Circuit board, joint body, and manufacturing method thereof

The circuit board design addresses thermal stress and heat cycle reliability issues by using a silver-rich brazing material layer with low KAM values and copper circuit boards, achieving high durability and reduced crack rates through stress reduction.

JP7555397B2Active Publication Date: 2024-09-24DENKA CO LTD
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
JP2022512240
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2020-03-30
Filing Date
2021-03-29
Publication Date
2024-09-24
Estimated Expiration
2041-03-29

AI Technical Summary

Technical Problem

Circuit boards used in power modules for industrial equipment face reliability issues due to thermal stress and heat cycles, leading to cracks in ceramic substrates and peeling of metal plates, especially under severe conditions.

Method used

A circuit board design where a ceramic substrate and metal circuit board are bonded via a brazing material layer with a silver content of 70% by mass or more, and a KAM value of 0.55° or less, combined with a copper circuit board having a KAM value of 0.36° or less, and an exposed brazing material portion with specific thickness and length, to reduce residual stress.

Benefits of technology

The design significantly enhances durability against heat cycles, reducing crack rates to less than 1% by area, and improves manufacturing efficiency by minimizing residual stress and stress concentration.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007555397000007
    Figure 0007555397000007
  • Figure 0007555397000006
    Figure 0007555397000006
  • Figure 0007555397000004
    Figure 0007555397000004
Patent Text Reader

Abstract

Provided is a circuit board in which a ceramic substrate and a metal circuit board are joined via a brazing material layer that contains silver, wherein the average of the KAM values of the silver portion in the brazing material layer derived by the EBSP method is 0.55° or lower. Provided is a joined body in which a ceramic substrate and a metal board are joined via a brazing material layer that contains silver, wherein the average of the KAM values of the silver portion in the brazing material layer derived by the EBSP method is 0.55° or lower.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present disclosure relates to a circuit board, a joint, and a method for manufacturing the same. [Background technology]

[0002] As industrial equipment such as robots and motors become more sophisticated, the amount of heat generated by semiconductor elements mounted on power modules is also steadily increasing. In order to efficiently dissipate this heat, circuit boards equipped with ceramic substrates having good thermal conductivity are used. Thermal stress is generated in such circuit boards due to the heating and cooling process when bonding the ceramic substrate and the metal plate, and the heat cycle during use. This may lead to cracks in the ceramic substrate and peeling off of the metal plate.

[0003] On the other hand, technology for improving reliability by mitigating thermal stress generated in ceramic circuit boards is being studied. For example, Patent Document 1 studies improving heat cycle resistance characteristics by setting the average size and number density of the Cu-rich phase in the brazing material layer within a predetermined range. Patent Document 2 proposes forming an Ag-rich phase along the bonding interface between the ceramic substrate and the circuit pattern. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] International Publication No. 2018 / 221492 [Patent Document 2] International Publication No. 2019 / 022133 Summary of the Invention [Problem to be solved by the invention]

[0005] Circuit boards are required to have sufficiently excellent reliability depending on the application in which they are used. For example, in the field of power modules for train drives and electric vehicles, etc., they are required to maintain excellent reliability even under severe heat cycle conditions. This is because, for example, when the cooling temperature is lowered, the tensile stress generated in the ceramic substrate increases, making the ceramic substrate more susceptible to cracks. Therefore, the present disclosure provides a circuit board having excellent durability against heat cycles and a manufacturing method thereof. The present disclosure also provides a bonded body having excellent durability against heat cycles and a manufacturing method thereof. [Means for solving the problem]

[0006] A circuit board according to one aspect of the present disclosure is a circuit board in which a ceramic substrate and a metal circuit plate are joined via a brazing filler layer containing silver, and the average KAM value of the silver portion in the brazing filler layer as determined by the EBSP method is 0.55° or less.

[0007] Here, the KAM (Kernel Average Misorientation) value indicates the difference in orientation between adjacent measurement points within a crystal grain, and is determined by crystal orientation analysis using the EBSP (Electron Back Scattering Pattern) method. The smaller the KAM value, the smaller the crystal distortion.

[0008] Since the linear thermal expansion coefficients of the ceramic substrate and the metal circuit plate are significantly different, residual stress occurs at the joint between the ceramic and the metal circuit plate due to the difference in temperature at the time of joining. The residual stress appears as distortion of the crystal structure of the components contained in the brazing material layer. If this residual stress becomes large, cracks are likely to occur in the ceramic substrate, and durability against heat cycles is impaired. In the circuit substrate of the present disclosure, the average value of the KAM value of the silver portion in the brazing material layer is sufficiently small, so that the residual stress at the joint between the ceramic substrate and the metal circuit plate is sufficiently reduced. Therefore, the circuit substrate of the present disclosure has excellent durability against heat cycles.

[0009] The metal circuit plate may be a copper circuit plate. The average KAM value of the copper contained in the copper circuit plate, as determined by the EBSP method, may be 0.36° or less. This allows the residual stress in the joint of the circuit board to be sufficiently reduced, and the durability against heat cycles to be further improved.

[0010] The brazing material layer of the circuit board may have an exposed portion exposed from an end of the metal circuit plate. In this case, the average length L of the exposed portion may be 20 μm or more, and the average thickness T of the exposed portion may be 4 to 30 μm. This allows stress concentration at the joint to be sufficiently alleviated, and durability against heat cycles to be further improved.

[0011] A bonded structure according to one aspect of the present disclosure is a bonded structure in which a ceramic substrate and a metal plate are bonded via a brazing filler layer containing silver, and the average KAM value of the silver portion in the brazing filler layer as determined by the EBSP method is 0.55° or less.

[0012] Since the linear thermal expansion coefficients of the ceramic substrate and the metal plate are significantly different, residual stress occurs at the joint between the ceramic and the metal plate due to the difference in temperature at the time of joining. The residual stress appears as a distortion of the crystal structure of the components contained in the brazing material layer. If this residual stress becomes large, cracks are likely to occur in the ceramic substrate, and durability against heat cycles is impaired. In the joint of the present disclosure, the average value of the KAM value of the silver part in the brazing material layer is sufficiently small, so that the residual stress at the joint between the ceramic substrate and the metal plate is sufficiently reduced. Therefore, the joint of the present disclosure is excellent in durability against heat cycles. By using such a joint, a circuit board excellent in durability against heat cycles can be obtained.

[0013] The metal plate may be a copper plate. When the metal plate is a copper plate, the average KAM value of the copper contained in the copper plate, determined by the EBSP method, may be 0.36° or less. This sufficiently reduces the residual stress in the joint of the joint body, and further improves the durability against heat cycles.

[0014] The brazing material layer of the joined body may have a silver content of 70 mass % or more, and the brazing material layer may have an average thickness T of 4 to 30 μm, thereby making it possible to reduce the size and thickness of the joined body while sufficiently reducing stress generated in the joint and further improving durability against heat cycles.

[0015] A method for producing a bonded body according to one aspect of the present disclosure includes the steps of applying a brazing material containing silver to a main surface of a ceramic substrate, stacking the ceramic substrate and a metal plate via the brazing material to obtain a laminate, firing the laminate by holding it at a firing temperature of 750°C or higher for 10 minutes or more, and annealing the fired laminate by holding it at a temperature of 550°C or higher and less than 750°C for 10 minutes or more.

[0016] In the above manufacturing method, the laminate is annealed by holding it at a sintering temperature of 750°C or higher for 10 minutes or more, and then the sintered laminate is annealed by holding it at a temperature of 550°C or higher and lower than 750°C for 10 minutes or more. Usually, when the laminate is sintered at a sintering temperature of 750°C or higher and cooled to room temperature, a large residual stress occurs at the joint of the bonded body due to the difference in the linear thermal expansion coefficient between the ceramic substrate and the metal plate. However, in the above manufacturing method, the annealing is performed by holding it at a temperature of 550°C or higher and lower than 750°C for 10 minutes or more, so that the residual stress at the joint can be relaxed. Therefore, the residual stress at the joint is sufficiently reduced, and a bonded body having excellent durability against heat cycles can be manufactured.

[0017] In the above manufacturing method, the laminate may be held at a firing temperature of 750°C or higher for less than 3 hours, and may be cooled from the firing temperature to less than 750°C at a temperature drop rate of 1°C / min or more. This can improve manufacturing efficiency and can suppress the diffusion of silver contained in the brazing material into the metal plate. This can improve heat cycle characteristics.

[0018] The above-mentioned bonded body obtained by annealing is a ceramic substrate and a copper plate as a metal plate bonded via a brazing material layer containing silver, and the average KAM value of the silver part in the brazing material layer obtained by the EBSP method may be 0.55° or less, and the average KAM value of the copper contained in the copper plate may be 0.36° or less. In such a bonded body, the average KAM value of the silver part in the brazing material layer and the copper contained in the copper plate is sufficiently small, so that the residual stress in the bonded part between the ceramic substrate and the metal plate is sufficiently reduced. Therefore, the durability against heat cycles is sufficiently excellent.

[0019] A method for producing a circuit board according to one aspect of the present disclosure includes a step of forming a metal circuit plate by removing a part of the metal plate in the bonded body obtained by the above-mentioned production method, thereby obtaining a circuit board. The circuit board thus obtained uses the above-mentioned bonded body, and therefore has sufficiently reduced residual stress at the bonded portion between the ceramic substrate and the metal circuit plate. Therefore, the circuit board has excellent durability against heat cycles.

[0020] The brazing material layer of the circuit board obtained by the above manufacturing method may have an exposed portion exposed from an end of the metal circuit board. In this case, the average length L of the exposed portion may be 20 μm or more, and the average thickness T of the brazing material layer may be 4 to 30 μm. This allows the circuit board to be made smaller and thinner, while sufficiently mitigating stress generated in the joint, thereby further improving durability against heat cycles. Effect of the Invention

[0021] According to the present disclosure, it is possible to provide a circuit board having excellent durability against heat cycles and a method for manufacturing the same. It is also possible to provide a bonded body having excellent durability against heat cycles and a method for manufacturing the same. Such a circuit board and bonded body can be suitably used for, for example, a power module. [Brief description of the drawings]

[0022] [Figure 1] FIG. 1 is a plan view of a circuit board according to an embodiment. [Diagram 2] FIG. 2 is a cross-sectional view taken along line II-II in FIG. [Diagram 3] FIG. 3 is a perspective view of a bonded body according to one embodiment. [Figure 4] FIG. 4 is a cross-sectional view taken along line IV-IV in FIG. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0023] Hereinafter, an embodiment of the present disclosure will be described with reference to the drawings as needed. However, the following embodiment is an example for explaining the present disclosure, and is not intended to limit the present disclosure to the following content. In the description, the same reference numerals are used for the same elements or elements having the same functions, and redundant descriptions are omitted as needed. Furthermore, positional relationships such as up, down, left, and right are based on the positional relationships shown in the drawings, unless otherwise specified. Furthermore, the dimensional ratios of each element are not limited to the ratios shown in the drawings.

[0024] 1 is a plan view of a circuit board according to the present embodiment. The circuit board 100 includes a ceramic substrate 10 and three metal circuit plates 20 bonded to a main surface 10A of the ceramic substrate 10. The ceramic substrate 10 and the metal circuit plates 20 are bonded via a brazing material layer 30. Ends of the brazing material layer 30 are exposed along the outer edge of the metal circuit plate 20.

[0025] Fig. 2 is a cross-sectional view taken along line II-II in Fig. 1. Fig. 2 shows a part of a cross section of the circuit board 100 when cut along a plane perpendicular to the main surfaces 10A and 10B of the ceramic substrate 10. The joints 40 between the ceramic substrate 10 and the pair of metal circuit plates 20 each include a brazing material layer 30.

[0026] The material of the ceramic substrate 10 is not particularly limited. Examples of the ceramics contained in the ceramic substrate 10 include nitride ceramics such as silicon nitride and aluminum nitride, oxide ceramics such as aluminum oxide and zirconium oxide, carbide ceramics such as silicon carbide, and boride ceramics such as lanthanum boride. When the metal plate is bonded by the active metal method, the material of the ceramic substrate 10 may be non-oxide ceramics such as aluminum nitride and silicon nitride. Among these, the ceramic substrate may be made of silicon nitride from the viewpoint of mechanical strength and fracture toughness.

[0027] The ceramic substrate 10 may have a thickness of, for example, 0.1 to 3 mm, 0.2 to 1.2 mm, or 0.25 to 1.0 mm. The metal circuit plate 20 may have a thickness of, for example, 0.1 to 1.5 mm.

[0028] The brazing material layer 30 may be made of an Ag-Cu-Sn brazing material containing silver, copper, tin, and an active metal containing at least one selected from the group consisting of titanium, zirconium, hafnium, and niobium. The silver content in the brazing material layer 30 may be 70 mass% or more, 80 mass% or more, or 85 mass% or more. This allows the residual stress in the joint 40 to be sufficiently reduced while improving the denseness of the brazing material layer 30.

[0029] The active metal in the brazing material layer 30 may be 0.5 to 5 parts by mass relative to 100 parts by mass of the total of silver and copper. By making the content of the active metal 0.5 parts by mass or more, it is possible to improve the bonding strength between the ceramic substrate 10 and the brazing material layer 30. On the other hand, by making the content of the active metal 5 parts by mass or less, it is possible to suppress the formation of a brittle alloy layer at the bonding interface. The active metal may be contained as a hydride, and may contain, for example, titanium hydride (TiH2). The content of TiH2 in the brazing material layer 30 may be 1 to 5 parts by mass relative to 100 parts by mass of the total of silver and copper. This makes it possible to sufficiently increase the bonding strength between the ceramic substrate 10 and the metal circuit plate 20.

[0030] The amount of tin in the brazing material layer 30 may be 0.5 to 5 parts by mass relative to 100 parts by mass of the total of silver and copper. This makes it possible to achieve a high level of both the effect of reducing residual stress and the wettability of the brazing material to the ceramic substrate 10. The amount of copper contained in the brazing material layer 30 may be 5 to 20 parts by mass relative to 100 parts by mass of silver. This makes it possible to sufficiently reduce the residual stress in the joint 40 while improving the denseness of the brazing material layer 30.

[0031] The average KAM (Kernel Average Misorientation) value of the silver portion in the brazing material layer 30 is 0.55° or less. From the viewpoint of further reducing the residual stress in the joint 40, the average KAM value may be 0.53° or less, or may be 0.4° or less. The KAM value of the silver portion may be 0.01° or more, 0.05° or more, 0.10° or more, 0.20° or more, or 0.30° or more. This allows the annealing time during manufacturing to be shortened.

[0032] The KAM value is a value indicating the orientation difference between adjacent measurement points in the crystal grain of the silver part, and is obtained by the EBSP (Electron Back Scattering Pattern) method using a commercially available OIM (Orientation Imaging Microscopy) crystal orientation analyzer. The orientation difference in the crystal grain may be measured using analysis software attached to the OIM crystal orientation analyzer. The average KAM value of the silver part is obtained by measuring at five points of the brazing material layer 30 and calculating the arithmetic average value of each measurement value. When components other than silver are contained in each measurement field, the silver part is separated from the other components by energy dispersive X-ray analysis (EDS) and the average KAM value of the silver part is obtained. In this disclosure, the "silver part" refers to the area of ​​the brazing material layer where silver is detected by EDS.

[0033] The metal circuit plate 20 may be a copper circuit plate from the viewpoint of improving electrical conductivity and heat dissipation. The average KAM value of copper contained in the copper circuit plate may be 0.36° or less, or 0.35° or less. This can further reduce the residual stress in the joint 40. The average KAM value of copper may be 0.01° or more, 0.05° or more, 0.10° or more, 0.20° or more, or 0.30° or more. This can shorten the annealing time during manufacturing. The average KAM value of copper can be obtained in the same manner as the average KAM value of the silver part in the brazing material layer 30.

[0034] The thickness of the metal circuit plate 20 may be 0.1 to 1.5 mm. From the viewpoint of improving heat dissipation, it may be 0.3 mm or more, or may be 0.4 mm or more. The side portion 28 of the metal circuit plate 20 may be formed so as to widen as it approaches the ceramic substrate 10 as shown in Fig. 2. However, the shape of the side portion of the metal circuit plate 20 is not limited to the shape shown in Fig. 2.

[0035] An end of the brazing material layer 30 is exposed at the outer edge of the metal circuit plate 20. In the present disclosure, the end of the brazing material layer 30 that is not covered by the metal circuit plate 20 at the outer edge of the metal circuit plate 20 is referred to as an exposed portion 32. Although it is not essential to have the exposed portion 32, having the exposed portion 32 can alleviate stress concentration that occurs at the joint 40. This can further improve durability against heat cycles.

[0036] The average values ​​of the thickness T and length L of the exposed portion 32 are the arithmetic average values ​​of the thickness T and length L measured at five arbitrarily selected points (five visual fields) of the exposed portion 32. The average value of the length L of the exposed portion 32 may be 20 μm or more, or may be 30 μm or more. Residual stress caused by the difference in the linear thermal expansion coefficient between the ceramic substrate 10 and the metal circuit plate 20 tends to concentrate at the outer edge of the metal circuit plate 20. Therefore, by having the average value of the length L of the exposed portion 32 within the above-mentioned range, the concentration of residual stress is alleviated, and durability against heat cycles can be further improved. From the viewpoint of miniaturizing the circuit board 100, the average value of the length L of the exposed portion 32 may be 150 μm or less, 100 μm or less, 75 μm or less, or 50 μm or less.

[0037] The average value of the thickness T of the exposed portion 32 may be 4 to 30 μm, 6 to 20 μm, or 6 to 15 μm. This allows the bonding strength of the bonding portion 40 to be sufficiently high. The average value of the thickness T of the exposed portion 32 is the thickness of the brazing material layer 30 between the ceramic substrate 10 and the metal circuit plate 20. may be equal to the average value of However, in a modified example, the average value of the thickness T of the exposed portion 32 may be different from the average value of the thickness of the brazing material layer 30 between the ceramic substrate 10 and the metal circuit plate 20. Both of these average values ​​of thickness may be within the above-mentioned range (the range of the average value of thickness T). When the thickness T varies depending on the position of the exposed portion 32 in one field of view, the average value of the maximum and minimum values ​​of the thickness T in that field of view is the thickness T of that field of view.

[0038] The metal circuit board 20 may have a plating film on the surface portion. From the viewpoint of improving weather resistance and solder wettability, the plating film may be a Ni plating film, a Ni alloy plating film, or a gold plating film. The Ni plating film may be an electroless Ni plating film. The electroless Ni plating film may be a nickel-phosphorus plating film containing 1 to 12 mass % of nickel. By having such an electroless Ni plating film, the circuit board 100 can be excellent in durability against heat cycles and in solder wettability. The exposed portion 32 may also have a similar plating film on the surface portion.

[0039] In FIG. 1, only one main surface 10A of the ceramic substrate 10 is shown, but the ceramic substrate 10 has a metal circuit plate 20 bonded to the other main surface 10B via a brazing material layer 30 as shown in FIG. 2. In a modified example, a heat sink may be bonded to one of the main surfaces 10A and 10B via a brazing material layer, instead of the metal circuit plate 20. In this case, the metal circuit plate 20 and the heat sink may be made of the same material or different materials. The metal circuit plate 20 has a function of transmitting an electric signal, whereas the heat sink may have a function of transmitting heat. However, the heat sink may have a function of transmitting an electric signal.

[0040] The brazing material layer that bonds the heat sink plate to the main surface of the ceramic substrate may have the same composition and thickness as the brazing material layer that bonds the metal circuit plate. Also, like the brazing material layer 30, the end of the brazing material layer may be exposed from the outer edge of the heat sink plate.

[0041] In the circuit board 100, the average value of the KAM value of the silver portion in the brazing material layer 30 is sufficiently small, so that the residual stress in the joint 40 between the ceramic substrate 10 and the metal circuit plate 20 is sufficiently reduced. Therefore, the circuit board 100 has excellent durability against heat cycles. As an example, the crack rate of the circuit board 100 after the heat cycle test may be less than 1 area %, less than 0.5 area %, or less than 0.3 area %. The heat cycle test here is a test in which a series of steps of holding at -55°C for 15 minutes, at 25°C for 15 minutes, at 150°C for 15 minutes, and at 25°C for 15 minutes is considered as one cycle, and this test is performed 2000 times. The crack rate is the ratio of the area of ​​the crack to the area of ​​the metal circuit plate 20.

[0042] 3 is a perspective view of a bonded body according to one embodiment. The bonded body 200 includes a pair of metal plates 11 arranged to face each other, and a ceramic substrate 10 between the pair of metal plates 11.

[0043] 4 is a cross-sectional view of the bonded body 200 taken along line IV-IV in FIG. 3. Metal plates 11 are bonded to the main surfaces 10A and 10B of the ceramic substrate 10 via brazing layers 31, respectively. That is, the bonded body 200 has two bonding portions 41. The bonded body 200 can be used as a raw material for the circuit board 100. That is, the ceramic substrate 10 in the bonded body 200 has a thickness of 100 mm, and the thickness of the ceramic substrate 10 in the circuit board 100 is 100 mm. Same as Composition (material), shape and thickness By The composition (material) and thickness of the metal plate 11 and the brazing material layer 31 in the bonded body 200 may also be the same as those of the metal circuit plate 20 and the brazing material layer 30 in the circuit board 100.

[0044] The average KAM (Kernel Average Misorientation) value of the silver part in the brazing material layer 31 constituting the joint 41 is also 0.55° or less, similar to the silver part in the brazing material layer 30 of the circuit board 100. From the viewpoint of further reducing the residual stress in the joint 41, this average KAM value may be 0.53° or less, or may be 0.4° or less. The average KAM value of the silver part in the brazing material layer 31 may be 0.01° or more, or may be 0.05° or more. This makes it possible to shorten the annealing time during manufacturing. The method of determining the average KAM value is the same as that of the silver part in the brazing material layer 30 of the circuit board 100.

[0045] The metal plate 11 may be a copper plate from the viewpoint of improving electrical conductivity and heat dissipation. The average KAM value of copper contained in the copper plate may be 0.36° or less, or may be 0.35° or less. This can further reduce the residual stress in the joint 41. The average KAM value of copper in the copper plate may be 0.01° or more, or may be 0.05° or more. This can shorten the annealing time during manufacturing. The method of determining the average KAM value of copper in the copper plate is the same as that of copper contained in the copper circuit board.

[0046] The thickness of the metal plate 11 may be 0.1 to 1.5 mm. From the viewpoint of improving heat dissipation, the thickness may be 0.3 mm or more, or 0.4 mm or more. Lord of It is not essential to provide the metal plate 11 on both the surface 10A and the main surface 10B, and the metal plate 11 may be provided on only one of the surfaces. Furthermore, when the metal plate 11 is provided on both the main surface 10A and the main surface 10B of the ceramic substrate 10, the material, thickness, shape, etc. of the two metal plates 11 may be the same or different from each other. The brazing material layer 31 may be provided over the entire area between the ceramic substrate 10 and the metal plate 11, or may be provided only in the portion where the metal circuit plate 20 is formed.

[0047] Since the average value of the KAM value of the silver portion in the brazing material layer 31 in the bonded body 200 is sufficiently small, the residual stress in the bonded portion 41 between the ceramic substrate 10 and the metal plate 11 is sufficiently reduced. Therefore, the bonded body 200 has excellent durability against heat cycles. By using such a bonded body 200, a circuit board 100 having excellent durability against heat cycles can be obtained.

[0048] An example of a method for manufacturing the bonded body and the circuit board according to the present disclosure will be described below. First, a step of forming a slurry containing an inorganic compound powder, a binder resin, a sintering aid, a plasticizer, a dispersant, a solvent, and the like, into a green sheet is performed.

[0049] Examples of inorganic compounds include nitride ceramics such as silicon nitride and aluminum nitride, oxide ceramics such as aluminum oxide and zirconium oxide, carbide ceramics such as silicon carbide, and boride ceramics such as lanthanum boride. Examples of sintering aids include rare earth metals, alkaline earth metals, metal oxides, fluorides, chlorides, nitrates, and sulfates. These may be used alone or in combination of two or more. The use of a sintering aid can promote the sintering of inorganic compound powder. Examples of binder resins include methyl cellulose, ethyl cellulose, polyvinyl alcohol, polyvinyl butyral, and (meth)acrylic resins.

[0050] Examples of the plasticizer include purified glycerin, glycerin trioleate, diethylene glycol, phthalic acid plasticizers such as di-n-butyl phthalate, and dibasic acid plasticizers such as di-2-ethylhexyl sebacate. Examples of the dispersant include poly(meth)acrylate and (meth)acrylic acid-maleate copolymer. Examples of the solvent include organic solvents such as ethanol and toluene.

[0051] Examples of the method for forming the slurry include a doctor blade method and an extrusion molding method. Next, the green sheet obtained by molding is degreased and sintered. The degreasing may be performed, for example, by heating at 400 to 800°C for 0.5 to 20 hours. This can reduce the amount of residual organic matter (carbon) while suppressing oxidation and deterioration of inorganic compounds. The sintering is performed by heating at 1700 to 1900°C in a non-oxidizing gas atmosphere such as nitrogen, argon, ammonia, or hydrogen. This can obtain the ceramic substrate 10. If necessary, the edge of the ceramic substrate 10 may be cut by laser processing to adjust the shape. In addition, a scribe line may be formed on the main surface 10A and / or the main surface 10B of the ceramic substrate 10.

[0052] The above-mentioned degreasing and sintering may be performed in a state where a plurality of green sheets are laminated. When the green sheets are laminated and degreasing and sintering are performed, a release layer made of a release agent may be provided between the green sheets in order to facilitate separation of the base material after firing. For example, boron nitride (BN) may be used as the release agent. The release layer may be formed by applying, for example, a slurry of boron nitride powder by a method such as spraying, brushing, roll coating, or screen printing. The number of green sheets to be laminated may be, for example, 5 to 100 sheets, or 10 to 70 sheets, from the viewpoint of efficiently mass-producing ceramic substrates while sufficiently advancing degreasing.

[0053] In this manner, the ceramic substrate 10 as shown in Fig. 3 and Fig. 4 is obtained. Next, a process of obtaining a bonded body using the ceramic substrate 10 and a pair of metal plates 11 is performed. Specifically, first, a brazing material is applied to the main surface 10A and the main surface 10B of the ceramic substrate 10, and the pair of metal plates 11 are bonded to the main surface 10A and the main surface 10B, respectively. The metal plates 11 may have a flat plate shape similar to that of the ceramic substrate 10.

[0054] The brazing material is applied to the main surface 10A and the main surface 10B of the ceramic substrate 10 by a method such as a roll coater method, a screen printing method, or a transfer method. The brazing material contains, for example, silver powder, copper powder, tin powder, and powder of an active metal or a compound thereof (hydride), an organic solvent, and a binder. The content of the tin powder may be 0.5 to 5 parts by mass relative to a total of 100 parts by mass of the silver powder and the copper powder. The content of the metal hydride powder may be 1 to 8 parts by mass relative to a total of 100 parts by mass of the silver powder and the copper powder. The viscosity of the brazing material may be, for example, 5 to 20 Pa·s. The content of the organic solvent in the brazing material may be, for example, 5 to 25% by mass, and the content of the binder may be, for example, 2 to 15% by mass.

[0055] For example, the silver powder has a specific surface area of ​​0.1 to 0.5 m 2 / g may be used. This improves the bonding property and improves the uniformity of the structure of the Ag-Cu-Sn brazing material layer. The specific surface area can be measured by gas adsorption. The copper powder has the effect of improving the melting property of the Ag-Cu-Sn brazing material. The tin powder has the effect of reducing the contact angle of the brazing material with respect to the ceramic substrate 10 and improving the wettability of the brazing material.

[0056] A metal plate 11 is placed on the main surface 10A and the main surface 10B of the ceramic substrate 10 to which the brazing material is applied to obtain a laminate. Then, a firing step is performed in which the laminate is fired in a heating furnace. The temperature inside the furnace during firing (firing temperature) is 750° C. or higher, and may be 750 to 950° C. or 780 to 900° C. The time (firing time) for holding the firing temperature is 10 minutes or more, and may be 15 minutes or more. From the viewpoint of suppressing the diffusion of silver into the metal plate 11, the firing time may be less than 3 hours, or may be less than 90 minutes.

[0057] The atmosphere in the heating furnace during firing may be an inert gas such as nitrogen, and may be reduced pressure (1.0×10 -3The heating may be performed at a pressure of 1000 MPa (or less) or in a vacuum. By firing the laminate under such conditions, the ceramic substrate 10 and the metal plate 11 can be sufficiently bonded to each other. The heating furnace may be a continuous type that continuously produces a plurality of bonded bodies, or may be a batch type that produces one or a plurality of bonded bodies. Heating may be performed while pressing the laminate in the stacking direction.

[0058] Next, an annealing step is performed in which the fired laminate is annealed by holding it at a furnace temperature of 500°C or more and less than 750°C for 10 minutes or more. The furnace temperature during annealing (annealing temperature) may be 550°C or more and 700°C or less, or 550°C or more and 650°C or less. The annealing time may be 20 minutes or more from the viewpoint of sufficiently reducing residual stress in the joint. The annealing time may be less than 4 hours from the viewpoint of improving manufacturing efficiency. The annealing may be performed using the same heating furnace as that used during firing, or a different heating furnace. The annealing may be performed under an inert gas atmosphere such as nitrogen, or may be performed under reduced pressure below atmospheric pressure, or may be performed under vacuum.

[0059] After the firing step, the inside of the furnace may be cooled at a temperature drop rate of 1° C. / min or more to the above-mentioned annealing temperature. This can improve the manufacturing efficiency and suppress the diffusion of silver contained in the brazing material into the metal plate. From the same viewpoint, the temperature drop rate may be 2° C. / min or more, or may be 3° C. / min or more. On the other hand, from the viewpoint of reducing thermal shock, the temperature drop rate may be less than 20° C. / min.

[0060] Through the above steps, a bonded body 200 can be obtained in which the ceramic substrate 10 and the metal plates 11 are bonded to the main surfaces 10A and 10B of the ceramic substrate 10 via the brazing layers 31. This manufacturing method includes a step of annealing after firing, so that the residual stress in the bonded portion 41 can be reduced. Therefore, a bonded body 200 having excellent durability against heat cycles can be manufactured.

[0061] When manufacturing a circuit board, a step is performed in which a part of the metal plate 11 in the bonded body 200 obtained in the above-mentioned step is removed to form the metal circuit plate 20. This step may be performed by, for example, photolithography. Specifically, first, a photosensitive resist is printed on the main surface of the bonded body 200 (the main surface of the metal plate 11). Then, an exposure device is used to form a resist pattern having a predetermined shape. The resist may be either negative type or positive type. Uncured resist is removed by, for example, washing.

[0062] After forming the resist pattern, the portions of the metal plate that are not covered by the resist pattern are removed by etching. As a result, the main surface 10A and a part of the main surface 10B of the ceramic substrate 10 are exposed in the portions. The resist pattern is then removed to obtain the circuit board 100. Note that the shape of the side portion 28 of the metal circuit plate 20 and the length L and thickness T of the exposed portion 32 of the brazing material layer 30 can be adjusted by changing the etching conditions or the number of times of etching.

[0063] The etching solution is not particularly limited, and for example, a ferric chloride solution, a cupric chloride solution, sulfuric acid, and hydrogen peroxide solution can be used. After etching, if the brazing material layer or the like remains on the main surface 10A and the main surface 10B of the ceramic substrate 10, they may be removed using a solution containing at least one selected from the group consisting of an aqueous ammonium halide solution, an inorganic acid such as sulfuric acid and nitric acid, and hydrogen peroxide solution. The method for removing the resist pattern is not particularly limited, and may be performed by, for example, immersing in an alkaline aqueous solution.

[0064] The circuit board 100 thus obtained uses the bonded body 200, and therefore the residual stress in the bonded portion 40 between the ceramic substrate 10 and the metal circuit plate 20 is sufficiently reduced. That is, the average value of the KAM value of the silver portion in the brazing material layer 30 of the circuit board 100 is equivalent to the average value of the KAM value of the silver portion in the brazing material layer 31 of the bonded body 200. The average value of the KAM value of the metal contained in the metal circuit plate 20 of the circuit board 100 is also equivalent to the average value of the KAM value of the metal contained in the metal plate 11 of the bonded body 200. Therefore, the circuit board 100 is excellent in durability against heat cycles, like the bonded body 200. Although an example of the manufacturing method of the bonded body 200 and the circuit board 100 has been described above, the present invention is not limited thereto.

[0065] The circuit board 100 has excellent durability against heat cycles, and may be used, for example, in a power module that handles large currents.

[0066] Although the embodiments of the present disclosure have been described above, the present disclosure is not limited to the above embodiments. For example, the brazing material layer 31 in the bonded body 200 may be formed only on the portion that will become the metal circuit plate 20, or on the portion and its vicinity, as shown in FIG. 4. Also, the brazing material layer 31 may be formed so as to cover the entire main surface 10A and the main surface 10B of the ceramic substrate 10. In FIG. 4, the brazing material layer 31 and the metal plate 11 are provided on both the main surface 10A and the main surface 10B of the ceramic substrate 10, but in another example, the brazing material layer 31 and the metal plate 11 may be provided on only one of the main surfaces. EXAMPLES

[0067] The present disclosure will be described in more detail with reference to examples and comparative examples, but the present disclosure is not limited to the following examples.

[0068] Example 1 [Preparation of junction] To prepare the brazing material, the following raw material powders were prepared. Silver powder: manufactured by Fukuda Metal Foil & Powder Co., Ltd., Ag-HWQ (trade name), average particle size D50: 2.5 μm, specific surface area 0.4 m2 / g Copper powder: manufactured by Fukuda Metal Foil & Powder Co., Ltd., Cu-HWQ (trade name), average particle size D50: 3.0 μm, specific surface area: 0.4 m 2 / g Tin powder: Manufactured by Fukuda Metal Foil and Powder Co., Ltd.: Sn-HPN (trade name), average particle diameter D50: 3μm, specific surface area 0.1m 2 / g Titanium hydride powder: TCH-100 (product name), manufactured by Toho Tech Co., Ltd.

[0069] A brazing filler metal was prepared by mixing 1 part by mass of tin powder and 3.5 parts by mass of titanium hydride powder with a total of 100 parts by mass of silver powder (90 parts by mass) and copper powder (10 parts by mass), and adding an organic solvent and a binder, etc. A brazing filler metal was applied to both main surfaces of a commercially available silicon nitride substrate (thickness: 0.32 mm) with a coating amount of 8 mg / cm. 2 The coating was performed by screen printing.

[0070] A copper plate (thickness: 0.5 mm, purity: 99.60% oxygen-free copper plate (JIS H 3100, C1020)) was stacked on each of the main surfaces of the silicon nitride substrate to obtain a laminate. The laminate was heated in a nitrogen atmosphere using an electric furnace at a furnace temperature of 860°C for 18 minutes to melt the brazing powder and bond the ceramic substrate and the metal plate (firing process). Then, the furnace temperature was cooled to 600°C at an average temperature drop rate of 10°C / min. Annealing was performed by holding the furnace temperature at 600°C for 10 minutes in a nitrogen atmosphere (annealing process). Then, heating was stopped and the substrate was naturally cooled to room temperature in a nitrogen atmosphere. The average temperature drop rate of the furnace temperature after the annealing process was 6°C / min. In this way, a bonded body was produced in which a ceramic substrate and a pair of metal plates were bonded via a brazing layer.

[0071] [KAM value measurement] After embedding the bonded body in resin, a coater machine was used to cut the bonded body in the thickness direction so as to pass through the center of gravity. The cross section of the bonded body was subjected to flat milling to obtain a sample for EBSD measurement. EBSD measurement of the cut surface was performed using an OIM (Orientation Imaging Microscopy) crystal orientation analyzer manufactured by TSL Solutions Co., Ltd. The measurement voltage was 15 kV, the working distance was 17 mm, and the sample tilt angle was 70°.

[0072] The measurement field of view was 240 μm × 160 μm, and the measurement distance d = 0.2 μm, and the KAM value was measured at five points on both the brazing layer and the copper plate using an OIM crystal orientation analyzer. For the brazing layer, the silver and copper parts in the brazing layer were separated using EDS measurement, and the KAM value of the silver part was obtained. The average KAM value of the silver part measured at five points was as shown in Table 1. The average KAM value of copper measured at five points on the copper plate was as shown in Table 1.

[0073] [Creating a circuit board] An etching resist was printed on the copper plate at predetermined positions on both main surfaces of the bonded body, and a resist pattern having a predetermined shape was formed on the main surface of the copper plate using an exposure device, followed by etching using a ferric chloride solution. Further, etching was performed using a mixed solution of ammonium fluoride and hydrogen peroxide to remove the portion where the resist pattern was not formed, thereby forming a predetermined circuit pattern and an exposed portion of the brazing material layer along the outer edge of the circuit pattern.

[0074] Next, the substrate was pretreated by degreasing and chemical polishing, and then anti-rust treatment was performed using a benzotriazole compound. In this way, a circuit board was obtained in which a ceramic substrate and a metal circuit plate were bonded via a brazing layer containing silver, as shown in Figure 1.

[0075] [Measurement of exposed part length L and thickness T] The exposed portion of the brazing material layer in the circuit board was observed using a scanning electron microscope (SU6600, manufactured by Hitachi High-Technologies Corporation). Reflected electron image observation (magnification: 200x) was performed in five fields of view (each field of view was 400μm long × 600μm wide), and the length and thickness of the exposed portion for each field of view were determined. The thickness for each field of view was taken as the average of the maximum and minimum thicknesses of the exposed portion. The average length L and thickness T for the five fields of view were determined. The results are shown in Table 1.

[0076] [Evaluation of heat cycle characteristics] A heat cycle test was performed on the fabricated circuit board. Specifically, a series of steps of holding at -78°C for 5 minutes, 25°C for 5 minutes, 350°C for 5 minutes, and 25°C for 5 minutes was defined as one cycle, and this cycle was repeated 15 times. After that, etching was performed using a ferric chloride solution, and then etching was performed using a mixed solution of ammonium fluoride and hydrogen peroxide to remove the circuit pattern and brazing layer.

[0077] Using a scanner, an image of the main surface of the ceramic substrate from which the circuit pattern and the brazing material layer had been removed was obtained at a resolution of 600 dpi x 600 dpi. The image was binarized using image analysis software GIMP2 (threshold 140) to calculate the area of ​​the cracks. The calculated crack area was divided by the area of ​​the circuit pattern to obtain the crack ratio. The results are shown in Table 1.

[0078] Example 2 A laminate was obtained in the same manner as in Example 1. A bonded body in which a ceramic substrate and a pair of metal plates were bonded via a brazing material layer was produced in the same manner as in Example 1, except that the conditions of the firing step and the annealing step were changed as shown in Table 2. The firing step and the annealing step were performed in a vacuum atmosphere (1.0×10 -3 After the annealing process, the heating was stopped and the sample was allowed to cool naturally to room temperature in a vacuum atmosphere. The average cooling rate after the annealing process was 3°C / min.

[0079] The KAM value was measured, the circuit board was prepared, the length L and thickness T of the exposed portion were measured, and the heat cycle characteristics were evaluated in the same manner as in Example 1. The results are shown in Table 3.

[0080] (Examples 3 and 4) A laminate was obtained in the same manner as in Example 1. A bonded body in which a ceramic substrate and a pair of metal plates were bonded via a brazing material layer was produced in the same manner as in Example 1, except that the conditions of the firing step and the annealing step were changed as shown in Table 2. After the annealing step, heating was stopped and the body was naturally cooled to room temperature in a vacuum atmosphere. The average rate of temperature drop in the furnace after the annealing step was 6° C. / min.

[0081] The KAM value was measured, the circuit board was prepared, the length L and thickness T of the exposed portion were measured, and the heat cycle characteristics were evaluated in the same manner as in Example 1. The results are shown in Table 3.

[0082] (Examples 5 and 6) A laminate was obtained in the same manner as in Example 1, except that the composition of the brazing material was as shown in Table 1. Then, a bonded body in which a ceramic substrate and a pair of metal plates were bonded via a brazing material layer was produced in the same manner as in Example 1, except that the conditions of the firing step and the annealing step were changed as shown in Table 2. In Example 5, after the annealing step, heating was stopped and the laminate was placed in a vacuum atmosphere (1.0×10 -3 The samples were naturally cooled to room temperature in a furnace at a pressure of 100 Pa or less. The average rate at which the temperature in the furnace decreased after the annealing step was 3° C. / min. In Example 6, after the annealing step, the heating was stopped and the samples were naturally cooled to room temperature in a nitrogen atmosphere. The average rate at which the temperature in the furnace decreased after the annealing step was 6° C. / min.

[0083] The KAM value was measured, the circuit board was prepared, the length L and thickness T of the exposed portion were measured, and the heat cycle characteristics were evaluated in the same manner as in Example 1. The results are shown in Table 3.

[0084] Comparative Example 1 A bonded body was obtained in the same manner as in Example 1, except that no annealing step was performed during the preparation of the bonded body. After the firing step, the average temperature drop rate to room temperature was 6° C. / min. The KAM value was measured, a circuit board was prepared, the length L and thickness T of the exposed portion were measured, and the heat cycle characteristics were evaluated in the same manner as in Example 1. The results are shown in Table 3.

[0085] Comparative Example 2 A bonded body was produced in the same manner as in Comparative Example 1, except that the composition of the brazing material was as shown in Table 1. After the firing process, the average temperature drop rate to room temperature was 6°C / min. The KAM value was measured, a circuit board was produced, the length L and thickness T of the exposed portion were measured, and the heat cycle characteristics were evaluated in the same manner as in Example 1. The results are shown in Table 3.

[0086] [Table 1]

[0087] [Table 2]

[0088] [Table 3]

[0089] As shown in Table 3, in Examples 1 to 6 in which the annealing step was performed, the crystal distortion of the silver and copper contained in the brazing material layer and the copper plate, respectively, was smaller than in Comparative Examples 1 and 2. This confirmed that the crack rate could be reduced. [Industrial Applicability]

[0090] According to the present disclosure, there is provided a circuit board having excellent durability against heat cycles and a method for manufacturing the same. Also, there is provided a bonded body having excellent durability against heat cycles and a method for manufacturing the same, and a circuit board having excellent durability against heat cycles is provided. [Explanation of symbols]

[0091] 10...ceramic substrate, 10A, 10B...main surface, 11...metal plate, 20...metal circuit plate, 28...side portion, 30, 31...soldering material layer, 32...exposed portion, 40, 41...joint, 100...circuit board, 200...joint body.

Claims

1. A circuit board in which a silicon nitride substrate and a copper circuit plate are joined via a brazing material layer containing silver, copper, tin, and titanium, A circuit board, wherein the average KAM value of the silver portion in the brazing material layer, as determined by an EBSP method, is 0.55° or less.

2. A circuit board as described in claim 1, wherein the average KAM value of the copper contained in the copper circuit board, determined by the EBSP method, is 0.36° or less.

3. the brazing material layer has an exposed portion exposed from an end portion of the copper circuit board, The average length L of the exposed portion is 20 μm or more, 3. The circuit board according to claim 1, wherein an average value of a thickness T of the exposed portion is 4 to 30 μm.

4. A bonded body in which a silicon nitride substrate and a copper plate are bonded via a brazing material layer containing silver, copper, tin, and titanium, A joint, wherein the average KAM value of the silver portion in the brazing material layer, as determined by an EBSP method, is 0.55° or less.

5. The joint described in claim 4, wherein the average KAM value of the copper contained in the copper plate, determined by the EBSP method, is 0.36° or less.

6. The silver content in the brazing material layer is 70% by mass or more, The bonded body according to claim 4 or 5, wherein the brazing material layer has an average thickness T of 4 to 30 μm.

7. A step of applying a brazing material containing silver, copper, tin and titanium hydride to a main surface of a silicon nitride substrate; a step of stacking the silicon nitride substrate and a copper plate via the brazing material to obtain a laminate; A step of firing the laminate at a firing temperature of 750° C. or more for 10 minutes or more; and annealing the sintered laminate at a temperature of 550°C or higher and lower than 750°C for 10 minutes or longer to obtain a joined body in which the silicon nitride substrate and the copper plate are joined via a brazing material layer containing silver, copper, tin and titanium, and an average KAM value of the silver portion of the brazing material layer as determined by an EBSP method is 0.55° or less.

8. The time for which the laminate is held at a firing temperature of 750° C. or higher is less than 3 hours; The method for producing a bonded body according to claim 7, wherein the temperature is decreased from the sintering temperature to less than 750°C at a temperature decreasing rate of 1°C / min or more.

9. The method for producing a joint body according to claim 7 or 8, wherein an average KAM value of copper contained in the copper plate of the joint body obtained by annealing is 0.36° or less.

10. A method for producing a circuit board, comprising a step of removing a part of the copper plate in the bonded body obtained by the method according to any one of claims 7 to 9 to form a copper circuit plate, thereby obtaining a circuit board.

11. the circuit board has an exposed portion where the brazing material layer is exposed from an end portion of the copper circuit plate, The average length L of the exposed portion is 20 μm or more, The method for manufacturing a circuit board according to claim 10, wherein an average thickness T of the brazing material layer is 4 to 30 μm.

Citation Information

Patent Citations

  • Metal-ceramic composite substrate, its production and brazing material used for that

    JP1998251075A

  • Manufacturing method of junction

    JP2005051066A

  • Ceramic circuit board

    JP2005252087A

  • Method of joining members having different thermal expansion coefficients

    JP2008044009A

  • Joint body of ceramic body with metal body and method for joining ceramic body with metal body

    JP2015030658A