have an M w(GPC) / M n(GPC) The present invention may be characterized by the following:
[0018] The ethylene / alpha-olefin interpolymer composition can have a weight average molecular weight from a lower limit of 15,000 g / mol, 20,000 g / mol, or 30,000 g / mol to an upper limit of 100,000 g / mol, 120,000 g / mol, or 150,000 g / mol. z(GPC) / M w(GPC)can be less than 3.0, or less than 2.0, and greater than 1.0. A bimodal polymer composition can show two peaks in an ICCD elution profile. In that case, the high temperature fraction can have a peak position molecular weight of 70,000 g / mol or less, or 50,000 g / mol or less. The high temperature fraction can have a peak position molecular weight of at least 15,000, or at least 20,000 g / mol. The low temperature fraction can have a peak position molecular weight of at least 30,000, or at least 40,000, or at least 50,000 g / mol. The low temperature fraction can have a peak position molecular weight of 250,000 or less, or 200,000 or less, or 150,000 g / mol or less.
[0019] These ethylene / alpha-olefin interpolymer compositions may be characterized by a tan delta at 1 radian / sec of at least 45, or at least 50. The ethylene / alpha-olefin interpolymers may be characterized by a ratio of tan delta at 1 radian / sec and 190° C. to tan delta at 100 radian / sec and 190° C. of at least 12. These characteristics may be measured by dynamic mechanical analysis (DMS).
[0020] These ethylene / alpha-olefin interpolymer compositions may be characterized by at least two distinguishable peaks between 35° C. and 110° C. on an improved comonomer composition distribution (ICCD) elution profile with a distinct valley between the peaks (at least a 10% drop compared to the peak height of the minor peak), and the peak positions should be separated by a minimum of 10° C. Each peak is separated by a vertical line at the point of the lowest height of the adjacent valley.
[0021] The peak temperature of the low temperature peak may be at least 50° C., or at least 60° C., and less than 90° C., or less than 75° C. The peak temperature of the high temperature peak may be at least 90° C., or at least 95° C., and less than 110° C., or less than 105° C., or less than 100° C. The inventors have found that low temperature peaks in the range of 50-75° C. are particularly useful for producing highly crimped fibers.
[0022] The weight fraction of the low temperature peak fraction may be at least 25, or at least 30 and less than 65, or less than 60, or less than 55 weight percent based on the total weight of the eluted polymer. The weight fraction of the high temperature peak fraction may be at least 35, or at least 40, or at least 45 and no more than 75 weight percent based on the total weight of the eluted polymer.
[0023] The full width at half maximum of the high temperature peak may be less than 6.0° C. The narrow peak of the high density fraction indicates a narrower compositional distribution and does not contain very high or very low molecular weight species that may interfere with spinning performance or produce extractables.
[0024] The ethylene / alpha olefin composition may have a Composition Distribution Breadth Index (CDBI) of less than 0.5 (i.e., less than 50%), less than 0.3 (30%), less than 0.25 (25%), less than 0.22 (less than 22%), or less than 0.2 (20%).
[0025] The ethylene / alpha-olefin interpolymer composition may have a comonomer distribution constant (CDC) of less than 100, preferably 30-80.
[0026] The ethylene / alpha-olefin interpolymer composition may be characterized by a molecular weighted comonomer distribution index (MWCDI) of greater than 0.20, or greater than 0.25, or greater than 0.30, or greater than 0.35, or greater than 0.40, or greater than 0.45, or greater than 0.50. MWCDI is a measure of the slope of comonomer incorporation as a function of molecular weight obtained from conventional gel permeation chromatography. If the MWCDI is greater than 0.25 (20,000-200,000 g / mol molecular weight range), the resin structure is considered to have significant inverse comonomer incorporation, with more comonomer on the high molecular weight side of the distribution.
[0027] The ethylene / alpha olefin interpolymer compositions disclosed herein may be characterized by a low amount of long chain branching (LCB). This may be indicated by a low zero shear viscosity ratio (ZSVR). Specifically, the ZSVR may be less than 1.35, or less than or equal to 1.30. The ZSVR may be at least 1.10.
[0028] The ethylene / alpha olefin interpolymer composition comprises 1 It may be characterized by a vinyl saturation number per 1,000,000 carbon atoms of less than 230, or less than 210, or less than 190, or less than 170, or less than 150, as determined by H-NMR.
[0029] Any conventional polymerization process may be used to produce the ethylene / α-olefin interpolymer composition.Such conventional polymerization processes include, but are not limited to, solution polymerization processes using one or more conventional reactors, such as loop reactors, isothermal reactors, stirred tank reactors, batch reactors, in parallel, in series, and / or any combination thereof.Such conventional polymerization processes also include gas phase, solution, or slurry polymerization, or any combination thereof, using any type of reactor or reactor configuration known in the art.
[0030] Generally, the solution phase polymerization process is carried out in one or more well-stirred reactors, such as one or more isothermal loop reactors or one or more adiabatic reactors, at a temperature in the range of 115-250°C, e.g., 115-200°C, and a pressure in the range of 300-1000 psi, e.g., 400-750 psi. In one example, the temperature of the first reactor of a dual reactor is in the range of 115-190°C, e.g., 115-150°C, and the temperature of the second reactor is in the range of 150-200°C, e.g., 170-195°C. In another example, the reactor temperature of a single reactor is in the range of 115-190°C, e.g., 115-150°C. The residence time in a solution phase polymerization process is typically in the range of 2-30 minutes, e.g., 10-20 minutes. Ethylene, solvent, hydrogen, one or more catalyst systems, optionally one or more cocatalysts, and optionally one or more comonomers are continuously fed into one or more reactors. Exemplary solvents include, but are not limited to, isoparaffin. For example, such solvents are commercially available under the name ISOPAR E from ExxonMobil Chemical Co. (Houston, Tex). The resulting mixture of ethylene / alpha-olefin interpolymer and solvent is then removed from the reactor, and the ethylene / alpha-olefin interpolymer is isolated. The solvent is typically recovered through a solvent recovery unit, i.e., a heat exchanger and a gas-liquid separator drum, and then recycled to the polymerization system.
[0031] The ethylene / α-olefin interpolymer compositions can be produced via solution polymerization in a dual reactor system, such as a dual loop reactor system, in which ethylene, and optionally one or more α-olefins, are polymerized in the presence of one or more catalyst systems. Additionally, one or more cocatalysts may be present.
[0032] Ethylene / alpha-olefin interpolymers can be produced through solution polymerization in a single reactor system, for example, a single loop reactor system, where ethylene and optionally one or more alpha-olefins are polymerized in the presence of one or more catalyst systems. In a dual reactor system, two different catalysts can be used. One or both of the two different catalysts have the formula (I) shown below. This allows the production of the bimodal interpolymer composition as described above.
[0033] An exemplary catalyst system suitable for producing the first ethylene / a-olefin interpolymer can be a catalyst system that includes a procatalyst component that includes a metal-ligand complex of formula (I). [ka]
[0034] In formula (I), M is a metal selected from titanium, zirconium, or hafnium, the metal is in a formal oxidation state of +2, +3, or +4, n is 0, 1, or 2, and when n is 1, X is a monodentate or bidentate ligand, and when n is 2, each X is a monodentate ligand and is the same or different, the metal-ligand complex is globally neutrally charged, and each Z is independently selected from -O-, -S-, -N(R N )-, or -P(R P )-, and L is selected from (C1-C 40 ) hydrocarbylene or (C1-C 40 ) heterohydrocarbylene, wherein each R N and R P However, independently (C1-C 30 ) hydrocarbyl, or (C1-C 30 ) heterohydrocarbyl, (C1-C 40 ) the hydrocarbylene has a moiety that includes a linker skeleton of 1 to 10 carbon atoms (to which L is attached) connecting the two Z groups of formula (I), or (C1-C 40) heterohydrocarbylene has a moiety that includes a linker skeleton of 1 to 10 atoms connecting the two Z groups of formula (I), (C1-C 40 Each of the 1 to 10 atoms of the 1 to 10 atom linker backbone of the heterohydrocarbylene is independently a carbon atom or a heteroatom, and each heteroatom is independently O, S, S(O), S(O), Si(R C )2, Ge(R C )2, P(R C ), or N(R C ) and each R C However, independently (C1-C 30 ) hydrocarbyl or (C1-C 30 ) heterohydrocarbyl, R 1 and R 8 However, independently, -H, (C1--C 40 ) hydrocarbyl, (C1-C 40 ) heterohydrocarbyl, -Si(R C )3, -Ge(R C )3, -P(R P )2, -N(R N )2, -OR C , -SR C , -NO2, -CN, -CF3, R C S(O)-, R C S(O)2-, (R C )2C=N-, R C C(O)O-, R C OC(O)-, R C C(O)N(R N )-, (R N ) 2NC(O)-, halogen, and a radical having formula (II), formula (III), or formula (IV). [ka]
[0035] In formulas (II), (III), and (IV), R 31-35 , R 41-48 , or R 51-59 Each of the groups independently represents (C1-C 40 ) hydrocarbyl, (C1-C 40) heterohydrocarbyl, -Si(R C )3, -Ge(R C )3, -P(R P )2, -N(R N )2, -N=CHR C , -OR C , -SR C , -NO2, -CN, -CF3, R C S(O)-, R C S(O)2-, (R C )2C=N-, R C C(O)O-, R C OC(O)-, R C C(O)N(R N )-, (R N )2NC(O)-, halogen, or -H; R 1 or R 8 is a radical having the formula (II), formula (III), or formula (IV), C , R N , and R P is as defined above.
[0036] In formula (I), R 2-4 , R 5-7 , or R 9-16 Each of the groups independently represents (C1-C 40 ) hydrocarbyl, (C1-C 40 ) heterohydrocarbyl, -Si(R C )3, -Ge(R C )3, -P(R P )2, -N(R N )2, -N=CHR C , -OR C , -SR C , -NO2, -CN, -CF3, R C S(O)-, R C S(O)2-, (R C )2C=N-, R C C(O)O-, R C OC(O)-, R C C(O)N(R N )-, (R N )2NC(O)-, halogen, and -H; R C, R N , and R P is as defined above.
[0037] The catalyst system comprising the metal-ligand complex of formula (I) can be made catalytically active by any technique known in the art for activating metal-based catalysts for olefin polymerization reactions. For example, those comprising the metal-ligand complex of formula (I) can be made catalytically active by contacting the complex with an activating cocatalyst or combining the complex with an activating cocatalyst. Activating cocatalysts suitable for use herein include alkylaluminum, polymeric or oligomeric alumoxanes (also known as aluminoxanes), neutral Lewis acids, and non-polymeric, non-coordinating, ion-forming compounds, including the use of such compounds under oxidizing conditions. A suitable activation technique is bulk electrolysis. Combinations of one or more of the foregoing activating cocatalysts and techniques are also contemplated. The term "alkylaluminum" means monoalkylaluminum dihydrides or dihalides, dialkylaluminum hydrides or halides, or trialkylaluminum. Examples of polymeric or oligomeric alumoxanes include methylalumoxane, triisobutylaluminum modified methylalumoxane, and isobutylalumoxane.
[0038] The Lewis acid activator (cocatalyst) may be any of the Lewis acid activators having one to three (C1-C 20 Examples of Group 13 metal compounds include tri((C1-C2) hydrocarbyl substituents. 20 )hydrocarbyl)-substituted aluminum compounds, or tri((C1-C 20 Additional examples of Group 13 metal compounds include tri(hydrocarbyl)-substituted aluminum, tri((C-C 20 )hydrocarbyl)-boron compounds, tri((C1-C 10 ) alkyl) aluminum, tri((C6-C 18)aryl)boron compounds and their halogenated (including perhalogenated) derivatives. Other examples of Group 13 metal compounds are tris(fluoro-substituted phenyl)borane, tris(pentafluorophenyl)borane. Activating cocatalysts include tris((C1-C 20 )hydrocarbyl)borate (e.g. trityl tetrafluoroborate) or tri((C 20 )hydrocarbyl)ammonium tetra((C1-C 20 As used herein, the term "ammonium" refers to a ((C1-C2) hydrocarbyl) borane, such as bis(octadecyl)methylammonium tetrakis(pentafluorophenyl)borane. 20 )Hydrocarbyl)4N + , ((C1-C 20 )hydrocarbyl)3N(H) + , ((C1-C 20 )hydrocarbyl)2N(H)2 + , (C1-C 20 ) HydrocarbylN(H)3 + , or N(H)4 + Each of the nitrogen cations (C1-C 20 ) Hydrocarbyls, when present in two or more occurrences, may be the same or different.
[0039] As a combination of neutral Lewis acid activators (cocatalysts), tri((C1-C4) alkyl)aluminum and tri((C6-C 18Examples include mixtures containing a mixture of neutral Lewis acids with a tris(pentafluorophenyl)borane, especially tris(pentafluorophenyl)borane. Other examples are combinations of such neutral Lewis acid mixtures with polymeric or oligomeric alumoxanes, and combinations of a single neutral Lewis acid, especially tris(pentafluorophenyl)borane, with polymeric or oligomeric alumoxanes. The ratio of the number of moles of (metal-ligand complex):(tris(pentafluorophenylborane):(alumoxane) [e.g., (Group 4 metal-ligand complex):(tris(pentafluorophenylborane):(alumoxane)] can be 1:1:1 to 1:10:30, or 1:1:1.5 to 1:5:10.
[0040] A catalyst system comprising the metal-ligand complex of formula (I) can be activated to form an active catalyst composition by combining one or more cocatalysts, such as cation-forming cocatalysts, strong Lewis acids, or combinations thereof. Suitable activating cocatalysts include polymeric or oligomeric aluminoxanes, particularly methylaluminoxane, as well as inert, compatible, non-coordinating, ion-forming compounds. Exemplary suitable cocatalysts include modified methylaluminoxane (MMAO), bis(hydrogenated tallow alkyl)methyl, tetrakis(pentafluorophenyl)borate (1 - ) amines, and combinations thereof.
[0041] One or more of the aforementioned activating cocatalysts may be used in combination with each other. A combination of a mixture of tri((C1-C4)hydrocarbyl)aluminum, tri((C1-C4)hydrocarbyl)borane, or ammonium borate with an oligomeric or polymeric alumoxane compound is preferred. The ratio of the total number of moles of the one or more metal-ligand complexes of formula (I) to the total number of moles of the one or more activating cocatalysts is 1:10,000 to 100:1. The ratio may be at least 1:5000, or at least 1:1000, and may be 10:1 or less, or 1:1 or less. The preferred number of moles of alumoxane used when alumoxane alone is used as the activating cocatalyst may be at least 100 times the number of moles of the metal-ligand complexes of formula (I). When tris(pentafluorophenyl)borane alone is used as the activating cocatalyst, the number of moles of tris(pentafluorophenyl)borane to the total number of moles of the one or more metal-ligand complexes of formula (I) that can be used ranges from 0.5:1 to 10:1, 1:1 to 6:1, or 1:1 to 5:1. The remaining activating cocatalysts are generally used in a molar amount approximately equal to the total molar amount of the one or more metal-ligand complexes of formula (I).
[0042] fiber. The above ethylene / alpha-olefin interpolymer, either alone or in combination with other materials, forms a first region of the fiber.
[0043] At least 75%, at least 80%, at least 85%, at least 90%, at least 95%, at least 97%, at least 98%, at least 99%, or at least 100% (all percentages are weight percentages based on the total weight of the first region) of the fiber can be ethylene / alpha-olefin interpolymer. The remainder of the first region can be additional components such as one or more other polymers and / or one or more additives. The other polymer can be another polyethylene (e.g., a polyethylene homopolymer or an ethylene / alpha-olefin interpolymer), a propylene-based polymer (e.g., a polypropylene homopolymer, a propylene-ethylene copolymer, or a propylene / alpha-olefin interpolymer). The amount of the other polymer can be up to 25%. Possible additives may include, but are not limited to, antistatic agents, color enhancers, dyes, lubricants, fillers such as TiO2 or CaCO3, opacifiers, nucleating agents, processing aids, pigments, primary antioxidants, secondary antioxidants, processing aids, UV stabilizers, antiblocking agents, slip agents, tackifiers, flame retardants, antimicrobial agents, odor reducers, antifungal agents, and combinations thereof. The ethylene / alpha-olefin interpolymer polymer composition may contain a total of about 0.01, or about 0.1, or about 1 to about 25, or about 20, or about 15, or about 10 weight percent of such additives, based on the weight of the ethylene-based polymer composition including such additives.
[0044] The fibers of the present invention may comprise the ethylene / alpha-olefin interpolymer composition according to the present invention, alone or in combination with one or more polymers, as an outer layer, e.g., sheath. As used herein, the term outer layer refers to at least any portion of the fiber surface. The fibers of the present invention may comprise the ethylene / alpha-olefin interpolymer composition according to the present invention, alone or in combination with one or more polymers, as an inner layer, e.g., core. The fibers of the present invention may comprise an ethylene / alpha-olefin interpolymer adjacent to the second region or adjacent to the segmented pie.
[0045] The second region comprises a different polymer composition from the ethylene / alpha olefin interpolymer. For example, the second region may comprise a different polyolefin, such as polypropylene, or a polyester, such as polyethylene terephthalate or polybutylene terephthalate, or a combination thereof, with or without the additives described above. The second region preferably comprises at least 75, or at least 80, or at least 85, or at least 90, or at least 99 percent by weight of the polymeric material, and the remainder of the second region may be additional components, such as additives. Possible additives may include, but are not limited to, antistatic agents, color enhancers, dyes, lubricants, fillers such as TiO2 or CaCO3, opacifiers, nucleating agents, processing aids, pigments, primary antioxidants, secondary antioxidants, processing aids, UV stabilizers, antiblocking agents, slip agents, tackifiers, flame retardants, antibacterial agents, odor reducers, antifungal agents, and combinations thereof. The ethylene / alpha-olefin interpolymer polymer composition can contain from about 0.01, or about 0.1, or about 1 to about 25, or about 20, or about 15, or about 10 weight percent total weight of such additives, based on the weight of the ethylene-based polymer composition including such additives.
[0046] The first regions can be at least 20, or at least 30, or at least 40, or at least 50, or at least 60, or at least 70, or at least 80% by weight of the fiber. The first regions can be up to 80, or up to 70, or up to 60, or up to 50, or up to 40, or up to 30, or up to 20% by weight of the fiber. In bicomponent fibers, the second regions can be at least 20, or at least 30, or at least 40, or at least 50, or at least 60, or at least 70, or at least 80% by weight of the fiber and up to 80, or up to 70, or up to 60, or up to 50, or up to 40, or up to 30, or up to 20% by weight of the fiber. Alternatively, the weight ratio of the first component or region to the second component or region may be at least 20 / 80, or at least 30 / 70, or at least 40 / 60, and not more than 80 / 20, or 70 / 30, or 60 / 40.
[0047] The fibers taught herein can be formed by any conventional spinning technique, including melt spinning. The ethylene-based polymer composition is formed into bicomponent fibers through different techniques, for example, through melt spinning. Such monocomponent fibers can be continuous filaments or can be staple fibers. The continuous filaments can be further crimped and / or stretched and then cut to produce staple fibers. For example, the staple fibers can have a length of, for example, at least 0.2, or at least 0.5, or at least 1 cm, and no more than 16, or no more than 12, or no more than 10 cm.
[0048] In melt spinning, the ethylene / alpha-olefin interpolymer composition, or a blend of the ethylene / alpha-olefin interpolymer composition with one or more other polymers, is melted, coextruded, and forced through fine orifices in a metal plate called a spinneret into air or other gas where it cools and solidifies to form the bicomponent fibers of the invention. The solidified filaments can be drawn through air jets, rotating rolls, or godets and laid down as a web on a conveyor belt.
[0049] The bicomponent fibers of the present invention according to the present invention can be formed into nonwoven fabrics. Nonwoven fabrics according to the present disclosure can be manufactured through different techniques. Such methods include, but are not limited to, spunbonding process, carded web process, airlaid process for laying webs, and are bonded by methods including, but are not limited to, thermocalendering process, adhesive bonding process, hot air bonding process, needle punching process, hydroentangling process, electrospinning process, and combinations thereof. The fabric can be further laminated to other nonwoven fabrics or films in various lamination techniques such as adhesive lamination, thermal lamination, extrusion lamination, needle punching, hydroentangling, and combinations thereof. Advantageously, the nonwoven fabrics disclosed herein can be formed directly from the component polymeric material(s) by the spunbonding process. In the spunbond process, the manufacture of a nonwoven fabric involves the steps of: (a) extruding strands of one or more polymeric compositions from a spinneret, (b) quenching the strands of one or more polymeric compositions with a generally cooled air stream to promote solidification of the molten strands of one or more polymeric compositions, (c) attenuating the filaments by advancing them through a quench zone with a drawing tension that can be applied either by air pressure entraining the filaments in the air stream or by winding them around mechanical drawing rolls of the type commonly used in the textile fiber industry, (d) collecting the drawn strands into a web on a foraminous surface, such as a moving screen or porous belt, and (e) bonding the web of loose strands into a nonwoven fabric. Bonding can be accomplished by a variety of means, including, but not limited to, thermal calendering, adhesive bonding, hot air bonding, needle punching, hydroentangling, and combinations thereof.
[0050] The fibers disclosed herein have the following characteristics:
[0051] The fibers may have a diameter of at least 3 microns, or at least 5 microns, or at least 10 microns and less than 50 microns, or less than 30 microns.
[0052] The fibers can have a denier per filament in the range of less than 50 g / 9000 m. All individual values and subranges less than 50 g / 9000 m are included herein and disclosed herein, for example, the denier per filament can be from a lower limit of 0.1, 0.5, 1, 5, 10, 15, 17, 20, 25, 30, 33, 40, 44, or 50 g / 9000 m. For example, the fibers may have a denier per filament in the range of less than 40 g / 9000 m, alternatively the fibers may have a denier per filament in the range of less than 30 g / 9000 m, alternatively the fibers may have a denier per filament in the range of less than 20 g / 9000 m, alternatively the fibers may have a denier per filament in the range of less than 10 g / 9000 m, or alternatively the fibers may have a denier per filament in the range of 0.5 to 10 g / 9000 m.
[0053] The nonwoven fabrics disclosed herein may have the following characteristics:
[0054] The fabrics disclosed herein provide relatively high shrinkage.Low levels of vinyl unsaturation in the ethylene-based polymer composition are also important because such low levels of vinyl unsaturation immediately provide the ethylene-based polymer composition with improved processability.
[0055] Spunbond nonwovens can be formed into multi-layer or laminate structures. Such multi-layer structures include at least two or more layers, at least one or more of which is a spunbond nonwoven as disclosed herein, and one or more other layers are selected from one or more meltblown nonwoven layers, one or more wetlaid nonwoven layers, one or more airlaid nonwoven layers, one or more film layers, any nonwoven or one or more webs produced by a melt spinning process. Cast films, blown films, one or more coating layers derived from a coating composition, for example, via extrusion coating, spray coating, gravure coating, printing, dipping, kiss rolling, or blade coating, etc. Laminated structures can be bonded via any number of bonding methods, thermal bonding, adhesive lamination, hydroentanglement, needle punching. The structures can range from S to SX, or SXX, or SXXX, or SXXXX, or SXXXXX, where S is a nonwoven as disclosed herein, and X can be a film, coating, or other nonwoven material in any combination, or one or more of the X can also be S. The additional spunbond layers may be made from an ethylene-based polymer composition as described herein, and optionally in combination with one or more polymers and / or additives.
[0056] In the case of staple or binder fibers, the fibers may be mixed with a variety of other fibers, including synthetic fibers such as polyethylene (PE), PP, polyethylene terephthalate (PET), or natural fibers such as cellulose, rayon, or cotton. These fibers can be wet laid, air laid, or carded into a nonwoven web. The nonwoven web can then be laminated to other materials.
[0057] Spunbond nonwovens can be used in a variety of end uses including, but not limited to, sanitary absorbent products such as diapers, feminine hygiene products, adult incontinence products, wipes, bandages, wound dressings, etc., disposable slippers and footwear, isolation gowns, surgical gowns, surgical drapes and covers, surgical scrub suits, caps, masks, medical packaging, etc.
[0058] The fibers are at least 2, or at least 2.5, or at least 3 mm -1 For example, a fiber having an ethylene / alpha-olefin interpolymer described herein as a sheath on a polypropylene core may have a curvature of at least 2, or at least 2.5, or at least 3 when extruded at a temperature of 230-250° C. (preferably about 240° C.) through a die having a length-to-diameter ratio of about 4 / 1 at a pressure of about 0.1-0.3 (or 0.14-0.28) MPa. Under these conditions, the curvature may be up to 15 or 12 mm. -1 As another example, a fiber having an ethylene / alpha-olefin interpolymer described herein as a sheath on a polypropylene core can have a curvature of at least 2 when extruded at a temperature of 200-220° C. (preferably about 210° C.) through a die having a length to diameter ratio of about 4 / 1 at a pressure of about 0.1-0.3 (or 0.14-0.28) MPa.
[0059] Test Method density Density measurements of the ethylene / alpha-olefin interpolymers were performed according to ASTM D792, Method B.
[0060] Melt index (I2) and (I10) The melt index (I2) values of the ethylene / alpha-olefin interpolymers are measured at 190° C. and 2.16 kg according to ASTM D1238. Similarly, the melt index (I10) values of the ethylene / alpha-olefin interpolymers are measured at 190° C. and 10 kg according to ASTM D1238. Values are reported in g / 10 min, which corresponds to grams dissolved per 10 minutes. Dynamic mechanical spectroscopy (DMS)
[0061] The samples are compression molded into 3 mm thick x 25 mm diameter circular plaques at 177°C for 5 minutes under 10 MPa pressure. The samples are then removed from the press and placed on a counter to cool. Constant temperature frequency sweep measurements are performed on the compression molded plaques using an ARES strain controlled rheometer (TA Instruments) with 25 mm parallel plates under a nitrogen purge. For each measurement, the rheometer is allowed to thermally equilibrate for at least 30 minutes and then the gap is zeroed. The sample disk is placed on the plates and melted at 190°C for 5 minutes. The plates are then closed to a 2 mm gap, the sample is trimmed, and the test is then started. The method may incorporate an additional 5 minute delay to allow for temperature equilibration. The experiment is performed at 190°C over a frequency range of 0.1 to 100 rad / sec, at 5 points every 10 intervals. The strain amplitude is constant at 10%. The stress response is analyzed in terms of amplitude and phase, from which the storage modulus (G'), loss modulus (G"), complex modulus (G*), dynamic viscosity (η*), and tan δ (or tan delta) are calculated. Tan delta at 1 rad / sec and tan delta at 100 rad / sec are obtained.
[0062] Improved Comonomer Composition Distribution (ICCD) The improved comonomer composition distribution (ICCD) test is carried out using a Crystallization Elution Fractionation instrument (CEF) (PolymerChar (Spain)) equipped with an IR-5 detector (PolymerChar (Spain)) and a two-angle light scattering detector model 2040 (Precision Detectors, now Agilent Technologies). The ICCD column is packed with gold-coated nickel particles (Bright 7GNM8-NiS, Nippon Chemical Industrial Co.) in a 15 cm (length) x ¼ inch (ID) stainless steel tube. The column is packed and conditioned using a slurry method according to references (Cong, R; Parrott, A.; Hollis, C.; Cheatham, M. WO2017040127A1). The final pressure of the trichlorobenzene (TCB) slurry packing is 150 bar. The column is placed in the detector oven just before the IR-5 detector. Ortho-dichlorobenzene (ODCB, 99% anhydrous grade or technical grade) is used as the eluent. Silica gel 40 (particle size 0.2-0.5 mm, catalog number 10181-3) is obtained from EMD Chemicals and can be used to dry the ODCB solvent. The ICCD instrument is equipped with an autosampler with nitrogen (N2) purging. ODCB is sparged with dry N2 for 1 h before use. Sample preparation is performed at 4 mg / ml (unless otherwise noted) with the autosampler shaking at 160 °C for 1 h. The injection volume is 300 μl. The temperature profile of the ICCD is crystallization from 105 °C to 30 °C at 3 °C / min, then thermal equilibration at 30 °C for 2 min (including soluble fraction elution time set at 2 min), followed by heating from 30 °C to 140 °C at 3 °C / min. The flow rate during elution is 0.50 ml / min. Data is collected at one data point / sec. Column temperature calibration was performed using a standard linear homopolymer polyethylene (zero comonomer content, melt index (I2) of 1.0 g / 10 min, polydispersity M of approximately 2.6 by conventional gel permeation chromatography). w(GPC) / M n(GPC)The ICCD temperature calibration can be performed using a mixture of 1.0 mg / mL of DMSO in ODCB, and 2 mg / mL of eicosane in ODCB. The ICCD temperature calibration involves the steps of (1) calculating the delay volume, defined as the temperature offset between the measured peak elution temperature of eicosane minus 30.00° C., and (2) subtracting the temperature offset of the elution temperature from the ICCD uncorrected temperature data. (Note that this temperature offset is a function of experimental conditions such as elution temperature, elution flow rate, etc.); (3) creating a linear calibration line that converts elution temperatures ranging from 30.00°C to 140.00°C, such that the linear homopolymer polyethylene standard has a peak temperature at 101.0°C and eicosane has a peak temperature of 30.0°C; and (4) linearly extrapolating elution temperatures below 30.0°C by using an elution heating rate of 3°C / min according to reference (Cerk and Cong et al., US9,688,795) for the soluble fraction measured isothermally at 30°C.
[0063] A calibration curve of comonomer content for ICCD (comonomer content in mole percent versus elution temperature (T)) is made by using 12 standards with known comonomer content (linear ethylene homopolymers, and 11 ethylene-octene random copolymers with weight average molecular weights ranging from 35,000 to 128,000 g / mol made with a single-site metallocene catalyst). All these standards are analyzed in the same manner as specified previously at 4 mg / mL. The comonomer contents in mole percent and their peak temperatures on the elution curve are as follows:
number
[0064] Determination of peaks and full width at half maximum in ICCD elution profiles A single baseline is subtracted from the IR measurement signal to create a relative mass elution profile plot that starts and ends at zero relative mass at its lowest and highest elution temperatures (typically 35 °C to 119 °C). For convenience, this is expressed as a quantity normalized to an overall area equivalent to 1. In the relative mass elution profile plot from the ICCD, the weight fraction (w T (T)) can be obtained. T (T) vs. T) is 35.0℃ to 119.0℃ with a 0.200℃ increase in temperature steps from ICCD, as follows:
number
[0065] w T In a (T) vs. T elution profile, a single peak is defined as a curve with one maximum in the middle and two minimums on either side (lower and higher temperature). The heights of both of the two minimums must be at least 10% lower than the height of the maximum. If one or both of the minimums have a height less than 10% lower than the height of the maximum, i.e., if one or both of the minimums have a height greater than 90% of the height of the maximum, then such a curve is considered a shoulder associated with another peak, but not a peak itself. Each individual peak is then divided into a series of peaks, w T Measure the width in degrees Celsius at 50% of the maximum height of that peak in the (T) vs. T elution profile plot. This width is called the full width at half maximum of the peak.
[0066] If the ICCD elution profile has multiple peaks, the separation point between the peaks (T 分離 The nth peak (WT) can be defined as the lowest point between two adjacent peaks. ピークn The weight fraction of ) can be calculated according to the following equation:
number
[0067] The full width at half maximum is defined as the temperature difference between the first intersecting point of the front temperature and the first intersecting point of the rear temperature at half the maximum peak height of that individual peak. The front temperature at half the maximum peak is searched forward from 35.0°C, and the rear temperature at half the maximum peak is searched backward from 119.0°C.
[0068] Comonomer Distribution Constant (CDC) The comonomer distribution constant (CDC) is calculated by the ICCD w T (T) vs. T calculated from the elution profile. (1) In the range of 35.0℃ to 119.0℃, increase the temperature step by 0.200℃ from ICCD to w T Obtain the (T) vs. T dissolution profile. The total weight fraction from 35 °C to 119 °C should be normalized to 1.0 and follow Equation 2. (2) The median temperature (T 中央値 ) calculating
number
number
number
number
[0069] Conventional Gel Permeation Chromatography (Conventional GPC) and MWCDI The chromatographic system consisted of a PolymerChar GPC-IR (Valencia, Spain) high temperature GPC chromatograph equipped with a built-in IR5 infrared detector (IR5). The autosampler oven compartment was set at 160°C and the column compartment was set at 150°C. The columns used were four Agilent "Mixed A" 30 cm, 20 micron linear mixed bed columns. The chromatographic solvent used was 1,2,4 trichlorobenzene containing 200 ppm butylated hydroxytoluene (BHT). The solvent source was nitrogen injection. The injection volume used was 200 microliters and the flow rate was 1.0 milliliters / min.
[0070] Calibration of the GPC column set is performed with at least 20 narrow molecular weight distribution polystyrene standards with molecular weights ranging from 580 to 8,400,000 g / mol arranged in six "cocktail" mixtures with at least 10 intervals between individual molecular weights. Standards are purchased from Agilent Technologies. Polystyrene standards are prepared at 0.025 grams in 50 milliliters of solvent for molecular weights equal to or greater than 1,000,000 g / mol, and 0.05 grams in 50 milliliters of solvent for molecular weights less than 1,000,000 g / mol. Dissolve the polystyrene standards with gentle stirring at 80°C for 30 minutes. Convert the polystyrene standard peak molecular weights to ethylene / alpha-olefin interpolymer molecular weights using the following equation (described in Williams and Ward, J. Polym. Sci., Polym. Let., 6, 621 (1968)): M ポリエチレン=A×( M ポリエチレン) (Equation 7) where M is the molecular weight, A has a value of 0.4315, and B is equal to 1.0.
[0071] Use a fifth-order polynomial to fit the equivalent calibration points to each ethylene / alpha-olefin interpolymer, such as that obtained using the NIST standard NBS1475 at a molecular weight of 52,000 g / mol. Make a small adjustment (approximately 0.39-0.44) to A to correct for column resolution and band broadening effects.
[0072] A total plate count of the GPC column set is performed using eicosane (prepared at 0.04 g in 50 milliliters of TCB and dissolved for 20 minutes with gentle agitation). Plate count (Equation 8) and symmetry (Equation 9) are measured with a 200 microliter injection according to the following equations:
number
number
[0073] Samples are prepared semi-automatically using PolymerChar "Instrument Control" software, which targets a sample weight of 2 mg / ml and adds solvent (containing 200 ppm BHT) via the PolymerChar high temperature autosampler to a septa-capped vial that has been pre-flushed with nitrogen. Samples are dissolved at 160° C. for 3 hours under "slow" shaking.
[0074] Mn(GPC) , M w(GPC)、 and M. z(GPC) The calculation of is performed using PolymerChar GPCOne™ software, at each equally spaced data collection point i(IR i ) and the ethylene / alpha-olefin interpolymer equivalent molecular weight (M in g / mol) obtained from the narrow standard calibration curve of point i from Equation 7. ポリエチレン、i ) according to Equations 11a-c. Based on the results of GPC using the built-in IR5 detector (measurement channel) of the PolymerChar GPC-IR chromatograph. Subsequently, the GPC molecular weight distribution (GPC-MWD) plot (wt GPC (lgMW) vs. lgMW plot (wt GPC (lgMW) is the weight fraction of interpolymer molecules having a molecular weight of lgMW. Molecular weight is in g / mol, and wt GPC (lgMW) follows equation 10.
number
[0075] Number average molecular weight M n(GPC) , weight average molecular weight M w(GPC) and z-average molecular weight M z(GPC) can be calculated as follows:
number
number
number
[0076] To monitor deviations over time, a flow marker (decane) is introduced into each sample via a micropump controlled by the PolymerChar GPC-IR system. This flow marker (FM) is used to linearly correct the pump flow rate (Flow (nominal)) of each sample by aligning the RV of the respective decane peak in the sample (RV (FM sample)) with the RV of the decane peak in the narrow standard calibration (RV (FM calibration)). Any change in time of the decane marker peak is then assumed to be related to a linear shift in flow rate (Flow (effective)) throughout the experiment. To facilitate the highest accuracy of the RV measurement of the flow marker peak, a least squares fitting routine is used to fit the peaks of the flow marker concentration chromatogram to a quadratic equation. The first derivative of the quadratic equation is then used to determine the true peak position. After calibrating the system based on the flow marker peak, the effective flow rate (with respect to the narrow standard calibration) is calculated as in Equation 12. Processing of the flow marker peaks is performed via PolymerChar GPCOne™ software. Acceptable flow correction is made so that the effective flow is within 0.5% of the nominal flow. flow rate 有効 =Flow rate 公称 ××(RV(FM 較正済み ) / RV(FM 試料 ))(Equation 12)
[0077] Calibration of the IR5 detector ratio can be performed using at least eight ethylene / alpha-olefin interpolymer standards (one polyethylene homopolymer and seven ethylene / octene copolymers) with known short chain branching (SCB) frequencies (as measured by 13C NMR methods) ranging from homopolymer (0 SCB / 1000 total C) to approximately 50 SCB / 1000 total C (where total C = carbons in the backbone + carbons in the branches). Each standard has a weight average molecular weight, as determined by GPC, of 36,000 g / mol to 126,000 g / mol. Each standard has a molecular weight distribution (M) of 2.0 to 2.5, as determined by GPC. w(GPC) / M n(GPC)) The "IR5 Area Ratio (or "IR5 Methyl Channel Area / IR5 Measurement Channel Area") of "Baseline Divided Area Response of IR5 Methyl Channel Sensor" to "Baseline Divided Area Response of IR5 Measurement Channel Sensor" (standard filters and filter wheels supplied by PolymerChar: part number IR5_FWM01 are included as part of the GPC-IR instrument) is calculated for each of the "SCB" standards. A linear fit of the "IR5 Area Ratio" versus SCB frequency is constructed in the form of the following equation: SCB / 1000 total C = A0 + [A1 x (IR5 メチルチャネル面積 / IR5 測定チャネル面積 )](Equation 13) where A0 is the intercept of "SCB / 1000 Total C" at an "IR5 Area Ratio" of zero, and A1 is the slope of "SCB / 1000 Total C" vs. "IR5 Area Ratio", which represents the increase in "SCB / 1000 Total C" as a function of "IR5 Area Ratio".
[0078] A series of linear baseline divided chromatographic heights for chromatograms generated by the "IR5 methyl channel sensor" are established as a function of column elution volume to generate a baseline-corrected chromatogram (methyl channel). A series of linear baseline divided chromatographic heights for chromatograms generated by the "IR5 measurement channel" are established as a function of column elution volume to generate a baseline-corrected chromatogram (measurement channel).
[0079] The "IR5 Height Ratio" of the "Baseline Corrected Chromatogram (Methyl Channel)" vs. the "Baseline Corrected Chromatogram (Measurement Channel)" is calculated at each column elution volume index (each equally spaced index, representing one data point per second at 1 ml / min elution) across the sample integration boundary. The "IR5 Height Ratio" is multiplied by coefficient A1 and coefficient A0 is added to this result to generate the predicted SCB frequency for the sample. The result is converted to mole percent comonomer as per Equation 14 below. Mole percent comonomer = {SCB f / [SCBf +((1000-SCB f * length of comonomer) / 2)}*100 (Equation 14) During the ceremony, “SCB f " is the "SCB per 1000 total C" and "comonomer length" is the number of carbons in the comonomer, e.g., 8 for octene, 6 for hexene, etc.
[0080] Convert each elution volume index to a molecular weight value (Mwi) using the method of Williams and Ward (Equation 7, above). Plot the "mole percent comonomer" as a function of Ig(Mwi) and calculate the slope from an Mwi of 20,000 to an Mwi of 200,000 g / mol (the end group correction for chain ends is omitted in this calculation). Linear regression is used to calculate the slope between an Mwi of 20,000 and 200,000 g / mol and the height of the concentration chromatogram (wt GPC The slope of the (lgMW) vs. lgMW plot) is at least 10% of the peak height in the chromatogram. This slope is defined as the molecular weight comonomer distribution index (MWCDI).
[0081] Zero Shear Viscosity Ratio (ZSVR) The zero shear viscosity ratio is determined by the equivalent weight average molecular weight (M w(GPC) ) to that of a linear polyethylene material (see ANTEC Proceedings).
number
[0082] ZSV value of interpolymer (η 0B ) is obtained from creep testing at 190°C via the method described below. w(GPC) The value is determined by the conventional GPC method discussed above (Equation 11b). The ZSV (η 0L ) and its M w(GPC) A correlation between ZSV-M and the linear polyethylene standard is established based on a series of linear polyethylene standards. w(GPC)For an explanation of the relationship between these two, see the ANTEC proceedings: Karjala et al., Detection of Low Levels of Long-chain Branching in Polyolefins, Annual Technical Conference-Society of Plastics Engineers (2008), 66 th It can be found at 887-891.
[0083] Creep Test ZSV value of interpolymer (η 0B) are obtained from constant stress rheometer creep tests at 190°C in a nitrogen environment using a DHR (TA Instrument). The samples are subjected to flow between two 25 mm diameter plate fixtures arranged parallel to each other. The samples are prepared by compression molding pellets of the interpolymer into circular plaques of approximately 1.5-2.0 mm thickness. The plaques are further cut into 25 mm diameter disks and sandwiched between the plate fixtures of the TA Instrument. After loading the samples, the TA Instrument oven is closed for 5 minutes before setting the gap between the plate fixtures to 1.5 mm, opening the oven to trim the edges of the samples, and closing the oven again. Before and after the creep test, a logarithmic frequency sweep from 0.1 to 100 rad / sec is performed at 190°C, 300 s soak time, and 10% strain to determine if the samples have degraded. A constant low shear stress of 20 Pa is applied to all of the samples to ensure that the steady-state shear rate is low enough to be in the Newtonian region. Steady state is determined by taking a linear regression on the data in the last 10% time window of a plot of "lg(J(t)) vs. lg(t)," where J(t) is creep compliance and t is creep time. If the slope of the linear regression is greater than 0.97, steady state is considered to have been reached and the creep test is then stopped. In all cases in this test, the slope meets the criterion within 1 hour. The steady state shear rate is determined from the slope of the linear regression of all the data points in the last 10% time window of a plot of "ε vs. t," where ε is strain. The zero shear viscosity is determined from the ratio of the applied stress to the steady state shear rate.
[0084] 1 H NMR method The stock solution (3.26 g) was added to 0.133 g of polymer sample in a 10 mm NMR tube. The stock solution was a mixture of tetrachloroethane-d2 (TCE) and perchloroethylene (50:50 by weight) with 0.001 M Cr 3+ The solution in the tube is N for 5 min. 2The polymer samples were swelled by purging with 0.5% CO. The capped sample tubes were left at room temperature overnight. The polymer samples were dissolved at 110°C with periodic vortex mixing. The samples were free of additives that may contribute to unsaturation, e.g. slip agents such as erucamide. Each tube was purged with 0.5% CO. 1 1 H NMR analysis is performed on a Bruker AVANCE 400 MHz spectrometer using a 10 mm cryoprobe at 120°C.
[0085] To measure the degree of unsaturation, two experiments are performed: one control experiment and one double presaturation experiment. In the control experiment, the data are processed with an exponential window function with 1 Hz line broadening and the baseline is corrected from approximately 7 to -2 ppm. The signal from the residual 1H of TCE is set to 100 and the sum of the integrals (Itotal) from -0.5 to 3 ppm is used as the signal from the whole polymer in the control experiment. The total number of carbons in the polymer, NC, is calculated according to Equation 16. NC=I 合計 / 2 (Equation 16)
[0086] In the double presaturation experiment, the data were processed with an exponential window function using 1 Hz line broadening and baseline corrected from approximately 6.6 to 4.5 ppm. 1 The signal from H was set to 100 and the corresponding integral for unsaturation (I ビニレン , I 三置換体 , I ビニル , and I ビニリデン ) is integrated. The use of NMR spectroscopy to determine polyethylenic unsaturation is well known, see for example Busico, V., et al., Macromolecules, 2005, 38, 6988. The number of vinylene, trisubstituted, vinyl, and vinylidene unsaturated units is calculated as follows: N ビニレン =I ビニレン / 2 (Equation 17), N 三置換体 =I 三置換体 (Equation 18), N ビニル =I ビニル / 2 (Equation 19), Nビニリデン =I ビニリデン / 2 (Equation 20).
[0087] The unsaturated units per 1,000 total carbons, i.e., all polymer carbons including backbone and branches, are calculated as follows: N ビニレン / 1,000C=(N ビニレン / NC)*1,000(Equation 21), N 三置換体 / 1,000C=(N 三置換体 / NC)*1,000(Equation 22), N ビニル / 1,000C=(N ビニル / NCH2)*1,000 (Equation 23), N ビニリデン / 1,000C=(N ビニリデン / NC)*1,000 (Equation 24).
[0088] From the residual protons from TCE-d2 1 For the H signal, the chemical shift standard is set to 6.0 ppm. The control is run with a ZG pulse, NS=4, DS=12, SWH=10,000 Hz, AQ=1.64 sec, D1=14 sec. The double presaturation experiment is run with a modified pulse sequence of O1P=1.354 ppm, O2P=0.960 ppm, PL9=57 db, PL21=70 db, NS=100, DS=4, SWH=10,000 Hz, AQ=1.64 sec, D1=1 sec (D1 is the presaturation time), D13=13 sec.
[0089] 13 C NMR method Samples are prepared by adding approximately 3 g of a 50 / 50 mixture of tetra-chloroethane-d2 / orthodichlorobenzene containing 0.025 M Cr(AcAc)3 to 0.25 g of polymer sample in a Norell 1001-7 10 mm NMR tube. Oxygen is removed from the sample by purging the tube headspace with nitrogen. The sample is then dissolved and homogenized by heating the tube and its contents to approximately 150°C using a heating block and heat gun. Each sample is visually inspected to ensure homogeneity. Samples are thoroughly mixed immediately prior to analysis and are not allowed to cool before being inserted into the heated NMR probe. This is necessary to ensure that the sample is homogenous and representative of the entire sample. All data are collected using a Bruker 400 MHz spectrometer equipped with a Bruker cryoprobe. Data are acquired using inverse gated decoupling with a 6 second pulse repetition delay, a 90 degree flip angle, and a sample temperature of 120°C. All measurements are performed with the sample unspun in locked mode. Samples are allowed to thermally equilibrate for 7 minutes prior to data acquisition. 13C NMR chemical shifts are internally referenced to the EEE triad at 30 ppm.
[0090] C13 NMR Comonomer Content: The use of NMR spectroscopy to determine polymer composition is well known. General methods for polymer analysis by NMR spectroscopy are provided in ASTM D 5017-96, JC Randal et al. in "NMR and Macromolecules" ACS Symposium series 247, JC Randal, Ed., Am. Chem. Soc., Washington, DC, 1984, Ch. 9, and JC Randal in "Polymer Sequence Determination", Academic Press, New York (1977).
[0091] Denier Measurement Fiber size is measured via optical microscope. Denier (defined as the weight of 9000 meters of such a fiber) is calculated based on the density of each polymer component and fiber size.
[0092] Shrinkage The crimp is measured via optical microscopy. The crimp (defined as the curvature of the fiber) is calculated based on the inverse of the radius of the approximate helix formed by the fiber. It is equal to the radius of the circle formed by projecting the approximate helix formed by the fiber onto a surface perpendicular to it. The average value of at least five samples is reported. EXAMPLES
[0093] Example 1 Synthesis of Ethylene / Alpha Olefin Polymer All feedstocks (ethylene monomer and 1-octene comonomer) and process solvents (high purity narrow boiling range isoparaffinic solvent, commercially available from ExxonMobil Chemical under the product name Isopar-E) are purified with molecular sieves before being introduced into the reaction environment. Hydrogen is supplied under pressure as a high purity grade and is not further purified. The reactor ethylene feed stream is pressurized to a pressure above the reaction pressure via a mechanical compressor. The solvent and comonomer feeds are pressurized to above the reaction pressure via pumps. The individual catalyst components are manually batch diluted with purified solvent to the preferred component concentrations and pressurized to a pressure above the reaction pressure. All reaction feed streams are metered using mass flow meters and independently controlled by computer automated valve control systems.
[0094] Two reactor systems are used in a series configuration. Each continuous solution polymerization reactor consists of a liquid-filled, non-adiabatic, isothermal circulating loop reactor replicating a continuous stirred tank reactor (CSTR) with heat removal. Independent control of all fresh solvent, ethylene, hydrogen, and catalyst component feeds is possible. The total fresh feed streams (solvent, ethylene, 1-octene, and hydrogen) to each reactor are temperature controlled to maintain them in a single solution phase by passing the feed streams through heat exchangers. The total fresh feed to each polymerization reactor is injected into the reactor at two locations, with reactor volumes approximately equal between each injection location. The fresh feed is controlled, with each injector receiving half of the total fresh feed mass flow rate. The catalyst components are injected into the polymerization reactors through specially designed injection stringers. The main catalyst (pre-catalyst) component feeds are computer controlled to maintain the ethylene conversion of each reactor at a specific target. The co-catalyst components are fed based on specific molar ratios calculated relative to the main catalyst (pre-catalyst) components. Immediately after each reactor feed injection location, the feed stream is mixed with the contents of the circulation polymerization reactor using static mixing elements. The contents of each reactor are continuously circulated through a heat exchanger that serves to remove most of the heat of reaction and at a coolant side that serves to maintain an isothermal reaction environment at a specific temperature. Circulation around each reactor loop is provided by a pump.
[0095] In a dual series reactor configuration, the effluent from the first polymerization reactor (containing solvent, ethylene, 1-octene, hydrogen, catalyst components, and polymer) exits the first reactor loop and is added to the second reactor loop.
[0096] The second reactor effluent enters a zone where it is inactivated by the addition and reaction with water. Following catalyst inactivation and additive addition, the reactor effluent enters a devolatilization system where the polymer is removed from the non-polymer stream. The isolated polymer melt is pelletized and collected. The non-polymer stream passes through various equipment that separates most of the ethylene, which is removed from the system. The solvent and most of the unreacted 1-octene are recycled to the reactor after passing through a purification system. A small amount of solvent and 1-octene are purged from the process.
[0097] Reactor stream feed data flows used to generate the examples correspond to the values in Table 1. The data is presented to allow the reaction system to be more easily treated as a once-through flow diagram, taking into account the complexity of the solvent recycle system. The catalyst components used are referenced in Table 2.
[0098] The polymers prepared were tested for various properties according to the methods described above. In addition, ASPUN 1000 sb was used, both from The Dow Chemical Company. (商標) 6835 Unimodal Ethylene / 1-Octene Copolymer, and ASPUN (商標) 6000 bimodal ethylene / 1-octene copolymer. The results are shown in Table 3. [Table 1] [Table 2] [Table 3]
[0099] Example 2 - Fiber Preparation The fibers are spun on a Hills Bicomponent Continuous Filament Fiber Spinning Line. Bicomponent fibers with a highly eccentric core-sheath configuration were made with an Exxon 3854 PP core and one of the ethylene / alpha-olefin interpolymers as the sheath. The fibers were spun on a Hills Line according to the following conditions: The extruder profile is adjusted to achieve a melt temperature of 240°C. The throughput rate of each hole is 0.5 ghm (grams per minute per hour). One extruder uses Exxon 3854 PP and another uses the ethylene / alpha-olefin interpolymer, operating with a 40 / 60 core / sheath ratio (by weight) using a Hills Bicomponent die. The die consists of 144 holes with a hole diameter of 0.6 mm and a length / diameter (L / D) of 5 / 1. The quench air temperature and flow rate are set at 15-18°C and 520 cfm (cubic feet per minute), respectively. After the quench zone, the 144 filaments are subjected to drawing tension by using air pressure in a slot unit to entrain the filaments in the air stream. The airflow velocity is controlled by the pressure of the slot aspirator.
[0100] Table 4 shows the curvature of bicomponent fibers made from Example 1, ASPUN™ 6835, and ASPUN™ 6000. The bicomponent fiber made from Example 1 shows a significantly higher curvature than the samples made from ASPUN™ 6835 and ASPUN™ 6000. [Table 4]
[0101] Example 3 - Fiber Preparation The fibers are spun on a Hills Bicomponent Continuous Filament Fiber Spinning Line. Bicomponent fibers with a highly eccentric core-sheath configuration were made with an Exxon 3854 PP core and one of the ethylene / alpha-olefin interpolymers as the sheath. The fibers were spun on a Hills Line according to the following conditions: The extruder profile is adjusted to achieve a melt temperature of 210°C. The throughput rate of each hole is 0.5 ghm (grams per minute per hour). One extruder uses Exxon 3854 PP and another uses the ethylene / alpha-olefin interpolymer, using a Hills Bicomponent die and operating with a 40 / 60 core / sheath ratio (by weight). The die consists of 144 holes with a hole diameter of 0.6 mm and a length / diameter of 5 / 1. The quench air temperature and flow rate are set at 15-18 °C and 520 cfm (cubic feet per minute), respectively. After the quench zone, drawing tension is applied to the 144 filaments by entraining the filaments in the air stream using air pressure in a slot unit. The speed of the air stream is controlled by the pressure of the slot aspirator. The curvatures of the fiber examples are shown in Table 5. [Table 5] The present application also relates to the following aspects: (1) A crimped fiber having a fiber centroid, comprising a first region having a first centroid and a second region having a second centroid, the first region comprising an ethylene / alpha olefin interpolymer composition in an amount of at least 75 weight percent based on a total weight of the first region, the ethylene / alpha olefin interpolymer composition characterized by a low temperature peak and a high temperature peak in an elution profile via an Improved Comonomer Composition Distribution (ICCD) procedure, the high temperature peak having a full width at half maximum of less than 6.0° C., the second region being a material comprising a polymer different from the ethylene / alpha-olefin interpolymer of the first region, the regions being positioned such that at least one of the first centroid and the second centroid is not the same as the fiber centroid. (2) The ethylene / alpha olefin interpolymer composition has a viscosity of 0.930 to 0.965 g / cm 3 1. The fiber of claim 1, further characterized by one or more of the following: a density in the range of 10 to 60 g / 10 min, said I2 being measured according to ASTM D1238, 190C, 2.16 kg; a molecular weight distribution, expressed as the ratio of weight average molecular weight to number average molecular weight (Mw(GPC) / Mn(GPC)), in the range of 1.5 to 2.5; and a tan delta at 1 radian / sec of at least 50. (3) The fiber of (1) or (2) above, wherein at least one of the first or second regions has a center of gravity offset of at least 0.1. (4) The fiber according to any one of (1) to (3) above, wherein the first and second regions are arranged in a core-sheath, side-by-side, segmented pie, or sea-island structure. (5) The fiber according to any one of (1) to (4) above, wherein a weight ratio of the first region to the second region is 80:20 to 20:80. (6) The fibers have a thickness of at least 2.0, preferably at least 2.5 mm -1 The fiber according to any one of the above (1) to (5), having a curvature of (7) The fiber according to any one of (1) to (6) above, wherein the second region contains polypropylene. (8) The fiber according to any one of (1) to (7) above, further comprising a third region comprising a polymer different from those of the first and second regions.
Claims
1. A fiber center of gravity, comprising a first region having a first center of gravity and a second region having a second center of gravity, the first region comprises an ethylene / alpha olefin interpolymer composition comprising at least 70 mole percent ethylene-based repeat units and up to 30 mole percent alpha olefin-based repeat units having 3 to 10 carbon atoms in an amount of at least 75 weight percent based on the total weight of the first region; the ethylene / alpha olefin interpolymer composition is characterized by a low temperature peak at least 50° C. and less than 90° C. and a high temperature peak at least 90° C. and less than 100° C. in an elution profile via an improved comonomer composition distribution (ICCD) procedure, the high temperature peak having a full width at half maximum of less than 6.0° C.; The ethylene / alpha olefin interpolymer composition has a viscosity of 0.900 to 0.940 g / cm 3 and a low density fraction having a density in the range of at least 0.950 g / cm 3 and a high density fraction having a density of The ethylene / alpha olefin interpolymer composition has a high temperature fraction having a peak position molecular weight of 15,000 g / mol to 70,000 g / mol or less and a low temperature fraction having a peak position molecular weight of 30,000 to 250,000; the second region is a material comprising a polymer different from the ethylene / alpha-olefin interpolymer of the first region; The region is disposed such that at least one of the first centroid and the second centroid is not the same as the fiber centroid.
2. The ethylene / alpha olefin interpolymer composition has a viscosity of 0.930 to 0.965 g / cm 3 Density in the range of 10 to 60 g / 10 min., melt index (I 2 13. The fiber of claim 1, further characterized by one or more of: an I2 measured according to ASTM D1238, 190C, 2.16 kg; a molecular weight distribution expressed as the ratio of weight average molecular weight to number average molecular weight (Mw(GPC) / Mn(GPC)) in the range of 1.5 to 2.5; and a tan delta at 1 radian / sec of at least 50.
3. 3. The fiber of claim 1 or 2, wherein at least one of the first or second regions has a center of gravity offset of at least 0.
1.
4. 4. The fiber of any one of claims 1 to 3, wherein the first and second regions are arranged in a core-sheath configuration, a side-by-side, a segmented pie configuration, or an islands-in-the-sea configuration.
5. The fiber of any one of claims 1 to 4, wherein a weight ratio of the first regions to the second regions is from 80:20 to 20:
80.
6. The fibers have a thickness of at least 2.0, preferably at least 2.5 mm -1 The fiber according to any one of claims 1 to 5, having a curvature of
7. The fiber of any of claims 1 to 6, wherein the second region comprises polypropylene.
8. The fiber of any of claims 1 to 7, further comprising a third region comprising a different polymer than those of the first and second regions.
Citation Information
Patent Citations
Latently crimping conjugate yarn and production thereof
JP1990191720A
Ethylene-based polymer composition for use as a blending component in shrink film applications
JP2013528689A
Nonwoven fabric, sheet for absorbent article and absorbent article using the same
JP2015165061A
Latent crimpable composite fiber and manufacturing method therefor, conjugate fiber and nonwoven fabric